Lanthanum-based glass structure
A lanthanum-based glass structure with a hierarchical nanoporous layer and low reflectance is achieved by treating the glass substrate with a pH 10.0 or more solution, addressing the high reflectance issue and providing self-cleaning and high transparency benefits.
Patent Information
- Application Number
- JP2023066718
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods for forming a functional network structure on lanthanum-based glass surfaces result in a porous layer with relatively high reflectance, and there is no reported lanthanum-based glass structure with a porous layer having a reflectance of 7.0% or less in the wavelength range of 400 to 700 nm.
A lanthanum-based glass structure is developed with a porous layer that has a reflectance of 7.0% or less at a wavelength of 400 to 700 nm, featuring a hierarchical nanoporous layer formed integrally with the glass substrate, achieved by treating the glass substrate with a treatment solution of pH 10.0 or more.
The structure exhibits low reflectance, high transparency, and self-cleaning properties due to its hierarchical nanoporous layer, preventing dirt accumulation and fogging, suitable for applications requiring high refractive index and light transmittance.
Smart Images

Figure 2024152491000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to lanthanum-based glass structures. [Background technology]
[0002] The surfaces of glass materials such as window glass and mirrors inherently have excellent hydrophilicity, and extremely clean glass surfaces have superhydrophilicity with a water droplet contact angle of 10° or less. However, the surface usually has a mixed hydrophilic and hydrophobic state due to the adsorption of hydrocarbons and the like in the air, and the effective hydrophilicity is reduced. In such cases, it is known that moisture adhering to the surface forms a number of fine water droplets on the surface, causing the surface to become cloudy.
[0003] In response to such problems, Patent Document 1 discloses a functional network structure comprising a network layer that forms a three-dimensional network structure on the surface of a substrate made of silicate glass, the network layer being characterized in that the mesh size on the surface is several tens to 1000 nm and gradually becomes smaller in the direction from the surface to the inside. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-189351 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when lanthanum glass is used as a substrate by the same manufacturing method as in Patent Document 1, it is not possible to form a functional network structure as in Patent Document 1, nor a lanthanum glass structure having a porous layer with a relatively low reflectance. Therefore, there have been no reports on functional network structures of lanthanum glass, nor on lanthanum glass structures having a porous layer with a relatively low reflectance. Lanthanum glass is characterized by a high refractive index and low dispersion, and is therefore sometimes used as optical glass.
[0006] Therefore, the present invention has been made to solve the above problems, and has an object to provide a lanthanum glass structure having a porous layer and a reflectance of 7.0% or less at a wavelength of 400 to 700 nm on the porous layer side.
[0007] Furthermore, the present invention can provide a lanthanum-based glass structure having a hierarchical nanoporous layer as a porous layer. The "hierarchical nanoporous layer" in the present invention has a three-dimensional network structure similar to the functional network structure of Patent Document 1. [Means for solving the problem]
[0008] The present inventors have found that the above problems can be solved by the following means.
[0009] <Aspect 1> A porous layer and a lanthanum-based glass substrate, the porous layer is integrally formed with the lanthanum based glass substrate; and The reflectance of the porous layer side at a wavelength of 400 to 700 nm is 7.0% or less. Lanthanide glass structures. <Aspect 2> 10. The structure of claim 1, wherein the porous layer is a hierarchical nanoporous layer. <Aspect 3> 3. The structure according to aspect 1 or 2, wherein the average mesh size on the surface of the porous layer is 1000 nm or less. <Aspect 4> The structure according to any one of aspects 1 to 3, wherein the porous layer has a thickness of 10 nm or more. <Aspect 5> The structure according to any one of aspects 1 to 4, wherein the surface of the porous layer is hydrophilic. Aspect 6 The structure according to any one of aspects 1 to 5, having a haze value of 5.0% or less. Aspect 7 A method for producing the lanthanum-based glass structure according to any one of aspects 1 to 6, comprising the steps of: The method includes immersing an untreated lanthanum glass substrate in a treatment solution having a pH value of 10.0 or more at the start of the treatment. method. <Aspect 8> 8. The method of claim 7, wherein the treatment solution is an aqueous carbonate solution. Effect of the Invention
[0010] According to the present invention, it is possible to provide a lanthanum based glass structure having a porous layer and having a reflectance of 7.0% or less at a wavelength of 400 to 700 nm on the porous layer side, and a method for producing the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 shows SEM images of the surface of each of the structures of Examples 1 and 2 and Comparative Examples 1 to 4. [Diagram 2] FIG. 2 is a diagram showing the reflectance of each of the structures of Examples 1 and 2 and Comparative Examples 1 to 4. [Diagram 3] FIG. 3 is a diagram showing the water droplet contact angle of each of the structures of Examples 1 and 2 and Comparative Examples 2 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0013] <Lanthanum-based glass structure> The lanthanum-based glass structure of the present invention (hereinafter also simply referred to as the "structure of the present invention") is A porous layer and a lanthanum-based glass substrate, The porous layer is integrally formed with the lanthanum-based glass substrate; and The reflectance of the porous layer side at a wavelength of 400 to 700 nm is 7.0% or less. Lanthanide glass structures It is.
