Semiconductor device
The semiconductor device design with controlled tantalum and nitrogen layers enhances electrical performance, on-state current, and reliability, addressing challenges of miniaturization and integration while reducing power consumption.
Patent Information
- Application Number
- JP2024062675
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-25
AI Technical Summary
Existing semiconductor devices face challenges in achieving good electrical characteristics, large on-state current, reduced variation in electrical characteristics, high reliability, miniaturization, and low power consumption.
A semiconductor device configuration with specific layers and materials, including a first conductive layer, an oxide semiconductor layer, and conductive layers containing tantalum and nitrogen, with controlled abundance ratios and crystal orientations, to enhance electrical performance and reliability.
The configuration provides a semiconductor device with improved electrical characteristics, large on-state current, reduced variation in transistor characteristics, high reliability, and potential for miniaturization and integration, while maintaining low power consumption.
Smart Images

Figure 2024152667000001_ABST
Abstract
Description
[Technical Field]
[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, a display device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device.
[0002] One embodiment of the present invention is not limited to the above technical field. Examples of the technical field of one embodiment of the present invention include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, an input device (for example, a touch sensor), an input / output device (for example, a touch panel), a driving method thereof, or a manufacturing method thereof.
[0003] In this specification and the like, a semiconductor device is a device that utilizes semiconductor characteristics, and refers to a semiconductor element (transistor, diode, photodiode, etc.), a circuit including a semiconductor element, a device having a circuit including a semiconductor element, etc. It also refers to any device that can function by utilizing semiconductor characteristics. For example, an integrated circuit, a chip including an integrated circuit, and an electronic component in which a chip is housed in a package are examples of semiconductor devices. Furthermore, memory devices, display devices, light-emitting devices, lighting devices, and electronic devices may themselves be semiconductor devices and each may have a semiconductor device. [Background technology]
[0004] In recent years, semiconductor devices have been developed and are mainly used in LSIs (Large Scale Integration), CPUs (Central Processing Units), memories, etc. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors) processed from semiconductor wafers and formed into chips, and on which electrodes serving as connection terminals are formed.
[0005] 2. Description of the Related Art Semiconductor circuits (IC (Integrated Circuit) chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as components in a variety of electronic devices.
[0006] Furthermore, technology for constructing transistors using semiconductor thin films formed on substrates with insulating surfaces has attracted attention. Such transistors are widely used in electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). Silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, but oxide semiconductors have also attracted attention as other materials.
[0007] Furthermore, transistors using oxide semiconductors are known to have extremely low leakage current in a non-conducting state. For example, Patent Document 1 discloses a low-power consumption CPU that utilizes the low leakage current characteristic of transistors using oxide semiconductors. Furthermore, for example, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the low leakage current characteristic of transistors using oxide semiconductors.
[0008] Furthermore, in recent years, with the trend toward smaller and lighter electronic devices, there has been an increasing demand for higher density integrated circuits, and there is also a demand for improved productivity in semiconductor devices including integrated circuits. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 2012-257187 [Patent Document 2] Japanese Patent Application Laid-Open No. 2011-151383 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of one embodiment of the present invention is to provide a semiconductor device having favorable electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device having large on-state current.An object of one embodiment of the present invention is to provide a semiconductor device in which variation in electrical characteristics of transistors is small.An object of one embodiment of the present invention is to provide a semiconductor device with favorable reliability.An object of one embodiment of the present invention is to provide a semiconductor device that can be miniaturized or highly integrated.An object of one embodiment of the present invention is to provide a semiconductor device with low power consumption.
[0011] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these will become apparent from the description of the specification, drawings, claims, etc., and it is possible to extract other problems from the description of the specification, drawings, claims, etc. [Means for solving the problem]
[0012] One embodiment of the present invention is a semiconductor device including a first conductive layer, a first insulating layer over the first conductive layer, an oxide semiconductor layer over the first insulating layer, a second conductive layer, a third conductive layer, and a second insulating layer over the oxide semiconductor layer, a third insulating layer over the second conductive layer and the third conductive layer, and a fourth conductive layer over the second insulating layer. The third insulating layer has an opening that reaches the oxide semiconductor layer. The second insulating layer and the fourth conductive layer are disposed in the opening. The height of the top surface of the third insulating layer is equal to the height of the top surface of the fourth conductive layer. The second conductive layer and the third conductive layer each contain tantalum and nitrogen. In each of the second conductive layer and the third conductive layer, the abundance ratio of tantalum in the first bonding state is 3% or less and the abundance ratio of tantalum in the second bonding state is 5% or more. The first bonding state is a bonding state of metal tantalum and a bonding state of tantalum nitride in which the nitrogen content per tantalum is stoichiometrically low. The second bonding state is that of tantalum nitride, which has stoichiometric nitrogen per tantalum.
[0013] In the semiconductor device, the abundance ratio of the first bonding state and the abundance ratio of the second bonding state are preferably calculated by performing a waveform analysis of an XPS spectrum of tantalum 4f obtained by X-ray photoelectron spectroscopy.
[0014] In the above-mentioned semiconductor device, it is preferable that each of the second conductive layer and the third conductive layer has, in an XRD spectrum, a first peak having a peak position in the range of 2θ=35.5±1.0 degrees and a second peak having a peak position in the range of 2θ=41.2±2.0 degrees, and that the ratio of the peak height of the second peak to the peak height of the first peak is 0.2 or more and 1.0 or less.
[0015] In the above semiconductor device, the oxide semiconductor layer preferably contains one or both of indium and zinc.
[0016] One embodiment of the present invention is a semiconductor device including a first conductive layer, a first insulating layer over the first conductive layer, an oxide semiconductor layer over the first insulating layer, a second conductive layer, a third conductive layer, and a second insulating layer over the oxide semiconductor layer, a third insulating layer over the second conductive layer and the third conductive layer, and a fourth conductive layer over the second insulating layer. The third insulating layer has an opening that reaches the oxide semiconductor layer. The second insulating layer and the fourth conductive layer are disposed in the opening. The height of the top surface of the third insulating layer is equal to the height of the top surface of the fourth conductive layer. In an XRD spectrum, each of the second conductive layer and the third conductive layer has a first peak having a peak position in a range of 2θ = 35.5 ± 1.0 degrees and a second peak having a peak position in a range of 2θ = 41.2 ± 2.0 degrees. The ratio of the peak height of the second peak to the peak height of the first peak is 0.2 to 1.0.
[0017] In the above semiconductor device, each of the second conductive layer and the third conductive layer preferably contains tantalum and nitrogen.
[0018] In the above semiconductor device, the oxide semiconductor layer preferably contains one or both of indium and zinc. [Effects of the Invention]
[0019] According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device having large on-state current can be provided. According to one embodiment of the present invention, a semiconductor device in which variation in electrical characteristics of transistors is reduced can be provided. According to one embodiment of the present invention, a semiconductor device with favorable reliability can be provided. According to one embodiment of the present invention, a semiconductor device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a semiconductor device with low power consumption can be provided.
[0020] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc. [Brief explanation of the drawings]
[0021] [Figure 1] Fig. 1A is a plan view showing an example of a semiconductor device, and Figs. 1B to 1D are cross-sectional views showing an example of the semiconductor device. [Figure 2] 2A and 2B are cross-sectional views showing an example of a semiconductor device. [Figure 3] FIG. 3 is a cross-sectional view showing an example of a semiconductor device. [Figure 4] 4A and 4B are cross-sectional views showing an example of a semiconductor device. [Figure 5] 5(A) and 5(B) are cross-sectional views showing an example of a semiconductor device. [Figure 6] Fig. 6(A) is a plan view showing an example of a semiconductor device, and Fig. 6(B) is a cross-sectional view showing an example of a semiconductor device. [Figure 7] FIG. 7 is a cross-sectional view showing an example of a semiconductor device. [Figure 8] 8A is a block diagram illustrating a configuration example of a storage device according to one embodiment of the present invention, and FIG. 8B is a perspective view illustrating a configuration example of a storage device according to one embodiment of the present invention. [Figure 9] 9A to 9I are circuit diagrams illustrating configuration examples of memory cells according to one embodiment of the present invention. [Figure 10] FIG. 10 is a cross-sectional view showing an example of a storage device. [Figure 11] FIG. 11 is a cross-sectional view showing an example of a storage device. [Figure 12] 12(A) and 12(B) are diagrams showing an example of an electronic component. [Figure 13] 13(A) and 13(B) are diagrams showing an example of an electronic device, and FIGS. 13(C) to 13(E) are diagrams showing an example of a mainframe computer. [Figure 14] FIG. 14 is a diagram illustrating an example of space equipment. [Figure 15] FIG. 15 is a diagram illustrating an example of a storage system that can be applied to a data center. [Figure 16] 16(A) to 16(C) are cross-sectional schematic diagrams of samples according to the example. [Figure 17] 17(A) to 17(C) are XPS spectra according to the example. [Figure 18] 18(A) to 18(H) are XPS spectra according to the example. [Figure 19] FIG. 19 shows the results of XPS analysis according to the example. [Figure 20] FIG. 20 is a diagram showing the resistivity of a tantalum nitride film according to an example. [Figure 21] FIG. 21 is a diagram showing the relationship between conductivity and chemical shift value according to an example. [Figure 22] FIG. 22 shows the results of XRD analysis according to the example. [Figure 23] FIG. 23 shows the results of XRD analysis according to the example. [Figure 24]FIG. 24 shows the results of XRD analysis according to the example. [Figure 25] FIG. 25 shows the results of D-SIMS analysis according to the example. [Figure 26] 26(A) to 26(H) are cross-sectional STEM images of the sample according to the example. [Figure 27] 27(A) and 27(B) are cross-sectional STEM images of the sample according to the example. [Figure 28] 28(A) and 28(B) are diagrams showing the results of EDX analysis according to the example. [Figure 29] Figures 29(A) and 29(B) are cross-sectional STEM images of the sample according to the example, and Figures 29(C) to 29(F) are EDX maps of the sample according to the example. [Figure 30] 30(A) to 30(D) are UPS spectra according to the example. [Figure 31] 31(A) to 31(D) are UPS spectra according to the example. [Figure 32] 32(A) to 32(C) are UPS spectra according to the example. [Figure 33] Fig. 33(A) is a diagram illustrating a Tauc plot according to an example, and Fig. 33(B) is an absorption spectrum according to an example. [Figure 34] 34(A) to 34(C) are diagrams illustrating Tauc plots according to an embodiment. [Figure 35] 35A to 35D show the Id-Vg characteristics of the transistors fabricated in this example. [Figure 36] 36A to 36D show the Id-Vg characteristics of the transistors fabricated in this example. [Figure 37] FIG. 37 is a diagram showing the resistivity of a tantalum nitride film according to an example. [Figure 38] FIG. 38 is a diagram showing the results of the TLM method according to the example. [Figure 39]Fig. 39(A) is a diagram showing the relationship between contact conductance and chemical shift value according to an example, and Fig. 39(B) is a result of XPS analysis according to an example. DETAILED DESCRIPTION OF THE INVENTION
[0022] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes can be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0023] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and repeated explanations thereof will be omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be assigned.
[0024] Furthermore, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.
[0025] In this specification, the ordinal numbers "first" and "second" are used for convenience and do not limit the number of components or the order of the components (for example, the order of processes or the order of stacking). Furthermore, the ordinal numbers attached to components in one part of this specification may not match the ordinal numbers attached to the same components in other parts of this specification or in the claims.
[0026] A transistor is a type of semiconductor element that can perform functions such as amplifying current or voltage and performing switching operations to control conduction or non-conduction. The term "transistor" as used herein includes an IGFET (Insulated Gate Field Effect Transistor) and a TFT (Thin Film Transistor).
[0027] In this specification and the like, a transistor using an oxide semiconductor or a metal oxide for a semiconductor layer and a transistor having an oxide semiconductor or a metal oxide for a channel formation region may be referred to as an OS transistor. A transistor having silicon for a channel formation region may be referred to as a Si transistor.
[0028] In this specification and the like, a transistor is an element having at least three terminals including a gate, a drain, and a source. A region (also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode) is provided, and a current can flow between the source and the drain through the channel formation region. In this specification and the like, the channel formation region refers to a region through which a current mainly flows.
[0029] Furthermore, the functions of "source" and "drain" may be interchangeable when transistors of different polarities are used, or when the direction of current flow changes during circuit operation, etc. For this reason, the terms "source" and "drain" may be used interchangeably in this specification.
[0030] Note that impurities in a semiconductor refer to, for example, elements other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity. The presence of impurities can, for example, increase the density of defect states in the semiconductor or reduce the crystallinity. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specific examples include hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water can also function as an impurity. For example, the inclusion of impurities can cause oxygen deficiency (V O (also referred to as "interstitial space") may be formed.
[0031] In this specification and the like, an oxynitride refers to a material having a composition in which oxygen is contained in a larger amount than nitrogen, and a nitride oxide refers to a material having a composition in which nitrogen is contained in a larger amount than oxygen.
[0032] To analyze the content of elements such as hydrogen, oxygen, carbon, and nitrogen contained in a film, for example, secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) can be used. XPS is suitable when the content of the target element is high (e.g., 0.5 atomic% or more, or 1 atomic% or more). On the other hand, SIMS is suitable when the content of the target element is low (e.g., 0.5 atomic% or less, or 1 atomic% or less). When comparing the content of elements, it is more preferable to perform a combined analysis using both SIMS and XPS analytical techniques.
[0033] The terms "film" and "layer" can be interchangeable depending on the circumstances. For example, the term "conductive layer" can be changed to the term "conductive film." Or, for example, the term "insulating film" can be changed to the term "insulating layer."
[0034] Furthermore, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes cases in which the angle is -5 degrees or more and 5 degrees or less. Furthermore, "substantially parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. Furthermore, "perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes cases in which the angle is 85 degrees or more and 95 degrees or less. Furthermore, "substantially perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.
[0035] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes or wiring, as well as switching elements such as transistors, resistive elements, coils, and other elements with various functions.
[0036] In this specification, unless otherwise specified, the off-state current refers to the leakage current between the source and drain when the transistor is in the off state (also called the non-conducting state or the cut-off state). Unless otherwise specified, the off-state current refers to the leakage current between the source and the gate when the voltage V gs is the threshold voltage V th (For p-channel transistors, V th This refers to a state of being (higher than)
[0037] In this specification, "normally on" refers to a state in which a channel exists and current flows through a transistor even when no voltage is applied to the gate, and "normally off" refers to a state in which no current flows through a transistor when no potential is applied to the gate or when a ground potential is applied to the gate.
[0038] In this specification, the term "leakage current" may be used to mean the same thing as "off-state current." In this specification, the term "off-state current" may refer to, for example, a current that flows between the source and drain of a transistor when the transistor is in an off state.
[0039] In this specification, the top surface shape of a certain component refers to the contour shape of the component in a plan view. The plan view refers to a view from the normal direction of the surface on which the component is formed or the surface of the support (e.g., substrate) on which the component is formed.
[0040] In this specification, the phrase "top surface shapes that are approximately the same" refers to at least a portion of the contours of stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer. In these cases, the phrase "top surface shapes that are approximately the same" may also be used. Furthermore, when the top surface shapes are the same or approximately the same, it can also be said that the positions in plan view are the same or approximately the same, the edges are aligned or approximately aligned, or the side edges are aligned or approximately the same.
[0041] In this specification, "equal heights" refers to a configuration in which the heights from a reference surface (e.g., a flat surface such as a substrate surface) are equal in cross-sectional view. For example, in the manufacturing process of a semiconductor device, a planarization process (typically a CMP process) may be performed to expose the surface of a single layer or multiple layers. In this case, the surfaces processed by the CMP process are configured to have the same height from the reference surface. However, the heights of multiple layers may differ depending on the processing equipment, processing method, or material of the processed surface during the CMP process. In this specification, this case is also considered to be "equal heights." For example, in the case of a structure having two layers (here, a first layer and a second layer) with different heights relative to the reference surface, the difference in height between the top surface of the first layer and the top surface of the second layer is 20 nm or less, this is also considered to be "equal heights."
[0042] Generally, it is difficult to clearly distinguish between an "exact match" and an "approximate match." For this reason, in this specification, "match" includes both an exact match and an approximate match.
[0043] The openings include, for example, grooves, slits, etc. Furthermore, the area in which the openings are formed may be referred to as an opening portion.
[0044] Although the drawings used in this embodiment mode show the case where the sidewall of the insulating layer in the opening portion of the insulating layer is approximately perpendicular to the substrate surface or the surface where the insulating layer is formed, the sidewall may have a tapered shape.
[0045] In this specification and the like, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined with respect to the substrate surface or the surface to be formed. For example, there is a region in which the angle (also called the taper angle) between the inclined side surface and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. Note that the side surface of the structure, the substrate surface, and the surface to be formed do not necessarily need to be completely flat, and may be approximately planar with a slight curvature or approximately planar with a slight unevenness.
[0046] In this specification and the like, when it is stated that A is in contact with B, it means that at least a part of A is in contact with B. Therefore, for example, it can be rephrased as saying that A has a region in contact with B.
[0047] In this specification and the like, when it is stated that A is located on B, it means that at least a part of A is located on B. Therefore, for example, it can be rephrased as, A has a region located on B.
[0048] In this specification and the like, when it is stated that A covers B, it means that at least a part of A covers B. Therefore, for example, it can be rephrased as saying that A has a region that covers B.
[0049] In this specification and the like, when it is stated that A overlaps with B, it means that at least a portion of A overlaps with B. Therefore, for example, it can be rephrased as saying that A has a region that overlaps with B.
[0050] In this specification and the like, the term "step discontinuity" refers to a phenomenon in which a layer, film, or electrode is divided due to the shape of the surface on which it is formed (for example, a step or the like).
[0051] (Embodiment 1) In this embodiment, a structural example of a semiconductor device according to one embodiment of the present invention will be described with reference to Figures 1A to 7. Note that the semiconductor device according to one embodiment of the present invention includes a transistor.
[0052] <Configuration example of semiconductor device> The structure of a semiconductor device including a transistor 200 will be described with reference to FIGS. 1A to 1D. FIG. 1A is a plan view of the semiconductor device, and FIGS. 1B to 1D are cross-sectional views of the semiconductor device. FIG. 1B is a cross-sectional view of a portion indicated by a dashed-dotted line A1-A2 in FIG. 1A, and is also a cross-sectional view of the transistor 200 in the channel length direction. FIG. 1C is a cross-sectional view of a portion indicated by a dashed-dotted line A3-A4 in FIG. 1A, and is also a cross-sectional view of the transistor 200 in the channel width direction. FIG. 1D is a cross-sectional view of a portion indicated by a dashed-dotted line A5-A6 in FIG. 1A. Note that some elements are omitted from the plan view of FIG. 1A for clarity.
[0053] A semiconductor device of one embodiment of the present invention includes an insulating layer 214 over a substrate (not shown), a transistor 200 over the insulating layer 214, an insulating layer 280 over the transistor 200, an insulating layer 282 over the insulating layer 280, and an insulating layer 283 over the insulating layer 282. The insulating layer 214, the insulating layer 280, the insulating layer 282, and the insulating layer 283 function as interlayer films.
[0054] 1A to 1D, the transistor 200 includes an insulating layer 216 over an insulating layer 214, a conductive layer 215 embedded in the insulating layer 216, an insulating layer 222 over the insulating layer 216 and the conductive layer 215, an insulating layer 224 over the insulating layer 222, an oxide semiconductor layer 230 over the insulating layer 224, a conductive layer 242a and a conductive layer 242b over the oxide semiconductor layer 230, an insulating layer 271a over the conductive layer 242a, an insulating layer 271b over the conductive layer 242b, an insulating layer 250 over the oxide semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. An insulating layer 275 is provided over the insulating layer 271a and the insulating layer 271b, and an insulating layer 280 is provided over the insulating layer 275.
[0055] In the following, the conductive layer 242a and the conductive layer 242b may be collectively referred to as the conductive layer 242. Furthermore, the insulating layer 271a and the insulating layer 271b may be collectively referred to as the insulating layer 271.
[0056] The insulating layer 280 and the insulating layer 275 have openings that reach the oxide semiconductor layer 230. The insulating layer 250 and the conductive layer 260 are disposed in the openings. In addition, in the channel length direction of the transistor 200, the conductive layer 260 and the insulating layer 250 are provided between the insulating layer 271a and the conductive layer 242a and between the insulating layer 271b and the conductive layer 242b.
[0057] The conductive layer 260 is formed in a self-aligned manner so as to fill the openings formed in the insulating layer 280 and the insulating layer 275. By forming the conductive layer 260 in this manner, the conductive layer 260 can be reliably positioned in the region between the conductive layer 242a and the conductive layer 242b without alignment.
[0058] As shown in FIGS. 1B and 1C, the height of the upper surface of the conductive layer 260 is the same as the height of the upper surface of the insulating layer 280.
[0059] In the transistor 200, the conductive layer 260 functions as a first gate (also referred to as a top-gate) electrode, and the conductive layer 215 functions as a second gate (also referred to as a back-gate) electrode. The insulating layer 250 functions as a first gate insulating layer, and the insulating layers 222 and 224 function as second gate insulating layers. Note that a gate insulating layer may also be referred to as a gate insulating film. The conductive layer 242a functions as one of a source electrode and a drain electrode, and the conductive layer 242b functions as the other of the source electrode and the drain electrode. At least part of a region of the oxide semiconductor layer 230 that overlaps with the conductive layer 260 functions as a channel formation region.
[0060] The conductive layer 215 is disposed so as to overlap with the oxide semiconductor layer 230 and the conductive layer 260. Here, the conductive layer 215 is provided to be embedded in an opening formed in the insulating layer 216. Note that part of the conductive layer 215 is sometimes embedded in the insulating layer 214.
[0061] The conductive layer 215 may function as a second gate electrode. In this case, the potential applied to the conductive layer 215 may be changed independently of the potential applied to the conductive layer 260, thereby controlling the threshold voltage V th In particular, applying a negative potential to conductive layer 215 can control the V th Therefore, when a negative potential is applied to the conductive layer 215, the drain current when the potential applied to the conductive layer 260 is 0 V can be made smaller than when no negative potential is applied.
[0062] As shown in FIG. 1A, the conductive layer 215 is preferably larger than a region of the oxide semiconductor layer 230 that does not overlap with the conductive layers 242a and 242b. In particular, as shown in FIG. 1C, the conductive layer 215 preferably extends to a region outside the end portion of the oxide semiconductor layer 230 in the channel width direction. That is, the conductive layer 215 and the conductive layer 260 preferably overlap with each other with an insulating layer interposed therebetween on the outside of the side surface of the oxide semiconductor layer 230 in the channel width direction. With this structure, the channel formation region of the oxide semiconductor layer 230 can be electrically surrounded by the electric field of the conductive layer 260 functioning as the first gate electrode and the electric field of the conductive layer 215 functioning as the second gate electrode. In this specification, a transistor structure in which the channel formation region is electrically surrounded by at least the electric field of the first gate electrode is referred to as a surrounded channel (S-channel) structure.
[0063] In this specification, a transistor with an S-channel structure refers to a transistor structure in which a channel formation region is electrically surrounded by the electric fields of one and the other of a pair of gate electrodes. The S-channel structure disclosed in this specification is different from the fin structure and the planar structure. On the other hand, the S-channel structure disclosed in this specification can also be considered a type of fin structure. In this specification, a fin structure refers to a structure in which the gate electrode is disposed so as to surround at least two sides of the channel (specifically, two, three, or four sides, etc.). By employing the fin structure and the S-channel structure, resistance to the short channel effect can be increased, in other words, a transistor that is less susceptible to the short channel effect can be obtained.
