Method of producing positive electrode active material, method of manufacturing sodium ion battery, positive electrode active material, and sodium ion battery
By producing a Na-containing transition metal oxide with a P2 type structure and further doping it with Na, the reversible capacity of the positive electrode active material is enhanced, resulting in higher performance.
Patent Information
- Application Number
- JP2023066525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-14
AI Technical Summary
Conventional positive electrode active materials with a P2 type structure have not fully exploited their reversible capacity potential.
A method involving the production of a Na-containing transition metal oxide with a P2 type structure, followed by further doping with Na using a reducing solution, to enhance the Na content and stabilize the structure.
The method results in a positive electrode active material with higher Na content and capacity, achieving improved performance.
Smart Images

Figure 2024152374000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a method for producing a positive electrode active material, a method for producing a sodium ion battery, a positive electrode active material, and a sodium ion battery. [Background technology]
[0002] As disclosed in Patent Document 1, a Na-containing transition metal oxide having a P2 type structure is known as a positive electrode active material. Here, the Na-containing transition metal oxide having a P2 type structure is used as a positive electrode active material for, for example, a sodium ion battery. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-201588 A Summary of the Invention [Problem to be solved by the invention]
[0004] It is difficult to say that the potential of conventional positive electrode active materials having a P2 type structure has been fully utilized in terms of reversible capacity. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A method for producing a positive electrode active material, comprising: Obtaining a Na-containing transition metal oxide having a P2 type structure, and The Na-containing transition metal oxide is further doped with Na. A method for producing a positive electrode active material. <Aspect 2> The method for producing aspect 1, By bringing a reducing solution containing Na ions into contact with the Na-containing transition metal oxide, the Na-containing transition metal oxide is further doped with Na. Production method. <Aspect 3> A method for manufacturing a sodium ion battery, comprising: manufacturing a positive electrode active material by the method of Aspect 1 or 2; obtaining a positive electrode active material layer using the manufactured positive electrode active material; and obtaining a sodium ion battery using the positive electrode active material layer. A method for manufacturing a sodium ion battery. <Aspect 4> A positive electrode active material, comprising: having a P2-type structure; Na a Mn x-p Ni y-q Co z-r M p+q+r O 2 (where 0.70 < a ≤ 1.40, x + y + z = 1, 0 ≤ p + q + r < 0.17, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), having a chemical composition represented by: Positive electrode active material. <Aspect 5> A sodium ion battery, comprising a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains the positive electrode active material of Aspect 4. Sodium ion battery.
Advantages of the Invention
[0006] The positive electrode active material of the present disclosure has a high capacity.
Brief Description of the Drawings
[0007] [Figure 1] An example of the process flow for manufacturing a positive electrode active material is shown. [Diagram 2] An example of the process flow for manufacturing a sodium ion battery is shown. [Diagram 3] 1 illustrates a schematic diagram of an example of the configuration of a sodium ion battery. [Figure 4] 1 shows X-ray diffraction patterns of the positive electrode active materials of Comparative Example, Example 1, and Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1. Manufacturing method of positive electrode active material As shown in FIG. 1, a method for producing a positive electrode active material according to one embodiment includes obtaining a Na-containing transition metal oxide having a P2 type structure (step S1), and further doping the Na-containing transition metal oxide with Na (step S2).
[0009] 1.1 Process S1 In step S1, the Na-containing transition metal oxide having a P2 type structure can be obtained, for example, by obtaining a precursor containing Na and a transition metal element, optionally shaping the precursor, optionally pre-firing the precursor, and then performing main firing.
[0010] In step S1, the precursor may be obtained by, for example, mixing a transition metal source and a Na source. The transition metal source may be, for example, a transition metal salt such as a carbonate, sulfate, nitrate, acetate, or the like, or a transition metal compound such as a transition metal hydroxide. The transition metal element may be at least one of Mn, Ni, and Co. The transition metal source may be Me(CO 3 ) x (Me is at least one transition metal element selected from Mn, Ni, and Co, and x is the valence of Me), or a salt represented by Me(SO 4 ) x or a salt represented by Me(NO 3 ) x or a salt represented by Me(CH 3 COO) x or a salt represented by Me(OH) xThe Na source may be, for example, a Na salt such as a carbonate or sulfate, or a Na compound such as sodium oxide or sodium hydroxide. The amount of the Na source mixed with the transition metal source may be determined taking into account the amount of Na lost during the subsequent firing. In step S1, the surface of the particle made of the transition metal source may be coated with the Na source to obtain a coated particle as a precursor. Here, the coated particle may be obtained by coating at least a part of the surface of the particle made of the transition metal source with the Na source. The coated particle may be obtained by coating 40 area % or more, 50 area % or more, 60 area % or more, or 70 area % of the surface of the particle made of the transition metal source with the Na source.
