Cell and electronic appliance

By alternating positive and negative electrodes with specific cathode active materials and varying orientations, the battery achieves high energy density and safety while reducing costs, addressing the limitations of existing lithium-ion batteries.

JP2024152579AActive Publication Date: 2024-10-25AESC JAPAN LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023210709
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-12-14
Publication Date
2024-10-25
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in achieving high energy density, safety, and cost efficiency due to the mismatched performance of positive and negative electrode materials, particularly with phosphate and ternary cathode materials, which affect the overall capacity and energy density of the cell.

Method used

The solution involves alternating positive and negative electrodes with different cathode active materials, where the first positive electrode film uses phosphate materials like lithium iron phosphate and the second positive electrode film uses high-energy density materials such as lithium nickel cobalt manganese oxide, while the negative electrode films have varying orientations (OI values) to optimize energy density and safety.

Benefits of technology

This approach maximizes energy density, safety, and reduces costs by balancing the performance of the electrodes, achieving energy densities up to 246 wh/kg with excellent cycling performance and capacity retention rates exceeding 90% after 1000 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152579000001_ABST
    Figure 2024152579000001_ABST
Patent Text Reader

Abstract

PURPOSE: To provide a cell and an electronic appliance.SOLUTION: In a cell and an electronic appliance, a first positive electrode film and a second positive electrode film are disposed on two opposite surfaces of a positive electrode current collector. The capacity of a second positive electrode active material per gram is larger than that of a first positive electrode active material per gram. A first negative electrode film and a second negative electrode film are disposed on two opposite surfaces of a negative electrode current collector. OI2-OI1>5 is satisfied, in which OI2 represents an OI value of the second negative electrode film and OI1 represents an OI value of the first negative electrode film. Since a positive electrode and a negative electrode match with each other in the cell rationally, it is possible to take advantage of the overall energy density and capacity of the cell fully, and at the same time consider the safety.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cell and an electronic device. [Background technology]

[0002] In 2021, sales of new energy vehicles in China will exceed 3.3 million units, and in 2022, the total annual sales volume of China's new energy market will exceed 5.5 million units. Most of them are equipped with lithium-ion batteries. There is a consensus worldwide about the rapid growth of new energy vehicles, and the development of lithium-ion batteries has entered a golden age.

[0003] Lithium-ion batteries have undergone rapid development in recent years, during which most performance indicators have been fundamentally improved. Currently, energy density, safety, and cost are the main concerns of major cell suppliers.

[0004] However, the gravimetric energy density of conventional lithium iron phosphate power cells is generally 160Wh / kg to 190Wh / kg. Lithium manganese iron phosphate, which has a similar structure and energy storage mechanism to lithium iron phosphate, has a theoretical capacity equivalent to that of lithium iron phosphate and a higher voltage platform, so it can provide a higher energy density, but it is still difficult to exceed 200Wh / kg. Ternary lithium-ion batteries have a relatively high energy density, but their high price and thermal safety make consumers hesitate. Therefore, the industry chooses to use phosphate cathode materials together with high energy density cathode materials such as ternary cathodes and lithium-excess lithium manganese cathodes.

[0005] Common phosphate positive electrodes and ternary materials are used by mixing in a slurry. Phosphates have low electrical conductivity, so they require more conductive agents. They also have a large specific surface area, so they require more binders. As a result, the ratio of the main components in the electrode plate is low, which affects the overall energy density of the cell. At the same time, the phosphate positive electrode material, which has low ionic and electronic conductivity, can be adsorbed on the surface of the ternary material, which affects the capacity performance of the ternary material.

[0006] In addition, materials such as lithium iron phosphate, lithium manganese iron phosphate, ternary cathode materials, and lithium-rich lithium manganese-based materials each have suitable anode graphite materials. The use of mixed cathodes poses new challenges in graphite selection. Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve the difficulty of matching the positive and negative electrode materials of secondary batteries in the prior art and the impact it has on the overall energy density and capacity performance of the cell, the present invention provides a cell and an electronic device. The cell of the present invention has a reasonably matched positive and negative electrodes, so that the overall energy density and capacity performance of the cell can be maximized, and at the same time, safety can be taken into consideration. [Means for solving the problem]

[0008] The present invention mainly solves the above technical problems through the following technical solutions:

[0009] According to a first aspect, the present invention provides a cell including positive and negative plates alternately arranged along a thickness direction of the cell, and a separator is provided between the positive and negative plates. The positive plate includes a positive current collector, a first positive film, and a second positive film, the first positive film and the second positive film being respectively disposed on two opposite surfaces of the positive current collector. The first positive film includes a first positive active material including a phosphate material, and the second positive film includes a second positive active material having a capacity per gram greater than the capacity per gram of the first positive active material. The negative plate includes a negative current collector, a first negative film, and a second negative film, the first negative film and the second negative film being respectively disposed on two opposite surfaces of the negative current collector. The first negative film includes a first negative active material, and the second negative film includes a second negative active material, satisfying OI2-OI1>5. Here, OI2 is the OI value of the second negative film and OI1 is the OI value of the first negative film.