[0064] By forming the transistor 200 with the S-channel structure, the channel formation region can be electrically surrounded. Note that the S-channel structure electrically surrounds the channel formation region, and therefore can be considered to be substantially equivalent to a GAA (Gate All Around) structure or a LGAA (Lateral Gate All Around) structure. By forming the transistor 200 with the S-channel structure, the GAA structure, or the LGAA structure, the channel formation region formed at or near the interface between the oxide semiconductor layer 230 and the gate insulating layer can be the entire bulk of the oxide semiconductor layer 230. Therefore, the density of the current flowing through the transistor can be improved, which is expected to improve the on-state current or the field-effect mobility of the transistor.
[0065] 1C, the conductive layer 215 is extended to function as a wiring. However, the present invention is not limited to this, and a conductor functioning as a wiring may be provided under the conductive layer 215. Furthermore, it is not necessary to provide one conductive layer 215 for each transistor. For example, the conductive layer 215 may be shared by a plurality of transistors.
[0066] 1C , in the channel width direction of the transistor 200, the height of the bottom surface of the conductive layer 260 in a region that does not overlap with the oxide semiconductor layer 230, relative to the insulating layer 222, is preferably lower than the height of the bottom surface of the oxide semiconductor layer 230. When the conductive layer 260 functioning as a gate electrode covers the side surfaces and the top surface of the channel formation region of the oxide semiconductor layer 230, the electric field of the conductive layer 260 can be easily applied to the entire channel formation region of the oxide semiconductor layer 230. Therefore, the on-state current of the transistor 200 can be increased, and the frequency characteristics can be improved.
[0067] 1C , the oxide semiconductor layer 230 may have a curved surface between the side surface and the top surface in a cross-sectional view in the channel width direction of the transistor 200. With such a shape, coverage of the oxide semiconductor layer 230 with the insulating layer 250 and the conductive layer 260 can be improved.
[0068] The transistor 200 includes a metal oxide (also referred to as an oxide semiconductor) functioning as a semiconductor in the oxide semiconductor layer 230 including a channel formation region. That is, the transistor 200 can be said to be an OS transistor.
[0069] The semiconductor device according to this embodiment includes an OS transistor. The OS transistor has a small off-state current, which allows a semiconductor device with low power consumption to be realized. Furthermore, the OS transistor has high frequency characteristics, which allows a semiconductor device with high operating speed to be realized. Furthermore, by using an OS transistor, a semiconductor device with favorable electrical characteristics, a semiconductor device with little variation in the electrical characteristics of transistors, a semiconductor device with large on-state current, and a highly reliable semiconductor device can be realized.
[0070] 2A shows an enlarged view of the vicinity of the channel formation region in FIG. 1B. As shown in FIG. 2A, the oxide semiconductor layer 230 includes a region 230i that functions as a channel formation region and regions 230na and 230nb that sandwich the region 230i and function as source and drain regions. At least a part of the region 230i overlaps with the conductive layer 260. In other words, the region 230i is provided in a region between the conductive layer 242a and the conductive layer 242b. The region 230na overlaps with the conductive layer 242a, and the region 230nb overlaps with the conductive layer 242b.
[0071] An OS transistor is a transistor in which impurities and oxygen vacancies (V O ), the electrical characteristics are likely to fluctuate and reliability may be reduced. In addition, in oxide semiconductors, defects in which hydrogen enters oxygen vacancies (hereinafter referred to as V O H) and generate electrons that act as carriers. O When H is formed, the donor concentration in the channel formation region may increase. As the donor concentration in the channel formation region increases, the threshold voltage may vary. Therefore, if oxygen vacancies are present in the channel formation region of the oxide semiconductor, the OS transistor is likely to be normally on. Therefore, in the channel formation region of the oxide semiconductor, impurities, oxygen vacancies, and V O It is preferable that H is reduced as much as possible. In other words, it is preferable that the region in the oxide semiconductor where the channel is formed has a reduced carrier concentration and is i-type (intrinsic) or substantially i-type.
[0072] In response to this problem, an insulator containing oxygen that is released by heating (hereinafter may be referred to as excess oxygen) is provided near the oxide semiconductor, and heat treatment is performed to supply oxygen from the insulator to the oxide semiconductor, thereby eliminating oxygen vacancies and V OHowever, if an excessive amount of oxygen is supplied to the source region or the drain region, this may cause a decrease in the on-state current or a decrease in the field-effect mobility of the transistor 200. Furthermore, variations in the amount of oxygen supplied to the source region or the drain region within the substrate surface will cause variations in the characteristics of a semiconductor device having the transistor.
[0073] Therefore, in the oxide semiconductor layer 230, the region 230i that functions as a channel formation region preferably has a reduced carrier concentration and is i-type or substantially i-type, whereas the regions 230na and 230nb that function as a source region or a drain region preferably have a high carrier concentration and are n-type. O It is preferable to reduce H so that an excessive amount of oxygen is not supplied to the regions 230na and 230nb.
[0074] In other words, in the oxide semiconductor layer 230, the regions 230na and 230nb preferably have high carrier concentrations and are n-type, while the region 230i preferably has a reduced carrier concentration and is i-type or substantially i-type. In other words, it is preferable that the n-type region does not extend to the channel formation region.
[0075] For example, by reducing oxygen vacancies or lowering the concentration of impurities such as hydrogen, nitrogen, and metal elements in the region 230i compared to the regions 230na and 230nb, the region 230i can be made into a high-resistivity region with a low carrier concentration. In this case, the region 230i can be said to be i-type (intrinsic) or substantially i-type.
[0076] Furthermore, for example, by suppressing the reduction in the amount of oxygen vacancies in the regions 230na and 230nb or by suppressing the reduction in the impurity concentration, the regions 230na and 230nb can be made into regions with a high carrier concentration and low resistance. In this case, the regions 230na and 230nb are n-type regions with a high carrier concentration and low resistance compared to the region 230i.
[0077] Furthermore, a region may be formed between the region 230i and the region 230na, whose carrier concentration is equal to or lower than that of the region 230na, and equal to or higher than that of the region 230i. That is, this region functions as a junction region between the region 230i and the region 230na. The junction region may have a hydrogen concentration equal to or lower than that of the region 230na, and equal to or higher than that of the region 230i. The junction region may have an oxygen vacancy equal to or lower than that of the region 230na, and equal to or higher than that of the region 230i. The same applies to the region between the region 230i and the region 230nb.
[0078] 2A illustrates an example in which the bottom surfaces of the regions 230na and 230nb are located above the insulating layer 224, but the present invention is not limited to this. For example, the bottom surfaces of the regions 230na and 230nb may be formed up to the interface between the oxide semiconductor layer 230 and the insulating layer 224.
[0079] It may be difficult to clearly detect the boundaries between regions in the oxide semiconductor layer 230. The concentrations of metal elements and impurities such as hydrogen and nitrogen detected in each region may vary continuously within each region, rather than varying stepwise from region to region. That is, it is sufficient that the concentrations of impurities such as hydrogen and nitrogen decrease in a region closer to the channel formation region.
[0080] The conductive layer 242a and the conductive layer 242b are each in contact with the oxide semiconductor layer 230. Therefore, it is preferable that the conductive layer 242a and the conductive layer 242b each be made of a conductive material that is not easily oxidized or a conductive material that has a function of suppressing oxygen diffusion. This can suppress a decrease in the conductivity of the conductive layer 242a and the conductive layer 242b. Furthermore, it is preferable that the conductive layer 242a and the conductive layer 242b each be made of a conductive material that maintains low electrical resistance even when oxidized or a conductive oxide material. This can suppress a decrease in the conductivity of the conductive layer 242a and the conductive layer 242b even when the conductive layer 242a and the conductive layer 242b are oxidized. Examples of the conductive material include a conductive material containing nitrogen and a conductive material containing oxygen.
[0081] For the conductive layer 242a and the conductive layer 242b, for example, a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, a nitride containing titanium and aluminum, or the like may be used. Alternatively, for example, ruthenium, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel may be used. These materials are preferable because they are conductive materials that are resistant to oxidation or that maintain conductivity even after absorbing oxygen.
[0082] In one embodiment of the present invention, the conductive layers 242a and 242b are preferably formed using a tantalum compound. The tantalum compound preferably contains tantalum nitride. In this case, each of the conductive layers 242a and 242b contains at least tantalum and nitrogen.
[0083] Depending on its composition, tantalum nitride has various crystal structures, such as β-TaN (hexagonal), θ-TaN (hexagonal), δ-TaN (cubic), ε-TaN (hexagonal), Ta3N5 (tetragonal), Ta4N5 (tetragonal), and Ta5N6 (hexagonal). Tantalum compounds may have two or more of these crystal structures. Depending on their composition, tantalum compounds may contain metallic tantalum. When tantalum compounds contain oxygen, they may have tantalum oxide nitride, tantalum oxynitride, tantalum oxide, etc.
[0084] Furthermore, tantalum in a tantalum compound has various bonding states depending on its crystal structure. For example, examples of bonding states of tantalum include the bonding state of metallic tantalum, the bonding state of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically small, the bonding state of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically equal, the bonding state of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically large, the bonding state of tantalum nitride oxide, the bonding state of tantalum oxynitride, and the bonding state of tantalum oxide.
[0085] In this specification, the bonding state of metallic tantalum refers to the metallic bonding state of tantalum. Metallic tantalum may also refer to an aggregate of tantalum atoms. Tantalum nitride with a stoichiometrically low nitrogen content per tantalum refers to tantalum nitride with a smaller ratio of nitrogen atoms to tantalum compared to tantalum nitride with a stoichiometrically high nitrogen content per tantalum refers to tantalum nitride with a larger ratio of nitrogen atoms to tantalum compared to tantalum nitride with a stoichiometrically high nitrogen content per tantalum. Tantalum nitride with a stoichiometrically high nitrogen content per tantalum refers to tantalum nitride with a Ta:N=1:1 atomic ratio.
[0086] In this specification, the bonding state of metallic tantalum and the bonding state of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically small are referred to as the first bonding state of tantalum. The bonding states of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically equal and the bonding state of tantalum nitride oxide are referred to as the second bonding state of tantalum. The bonding state of tantalum nitride in which the amount of nitrogen per tantalum is stoichiometrically large is referred to as the third bonding state of tantalum. The bonding state of tantalum oxynitride is referred to as the fourth bonding state of tantalum. The bonding state of tantalum oxide is referred to as the fifth bonding state of tantalum.
[0087] The bonding state of tantalum can be evaluated by, for example, narrow scan analysis using XPS. In an analysis using XPS (referred to as XPS analysis), the chemical shift value (also referred to as binding energy value) varies depending on the bonding state of the elements. Specifically, in a spectrum (referred to as XPS spectrum) obtained by XPS analysis of tantalum 4f, when tantalum exists in the bonding state of metallic tantalum, the chemical shift value has a peak position in the range of 21.5 eV to 22 eV, which is Ta4f 7 / 2 When tantalum exists in a tantalum nitride bonding state in which the amount of nitrogen per tantalum is stoichiometrically equal, a peak of Ta4f is observed. 7 / 2 When tantalum exists in a bonded state of tantalum oxide, a peak of Ta4f is observed, which has a chemical shift value of 26 eV to 27 eV. 7 / 2 A peak of is observed.
[0088] In this specification, a peak in XPS analysis refers to a convex shape that appears in an XPS spectrum. Note that a single peak may be formed by overlapping multiple peaks. Furthermore, a peak position in XPS analysis refers to the binding energy value at the maximum value of the convex shape (peak) that appears in the XPS spectrum.
[0089] As described above, since the chemical shift value varies depending on the bonding state, for example, by performing waveform analysis of the XPS spectrum, the abundance ratio of each bonding state of the element can be calculated. Specifically, the abundance ratio of each bonding state of tantalum can be calculated by fitting the actually measured XPS spectrum of tantalum 4f with a synthetic spectrum of peaks set for each bonding state of tantalum.
[0090] In this specification, the abundance ratio of the bonding state of an element is defined as the ratio of the peak area in the XPS spectrum corresponding to the bonding state of a certain element to the sum of the peak areas in the XPS spectrum corresponding to each assumed bonding state of the element. For example, when a first bonding state, a second bonding state, and a third bonding state of the element are assumed, the abundance ratio of the first bonding state of the element is calculated from the ratio of the peak area in the XPS spectrum corresponding to the first bonding state of the element to the sum of the peak areas in the XPS spectrum corresponding to the first bonding state of the element, the peak areas in the XPS spectrum corresponding to the second bonding state of the element, and the peak areas in the XPS spectrum corresponding to the third bonding state of the element.
[0091] The 5d orbital of tantalum is believed to be the main contributor to the conduction band of tantalum nitride. To maintain the conductivity of a tantalum compound, it is necessary to suppress the loss of electrons in the 5d orbital of tantalum. Therefore, in order to suppress the loss of electrons in the 5d orbital of tantalum and to suppress a decrease in the conductivity of the tantalum compound, it is preferable that the sum of the abundance ratio of the first bonding state of tantalum and the abundance ratio of the second bonding state of tantalum be high in the conductive layers 242a and 242b.
[0092] On the other hand, because the reducing power of tantalum in the first bonding state is high (tantalum is easily oxidized in the first bonding state), using a tantalum compound with a high abundance ratio of tantalum in the first bonding state for the conductive layers 242a and 242b may cause oxygen vacancies in the oxide semiconductor layer 230, resulting in a normally-on transistor. Furthermore, when the conductive layers 242a and 242b are formed using a tantalum compound with a high abundance ratio of tantalum in the first bonding state, damage to the oxide semiconductor layer 230, which is the surface on which the conductive layers 242a and 242b are formed, may be increased, resulting in a decrease in the reliability of the transistor. Therefore, the abundance ratio of tantalum in the first bonding state in the conductive layers 242a and 242b is preferably low.
[0093] From the above, in each of the conductive layers 242a and 242b, the abundance ratio of tantalum in the first bonding state is preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less. Also, in each of the conductive layers 242a and 242b, the abundance ratio of tantalum in the second bonding state is preferably 5% or more, and more preferably 10% or more.
[0094] The conductive layer 242a and the conductive layer 242b preferably contain the δ-TaN phase. For example, the conductive layer 242a and the conductive layer 242b may have a crystal orientation of <111> The δ-TaN phase has a crystal orientation of <200> It is preferable that the tantalum compound contains a δ-TaN phase, which is represented by the formula (1). By containing the δ-TaN phase, it is possible to suppress a decrease in the electrical conductivity of the tantalum compound. Note that the crystal orientation described in this specification refers to the crystal orientation of the crystalline phase relative to the surface on which the tantalum compound is formed.
[0095] In addition, the crystal orientation is <111> The δ-TaN phase and the crystal orientation are <200> The δ-TaN phase can be confirmed by, for example, analysis using X-ray diffraction (XRD) (referred to as XRD analysis). In XRD analysis, <111> The peak derived from the δ-TaN phase has a peak position in the range of 2θ=35.5±1.0° (2θ range of 34.5° to 36.5°). <200> The peak derived from the δ-TaN phase has a peak position in the range of 2θ = 41.2 ± 2.0 degrees (2θ range of 39.2 degrees to 43.2 degrees). In this specification, a peak in the XRD spectrum having a peak position in the range of 2θ = 35.5 ± 1.0 degrees (2θ range of 34.5 degrees to 36.5 degrees) may be referred to as the first peak. Also, a peak having a peak position in the range of 2θ = 41.2 ± 2.0 degrees (2θ range of 39.2 degrees to 43.2 degrees) may be referred to as the second peak.
[0096] In this specification, a peak in XRD analysis refers to a convex shape that appears in an XRD spectrum. Note that a single peak may be formed by overlapping multiple peaks. Furthermore, a peak height in XRD analysis refers to the maximum value of a convex shape (peak) that appears in an XRD spectrum. Furthermore, a peak position in XRD analysis refers to the 2θ value at the maximum value of a convex shape (peak) that appears in an XRD spectrum.
[0097] For example, in XRD analysis, it is preferable that a diffraction peak from the (111) plane in the δ-TaN phase and a diffraction peak from the (200) plane in the δ-TaN phase are observed. Furthermore, it is preferable that the conductive layer 242a and the conductive layer 242b each have a first peak and a second peak in the XRD spectrum.
[0098] In addition, in the conductive layer 242a and the conductive layer 242b, the crystal orientation is <111> The content of the δ-TaN phase is <200> It is preferable that the content of the δ-TaN phase is equal to or higher than that of the δ-TaN phase having a crystal orientation of <111> The crystal orientation is <200> The ratio of the content of the δ-TaN phase between the tantalum compound and the tantalum compound is preferably 1 or a value close to 1. By adopting such a configuration, the crystal grain boundaries in the tantalum compound are reduced, and the reliability of the transistor can be improved.
[0099] In addition, the crystal orientation is <111> The content of δ-TaN phase and the crystal orientation are <200> The magnitude relationship between the content of the δ-TaN phase and the content of the δ-TaN phase can be evaluated, for example, by XRD analysis. For example, in the XRD spectrum, each of the conductive layers 242a and 242b preferably has a first peak and a second peak. Furthermore, the peak height of the first peak is preferably equal to or higher than the peak height of the second peak. For example, the ratio of the peak height of the second peak to the peak height of the first peak is preferably 0.1 or more and 1.0 or less, and more preferably 0.2 or more and 1.0 or less. Alternatively, for example, the ratio of the peak height of the second peak to the peak height of the first peak is preferably 1 or a value close to 1. Note that, in this specification, a value close to a certain value A refers to a value between 0.8×A and 1.2×A.
[0100] Here, the ratio of the number of nitrogen atoms to the number of tantalum atoms is referred to as the N / Ta ratio. For example, the N / Ta ratio of each of the conductive layers 242a and 242b is preferably 1.0 to 2.0, more preferably 1.1 to 1.8, and even more preferably 1.2 to 1.5. By increasing the N / Ta ratio, oxidation of the tantalum compound can be suppressed. Furthermore, the oxidation resistance of the tantalum compound can be improved. Furthermore, diffusion of oxygen into the tantalum compound can be suppressed. Therefore, formation of an oxide layer between the conductive layer 242a and the oxide semiconductor layer 230 and the conductive layer 242b can be prevented, or the thickness of the oxide layer can be reduced.
[0101] Note that the abundance ratio of the first bonding state of tantalum, the abundance ratio of the second bonding state of tantalum, and the crystal orientation of the conductive layer 242a and the conductive layer 242b are determined in accordance with the characteristics desired for the transistor 200. <111> The content of δ-TaN phase and the crystal orientation are <200> The content of the δ-TaN phase, the N / Ta ratio, and the like can be set appropriately.
[0102] Note that hydrogen contained in the oxide semiconductor layer 230 or the like might diffuse to the conductive layer 242a or the conductive layer 242b. In particular, when a nitride containing tantalum is used for the conductive layer 242a or the conductive layer 242b, hydrogen contained in the oxide semiconductor layer 230 or the like is likely to diffuse to the conductive layer 242a or the conductive layer 242b, and the diffused hydrogen might bond to nitrogen contained in the conductive layer 242a or the conductive layer 242b. That is, hydrogen contained in the oxide semiconductor layer 230 or the like might be absorbed by the conductive layer 242a or the conductive layer 242b.
[0103] Furthermore, when heat treatment is performed with the conductive layer 242a and the oxide semiconductor layer 230 in contact with each other, the sheet resistance of the region of the oxide semiconductor layer 230 overlapping with the conductive layer 242a may decrease. Also, the carrier concentration may increase. Therefore, the resistance of the region of the oxide semiconductor layer 230 overlapping with the conductive layer 242a can be reduced in a self-aligned manner. The same applies to the region of the oxide semiconductor layer 230 overlapping with the conductive layer 242b.
[0104] The conductive layer 242 is preferably formed using a conductive film having compressive stress. This allows strain (hereinafter sometimes referred to as tensile strain) that expands in the tensile direction to be formed in the regions 230na and 230nb. The tensile strain causes V O The region 230na and the region 230nb can be stable n-type regions by stably forming H. The compressive stress of the conductive layer 242 is a stress that attempts to relax the compressed shape of the conductive layer 242, and is a stress having a vector in the direction from the center of the conductive layer 242 to the end.
[0105] The magnitude of the compressive stress of the conductive layer 242 can be, for example, 500 MPa or more, preferably 1000 MPa or more, more preferably 1500 MPa or more, and even more preferably 2000 MPa or more. Note that the magnitude of the stress of the conductive layer 242 may be determined by forming a sample in which a conductive film used for the conductive layer 242 is formed on a substrate and measuring the stress of the sample.
[0106] The conductive layer 242a and the conductive layer 242b may have a single-layer structure or a stacked-layer structure. For example, as shown in FIG. 2B, the conductive layer 242a and the conductive layer 242b may each have a two-layer structure. In this case, the conductive layer 242a is a stacked body of a conductive layer 242a1 and a conductive layer 242a2 on the conductive layer 242a1, and the conductive layer 242b is a stacked body of a conductive layer 242b1 and a conductive layer 242b2 on the conductive layer 242b1. In this case, the layers in contact with the oxide semiconductor layer 230 (the conductive layers 242a1 and 242b1) are preferably made of the above-mentioned conductive material that is not easily oxidized or a conductive material that has a function of suppressing oxygen diffusion. This can suppress excessive oxidation of the conductive layers 242a and 242b by oxygen contained in the oxide semiconductor layer 230. Furthermore, a decrease in the conductivity of the conductive layers 242a and 242b can be suppressed.
[0107] In the following, the conductive layer 242a1 and the conductive layer 242b1 may be collectively referred to as the conductive layer 242_1, and the conductive layer 242a2 and the conductive layer 242b2 may be collectively referred to as the conductive layer 242_2.
[0108] The conductivity of the conductive layer 242_2 is preferably higher than that of the conductive layer 242_1. In this case, the conductive layer 242_2 may have at least a part having a region with higher conductivity than the conductive layer 242_1. For example, the thickness of the conductive layer 242_2 is preferably larger than that of the conductive layer 242_1. This can improve the operating speed of the transistor 200. Furthermore, a semiconductor device with reduced wiring delay can be manufactured.
[0109] Here, the conductive layers 242_1 and 242_2 are preferably made of conductive materials containing the same constituent elements but different chemical compositions. In this case, the conductive film to be the conductive layer 242_1 and the conductive film to be the conductive layer 242_2 can be successively formed without exposure to the air environment. By forming the conductive layer 242_1 without exposure to the air, impurities or moisture from the air environment can be prevented from adhering to the surface of the conductive layer 242_1, and the vicinity of the interface between the conductive layer 242_1 and the conductive layer 242_2 can be kept clean.
[0110] When the conductive layer 242_1 and the conductive layer 242_2 each contain a tantalum compound, the conductive layer 242_1 in contact with the oxide semiconductor layer 230 can be formed using any of the above-described tantalum compounds.
[0111] For example, the abundance ratio of tantalum in the first bonding state in the conductive layer 242_2 is preferably higher than the abundance ratio of tantalum in the first bonding state in the conductive layer 242_1. By adopting such a configuration, the conductivity of the conductive layer 242_2 can be increased. Alternatively, for example, in an XRD spectrum, the conductive layer 242_2 preferably has a first peak and a second peak, and the peak height of the first peak is lower than the peak height of the second peak. By adopting such a configuration, the conductivity of the conductive layer 242_2 can be increased.
[0112] Alternatively, for example, the N / Ta ratio in the conductive layer 242_2 is preferably lower than the N / Ta ratio in the conductive layer 242_1. For example, the N / Ta ratio in the conductive layer 242_2 is preferably 0.3 or more and less than 1.0, more preferably 0.5 or more and less than 1.0, and even more preferably 0.6 or more and less than 1.0. By lowering the N / Ta ratio, the resistivity of the tantalum compound can be reduced. Therefore, a semiconductor device with reduced wiring delay can be manufactured.
[0113] Note that the abundance ratio of the first bonding state of tantalum and the crystal orientation of the conductive layer 242_2 are set to 0.1 or 0.1 in accordance with the characteristics desired for the transistor 200. <111> The content of δ-TaN phase and the crystal orientation are <200> The content of the δ-TaN phase, the N / Ta ratio, and the like can be set appropriately.