[0011] In step S1, the precursor may be obtained by mixing, for example, a transition metal source, a Na source, and an M source containing element M. Here, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. The element M can further stabilize the P2 type structure. The M source may be, for example, a salt such as a nitrate, sulfate, carbonate, or acetate, or a compound other than a salt such as a hydroxide. The amount of the M source in the precursor may be appropriately determined according to the target composition of the Na-containing transition metal oxide after firing.
[0012] In step S1, the precursor may be obtained by, for example, obtaining a precipitate using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound, and then mixing the precipitate with a Na source and, optionally, an element M source. Examples of ion sources capable of forming a precipitate with transition metal ions include sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. Examples of transition metal compounds include salts and hydroxides such as nitrates, sulfates, carbonates, and acetates. In step S1, the ion source and the transition metal compound may be prepared as respective solutions, and the respective solutions may be dropped and mixed to obtain a precipitate. In this case, various sodium compounds may be used as bases, and an aqueous ammonia solution or the like may be added to adjust the basicity. More specifically, in step S1, a precipitate containing at least one transition metal element selected from Mn, Ni, and Co may be obtained. The precipitate may be obtained by, for example, a solution method such as a coprecipitation method or a sol-gel method. In the case of the coprecipitation method, for example, Me(SO 4 ) x and Na 2 CO 3 The precipitate is obtained by preparing an aqueous solution of the above and dropping and mixing each aqueous solution. After collecting the precipitate, the precipitate may be mixed with a Na source. The amount of the Na source to be mixed with the precipitate may be determined taking into consideration the amount of Na lost during the subsequent firing. The surface of the particles made of the precipitate may be coated with a Na salt to obtain coated particles as a precursor. The coverage rate of the coated particles is as described above.
[0013] In step S1, the pre-baking of the precursor obtained as described above may be performed at a temperature equal to or lower than that of the main baking. For example, the pre-baking may be performed at a temperature lower than 700° C. The pre-baking time is not particularly limited. Alternatively, the pre-baking may be omitted.
[0014] In step S1, the precursor may be sintered at a temperature of, for example, 700°C or higher and 1100°C or lower. The temperature is preferably 800°C or higher and 1000°C or lower. If the sintering temperature is too low, Na doping is not performed, and if the sintering temperature is too high, an O3 type structure is likely to be formed instead of a P2 type structure. The temperature rise conditions from the preliminary sintering temperature to the sintering temperature are not particularly limited. The sintering time is also not particularly limited, and may be, for example, 30 minutes or longer and 10 hours or shorter. The sintering atmosphere is also not particularly limited, and may be, for example, an oxygen-containing atmosphere such as air atmosphere or an inert gas atmosphere.
[0015] In step S1, after the main firing, the Na-containing transition metal oxide having a P2 type structure may be doped with the element M. That is, after synthesizing a Na-containing transition metal oxide having a P2 type structure that does not contain the element M, the oxide may be doped with the element M. The doping with the element M may be performed by, for example, ion exchange.
[0016] The Na-containing transition metal oxide having a P2 type structure obtained by step S1 may contain, for example, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, at least one of Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, the performance of the positive electrode active material is likely to be further improved. More specifically, the Na-containing transition metal oxide obtained by step S1 contains Na c Mn x-p Ni y-q Co z-r M p+q+r O 2(Here, 0 < c ≤ 0.70, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) It may have a chemical composition represented by. When the Na-containing transition metal oxide has such a chemical composition, the P2-type structure is likely to be maintained. In the above chemical composition, c is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more. Also, x is 0 or more, may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, may be 0.10 or more or 0.20 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, may be 0.10 or more, 0.20 or more, or 0.30 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The contribution of the element M to charge and discharge is small. In this regard, in the above chemical composition, since p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.15 or less, 0.13 or less, 0.11 or less, 0.09 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less. On the other hand, when the element M is included, the P2-type structure is likely to be stabilized. In this regard, in the above chemical composition, p + q + r is 0 or more, and may be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.)