[0014] The inventors of the present invention have succeeded in producing a lanthanum-based glass structure having a novel porous layer by a manufacturing method different from that of the above-mentioned Patent Document 1. Specifically, the inventors have found through intensive research that the pH value of the treatment solution is important for forming a porous layer integrally with the lanthanum-based glass untreated substrate. Without being limited by theory, it is presumed that the structure of the present invention is finally obtained by immersing the lanthanum-based glass untreated substrate in a treatment solution having a pH value in a specific range, whereby some components of the lanthanum-based glass are dissolved from the surface of the untreated substrate.
[0015] In addition, the structure of the present invention has a relatively low reflectance, and more specifically, the reflectance at wavelengths of 400 to 700 nm on the porous layer side is 7.0% or less. More specifically, the reflectance at wavelengths of 400 to 700 nm on the structure of the present invention can be 7.0% or less, 6.8% or less, 6.5% or less, 6.0% or less, 5.5% or less, 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, or 2.0% or less. Such a low reflectance on the porous layer side means that the porous layer is a hierarchical nanoporous layer. In the present invention, the reflectance can be measured by irradiating the sample with light from a halogen lamp through a microscope and dividing the reflected light by wavelength with a spectroscope.
[0016] In the present invention, the hierarchical nanoporous layer means a layer having a three-dimensional network structure, in which the size of the mesh gradually decreases from the surface toward the inside, so that the porosity (air porosity) of the outer surface of the porous layer is high and the porosity decreases toward the substrate side. Whether the size of the mesh of the hierarchical nanoporous layer gradually decreases from the surface toward the inside can be determined by observing the cross section of the structure of the present invention with a scanning electron microscope (SEM). More specifically, the hierarchical nanoporous layer may have a large mesh size near the surface and a tendency for the mesh size to gradually decrease toward the inside (the substrate side where the hierarchical nanoporous layer is present). Therefore, it is sufficient that the size of the mesh tends to decrease overall from the surface toward the inside, and the pore size may not change much near the surface, and there may be slightly larger pores below the outermost surface due to fluctuations in the formation of the structure.
[0017] In this way, when the porous layer according to the present invention is a hierarchical nanoporous layer, the structure of the present invention can have the characteristic that the mesh (pores) gradually become smaller in the direction from the surface to the inside, like the functional network structure of silicate glass in Patent Document 1. Therefore, like the structure in Patent Document 1, the structure of the present invention can prevent dirt such as dust and dirt from penetrating deep into the hierarchical nanoporous layer, and can effectively exhibit the original surface characteristics of the material constituting the hierarchical nanoporous layer. Therefore, for example, when the surface of the structure of the present invention is brought into contact with water, the water penetrates between the hierarchical nanoporous layer and the dirt, and a self-cleaning effect is exhibited to float and remove the dirt, thereby obtaining a long-lasting antifouling property. In addition, since the self-cleaning effect can prevent clogging of the hierarchical nanoporous layer, even if moisture adheres to the surface of the structure of the present invention, the water is absorbed into the three-dimensional network structure, and the attached moisture is spread widely in the planar direction of the surface, making it possible to exhibit excellent antifogging properties.