[0114] Note that it may be difficult to clearly detect the boundary between the conductive layer 242_1 and the conductive layer 242_2. When a tantalum compound is used for the conductive layer 242, the tantalum concentration and the nitrogen concentration detected in each layer may not necessarily change stepwise in each layer but may change continuously (also referred to as gradation) in the region between the conductive layer 242_1 and the conductive layer 242_2. That is, the closer to the oxide semiconductor layer 230 the region of the conductive layer 242 is, the higher the N / Ta ratio should be. Therefore, the N / Ta ratio in the region located below the conductive layer 242 is preferably higher than the N / Ta ratio in the region located above the conductive layer 242.
[0115] The thickness of the conductive layer 242_1 is 0.1 nm to 5.0 nm, preferably 0.5 nm to 3.0 nm, and more preferably 1.0 nm to 3.0 nm. In this case, the conductive layer 242_1 may have at least a portion having a thickness as described above. The thickness of the conductive layer 242_2 is preferably thicker than that of the conductive layer 242_1. In this case, the conductive layer 242_2 may have at least a portion having a thickness thicker than that of the conductive layer 242_1.
[0116] Although the conductive layers 242_1 and 242_2 are formed using conductive materials that contain the same constituent elements but have different chemical compositions in the above example, the present invention is not limited to this example, and the conductive layers 242_1 and 242_2 may be formed using different conductive materials.
[0117] <Materials for semiconductor devices> Materials that can be used in the semiconductor device of this embodiment will be described below. Each layer included in the semiconductor device of this embodiment may have either a single-layer structure or a stacked-layer structure. FIGS. 1B to 1D show an example in which the insulating layer 214, the conductive layer 215, the insulating layer 222, the oxide semiconductor layer 230, the conductive layer 242a, the conductive layer 242b, the insulating layer 271a, the insulating layer 271b, the insulating layer 250, and the conductive layer 260 each have a single-layer structure. FIG. 3 shows an example in which the insulating layer 214, the conductive layer 215, the insulating layer 222, the oxide semiconductor layer 230, the conductive layer 242a, the conductive layer 242b, the insulating layer 271a, the insulating layer 271b, the insulating layer 250, and the conductive layer 260 each have a stacked-layer structure.
[0118] [Oxide semiconductor layer 230] As described above, the oxide semiconductor layer 230 has a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The oxide semiconductor layer 230 further has a source region and a drain region. The source region and the drain region are n-type regions (low-resistance regions) with higher carrier concentrations than the channel formation region.
[0119] The crystallinity of a semiconductor material used for the oxide semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor, a single crystal semiconductor, and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a crystalline semiconductor is preferable because deterioration of transistor characteristics can be suppressed.
[0120] The band gap of a metal oxide functioning as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide with a wide band gap, the off-state current of a transistor can be reduced. Because the off-state current of an OS transistor is small, the power consumption of a semiconductor device can be sufficiently reduced. Furthermore, because the frequency characteristics of an OS transistor are high, the semiconductor device can operate at high speed.
[0121] Examples of metal oxides that can be used for the oxide semiconductor layer 230 include indium oxide, gallium oxide, and zinc oxide. The metal oxide preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, the element M, and zinc. The metal oxide preferably contains one or both of indium and zinc. The element M is a metal element or a metalloid element having a high bond energy with oxygen, for example, a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of the element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M contained in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. Note that in this specification and the like, metal elements and metalloid elements may be collectively referred to as "metal elements," and the "metal elements" described in this specification and the like may include metalloid elements.
[0122] The oxide semiconductor layer 230 may be formed of, for example, indium oxide (In oxide), indium zinc oxide (In-Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In-Sn oxide), indium titanium oxide (In-Ti oxide), indium gallium oxide (In-Ga oxide), indium gallium aluminum oxide (In-Ga-Al oxide), indium gallium tin oxide (In-Ga-Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga-Zn oxide, also referred to as GZO), aluminum zinc oxide (Al-Zn oxide, also referred to as AZO), Examples of usable materials include indium aluminum zinc oxide (In-Al-Zn oxide, also referred to as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also referred to as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also referred to as IGZTO), and indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also referred to as IGAZO, IGZAO, or IAGZO). Alternatively, silicon-containing indium tin oxide, gallium tin oxide (Ga-Sn oxide), and aluminum tin oxide (Al-Sn oxide) can be used.
[0123] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.
[0124] Note that the metal oxide may contain one or more metal elements with higher period numbers in the periodic table instead of or in addition to indium. The greater the overlap of the orbitals of metal elements, the greater the carrier conduction in the metal oxide. Therefore, including a metal element with a higher period number in the periodic table may improve the field-effect mobility of a transistor. Examples of metal elements with higher period numbers in the periodic table include metal elements belonging to the fifth period and the sixth period. Specific examples of such metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.
[0125] The metal oxide may also contain one or more nonmetallic elements. The presence of a nonmetallic element in the metal oxide may increase the carrier concentration or narrow the band gap, thereby increasing the field-effect mobility of the transistor. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.
[0126] Furthermore, by increasing the ratio of the number of zinc atoms to the total number of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline, and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing fluctuations in the electrical characteristics of the transistor and improving its reliability.
[0127] Furthermore, by increasing the ratio of the number of atoms of element M to the sum of the numbers of atoms of all metal elements contained in the metal oxide, a metal oxide with a wide band gap can be obtained. Furthermore, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, resulting in a transistor with a small off-state current. Furthermore, a shift in the threshold voltage of the transistor can be suppressed. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, resulting in improved reliability.
[0128] The electrical characteristics and reliability of a transistor vary depending on the composition of the metal oxide used for the oxide semiconductor layer 230. Therefore, by varying the composition of the metal oxide depending on the electrical characteristics and reliability required of the transistor, a semiconductor device that has both excellent electrical characteristics and high reliability can be provided.
[0129] When the metal oxide is an In-M-Zn oxide, the atomic ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxides include In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and compositions in the vicinity thereof. Note that the term "nearby compositions" refers to compositions within a ±30% range of the desired atomic ratio. By increasing the atomic ratio of indium in the metal oxide, the on-state current, field-effect mobility, and the like of a transistor can be increased.
[0130] Furthermore, the atomic ratio of In in the In-M-Zn oxide may be less than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions close to these. By increasing the proportion of M atoms in the metal oxide, the generation of oxygen vacancies can be suppressed.
[0131] When the element M contains a plurality of metal elements, the total proportion of the number of atoms of the metal elements can be regarded as the proportion of the number of atoms of the element M.
[0132] In this specification and the like, the ratio of the number of indium atoms to the sum of the numbers of atoms of all contained metal elements may be referred to as the indium content. The same applies to other metal elements.
[0133] Furthermore, when the metal oxide is an In-Zn oxide, the atomic ratio of the metal elements in the In-Zn oxide may be, for example, In:Zn=1:1, In:Zn=2:1, In:Zn=4:1, or a similar composition. The In-Zn oxide may also contain a trace amount of element M. For example, when the element M is Sn, the atomic ratio of the metal elements in the metal oxide may be, for example, In:Sn:Zn=2:0.1:1, In:Sn:Zn=4:0.1:1, or a similar composition.
[0134] The composition of the metal oxide used in the oxide semiconductor layer 230 can be analyzed using, for example, energy dispersive X-ray spectrometry (EDX), XPS, inductively coupled plasma-mass spectrometry (ICP-MS), or inductively coupled plasma-atomic emission spectrometry (ICP-AES). Alternatively, a combination of these techniques may be used for the analysis. Note that for elements with low content, the actual content may differ from the content obtained by analysis due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content.
[0135] The metal oxide can be formed by sputtering or atomic layer deposition (ALD). When forming a metal oxide by sputtering, the composition of the formed metal oxide may differ from that of the target. In particular, the zinc content in the formed metal oxide may be reduced to about 50% of that of the target. Alternatively, the metal oxide may be formed by chemical vapor deposition (CVD), molecular beam epitaxy (MBE), pulsed laser deposition (PLD), or other methods.
[0136] The oxide semiconductor layer 230 may have a stacked structure including two or more metal oxide layers. The two or more metal oxide layers included in the oxide semiconductor layer 230 may have the same or approximately the same composition. By using a stacked structure of metal oxide layers with the same composition, for example, the same sputtering target can be used for formation, thereby reducing manufacturing costs.
[0137] The two or more metal oxide layers included in the oxide semiconductor layer 230 may have different compositions.
[0138] FIG. 3 shows an example in which the oxide semiconductor layer 230 has a two-layer structure including an oxide semiconductor layer 230a and an oxide semiconductor layer 230b on the oxide semiconductor layer 230a.
[0139] For example, the oxide semiconductor layer 230b is preferably made of a material having higher conductivity than the oxide semiconductor layer 230a. By using a material having high conductivity for the oxide semiconductor layer 230b in contact with the source and drain electrodes (the conductive layers 242a and 242b), the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242a and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242b can be reduced, and a transistor with high on-state current can be obtained.
[0140] The carrier concentration of the oxide semiconductor layer 230b is preferably higher than that of the oxide semiconductor layer 230a. Increasing the carrier concentration of the oxide semiconductor layer 230b increases the conductivity, and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242a and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242b can be reduced, resulting in a transistor with a large on-state current.
[0141] The oxide semiconductor layer 230 is not limited to the above-described configuration, and the oxide semiconductor layer 230b may be made of a material having lower conductivity than the oxide semiconductor layer 230a. The carrier concentration of the oxide semiconductor layer 230b may be lower than the carrier concentration of the oxide semiconductor layer 230a.
[0142] Furthermore, the band gap of the first metal oxide used in the oxide semiconductor layer 230a is preferably different from the band gap of the second metal oxide used in the oxide semiconductor layer 230b. For example, the difference between the band gaps of the first metal oxide and the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and even more preferably 0.3 eV or more.
[0143] The band gap of the second metal oxide used for the oxide semiconductor layer 230b is preferably smaller than the band gap of the first metal oxide used for the oxide semiconductor layer 230a, which can reduce the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242a and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 242b, thereby providing a transistor with high on-state current.
[0144] For example, the content of element M in the second metal oxide is preferably lower than the content of element M in the first metal oxide. More specifically, for example, it is preferable to use a metal oxide having a composition of In:M:Zn=1:3:2 (atomic ratio) or a composition thereabout for the oxide semiconductor layer 230a, and a metal oxide having a composition of In:M:Zn=1:1:1 (atomic ratio) or a composition thereabout for the oxide semiconductor layer 230b. In this case, it is particularly preferable to use one or more of gallium, aluminum, and tin as the element M.
[0145] Note that the oxide semiconductor layer 230 is not limited to the above-described structure, and the band gap of the second metal oxide may be larger than the band gap of the first metal oxide.
[0146] Furthermore, the content of element M in the second metal oxide is preferably lower than the content of element M in the first metal oxide. For example, the content of gallium in the second metal oxide is preferably lower than the content of gallium in the first metal oxide. Furthermore, the second metal oxide may contain a trace amount of element M or may not contain element M. For example, the second metal oxide may contain a trace amount of tin. For example, it is preferable that the second metal oxide used in the oxide semiconductor layer 230b be an In-Zn oxide and the first metal oxide used in the oxide semiconductor layer 230a be an In-M-Zn oxide. Specifically, the second metal oxide may be an In-Zn oxide and the first metal oxide may be an In-Ga-Zn oxide.
[0147] For example, the oxide semiconductor layer 230b preferably includes a metal oxide having an atomic ratio of In:Zn=1:1 or a similar composition, a metal oxide having an atomic ratio of In:Zn=2:1 or a similar composition, a metal oxide having an atomic ratio of In:Sn:Zn=2:0.1:1 or a similar composition, a metal oxide having an atomic ratio of In:Zn=4:1 or a similar composition, a metal oxide having an atomic ratio of In:Sn:Zn=4:0.1:1 or a similar composition, or an indium oxide.The oxide semiconductor layer 230a preferably includes a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a similar composition, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a similar composition, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a similar composition. This allows the on-state current of the transistor 200 to be increased, and the transistor structure to have high reliability and little variation can be obtained.
[0148] The oxide semiconductor layer 230 is not limited to the above-described structure, and the content of the element M in the second metal oxide may be higher than the content of the element M in the first metal oxide.
[0149] The oxide semiconductor layer 230 preferably includes a crystalline metal oxide layer. Examples of the structure of a crystalline metal oxide include a c-axis aligned crystal (CAAC) structure, a polycrystalline structure, and a nano-crystal (nc) structure. By using a crystalline metal oxide layer for the oxide semiconductor layer 230, the density of defect states in the oxide semiconductor layer 230 can be reduced, and a highly reliable semiconductor device can be realized.
[0150] Since it is difficult to identify clear grain boundaries in CAAC-OS, it is said that the decrease in electron mobility due to grain boundaries is unlikely to occur. Therefore, metal oxides having CAAC-OS have stable physical properties. Therefore, metal oxides having CAAC-OS are heat-resistant and highly reliable. CAAC-OS is an oxide semiconductor with a CAAC structure.
[0151] In the nc-OS, there is no regularity in the crystal orientation between different nanocrystals, and therefore no orientation is observed throughout the film. In other words, when the nc-OS is used as the oxide semiconductor layer 230, the film characteristics of the oxide semiconductor layer 230 are constant regardless of the direction of carrier flow in the oxide semiconductor layer 230, and the electrical characteristics of the transistor are stable. Note that the nc-OS is an oxide semiconductor with an nc structure.
[0152] Oxide semiconductors have a variety of structures, each with different characteristics. The oxide semiconductor layer 230b may include two or more of a CAAC-OS, an nc-OS, an amorphous-like oxide semiconductor (a-like OS), an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, and a cloud-aligned composite oxide semiconductor (CAC-OS).
[0153] The higher the crystallinity of the metal oxide layer used for the oxide semiconductor layer 230, the more the density of defect states in the oxide semiconductor layer 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.
[0154] When a metal oxide layer is formed by sputtering, the higher the substrate temperature (stage temperature) during formation, the higher the crystallinity of the formed metal oxide layer.Furthermore, the higher the ratio of the flow rate of oxygen gas to the total deposition gas used during formation (hereinafter also referred to as oxygen flow rate ratio), the higher the crystallinity of the formed metal oxide layer.
[0155] The crystallinity of the oxide semiconductor layer 230 can be analyzed by, for example, XRD, a transmission electron microscope (TEM), or electron diffraction (ED), or a combination of these techniques may be used for the analysis.
[0156] The oxide semiconductor layer 230 may have a stacked structure of two or more metal oxide layers with different crystallinity. For example, the oxide semiconductor layer 230 may have a stacked structure of a first metal oxide layer and a second metal oxide layer provided on the first metal oxide layer, and the second metal oxide layer may have a region with higher crystallinity than the first metal oxide layer. Alternatively, the second metal oxide layer may have a region with lower crystallinity than the first metal oxide layer. In this case, the first metal oxide layer and the second metal oxide layer may have different compositions or may have the same or approximately the same composition.
[0157] For example, it is preferable to use a metal oxide having an In:M:Zn=1:3:2 (atomic ratio) or a similar composition, or a metal oxide having an In:M:Zn=1:3:4 (atomic ratio) or a similar composition, for the oxide semiconductor layer 230a, and a metal oxide having an In:M:Zn=1:1:1 (atomic ratio) or a similar composition, for the oxide semiconductor layer 230b. Using a metal oxide with a high In / Zn ratio for the oxide semiconductor layer 230a can improve the crystallinity of the oxide semiconductor layer 230a. Furthermore, forming the oxide semiconductor layer 230b on the highly crystalline oxide semiconductor layer 230a can also easily improve the crystallinity of the oxide semiconductor layer 230b. This can improve the crystallinity of the entire oxide semiconductor layer 230, which is preferable. In this case, it is particularly preferable to use gallium, aluminum, or tin as the element M. For example, two IGZO layers with different compositions may be stacked. Alternatively, for example, a laminated structure of any one selected from indium oxide, indium gallium oxide, and IGZO and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.
[0158] The thickness of the oxide semiconductor layer 230 is preferably 5 nm or more and 100 nm or less, more preferably 5 nm or more and 50 nm or less, and further preferably 10 nm or more and 50 nm or less.
[0159] When the oxide semiconductor layer 230 has a two-layer structure of an oxide semiconductor layer 230a and an oxide semiconductor layer 230b on the oxide semiconductor layer 230a, the sum of the thicknesses of the oxide semiconductor layer 230a and the oxide semiconductor layer 230b is preferably within the above range. In addition, the thickness of the oxide semiconductor layer 230b is preferably larger than the thickness of the oxide semiconductor layer 230a.
[0160] The hydrogen contained in the oxide semiconductor reacts with the oxygen that bonds with the metal atoms to form water, and oxygen vacancies (V O ) may be formed. O H functions as a donor and can generate electrons as carriers. Furthermore, some hydrogen atoms can bond with oxygen atoms that are bonded to metal atoms to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing a large amount of hydrogen is likely to be normally on. Furthermore, hydrogen in an oxide semiconductor is easily moved by stresses such as heat and an electric field. Therefore, if an oxide semiconductor contains a large amount of hydrogen, the reliability of the transistor may be reduced.
[0161] V in the oxide semiconductor layer 230 O It is preferable to reduce H as much as possible to make the oxide semiconductor layer 230 highly intrinsic or substantially highly intrinsic. O To obtain an oxide semiconductor with a sufficiently reduced amount of H, it is important to remove impurities such as water and hydrogen from the oxide semiconductor (this process may be referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the oxide semiconductor to repair oxygen vacancies. O Stable electrical characteristics can be obtained by using an oxide semiconductor in which impurities such as H are sufficiently reduced for a channel formation region of a transistor. Note that supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as oxygen-adding treatment.
[0162] The carrier concentration of the oxide semiconductor in the region that functions as the channel formation region is 1×10 18 cm -3 Preferably, it is 1×10 or less. 17 cm-3 More preferably, it is less than 1×10 16 cm -3 More preferably, it is less than 1×10 13 cm -3 More preferably, it is less than 1×10 12 cm -3 The lower limit of the carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is not particularly limited. -9 cm -3 It can be said that:
[0163] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.
[0164] When an oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5 x 10 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 or less, more preferably 1 × 10 18 atoms / cm 3 The silicon concentration in the channel formation region of the oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5 x 10 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3Less than or equal to 3×10 18 atoms / cm 3 or less, more preferably 1 × 10 18 atoms / cm 3 The following applies.
[0165] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor is likely to be normally on. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. For this reason, the nitrogen concentration in the channel formation region of an oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5 x 10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3 Less than or equal to 5 × 10 18 atoms / cm 3 Less than or equal to 1×10 18 atoms / cm 3 Less than 5 × 10, more preferably 17 atoms / cm 3 The following applies.
[0166] Furthermore, hydrogen contained in an oxide semiconductor reacts with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. When hydrogen enters the oxygen vacancy, electrons serving as carriers may be generated. Furthermore, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons serving as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to be normally on. For this reason, it is preferable to reduce hydrogen as much as possible in the channel formation region of the oxide semiconductor. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5 x 1019 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5 × 10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 Less than.
[0167] Furthermore, when an oxide semiconductor contains an alkali metal or alkaline earth metal, defect levels may be formed and carriers may be generated. Therefore, a transistor using an oxide semiconductor containing an alkali metal or alkaline earth metal is likely to be normally on. Therefore, when the concentration of the alkali metal or alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is set to 1×10 18 atoms / cm 3 Less than or equal to 2 x 10 16 atoms / cm 3 Do the following:
[0168] When an oxide semiconductor with sufficiently reduced impurities is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.
[0169] [Insulating layer] It is preferable to use an inorganic insulating film for each of the insulating layers (insulating layer 214, insulating layer 216, insulating layer 222, insulating layer 224, insulating layer 250, insulating layer 271, insulating layer 275, insulating layer 280, insulating layer 282, insulating layer 283, etc.) included in the semiconductor device. Examples of inorganic insulating films include an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film. Examples of oxide insulating films include a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, an yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminate film. Examples of nitride insulating films include a silicon nitride film and an aluminum nitride film. Examples of oxynitride insulating films include a silicon oxynitride film, an aluminum oxynitride film, a gallium oxynitride film, an yttrium oxynitride film, and a hafnium oxynitride film. Examples of the nitride oxide insulating film include a silicon nitride oxide film and an aluminum nitride oxide film. An organic insulating film may also be used for an insulating layer included in a semiconductor device.
[0170] For example, as transistors become more miniaturized and highly integrated, thinner gate insulating layers can cause problems such as leakage current. Using a high-k material for the gate insulating layer allows for lower voltage operation of the transistor while maintaining the physical film thickness. It also makes it possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer. Meanwhile, using a material with a low dielectric constant for the insulating layer that functions as an interlayer film can reduce the parasitic capacitance that occurs between wiring. Therefore, materials can be selected according to the function of the insulating layer. Materials with a low dielectric constant also have high dielectric strength.
[0171] Examples of high-k materials include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.
[0172] Examples of materials with a low dielectric constant include inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide, and resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic resin. Other inorganic insulating materials with a low dielectric constant include silicon oxide doped with fluorine, silicon oxide doped with carbon, and silicon oxide doped with carbon and nitrogen. Another example is silicon oxide having vacancies. These silicon oxides may contain nitrogen.
[0173] Furthermore, a material capable of exhibiting ferroelectricity may be used for the insulating layer of a semiconductor device. Examples of materials capable of exhibiting ferroelectricity include metal oxides such as hafnium oxide, zirconium oxide, and hafnium zirconium oxide. Examples of materials capable of exhibiting ferroelectricity include hafnium oxide to which element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) has been added. The ratio of the number of hafnium atoms to the number of element J1 can be appropriately set; for example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close to 1:1. Examples of materials capable of exhibiting ferroelectricity include zirconium oxide to which element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) has been added. The ratio of the number of zirconium atoms to the number of atoms of element J2 can be set appropriately. For example, the ratio of the number of zirconium atoms to the number of atoms of element J2 can be set to 1:1 or close to 1:1. Furthermore, as a material that can have ferroelectricity, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as lead zirconate titanate (PZT), barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.
[0174] Examples of materials that may exhibit ferroelectricity include metal nitrides containing elements M1, M2, and nitrogen. Here, element M1 is one or more elements selected from aluminum, gallium, indium, etc. Furthermore, element M2 is one or more elements selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. The ratio of the number of atoms of element M1 to the number of atoms of element M2 can be appropriately set. Furthermore, metal oxides containing element M1 and nitrogen may exhibit ferroelectricity even without element M2. Examples of materials that may exhibit ferroelectricity include materials obtained by adding element M3 to the above metal nitrides. Furthermore, element M3 is one or more elements selected from magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of element M1 to the number of atoms of element M2 to the number of atoms of element M3 can be appropriately set.
[0175] Furthermore, materials that can have ferroelectricity include perovskite-type oxynitrides such as SrTaO2N and BaTaO2N, and GaFeO3 with a κ-alumina structure.
[0176] In the above description, metal oxides and metal nitrides are used as examples, but the present invention is not limited thereto. For example, metal oxynitrides in which nitrogen is added to the above metal oxides, or metal oxynitrides in which oxygen is added to the above metal nitrides, may also be used.
[0177] Furthermore, as a material capable of exhibiting ferroelectricity, for example, a mixture or compound made of a plurality of materials selected from the materials listed above can be used. Alternatively, the insulating layer can have a laminated structure made of a plurality of materials selected from the materials listed above. However, since the crystal structure (characteristics) of the materials listed above may change not only depending on the film formation conditions but also on various processes, in this specification and the like, not only materials that exhibit ferroelectricity are called ferroelectrics, but also materials capable of exhibiting ferroelectricity.