[0017] 1.2 Process S2 By passing through the above step S1, a Na-containing transition metal oxide having a P2 type structure can be obtained. However, according to the knowledge of the present inventors, it is difficult to obtain a sufficient amount of Na contained in the Na-containing transition metal oxide by only passing through the above step S1. For example, the molar ratio of Na (above) in the Na-containing transition metal oxide after the above firing is only 0.70 or less, and the potential of the reversible capacity of the P2 type positive electrode active material cannot be fully utilized.
[0018] On the other hand, in step S2, the Na-containing transition metal oxide obtained in step S1 is further doped with Na, so that the molar ratio of Na in the Na-containing transition metal oxide (a) can be increased to more than 0.70. In step S2, for example, the Na-containing transition metal oxide may be further doped with Na without applying a driving force by voltage. For example, the Na-containing transition metal oxide may be doped with Na by contacting a Na-doping source with the Na-containing transition metal oxide.
[0019] Specifically, in step S2, it is preferable to contact the Na-containing transition metal oxide with a reducing solution containing Na ions to further dope the Na-containing transition metal oxide with Na. The "reducing solution" means a solution having reducing properties, and may be, for example, a solution containing an electrophile. The reducing solution may be, for example, a solution obtained by dissolving an electrophile and a Na source in a solvent. The solvent may be various organic solvents capable of dissolving the electrophile and the Na source. The solvent is preferably, for example, an ether-based solvent such as tetrahydrofuran or dimethoxyethane. The electrophile may be various substances that dissolve in the above-mentioned solvent. The electrophile is preferably an aromatic organic compound such as biphenyl. The Na source may be various substances that dissolve in the above-mentioned solvent to generate Na ions. The Na source may be metallic sodium or a Na compound.
[0020] The concentration of the electrophile and Na ions contained in the reducing solution may be appropriately determined according to the desired doping amount. According to the findings of the present inventors, the greater the amount of Na ions contained in the reducing solution relative to the amount of Na-containing transition metal oxide contacted with the reducing solution, the greater the amount of Na doping of the Na-containing transition metal oxide. For example, when the above-mentioned Na-containing transition metal oxide is immersed in the reducing solution, the molar ratio (Na ions / Na-containing transition metal oxide) of the Na ions contained in the reducing solution to the Na-containing transition metal oxide immersed in the reducing solution may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more, or 2.0 or less, 1.5 or less, 1.0 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, or 0.2 or less. In particular, when the molar ratio (Na ion / Na-containing transition metal oxide) is 0.1 or more and 0.8 or less, a positive electrode active material having excellent performance is easily obtained. The molar ratio (electrophile / Na ion) of the electrophile and the Na ion contained in the reducing solution is not particularly limited, and may be, for example, 0.5 or more and 2.0 or less, 0.7 or more and 1.5 or less, or 0.9 or more and 1.1 or less.
[0021] In step S2, for example, the Na-containing transition metal oxide can be further doped with Na by simply contacting the Na-containing transition metal oxide with the above-mentioned reducing solution. The contact form between the reducing solution and the Na-containing transition metal oxide is not particularly limited. For example, the Na-containing transition metal oxide may be immersed in the reducing solution, or the reducing solution may be sprayed onto the Na-containing transition metal oxide. There is no particular limit to the temperature during contact, and the solution may be heated or not heated. The Na-containing transition metal oxide may be immersed in the reducing solution and then stirred. There is no particular limit to the time for which the Na-containing transition metal oxide is contacted with the reducing solution, and it may be appropriately determined according to the desired doping amount. The contact time may be, for example, 1 minute or more, 30 minutes or more, or 1 hour or more, and may be 48 hours or less, 40 hours or less, or 30 hours or less.
[0022] 2.Cathode active material As described above, a positive electrode active material having a P2 type structure (P2 type Na-containing transition metal oxide) can be produced through steps S1 and S2, which has a larger Na content and a higher capacity than conventional positive electrode active materials. The positive electrode active material obtained through steps S1 and S2 may have the following characteristics, for example.