[0018] Furthermore, when the porous layer according to the present invention is a hierarchical nanoporous layer, the structure of the present invention can make the volume fraction of the pores in the network gradually smaller in the direction from the surface to the inside (i.e., the volume fraction of the glass substrate constituting the network gradually increases in the direction from the surface to the inside), thereby making it possible to make the refractive index relatively small at the surface of the hierarchical nanoporous layer and increasing the refractive index toward the deeper part. This makes it possible to suppress light reflection in the lanthanum based glass structure having a hierarchical nanoporous layer.
[0019] Furthermore, since the structure of the present invention uses a lanthanum-based glass substrate, it can be suitably used in a wide range of applications, including camera lenses and medical optical instruments that require a high refractive index, as well as optical fibers, displays (liquid crystal, micro LEDs, etc.), optical filters, and the like, due to their high refractive index.
[0020] The haze value of the structure of the present invention may be 5.0% or less, 4.0% or less, 3.0% or less, 2.0% or less, 1.0% or less, 0.9% or less, 0.8% or less, 0.7% or less, 0.6% or less, 0.5% or less, 0.4% or less, 0.3% or less, 0.2% or less, or 0.1 or less. Therefore, the structure of the present invention has high transparency and can be preferably used in applications requiring high light transmittance (for example, optical applications, etc.). In the present invention, the haze value can be measured by combining a spectrophotometer and an integrating sphere. More specifically, the haze value can be calculated from the intensity of the light that goes straight and the total intensity of the scattered light by irradiating a light beam on a sample.
[0021] <Porous Layer> In the structure of the present invention, the porous layer is formed integrally with the substrate. Here, "integrally" means that there is no other layer between the porous layer and the substrate, and in particular, the porous layer and the substrate exist without a break (i.e., the two exist seamlessly).
[0022] The porous layer of the present invention may also be a hierarchical nanoporous layer.
[0023] In the structure of the present invention, the size of the mesh on the surface of the porous layer can be 1500nm or less, 1000nm or less, 500nm or less, 300nm or less, 100nm or less, 90nm or less, 80nm or less, 70nm or less, 60nm or less, 50nm or less, 40nm or less, 30nm or less, or 20nm or less. Thus, when the size of the mesh on the surface of the porous layer is 1500nm or less, particularly 1000nm or less, it is smaller than the size of general dust and the like, and can prevent the penetration of house dust, which is generally said to be 10μm or more, into the depths of the porous layer. In addition, when the size of the mesh on the surface of the porous layer is 500nm or less, it can prevent the penetration of indoor floating dust, which is generally said to be 1 to 10μm, into the depths of the porous layer. Furthermore, when the size of the mesh on the surface of the porous layer is less than 100nm, it can prevent the penetration of small bacteria, which is generally said to be 100nm or more, into the depths of the network structure layer.
[0024] In the structure of the present invention, the average mesh size on the surface of the porous layer can be 1000 nm or less, 500 nm or less, 300 nm or less, 100 nm or less, 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, or 20 nm or less.
[0025] In the present invention, the lower limit of the size of the mesh on the surface of the porous layer is not particularly limited, and may be, for example, 10 nm or more, or 20 nm or more.
[0026] In the present invention, the size of the mesh on the surface of the porous layer refers to, for example, the longest diameter of the pores in an SEM image of the surface of the porous layer, and the average size of the mesh on the surface of the porous layer is the average value calculated from the sizes of at least 10 meshes, preferably as many as possible, observed by SEM.
[0027] In the structure of the present invention, the thickness of the porous layer is not particularly limited, and may be, for example, 10 nm or more, 50 nm or more, 100 nm or more, 200 nm or more, 300 nm or more, 400 nm or more, or 500 nm or more, and may be 2000 nm or less, 1500 nm or less, 1000 nm or less, 800 nm or less, or 500 nm or less. In the present invention, the thickness of the porous layer can be confirmed, for example, by observing the cross section of the structure of the present invention by SEM.
[0028] In the structure of the present invention, the water droplet contact angle of the surface of the porous layer may be 10° or less. Therefore, in the structure of the present invention, the surface of the porous layer may have extremely excellent hydrophilicity, particularly superhydrophilicity. In the present invention, the water droplet contact angle can be measured, for example, according to the method specified in JIS R3257:1999, by photographing a water droplet from a nearly horizontal direction with a camera and determining the angle from the image.