[0178] Metal oxides containing either or both of hafnium and zirconium can retain ferroelectricity even when processed into thin films of a few nanometers. Furthermore, metal oxides containing either or both of hafnium and zirconium can retain ferroelectricity even in very small areas. Therefore, the use of metal oxides containing either or both of hafnium and zirconium allows for miniaturization of semiconductor devices.
[0179] In this specification, a layer of a material that can have ferroelectricity may be referred to as a ferroelectric layer, a metal oxide film, or a metal nitride film. Also, in this specification, a device having such a ferroelectric layer, a metal oxide film, or a metal nitride film may be referred to as a ferroelectric device.
[0180] Ferroelectricity is believed to be exhibited by the displacement of oxygen or nitrogen in crystals contained in the ferroelectric layer due to an external electric field. Furthermore, it is believed that the exhibiting of ferroelectricity depends on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, for an insulating layer to exhibit ferroelectricity, the insulating layer must contain crystals. In particular, an insulating layer containing crystals with an orthorhombic crystal structure is preferred because it exhibits ferroelectricity. The crystal structure of the crystals contained in the insulating layer may be one or more selected from the group consisting of tetragonal, orthorhombic, monoclinic, and hexagonal. The insulating layer may also have an amorphous structure. In this case, the insulating layer may have a composite structure having an amorphous structure and a crystalline structure.
[0181] Furthermore, a transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulating layer that has a function of suppressing the permeation of impurities and oxygen. The insulating layer that has a function of suppressing the permeation of impurities and oxygen can be, for example, a single-layer or stacked insulating layer containing one or more elements selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, the insulating layer that has a function of suppressing the permeation of impurities and oxygen can be made of a metal oxide such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, or tantalum oxide, or a metal nitride such as aluminum nitride, silicon nitride oxide, or silicon nitride.
[0182] Specifically, examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide. Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include oxides containing aluminum and hafnium (hafnium aluminate). Examples of insulating layers that have the function of suppressing the permeation of impurities such as water and hydrogen and oxygen include metal nitrides such as aluminum nitride, aluminum titanium nitride, titanium nitride, silicon nitride oxide, and silicon nitride.
[0183] An insulating layer, such as a gate insulating layer, that is in contact with or near an oxide semiconductor layer preferably has a region containing excess oxygen. For example, when an insulating layer having a region containing excess oxygen is in contact with or near an oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Examples of insulating layers that are likely to have a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.
[0184] At least one of the insulating layer 214, the insulating layer 275, the insulating layer 282, and the insulating layer 283 preferably functions as a barrier insulating film that suppresses diffusion of impurities from the substrate side or from above the transistor 200 to the transistor 200. Therefore, at least one of the insulating layer 214, the insulating layer 275, the insulating layer 282, and the insulating layer 283 is preferably made of an insulating material that has a function of suppressing diffusion of impurities. Alternatively, it is preferably made of an insulating material that has a function of suppressing diffusion of oxygen.
[0185] In this specification and the like, a barrier insulating film refers to an insulating film having barrier properties. The barrier properties refer to a property that makes it difficult for a corresponding substance to diffuse (also referred to as a property that makes it difficult for a corresponding substance to permeate, a property that has low permeability of a corresponding substance, or a function of suppressing the diffusion of a corresponding substance). Alternatively, the barrier properties refer to a function of capturing or fixing (also referred to as gettering) a corresponding substance. Note that hydrogen in the description of hydrogen diffusion or hydrogen incorporation refers to, for example, hydrogen atoms, hydrogen molecules, water molecules, and OH. - The term "diffusion of impurities" refers to at least one of hydrogen-bonded substances such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (NO, NO, NO, etc.), copper atoms, etc. The term "oxygen" refers to at least one of oxygen atoms, oxygen molecules, etc.
[0186] For the insulating layers 214, 275, 282, and 283, it is preferable to use an insulator that has a function of suppressing diffusion of impurities and oxygen. For example, aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, or silicon nitride oxide can be used. For example, it is preferable to use silicon nitride, which has a higher barrier property against hydrogen, for the insulating layers 214, 275, and 283. Furthermore, it is preferable to use an insulator that has a function of capturing or fixing hydrogen for the insulating layers 214 and 282. This can suppress diffusion of impurities from the substrate side to the transistor 200 through the insulating layer 214. Alternatively, it can suppress diffusion of impurities from an interlayer insulating film, etc., disposed outside the insulating layer 283 to the transistor 200 side. Alternatively, it can suppress diffusion of oxygen contained in the insulating layer 224, etc., to the substrate side through the insulating layer 214. Alternatively, oxygen contained in the insulating layer 280 or the like can be prevented from diffusing upward from the transistor 200 through the insulating layer 282 or the like. In this way, the transistor 200 is preferably surrounded by the insulating layers 214, 275, 282, and 283, which have the function of preventing the diffusion of impurities and oxygen.
[0187] Examples of insulators capable of capturing or fixing hydrogen include metal oxides with an amorphous structure. For the insulating layer 214 and the insulating layer 282, it is preferable to use, for example, a metal oxide such as magnesium oxide or an oxide containing one or both of aluminum and hafnium. In such metal oxides with an amorphous structure, oxygen atoms have dangling bonds, which may have the property of capturing or fixing hydrogen through the dangling bonds. In other words, metal oxides with an amorphous structure can be said to have a high ability to capture or fix hydrogen. By using such a metal oxide with an amorphous structure as a component of the transistor 200 or providing it around the transistor 200, hydrogen contained in the transistor 200 or hydrogen present around the transistor 200 can be captured or fixed. In particular, it is preferable to capture or fix hydrogen contained in the channel formation region of the transistor 200. With such a structure, a highly reliable transistor 200 and a semiconductor device can be manufactured.
[0188] Furthermore, the insulating layer 214 and the insulating layer 282 preferably have an amorphous structure, but may have a crystalline region formed in part. Furthermore, the insulating layer 214 and the insulating layer 282 may have a multilayer structure in which a layer with an amorphous structure and a layer having a crystalline region are stacked. For example, a stacked structure in which a layer having a crystalline region, typically a layer with a polycrystalline structure, is formed on a layer with an amorphous structure may be used.
[0189] The insulating layer 214, the insulating layer 275, the insulating layer 282, and the insulating layer 283 may be formed by, for example, a sputtering method. The sputtering method does not require the use of molecules containing hydrogen in the film formation gas, and therefore can reduce the hydrogen concentrations in the insulating layer 214, the insulating layer 275, the insulating layer 282, and the insulating layer 283. Note that the film formation method is not limited to the sputtering method, and a CVD method, an MBE method, a PLD method, an ALD method, or the like may also be used as appropriate.
[0190] FIG. 3 shows an example in which the insulating layer 214 has a two-layer structure including an insulating layer 214a and an insulating layer 214b on the insulating layer 214a.
[0191] When the insulating layer 214 has a stacked-layer structure, the insulating layer 214a preferably has the above-described barrier insulating layer against hydrogen. The insulating layer 214b preferably has a function of capturing or fixing hydrogen. With such a structure, hydrogen diffusion into a region surrounded by the insulating layer 214a and the insulating layer 283 can be suppressed. Furthermore, since the transistor 200 is included in the region, hydrogen contained in the transistor 200 can be captured or fixed.
[0192] Furthermore, the insulating layer 216 and the insulating layer 280 are preferably made of a material with a lower dielectric constant than the insulating layer 214. Using a material with a low dielectric constant as an interlayer film can reduce parasitic capacitance between wirings. For example, the insulating layer 216 and the insulating layer 280 can be made of silicon oxide, silicon oxynitride, or silicon nitride oxide. For example, silicon oxide doped with fluorine, silicon oxide doped with carbon, or silicon oxide doped with carbon and nitrogen can be used. For example, silicon oxide having vacancies can also be used. These silicon oxides can contain nitrogen. Silicon oxide and silicon oxynitride are particularly preferred because they are thermally stable. Materials such as silicon oxide, silicon oxynitride, and silicon oxide having vacancies are particularly preferred because they allow for the easy formation of regions containing excess oxygen.
[0193] It is preferable that the concentration of impurities such as water and hydrogen is reduced in the insulating layer 280. For example, an oxide containing silicon, such as silicon oxide or silicon oxynitride, may be used as the insulating layer 280. The top surface of the insulating layer 280 may be planarized.
[0194] The insulating layer 250 preferably has a function of capturing or fixing hydrogen. This can reduce the hydrogen concentration in the oxide semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor). Therefore, the V O By reducing H, the channel forming region can be made i-type or substantially i-type.
[0195] Examples of materials for insulating layers capable of capturing or fixing hydrogen include metal oxides such as oxides containing hafnium, oxides containing magnesium, oxides containing aluminum, and oxides containing aluminum and hafnium (hafnium aluminate). These metal oxides may further contain zirconium, such as oxides containing hafnium and zirconium. Metal oxides with an amorphous structure have dangling bonds in some oxygen atoms, which enhance their ability to capture or fix hydrogen. Therefore, these metal oxides preferably have an amorphous structure. For example, silicon may be added to these metal oxides to achieve an amorphous structure. For example, an oxide containing hafnium and silicon (hafnium silicate) is preferably used. Metal oxides may have crystalline regions and / or grain boundaries.
[0196] The ability to capture or fix a corresponding substance can also be said to have the property of making it difficult for the corresponding substance to diffuse. Therefore, the ability to capture or fix a corresponding substance can be rephrased as barrier properties.
[0197] The insulating layer 250 preferably has a region containing excess oxygen because the insulating layer 250 is in contact with the oxide semiconductor layer 230. The insulating layer 250 having a region containing excess oxygen can reduce oxygen vacancies in the oxide semiconductor layer 230. Examples of insulating layers that are likely to have a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.
[0198] FIG. 3 shows an example in which the insulating layer 250 has a two-layer structure including an insulating layer 250a and an insulating layer 250b on the insulating layer 250a.
[0199] In the case where the insulating layer 250 has a stacked-layer structure, a layer in contact with the oxide semiconductor layer 230 preferably has a function of capturing or fixing hydrogen. That is, in FIG. 3, the insulating layer 250a preferably has a function of capturing or fixing hydrogen. In addition, the insulating layer 250b is preferably the above-described barrier insulating layer against hydrogen.
[0200] The insulating layer 250a has a function of capturing or fixing hydrogen, which allows hydrogen contained in the oxide semiconductor layer 230 to be captured or fixed more effectively. This reduces the hydrogen concentration in the oxide semiconductor layer 230. For example, hafnium silicate or the like may be used as the insulating layer 250a. The insulating layer 250a preferably has an amorphous structure.
[0201] By making the insulating layer 250a amorphous, it is possible to suppress the formation of crystal grain boundaries. By suppressing the formation of crystal grain boundaries, it is possible to improve the flatness of the insulating layer 250a. This makes the film thickness distribution of the insulating layer 250a uniform, and it is possible to reduce extremely thin film thickness portions, thereby improving the breakdown voltage of the insulating layer 250a. It is also possible to make the film thickness distribution of the film provided on the insulating layer 250a uniform.
[0202] Furthermore, by suppressing the formation of grain boundaries in the insulating layer 250a, it is possible to reduce leakage current caused by defect levels in the grain boundaries, and thus the insulating layer 250a can function as an insulating film with low leakage current.
[0203] Furthermore, since hafnium oxide is a high-k material, hafnium silicate can also be a high-k material depending on the silicon content. Therefore, when the insulating layer 250a is used as a gate insulating layer, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. In addition, it is possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer.
[0204] The insulating layer 250b is formed as a barrier insulating layer against hydrogen, which can prevent impurities contained in the conductive layer 260 from diffusing into the oxide semiconductor layer 230. Silicon nitride has a high barrier property against hydrogen and is therefore suitable for the insulating layer 250b.
[0205] With such a structure, a semiconductor device having good electrical characteristics, high reliability, little variation in the electrical characteristics of the transistors, and a large on-state current can be provided.
[0206] It is also preferable to use a high-k material for the insulating layer 250. An example of a high-k material is an oxide containing one or both of aluminum and hafnium. Using a high-k material for the insulating layer 250 makes it possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. It also makes it possible to reduce the equivalent oxide thickness (EOT) of the insulating layer that functions as the gate insulating layer.
[0207] From the above, it is preferable to use an oxide containing one or both of aluminum and hafnium as the insulating layer 250a, it is more preferable to use an oxide having an amorphous structure and containing one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.
[0208] Additionally, insulating layer 250 may comprise an insulating layer of a thermally stable structure, such as silicon oxide or silicon oxynitride.
[0209] The insulating layer 250 preferably has a barrier insulating layer against oxygen, which can prevent the conductive layer 242a, the conductive layer 242b, the conductive layer 260, and the like from being oxidized. When the insulating layer 250 has a stacked-layer structure, a layer in contact with the conductive layer 242a and the conductive layer 242b and a layer in contact with the conductive layer 260 are preferably barrier insulating layers against oxygen.
[0210] For example, by using a barrier insulating layer against hydrogen and oxygen as the insulating layer 250b, it is possible to prevent oxidation of the conductive layer 260. It is also possible to prevent oxygen contained in the oxide semiconductor layer 230 from diffusing into the conductive layer 260 and forming oxygen vacancies in the oxide semiconductor layer 230.
[0211] Examples of the barrier insulating layer against oxygen include oxides containing one or both of aluminum and hafnium, magnesium oxide, gallium oxide, gallium zinc oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).
[0212] The thickness of the insulating layer 250 is preferably 0.1 nm or more and 30 nm or less, preferably 0.1 nm or more and 20 nm or less, preferably 0.1 nm or more and 10 nm or less, more preferably 0.1 nm or more and 5.0 nm or less, more preferably 0.5 nm or more and 5.0 nm or less, more preferably 1.0 nm or more and less than 5.0 nm, and even more preferably 1.0 nm or more and 3.0 nm or less.
[0213] 4(A) and 4(B) show an example in which the insulating layer 250 has a three-layer structure including an insulating layer 250c, an insulating layer 250a on the insulating layer 250c, and an insulating layer 250b on the insulating layer 250a.
[0214] The insulating layer 250a and the insulating layer 250b can have the same configuration as described above.
[0215] The insulating layer 250c is preferably made of a material with a low dielectric constant. As a material with a low dielectric constant, silicon oxide or silicon oxynitride is preferably used. The insulating layer 250c is a layer in contact with the oxide semiconductor layer 230. By using an oxide insulating layer for the insulating layer 250c, oxygen can be supplied to the oxide semiconductor layer 230. Furthermore, by providing the insulating layer 250b, oxygen contained in the insulating layer 250c can be prevented from diffusing into the conductive layer 260, and thus oxidation of the conductive layer 260 can be prevented. Furthermore, a decrease in the amount of oxygen supplied from the insulating layer 250c to the oxide semiconductor layer 230 can be prevented.
[0216] Also, Figures 5(A) and 5(B) show an example in which insulating layer 250 has a four-layer structure including insulating layer 250d, insulating layer 250c on insulating layer 250d, insulating layer 250a on insulating layer 250c, and insulating layer 250b on insulating layer 250a.
[0217] The insulating layers 250a to 250c can have the same structure as described above.
[0218] The insulating layer 250d preferably has a barrier property against oxygen. The insulating layer 250d is a layer in contact with the oxide semiconductor layer 230. When the insulating layer 250d has a barrier property against oxygen, oxygen can be prevented from being released from the oxide semiconductor layer 230. For example, aluminum oxide may be used as the insulating layer 250d. Aluminum oxide has a function of capturing or fixing hydrogen, and is therefore suitable for the insulating layer 250d in contact with the oxide semiconductor layer 230.
[0219] To miniaturize transistors, the insulating layers 250a to 250d are preferably thin. The thickness of each of the insulating layers 250a to 250d is preferably 0.1 nm to 10 nm, more preferably 0.1 nm to 5 nm, more preferably 0.5 nm to 5 nm, still more preferably 1 nm to less than 5 nm, and even more preferably 1 nm to 3 nm. Note that each of the insulating layers 250a to 250d may have a region with the above-described thickness in at least a portion thereof.
[0220] Typically, the thicknesses of the insulating layers 250d, 250c, 250a, and 250b are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. With such a structure, the transistor can have good electrical characteristics even when miniaturized or highly integrated.
[0221] To thin the insulating layers 250a to 250d as described above, it is preferable to form the insulating layers by an ALD method. The ALD method includes a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, and a plasma-enhanced ALD method in which a plasma-excited reactant is used. The PEALD method may be preferable because it uses plasma, which enables film formation at a lower temperature.
[0222] The ALD method can deposit atoms layer by layer, and therefore has the advantages of being able to form extremely thin films, being able to form films on structures with high aspect ratios, being able to form films with few defects such as pinholes, being able to form films with excellent coverage, being able to form films at low temperatures, etc. Therefore, insulating layer 250 can be formed with good coverage on the side surfaces of openings formed in insulating layer 280 or the like, and with the thin film thickness as described above.
[0223] Although the above description has been given of a structure in which the insulating layer 250 has a three-layer structure of insulating layers 250a to 250c or a four-layer structure of insulating layers 250a to 250d, the present invention is not limited to this. The insulating layer 250 can have a structure including at least one of the insulating layers 250a to 250d. As an example, the insulating layer 250 may have a three-layer structure including the insulating layer 250d, the insulating layer 250c on the insulating layer 250d, and the insulating layer 250b on the insulating layer 250c. By forming the insulating layer 250 using one, two, or three of the insulating layers 250a to 250d, the manufacturing process of the semiconductor device can be simplified and productivity can be improved.
[0224] The insulating layer 222 preferably has a function of suppressing the diffusion of hydrogen. The insulating layer 222 preferably has a function of suppressing the diffusion of oxygen. For example, the insulating layer 222 preferably has a function of suppressing the diffusion of either or both of hydrogen and oxygen more than the insulating layer 224.
[0225] The insulating layer 222 may be formed using an insulator containing an oxide of one or both of aluminum and hafnium, which are insulating materials. Alternatively, an oxide containing hafnium and zirconium, such as hafnium zirconium oxide, is preferably used. When the insulating layer 222 is formed using such a material, the insulating layer 222 functions as a layer that suppresses release of oxygen from the oxide semiconductor layer 230 to the substrate and diffusion of impurities from the periphery of the transistor 200 to the oxide semiconductor layer 230. Therefore, the insulating layer 222 can suppress diffusion of impurities into the transistor 200 and generation of oxygen vacancies in the oxide semiconductor layer 230. Furthermore, reaction of the conductive layer 215 with oxygen contained in the insulating layer 224 and the oxide semiconductor layer 230 can be suppressed.
[0226] Alternatively, for example, aluminum oxide, bismuth oxide, germanium oxide, niobium oxide, silicon oxide, titanium oxide, tungsten oxide, yttrium oxide, or zirconium oxide may be added to the insulator. Alternatively, these insulators may be nitrided. Furthermore, the insulating layer 222 may be formed by stacking silicon oxide, silicon oxynitride, or silicon nitride on these insulators.
[0227] Furthermore, since the insulating layer 222 has a region that functions as a second gate insulating layer, it may be made of a single layer or a multilayer of an insulator containing a high-k material, which will be described later. Note that the insulating layer 222 may also be made of a material with a high dielectric constant, such as lead zirconate titanate (PZT), strontium titanate (SrTiO3), or (Ba,Sr)TiO3 (BST).
[0228] As shown in FIG. 3, the insulating layer 222 may have a stacked structure of an insulating layer 222a over the insulating layer 216 and the conductive layer 215 and an insulating layer 222b over the insulating layer 222a.
[0229] The insulating layer 222b may be any insulating layer that can be used for the insulating layer 222 described above.
[0230] The insulating layer 222a is provided between the insulating layer 216 and the conductive layer 215 and the insulating layer 222b. The insulating layer 222a preferably has a function of suppressing hydrogen diffusion, thereby suppressing hydrogen diffusion from below the insulating layer 222a to the transistor 200.
[0231] The insulating layer 222a is preferably made of silicon nitride deposited by, for example, the ALD method (particularly the PEALD method). By using the ALD method to deposit the insulating layer 222a, the insulating layer 222a can be deposited with good coverage even if unevenness is formed between the insulating layer 216 and the conductive layer 215. Therefore, it is possible to prevent pinholes or discontinuities from being formed in the insulating layer 222b deposited on the insulating layer 222a.
[0232] Since the insulating layer 224 is in contact with the oxide semiconductor layer 230, the insulating layer 224 may be formed using, for example, silicon oxide, silicon oxynitride, or the like as appropriate.
[0233] Note that one or both of the insulating layer 222 and the insulating layer 224 may have a stacked structure of two or more layers. In this case, the insulating layer 224 is not limited to a stacked structure made of the same material, and may have a stacked structure made of different materials. The insulating layer 224 may be formed in an island shape overlapping with the oxide semiconductor layer 230. In this case, the insulating layer 275 is in contact with the side surface of the insulating layer 224 and the top surface of the insulating layer 222. Note that in this specification and the like, the term "island shape" refers to a state in which two or more layers formed in the same process and made of the same material are physically separated.
[0234] The insulating layer 271 preferably functions as at least a barrier insulating film against oxygen. For example, the insulating layer 271 preferably has a function of suppressing oxygen diffusion more than the insulating layer 280.
[0235] Furthermore, since the insulating layers 271a and 271b are in contact with the conductive layers 242a and 242b, respectively, they are preferably made of an inorganic insulator that does not easily oxidize the conductive layers 242a and 242b. For example, the insulating layers 271a and 271b are preferably made of a nitride insulating layer that can be used for the insulating layer 250b. For example, silicon nitride can be used for the insulating layers 271a and 271b.
[0236] The insulating layers 271a and 271b are inorganic insulators that function as etching stoppers and protect the conductive layers 242a and 242b when processing the conductive layers 242a and 242b. For example, as shown in FIG. 3, it is preferable that the insulating layer 271a has a stacked structure of an insulating layer 271a1 and an insulating layer 271a2 on the insulating layer 271a1, and that the insulating layer 271b has a stacked structure of an insulating layer 271b1 and an insulating layer 271b2 on the insulating layer 271b1. Here, it is preferable that the insulating layers 271a1 and 271b1 are nitride insulating layers that can be used for the insulating layer 250b. It is also preferable that the insulating layers 271a2 and 271b2 are oxide insulating layers that can be used for the insulating layer 250c so as to function as etching stoppers. For example, the insulating layer 271a1 and the insulating layer 271b1 can be made of silicon nitride, and the insulating layer 271a2 and the insulating layer 271b2 can be made of silicon oxide.
[0237] The insulating layers that become the insulating layers 271a and 271b function as masks for the conductive layers that become the conductive layers 242a and 242b, so the conductive layers 242a and 242b do not have a curved surface between their side surfaces and top surfaces. As a result, the conductive layer 242a has a corner-shaped end where the side surface and top surface intersect. The corner-shaped end where the side surface and top surface intersect of the conductive layer 242a increases the cross-sectional area of the conductive layer 242a compared to when the end has a curved surface. The same applies to the conductive layer 242b. Furthermore, by using a nitride insulating layer that does not easily oxidize metal for the insulating layers 271a and 271b, excessive oxidation of the conductive layers 242a and 242b can be suppressed. As a result, the resistance of the conductive layers 242a and 242b is reduced, thereby increasing the on-state current of the transistor 200.
[0238] The insulating layer 275 is provided to cover the insulating layer 224, the oxide semiconductor layer 230, the conductive layer 242, and the insulating layer 271. The insulating layer 275 preferably has a function of capturing hydrogen or fixing hydrogen. In that case, the insulating layer 275 preferably includes an insulator such as silicon nitride or a metal oxide having an amorphous structure, such as aluminum oxide or magnesium oxide. Alternatively, for example, the insulating layer 275 may be a stacked film of aluminum oxide and silicon nitride on the aluminum oxide.
[0239] By providing the insulating layer 271 and the insulating layer 275 as described above, it is possible to enclose the conductive layer 242 with a barrier insulating film against oxygen. With this configuration, it is possible to suppress a situation in which the conductive layer 242 is directly oxidized by oxygen contained in the insulating layer 280, which increases the resistivity and reduces the on-current.
