Curable composition for electrolyte gel, electrolyte gel, storage battery and electronic device

The curable composition for electrolyte gels, incorporating specific components, enhances ionic conductivity and flexibility, addressing the limitations of conventional electrolytes in lithium-ion batteries by eliminating organic solvents and improving safety and performance.

JP2024152468APending Publication Date: 2024-10-25KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066691
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional electrolyte gels in lithium-ion batteries suffer from inadequate ionic conductivity, high resistance, and flammability due to the use of organic solvents, and lack flexibility for impact resistance.

Method used

A curable composition comprising a liquid polymer with crosslinkable functional groups, phosphoric acid monoester or diester, a compound with hydroxyl, acidic, or sulfonyl groups and an ether bond, an initiator, and an electrolyte, which allows for high concentration dissolution of the electrolyte without organic solvents, resulting in a flexible and low-resistance electrolyte gel.

Benefits of technology

The composition achieves excellent ionic conductivity and flexibility, reducing the risk of flammability and enabling high-performance lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152468000001
    Figure 2024152468000001
  • Figure 2024152468000002
    Figure 2024152468000002
  • Figure 2024152468000003
    Figure 2024152468000003
Patent Text Reader

Abstract

To achieve a curable composition that yields an electrolyte gel with superior ionic conductivity.SOLUTION: A curable composition for electrolyte gel according to the present disclosure includes component (A): a crosslinkable functional group-containing liquid polymer, component (B): at least one of phosphoric monoester and phosphodiester, component (C): a compound containing a group selected from a hydroxy group, an acidic group, a sulfonyl group and an ether bond, with two or more oxygen atoms present in each molecule, component (D): an initiator, and component (E): an electrolyte,.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition for an electrolyte gel, an electrolyte gel, a storage battery, and an electronic device. [Background technology]

[0002] Batteries, such as lithium-ion batteries, are increasingly being used as energy storage devices in many applications, in particular due to their high energy density or specific energy and low self-discharge. For example, lithium-ion batteries are already used as batteries in automobiles (particularly as energy storage devices in electric vehicles), as storage devices in IoT devices such as laptops and smartphones, and as storage devices in stationary storage devices for domestic and industrial use.

[0003] Lithium-ion batteries contain an electrolyte that is placed in or between two distinct electrodes, an anode and a cathode, where electrochemical energy is stored in the battery by conversion of chemical energy into electrical energy.

[0004] Patent Document 1 discloses a polymer electrolyte including a polymer gel containing a non-aqueous solvent containing an electrolyte, the polymer gel including units derived from a specific monomer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-189166 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the above-mentioned conventional techniques have room for further improvement in terms of ion conductivity. An object of one aspect of the present invention is to provide a curable composition capable of obtaining an electrolyte gel having excellent ion conductivity, and to realize use of the same. [Means for solving the problem]

[0007] In order to solve the above problems, a curable composition for an electrolyte gel according to one embodiment of the present invention contains: component (A): a liquid polymer containing a crosslinkable functional group; component (B): at least one of a phosphoric acid monoester and a phosphoric acid diester; component (C): a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond, and containing two or more oxygen atoms in the molecule; component (D): an initiator; and component (E): an electrolyte. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide a curable composition capable of obtaining an electrolyte gel having excellent ion conductivity, and use of the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an example of an embodiment of the present invention will be described in detail, but the present invention is not limited thereto. Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more, B or less". In addition, all documents described in this specification are incorporated by reference in this specification.

[0010] 1. Curable composition for electrolyte gel The electrolyte gel curable composition according to one embodiment of the present invention contains a crosslinkable functional group-containing liquid polymer (A), a phosphoric acid monoester and / or phosphoric acid diester (B), a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond and containing two or more oxygen atoms in the molecule (C), an initiator (D), and an electrolyte (E). In this specification, the electrolyte gel curable composition means a curable composition for obtaining an electrolyte gel. Hereinafter, the electrolyte gel curable composition is also simply referred to as a curable composition. The electrolyte gel can be obtained by curing the curable composition. In this specification, "curing" means "gelling".

[0011] The polymer electrolyte as disclosed in Patent Document 1 does not have sufficiently high ionic conductivity compared to liquid electrolytes, and further improvement in ionic conductivity is required for application to electrolyte layers of lithium ion storage batteries and the like at a practical level.

[0012] In addition, in the conventional technology such as Patent Document 1, when preparing an electrolyte gel, it was necessary to add an organic solvent in order to ensure the ionic conductivity of the electrolyte. However, since the electrolyte gel contains an organic solvent, there was a concern that the electrolyte gel would catch fire if an ignition source was near the electrolyte gel. Furthermore, when an organic solvent was used to dissolve the electrolyte, it was difficult to dissolve and fill the electrolyte at a high concentration. As a result, the resistance value of the electrolyte gel was high, and it was therefore difficult to set the ionic conductivity to a high value.

[0013] The present inventors have newly discovered that the presence of components (A) and (B) allows the component (E) to be dissolved in a high concentration in the curable composition without using an organic solvent. This allows the resistance of the electrolyte gel to be reduced. Furthermore, it has been newly discovered that the presence of component (C) allows a cured product to be obtained with an ultra-low resistance close to that of a liquid electrolyte layer, which could not be obtained with components (A) and (B) alone. This allows the ionic conductivity of the electrolyte gel to be improved. Another advantage of component (B) is that it is flame retardant.

[0014] For example, when a composition containing an epoxy resin as a main component is polymerized to obtain a cured product, the resulting cured product is hard and has poor flexibility due to the large number of reaction sites. When the cured product is used as an electrolyte gel to be incorporated into a lithium ion battery or the like, it is preferable that the cured product has flexibility because it is resistant to impact. From this viewpoint, there is room for improvement in the conventional technology. In contrast, the curable composition contains component (A) having a crosslinkable functional group. Therefore, the number of reaction sites can be controlled, and the resulting cured product is rubber-like and flexible.

[0015] Furthermore, by containing the component (D), the curable composition can be cured at room temperature, by heating, or by UV curing.

[0016] [Component (A): Liquid polymer containing crosslinkable functional groups] The curable composition contains a crosslinkable functional group-containing liquid polymer as component (A). The main chain of component (A) is not particularly limited, and may be, for example, a vinyl polymer or a polyoxyalkylene polymer.

[0017] The (A) component may be a polymer containing an ether bond in the main chain or side chain. For example, the (A) component is preferably a polymer containing an ether bond in the side chain, and more preferably a vinyl polymer containing an ether bond in the side chain. It is speculated that the (A) component crosslinks while holding the (E) component by the ether bond, and therefore the inhibition of curing at room temperature by the (E) component can be suppressed. The curable composition exhibits good curability, and therefore the occurrence of bleeding on the surface of the cured product can also be suppressed. It is also speculated that the fact that the (A) component has an ether bond allows the (E) component to be highly loaded contributes to lowering the resistance value of the electrolyte gel.