[0029] <Lanthanum-based glass substrate> The structure of the present invention has a lanthanum-based glass substrate.
[0030] In the present invention, the lanthanum-based glass constituting the lanthanum-based glass substrate means a glass containing a large amount of lanthanum oxide (La2O3), and such glass generally has a large refractive index. More specifically, the content of lanthanum oxide in the lanthanum-based glass may be, for example, 15% by mass or more, 18% by mass or more, 20% by mass or more, 22% by mass or more, 25% by mass or more, 28% by mass or more, or 30% by mass or more. The upper limit of the content of lanthanum oxide is not particularly limited, and may be, for example, 99.9% by mass or less, 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, 40% by mass or less, or 30% by mass or less. The refractive index of the lanthanum-based glass may be, for example, 1.65 or more, 1.70 or more, 1.75 or more, 1.80 or more, 1.85 or more, or 1.88 or more. Furthermore, the upper limit of the refractive index of the lanthanum-based glass is not particularly limited, and may be, for example, 2.20 or less.
[0031] In the present invention, the components of the lanthanum-based glass may include, in addition to lanthanum oxide, at least one selected from the group consisting of boron oxide (B2O3), gadolinium oxide (Gd2O3), tungsten oxide (WO3), zirconia oxide (ZrO2), tantalum oxide (Ta2O5), and silicon dioxide (SiO2).
[0032] The lanthanum-based glass may be commercially available, for example, Ohara S-LAH58 manufactured by Ohara Corporation.
[0033] <Other configurations> In addition to the porous layer and substrate described above, the structure of the present invention may optionally further include other components.
[0034] For example, a porous layer can be coated or filled with a functional material, which can impart surface properties with a desired function.
[0035] More specifically, for example, a hydrophilic organic material such as polyethylene glycol that can be bonded to the surface of each mesh of the porous layer by a methoxysilane or chlorosilane group can be coated on the porous layer to exhibit superior superhydrophilicity.
[0036] In addition, for example, hydrophobic organic molecules such as alkyl chains or fluoroalkyl chains that can be bonded to the surface of each mesh in the network structure layer via methoxysilane or chlorosilane groups can be coated onto the porous layer to exhibit excellent super-water repellency.
[0037] Furthermore, for example, highly hydrophobic materials such as oil components and paraffin can be filled into the porous layer to exhibit excellent water repellency.
[0038] Furthermore, a conductive material such as metal, metal particles, or a conductive polymer can be filled into the porous layer to impart conductivity to the porous layer made of an insulating or dielectric material.
[0039] Furthermore, a coloring material such as pigment particles or dye molecules can be filled into the network structure layer to impart a desired color to the porous layer.
[0040] <<Method for manufacturing lanthanum-based glass structure>> The present invention also provides a method for producing a lanthanum-based glass structure (hereinafter also simply referred to as the "production method of the present invention").
[0041] The manufacturing method of the present invention is a method comprising immersing an untreated lanthanum glass substrate in a treatment solution having a pH value of 10.0 or more at the start of the treatment. In the present invention, the term "untreated lanthanum glass substrate" refers to a substrate before it is subjected to a treatment by the manufacturing method of the present invention, and may be a substrate that has been subjected to a treatment other than the treatment by the manufacturing method of the present invention.
[0042] The lanthanum-based glass structure obtained by the method of the present invention is the above-mentioned structure of the present invention, and therefore the details of the lanthanum-based glass constituting the lanthanum-based glass untreated substrate used are as described above, and therefore will not be described here.
[0043] In the manufacturing method of the present invention, the treatment solution is not particularly limited as long as it has a pH of 10.0 or more at the start of treatment. More specifically, the pH value of the treatment solution may be 10.0 or more, 10.1 or more, 10.2 or more, 10.3 or more, 10.4 or more, 10.5 or more, 10.6 or more, 10.7 or more, 10.8 or more, 10.9 or more, 11.0 or more, 11.1 or more, 11.2 or more, 11.3 or more, 11.4 or more, 11.5 or more, 11.6 or more, 11.7 or more, 11.8 or more, or 11.9 or more. The upper limit of the pH value of the treatment solution is not particularly limited, and may be, for example, 14.0 or less, 13.5 or less, 13.0 or less, 12.5 or less, or 12.0 or less. In the present invention, the pH value of the treatment solution can be measured at room temperature (25°C) using a commercially available pH meter.