[0010] According to a second aspect, the present invention further provides an electronic device including a cell as described above. Effect of the Invention

[0011] The positive and progressive effects of the present invention are as follows: The present invention maximizes the matching in the mixed system by selecting different positive electrode compositions for different negative electrode compositions, and realizes the combination of high energy density, high safety and low cost. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic structural diagram of cells fabricated in Examples 1 and 2 of the present invention (1: negative electrode current collector; 2: positive electrode current collector; 4: second positive electrode film; 5: first positive electrode film; 6: second negative electrode film; 7: first negative electrode film). [Diagram 2]FIG. 1 is a simplified structural diagram of cells produced in Examples 1 and 2 of the present invention (1: negative electrode current collector; 2: positive electrode current collector; 3: separator; 4: second positive electrode film; 5: first positive electrode film; 6: second negative electrode film; 7: first negative electrode film). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the following text, the present invention will be described in more detail, making the present invention easier to understand. It should be understood that the words or terms used in this specification and claims should not be interpreted as having the meanings defined in common dictionaries. It should be further understood that the words or terms should be interpreted as having the meanings in the relevant technical context and the meanings consistent with the technical concept of the present invention, based on the principle that the inventor can properly define the meanings of the words or terms and best interpret the present invention.

[0014] cell

[0015] In a cell according to the first aspect of the present invention,

[0016] The two surfaces of the positive electrode are respectively made of phosphate materials and high-density active materials, which correspond to the high energy density film and high-speed charging dynamics film of the negative electrode in a one-to-one relationship. The positive and negative electrodes are matched with each other to achieve a balance between energy density and fast charging performance.

[0017] Positive plate

[0018] In the present invention, the first positive electrode film is adjacent to the second negative electrode film via a separator, and the second positive electrode film is adjacent to the first negative electrode film via a separator.

[0019] In the present invention, as the first positive electrode active material, the phosphate material can be the positive electrode phosphate material commonly used in the field, and is preferably lithium iron phosphate and / or lithium manganese iron phosphate.The use of phosphate material can reduce system cost and improve safety performance.

[0020] Preferably, based on the mass of the first positive electrode film, the mass content of the phosphate material is 92% to 97%, for example, 94% or 95%.

[0021] Preferably, the discharge capacity per gram of the phosphate material at a current density of 0.1 C is 160 mAh / g or less, more preferably 127 mAh / g to 160 mAh / g, for example 141 mAh / g or 157 mAh / g.

[0022] In the present invention, the second positive electrode active material is a high energy density active material commonly used in the field, and its use can improve the energy density and low temperature cycling performance of the battery.

[0023] Preferably, the second positive electrode active material includes one or more of lithium manganate, lithium cobalt oxide, lithium nickelate, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium-rich lithium manganese based materials.

[0024] When the second positive electrode active material includes lithium nickel cobalt aluminum oxide or lithium nickel cobalt manganese oxide, the mass content of Ni in the lithium nickel cobalt aluminum oxide or lithium nickel cobalt manganese oxide is 60% or more, based on the mass of the lithium nickel cobalt aluminum oxide or lithium nickel cobalt manganese oxide.

[0025] Preferably, based on the mass of the second positive electrode film, the content of the second positive electrode active material is 94% to 98%, for example, 96%.

[0026] Preferably, the discharge capacity per gram of the second positive electrode active material at a current density of 0.1 C is 180 mAh / g or more, more preferably 180 mAh / g to 210 mAh / g, for example, 198 mAh / g.

[0027] In some preferred embodiments, the content of the second positive electrode active material is greater than the content of the first positive electrode active material.

[0028] In some preferred embodiments, the first positive electrode active material is lithium manganese iron phosphate and the second positive electrode active material is lithium nickel cobalt manganese oxide.

[0029] The lithium manganese iron phosphate is preferably LiMn 0.6 Fe 0.4 PO4, and the lithium nickel cobalt manganese oxide is preferably LiNi 0.8 Co 0.1 Mn 0.1 It's O2.

[0030] In some preferred embodiments, the first positive electrode active material is lithium iron phosphate and the second positive electrode active material is lithium nickel cobalt manganese oxide.

[0031] The lithium iron phosphate is preferably LiFePO4, and the lithium nickel cobalt manganese oxide is preferably LiNi 0.8 Co 0.1 Mn 0.1 It's O2.

[0032] In the present invention, the thickness ratio of the first positive electrode film to the second positive electrode film is preferably (1.1 to 2.5), for example, 1.98:1 or 1.63:1.