[0018] As the vinyl monomer constituting the main chain of the vinyl polymer, various monomers can be used, but it is preferable to include a vinyl monomer having an ether bond.Specific examples of the vinyl monomer having an ether bond include methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 2-ethylcarbitoloxy (meth)acrylate, and phenoxyethyl (meth)acrylate.

[0019] It can also be said that the vinyl polymer preferably has a side chain containing an ether bond, and the side chain containing an ether bond is preferably at least one selected from the group consisting of a methoxypolyethylene glycol group, a methoxypropylene glycol group, a methoxytriethylene glycol group, a methoxyethyl group, an ethylcarbitol group, and a phenoxyethyl group.

[0020] Specific examples of other vinyl monomers include (meth)acrylic acid; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, Nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, γ-(methacryloyloxypropyl)trimethoxysilane, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, (meth)acrylic acid (Meth)acrylic acid ester monomers such as 2-trifluoromethylethyl, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate; styrene-based monomers such as styrene, vinyltoluene, α-methylstyrene, chlorostyrene, and styrenesulfonic acid and their salts; fluorine-containing vinyl monomers such as perfluoroethylene, perfluoropropylene, and vinylidene fluoride; silicon-containing vinyl monomers such as vinyltrimethoxysilane and vinyltriethoxysilane; maleic anhydride, maleic acid, and monoalkyl and dialkyl esters of maleic acid; fumaric acid, and monoalkyl and dialkyl esters of fumaric acid;Examples of the monomers include maleimide monomers such as maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide; nitrile group-containing vinyl monomers such as acrylonitrile and methacrylonitrile; amide group-containing vinyl monomers such as acrylamide and methacrylamide; vinyl esters such as vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate; alkenes such as ethylene and propylene; conjugated dienes such as butadiene and isoprene; vinyl chloride, vinylidene chloride, allyl chloride, and allyl alcohol.

[0021] These may be used alone or in combination. The (meth)acrylic acid herein refers to acrylic acid and / or methacrylic acid.

[0022] The main chain of the component (A) is preferably a (meth)acrylic polymer, since the product has excellent physical properties such as flexibility, viscosity, and elongation at low temperatures. That is, the main chain of the vinyl polymer is preferably produced by polymerizing mainly (meth)acrylic acid ester monomers, and more preferably produced by polymerizing mainly acrylic acid ester monomers. Here, "mainly" means that of the monomer units constituting the vinyl polymer, 50 mol % or more are (meth)acrylic acid ester monomers, and preferably 70 mol % or more are (meth)acrylic acid ester monomers.

[0023] Particularly preferred acrylic acid ester monomers include acrylic acid alkyl ester monomers, specifically ethyl acrylate, 2-methoxyethyl acrylate, stearyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, and 2-methoxybutyl acrylate. These preferred monomers may be copolymerized or block copolymerized with other monomers.

[0024] The molecular weight distribution of the vinyl polymer, i.e., the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC), is not particularly limited, but is preferably less than 1.8, more preferably 1.7 or less, even more preferably 1.6 or less, even more preferably 1.5 or less, particularly preferably 1.4 or less, and most preferably 1.3 or less. If the molecular weight distribution is too large, the viscosity at the same molecular weight between crosslinking points increases, and handling tends to become difficult. In this specification, the GPC measurement is performed using chloroform as the mobile phase and a polystyrene gel column, and the number average molecular weight and the like can be calculated in terms of polystyrene.

[0025] The number average molecular weight of the vinyl polymer is not particularly limited, but is preferably in the range of 500 to 1,000,000, more preferably 1,000 to 100,000, even more preferably 5,000 to 80,000, and even more preferably 8,000 to 50,000, as measured by GPC. If the molecular weight is too low, the viscosity is low and handling is easy, but the resulting cured product tends to have insufficient elongation and / or poor flexibility. On the other hand, if the molecular weight is too high, handling tends to be difficult.

[0026] The component (A) may be a polymer containing an ether bond in the main chain. Examples of the main chain of such a polymer include polyoxyalkylene polymers, such as polyacetal, polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers. Among these, it is preferable that the main chain of the component (A) is at least one selected from the group consisting of polyacetal, polyoxyethylene, and polyoxypropylene.

[0027] The polyoxyalkylene polymer is represented by the following general formula (1): -R 3 -O- (1) (In the formula, R3 is a linear or branched alkylene group having 1 to 14 carbon atoms. 3 is preferably a linear or branched alkylene group having 1 to 14 carbon atoms, more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. The repeating unit represented by the general formula (1) is not particularly limited, and examples thereof include

[0028] [ka]

[0029] The main chain skeleton of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units. In particular, those composed of a polymer mainly composed of a propylene oxide polymer are preferred because they are amorphous and have a relatively low viscosity.

[0030] The polyoxyalkylene polymer may be linear or branched, and its number average molecular weight, calculated as polystyrene by GPC, is 3,000 to 100,000, more preferably 3,000 to 50,000, and particularly preferably 3,000 to 30,000. If the number average molecular weight is less than 3,000, the cured product obtained from the polyoxyalkylene polymer tends to have poor elasticity, while if it exceeds 100,000, the viscosity becomes high, which tends to be poor in terms of workability.

[0031] The molecular weight distribution of the polyoxyalkylene polymer is not particularly limited, but is preferably narrow, preferably less than 2.00, more preferably 1.60 or less, and particularly preferably 1.40 or less. If the molecular weight distribution is large, the viscosity increases, which tends to deteriorate the workability.

[0032] From the viewpoint of flexibility of the obtained cured product, the lower limit of the content of the (A) component in 100% by weight of the curable composition is preferably 50% by weight or more, more preferably 55% by weight or more. The upper limit of the content of the (A) component in 100% by weight of the curable composition is less than 100% by weight, and from the viewpoint of ion conductivity, it is preferably 50% by weight or less, more preferably 30% by weight or less.

[0033] The polymerization ratio of the monomer having an ether bond in the component (A) is preferably 25 mol% or more. In order to dissolve the electrolyte at a high concentration in the curable composition without using a solvent, the ratio of the vinyl monomer having an ether bond in the vinyl polymer is preferably more than 30 mol%, more preferably 40 mol% or more and 100% or less, and even more preferably 50 mol% or more and 99% mol% or less.