[0023] 2.1 Crystal structure The positive electrode active material has at least a P2 type structure (belonging to space group P63mc). The positive electrode active material has a P2 type structure and may have a crystal structure other than the P2 type structure. Examples of the crystal structure other than the P2 type structure include various crystal structures (P3 type structure, etc.) formed when Na is desorbed from the P2 type structure. The positive electrode active material may have a P2 type structure as a main phase, or may have a crystal structure other than the P2 type structure as a main phase. The positive electrode active material may have a crystal structure that is a main phase that changes depending on the charge / discharge state.
[0024] 2.2 Chemical composition The positive electrode active material may contain at least one element selected from Mn, Ni, and Co, Na, and O as constituent elements. In particular, when the positive electrode active material contains at least Mn, at least one of Ni and Co, Na, and O as constituent elements, and especially when the positive electrode active material contains at least Na, Mn, Ni, Co, and O as constituent elements, it is easy to ensure higher performance. However, the positive electrode active material may, for example, release Na almost completely upon charging, and the molar concentration of Na may approach 0 to the limit. The positive electrode active material may also contain the above element M. The positive electrode active material may also contain other impurity elements.
[0025] The chemical composition of the positive electrode active material with the P2 structure is Na a Mn x-p Ni y-q Co z-r M p+q+r O 2(Here, 0.70 < a ≤ 1.40, x + y + z = 1, 0 ≤ p + q + r < 0.17, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), and it may be represented by this. In this chemical composition, a may be greater than 0.70, may be 0.80 or more, 0.90 or more, 1.00 or more, or greater than 1.00, and may be 1.40 or less, 1.35 or less, 1.30 or less, 1.25 or less, 1.20 or less, 1.15 or less, or 1.10 or less. For the compositions of x, y, z, p, q, r, and O, they may be the same as those exemplified as the chemical composition of the Na-containing transition metal oxide obtained in step S1, and the description thereof is omitted here.)
[0026] 2.3 Shape The positive electrode active material may be particulate. The positive electrode active material particles may be solid particles, may be hollow particles, or may have voids. The positive electrode active material particles may be primary particles or may be secondary particles aggregated from a plurality of primary particles. The average particle diameter (D50) of the positive electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Note that the average particle diameter D50 referred to in the present application is the particle diameter (median diameter) at the integrated value of 50% in the volume-based particle size distribution determined by the laser diffraction / scattering method.)
[0027] 2.4 Others The positive electrode active material may contain components resulting from the above-described manufacturing process as impurities. For example, the positive electrode active material may contain components derived from the reducing solution. Specifically, the positive electrode active material may contain an aromatic organic compound such as biphenyl. Further, the positive electrode active material may contain an ether compound such as tetrahydrofuran or dimethoxyethane.)
[0028] 3. Method for manufacturing a sodium ion battery The cathode active material produced as described above is used, for example, as a cathode active material for a sodium ion battery. The method for producing a sodium ion battery according to an embodiment may include, for example, as shown in FIG. 2, producing a cathode active material by the production method of the present disclosure, obtaining a cathode active material layer using the produced cathode active material, and obtaining a sodium ion battery using the cathode active material layer. In this way, the method for producing a sodium ion battery according to the present disclosure may be produced by the same method as in the past, except that after producing the cathode active material according to the present disclosure, a cathode active material layer is obtained using the cathode active material. For example, it is as follows. (1) The cathode active material of the present disclosure is dispersed in a solvent to obtain a cathode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The cathode layer slurry is then applied to the surface of a cathode current collector using a doctor blade or the like, and then dried to form a cathode active material layer on the surface of the cathode current collector, thereby forming a cathode. (2) The negative electrode active material and the like are dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is then applied to the surface of a negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to produce a sodium ion battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).