[0044] In the manufacturing method of the present invention, the pH of the solution before and after the treatment of the lanthanum glass untreated substrate with the treatment solution may vary. For example, more specifically, the width between the pH at the start of treatment and the pH value after treatment in the treatment solution (the absolute value of the difference between the pH at the start of treatment and the pH after treatment for the structures of Examples 1 and 2) may be, for example, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more. The upper limit of this width is not particularly limited, and may be, for example, 2.0 or less, 1.5 or less, or 1.0 or less.
[0045] In the manufacturing method of the present invention, the treatment solution may be, for example, an aqueous carbonate solution. More specifically, examples of the treatment solution include, but are not limited to, an aqueous sodium carbonate solution or an aqueous potassium carbonate solution.
[0046] In addition, the concentration of carbonate in the treatment solution is not particularly limited and may be set appropriately according to the treatment temperature, the target thickness of the structure formed, and the like, and may be, for example, 0.5 mol / L or more, 0.8 mol / L or more, 1.0 mol / L or more, 1.5 mol / L or more, or 2.0 mol / L or more, and may be 10 mol / L or less, 9.0 mol / L or less, or 8.5 mol / L or less.
[0047] In the production method of the present invention, the treatment temperature of the untreated lanthanum glass substrate with the treatment solution is not particularly limited and may be appropriately set according to the size of the untreated lanthanum glass substrate to be treated, and may be, for example, 70 to 150°C, or 100 to 130°C.
[0048] In the manufacturing method of the present invention, the treatment time of the untreated lanthanum glass substrate with the treatment solution is not particularly limited and may be appropriately set according to the treatment temperature, the target thickness of the structure formed, or the size of the untreated lanthanum glass substrate to be treated, and may be, for example, 1 to 50 hours, or 10 to 30 hours. Depending on the treatment temperature, the treatment time may be 50 hours or more, or 100 hours or more.
[0049] Furthermore, the manufacturing method of the present invention may further include, for example, pretreating the untreated lanthanum based glass substrate.
[0050] The pretreatment is not particularly limited, and may be, for example, ultrasonic cleaning, cleaning with an alcohol solution, or a combination thereof. EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0052] Examples 1 and 2, and Comparative Examples 1 to 4 As the untreated lanthanum-based glass substrate, a disk-shaped glass plate material, Ohara S-LAH58 manufactured by Ohara Corporation, having a diameter of 23.8 mm and a thickness of 1.0 mm was used.
[0053] Six of the above untreated lanthanum glass substrates were immersed in the aqueous treatment solutions shown in Table 1 below and treated at a treatment temperature of 120° C. for 20 hours to obtain structures of Examples 1 and 2 and Comparative Examples 1 to 4. In each of the treatment solutions, the solute concentration was 1.0 mol / L.
[0054] [Table 1]
[0055] <Scanning Electron Microscope (SEM) Observation> The surface and cross section of each structure sample were observed using a scanning electron microscope (SU8200, Hitachi High-Technologies Corporation). The SEM images of the surface of each structure sample obtained are shown in Figure 1.
[0056] FIG. 1 shows SEM images of the surfaces of the structure samples of Examples 1 and 2 and Comparative Examples 1 to 4.
[0057] 1, it was found that the surfaces of the structures of Examples 1 and 2 and Comparative Examples 1 and 2 had a porous structure. It was also found that the mesh size on the surface of the structure of Example 1 was about 8 to 15 nm, and the mesh size on the surface of the structure of Example 2 was about 10 to 20 nm.
[0058] On the other hand, the surfaces of the structures of Comparative Examples 3 and 4 had a coarse crack-like structure, unlike those of Examples 1 and 2 and Comparative Examples 1 and 2, and it was found that no porous layer was formed.
[0059] Although not shown, SEM images of the cross sections of the structures of Examples 1 and 2 show that the porous layer is integrally formed with the substrate in both cases. Also, it was found that each porous layer has a three-dimensional network structure, with the mesh size gradually decreasing from the surface toward the inside, that is, the porous layer has a hierarchical nanoporosity.