[0034] <Synthesis method of component (A)> The vinyl polymer can be obtained by various polymerization methods. The polymerization method is not particularly limited, but the radical polymerization method is preferred from the viewpoints of versatility of monomers, ease of control, etc., and among radical polymerization methods, the controlled radical polymerization method is more preferred. The controlled radical polymerization method can be classified into a "chain transfer agent method" and a "living radical polymerization method". The living radical polymerization method is more preferred because it is easy to control the molecular weight and molecular weight distribution of the obtained vinyl polymer, and the atom transfer radical polymerization method is particularly preferred because of the availability of raw materials and the ease of introducing functional groups into the polymer terminals. For each of these polymerization methods, for example, the descriptions in JP-A-2005-232419 and JP-A-2006-291073 can be referred to.

[0035] The synthesis method of the polyoxyalkylene polymer is not particularly limited, and examples thereof include a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organoaluminum compound with porphyrin as disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst as disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. No. 3,278,457, U.S. Pat. No. 3,278,458, U.S. Pat. No. 3,278,459, U.S. Pat. No. 3,427,256, U.S. Pat. No. 3,427,334, and U.S. Pat. No. 3,427,335, and the like, a polymerization method using a catalyst made of a polyphosphazene salt as disclosed in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound as disclosed in JP-A-11060722.

[0036] <Crosslinkable functional group> The crosslinkable functional group contained in component (A) is not particularly limited, but from the viewpoints of excellent storage stability and properties of the cured product after crosslinking, it is preferably at least one type selected from the group consisting of a radical crosslinkable functional group, an epoxy group, and a hydrolyzable silyl group.

[0037] When rubber-like properties are particularly required for the cured product obtained by curing the curable composition, it is preferable that at least one of the crosslinkable functional groups is located at the end of the molecular chain, since the molecular weight between crosslinking points, which has a large effect on rubber elasticity, can be large. More preferably, the (A) component has all of the crosslinkable functional groups at the end of the molecular chain.

[0038] (Radical crosslinking functional group) The radical crosslinkable functional group is not particularly limited, and examples thereof include vinyl groups and (meth)acryloyl groups. When the crosslinkable functional group of the (A) component is a radical crosslinkable functional group, the lower limit of the number of radical crosslinkable functional groups contained in the (A) component in the molecule is preferably 1.0 or more on average per molecule, more preferably 1.2 or more, and even more preferably 1.4 or more. The upper limit of the number of radical crosslinkable functional groups is preferably 2 or less on average per molecule. If the number of radical crosslinkable functional groups is within the above range, the (A) components are sufficiently crosslinked with each other by the catalyst and the initiator, and a cured product with sufficient strength is obtained.

[0039] In one embodiment, the (meth)acryloyl group has a structure represented by the following general formula (2). -OC(O)C(R 5 )=CH2(2) In general formula (2), R 5 R is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. The hydrocarbon group may be optionally substituted with one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, sulfur atoms, fluorine atoms, chlorine atoms, bromine atoms and iodine atoms. 5 Specific examples of the alkyl group include H, CH3, CH2CH3, (CH2) n Examples of the aryl group include CH3 (n is an integer from 2 to 19), C6H5, CH2OH, and CN. From the viewpoint of the reactivity of the component (A), R 5 is preferably H or CH3.

[0040] Examples of the method for introducing a (meth)acryloyl group into a vinyl polymer include the method described in paragraphs

[0081] to

[0090] of Japanese Patent No. 5536383. Methods for introducing a (meth)acryloyl group into a polyoxyalkylene polymer are not particularly limited, but examples of commonly known methods include a method of reacting a hydroxyl-terminated polyoxyalkylene polymer with a polyisocyanate and a hydroxyl-containing (meth)acrylic monomer in the presence of a catalyst, the method described in paragraphs

[0019] to

[0064] of Japanese Patent Publication No. 2011-63767, the method described in paragraphs

[0029] to

[0045] of Japanese Patent Publication No. 2012-17430, and the method described in paragraphs

[0031] to

[0068] of Japanese Patent Publication No. 2014-237734.

[0041] (epoxy group) In one embodiment, the epoxy group is not particularly limited, but examples thereof include glycidyl group, glycidyl ether group, 3,4-epoxycyclohexyl group, oxetane group, aminoglycidyl group, and phenoxyglycidyl group. When the crosslinkable functional group of component (A) is an epoxy group, the lower limit of the number of epoxy groups contained in the molecule of component (A) is preferably 1.0 or more on average per molecule, more preferably 1.4 or more, and even more preferably 2.0 or more. The upper limit of the number of epoxy groups is preferably 4.0 or less on average per molecule.

[0042] (Hydrolyzable silyl group) In one embodiment, the hydrolyzable silyl group includes a group represented by general formula (3). -[Si(R 1 ) 2-b (Y) b O] m -Si(R 2 ) 3-a (Y) a (3) In the formula, R 1 , R 2each represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, or a triorganosiloxy group represented by (R')3SiO- (R' is a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the three R's may be the same or different), and R 1 or R 2 When two or more are present, they may be the same or different. Y represents a hydroxyl group or a hydrolyzable group, and when two or more Y are present, they may be the same or different. a represents 0, 1, 2, or 3, and b represents 0, 1, or 2. m is an integer of 0 to 19, provided that a+mb≧1 is satisfied.

[0043] Examples of hydrolyzable groups include commonly used groups such as hydrogen atom, alkoxy group, acyloxy group, ketoximate group, amino group, amide group, aminooxy group, mercapto group, and alkenyloxy group. Among these, alkoxy group, amide group, and aminooxy group are preferred, and alkoxy group is particularly preferred because it is mildly hydrolyzable and easy to handle. Among alkoxy groups, the smaller the number of carbon atoms, the higher the reactivity. In other words, the reactivity decreases in the order of methoxy group > ethoxy group > propoxy group, and these can be selected according to the purpose and application.

[0044] The hydrolyzable groups or hydroxyl groups can be bonded to one silicon atom in the range of 1 to 3, and (a+Σb) is preferably in the range of 1 to 5. When two or more hydrolyzable groups or hydroxyl groups are bonded to the hydrolyzable silyl group, they may be the same or different. The number of silicon atoms forming the hydrolyzable silyl group is one or more, but in the case of silicon atoms linked by siloxane bonds, etc., it is preferable that the number is 20 or less. In particular, the hydrolyzable silyl group represented by the general formula (4) is preferable in terms of easy availability. -Si(R 2 ) 3-a (Y) a (4) (In the formula, R 2and Y is the same as above, and a is an integer of 1 to 3. Although there are no particular limitations, it is preferable that a is 2 or more in order to provide good curability and good physical properties of the cured product.

[0045] As the vinyl polymer having such hydrolyzable silyl group, a polymer having a hydrolyzable silyl group, in which two hydrolyzable groups are bonded to one silicon atom, is often used. However, when used at low temperatures, particularly when a very fast curing speed is required, the curing speed is not sufficient, and when flexibility after curing is required, the crosslinking density must be reduced, and therefore, stickiness (surface tack) may occur due to insufficient crosslinking density. In such a case, it is preferable to use one in which a is 3 (for example, a trimethoxy functional group).