[0029] 4. Sodium-ion battery The technology of the present disclosure also has an aspect as a sodium ion battery. For example, as shown in FIG. 3, a sodium ion battery 100 according to one embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30, and is characterized in that the positive electrode active material layer 10 contains the positive electrode active material of the present disclosure. As shown in FIG. 3, the sodium ion battery 100 may include a positive electrode current collector 40 and a negative electrode current collector 50. In the sodium ion battery 100, the configuration other than the positive electrode active material is the same as that of a conventional battery, and may have, for example, the configuration described in Patent Document 1 (JP Patent Publication 2012-201588 A). EXAMPLES
[0030] As described above, one embodiment of the method for producing a positive electrode active material of the present disclosure has been described, but the method for producing a positive electrode active material of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the present disclosure. Below, the technology of the present disclosure will be described in more detail while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0031] 1. Preparation of Positive Electrode Active Material 1.1 Coprecipitation synthesis of transition metal sources MnSO 4 5H 2 O, NiSO 4 6H 2 O and CoSO 4 7H 2 The first solution was obtained by weighing out the desired composition ratio and dissolving it in distilled water to a concentration of 1.2 mol / L. 2 CO 3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain the second liquid. Next, 500 mL of each of the first and second liquids was dropped at a rate of about 4 mL / min into a reaction vessel containing 1000 mL of pure water in advance. After the dropwise addition, the mixture was stirred at a stirring speed of 150 rpm for 1 hour at room temperature. The precipitate was washed with pure water and subjected to solid-liquid separation using a centrifuge. The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then fine particles were removed by air classification to obtain mixed salt particles (transition metal source) containing Mn, Ni, and Co.
[0032] 1.2 Mixing transition metal source and Na source (Na coating) Na 2 CO 3 By stirring in distilled water until completely dissolved, Na 2 CO 3 An aqueous solution of Na 2 CO 3 The above mixed salt particles were mixed in an aqueous solution to prepare a slurry. 2 CO 3 After drying, the above mixed salt particles were 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 The resulting slurry was dried by spray drying. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 / min and spray air pressure of 0.3 MPa, the surface of the above mixed salt particles was sprayed with Na 2 CO 3 to obtain coated particles.
[0033] 1.3 Sintering of coated particles The coated particles were sintered in an electric furnace using an alumina crucible under an air atmosphere. Specifically, the coated particles were subjected to the "first heating step", "pre-firing step", "second heating step", "main firing step" and "furnace cooling step" as shown in Table 1 below, and then the sintered product was taken out of the electric furnace at 250°C and pulverized in a mortar in a dry atmosphere with a dew point of -30°C or less to obtain a Na-containing transition metal oxide having a P2 type structure.
[0034] [Table 1]
[0035] 1.4 Na-doped (Examples 1 and 2) Biphenyl was mixed and dissolved in tetrahydrofuran (THF) in a glove box (Ar atmosphere) to obtain a biphenyl solution at 1 mol / L. Metal Na was further added to the biphenyl solution in the same mole as biphenyl, and the solution was stirred for 2 hours to obtain a reduced solution containing 1 mol / L Na ions. The above-mentioned Na-containing transition metal oxide was added to the obtained reduced solution, immersed, and stirred for 24 hours. After stirring, the Na-containing transition metal oxide was washed with THF and subjected to solid-liquid separation by vacuum filtration. The obtained precipitate was dried overnight at 120°C to obtain a positive electrode active material (the above-mentioned Na-containing transition metal oxide further doped with Na). Here, the molar ratio (Na ion / Na-containing transition metal oxide) between the Na ions contained in the reduced solution and the Na-containing transition metal oxide immersed in the reduced solution was changed as shown in Table 2 below to obtain the positive electrode active materials of Examples 1 and 2.
[0036] 1.5 Comparative Example The Na-containing transition metal oxide was not doped, and was used as it was as the positive electrode active material after cooling outside the furnace and pulverization in a mortar.
[0037] 2. Identification of the chemical composition and crystal structure of the positive electrode active material The chemical composition of each of the positive electrode active materials of Examples 1 and 2 and the Comparative Example was determined by ICP analysis. X Mn 0.5 Ni 0.2 Co 0.3 O 2 That is, the composition ratio of the transition metals was the same, but the composition ratio of Na was different. In addition, X-ray diffraction measurements were performed on each of the positive electrode active materials of Examples 1 and 2 and Comparative Example to identify the crystal structure. FIG. 4 shows the respective X-ray diffraction patterns. As shown in FIG. 4, the positive electrode active materials of Examples 1 and 2 and Comparative Example all had a P2 type crystal structure.