[0060] In contrast, SEM images of the cross sections of the structures of Comparative Examples 1 and 2 showed that in both cases, the porous layer was integrally formed with the substrate, but the mesh size of each porous layer was approximately uniform in the direction from the surface to the inside (not shown).
[0061] <Reflectance measurement> The reflectance of each structure sample was measured using a microscope (Shibuya Optical Co., Ltd., SMP-100 type). The measurement results are shown in Figure 2. For reference, the reflectance of untreated glass (Ohara S-LAH58, Ohara Corporation) was also measured in the same manner.
[0062] 2, the reflectance at wavelengths of 400 to 700 nm was 7.0% or less in both of the structures of Examples 1 and 2, that is, the reflectance was low. It is presumed that the low reflectance is due to the fact that the porous layers of the structures of Examples 1 and 2 are hierarchical nanoporous layers.
[0063] On the other hand, it was found that the reflectance was particularly high for the structures of Comparative Examples 1 and 2. In addition, from the waveforms of those reflectances, it is inferred that the porous layers of the structures of Comparative Examples 1 and 2 did not become hierarchical nanoporous layers, and interference due to pores in the porous layers was significant.
[0064] <Haze value measurement> The haze value of each structure sample was measured using a spectrophotometer (V-770 manufactured by JASCO Corporation) in combination with an integrating sphere (ISN-923 manufactured by JASCO Corporation). The measurement results are shown in Table 2 below. For reference, the haze value of untreated glass (Ohara S-LAH58 manufactured by Ohara Corporation) was also measured in the same manner.
[0065] [Table 2]
[0066] As is clear from the results in Table 2, the haze value of the structure of Example 1 was 0.5, and the haze value of Example 2 was 0.1, indicating that both had high transparency.
[0067] On the other hand, the haze value of Comparative Example 1 was particularly high at 11.6, and although not shown, it was clearly evident that the surface of the structure of Comparative Example 1 was cloudy.
[0068] <Contact angle measurement> The water droplet contact angle of each structure sample (except Comparative Example 1) was measured according to the method specified in JIS R3257:1999 by photographing a water droplet from a nearly horizontal direction with a camera and determining the angle from the image. The measurement results are shown in Figure 3. Note that the structure sample of Comparative Example 1 had a large number of precipitates on the porous layer, and therefore does not fall under the "porous layer" defined in the present invention, particularly the "hierarchical nanoporous layer," and therefore the contact angle was not measured.
[0069] As is clear from the results in FIG. 3, the water droplet contact angle on the surface was 10° or less in all of the structures.
[0070] In addition, the structures of Comparative Examples 3 and 4 had a water droplet contact angle of 10° or less at the time of measurement, but the contact angle increased within 3 months after preparation, indicating that the hydrophilicity of these structures was not durable.
[0071] <summary> As described above, the structures of Examples 1 and 2 have a hierarchical nanoporous layer and have low reflectance, and in particular, the reflectance at wavelengths of 400 to 700 nm on the porous layer side was found to be 7.0% or less. Furthermore, the structures of Examples 1 and 2 were found to have low haze values and to be superhydrophilic.
Claims
1. A porous layer and a lanthanum-based glass substrate, the porous layer is integrally formed with the lanthanum based glass substrate; and The reflectance of the porous layer side at a wavelength of 400 to 700 nm is 7.0% or less. Lanthanide glass structures.
2. The structure of claim 1 , wherein the porous layer is a hierarchical nanoporous layer.
3. 2. The structure according to claim 1, wherein the average mesh size on the surface of the porous layer is 1000 nm or less.
4. The structure of claim 1 , wherein the porous layer has a thickness of 10 nm or more.
5. The structure of claim 1 , wherein the surface of the porous layer is hydrophilic.
6. 10. The structure of claim 1, having a haze value of 5.0% or less.
7. A method for producing the lanthanum-based glass structure according to any one of claims 1 to 6, comprising the steps of: The method includes immersing an untreated lanthanum glass substrate in a treatment solution having a pH value of 10.0 or more at the start of the treatment. method.
8. The method of claim 7 , wherein the treatment solution is an aqueous carbonate solution.