[0046] In addition, those where a is 3 (e.g., trimethoxy functional group) cure faster than those where a is 2 (e.g., dimethoxy functional group), but in terms of storage stability and mechanical properties (elongation, etc.), those where a is 2 may be superior. In order to balance the cure properties and physical properties, those where a is 2 (e.g., dimethoxy functional group) and those where a is 3 (e.g., trimethoxy functional group) may be used in combination.

[0047] For example, when Y is the same, the more a, the higher the reactivity of Y, so by selecting Y and a, it is possible to control the curability and the mechanical properties of the cured product, and can be selected according to the purpose and use. In addition, when a is 1, it can be used as a chain extender by mixing with a polymer having a hydrolyzable silyl group, specifically at least one polymer selected from polysiloxane, polyoxypropylene, and polyisobutylene. It is possible to obtain a composition that has low viscosity before curing and high elongation at break, low bleeding, and low surface contamination after curing.

[0048] The number of hydrolyzable silyl groups in component (A) is not particularly limited, but from the viewpoint of the curability of the composition and the physical properties of the cured product, it is preferable for the molecule to have an average of at least 1, more preferably from 1.1 to 4.0, and even more preferably from 1.2 to 3.5.

[0049] A known method can be used to introduce a hydrolyzable silyl group into the component (A). For example, the method described in paragraphs

[0083] to

[0117] of JP-A-2007-302749 can be mentioned. Methods for producing vinyl polymers having a hydrolyzable silyl group at the molecular chain end, particularly (meth)acrylic polymers, are disclosed in JP-B-3-14068, JP-B-4-55444, JP-A-6-211922, etc. In addition, the method for introducing an alkoxysilyl group into an oxyalkylene polymer obtained by using a composite metal cyanide complex catalyst described in JP-A-3-72527, and the method for introducing an alkoxysilyl group into an oxyalkylene polymer obtained by using a polyphosphazene salt and active hydrogen as catalysts described in JP-A-11-60723 can also be referred to.

[0050] (Other resins) The component (A) may be used alone or in combination with other resins.

[0051] [Component (B): phosphoric acid monoester and phosphoric acid diester] The curable composition contains at least one of a phosphoric acid monoester and a phosphoric acid diester as component (B), which allows component (E) to be dissolved in the curable composition and ensures the ionic conductivity of the resulting electrolyte gel.

[0052] <Phosphate monoester> Examples of the phosphoric acid monoester include monomethyl phosphate, monobutyl phosphate, mono 2-ethylhexyl phosphate, monoisodecyl phosphate, monobutoxyethyl acid phosphate, monoisotridecyl acid phosphate, monooleyl acid phosphate, monoethylene glycol acid phosphate, monophenyl phosphate, and monobenzyl phosphate.

[0053] <Phosphate diester> Examples of the phosphoric acid diester include dimethyl phosphate, dibutyl phosphate, di-2-ethylhexyl phosphate, diisodecyl phosphate, dibutoxyethyl acid phosphate, diisotridecyl acid phosphate, dioleyl acid phosphate, diethylene glycol acid phosphate, diphenyl phosphate, and dibenzyl phosphate.

[0054] The curable composition may contain at least a phosphoric acid monoester or a phosphoric acid diester, and may or may not further contain phosphoric acid and / or a phosphoric acid triester.

[0055] Specific examples of the phosphoric acid and / or phosphoric acid triester include phosphoric anhydride, tributyl phosphate, tris(2-ethylhexyl) phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, 2-ethylhexyl diphenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, tris(chloropropyl) phosphate, and the like.

[0056] The curable composition may contain a mixture containing at least one of a phosphoric acid monoester and a phosphoric acid diester. That is, a mixture containing at least one of a phosphoric acid monoester and a phosphoric acid diester may be used as a supply source of at least one of a phosphoric acid monoester and a phosphoric acid diester. In this specification, a mixture containing at least one of a phosphoric acid monoester and a phosphoric acid diester means a mixture that may contain phosphoric acid and a phosphoric acid triester in addition to at least one of a phosphoric acid monoester and a phosphoric acid diester. Examples of such a mixture include methyl acid phosphate, butyl acid phosphate, 2-ethylhexyl acid phosphate, isodecyl acid phosphate, and the like. Alternatively, although a phosphoric acid diester is listed as the main component, a commercially available product that may also contain phosphoric acid and / or a phosphoric acid ester other than a phosphoric acid diester may also be used. The content of the phosphoric acid monoester and the phosphoric acid diester in 100% by weight of such a mixture may be, for example, 5% by weight or more, 30% by weight or more, or 50% by weight or more.

[0057] From the viewpoint of coatability, the content of the (B) component in the curable composition is preferably 5 to 1000 parts by weight, more preferably 10 to 500 parts by weight, and even more preferably 20 to 400 parts by weight, relative to 100 parts by weight of the (A) component.

[0058] [Component (C): a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond, and containing two or more oxygen atoms in the molecule] The curable composition contains component (C): a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond, and containing two or more oxygen atoms in the molecule. In this specification, the term "compound having two or more oxygen atoms in the molecule" refers to a compound containing two or more oxygen atoms, including the oxygen atoms contained in the "group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond" of the compound. It is presumed that component (C) contributes to improving ion conductivity by coordinating or solvating with the cation derived from component (E) due to the two or more oxygen atoms. Component (C) is preferably liquid at room temperature (23°C) in order to improve ion conductivity. In this specification, component (C) is a compound different from components (A), (B), (D), and (E).

[0059] <Compounds containing a hydroxyl group> Examples of compounds having a hydroxyl group include glycols and triols, specifically ethylene glycol, propylene glycol, diethylene glycol, and glycerin.

[0060] <Compounds having an acidic group> The compound having an acidic group is not particularly limited, and examples thereof include a compound having a carboxyl group, a compound having a sulfonic acid group, nitric acid, nitrous acid, phosphoric acid, etc. Specific examples of the compound having a carboxyl group include carboxylic acids such as formic acid, oxalic acid, acetic acid, propynoic acid, butyric acid, hexanoic acid, octylic acid, 2-ethylhexanoic acid, decanoic acid, and neodecanoic acid, their anhydrides, 4-methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, glyceryl bis(anhydrotrimellitate) monoacetate, trimellitic anhydride (1,2,4-benzenetricarboxylic acid 1,2-anhydride), methylbicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, octenylsuccinic anhydride, and dodecenylsuccinic anhydride. Examples of compounds having a sulfonic acid group include sulfuric acid, dimethyl sulfate, chlorosulfonic acid, and alkylbenzenesulfonic acid.