[0033] In the present invention, the thickness of the first positive electrode film is 50 μm to 120 μm, preferably 60 μm to 100 μm, for example, 76 μm or 91 μm.

[0034] In the present invention, the thickness of the second positive electrode film is 30 μm to 90 μm, preferably 40 μm to 70 μm, for example, 47 μm.

[0035] In the present invention, the positive active materials with different capacities are selected, which requires the negative electrode material to have a matching capacity. When the appropriate thickness ratio is selected, the thickness difference between the front and back of the negative electrode can be controlled to be small, which is advantageous for the processing of the negative electrode.

[0036] The thicknesses described in the present invention are calculated based on the following method.

[0037] Let the thickness of the first positive electrode film be h1, the specific discharge capacity of the first positive electrode film be x1, and the specific discharge capacity of the second negative electrode film be x2, the proportion of the first positive electrode active material be y1, the proportion of the second negative electrode active material be y2, the density of the first positive electrode film after rolling be z1, and the density of the second negative electrode film after rolling be z2, and N / P be a1. Then, the thickness h2 of the second negative electrode film is calculated by the following formula:

[0038]

number

[0039] Let the thickness of the second positive electrode film be h3, the specific discharge capacity of the second positive electrode film be x3, and the specific discharge capacity of the first negative electrode film be x4, the proportion of the second positive electrode active material be y3, the proportion of the first negative electrode active material be y4, the density of the second positive electrode film after rolling be z3, and the density of the first negative electrode film after rolling be z4, and N / P be a2. Then, the thickness h4 of the first negative electrode film is calculated by the following formula:

[0040]

number

[0041] N / P is 1.02 to 1.14, and a 1≧ N / P represents the "negative electrode capacity per unit area / positive electrode capacity per unit area" and is generally the ratio of the charging capacity.

[0042] z3>z1, and z3-z1>0.4g / cm 3 In the rolling process of the positive electrode film, a certain pressure and roll gap width need to be designed, so the density z1 of the first positive electrode film and the density z3 of the second positive electrode film are different.

[0043] In some specific embodiments, the thickness of the first positive electrode film is 50 μm to 120 μm, and the density of the first positive electrode film is 2.2 g / cm 3 ~2.6g / cm 3 The thickness of the second positive electrode film is 30 μm to 90 μm, and the density of the second positive electrode film is 3.3 g / cm 3 ~3.7g / cm 3 It is.

[0044] In the present invention, the first positive electrode film generally further includes a first positive electrode conductive agent, a first positive electrode binder, and a first positive electrode dispersant, and the second positive electrode film generally further includes a second positive electrode conductive agent, a second positive electrode binder, and a second positive electrode dispersant.

[0045] The first positive electrode conductive agent and the second positive electrode conductive agent are not particularly limited as long as they are conductive and do not cause a chemical change in the battery.Specific examples include graphite such as natural graphite or artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal carbon black, and carbon fiber, metal powder or metal fiber such as copper, nickel, aluminum, and silver, conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers, conductive metal oxides such as titanium dioxide, or conductive polymers such as polyphenylene derivatives.

[0046] In the first positive electrode film, the content of the first conductive agent is preferably 1% to 3%, for example, 2%, where the percentage is the percentage of the mass of the first conductive agent relative to the mass of the first positive electrode film.

[0047] In the second positive electrode film, the mass ratio of the second conductive agent is preferably 0.5% to 2%, for example, 1.5%, where the percentage is the mass percentage of the second conductive agent relative to the mass of the second positive electrode film.

[0048] The first positive electrode binder and the second positive electrode binder are used to strengthen the bond between the positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. The type of the binder is not particularly limited, and specific examples of the binder include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-hexafluoropropylene (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene copolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or their respective copolymers, and any one of the above or a mixture of two or more of them can be used.

[0049] In the first positive electrode film, the content of the first binder is preferably 1.5% to 4%, for example, 3.5%, where the percentage is the mass percentage of the first binder relative to the mass of the first positive electrode film. By increasing the ratio of the conductive agent and the binder in the first positive electrode film, the electrochemical performance of the phosphate material can be improved.

[0050] In the second positive electrode film, the mass ratio of the second binder is preferably 0.5% to 2%, where the percentage is the percentage of the mass of the second binder relative to the mass of the second positive electrode film.

[0051] Preferably, the content of the second positive electrode binder is lower than the content of the first positive electrode binder.

[0052] The first dispersant and the second dispersant may be substances that are commonly used in the art and can improve the dispersion uniformity of the active substance.

[0053] In the first positive electrode film, the content of the first dispersant may be 0% to 1%, where the percentage is the percentage of the mass of the first dispersant relative to the mass of the first positive electrode film.