[0240] The insulating layer 282 preferably has a function of suppressing diffusion of impurities from above into the insulating layer 280 and a function of capturing or fixing impurities such as hydrogen. The insulating layer 282 also preferably functions as a barrier insulating film against oxygen. An insulator such as a metal oxide having an amorphous structure, for example, aluminum oxide, may be used as the insulating layer 282. In this case, the insulating layer 282 contains at least oxygen and aluminum. By providing the insulating layer 282, which has a function of capturing or fixing impurities such as hydrogen, in contact with the insulating layer 280 in the region sandwiched between the insulating layer 214 and the insulating layer 283, the impurities such as hydrogen contained in the insulating layer 280 can be captured or fixed, and the amount of hydrogen in the region can be kept constant. This enables the manufacture of a highly reliable transistor 200 and semiconductor device with excellent characteristics.
[0241] It is more preferable to form the insulating layer 282 by sputtering an aluminum oxide film using an aluminum target in an atmosphere containing oxygen gas. The amount of oxygen implanted into layers below the insulating layer 282 can be controlled by the magnitude of the RF (Radio Frequency) power applied to the substrate by sputtering. For example, the smaller the RF power, the less oxygen is implanted into layers below the insulating layer 282, and the amount of oxygen is likely to saturate even if the insulating layer 282 is thin. Furthermore, the greater the RF power, the more oxygen is implanted into layers below the insulating layer 282.
[0242] A barrier insulating layer against hydrogen is preferably used for the insulating layer 283. This can suppress diffusion of hydrogen from above the insulating layer 283 to the oxide semiconductor layer 230. A silicon nitride film and a silicon nitride oxide film each have characteristics of releasing little impurities (for example, water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be suitably used for the insulating layer 283.
[0243] It is particularly preferable to use silicon nitride deposited by a sputtering method as the insulating layer 283. The sputtering method does not require the use of molecules containing hydrogen in the deposition gas, and therefore can reduce the hydrogen concentration in the insulating layer 283. Furthermore, by depositing the insulating layer 283 by a sputtering method, silicon nitride with high density can be formed.
[0244] [Conductive layer] Conductive layers (such as the conductive layer 215, the conductive layer 242, and the conductive layer 260) included in the semiconductor device preferably contain a metal element selected from aluminum, chromium, copper, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, and lanthanum, or an alloy containing any of the above metal elements or an alloy combining the above metal elements. The alloy containing any of the above metal elements may be a nitride of the alloy or an oxide of the alloy. For example, tantalum nitride, titanium nitride, tungsten, a nitride containing titanium and aluminum, a nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel is preferably used. Furthermore, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicide may also be used.
[0245] Nitrogen-containing conductive materials, such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum; oxygen-containing conductive materials, such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metal elements, such as titanium, tantalum, or ruthenium, are preferred because they are conductive materials that are resistant to oxidation, have the function of suppressing oxygen diffusion, or maintain conductivity even after absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide with added silicon (also referred to as ITSO), indium zinc oxide (also referred to as IZO®), and indium zinc oxide containing tungsten oxide. In this specification and elsewhere, a conductive film formed using a conductive material containing oxygen may be referred to as an oxide conductive film.
[0246] Conductive materials based on tungsten, copper, or aluminum are preferred because they have high conductivity.
[0247] Furthermore, a plurality of conductive layers formed from the above materials may be stacked. For example, a stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-described material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.
[0248] When a metal oxide is used for the channel formation region of a transistor, the conductive layer that functions as a gate electrode preferably has a stacked structure that combines a material containing the metal element and a conductive material containing oxygen. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.
[0249] The conductive layer 260 is preferably made of a highly conductive material such as tungsten. Furthermore, the conductive layer 260 is preferably made of a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion. As described above, examples of such conductive materials include conductive materials containing nitrogen (e.g., titanium nitride or tantalum nitride) and conductive materials containing oxygen (e.g., ruthenium oxide). This can suppress a decrease in the conductivity of the conductive layer 260.
[0250] The conductive layer 260 may also be made of a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. Alternatively, the conductive material containing the above-mentioned metal element and nitrogen (e.g., titanium nitride, tantalum nitride, etc.) may also be used. Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may also be used. Alternatively, indium gallium zinc oxide containing nitrogen may also be used. Using such a material may allow hydrogen contained in the metal oxide in which the channel is formed to be captured. Alternatively, hydrogen introduced from an outer insulating layer or the like may be captured.
[0251] 3 shows an example in which the conductive layer 260 has a two-layer structure consisting of a conductive layer 260a and a conductive layer 260b on the conductive layer 260a. In this case, it is preferable to use titanium nitride for the conductive layer 260a and tungsten for the conductive layer 260b, for example. This can increase the conductivity of the conductive layer 260.
[0252] The conductive layer 260a is preferably made of a conductive material that has the function of suppressing the diffusion of impurities. Alternatively, it is preferably made of a conductive material that has the function of suppressing the diffusion of oxygen. The conductive layer 260a has the function of suppressing the diffusion of oxygen, which can suppress the oxidation of the conductive layer 260b due to the oxygen contained in the insulating layer 250, thereby preventing a decrease in conductivity. As a conductive material that has the function of suppressing the diffusion of oxygen, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, ruthenium oxide, or the like is preferably used. Therefore, the conductive layer 260a may be made of a single layer or a stack of the above conductive materials. For example, the conductive layer 260a may be made of titanium nitride.
[0253] Furthermore, since the conductive layer 260 also functions as wiring, it is preferable to use a conductor with high conductivity. For example, the conductive layer 260b can be made of a conductive material containing tungsten, copper, or aluminum as a main component. The conductive layer 260b may have a layered structure, for example, a layered structure of titanium or titanium nitride and the above conductive material.
[0254] A material with high conductivity is preferably used for the conductive layer 215. Tungsten or aluminum is preferably used for the conductive layer 215. Alternatively, a conductive material containing nitrogen, such as tantalum nitride or titanium nitride, may be used for the conductive layer 215. A conductive material containing nitrogen is a conductive material that is not easily oxidized or has a function of suppressing oxygen diffusion, and therefore can be suitably used when an oxide insulating layer is used for one or both of the insulating layer 214 and the insulating layer 216.
[0255] 3 shows an example in which the conductive layer 215 has a two-layer structure including a conductive layer 215a and a conductive layer 215b on the conductive layer 215a. The conductive layer 215a is provided in contact with the bottom surface and sidewall of an opening formed in the insulating layer 216. The conductive layer 215b is provided so as to fill a recess formed in the conductive layer 215a. Here, the height of the top surface of the conductive layer 215b is the same as the height of the top surface of the conductive layer 215a and the height of the top surface of the insulating layer 216.
[0256] Here, the conductive layer 215a is preferably made of a conductive material that has a function of suppressing the diffusion of impurities and oxygen.
[0257] By using a conductive material having a function of suppressing impurity diffusion for the conductive layer 215a, it is possible to suppress the diffusion of impurities contained in the conductive layer 215b into the oxide semiconductor layer 230 through the insulating layer 216 or the like. Furthermore, by using a conductive material having a function of suppressing oxygen diffusion for the conductive layer 215a, it is possible to suppress a decrease in conductivity due to oxidation of the conductive layer 215b.
[0258] The conductive layer 215a may be a conductive layer that can be used for the conductive layer 260a. The conductive layer 215b is preferably a conductive material containing tungsten, copper, or aluminum as its main component. For example, the conductive layer 215b may be made of tungsten.
[0259] 3 shows a structure in which the conductive layer 215a and the conductive layer 215b are stacked, the present invention is not limited to this. For example, the conductive layer 215 may have a single layer structure or a stacked structure of three or more layers.
[0260] [substrate] Substrates on which transistors are formed can be, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (e.g., yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include those having an insulating region within the semiconductor substrate, such as an SOI (Silicon-On-Insulator) substrate. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Other examples include substrates having metal nitrides and substrates having metal oxides. Examples of substrates include an insulating substrate with a conductor or semiconductor provided thereon, a semiconductor substrate with a conductor or insulator provided thereon, and a conductive substrate with a semiconductor or insulator provided thereon. Alternatively, these substrates may be provided with elements. The elements provided on the substrate include a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.
[0261] According to one embodiment of the present invention, a novel transistor can be provided. Alternatively, a semiconductor device having favorable electrical characteristics can be provided. Alternatively, a semiconductor device with favorable reliability can be provided. Alternatively, a semiconductor device with little variation in transistor characteristics can be provided. Alternatively, a semiconductor device with high on-state current can be provided. Alternatively, a semiconductor device with high field-effect mobility can be provided. Alternatively, a semiconductor device with favorable frequency characteristics can be provided. Alternatively, a semiconductor device that can be miniaturized or highly integrated can be provided. Alternatively, a semiconductor device with low power consumption can be provided.
[0262] <Configuration Example of a Semiconductor Device Having a Transistor 200 and a Capacitor 100> 6A and 6B show a semiconductor device including the above-described transistor 200 and the capacitor 100. FIG. 6A is a plan view of the semiconductor device. FIG. 6B is a cross-sectional view of the portion indicated by the dashed dotted line A1-A2 in FIG. 6A, and is also a cross-sectional view of the transistor 200 in the channel length direction. Note that some elements are omitted from the plan view of FIG. 6A for clarity.
[0263] 6A and 6B, the capacitor 100 and the conductive layer 112 are arranged over the transistor 200. Here, it is preferable that the overlapping area between the capacitor 100 and the transistor 200 is large in a plan view. With such a structure, the area occupied by the semiconductor device including the capacitor 100 and the transistor 200 can be reduced. This enables miniaturization or high integration of the semiconductor device.
[0264] The semiconductor device includes a conductive layer 240a and a conductive layer 240b that function as plugs. The conductive layer 240a is provided in an opening formed in the insulating layer 285, the insulating layer 283, the insulating layer 282, the insulating layer 280, the insulating layer 275, and the insulating layer 271a, and the conductive layer 240b is provided in an opening formed in the insulating layer 285, the insulating layer 283, the insulating layer 282, the insulating layer 280, the insulating layer 275, and the insulating layer 271b.
[0265] 6B, the conductive layer 240a has a region in contact with the conductive layer 242a and a region in contact with at least part of the bottom surface of the conductive layer 112. The conductive layer 240b has a region in contact with the conductive layer 242b and a region in contact with at least part of the bottom surface of the conductive layer 110 included in the capacitor 100. That is, the conductive layer 240a is electrically connected to one of the source electrode and the drain electrode of the transistor 200, and the conductive layer 240b is electrically connected to the other of the source electrode and the drain electrode of the transistor 200.
[0266] The conductive layers 240a and 240b are preferably formed using a conductive material containing tungsten, copper, or aluminum as a main component.
[0267] 6B shows an example in which the conductive layer 240a and the conductive layer 240b each have a single-layer structure, but the present invention is not limited to this. For example, each of the conductive layer 240a and the conductive layer 240b may have a stacked structure of two or more layers.
[0268] For example, each of the conductive layers 240a and 240b may have a stacked structure including a first conductive layer provided along the side surface and bottom surface of the opening and a second conductive layer over the first conductive layer. When the conductive layers 240a and 240b have a stacked structure, the first conductive layer disposed near the insulating layer 285 and the insulating layer 280 is preferably formed using a conductive material capable of suppressing impurity penetration. For example, tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, ruthenium oxide, or the like is preferably used. The conductive material capable of suppressing impurity penetration may be used in a single layer or a stacked layer. This structure can prevent impurities contained in layers above the insulating layer 283 from entering the oxide semiconductor layer 230 through the conductive layer 240a and the conductive layer 240b. The second conductive layer also functions as a wiring, so a highly conductive conductor is preferably used. For example, the second conductive layer may be formed using a conductive material mainly containing tungsten, copper, or aluminum.
[0269] An insulating layer 241a is provided in contact with the inner walls of the openings formed in insulating layer 285, insulating layer 283, insulating layer 282, insulating layer 280, insulating layer 275, and insulating layer 271a, and with the side surfaces of conductive layer 240a. Furthermore, an insulating layer 241b is provided in contact with the inner walls of the openings formed in insulating layer 285, insulating layer 283, insulating layer 282, insulating layer 280, insulating layer 275, and insulating layer 271b, and with the side surfaces of conductive layer 240b.
[0270] The insulating layers 241a and 241b preferably function as barrier insulating films against hydrogen and / or oxygen. For example, silicon nitride, silicon nitride oxide, aluminum oxide, hafnium oxide, or the like is preferably used for the insulating layers 241a and 241b. Other examples of the materials that can be used include metal oxides such as magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, and tantalum oxide. The insulating layers 241a and 241b are provided in contact with the insulating layers 283, 282, and 275, respectively, and thus can prevent impurities contained in the insulating layer 280 or the like from entering the oxide semiconductor layer 230 through the conductive layers 240a and 240b. Silicon nitride is particularly suitable because of its high barrier property against hydrogen.
[0271] The insulating layer 241a is provided between the insulating layer 280 and the conductive layer 240a, and the insulating layer 241b is provided between the insulating layer 280 and the conductive layer 240b. The insulating layer 280 contains excess oxygen and is provided in the vicinity of the oxide semiconductor layer 230. The insulating layers 241a and 241b have a barrier property against oxygen, which can prevent oxygen contained in the insulating layer 280 from being absorbed by the conductive layers 240a and 240b.
[0272] 6B shows an example in which the insulating layer 241a and the insulating layer 241b each have a single-layer structure, but the present invention is not limited to this. For example, each of the insulating layer 241a and the insulating layer 241b may have a stacked structure of two or more layers.
[0273] For example, the insulating layers 241a and 241b may each have a structure in which a first insulating layer is provided in contact with the inner wall of the opening and a second insulating layer is provided further inside. When the insulating layers 241a and 241b have a stacked structure, the first insulating layer in contact with the inner wall of the opening formed in the insulating layer 280 or the like and the second insulating layer inside it preferably use a combination of a barrier insulating layer against oxygen and a barrier insulating layer against hydrogen. For example, aluminum oxide formed by the ALD method may be used as the first insulating layer, and silicon nitride formed by the PEALD method may be used as the second insulating layer. This structure can prevent the conductive layers 240a and 240b from being oxidized and further prevent hydrogen from being mixed into the conductive layers 240a and 240b.
[0274] <Capacitor element 100> The capacitor 100 is provided above the transistor 200. The capacitor 100 includes a conductive layer 110 functioning as a first electrode (also referred to as a lower electrode), a conductive layer 120 functioning as a second electrode (also referred to as an upper electrode), and an insulating layer 132 functioning as a dielectric. The pair of electrodes of the capacitor 100 is composed of the first electrode and the second electrode.
[0275] The conductive layer 110 and the conductive layer 120 can be formed using a single layer or a stack of the materials described above in the [Conductive Layer] section.
[0276] For example, the conductive layer 112 provided over the conductive layer 240a and the conductive layer 110 provided over the conductive layer 240b can be formed at the same time. In this case, the conductive layer 112 contains the same conductive material as the conductive layer 110. Note that the conductive layer 112 functions as a plug or a wiring electrically connected to the capacitor 100 or the transistor 200.
[0277] 6B shows that the conductive layer 112 and the conductive layer 110 have a single-layer structure, but the present invention is not limited to this. For example, the conductive layer 112 and the conductive layer 110 may have a stacked structure of two or more layers. For example, a conductor having a barrier property and a conductor having high adhesion to the conductor having high conductivity may be formed between a conductor having a barrier property and a conductor having high conductivity.
[0278] The insulating layer 132 can be formed using, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, aluminum nitride, hafnium oxide, hafnium oxynitride, hafnium nitride oxide, hafnium nitride, or the like, and can have a stacked layer or a single layer. Alternatively, for example, the insulating layer 132 can be formed using an insulator in which zirconium oxide, aluminum oxide, and zirconium oxide are stacked in this order.
[0279] Furthermore, for example, it is preferable to use a laminated structure of an insulator containing a material with high dielectric strength (a material with a low dielectric constant) and an insulator containing a material with a high dielectric constant (high-k) for the insulating layer 132. With this configuration, the capacitor 100 can ensure sufficient capacitance by having an insulator containing a high-k material, and the capacitor 100 can improve its dielectric strength by having an insulator containing a material with high dielectric strength, thereby suppressing electrostatic breakdown of the capacitor 100.
[0280] An insulating layer 150 is provided over the conductive layer 120 and the insulating layer 132. The insulating layer 150 functions as an interlayer film.
[0281] For example, the insulating layer 150 preferably contains the above-mentioned material with a low dielectric constant. Alternatively, the insulating layer 150 preferably has a laminated structure of an insulating layer containing an inorganic insulating material with a low dielectric constant and an insulating layer containing a resin with a low dielectric constant. Because silicon oxide and silicon oxynitride are thermally stable, combining them with a resin can provide a thermally stable laminated structure with a low dielectric constant. Using a material with a low dielectric constant for the insulating layer 150 can reduce the parasitic capacitance that occurs between wirings.
[0282] 6(A) and 6(B), the shape of the capacitor element 100 is a planar type, but the present invention is not limited to this. For example, the shape of the capacitor element 100 may be a cylindrical type as shown in FIG. 7. The semiconductor device shown in FIG. 7 has the same configuration below the insulating layer 150 as the semiconductor device shown in FIG. 6(A) and 6(B).
[0283] 7, an insulating layer 150 is disposed on an insulating layer 132, and an insulating layer 142 is disposed on the insulating layer 150. An opening 168 reaching the conductive layer 110 is formed in the insulating layer 132, the insulating layer 150, and the insulating layer 142.
[0284] 7 includes a conductive layer 115, an insulating layer 145 on the conductive layer 115 and the insulating layer 142, and a conductive layer 125 on the insulating layer 145. At least a portion of each of the conductive layer 115, the insulating layer 145, and the conductive layer 125 is disposed in the opening 168.
[0285] An insulating layer 151 is disposed on the conductive layer 125 and the insulating layer 145, an insulating layer 154 is disposed on the insulating layer 151, and a conductive layer 153 and an insulating layer 156 are disposed on the insulating layer 154. Furthermore, a conductive layer 140 is provided in openings formed in the insulating layers 132, 150, 142, 145, 151, and 154.
[0286] The conductive layer 115 functions as a first electrode of the capacitor 100, the conductive layer 125 functions as a second electrode of the capacitor 100, and the insulating layer 145 functions as a dielectric of the capacitor 100. The capacitor 100 has a configuration in which the first electrode and the second electrode face each other with a dielectric sandwiched between them on the side surface as well as the bottom surface in the opening 168, which allows the capacitance per unit area to be increased. Therefore, the deeper the opening 168, the larger the capacitance of the capacitor 100 can be. Increasing the capacitance per unit area of the capacitor 100 in this way can promote miniaturization or high integration of semiconductor devices.
[0287] The insulating layer 151 may be an insulating layer applicable to the insulating layer 150. The insulating layer 142 may be an insulating layer applicable to the insulating layer 282.
[0288] The shape of the opening 168 as viewed from above may be a rectangle, a polygon other than a rectangle, a polygon with curved corners, or a circle including an ellipse. Here, it is preferable that the overlapping area between the opening 168 and the transistor 200 is large in plan view. With such a configuration, the area occupied by a semiconductor device including the capacitor 100 and the transistor 200 can be reduced.
[0289] The conductive layer 115 is disposed in contact with the side surfaces of the insulating layer 150 and the insulating layer 142 in the opening 168. The height of the upper surface of the conductive layer 115 preferably coincides with the height of the upper surface of the insulating layer 142. The lower surface of the conductive layer 115 is in contact with the conductive layer 110 through the opening 168. The conductive layer 115 is preferably formed by an ALD method, a CVD method, or the like, and may be formed using, for example, a conductive layer that can be used for the conductive layer 215.
[0290] The insulating layer 145 is disposed to cover the conductive layer 115 and the insulating layer 142. The insulating layer 145 is preferably formed by an ALD method, a CVD method, or the like. The insulating layer 145 can be an insulating layer that can be used for the insulating layer 132.
[0291] The conductive layer 125 is disposed so as to fill the opening 168. The conductive layer 125 is preferably formed by an ALD method, a CVD method, or the like, and a conductive layer applicable to the conductive layer 215 may be used, for example.
[0292] The conductive layer 153 is provided over the insulating layer 154 and is covered with the insulating layer 156. A conductive layer applicable to the conductive layer 112 may be used for the conductive layer 153. An insulating layer applicable to the insulating layer 150 may be used for the insulating layer 156. Here, the conductive layer 153 is in contact with a top surface of the conductive layer 140 and functions as a terminal of the capacitor 100 or the transistor 200.
[0293] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.
[0294] (Embodiment 2) In this embodiment, a memory device including an OS transistor and a capacitor according to one embodiment of the present invention (hereinafter also referred to as an OS memory device) will be described with reference to FIGS. 8A to 11. The OS memory device includes at least a capacitor and an OS transistor that controls charging and discharging of the capacitor. The off-state current of the OS transistor is extremely small, so the OS memory device has excellent retention characteristics and can function as a nonvolatile memory.
[0295] <Storage device configuration example> 8A shows an example of the configuration of an OS memory device. The memory device 1400 includes a peripheral circuit 1411 and a memory cell array 1470. The peripheral circuit 1411 includes a row circuit 1420, a column circuit 1430, an output circuit 1440, and a control logic circuit 1460.
[0296] The column circuit 1430 includes, for example, a column decoder, a precharge circuit, a sense amplifier, a write circuit, etc. The precharge circuit has a function of precharging the wiring. The sense amplifier has a function of amplifying a data signal read from a memory cell. Note that the above wiring is connected to a memory cell in the memory cell array 1470, and will be described in detail later. The amplified data signal is output to the outside of the memory device 1400 as a data signal RDATA via the output circuit 1440. The row circuit 1420 also includes, for example, a row decoder, a word line driver circuit, etc., and can select a row to access.
[0297] The memory device 1400 is supplied with a low power supply voltage (VSS) from the outside as power supply voltages, a high power supply voltage (VDD) for the peripheral circuit 1411, and a high power supply voltage (VIL) for the memory cell array 1470. Control signals (CE, WEN, RES), an address signal ADDR, and a data signal WDATA are also input from the outside to the memory device 1400. The address signal ADDR is input to a row decoder and a column decoder, and the data signal WDATA is input to a write circuit.
[0298] The control logic circuit 1460 processes control signals (CE, WEN, RES) input from the outside to generate control signals for the row decoder and column decoder. The control signal CE is a chip enable signal, the control signal WEN is a write enable signal, and the control signal RES is a read enable signal. The signals processed by the control logic circuit 1460 are not limited to these, and other control signals can be input as necessary.
[0299] The memory cell array 1470 has a plurality of memory cells MC arranged in a matrix and a plurality of wirings. The number of wirings connecting the memory cell array 1470 and the row circuit 1420 is determined by the configuration of the memory cells MC, the number of memory cells MC in one column, etc. The number of wirings connecting the memory cell array 1470 and the column circuit 1430 is determined by the configuration of the memory cells MC, the number of memory cells MC in one row, etc.
[0300] 8A shows an example in which the peripheral circuit 1411 and the memory cell array 1470 are formed on the same plane; however, this embodiment is not limited to this. For example, as shown in FIG. 8B, the memory cell array 1470 may be provided so as to overlap a part of the peripheral circuit 1411. For example, a sense amplifier may be provided so as to overlap below the memory cell array 1470. OS transistors can be formed during a back-end-of-line (BEOL) process in which wiring of a memory device is formed. Therefore, when OS transistors are used in the memory cell array 1470 and transistors having silicon in their channel formation regions (hereinafter, sometimes referred to as Si transistors) are used in the peripheral circuit 1411 overlapping below the memory cell array 1470, a technique for forming OS transistors directly above the Si transistors (hereinafter, referred to as a BEOL-Tr technique) can be applied.