[0061] <Compounds having a sulfonyl group> Examples of compounds having a sulfonyl group include dimethyl sulfone, ethyl phenyl sulfone, diethyl sulfone, diphenyl sulfone, sulfolane, 2-methyl sulfolane, 3-methyl sulfolane, 4-methyl sulfolane, 2,4-dimethyl sulfolane, 3,4-dibromosulfolane, 3,3,4,4-tetrachlorosulfolane, sulfolene, and bisphenol S.

[0062] <Compounds having ether bonds> Examples of compounds having an ether bond include glyme (monoglyme, diglyme, triglyme, tetraglyme), ethylene glycol monobutyl ether, ethylene glycol butyl ether acetate, diethylene glycol monobutyl ether, and diethylene glycol butyl ether acetate.

[0063] From the viewpoint of availability, it is preferable that the component (C) is at least one selected from the group consisting of glycols, triols, phosphoric acids, carboxylic acids, and glymes. The content of the component (C) is preferably 0.01 to 1000 parts by weight, more preferably 0.05 to 500 parts by weight, and even more preferably 0.1 to 300 parts by weight, relative to 100 parts by weight of the component (A).

[0064] [Component (D): initiator] The curable composition includes an initiator as component (D). The component (D) is not particularly limited, and a radical initiator and / or a redox initiator is preferable from the viewpoint of curability. In one embodiment, the component (D) is a radical initiator. Examples of the radical initiator include a thermal radical initiator and a photoradical initiator.

[0065] Examples of the thermal radical initiator include organic peroxides. Specific examples thereof include hydroperoxides, dialkyl peroxides, peroxycarboxylic acids, peroxy esters, diacyl peroxides, peroxy carbonates, ketone peroxides, and peroxy ketals. From the viewpoint of curability and storage stability, peroxy esters, peroxy carbonates, ketone peroxides, and peroxy ketals are preferred, and peroxy esters and peroxy carbonates are particularly preferred. For example, examples of peroxy esters include t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, and t-butylperoxybenzoate.

[0066] As the thermal radical initiator, azo-based initiators can be used in addition to organic peroxides, specific examples of which include azobisisobutyronitrile and dimethylazobisisobutyrate.

[0067] From the viewpoints of curability and storage stability, the content of the organic peroxide component in the curable composition is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 15 parts by weight, and even more preferably 1 to 10 parts by weight, relative to 100 parts by weight of component (A).

[0068] When the (D) component is made to function as an oxidation-reduction initiator, it is necessary to use a reducing agent in addition to the organic peroxide. The reducing agent type is not particularly limited, and a normal reducing agent can be used. Specific examples of the reducing agent include sulfinic acid, organic amines, transition metal salts, and the like. Examples of the organic amine include azo compounds such as para-toluidine (p-methylaniline); azoisobutyric acid dinitrile; α-aminosulfones such as bis-(tolylsulfonemethyl)amine, bis-(tolylsulfonemethyl)ethylamine, and bis-(tolylsulfonemethyl)-benzylamine; tertiary amines such as diisopropyl-p-toluidine, dimethylaniline, and dimethyl-p-toluidine; amine-aldehyde condensation products, for example, condensation products of primary amines such as aniline or butylamine with aliphatic aldehydes such as butylaldehyde; and thiourea derivatives such as 2-mercaptobenzimidazole, methylthiourea, dibutylthiourea, tetramethylthiourea, and ethylenethiourea. Examples of transition metal salts include cobalt naphthenate, copper naphthenate, and vanadyl acetylacetonate. Among these, organic amines and transition metal salts are preferred from the viewpoint of reactivity, and para-toluidine and vanadyl acetylacetonate are more preferred. In particular, organic amines are preferred from the viewpoint of their influence on curability, storage stability, and ion conductivity.

[0069] When a redox initiator is used as the component (D), from the viewpoints of curability and storage stability, the content of the reducing agent in the curable composition is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, and even more preferably 0.1 to 5 parts by weight, relative to 100 parts by weight of the component (A).

[0070] Examples of photoradical initiators include acetophenone, propiophenone, benzophenone, xanthol, fluorene, benzaldehyde, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4-methylacetophenone, 3-pentylacetophenone, 2,2-diethoxyacetophenone, 4-methoxyacetophenone, 3-bromoacetophenone, 4-allylacetophenone, p-diacetylbenzene, 3-methoxybenzophenone, 4-methylbenzophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 4-chloro-4'-benzylbenzophenone, and 3-chloroxanthones. , 3,9-dichloroxanthone, 3-chloro-8-nonylxanthone, benzoyl, benzoin methyl ether, benzoin butyl ether, bis(4-dimethylaminophenyl)ketone, benzyl methoxyketal, 2-chlorothioxanthone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1.

[0071] Further examples of the photoradical initiator include acylphosphine oxide-based photopolymerization initiators. Acylphosphine oxide-based photopolymerization initiators are preferred because they have excellent deep curing properties when irradiated with UV light. Specific examples of acylphosphine oxide-based photopolymerization initiators include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, bis(2,6-dimethylbenzoyl)-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-isobutylphosphine oxide, bis(2,6-dimethoxybenzoyl)-isobutylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-phenylphosphine oxide. Among these, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide are preferred.

[0072] Among the above-mentioned photoradical initiators, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide are preferred due to their high reactivity. In one embodiment, the curable composition contains both an acylphosphine oxide and a phenyl ketone compound.

[0073] From the viewpoints of curability and storage stability, the content of the photoradical initiator in the curable composition is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 15 parts by weight, and even more preferably 0.1 to 10 parts by weight, relative to 100 parts by weight of the (A) component.

[0074] [(E) Component: Electrolyte] The curable composition includes an electrolyte as component (E). Component (E) is not particularly limited and may be a normal electrolyte. Component (E) may be an electron pair compound of a fluorine atom-containing anion and a lithium cation. There is no particular limitation on the electron pair compound of a fluorine atom-containing anion and a lithium cation, and specific examples thereof include lithium hexafluorophosphate, LiPF3(CF2CF3)3, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(perfluoroethanesulfonyl)imide, lithium (fluorosulfonyl)(nonafluorobutanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium tris(trifluoromethanesulfonyl)methide, lithium bis(oxalato)borate, and lithium difluoro(oxalato)borate. Among these, lithium hexafluorophosphate and lithium bis(trifluoromethanesulfonyl)imide are preferred in terms of stability and ionic conductivity. Other examples of the component (E) that can be used include 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, N-(2-methoxyethyl)-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, and methyltrioctylammonium bis(trifluoromethylsulfonyl)imide.