[0054] In the second positive electrode film, the content of the second dispersant may be 0% to 1%, where the percentage is the percentage of the mass of the second dispersant relative to the mass of the second positive electrode film.

[0055] In the present invention, the method for preparing a positive plate includes the steps of coating a raw material mixture for a first positive film and a raw material mixture for a second positive film on two surfaces of a positive current collector respectively to obtain a positive plate.

[0056] In the present invention, surface density generally refers to the mass of raw mixture applied per unit area and refers to one surface.

[0057] In some specific embodiments of the present invention, the surface density of the first and second positive electrode films is 15 mg / cm 2 ~32mg / cm 2 and preferably 20 mg / cm 2 ~25mg / cm 2 For example, 22 mg / cm 2 It is.

[0058] In some preferred embodiments, the surface density of the second positive electrode film is less than the surface density of the first positive electrode film.

[0059] In some preferred embodiments, the surface density of the raw material composition of the second positive electrode film during coating is 60% to 95% of the surface density of the raw material composition of the first positive electrode film during coating.

[0060] Negative plate

[0061] In the present invention, the OI value refers to the degree of orientation and can be calculated based on the data measured by XRD. The OI value is the ratio of the peak area of ​​the 004 characteristic peak in the X-ray diffraction spectrum of the negative electrode film to the peak area of ​​the 110 characteristic peak in the X-ray diffraction spectrum of the negative electrode film.

[0062] In the present invention, OI1=C 004 / C 110 where C 004 is the peak area of ​​the 004 characteristic diffraction peak in the X-ray diffraction spectrum of the first negative electrode film, and C 110 is the peak area of ​​the 110 characteristic diffraction peak in the X-ray diffraction spectrum of the first negative electrode film.

[0063] OI2=C' 004 / C' 110 where C' 004 is the peak area of ​​the 004 characteristic diffraction peak in the X-ray diffraction spectrum of the second negative electrode film, and C' 110 is the peak area of ​​the 110 characteristic diffraction peak in the X-ray diffraction spectrum of the second negative electrode film.

[0064] In the present invention, XRD is measured using a Bruker D8A25 X-ray diffractometer.

[0065] The magnitude of the OI value of the negative electrode film can reflect the degree of stacking orientation of the negative electrode active material particles in the negative electrode film, so it directly affects the expansion of the negative electrode plate during cycling. During charging, lithium ions are desorbed from the positive electrode active material and inserted into the negative electrode active material, so the OI value of the negative electrode film has a significant impact on the charging speed and cycle life of lithium-ion batteries.

[0066] When the difference between OI2 and OI1 is greater than 5, the high energy and high rate properties of different active materials on the two surfaces of the negative plate can be fully utilized. Specifically, the high energy active materials have the advantages of high capacity per gram and high degree of orientation, which can further increase the energy density. In the prior art, active materials with high and low OI are mixed and used together, but mixing a low OI value with a high OI usually cannot produce good rate capability and high kinetic performance. In the present invention, active materials with high and low OI values ​​are applied to two opposing surfaces of the negative current collector, respectively, so that a combination of high kinetics and energy density can be achieved.

[0067] In some specific embodiments, the OI value OI1 of the first negative electrode film is 2-15, and preferably 4-10.

[0068] In some specific embodiments, the OI value OI2 of the second negative electrode film is 15-50, and preferably 15-40.

[0069] In some preferred embodiments, OI2-OI1 is 5-15, such as 12 or 14.

[0070] In the present invention, the first negative electrode active material and the second negative electrode active material can each independently include one or two of graphite and silicon material, where the graphite includes natural graphite or artificial graphite, and the silicon material includes at least one of silicon-carbon material or carbon-silicon-oxygen material.

[0071] It should be understood that silicon-carbon material refers to a material that contains both silicon and carbon elements. For example, silicon-carbon material has a structure in which silicon nanocrystal particles are filled into the pores of a carbon skeleton. It should be understood that silicon-oxygen-carbon material refers to a material that simultaneously contains silicon, oxygen, and carbon elements. For example, silicon-oxygen-carbon material has a structure in which silicon nanocrystal particles are dispersed in a silicon dioxide matrix to form a composite, and elemental carbon is wrapped around the outer surface of the composite.

[0072] In the present invention, based on the mass of the first negative electrode film, the mass content of the first negative electrode active material is 93% to 98%, for example, 96%.

[0073] In the present invention, based on the mass of the first negative electrode film, the first negative electrode film may further include 0.2% to 1.5% of a first negative electrode conductive agent, 1% to 3% of a first negative electrode binder, and 0.01% to 1.5% of a first negative electrode dispersant.

[0074] In the present invention, based on the mass of the second negative electrode film, the mass content of the second negative electrode active material is preferably 95% to 98.5%, for example, 95%.