[0038] 3. Coin Cell Fabrication The above positive electrode active material, acetylene black (AB) as a conductive material, and PVdF as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF was 85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode slurry. The positive electrode slurry was applied onto an Al foil and vacuum dried overnight at 120°C to obtain a positive electrode. The obtained positive electrode and an electrolyte solution (solvent: EC / DMC, electrolyte: NaPF 6 A coin cell (CR2032) was fabricated using a 1M lithium ion battery (1M in concentration) and a metallic Na foil as the negative electrode.
[0039] 4. Coin Cell Evaluation The coin cell was charged and discharged in a thermostatic chamber maintained at 25° C. at a voltage range of 1.5-4.5 V and a rate of 0.1 C (1 C=200 mA / g), and the initial charge capacity and initial discharge capacity were measured.
[0040] 5. Evaluation Results Table 2 below shows the "molar ratio (Na ion / Na-containing transition metal oxide) between the Na ion contained in the reducing solution and the Na-containing transition metal oxide immersed in the reducing solution" in the Na doping step for each of Examples 1 and 2 and the Comparative Example, and the amount of Na determined by ICP analysis (Na X Mn 0.5 Ni 0.2 Co 0.3 O 2 The figure shows the capacitance (X value) and the initial charge / discharge capacity of the coin cell.
[0041] [Table 2]
[0042] As shown in Table 2, the positive electrode active material according to the comparative example, which was not doped with Na after the main firing, had an X value below 0.70, whereas the positive electrode active materials according to the examples 1 and 2, which were further doped with Na in a step separate from the main firing, had an X value above 0.70. As a result, the coin cells according to the examples 1 and 2 had significantly higher initial charge capacity and initial discharge capacity than the coin cells according to the comparative example. That is, it was found that the capacity potential of a P2 type positive electrode active material can be brought out by further doping with Na after obtaining a Na-containing transition metal oxide having a P2 type structure.
[0043] In the above examples, the case where coated particles containing Na and transition metals are obtained through coprecipitation and spray drying is illustrated, but the preparation conditions of the precursor before the main firing are not limited to this. In addition, in the above examples, the case where coated particles and P2 type Na-containing transition metal oxides having a specific chemical composition are prepared and the Na-containing transition metal oxide is further doped with Na is illustrated, but the chemical composition of the P2 type positive electrode active material is not limited to this. In addition, in the above examples, the case where Na is doped using a specific reducing solution is illustrated, but the type of reducing solution is not limited to this. In addition, after the main firing, various conditions can be changed as long as Na can be further doped in a process separate from the main firing. [Explanation of symbols]
[0044] 10 Cathode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector 100 Sodium-ion battery
Claims
1. A method for producing a positive electrode active material, comprising: Obtaining a Na-containing transition metal oxide having a P2 type structure; and The Na-containing transition metal oxide is further doped with Na. A method for producing a positive electrode active material.
2. The method according to claim 1, by contacting the Na-containing transition metal oxide with a reducing solution containing Na ions, the Na-containing transition metal oxide is further doped with Na. Manufacturing method.
3. A method for manufacturing a sodium ion battery, comprising: Producing a positive electrode active material by the method according to claim 1 or 2; Obtaining a positive electrode active material layer using the produced positive electrode active material; and Obtaining a sodium ion battery using the positive electrode active material layer. How sodium-ion batteries are manufactured.
4. A positive electrode active material, It has a P2 type structure, Na a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0.70<a≦1.40, x+y+z=1, 0≦p+q+r<0.17, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Cathode active material.
5. A sodium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode active material according to claim 4. Sodium-ion battery.
Citation Information
Patent Citations
Positive electrode material for sodium secondary battery, method for producing the positive electrode material for sodium secondary battery, electrode for sodium secondary battery using the positive electrode material for sodium secondary battery, sodium secondary battery including the electrode for sodium secondary battery, and electrical device using the sodium secondary battery
JP2014229452A
O3 / P2 mixed-phase sodium-containing doped layered oxide materials
JP2021520333A
Positive electrode active material for sodium secondary battery
JP2023003666A
Complex metal oxide, positive electrode active material for sodium secondary battery, positive electrode for sodium secondary battery, and the sodium secondary battery
JP2012201588A