[0075] From the viewpoints of the viscosity and ion conductivity of the curable composition, the content of the (E) component in the curable composition is preferably 10 to 1,000 parts by weight, more preferably 50 to 800 parts by weight, and even more preferably 100 to 700 parts by weight, relative to 100 parts by weight of the (A) component.

[0076] As described above, the curable composition can dissolve the component (E) at a high concentration. The content of the component (E) in 100% by weight of the curable composition may be 20% by weight or more, 30% by weight or more, 40% by weight or more, or 50% by weight or more.

[0077] [Component (F): radical reactive monomer] The curable composition may further contain a radically reactive monomer as component (F) from the viewpoints of viscosity adjustment, adjustment of the mechanical properties of the cured product, compatibility with electrolytes, etc. Component (F) is not particularly limited, but specific examples thereof include (meth)acrylic acid; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl ...propyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate, isopropyl (meth)acrylate ) 2-ethylhexyl acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, stearyl (meth)acrylate, glyceryl (meth)acrylate (meth)acrylic acid ester monomers such as dimethylsilyl, 2-aminoethyl (meth)acrylate, phenoxyethyl (meth)acrylate, γ-(methacryloyloxypropyl)trimethoxysilane, ethylene oxide adducts of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate; styrene monomers such as styrene, vinyltoluene, α-methylstyrene, chlorostyrene, and styrenesulfonic acid and its salts;Fluorine-containing vinyl monomers such as perfluoroethylene, perfluoropropylene, and vinylidene fluoride; silicon-containing vinyl monomers such as vinyltrimethoxysilane and vinyltriethoxysilane; maleic anhydride, maleic acid, monoalkyl esters and dialkyl esters of maleic acid; fumaric acid, monoalkyl esters and dialkyl esters of fumaric acid; maleimide monomers such as maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide; nitriles such as acrylonitrile and methacrylonitrile. amido group-containing vinyl monomers such as acrylamide, amino monomers, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, acrylmorpholine, methacrylamide, and other amide group-containing vinyl monomers, vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, vinyl cinnamate, and other vinyl esters, ethylene, propylene, and other alkenes, butadiene, isoprene, and other conjugated dienes, vinyl chloride, vinylidene chloride, allyl chloride, allyl alcohol, (2-oxo-1,3-dioxolan-4-yl)methyl (meth)acrylate, vinyl ethylene carbonate, and polyethylene glycol monoacrylate. In terms of the viscosity of the curable composition, solubility in the electrolyte, and the like, 4-hydroxybutyl (meth)acrylate (i.e., 4-hydroxybutyl (meth)acrylate), acrylic morpholine, allyl alcohol, (2-oxo-1,3-dioxolan-4-yl)methyl (meth)acrylate, and vinyl ethylene carbonate are preferred.

[0078] From the viewpoints of the viscosity and curability of the curable composition, and the flexibility of the cured product, the content of the (F) component in the curable composition is preferably 1 to 100 parts by weight, more preferably 2 to 80 parts by weight, and even more preferably 3 to 70 parts by weight, relative to 100 parts by weight of the (A) component.

[0079] [Other ingredients] The curable composition may contain other components in addition to the components (A), (B), (C), (D), and (E). The other components may be used alone or in combination of two or more. Examples of the other components are described below.

[0080] <Leveling agent> The curable composition may contain a leveling agent to adjust the surface unevenness when cured. Examples of the leveling agent include fluorine-based, silicone-based, acrylic-based, ether-based, and ester-based leveling agents.

[0081] <Antifoaming agent> The curable composition may contain an antifoaming agent to prevent the generation of bubbles. Preferred examples include acrylic, silicone, or fluorine-based antifoaming agents.

[0082] <Adhesion promoter> The curable composition may contain an adhesion promoter to improve adhesion to a substrate. As the adhesion promoter, a crosslinkable silyl group-containing compound or a vinyl monomer having a polar group is preferable, and a silane coupling agent or a vinyl monomer having an acidic group is more preferable.

[0083] As the silane coupling agent, for example, a silane coupling agent having both a functional group having atoms other than carbon and hydrogen atoms in the molecule and a crosslinkable silyl group can be used. Examples of the functional group having atoms other than carbon and hydrogen atoms include an epoxy group, an isocyanate group, an isocyanurate group, a carbamate group, an amino group, a mercapto group, a carboxyl group, a halogeno group, and a (meth)acrylic group.

[0084] <Filling agent> The curable composition may contain a filler to ensure a certain strength. The filler is not particularly limited, and silica other than fumed silica (e.g., crystalline silica, fused silica, hydrated silicic acid), dolomite, carbon black, titanium oxide, active zinc oxide, etc. are preferred from the viewpoint of improving the filling rate with a small amount. In particular, when it is desired to obtain a cured product with high strength using these fillers, it is preferable to mainly use at least one filler selected from crystalline silica, fused silica, hydrated silicic acid, carbon black, active zinc oxide, etc.

[0085] <Plasticizer> The curable composition may contain a plasticizer to adjust the viscosity, slump property, or mechanical properties such as hardness, tensile strength, or elongation when cured. Examples of the plasticizer include phthalate compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate (e.g., EASTMAN168 (manufactured by EASTMAN CHEMICAL)); 1,2-cyclohexanedicarboxylic acid diisononyl ester (e.g., Hexamol non-phthalate ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and tributyl acetyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters (Mesamoll (LANXESS)); phosphate ester compounds such as tricresyl phosphate and tributyl phosphate; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; epoxidized soybean oil, and epoxy plasticizers such as epoxy benzyl stearate.

[0086] [Method of producing curable composition] In the method for producing the curable composition, it is preferable to knead each component as follows. First, the (E) component is mixed with the (B) and (C) components to obtain a uniform electrolyte solution, and then the (A) component is added and further mixed and stirred. Finally, the (D) component is added and further mixed and stirred. The above can be performed at room temperature, but it is preferable to perform the above for a short time while heating in order to suppress the inclusion of moisture. The specific heating temperature is 50°C or more and 300°C or less, preferably 60°C or more and 200°C or less, and more preferably 70°C or more and 150°C or less.

[0087] The apparatus used for kneading includes a stirring and defoaming apparatus such as a triple roll mill, a planetary mixer, etc. The above-mentioned apparatuses may be used alone or in combination of two or more kinds.

[0088] 2. Electrolyte Gel The electrolyte gel according to one embodiment of the present invention is obtained by curing the above-mentioned curable composition. That is, the electrolyte gel contains the above-mentioned components (A) to (E), and can optionally contain the component (F) and other components. The electrolyte gel may also be called a gel electrolyte, a polymer electrolyte, or an electrolyte layer gel.