[0075] In some specific embodiments, the first and second negative electrode active materials are the same in type, and the mass content of the first negative electrode active material is lower than the mass content of the second negative electrode active material. When the mass contents of the first and second negative electrode active materials satisfy the above conditions, the capacity retention rate of the battery can be effectively improved.

[0076] In the present invention, based on the mass of the second negative electrode film, the second negative electrode film may further include 0.2% to 1.5% of a second negative electrode conductive agent, 0.5% to 2% of a second negative electrode binder, and 0.01% to 1.5% of a second negative electrode dispersant.

[0077] The first negative electrode conductive agent and the second negative electrode conductive agent are reagents used to ensure that the electrodes have good charge and discharge performance, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal carbon black, conductive fibers such as carbon fibers and metal fibers, metal powders such as fluorocarbon powder, aluminum powder, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium dioxide, or polyphenylene derivatives.

[0078] The first negative electrode binder and the second negative electrode binder are components that serve to bond between the active material and the conductive agent and to combine the active material and the current collector, and can generally be selected from polyvinylidene difluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polyacrylic acid (PAA), tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers.

[0079] In the present invention, the thickness of the first negative electrode film and the thickness of the second negative electrode film may be the same as or different from each other.

[0080] In some particular embodiments, the second negative electrode film has a greater compressed density than the first negative electrode film.

[0081] In some particular embodiments, the second negative film has a greater capacity per gram than the first negative film.

[0082] In some particular embodiments, the second negative electrode film is slightly thicker than the first negative electrode film.

[0083] In the present invention, the thickness of the first negative electrode film may be 50 μm to 100 μm, preferably 50 μm to 60 μm, for example, 52 μm.

[0084] In the present invention, the thickness of the second negative electrode film may be 50 μm to 100 μm, preferably 50 μm to 60 μm, for example, 54 μm.

[0085] In some particular embodiments, the first active positive electrode material is lithium manganese iron phosphate, the second active positive electrode material is lithium nickel cobalt manganese oxide, the first active negative electrode material is synthetic graphite, and the second active negative electrode material is synthetic graphite, where OI2-OI1 is 10.

[0086] In some more specific embodiments, the first active positive electrode material is lithium manganese iron phosphate and the first positive electrode film is 91 μm thick; the second active positive electrode material is lithium nickel cobalt manganese oxide and the second positive electrode film is 47 μm thick; the first active negative electrode material is artificial graphite and the first negative electrode film is 52 μm thick; the second active negative electrode material is artificial graphite and the second negative electrode film is 54 μm thick; and OI2-OI1 is 10.

[0087] In some particular embodiments, the first active positive electrode material is lithium iron phosphate, the second active positive electrode material is lithium nickel cobalt manganese oxide, the first active negative electrode material is synthetic graphite, and the second active negative electrode material is synthetic graphite, where OI2-OI1 is 12.

[0088] In some more specific embodiments, the first active cathode material is lithium iron phosphate and the first cathode film is 76 μm thick; the second active cathode material is lithium nickel cobalt manganese oxide and the second cathode film is 47 μm thick; the first active anode material is artificial graphite and the first anode film is 52 μm thick; the second active anode material is artificial graphite and the second anode film is 54 μm thick; and OI2-OI1 is 12.

[0089] In some specific embodiments of the present invention, the surface density of the first and second negative electrode films is less than 7 mg / cm 2 ~20mg / cm 2 and preferably 8 mg / cm 2 ~12mg / cm 2 For example, 10 mg / cm 2 It is.

[0090] In the present invention, the method for preparing a negative electrode plate includes the steps of coating a raw material mixture for a first negative electrode film and a raw material mixture for a second negative electrode film on two opposing surfaces of a negative electrode current collector, respectively, to obtain a negative electrode plate.

[0091] In the present invention, the method for fabricating the cell can adopt a conventional method in the field, and generally includes the steps of rolling and slitting the positive and negative plates, and then stacking the positive plate, the separator, and the negative plate in order by a cutting, laminating, or winding process to form a cell.

[0092] electronic equipment

[0093] An electronic device according to a third aspect of the present invention includes the above-mentioned cell.

[0094] Illustratively, the electronic device of the present invention may be a mobile device (e.g., a mobile phone, a tablet computer, a laptop computer, a video camera, a portable printer / copier, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, an electric ship and satellite, an energy storage system, a backup power source, etc., but the present invention is not limited thereto.

[0095] Based on the general knowledge of the field, the above preferred conditions can be combined in any way to obtain a more excellent embodiment of the present invention.The present invention will be further described based on the following examples, but the present invention is not limited to the scope of the described examples.Any experimental method that does not have specific conditions described in the following examples can be selected based on conventional methods and conditions or based on product instructions.