[0301] Alternatively, a configuration in which multiple memory cell arrays 1470 are stacked may be used. Stacking multiple memory cell arrays 1470 allows memory cells to be integrated and arranged without increasing the area occupied by the memory cell array 1470. That is, a 3D cell array can be configured. In this manner, memory cells can be highly integrated, and a semiconductor device with a large storage capacity can be provided. Note that a layer including an OS transistor is preferable because it can be monolithically stacked.
[0302] Note that the configurations of the peripheral circuit 1411, the memory cell array 1470, and the like shown in this embodiment are not limited to those described above. The arrangement or functions of these circuits, wirings connected to the circuits, circuit elements, and the like may be changed, deleted, or added as necessary. The memory device of one embodiment of the present invention has high operating speed and can retain data for a long period of time.
[0303] 9A to 9I will explain configuration examples of memory cells that can be applied to the above-described memory cell MC. FIG.
[0304] [DOSRAM] 9A to 9C show circuit configuration examples of a DRAM memory cell. In this specification and the like, a DRAM using a memory cell with one OS transistor and one capacitor may be referred to as a DOSRAM (registered trademark) (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 1471 shown in FIG. 9A includes a transistor M1 and a capacitor CA. The transistor M1 includes a gate (sometimes referred to as a top gate) and a back gate.
[0305] A first terminal of the transistor M1 is connected to a first terminal of the capacitor CA, a second terminal of the transistor M1 is connected to a wiring BIL, a gate of the transistor M1 is connected to a wiring WOL, a back gate of the transistor M1 is connected to a wiring BGL, and a second terminal of the capacitor CA is connected to a wiring LL.
[0306] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring LL functions as a wiring for applying a predetermined potential to the second terminal of the capacitor CA. When writing and reading data, the wiring LL may be at ground potential or a low-level potential. The wiring BGL functions as a wiring for applying a potential to the back gate of the transistor M1. The threshold voltage of the transistor M1 can be increased or decreased by applying an arbitrary potential to the wiring BGL.
[0307] The memory cell MC is not limited to the memory cell 1471, and the circuit configuration can be changed. For example, the memory cell MC may have a configuration in which the back gate of the transistor M1 is connected to the wiring WOL instead of the wiring BGL, as in the memory cell 1472 shown in FIG. 9B. For example, the memory cell MC may be a memory cell including a single-gate transistor, i.e., a transistor M1 without a back gate, as in the memory cell 1473 shown in FIG. 9C.
[0308] 10 shows a configuration example of a memory device including a DOSRAM. In the memory device shown in FIG. 10, a transistor 200 is provided above a transistor 300, and a capacitor 100 is provided above the transistors 300 and 200. Note that the transistor 200 described in the above embodiment can be used as the transistor 200. The capacitor 100 can be used as the capacitor 100.
[0309] When the memory device illustrated in FIG. 10 is used for the memory cell 1471, the transistor 200 can be used as the transistor M1 and the capacitor 100 can be used as the capacitor CA. By using an OS transistor as the transistor M1, the off-state current of the transistor M1 can be made very small. That is, written data can be held by the transistor M1 for a long time, so that the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be made unnecessary. Furthermore, since the off-state current is very small, multilevel data or analog data can be held in the memory cell 1471. The same applies to the memory cell 1472 and the memory cell 1473.
[0310] Furthermore, in the DOSRAM, if the sense amplifier is configured to overlap under the memory cell array 1470 as described above, the bit line can be shortened. This reduces the bit line capacitance, enabling the memory device to be driven at high speed.
[0311] 10 , a wiring 1001 is electrically connected to the source of the transistor 300, a wiring 1002 is electrically connected to the drain of the transistor 300, and a wiring 1007 is electrically connected to the gate of the transistor 300. A wiring 1003 is electrically connected to one of the source and drain of the transistor 200, a wiring 1004 is electrically connected to the first gate of the transistor 200, and a wiring 1006 is electrically connected to the second gate of the transistor 200. The other of the source and drain of the transistor 200 is electrically connected to one electrode of the capacitor 100, and a wiring 1005 is electrically connected to the other electrode of the capacitor 100.
[0312] <Transistor 300> The transistor 300 is provided over a substrate 311 and includes a conductive layer 316 functioning as a gate, an insulating layer 315 functioning as a gate insulating layer, a semiconductor region 313 formed of part of the substrate 311, and a low-resistance region 314a and a low-resistance region 314b functioning as a source region and a drain region. The transistor 300 may be either a p-channel or n-channel transistor.
[0313] Here, in the transistor 300 shown in FIG. 10, a semiconductor region 313 (a part of a substrate 311) where a channel is formed has a convex shape. A conductive layer 316 is provided to cover the side and top surfaces of the semiconductor region 313 with an insulating layer 315 interposed therebetween. The conductive layer 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN transistor because it utilizes the convex portion of the semiconductor substrate. An insulator may be provided in contact with the top of the convex portion and function as a mask for forming the convex portion. While the case where the convex portion is formed by processing a part of the semiconductor substrate has been described, a semiconductor film having a convex shape may also be formed by processing an SOI substrate.
[0314] Note that the transistor 300 illustrated in FIG. 10 is just an example, and the structure is not limited thereto. An appropriate transistor may be used depending on the circuit configuration or driving method.
[0315] <Wiring layer> Between each structure, a wiring layer provided with an interlayer film, wiring, plugs, etc. may be provided. Furthermore, multiple wiring layers may be provided depending on the design. Here, for a conductor functioning as a plug or wiring, multiple structures may be collectively assigned the same reference numeral. Furthermore, in this specification and the like, the wiring and the plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductor functions as the wiring, and cases where a part of the conductor functions as the plug.
[0316] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are stacked in this order as an interlayer film over the transistor 300. A conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. The conductive layer 328 and the conductive layer 330 function as plugs or wirings.
[0317] The insulating layer 322 may also function as a planarizing film that covers the underlying unevenness. For example, the top surface of the insulating layer 322 may be planarized by a planarization process using a CMP method or the like to enhance flatness.
[0318] A wiring layer may be provided over the insulating layer 326 and the conductive layer 330. For example, in FIG. 10, an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. A conductive layer 356 is formed over the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 functions as a plug or a wiring.
[0319] Similarly, a conductive layer 218 and a conductor that constitutes the transistor 200 are embedded in the insulating layer 210, the insulating layer 214, and the insulating layer 216. Note that the conductive layer 218 functions as a plug or wiring that is electrically connected to the transistor 300.
[0320] Here, similar to the insulating layer 241a and the insulating layer 241b described in the previous embodiment, the insulating layer 217 is provided in contact with the side surface of the conductive layer 218. The insulating layer 217 is provided in contact with the inner walls of the openings formed in the insulating layer 210, the insulating layer 214, and the insulating layer 216. In other words, the insulating layer 217 is provided between the conductive layer 218 and the insulating layer 210, the insulating layer 214, and the insulating layer 216. Note that the conductive layer 215 can be formed in parallel with the conductive layer 218, and therefore the insulating layer 217 may be formed in contact with the side surface of the conductive layer 215.
[0321] As the insulating layer 217, for example, an insulating layer applicable to the above-described insulating layer 241a and the insulating layer 241b may be used. The insulating layer 217 is provided in contact with the insulating layer 210, the insulating layer 214, and the insulating layer 222, and therefore can prevent impurities contained in the insulating layer 210, the insulating layer 216, or the like from being mixed into the oxide semiconductor layer 230 through the conductive layer 218. Silicon nitride is particularly suitable because it has a high barrier property against hydrogen. Furthermore, oxygen contained in the insulating layer 210 or the insulating layer 216 can be prevented from being absorbed by the conductive layer 218.
[0322] The insulating layer 217 can be formed by a method similar to that for the insulating layers 241a and 241b. For example, a silicon nitride film can be formed by a PEALD method, and an opening reaching the conductive layer 356 can be formed by anisotropic etching.
[0323] The insulating layer 210, the insulating layer 352, the insulating layer 354, and the like, which function as interlayer films, may be an insulating layer that can be used for the insulating layer 150.
[0324] Furthermore, the electrical characteristics of an OS transistor can be stabilized by surrounding it with an insulator that has the function of suppressing the permeation of impurities and oxygen. Therefore, the insulating layer 214, the insulating layer 350, and the like may be formed using the insulator that has the function of suppressing the permeation of impurities and oxygen, as described above in the section on "Insulating Layer."
[0325] Conductors functioning as plugs or wirings, such as the conductive layer 328, the conductive layer 330, the conductive layer 356, the conductive layer 218, and the conductive layer 112, can be any of the conductive layers described above in the section [Conductive Layer]. High-melting-point materials such as tungsten and molybdenum, which have both heat resistance and conductivity, are preferably used, and tungsten is preferred. Alternatively, low-resistance conductive materials such as aluminum and copper are preferably used. Wiring resistance can be reduced by using a low-resistance conductive material.
[0326] <Wiring or plug in layer provided with oxide semiconductor> As described in the above embodiment, the transistor 200 may be sealed with the insulating layer 214 and the insulating layer 283. With such a structure, hydrogen contained in the insulating layer 285, the insulating layer 150, and the like can be prevented from entering the insulating layer 280 and the like.
[0327] 10 , the insulating layer 241 is provided in contact with the conductive layer 240, and the insulating layer 217 is provided in contact with the conductive layer 218. By using a barrier insulating film against hydrogen as the insulating layer 241 and the insulating layer 217, it is possible to prevent hydrogen from being mixed into the insulating layer 214 and the insulating layer 283 through the conductive layer 240 and the conductive layer 218. In this manner, the transistor 200 is sealed with the insulating layer 214, the insulating layer 283, the insulating layer 241, and the insulating layer 217, and it is possible to prevent impurities contained in the insulating layer 285 and the like from being mixed in from the outside.
[0328] [NOSRAM] 9D to 9G show circuit configuration examples of a gain cell memory cell having two transistors and one capacitor. The memory cell 1474 shown in FIG. 9D includes a transistor M2, a transistor M3, and a capacitor CB. The transistor M2 has a gate and a back gate. In this specification and the like, a memory device having a gain cell memory cell using an OS transistor as the transistor M2 may be referred to as a nonvolatile oxide semiconductor RAM (NOSRAM (registered trademark)).
[0329] The first terminal of transistor M2 is connected to the first terminal of capacitor CB, the second terminal of transistor M2 is connected to wiring WBL, the gate of transistor M2 is connected to wiring WOL, and the back gate of transistor M2 is connected to wiring BGL. The second terminal of capacitor CB is connected to wiring CAL. The first terminal of transistor M3 is connected to wiring RBL, the second terminal of transistor M3 is connected to wiring SL, and the gate of transistor M3 is connected to the first terminal of capacitor CB.
[0330] The wiring WBL functions as a write bit line, the wiring RBL functions as a read bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitor CB. When writing and reading data, it is preferable to apply a high-level potential to the wiring CAL. Furthermore, when retaining data, it is preferable to apply a low-level potential to the wiring CAL. The wiring BGL functions as a wiring for applying a potential to the back gate of the transistor M2. The threshold voltage of the transistor M2 can be increased or decreased by applying an arbitrary potential to the wiring BGL.
[0331] An example of a storage device having NOSRAM is shown in Figure 11. In the storage devices described below, structures having the same functions as those constituting the storage device shown in Figure 10 are denoted by the same reference numerals. In the following, differences from the storage device described above will be mainly described, and overlapping portions will not be described.
[0332] 11 is a cross-sectional view of a memory device. The memory device illustrated in FIG. 11 differs from the memory device illustrated in FIG. 10 in that the wiring 1007 is not included and the gate of the transistor 300 is electrically connected to the other of the source and drain of the transistor 200 and one electrode of the capacitor 100.
[0333] 11, the gate of the transistor 300 and the other of the source and drain of the transistor 200 are electrically connected to one electrode of the capacitor 100. The conductive layer 316 is electrically connected to the capacitor 100 or the transistor 200 through the conductive layer 328, the conductive layer 330, the conductive layer 356, the conductive layer 218, and the conductive layer 240.
[0334] 11 is used for the memory cell 1474 or the like, the transistor 200 can be used as the transistor M2, the transistor 300 can be used as the transistor M3, and the capacitor 100 can be used as the capacitor CB. In addition, the wiring 1003 can be used as the wiring WBL, the wiring 1004 can be used as the wiring WOL, the wiring 1006 can be used as the wiring BGL, the wiring 1005 can be used as the wiring CAL, the wiring 1002 can be used as the wiring RBL, and the wiring 1001 can be used as the wiring SL.
[0335] Furthermore, the memory cell MC is not limited to the memory cell 1474, and the circuit configuration can be changed as appropriate. For example, the memory cell MC may have a configuration in which the back gate of the transistor M2 is connected to the wiring WOL instead of the wiring BGL, as in the memory cell 1475 shown in FIG. 9E. For example, the memory cell MC may be a memory cell including a single-gate transistor M2, i.e., a transistor M2 without a back gate, as in the memory cell 1476 shown in FIG. 9F. For example, the memory cell MC may have a configuration in which the wiring WBL and the wiring RBL are combined into a single wiring BIL, as in the memory cell 1477 shown in FIG. 9G.
[0336] By using an OS transistor as the transistor M2, the off-state current of the transistor M2 can be made very small. This allows written data to be held by the transistor M2 for a long time, reducing the frequency of refreshing the memory cell. Alternatively, refreshing the memory cell can be eliminated. Furthermore, the off-state current is very small, allowing multilevel data or analog data to be held in the memory cell 1474. The same applies to the memory cells 1475 to 1477.
[0337] The transistor M3 may be a Si transistor. The conductivity type of the Si transistor may be either an n-channel type or a p-channel type. The Si transistor may have a higher field-effect mobility than an OS transistor. Therefore, a Si transistor may be used as the transistor M3 functioning as a read transistor. Furthermore, by using a Si transistor as the transistor M3, the transistor M2 can be stacked on top of the transistor M3, thereby reducing the area occupied by the memory cell and achieving higher integration of the memory device.
[0338] Furthermore, the transistor M3 may be an OS transistor. When OS transistors are used for the transistors M2 and M3, the memory cell array 1470 can be configured as a circuit using only n-type transistors.
[0339] FIG. 9H shows an example of a gain cell type memory cell having three transistors and one capacitor. The memory cell 1478 shown in FIG. 9H includes transistors M4 to M6 and a capacitor CC. The capacitor CC is provided as appropriate. The memory cell 1478 is electrically connected to wirings BIL, RWL, WWL, BGL, and GNDL. The GNDL wiring is a wiring that applies a low-level potential. Note that the memory cell 1478 may be electrically connected to wirings RBL and WBL instead of wiring BIL.
[0340] The transistor M4 is an OS transistor having a back gate, and the back gate is electrically connected to the wiring BGL. Note that the back gate and the gate of the transistor M4 may be electrically connected to each other. Alternatively, the transistor M4 does not necessarily have a back gate.
[0341] Note that the transistors M5 and M6 may be n-channel Si transistors or p-channel Si transistors. Alternatively, the transistors M4 to M6 may be OS transistors. In this case, the memory cell array 1470 can be configured as a circuit using only n-channel transistors.
[0342] When the semiconductor device described in the above embodiment is used for the memory cell 1478, the transistor 200 can be used as the transistor M4, the transistors M5 and M6 can be used as the transistors M5 and M6, and the capacitor 100 can be used as the capacitor CC. By using an OS transistor as the transistor M4, the off-state current of the transistor M4 can be made very small.
[0343] 9I shows an example of a two-transistor gain cell memory cell. The memory cell 1479 shown in FIG. 9I includes a transistor M7 and a transistor M8. The memory cell 1479 is electrically connected to a wiring BIL, a wiring WWL, a wiring BGL, and a wiring SL.
[0344] The transistor M7 is an OS transistor having a back gate electrically connected to the wiring BGL. The back gate and the gate of the transistor M7 may be electrically connected to each other. Alternatively, the transistor M7 does not necessarily have a back gate.
[0345] 9I, the gate capacitance of the transistor M8 is used as a storage capacitance. That is, the memory cell 1479 can also be called a capacitor-less memory cell. The memory cell 1479 can also be considered to have a configuration in which the capacitor C B is not included in the memory cell 1477 shown in FIG. 9G, and can also be called a gain cell type memory cell with two transistors and no capacitor.
[0346] By using an OS transistor as the transistor M7, when the transistor M7 is turned off, the charge of the node electrically connected to the source electrode or the drain electrode of the transistor M7 and the gate electrode of the transistor M8 can be held for an extremely long time, thereby realizing a nonvolatile memory cell.
[0347] The transistor M8 may be an n-channel Si transistor or a p-channel Si transistor.
[0348] When the semiconductor device described in the above embodiment is used for the memory cell 1479, the transistor 200 can be used as the transistor M7, and the transistor 300 can be used as the transistor M8.
[0349] Alternatively, the transistor M8 may be an OS transistor, in which case the memory cell array 1470 can be configured as a circuit using only n-type transistors.
[0350] When the semiconductor device described in the above embodiment is used for the memory cell 1479, the transistor 200 can be used as the transistors M7 and M8. With this structure, the transistors M7 and M8 can be formed in the same layer. Therefore, compared to the case where the transistors M7 and M8 are provided in different layers, the manufacturing process for stacking layers including the memory cell 1479 can be simplified, and productivity can be improved.
[0351] When the transistor 200 is used as the transistor M7 and the transistor M8, the components of the transistor (including the channel length, channel width, cross-sectional shape, etc.) can be set appropriately according to the characteristics required for the transistor M7 and the transistor M8.
[0352] Regardless of the semiconductor material used for the transistors M1 to M8, the structures of the transistors M1 to M8 are not particularly limited. For example, planar transistors, staggered transistors, inverted staggered transistors, vertical channel transistors, etc. may be used. The transistors M1 to M8 may have either a top-gate or bottom-gate structure. Alternatively, gates may be provided above and below a semiconductor layer in which a channel is formed.
[0353] As described above, a configuration may be adopted in which multiple memory cell arrays 1470 are stacked. By stacking multiple memory cell arrays 1470, memory cells can be integrated and arranged without increasing the area occupied by the memory cell arrays 1470. In other words, a 3D cell array can be configured.
[0354] The structures and methods described in this embodiment can be used in appropriate combination with other structures and methods described in this embodiment or structures and methods described in other embodiments.
[0355] (Embodiment 3) In this embodiment, an OS transistor will be described. Note that the description of the OS transistor will also be briefly compared with a Si transistor.
[0356] For the OS transistor, an oxide semiconductor with a low carrier concentration is preferably used. For example, the carrier concentration of a channel formation region of the oxide semiconductor is 1×10 18 cm -3 Less than 1 × 10 17 cm -3 less than 1×10 16 cm -3 less than 1×10 13 cm -3 less than 1×10 10 cm -3 Less than 1 x 10 -9 cm -3 That is all. Note that when the carrier concentration of an oxide semiconductor film is reduced, it is preferable to reduce the impurity concentration in the oxide semiconductor film and reduce the density of defect states. In this specification and the like, a semiconductor having a low impurity concentration and a low density of defect states is referred to as a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor. Note that an oxide semiconductor having a low carrier concentration may be referred to as a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor.
[0357] Furthermore, a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor may have a low density of trap states due to a low density of defect states. Charges trapped in trap states of the oxide semiconductor take a long time to disappear and may behave like fixed charges. Therefore, a transistor in which a channel formation region is formed in an oxide semiconductor with a high density of trap states may have unstable electrical characteristics.
[0358] Therefore, reducing the impurity concentration in the oxide semiconductor is effective for stabilizing the electrical characteristics of a transistor. Furthermore, in order to reduce the impurity concentration in the oxide semiconductor, it is preferable to also reduce the impurity concentration in adjacent films. Examples of impurities include hydrogen and nitrogen. Note that the term "impurity" in an oxide semiconductor refers to, for example, any element other than the main component constituting the oxide semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity.
[0359] The band gap of the oxide semiconductor is preferably larger than that of silicon (typically 1.1 eV), preferably 2 eV or more, more preferably 2.5 eV or more, and further preferably 3.0 eV or more. By using an oxide semiconductor having a band gap larger than that of silicon, the off-state current (also referred to as Ioff) of the transistor can be reduced.
[0360] Furthermore, as Si transistors are miniaturized, a short channel effect (also known as SCE) occurs. This makes miniaturization of Si transistors difficult. One of the reasons for the short channel effect is the small band gap of silicon. On the other hand, OS transistors use an oxide semiconductor, which is a semiconductor material with a wide band gap, and therefore the short channel effect can be suppressed. In other words, OS transistors are transistors that do not have the short channel effect or have an extremely small short channel effect.
[0361] The short channel effect is a degradation of electrical characteristics that becomes apparent as transistors become smaller (reduced channel length). Specific examples of short channel effects include a decrease in threshold voltage, an increase in subthreshold swing (sometimes referred to as S value), and an increase in leakage current. Here, the S value refers to the amount of change in gate voltage in the subthreshold region that changes the drain current by one order of magnitude at a constant drain voltage.
[0362] Furthermore, the characteristic length is widely used as an index of resistance to short channel effects. Characteristic length is an index of how easily the potential in the channel formation region bends. The smaller the characteristic length, the steeper the potential rises, and therefore the more resistant it is to short channel effects.
[0363] An OS transistor is an accumulation-mode transistor, while a Si transistor is an inversion-mode transistor. Therefore, compared with a Si transistor, an OS transistor has a smaller characteristic length between the source region and the channel formation region and between the drain region and the channel formation region. Therefore, an OS transistor is more resistant to the short-channel effect than a Si transistor. That is, when a transistor with a short channel length is to be fabricated, an OS transistor is more suitable than a Si transistor.
[0364] Even when the carrier concentration of the oxide semiconductor is reduced to the point where the channel formation region becomes i-type or substantially i-type, the conduction band minimum of the channel formation region in a short-channel transistor is lowered due to the conduction-band-lowering (CBL) effect, so that the energy difference between the conduction band minimums of the source or drain region and the channel formation region can be reduced to 0.1 eV or more and 0.2 eV or less. As a result, the channel formation region of an OS transistor can be reduced to n - The source and drain regions are n-type regions. + The domain of type, n + / n - / n + accumulation-type junction-less transistor structure, or, n + / n - / n + This can also be regarded as an accumulation-type non-junction transistor structure.
[0365] By using the above-described structure, the OS transistor can have good electrical characteristics even when miniaturized or highly integrated. For example, good electrical characteristics can be obtained even when the gate length of the OS transistor is 20 nm or less, 15 nm or less, 10 nm or less, 7 nm or less, or 6 nm or less, or 1 nm or more, 3 nm or more, or 5 nm or more. On the other hand, since a short-channel effect occurs in a Si transistor, it may be difficult to achieve a gate length of 20 nm or less or 15 nm or less. Therefore, the OS transistor can be suitably used as a transistor having a shorter channel length than a Si transistor. Note that the gate length is the length of the gate electrode in the direction in which carriers move inside the channel formation region during transistor operation.
[0366] Furthermore, miniaturization of an OS transistor can improve the high-frequency characteristics of the transistor. Specifically, the cutoff frequency of the transistor can be improved. When the gate length of the OS transistor is within the above range, the cutoff frequency of the transistor can be set to 50 GHz or higher, preferably 100 GHz or higher, and more preferably 150 GHz or higher, for example, at room temperature.
[0367] As described above, compared to Si transistors, OS transistors have excellent advantages such as a smaller off-state current and the ability to be fabricated as transistors with a short channel length.
[0368] The structures, configurations, methods, and the like described in this embodiment can be used in appropriate combination with structures, configurations, methods, and the like described in other embodiments.
[0369] (Fourth embodiment) This embodiment will describe electronic components, electronic devices, mainframes, space equipment, and data centers (also referred to as data centers (DCs)) that can use the semiconductor devices described in the above embodiments. The electronic components, electronic devices, mainframes, space equipment, and data centers that use the semiconductor device of one embodiment of the present invention are effective in achieving high performance, such as low power consumption.