[0089] Methods for curing the curable composition include light irradiation, heating, and contact with moisture. Light rays and electron beams can be used for curing by light irradiation. Examples of sources for light rays and / or electron beams include high-pressure mercury lamps, low-pressure mercury lamps, electron beam irradiation devices, halogen lamps, light-emitting diodes, semiconductor lasers, and metal halides. The temperature during curing by light irradiation is preferably 0 to 150°C, more preferably 5 to 120°C. The temperature during curing by heating is preferably 50 to 150°C, more preferably 70 to 100°C. The relative humidity during curing by contact with moisture is preferably 5 to 95%, more preferably 10 to 80%.

[0090] [3. Storage Batteries and Electronic Devices] An embodiment of the present invention also includes a storage battery comprising the above-mentioned electrolyte gel. The storage battery may comprise an electrolyte gel between the positive electrode and the negative electrode. The storage battery may or may not comprise a separator between the positive electrode and the negative electrode in addition to the electrolyte gel. Examples of such storage batteries include lithium ion storage batteries, nickel metal hydride batteries, and NAS batteries.

[0091] An embodiment of the present invention also includes an electronic device comprising the above-mentioned electrolyte gel. Such electronic devices include a light control panel, a dye-sensitized solar cell, a sensor, an actuator, and a photoelectron device.

[0092] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0093] An embodiment of the present invention may include the following features. <1> A curable composition for an electrolyte gel, comprising: component (A): a liquid polymer containing a crosslinkable functional group; component (B): at least one of a phosphoric acid monoester and a phosphoric acid diester; component (C): a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond, and containing two or more oxygen atoms in the molecule; component (D): an initiator; and component (E): an electrolyte. <2> The component (A) is a polymer containing an ether bond in the main chain or side chain. <1> The curable composition for electrolyte gel according to claim 1. <3> the component (A) is a polymer containing an ether bond in a side chain, and the side chain containing an ether bond in the component (A) is at least one selected from the group consisting of a methoxypolyethylene glycol group, a methoxypropylene glycol group, a methoxytriethylene glycol group, a methoxyethyl group, an ethylcarbitol group, and a phenoxyethyl group; <2> The curable composition for electrolyte gel according to claim 1. <4> The component (A) is a polymer containing an ether bond in the main chain. <2> The curable composition for electrolyte gel according to claim 1. <5> The main chain of the component (A) is at least one selected from the group consisting of polyacetal, polyoxyethylene, and polyoxypropylene. <4> The curable composition for electrolyte gel according to claim 1. <6> The main chain of the component (A) is a (meth)acrylic polymer. <1> ~ <3> 13. The curable composition for an electrolyte gel according to claim 12, <7> The polymerization ratio of the monomer having an ether bond in the component (A) is 25 mol % or more. <1> ~ <6> 13. The curable composition for an electrolyte gel according to claim 12, <8> The crosslinkable functional group in the component (A) is at least one selected from the group consisting of a radical crosslinkable functional group, an epoxy group, and a hydrolyzable silyl group. <1> ~ <7> 13. The curable composition for an electrolyte gel according to claim 12, <9> The component (C) is at least one selected from the group consisting of glycols, triols, phosphoric acids, carboxylic acids, and glymes. <1> ~ <8> 13. The curable composition for an electrolyte gel according to claim 12, <10> The component (D) is a radical initiator. <1> ~ <9> 13. The curable composition for an electrolyte gel according to claim 12, <11> The component (E) is an electron pair compound of a fluorine atom-containing anion and a lithium cation. <1> ~ <10> 13. The curable composition for an electrolyte gel according to claim 12, <12> The content of the (E) component in 100% by weight of the curable composition for electrolyte gel is 20% by weight or more. <1> ~ <11> 13. The curable composition for an electrolyte gel according to claim 12, <13> <1> ~ <12> 2. An electrolyte gel obtained by curing the curable composition for an electrolyte gel according to claim 1. <14> <13> A storage battery comprising the electrolyte gel according to claim 1. <15> <13> An electronic device comprising the electrolyte gel according to claim 1. EXAMPLES

[0094] The present invention will be described in more detail below with reference to examples, but is not limited to these examples. In the following, unless otherwise specified, "%" refers to "% by weight."

[0095] [Evaluation method] [UV curability] The state of the obtained cured sheet was observed as follows. - Shape retention of the cured sheet - Presence or absence of bleeding on the surface of the cured sheet [Resistance and conductivity of hardened product] The surface resistivity, specific volume resistivity, and electrical conductivity of the obtained cured sheet were measured with a four-terminal probe using a low resistance resistivity meter (Lоresta-GP MCP-T610, manufactured by Nitto Seiko Analytech Co., Ltd.).

[0096] [Flexibility of the cured product] The rubber hardness of the cured product sheet was measured under a load of 1 kg using a type E durometer according to the test specified in JIS K 6253-3.

[0097] [Conductivity by impedance measurement] The impedance of the obtained cured sheet was measured using a VMP-300 (multipotentiostat / galvanostat, manufactured by Bio-Logic Science Instruments) and the electrical conductivity was calculated. 2 The thickness was calculated as 130 μm.

[0098] [Electrolyte gel for lithium-ion batteries] [Materials used in the Examples and Comparative Examples] Ingredient (A) RC-P(MEA) (Radical curing telechelic polyacrylate with two radical crosslinking functional groups at the ends (i.e. one at each end) and a main chain structure consisting solely of 2-methoxyethyl acrylate, number average molecular weight 6,000, molecular weight distribution 1.1, manufactured by Kaneka Corporation. Has a methoxyethyl group as a side chain.) MM200C (Polyacrylate with one radical crosslinking functional group at one end and a main chain structure of 2-methoxyethyl acrylate / ethyl acrylate / n-butyl acrylate = 94 / 3 / 3 (molar ratio), number average molecular weight 3,000, molecular weight distribution 1.1, manufactured by Kaneka Corporation. Has a methoxyethyl group as a side chain.) EBECRYL11 (polyethylene glycol diacrylate, manufactured by Daicel Allnex Co., Ltd.) ●(B) Component DP-4 (Dibutyl phosphate, manufactured by Daihachi Chemical Industry Co., Ltd.) AP-1 (monomethyl phosphate, manufactured by Daihachi Chemical Industry Co., Ltd.) ●(C) component Triglyme (Tokyo Chemical Industry Co., Ltd.) Glycerin (Tokyo Chemical Industry Co., Ltd.) 3-Methylsulfolane (Tokyo Chemical Industry Co., Ltd.) Phosphoric acid (Tokyo Chemical Industry Co., Ltd.) ●(D) Component · OMNIRAD 1173 (2-hydroxy-2-methyl-1-phenyl-propan-1-one, manufactured by BASF) · Omnirad819 (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, manufactured by BASF) ●(E) Component Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, manufactured by Tokyo Chemical Industry Co., Ltd.) Lithium bis(fluorosulfonyl)imide (LiFSI, manufactured by Tokyo Chemical Industry Co., Ltd.) [Examples 1 to 7] In a container, component (E) was mixed with components (B) and (C) in the amounts shown in Table 1, and the mixture was stirred with a spoon to dissolve component (E). The mixture was then heated at 100°C for 1 hour to promote dissolution. Component (A) was then added and stirred with a spoon, after which the mixture was kept at 100°C for 30 minutes to completely dissolve component (E). Finally, component (D) was added and mixed with a spoon to completely dissolve the mixture, yielding a curable composition for electrolyte gels. The obtained curable composition for electrolyte gels was poured into a mold of a specified size and cured with UV (using a high-pressure mercury lamp, cumulative light amount = 2000 mJ / cm2).2 ) to obtain a 1 mm thick cured sheet.