[0096] Example 1

[0097] (1) Preparation of the positive electrode plate

[0098] Preparation of the raw material mixture A1 for the first positive electrode film: lithium manganese iron phosphate (LiMn 0.6 Fe 0.4 PO4), conductive agent SP, and binder PVDF were mixed in a mass ratio of 95.5:2:2.5 and thoroughly stirred with a stirrer, after which a solvent N-methylpyrrolidone with a solid content of 55% was added and stirred to homogeneously mix to prepare a first positive electrode slurry A1. 0.6 Fe 0.4 The discharge capacity per gram of PO4 was 141 mAh / g.

[0099] Preparation of raw material mixture A2 for the second positive electrode film: LiNi 0.8 Co 0.1 Mn 0.1O2, conductive agent SP, and binder PVDF were mixed in a mass ratio of 97:1.5:1.5, thoroughly stirred with a stirrer, and then a solvent N-methylpyrrolidone was added at a solid content of 60%, and the mixture was stirred to mix uniformly to prepare a second positive electrode slurry A2. 0.8 Co 0.1 Mn 0.1 The discharge capacity per gram of O2 was 198 mAh / g.

[0100] The raw material mixture A1 for the first positive electrode film and the raw material mixture A2 for the second positive electrode film were mixed at 22 mg / cm 2 After uniformly applying the coating to the current collector at a surface density of 1000 ppm, the coating was dried in a coating dryer to prepare a positive electrode plate of a specified size.

[0101] (2) Preparation of negative electrode plate

[0102] Preparation of raw material mixture B1 for the first negative electrode film: artificial graphite, conductive agent SP, binder SBR+PAA, and dispersant CMC were mixed in a mass ratio of 96:1:2:1 and thoroughly stirred with a stirrer. Then, a solvent N-methylpyrrolidone or sterile water with a solid content of 58% was added and stirred to mix uniformly to prepare the first negative electrode slurry B1.

[0103] Preparation of raw material mixture B2 for the second negative electrode film: artificial graphite, conductive agent SP, binder SBR+PAA, and dispersant CMC were mixed in a mass ratio of 95:1.5:2.5:1, thoroughly stirred with a stirrer, and then a solvent N-methylpyrrolidone or sterile water with a solid content of 56% was added and stirred to mix uniformly to prepare the second negative electrode slurry B2.

[0104] The raw material mixture B1 for the first negative electrode film and the raw material mixture B2 for the second negative electrode film were each formed at a concentration of 10 mg / cm 2 The first and second negative electrode films were then processed using a coating dryer to produce negative electrode plates of the specified size. The orientation degree OI1 of the first negative electrode film was 8, and the orientation degree OI2 of the second negative electrode film was 18.

[0105] (3) Preparation of electrolyte:

[0106] The organic solvent was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), with a volume ratio of EC, EMC, and DEC of 20:20:60. In an argon atmosphere glove box with a humidity of <10 ppm, a sufficiently dried lithium salt (LiPF6) was dissolved in the above organic solvent and mixed uniformly to obtain an electrolyte with a LiPF6 concentration of 1 mol / L.

[0107] (4) Preparation of separator: A polypropylene separator with a thickness of 12 μm was selected.

[0108] (5) Assembly of cell and lithium-ion battery: The positive electrode plate, the negative electrode plate, and the separator were rolled-slit and cut-laminate to prepare a cell. Then, the bare cell JR was placed in the shell and sufficiently baked so that the humidity was 450 ppm or less, and a rectangular hard-shell lithium-ion battery was prepared by carrying out processes including electrolyte injection, battery formation, sealing, and inspection. The structure of the assembled cell is as shown in FIG. 1 and FIG. 2, in which the first negative electrode film 7 and the second negative electrode film 6 are provided on the two opposing surfaces of the negative electrode collector 1, respectively, and the first positive electrode film 5 and the second positive electrode film 4 are provided on the two opposing surfaces of the positive electrode collector 2, respectively. In addition, the first positive electrode film 5 and the second negative electrode film 6 are adjacent to each other via the separator 3, and the second positive electrode film 4 and the first negative electrode film 7 are adjacent to each other via the separator 3.

[0109] Example 2

[0110] The first positive electrode active material in the raw mixture of the first positive electrode film was replaced with lithium iron phosphate (LiFePO4), where the discharge capacity per gram of LiFePO4 at a current density of 0.1C was 157mAh / g.

[0111] The orientation degree OI of the first negative electrode film was 8, and the orientation degree OI of the second negative electrode film was 20.

[0112] The other ingredients and preparation method were the same as in Example 1.

[0113] Comparative Example 1

[0114] Both the first and second positive electrode films of the positive electrode plate were fabricated by coating the raw material mixture A1 of the first positive electrode film of Example 1.

[0115] Both the first and second negative electrode films of the negative electrode plate were prepared by applying the raw material mixture B2 of the second negative electrode film of Example 1, and the orientation degrees OI of the first and second negative electrode films were both 18.