[0370] [Electronic Components] FIG. 12A shows a perspective view of a substrate (mounting substrate 704) on which electronic component 700 is mounted. Electronic component 700 shown in FIG. 12A has semiconductor device 710 inside mold 711. FIG. 12A omits some parts to show the interior of electronic component 700. Electronic component 700 has lands 712 on the outside of mold 711. Lands 712 are electrically connected to electrode pads 713, and electrode pads 713 are electrically connected to semiconductor device 710 via wires 714. Electronic component 700 is mounted on, for example, a printed circuit board 702. A plurality of such electronic components are combined and electrically connected on printed circuit board 702 to complete mounting substrate 704.
[0371] The semiconductor device 710 also includes a drive circuit layer 715 and a memory layer 716. The memory layer 716 has a configuration in which multiple memory cell arrays are stacked. The memory layer 716 may have a configuration in which a single layer including a memory cell array is provided. The stacked configuration of the drive circuit layer 715 and the memory layer 716 can be a monolithic stacked configuration. In a monolithic stacked configuration, the layers can be connected without using through-electrode technology such as TSV (Through Silicon Via) or bonding technology such as Cu-Cu direct bonding. By monolithically stacking the drive circuit layer 715 and the memory layer 716, for example, a so-called on-chip memory configuration can be achieved, in which the memory is formed directly on the processor. The on-chip memory configuration enables the operation of the interface between the processor and the memory to be faster.
[0372] Furthermore, by configuring on-chip memory, it is possible to reduce the size of connection wiring, etc., compared to technologies that use through-electrodes such as TSV, and therefore it is possible to increase the number of connection pins. Increasing the number of connection pins enables parallel operation, which makes it possible to improve the memory bandwidth (also called memory bandwidth).
[0373] It is also preferable that the memory cell arrays included in the memory layer 716 are formed using OS transistors and that the memory cell arrays are monolithically stacked. By configuring the memory cell arrays as a monolithic stack, it is possible to improve either or both of the memory bandwidth and the memory access latency. Note that the bandwidth is the amount of data transferred per unit time, and the access latency is the time from access to the start of data exchange. Note that when Si transistors are used in the memory layer 716, it is more difficult to achieve a monolithic stack configuration than OS transistors. Therefore, it can be said that OS transistors have a superior structure to Si transistors in a monolithic stack configuration.
[0374] The semiconductor device 710 may also be referred to as a die. In this specification and the like, a die refers to a chip piece obtained by forming a circuit pattern on, for example, a disk-shaped substrate (also called a wafer) and dicing it into cubes during the semiconductor chip manufacturing process. Semiconductor materials that can be used for the die include, for example, silicon (Si), silicon carbide (SiC), and gallium nitride (GaN). For example, a die obtained from a silicon substrate (also called a silicon wafer) may be called a silicon die.
[0375] 12(B) shows a perspective view of an electronic component 730. The electronic component 730 is an example of a SiP (System in Package) or an MCM (Multi Chip Module). The electronic component 730 has an interposer 731 provided on a package substrate 732 (printed circuit board), and a semiconductor device 735 and multiple semiconductor devices 710 provided on the interposer 731.
[0376] The electronic component 730 shows an example in which the semiconductor device 710 is used as a high bandwidth memory (HBM). The semiconductor device 735 can be used in an integrated circuit such as a CPU, a GPU, or an FPGA (Field Programmable Gate Array).
[0377] For example, a ceramic substrate, a plastic substrate, or a glass epoxy substrate can be used for the package substrate 732. For example, a silicon interposer or a resin interposer can be used for the interposer 731.
[0378] The interposer 731 has multiple wirings and functions to electrically connect multiple integrated circuits with different terminal pitches. The multiple wirings are provided in a single layer or multiple layers. The interposer 731 also functions to electrically connect the integrated circuits provided on the interposer 731 to electrodes provided on the package substrate 732. For these reasons, the interposer is sometimes called a "rewiring substrate" or "intermediate substrate." In some cases, through electrodes are provided in the interposer 731, and the integrated circuits and the package substrate 732 are electrically connected using the through electrodes. In addition, with a silicon interposer, TSVs can also be used as through electrodes.
[0379] HBM requires many interconnects to achieve a wide memory bandwidth. Therefore, the interposer that implements HBM requires fine and high-density interconnects. Therefore, it is preferable to use a silicon interposer for implementing HBM.
[0380] Furthermore, SiPs and MCMs that use silicon interposers are less likely to experience a decrease in reliability due to differences in the coefficient of expansion between the integrated circuit and the interposer. Furthermore, because the silicon interposer has a highly flat surface, poor connection between the integrated circuit mounted on the silicon interposer and the silicon interposer is less likely to occur. It is particularly preferable to use silicon interposers in 2.5D packages (2.5-dimensional packaging), in which multiple integrated circuits are arranged horizontally on an interposer.
[0381] On the other hand, when electrically connecting multiple integrated circuits with different terminal pitches using a silicon interposer, TSVs, or the like, a space is required to accommodate the terminal pitch. Therefore, when attempting to reduce the size of the electronic component 730, the terminal pitch becomes an issue, making it difficult to provide the large number of interconnects required to achieve a wide memory bandwidth. Therefore, as described above, a monolithic stacked structure using OS transistors is preferable. A composite structure may also be used that combines a memory cell array stacked using TSVs with a monolithic stacked memory cell array.
[0382] A heat sink (heat sink) may be provided overlapping the electronic component 730. When a heat sink is provided, it is preferable to align the height of the integrated circuit provided on the interposer 731. For example, in the electronic component 730 shown in this embodiment, it is preferable to align the height of the semiconductor device 710 and the height of the semiconductor device 735.
[0383] Electrodes 733 may be provided on the bottom of the package substrate 732 in order to mount the electronic component 730 on another substrate. FIG. 12B shows an example in which the electrodes 733 are formed of solder balls. By providing solder balls in a matrix on the bottom of the package substrate 732, BGA (Ball Grid Array) mounting can be achieved. Alternatively, the electrodes 733 may be formed of conductive pins. By providing conductive pins in a matrix on the bottom of the package substrate 732, PGA (Pin Grid Array) mounting can be achieved.
[0384] The electronic component 730 can be mounted on other substrates using various mounting methods, including but not limited to BGA and PGA, such as a staggered pin grid array (SPGA), a land grid array (LGA), a quad flat package (QFP), a quad flat J-leaded package (QFJ), and a quad flat non-leaded package (QFN).
[0385] [Electronic equipment] Next, a perspective view of an electronic device 6500 is shown in FIG. 13A. The electronic device 6500 shown in FIG. 13A is a portable information terminal that can be used as a smartphone. The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, a control device 6509, and the like. Note that the control device 6509 includes, for example, one or more selected from a CPU, a GPU, and a memory device. The semiconductor device of one embodiment of the present invention can be applied to the display portion 6502, the control device 6509, and the like.
[0386] 13B is an information terminal that can be used as a notebook computer. The electronic device 6600 includes a housing 6611, a keyboard 6612, a pointing device 6613, an external connection port 6614, a display portion 6615, a control device 6616, and the like. Note that the control device 6616 includes, for example, one or more selected from a CPU, a GPU, and a memory device. The semiconductor device of one embodiment of the present invention can be applied to the display portion 6615, the control device 6616, and the like. Note that the use of the semiconductor device of one embodiment of the present invention in the control device 6509 and the control device 6616 is preferable because power consumption can be reduced.
[0387] [Large computer] 13C shows a perspective view of the mainframe 5600. The mainframe 5600 shown in FIG. 13C has a rack 5610 housing a plurality of rack-mounted computers 5620. The mainframe 5600 may also be called a supercomputer.
[0388] The computer 5620 can have the configuration shown in the perspective view of Fig. 13(D), for example. In Fig. 13(D), the computer 5620 has a motherboard 5630, which has a plurality of slots 5631 and a plurality of connection terminals. A PC card 5621 is inserted into the slot 5631. In addition, the PC card 5621 has connection terminals 5623, 5624, and 5625, which are each connected to the motherboard 5630.
[0389] A PC card 5621 shown in FIG. 13E is an example of a processing board including a CPU, a GPU, a storage device, and the like. The PC card 5621 includes a board 5622. The board 5622 includes a connection terminal 5623, a connection terminal 5624, a connection terminal 5625, a semiconductor device 5626, a semiconductor device 5627, a semiconductor device 5628, and a connection terminal 5629. Note that FIG. 13E illustrates semiconductor devices other than the semiconductor device 5626, the semiconductor device 5627, and the semiconductor device 5628, but for these semiconductor devices, the following descriptions of the semiconductor device 5626, the semiconductor device 5627, and the semiconductor device 5628 can be referred to.
[0390] Connection terminal 5629 has a shape that allows it to be inserted into slot 5631 of motherboard 5630, and connection terminal 5629 functions as an interface for connecting PC card 5621 and motherboard 5630. An example of the standard for connection terminal 5629 is PCI Express (registered trademark).
[0391] Connection terminals 5623, 5624, and 5625 can be interfaces for supplying power to PC card 5621, inputting signals, and the like. They can also be interfaces for outputting signals calculated by PC card 5621, and the like. Examples of standards for connection terminals 5623, 5624, and 5625 include USB (Universal Serial Bus), SATA (Serial ATA), and SCSI (Small Computer System Interface). Examples of standards for outputting video signals from connection terminals 5623, 5624, and 5625 include HDMI (registered trademark).
[0392] The semiconductor device 5626 has a terminal (not shown) for inputting and outputting signals, and the semiconductor device 5626 and the board 5622 can be electrically connected by inserting the terminal into a socket (not shown) provided on the board 5622.
[0393] The semiconductor device 5627 has a plurality of terminals, and the semiconductor device 5627 can be electrically connected to the board 5622 by, for example, reflow soldering the terminals to wiring provided on the board 5622. Examples of the semiconductor device 5627 include an FPGA, a GPU, and a CPU. For example, the electronic component 730 can be used as the semiconductor device 5627.
[0394] The semiconductor device 5628 has a plurality of terminals, and the semiconductor device 5628 can be electrically connected to the board 5622 by, for example, reflow soldering the terminals to wiring provided on the board 5622. Examples of the semiconductor device 5628 include a memory device. For example, the electronic component 700 can be used as the semiconductor device 5628.
[0395] The mainframe computer 5600 can also function as a parallel computer. By using the mainframe computer 5600 as a parallel computer, it is possible to perform large-scale calculations required for, for example, learning and inference in artificial intelligence.
[0396] [Space equipment] The semiconductor device of one embodiment of the present invention can be suitably used in space equipment such as equipment for processing and storing information.
[0397] A semiconductor device according to one embodiment of the present invention can include an OS transistor. The OS transistor exhibits small changes in electrical characteristics due to radiation exposure. In other words, the OS transistor has high radiation resistance and can be suitably used in an environment where radiation may be incident. For example, the OS transistor can be suitably used in outer space.
[0398] Fig. 14 shows an artificial satellite 6800 as an example of space equipment. The artificial satellite 6800 has a body 6801, a solar panel 6802, an antenna 6803, a secondary battery 6805, and a control device 6807. In Fig. 14, a planet 6804 is shown in outer space. Note that outer space refers to an altitude of 100 km or higher, for example, but the outer space described in this specification may also include the thermosphere, mesosphere, and stratosphere.
[0399] 14, a battery management system (also referred to as a BMS) or a battery control circuit may be provided for the secondary battery 6805. The use of an OS transistor in the battery management system or the battery control circuit is preferable because it has low power consumption and high reliability even in space.
[0400] Furthermore, outer space is an environment with radiation levels 100 times higher than on Earth. Examples of radiation include electromagnetic waves (electromagnetic radiation) such as X-rays and gamma rays, as well as particle radiation such as alpha rays, beta rays, neutron rays, proton rays, heavy ion rays, and meson rays.
[0401] When sunlight is irradiated onto the solar panel 6802, the power required for the operation of the satellite 6800 is generated. However, for example, in a situation where sunlight is not irradiated onto the solar panel or where the amount of sunlight irradiating the solar panel is small, the generated power is small. Therefore, there is a possibility that the power required for the operation of the satellite 6800 will not be generated. In order to operate the satellite 6800 even in a situation where the generated power is small, it is recommended to provide a secondary battery 6805 in the satellite 6800. Note that the solar panel may also be called a solar cell module.
[0402] The satellite 6800 can generate a signal. The signal is transmitted via an antenna 6803, and can be received by, for example, a receiver on the ground or another satellite. By receiving the signal transmitted by the satellite 6800, the position of the receiver that received the signal can be determined. As described above, the satellite 6800 can constitute a satellite positioning system.
[0403] The control device 6807 has a function of controlling the satellite 6800. The control device 6807 is configured using, for example, one or more selected from a CPU, a GPU, and a storage device. Note that the control device 6807 is preferably an OS transistor according to one embodiment of the present invention. The OS transistor has smaller variations in electrical characteristics due to radiation exposure than a Si transistor. That is, the OS transistor has high reliability even in an environment where radiation may be incident, and can be preferably used.
[0404] The artificial satellite 6800 can also be configured to include a sensor. For example, by including a visible light sensor, the artificial satellite 6800 can have the function of detecting sunlight reflected from an object on the ground. Alternatively, by including a thermal infrared sensor, the artificial satellite 6800 can have the function of detecting thermal infrared rays emitted from the earth's surface. As described above, the artificial satellite 6800 can function as, for example, an earth observation satellite.
[0405] Although an artificial satellite is described as an example of space equipment in this embodiment, the present invention is not limited thereto. For example, the semiconductor device of one embodiment of the present invention can be suitably used in space equipment such as a spaceship, a space capsule, or a space probe.
[0406] As described above, compared to Si transistors, OS transistors have the advantages of being able to achieve a wider memory bandwidth and having higher radiation resistance.
[0407] [Data Center] The semiconductor device of one embodiment of the present invention can be suitably used in a storage system applied to, for example, a data center. The data center is required to perform long-term data management, such as ensuring data immutability. To manage long-term data, the building must be large enough to accommodate the installation of storage devices and servers for storing a huge amount of data, a stable power source for storing the data, or cooling equipment required for storing the data.
[0408] By using the semiconductor device of one embodiment of the present invention in a storage system applied to a data center, it is possible to reduce the power required to store data and the size of the semiconductor device that stores data. Therefore, it is possible to reduce the size of the storage system, the size of the power supply for storing data, the scale of the cooling equipment, and the like. Therefore, it is possible to reduce the space required for the data center.
[0409] Furthermore, the semiconductor device of one embodiment of the present invention has low power consumption, which allows heat generation from the circuit to be reduced. Therefore, adverse effects of the heat generation on the circuit itself, peripheral circuits, and modules can be reduced. Furthermore, by using the semiconductor device of one embodiment of the present invention, a data center that operates stably even in a high-temperature environment can be realized. Therefore, the reliability of the data center can be improved.
[0410] Fig. 15 shows a storage system applicable to a data center. The storage system 7000 shown in Fig. 15 has a plurality of servers 7001sb as hosts 7001 (illustrated as Host Computers). It also has a plurality of storage devices 7003md as storage 7003 (illustrated as Storage). The host 7001 and storage 7003 are shown connected via a storage area network 7004 (illustrated as SAN: Storage Area Network) and a storage control circuit 7002 (illustrated as Storage Controller).
[0411] The host 7001 corresponds to a computer that accesses data stored in the storage 7003. The hosts 7001 may be connected to each other via a network.
[0412] Although the storage 7003 uses flash memory to reduce the data access speed, i.e., the time required to store and output data, this time is significantly longer than the time required for DRAM, which can be used as cache memory within the storage. In order to solve the problem of the long access speed of the storage 7003, a storage system typically provides cache memory within the storage to reduce the time required to store and output data.
[0413] The above-mentioned cache memory is used in the storage control circuit 7002 and the storage 7003. Data exchanged between the host 7001 and the storage 7003 is stored in the cache memory in the storage control circuit 7002 and the storage 7003, and then output to the host 7001 or the storage 7003.
[0414] By using OS transistors as transistors for storing data in the cache memory and holding a potential corresponding to the data, the frequency of refresh operations can be reduced, thereby lowering power consumption.Furthermore, by using a stacked memory cell array, miniaturization is possible.
[0415] Note that the application of a semiconductor device according to one embodiment of the present invention to one or more of electronic components, electronic devices, mainframe computers, space equipment, and data centers is expected to have an effect of reducing power consumption. Therefore, while energy demand is expected to increase with the improvement in performance or integration of semiconductor devices, the use of a semiconductor device according to one embodiment of the present invention can also reduce emissions of greenhouse gases, typified by carbon dioxide (CO). Furthermore, the semiconductor device according to one embodiment of the present invention is effective as a countermeasure against global warming due to its low power consumption.
[0416] The structures, configurations, methods, and the like described in this embodiment can be used in appropriate combination with structures, configurations, methods, and the like described in other embodiments. [Example]
[0417] In this example, a sample containing tantalum nitride was prepared, and the film formation condition dependency of tantalum nitride was evaluated. Specifically, the composition, conductivity, resistivity, and the like of tantalum nitride were obtained. In addition, a transistor containing tantalum nitride was prepared, and the electrical characteristics of the transistor were evaluated. Specifically, the Id-Vg characteristics of the transistor were obtained. Note that tantalum nitride described in this example can be rephrased as a tantalum compound.
[0418] <Dependence of tantalum nitride film formation conditions> In this section, we will explain the film formation condition dependency of tantalum nitride.
[0419] [Sample preparation 1] In this example, Samples 1A to 11A, Samples 1B to 11B, Samples 1C to 11C, and Samples 1D to 11D were fabricated. Hereinafter, Samples 1A to 11A may be collectively referred to as Sample Group A. Samples 1B to 11B may be collectively referred to as Sample Group B. Samples 1C to 11C may be collectively referred to as Sample Group C. Samples 1D to 11D may be collectively referred to as Sample Group D.
[0420] 16(A) shows a schematic cross-sectional view of sample group A and sample group B. As shown in Fig. 16(A), each of sample group A and sample group B has a layer 901, a layer 902 on layer 901, and a layer 903 on layer 902.
[0421] 16(B) shows a schematic cross-sectional view of sample group C and sample group D. As shown in FIG. 16(B), each of sample group C and sample group D has a layer 901, a layer 902 on layer 901, a layer 904 on layer 902, and a layer 903 on layer 904.
[0422] First, a description will be given of a method for manufacturing the sample group A. The structure of the sample group A is the same except that the deposition conditions for the layer 903 are different.
[0423] First, a silicon substrate was prepared as a layer 901. Next, a silicon oxide film with a thickness of 100 nm was formed as a layer 902. This silicon oxide film may be referred to as SiO2.
[0424] Next, a tantalum nitride film with a thickness of 50 nm was formed as the layer 903 by reactive sputtering using a tantalum target and nitrogen (N2) gas. For all samples 1A to 11A, the tantalum nitride film was formed with a target-substrate distance of 286 mm and a substrate temperature of room temperature. This tantalum nitride film may be referred to as SiNx.
[0425] Other deposition conditions for the tantalum nitride film are shown in Table 1. Note that "Sample name" in Table 1 is the sample name, "N2 / (N2+Ar)" in Table 1 is the nitrogen flow rate ratio, "Plasma power" in Table 1 is DC power, and "Pressure" in Table 1 is the deposition pressure. Table 1 also lists the results of XPS analysis of the tantalum nitride film contained in each of sample group A. The N / Ta ratio in Table 1 is the ratio of the number of nitrogen atoms to tantalum. Details of the XPS analysis will be described later.
[0426] [Table 1]
[0427] As a result, sample group A was prepared.
[0428] Next, a manufacturing method for Sample Group B will be described. Note that in the manufacturing method for Sample Group B, the steps up to the formation of the tantalum nitride film are the same as those in the manufacturing method for Sample Group A, and therefore the manufacturing method for Sample Group A described above can be referred to. Furthermore, for the deposition conditions of the tantalum nitride films for Samples 1B to 11B, Table 1 can be referred to by replacing Samples 1A to 11A in Table 1 with Samples 1B to 11B, respectively.
[0429] After forming a tantalum nitride film as the layer 903, a heat treatment was carried out at a temperature of 400° C. for 1 hour in a nitrogen atmosphere.
[0430] Thus, sample group B was prepared.
[0431] Next, a manufacturing method of Sample Group C will be described. Sample Group C differs from Sample Group A in that a layer 904 is provided between a layer 902 and a layer 903. The manufacturing method of Sample Group A described above can be referred to for the method of forming the layers 901, 902, and 903 in Sample Group C. In addition, Table 1 can be referred to for the deposition conditions of the tantalum nitride films in Samples 1C to 11C by replacing Samples 1A to 11A in Table 1 with Samples 1C to 11C, respectively.
[0432] A 50-nm-thick In-Ga-Zn oxide film was formed by sputtering as the layer 904. Since the In-Ga-Zn oxide film has a CAAC structure, the In-Ga-Zn oxide film may be referred to as CAAC-IGZO.
[0433] As a result, sample group C was prepared.
[0434] Next, a method for fabricating sample group D will be described. Note that in the method for fabricating sample group D, the steps up to the deposition of the tantalum nitride film are the same as those in the method for fabricating sample group C, and therefore the above-described method for fabricating sample group C can be referenced. Furthermore, for the deposition conditions of the tantalum nitride films of samples 1D to 11D, Table 1 can be referenced by replacing samples 1A to 11A in Table 1 with samples 1D to 11D, respectively.
[0435] After forming a tantalum nitride film as the layer 903, a heat treatment was carried out at a temperature of 400° C. for 1 hour in a nitrogen atmosphere.
[0436] As a result, sample group D was prepared.
[0437] As described above, the deposition conditions for the tantalum nitride films of Samples 1A, 1B, 1C, and 1D are the same. Therefore, these may be collectively referred to as Index 1. Similarly, Samples 2A, 2B, 2C, and 2D may be collectively referred to as Index 2. The same applies to Indexes 3 to 11.
[0438] [composition] XPS analysis was performed on the tantalum nitride films contained in each of sample group A. For the XPS analysis, Quantera SXM and Quantera II manufactured by PHI Corporation were used. Monochromated Al Kα rays (1486.6 eV) were used as the X-ray source. The detection area was 100 μmφ. The take-off angle was 90°. The detection depth was estimated to be approximately 8 nm.
[0439] The results of the XPS analysis of the tantalum nitride films contained in each of Sample Group A are shown in Table 1.
[0440] From Table 1, it was confirmed that the lower the nitrogen flow rate ratio, the lower the N / Ta ratio. It was also confirmed that the higher the DC power, the lower the N / Ta ratio. However, for Samples 4A to 6A, the N / Ta ratios were almost the same despite the different DC powers.
[0441] The XPS spectra of tantalum 4f for each sample obtained by XPS analysis are shown in Figures 17(A) to 18(H). The XPS spectrum of tantalum 4f shown in Figure 17(A) is the result for Sample 1A, the XPS spectrum of tantalum 4f shown in Figure 17(B) is the result for Sample 2A, and the XPS spectrum of tantalum 4f shown in Figure 17(C) is the result for Sample 3A. The XPS spectrum of tantalum 4f shown in Figure 18(A) is the result for Sample 4A, the XPS spectrum of tantalum 4f shown in Figure 18(B) is the result for Sample 5A, the XPS spectrum of tantalum 4f shown in Figure 18(C) is the result for Sample 6A, and the XPS spectrum of tantalum 4f shown in Figure 18(D) is the result for Sample 7A. The XPS spectrum of tantalum 4f shown in Figure 18(E) is the result for sample 8A, the XPS spectrum of tantalum 4f shown in Figure 18(F) is the result for sample 9A, the XPS spectrum of tantalum 4f shown in Figure 18(G) is the result for sample 10A, and the XPS spectrum of tantalum 4f shown in Figure 18(H) is the result for sample 11A. The bonding state of tantalum was evaluated using the XPS spectra of tantalum 4f shown in Figures 17(A) to 18(H).