[0099] [Comparative Example 1] A curable electrolyte gel composition and a cured sheet were prepared in the same manner as in Example 1, except that (C) was not added and the amounts of components (A) and (B) were adjusted.

[0100] [Comparative Example 2] A curable electrolyte gel composition and a cured sheet were prepared in the same manner as in Comparative Example 1, except that EBECRYL11 (polyethylene glycol diacrylate) was added instead of polyacrylate.

[0101] [Evaluation Results] The compositions and evaluation results of the examples and comparative examples are shown in Table 1 below. The amounts of each component in Table 1 can be said to be listed so that the total of the components other than component (D) is 100% by weight, or can be said to be listed so that the total of the components other than component (D) is 100 parts by weight. The electrical conductivity in Table 1 represents the electrical conductivity measured by the low resistance resistivity meter described above.

[0102] [Table 1]

[0103] (resistance and conductivity of hardened material) Comparative Examples 1 and 2, in which component (C) was not added, had higher surface resistivity and specific volume resistivity than Examples 1 to 7. That is, it was found that Examples 1 to 7 had better ion conductivity than Comparative Examples 1 and 2. In particular, Examples 1 to 6 also had higher electrical conductivity than Comparative Examples 1 and 2.

[0104] (UV curable) Cured sheets capable of retaining their shape were obtained in all of Examples 1 to 7 and Comparative Examples 1 and 2. Cured products of uniform composition without any bleeding on the surface were obtained in Examples 1 to 7. In contrast, bleeding that seemed to be component (B) was observed in Comparative Example 2, and a tendency for the components to separate was confirmed.

[0105] (Flexibility of the cured product) Examples 1 to 7 had the same or lower rubber hardness than Comparative Examples 1 and 2. In other words, it was found that Examples 1 to 7 were able to maintain flexibility compared to Comparative Examples 1 and 2. In particular, Examples 1 to 5 and 7 had lower rubber hardness than Comparative Example 2, and were excellent in flexibility.

[0106] (Overall review) By adding component (C), which is a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond and containing two or more oxygen atoms in the molecule, to components (A), (B), (D), and (E), it is possible to improve resistance compared to conventional materials while maintaining flexibility such as rubber hardness, and to ensure ionic conductivity at a practical level for lithium-ion batteries.

[0107] [Examples 8 and 9, Comparative Example 3] Curable electrolyte gel compositions and cured sheets were prepared in the same manner as in Example 1, except that the amounts of each component were changed as shown in Table 2.

[0108] [Evaluation Results] The compositions and evaluation results of the examples and comparative examples are shown in Table 2 below. The blending amount of each component in Table 2 is shown with the total amount of component (A) being 100 parts by weight. The electrical conductivity in Table 2 indicates the electrical conductivity measured by impedance measurement.

[0109] [Table 2]

[0110] It can be said that the conductivity by impedance measurement reflects ionic conductivity more than the conductivity measured by a low resistance resistivity meter. Examples 8 and 9 had higher conductivity and better ionic conductivity than Comparative Example 3. In particular, Example 8 had a significantly improved conductivity by impedance measurement (AC) compared to Comparative Example 3. [Industrial Applicability]

[0111] One embodiment of the present invention can be used in, for example, a storage battery, an electronic device, and the like.

Claims

1. Component (A): a liquid polymer containing a crosslinkable functional group; Component (B): at least one of a phosphoric acid monoester and a phosphoric acid diester, Component (C): a compound having a group selected from a hydroxyl group, an acidic group, a sulfonyl group, and an ether bond and containing two or more oxygen atoms in the molecule; Component (D): an initiator, A curable composition for electrolyte gel comprising: (E) component: an electrolyte;

2. The curable composition for an electrolyte gel according to claim 1 , wherein the component (A) is a polymer containing an ether bond in the main chain or a side chain.

3. The component (A) is a polymer containing an ether bond in a side chain, 3. The curable composition for electrolyte gel according to claim 2, wherein the side chain containing an ether bond in the component (A) is at least one selected from the group consisting of a methoxypolyethylene glycol group, a methoxypropylene glycol group, a methoxytriethylene glycol group, a methoxyethyl group, an ethylcarbitol group, and a phenoxyethyl group.

4. The curable composition for an electrolyte gel according to claim 2 , wherein the component (A) is a polymer containing an ether bond in its main chain.

5. The curable composition for an electrolyte gel according to claim 4, wherein the main chain of the component (A) is at least one selected from the group consisting of polyacetal, polyoxyethylene, and polyoxypropylene.

6. The curable composition for an electrolyte gel according to claim 1 , wherein the main chain of the component (A) is a (meth)acrylic polymer.

7. The curable composition for an electrolyte gel according to claim 2 , wherein a polymerization ratio of the monomer having an ether bond in the component (A) is 25 mol % or more.

8. 2. The curable composition for an electrolyte gel according to claim 1, wherein the crosslinkable functional group in the component (A) is at least one selected from the group consisting of a radical crosslinkable functional group, an epoxy group, and a hydrolyzable silyl group.

9. The curable composition for electrolyte gel according to claim 1, wherein the component (C) is at least one selected from the group consisting of glycols, triols, phosphoric acids, carboxylic acids, and glymes.

10. The curable composition for electrolyte gel according to claim 1 , wherein the component (D) is a radical initiator.

11. 2. The curable composition for an electrolyte gel according to claim 1, wherein the component (E) is an electron pair compound of a fluorine atom-containing anion and a lithium cation.

12. 2. The curable composition for electrolyte gel according to claim 1, wherein the content of the component (E) in 100% by weight of the curable composition for electrolyte gel is 20% by weight or more.

13. An electrolyte gel obtained by curing the curable composition for an electrolyte gel according to any one of claims 1 to 12.

14. A storage battery comprising the electrolyte gel according to claim 13.

15. An electronic device comprising the electrolyte gel of claim 13.

Citation Information

Patent Citations

  • Polymer-electrolyte

    JP2001189166A