[0116] The other ingredients and preparation method were the same as in Example 1.

[0117] Comparative Example 2

[0118] Both the first and second positive electrode films of the positive electrode plate were fabricated by coating the raw material mixture A2 of the second positive electrode film of Example 1.

[0119] Both the first negative electrode film and the second negative electrode film of the negative electrode plate were produced by applying the raw material mixture B1 of the first negative electrode film of Example 1, and the orientation degrees OI of the first negative electrode film and the second negative electrode film were both 8.

[0120] The other ingredients and preparation method were the same as in Example 1.

[0121] Comparative Example 3

[0122] A first negative electrode film was produced by applying raw material mixture B2 for the second negative electrode film of Example 1, and a second negative electrode film was produced by applying raw material mixture B1 for the first negative electrode film of Example 1. The orientation degree OI of the first negative electrode film was 18, and the orientation degree OI of the second negative electrode film was 8.

[0123] The other ingredients and preparation method were the same as in Example 1.

[0124] Comparative Example 4

[0125] The first negative electrode film was produced by applying the raw material mixture B2 for the second negative electrode film of Example 1. The first negative electrode film had an orientation degree OI of 18.

[0126] The orientation degree OI of the second negative electrode film was 20.

[0127] The other ingredients and preparation method were the same as in Example 1.

[0128] Comparative Example 5

[0129] Both the first and second positive electrode films of the positive electrode plate were fabricated by coating the raw material mixture A1 of the first positive electrode film of Example 1.

[0130] The orientation degree OI of the first negative electrode film was 18, and the orientation degree OI of the second negative electrode film was 7.

[0131] The other ingredients and preparation method were the same as in Example 1.

[0132] Comparative Example 6

[0133] Both the first and second negative electrode films of the negative electrode plate were prepared by applying the raw material mixture B2 of the second negative electrode film of Example 1, and the orientation degrees OI of the first and second negative electrode films were both 18.

[0134] The rest was the same as in Example 1.

[0135] The thicknesses of the films in Examples 1 and 2 and Comparative Examples 1 to 6 are as shown in Table 1.

[0136] [Table 1]

[0137] Demonstration example 1

[0138] The batteries produced in Examples 1 and 2 and Comparative Examples 1 to 6 were tested for capacity retention after 0 to 1000 cycles under conditions of 45° C. and a charge or discharge voltage of 1 C. The results are shown in Table 2.

[0139] [Table 2]

[0140] [Table 3]

[0141] As can be seen from Tables 2 and 3, the present invention provides a reasonable matching between the positive and negative electrode materials. Under these matching conditions, the batteries prepared in Examples 1 and 2 have the advantages of high energy density and excellent cycling performance. Specifically, the energy density can reach 246wh / kg or more, and the capacity retention rate after 1000 cycles can reach 90.32% or more.

[0142] Comparing Example 1 and Comparative Example 1, Comparative Example 1 used the same first and second positive electrode films, both of which were phosphate positive electrodes, and also used the same first and second negative electrode films, both of which were negative electrodes with high OI values. As can be seen from this, Comparative Example 1 had the same capacity retention as Example 1, but its energy density was lower than that of Example 1, being only 193wh / kg.

[0143] Comparing Example 1 and Comparative Example 2, Comparative Example 2 used the same first and second positive electrode films, both of which were 8-series high nickel ternary positive electrodes, and also used the same first and second negative electrode films, both of which were negative electrodes with low OI values. As can be seen from this, Comparative Example 2 maintained the high energy density characteristics of the positive electrode material, but the capacity retention rate after 1000 cycles was only 85.22%, lower than that of Example 1.

[0144] Comparing Example 1 and Comparative Example 3, in Comparative Example 3, the first negative electrode film (low OI value) was adjacent to the first positive electrode film, and the second negative electrode film (high OI value) was adjacent to the second positive electrode film. The energy density was comparable to that of Example 1, but the cycling stability was lower than that of Example 1.

[0145] Comparing Example 1 with Comparative Example 4, the first and second negative electrode films in Comparative Example 4 both adopted negative electrode materials with high OI values, and the difference between OI2 and OI1 was 2. As a result, the capacity retention after 1000 cycles was 90.1%, and the energy density was 248wh / kg.

[0146] Comparing Example 1 and Comparative Example 5, the first and second positive electrode films in Comparative Example 5 both use the same phosphate positive electrode material, and the energy density is only 191wh / kg, and the capacity retention rate after 1000 cycles is only 89.5%, both of which are lower than those of Example 1.

[0147] Comparing Example 1 and Comparative Example 6, in Comparative Example 6, the first and second negative electrode films both adopted the same negative electrode material with a high OI value, and the difference of OI2-OI1 was 0. Its energy density was equivalent to that of Example 1, but its cycling stability was lower than that of Example 1, with the capacity retention rate after 1000 cycles being only 87.62%.

[0148] As can be seen from the above comparison, the special matching relationship between the positive and negative electrode materials of the present invention produces excellent energy density and cycling performance.

[0149] Demonstration example 2

[0150] For the batteries produced in Examples 1 to 2, Comparative Example 1, Comparative Example 2, and Comparative Example 6, the negative electrodes of the cells were disassembled after 1000 cycles under conditions of 45° C. and a charge or discharge voltage of 1 C, and an ICP test analysis was performed. The results are shown in Table 4.

[0151] [Table 4]

[0152] As can be seen from Table 4, the cells made from Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 6 also had different ICP test element distributions after cycling. After 1000 cycles, there was Co and Ni on the negative plate, suggesting that the material used in the positive electrode contained nickel, cobalt, and manganese. [Industrial Applicability]

[0153] The cell provided by the present invention can be applied to a secondary battery.

[0154] The above specific embodiments further describe the objectives, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention, and is not intended to limit the present invention. Any modifications, equivalent replacements, changes, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention. [Explanation of symbols]

[0155] 1 Negative electrode current collector 2 Positive electrode current collector 3. Separator 4. Second positive electrode film 5 First positive electrode film 6 Second negative electrode film 7 First negative electrode film

Claims

1. A cell comprising positive and negative electrode plates alternately arranged along a thickness direction of the cell, and a separator provided between the positive and negative electrode plates, the positive plate includes a positive current collector, a first positive film, and a second positive film, the first positive film and the second positive film being disposed on two opposing surfaces of the positive current collector, respectively, the first positive film includes a first positive active material including a phosphate material, and the second positive film includes a second positive active material having a capacity per gram greater than a capacity per gram of the first positive active material; The negative plate includes a negative current collector, a first negative film, and a second negative film, the first negative film and the second negative film being disposed on two opposing surfaces of the negative current collector, respectively, the first negative film includes a first negative active material, and the second negative film includes a second negative active material; and 2 -OI 1 >5 and OI 2 is the OI value of the second negative electrode film, and OI 1 is the OI value of the first negative electrode film.

2. 2. The cell of claim 1 , wherein the first positive film is adjacent to the second negative film through the separator, and the second positive film is adjacent to the first negative film through the separator.

3. 2. The cell of claim 1, wherein a thickness ratio of the first positive electrode film to the second positive electrode film is (1.1-2.5):

1.

4. The first positive electrode active material and the second positive electrode active material are a. the phosphate material is lithium iron phosphate and / or lithium manganese iron phosphate; b. the second positive electrode active material comprises one or more of lithium manganate, lithium cobalt oxide, lithium nickelate, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium-rich lithium manganese-based materials; c. The first positive electrode active material has a discharge capacity per gram of 127 Ah / g to 160 mAh / g at a current density of 0.1 C; d. The discharge capacity per gram of the second positive electrode active material at a current density of 0.1 C is 180 Ah / g to 210 mAh / g; The cell of claim 1 , which satisfies one or more of the following conditions:

5. The first positive electrode active material and the second positive electrode active material are e. the mass content of the first positive electrode active material is 92% to 97% based on the mass of the first positive electrode film; f. The mass content of the second positive electrode active material is 94% to 98% based on the mass of the two positive electrode films; g. The mass content of the second positive electrode active material is greater than the mass content of the first positive electrode active material; The cell of claim 1 , which satisfies one or more of the following conditions:

6. The first negative electrode film and the second negative electrode film are a. OI value of the first negative electrode film 1 But it is 2 to 15, b. The OI value of the second negative electrode film 2 However, it is between 15 and 50, c. OI 2 -OI 1 But it is 5 to 15, The cell of claim 1 , which satisfies one or more of the following conditions:

7. 10. The cell of claim 1 , wherein the first and second anode active materials each independently comprise one or both of a graphite and a silicon material.

8. The thickness of the first negative electrode film and the thickness of the second negative electrode film are a. the thickness of the first negative electrode film and the thickness of the second negative electrode film are the same or different from each other; b. the first negative electrode film and the second negative electrode film have a thickness of 50 μm to 100 μm; The cell of claim 1 , which satisfies at least one of the following conditions:

9. The mass content of the first negative electrode active material is 93% to 98% based on the mass of the first negative electrode film; 10. The cell of claim 1, wherein a mass content of the second negative electrode active material is 95% to 98.5%, based on the mass of the second negative electrode film.

10. An electronic device comprising the cell according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Pole piece and pole piece assembly

    CN216213552U

  • Electrode assembly, secondary battery, battery module, battery pack, and power consumption device

    JP2023550218A

  • KR20210039599A