[0442] FIG. 19 shows the results of XPS analysis of the tantalum nitride films contained in each of the samples in sample group A. In FIG. 19, the horizontal axis indicates the sample name, the first vertical axis (left vertical axis) indicates the abundance ratio (percent) of each bonding state of tantalum, and the bar graph indicates the abundance ratio of each bonding state of tantalum. FIG. 19 also shows the results of measuring the sheet resistance of the tantalum nitride films contained in each of the samples in sample group A. In FIG. 19, the second vertical axis (right vertical axis) indicates the conductivity 1 / ρ [S / cm] of the tantalum nitride film, and the line graph indicates the conductivity of the tantalum nitride film. Details of the measurement of the sheet resistance will be described later.
[0443] FIG. 19 shows the abundance ratio of each bonding state of tantalum. The calculation method for the abundance ratio of the bonding state of tantalum can be found in the description of the first embodiment. Specifically, the abundance ratio of the bonding state of tantalum was calculated using waveform separation of the bonding state of the tantalum 4f orbital. Ta(N<1) in FIG. 19 indicates the bonding state of metallic tantalum and the bonding state of tantalum nitride in which the nitrogen content per tantalum is stoichiometrically small, and corresponds to the first bonding state of tantalum described in the first embodiment. Ta(N=1) in FIG. 19 indicates the bonding state of tantalum nitride in which the nitrogen content per tantalum is stoichiometrically equal, and the bonding state of tantalum oxynitride with a low oxygen content (the bonding state of tantalum nitride oxide), and corresponds to the second bonding state of tantalum described in the first embodiment. Ta(N>1) in FIG. 19 indicates the bonding state of tantalum nitride in which the nitrogen content per tantalum is stoichiometrically large, and corresponds to the third bonding state of tantalum described in the first embodiment. 19 indicates the bonding state of tantalum oxynitride, which corresponds to the fourth bonding state of tantalum described in embodiment 1. Ta2O5 shown in Fig. 19 indicates the bonding state of tantalum oxide, which corresponds to the fifth bonding state of tantalum described in embodiment 1.
[0444] The sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N=1) was 1.4% in sample 1A, 1.4% in sample 2A, 1.9% in sample 3A, 6.5% in sample 4A, 13.5% in sample 5A, 32.2% in sample 6A, 56.3% in sample 7A, 58.1% in sample 8A, 62.6% in sample 9A, 65.3% in sample 10A, and 73.1% in sample 11A. The abundance ratio of Ta(N<1) was 0% in samples 1A to 7A, 1.1% in sample 8A, 27.3% in sample 9A, 56% in sample 10A, and 63.1% in sample 11A.
[0445] 19, it was confirmed that the abundance ratio of the bonding state of tantalum changes by adjusting the DC power. Specifically, it was confirmed that the abundance ratio of the bonding state of tantalum tends to change as the DC power decreases, such that the bonding state of tantalum changes from Ta(N<1) to Ta(N=1) and from Ta(N=1) to Ta(N>1).
[0446] 19, it was confirmed that the bonding state of tantalum contained in Samples 1A to 3A was mainly Ta(N>1). The abundance ratio of Ta(N>1) was 73.2% in Sample 1A, 76.2% in Sample 2A, and 77.9% in Sample 3A.
[0447] [Resistivity, conductivity] The sheet resistance of each tantalum nitride film included in sample group A was measured using a sheet resistance meter. The sheet resistance meter used had an upper measurement limit of 90 MΩ / sq. The sheet resistance was converted to resistivity ρ by multiplying it by the film thickness (50 nm) of the tantalum nitride film. From this, the upper measurement limit of resistivity in this example was found to be 4.5×10 2 In addition, the conductivity was calculated from the resistivity ρ by taking the reciprocal of the resistivity ρ.
[0448] The measurement results of the sheet resistance values of the tantalum nitride films included in each of sample groups A, B, C, and D are shown in Table 2, FIG. 19, and FIG.
[0449] [Table 2]
[0450] The index shown in Table 2 is an index, and the resistivity shown in Table 2 is the resistivity of the tantalum nitride film. In Table 2, samples with sheet resistance values at the upper limit of measurement are marked with ">4.5×10 2 Table 2 shows the on-current I calculated from the Id-Vg characteristics. on , threshold voltage V th , σ(V th In Table 2, the on-state current I on Average value of threshold voltage V th The Id-Vg characteristics will be described in detail later. Sample group E will also be described later.
[0451] In FIG. 20, the horizontal axis represents the index, and the first vertical axis (left vertical axis) represents the resistivity [Ωcm]. The dotted line in FIG. 20 represents the measurement limit of the resistivity. Note that FIG. 20 also shows the N / Ta ratio. In FIG. 20, the second vertical axis (right vertical axis) represents the N / Ta ratio, and the black circles represent the N / Ta ratio.
[0452] 20, the resistivity of the tantalum nitride films in Samples 1A to 3A and Samples 1B to 3B was high, which indicates that they are not suitable for use as transistor electrodes. On the other hand, the resistivity of the tantalum nitride films in Samples 4A to 11A and Samples 4B to 11B was low. In particular, the resistivity of the tantalum nitride films in Samples 7A to 11A and Samples 7B to 11B was 2.59×10 -4 Ωcm to 3.75 x 10 -4 It was in the Ωcm range.
[0453] Furthermore, from the results of Samples 4A to 7A, the resistivity decreased from 3.19 × 10 to 3.19 × 10 as the DC power was reduced from 1.3 kW to 0.5 kW. -4 Ωcm to 2.85 x 10 -3 A similar trend was also confirmed for sample groups B, C, and D.
[0454] FIG. 21 shows the relationship between the conductivity and chemical shift value of the tantalum nitride film. In FIG. 21, the horizontal axis shows the sum of the abundance ratio of Ta (N<1) and the abundance ratio of Ta (N=1) (Ratio of Ta4f shift from equal or less N per Ta), and the vertical axis shows the conductivity of the tantalum nitride film. In FIG. 21, the results for Samples 3A to 11A are plotted. Also, in FIG. 21, the linear approximation line of the plot is shown by a dashed line. The mathematical formula for the linear approximation and the coefficient of determination (R 2 ) is shown in Figure 21.
[0455] Figure 21 confirms that there is a linear relationship between the conductivity and chemical shift value of tantalum nitride films. Specifically, it was confirmed that the conductivity of tantalum nitride films increases as the sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N=1) increases. In other words, it was confirmed that the conductivity of tantalum nitride films decreases as the sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N=1) decreases. It is believed that the 5d orbital of tantalum mainly contributes to the conduction band of tantalum nitride. Therefore, it is presumed that an increase in nitrogen content reduces the number of electrons in the 5d orbital of tantalum, resulting in a decrease in the conductivity of tantalum nitride films.
[0456] In the linear approximation formula shown in FIG. 21, x is equal to or greater than 0 and equal to or less than 1. When x=1 in the linear approximation formula shown in FIG. 21, y becomes the maximum value, and the maximum value of y is 5529.5922 S / cm. Furthermore, since the vertical axis represents the conductivity of the tantalum nitride film, the minimum value of the resistivity of the tantalum nitride film can be calculated by taking the reciprocal of the maximum value of y. The minimum value of the resistivity is 180.9 μΩcm. In other words, when the sum of the abundance ratio of Ta (N<1) and the abundance ratio of Ta (N=1) is 100%, the resistivity is 180.9 μΩcm.
[0457] [X-ray diffraction analysis] XRD analysis was performed on Samples 4A to 8A and Samples 4B to 8B. The θ-2θ scan method, a type of out-of-plane method, was used for the XRD analysis. The θ-2θ scan method measures X-ray diffraction intensity by varying the angle of incidence of the X-rays and adjusting the angle of the detector facing the X-ray source to the same angle. The θ-2θ scan method is sometimes called the powder method. The XRD analysis was performed using a multifunctional thin film material evaluation X-ray diffractometer, D8 DISCOVER (manufactured by Bruker AXS). The XRD analysis used Cu-Kα radiation (λ = 0.15418 nm) as the X-ray source, with a scanning range of 2θ = 20° to 45°, a step width of 0.01°, and a scanning speed of 6.0° / min.
[0458] The results of the XRD analysis of each sample are shown in Figure 22. In Figure 22, the horizontal axis represents the diffraction angle 2θ, and the vertical axis represents the intensity of the diffracted X-rays. Note that the peak observed near 2θ = 32.9 deg is due to diffraction from the (200) plane of silicon, and is a forbidden reflection that should not normally appear.
[0459] In Figure 22, the broken line shown near 2θ=35.5° indicates that the crystal orientation is <111> The dashed line shown in the vicinity of 2θ=36.5° is the peak position of the peak derived from the (002) plane of TaN. The dashed line shown in the vicinity of 2θ=38.7° is the peak position of the peak derived from the δ-TaN phase, which is a cubic crystal system. The dashed line shown in the vicinity of 2θ=38.7° is the peak position of the peak derived from the (002) plane of TaN. <101> The dashed line shown near 2θ=40.2 deg indicates the peak position of the TaN phase. <200> The broken line in the vicinity of 2θ=41.2 deg indicates the peak position of the hexagonal TaN phase (indicated as hex-TaN in Fig. 22). <200> This corresponds to the peak position of the second peak described in the first embodiment.
[0460] 22, two peaks derived from the δ-TaN phase were observed in Samples 4A to 8A and Samples 4B to 8B. Furthermore, in Samples 4A to 6A, the peak height of the first peak was higher than that of the second peak. Specifically, the ratio of the peak height of the second peak to the peak height of the first peak was 0.20 for Sample 4A, 0.35 for Sample 5A, and 0.70 for Sample 6A. This indicates that the crystal orientation of the tantalum nitride film can be controlled by the film formation conditions and the heat treatment performed after the tantalum nitride film formation.
[0461] The above-mentioned XRD analysis was also carried out on Samples 1A to 3A, Samples 1B to 3B, Samples 9A to 11A, and Samples 9B to 11B.
[0462] The results of the XRD analysis of each sample are shown in Figures 23 and 24. In Figures 23 and 24, the horizontal axis represents the diffraction angle 2θ, and the vertical axis represents the intensity of the diffracted X-rays. The peak observed near 2θ = 32.9 deg is due to diffraction from the (200) plane of silicon and is a forbidden reflection that should not actually appear. Figure 23 shows the XRD spectra of Samples 1A to 3A and Samples 1B to 3B, and Figure 24 shows the XRD spectra of Samples 8A to 11A and Samples 8B to 11B.
[0463] 24, two peaks derived from the δ-TaN phase and a peak derived from the TaN phase were observed in Samples 8A, 8B, 9A, and 9B, and a peak derived from the TaN phase was observed in Samples 10A, 10B, 11A, and 11B.
[0464] [D-SIMS analysis] Samples 4D to 7D were analyzed by dynamic mode secondary ion mass spectrometry (D-SIMS) (hereinafter referred to as D-SIMS analysis). The analysis direction of the D-SIMS analysis was from the silicon nitride film toward the substrate. The D-SIMS analysis revealed the oxygen ( 18 The D-SIMS analysis was performed using a quadrupole SIMS instrument (ADEPT1010) manufactured by ULVAC-PHI, Inc.
[0465] The results of the D-SIMS analysis of each sample are shown in Figure 25. In Figure 25, the horizontal axis represents the depth from the surface of the tantalum nitride film, and the vertical axis represents the depth from the surface of the tantalum nitride film. 18 Ionic strength of O 18 O).
[0466] 25, it was observed that the depth of oxygen mixed into the tantalum nitride film in Samples 4D to 7D was deepest in Sample 4D, next deepest in Sample 5D, next deepest in Sample 6D, and shallowest in Sample 7D. This is presumably consistent with the result that the sum of the abundance ratio of TaON and the abundance ratio of Ta2O5 in Samples 4D to 7D was highest in Sample 4D, next highest in Sample 5D, next highest in Sample 6D, and lowest in Sample 7D (see FIG. 19).
[0467] [STEM image] Cross-sectional STEM (Scanning Transmission Electron Microscopy) images of Samples 4C to 7C and Samples 4D to 7D were taken using a Hitachi High-Technologies "HD-2700" at an accelerating voltage of 200 kV. The samples were thinned using a Hitachi High-Technologies XVision200TBS.
[0468] Cross-sectional STEM images of each sample are shown in Figures 26(A) to 26(H). Figure 26(A) is a cross-sectional STEM image of sample 4C, Figure 26(B) is a cross-sectional STEM image of sample 5C, Figure 26(C) is a cross-sectional STEM image of sample 6C, Figure 26(D) is a cross-sectional STEM image of sample 7C, Figure 26(E) is a cross-sectional STEM image of sample 4D, Figure 26(F) is a cross-sectional STEM image of sample 5D, Figure 26(G) is a cross-sectional STEM image of sample 6D, and Figure 26(H) is a cross-sectional STEM image of sample 7D.
[0469] As a protective film for STEM observation, a carbon film was formed on the layer 903. C-cap shown in Figures 26(A) to 26(H) corresponds to this carbon film.
[0470] 26(A) to 26(D), columnar growth of crystal grains was observed in Samples 4C to 7C. In particular, columnar growth of crystal grains was clearly observed in the following order: Sample 4C, Sample 5C, Sample 6C, and Sample 7C. This indicates that the smaller the DC power, the more frequently columnar growth of crystal grains occurred. It is presumed that the frequent occurrence of columnar growth of crystal grains leads to the generation of grain boundaries, which in turn allow oxygen to diffuse deeper (see FIG. 25). It is also presumed that electron capture or scattering occurs at the grain boundaries. Among Samples 4C to 7C, the tantalum nitride film of Sample 7C was the most uniform.
[0471] 26(H), damage to the CAAC-IGZO was observed near the surface of the CAAC-IGZO in sample 7D, particularly in the region 1 to 2 nm from the interface between tantalum nitride and CAAC-IGZO. However, in samples 4D to 6D, no such damage was observed near the surface of the CAAC-IGZO (see FIGS. 26(E) to 26(G)).
[0472] From the above, it was found that the conductivity of tantalum nitride films can be increased by increasing the sum of the abundance ratio of Ta(N<1) and Ta(N=1). It was also found that damage to the CAAC-IGZO surface can be reduced by decreasing the abundance ratio of Ta(N<1).
[0473] It was also found that the inclusion of the δ-TaN phase in the tantalum nitride film reduces the number of grain boundaries in the film. <111> The content of δ-TaN phase and the crystal orientation are <200> It was found that the grain boundaries in the tantalum nitride film can be further reduced by making the content of the δ-TaN phase equal to that of the tantalum nitride film.
[0474] Therefore, it is presumed that the tantalum nitride films formed under the deposition conditions of Samples 4A to 7A shown in Table 1 are suitable for use as electrodes of OS transistors, and that the tantalum nitride films formed under the deposition conditions of Samples 4A to 6A shown in Table 1 are more suitable for use as electrodes of OS transistors.
[0475] [STEM image and EDX analysis] Cross-sectional STEM images were taken of Samples 10C and 10D using the conditions described above.
[0476] Furthermore, EDX line analysis and EDX mapping analysis were performed on Sample 10C and Sample 10D. In each analysis, attention was focused on oxygen at the interface between the tantalum nitride film and the oxide semiconductor layer. In the EDX line analysis, an EDAX Octane T Ultra W (Dual EDS) was used as the EDX detector mounted on the STEM device.
[0477] The cross-sectional STEM images of each sample are shown in Figures 27(A) and 27(B). Figure 27(A) is a cross-sectional STEM image of sample 10C, and Figure 27(B) is a cross-sectional STEM image of sample 10D.
[0478] As a protective film for STEM observation, a carbon film was formed on the layer 903. C-cap in Figures 27(A) and 27(B) corresponds to this carbon film.
[0479] The results of the EDX line analysis are shown in Figures 28(A) and 28(B). In Figures 28(A) and 28(B), the vertical axis represents intensity and the horizontal axis represents distance. The interface between the tantalum nitride film and the oxide semiconductor layer was adjusted to 20 nm on the horizontal axis. Figure 28(A) shows the results for Sample 10C, and Figure 28(B) shows the results for Sample 10D.
[0480] 27(A) and 28(A), a very uniform tantalum nitride film with a clear interface was observed. Meanwhile, in FIGS. 27(B) and 28(B), an oxide film was clearly observed at the interface between the tantalum nitride film and the oxide semiconductor layer. From the above, it was found that an oxide film was formed at the interface by heat treatment. The oxide film contained tantalum, oxygen, and nitrogen, and had a thickness of 4.59 nm.
[0481] The results of the STEM images and EDX mapping analysis are shown in Figures 29(A) to 29(F). Figure 29(A) is a STEM image of sample 10C, and Figure 29(B) is a STEM image of sample 10D. Figure 29(C) shows an EDX map of indium for sample 10C, and Figure 29(D) shows an EDX map of indium for sample 10D. Figure 29(E) shows an EDX map of oxygen for sample 10C, and Figure 29(F) shows an EDX map of oxygen for sample 10D. Note that the STEM images shown in Figures 29(A) and 29(B) are dark-field images (DF-STEM).
[0482] In the STEM image shown in FIG. 29(B), multiple bright spots were observed in the oxide semiconductor layer (for example, inside the circle shown in FIG. 29(B)). Furthermore, from FIG. 29(D), it is inferred that the region where the bright spots were observed is a lumpy region with a high indium content. Furthermore, from FIG. 29(F), it is inferred that the region with a high indium content is due to oxygen vacancies formed in the oxide semiconductor layer when the oxide semiconductor layer oxidizes the tantalum nitride film.
[0483] The characteristics of the tantalum nitride films obtained from the XRD analysis and STEM images are summarized in Table 3. The phases shown in Table 3 are the phases contained in the tantalum nitride films, and the macrostructures shown in Table 3 are the states of the tantalum nitride films. As described above, the tantalum nitride films included in indexes 4 to 6 had columnar crystal grains (column), and the tantalum nitride films included in indexes 7 and 10 were uniform (uniform).
[0484] [Table 3]
[0485] [Work function and optical band gap] Next, the work function and optical band gap of the tantalum nitride film were evaluated.
[0486] Samples 1F to 11F were fabricated to evaluate the work function, and Samples 1G to 11G were fabricated to evaluate the optical band gap. Hereinafter, Samples 1F to 11F may be collectively referred to as Sample Group F, and Samples 1G to 11G may be collectively referred to as Sample Group G.
[0487] 16(C) shows a schematic cross-sectional view of sample group F and sample group G. As shown in FIG. 16(C), each of sample group F and sample group G has a layer 901 and a layer 903 on layer 901.
[0488] First, a manufacturing method of Sample Group F will be described. Sample Group F differs from Sample Group A in that the layer 902 is not provided. The manufacturing method of Sample Group A described above can be referred to for the method of forming the layer 901 and the layer 903 in Sample Group F. In addition, Table 1 can be referred to for the deposition conditions of the tantalum nitride films in Samples 1F to 11F by replacing Samples 1A to 11A in Table 1 with Samples 1F to 11F, respectively.
[0489] Thus, sample group F was prepared.
[0490] Next, a description will be given of a manufacturing method for Sample Group G. The method for forming the layer 903 in Sample Group G can be referred to the manufacturing method for Sample Group A. The film formation conditions for the tantalum nitride films in Samples 1G to 11G can be referred to Table 1 by replacing Samples 1A to 11A in Table 1 with Samples 1G to 11G, respectively.
[0491] As the layer 901 of the sample group G, a quartz substrate was prepared.
[0492] As a result, sample group G was prepared.
[0493] Ultraviolet photoelectron spectroscopy (UPS) measurements were performed on sample group F. A VersaProbe manufactured by PHI was used for the UPS measurements. He I rays (21.22 eV) were used as the ultraviolet light source. The detection area was 8 mm square or less. The bias voltage was -10 V. Prior to the measurements, the sample surfaces were cleaned by argon ion sputtering.
[0494] The UPS spectra obtained by UPS measurements are shown in Figures 30(A) to 32(C). In Figures 30(A) to 32(C), the vertical axis represents intensity and the horizontal axis represents binding energy. Figure 30(A) is the UPS spectrum of sample 1G, Figure 30(B) is the UPS spectrum of sample 2G, Figure 30(C) is the UPS spectrum of sample 3G, and Figure 30(D) is the UPS spectrum of sample 4G. Figure 31(A) is the UPS spectrum of sample 5G, Figure 31(B) is the UPS spectrum of sample 6G, Figure 31(C) is the UPS spectrum of sample 7G, and Figure 31(D) is the UPS spectrum of sample 8G. Figure 32(A) is the UPS spectrum of sample 9G, Figure 32(B) is the UPS spectrum of sample 10G, and Figure 32(C) is the UPS spectrum of sample 11G.
[0495] The results of the UPS measurements are shown in Table 4. k (min) is the lowest energy beyond the work function barrier, and E k (max) is the highest energy beyond the barrier of the work function. The ionization energy corresponds to the work function, and is calculated from the energy of the irradiated light (21.22 eV) by E k (min) and E k It is calculated by subtracting the absolute value of the difference from (max).
[0496] [Table 4]
[0497] As shown in Table 4, the work function was 4.6 eV for Samples 4F to 7F. Furthermore, for Samples 8F to 11F, the work function tended to increase with increasing DC power. However, no clear correlation was observed for Samples 1F to 3F.
[0498] The electron affinity (energy difference from the vacuum level to the bottom of the conduction band) of IGZO with an atomic ratio of In:Ga:Zn=1:1:1 is 4.6 eV. Using IGZO for the semiconductor layer and tantalum nitride contained in Samples 4F to 7F for the source and drain electrodes may reduce contact resistance.
[0499] Next, analysis was performed on sample group G using UV-vis spectrophotometry. The transmittance and reflectance of each sample were measured, and an absorption spectrum and Tauc plot were created. The absorption edge was determined from the Tauc plot, and this absorption edge was used as the optical band gap. A UV-vis spectrophotometer (U4100 model, manufactured by Hitachi High-Tech Corporation) was used for the analysis using UV-vis spectrophotometry.
[0500] The results are shown in Figures 33(A) to 33(C). In Figure 33(A), the vertical axis represents the absorption coefficient, and the horizontal axis represents energy. In Figure 33(B), the vertical axis represents the absorption coefficient, and the horizontal axis represents energy. Figures 33(A) and 33(B) show the results for Samples 1G to 11G, respectively.
[0501] 33A, it was found that the tantalum nitride films of Samples 1G to 3G have a band gap. On the other hand, in Samples 4G to 11G, the absorption coefficient does not become 0 even at 0 eV on the horizontal axis, which indicates that the tantalum nitride films of Samples 4G to 11G have metallic properties.
[0502] As shown in FIG. 33B, the absorptances of Samples 4G to 11G converge to 32%, which indicates that the tantalum nitride films of Samples 4G to 11G have metallic properties.
[0503] Here, the vertical axis of Figure 33(A) is (hνα) n The results are shown in Figures 34(A) to 34(C). Here, h is Planck's constant, ν is the frequency, and α is the absorption coefficient. Figure 34(A) shows the results for sample 1G, Figure 34(B) shows the results for sample 2G, and Figure 34(C) shows the results for sample 3G. Tantalum nitride films with a high nitrogen content are said to be of the indirect transition type. Therefore, the Tauc plot assumes the indirect transition type, and n=1 / 2.
[0504] 34(A) to 34(C), the optical band gap of the tantalum nitride film was 1.364 eV for sample 1G, 1.383 eV for sample 2G, and 0.994 eV for sample 3G.
[0505] <Transistor electrical characteristics evaluation> In this section, the results of evaluating the electrical characteristics of a transistor including tantalum nitride will be described.
[0506] [Sample preparation 2] In this example, Samples 4E to 11E were fabricated. Hereinafter, Samples 4E to 11E may be collectively referred to as Sample Group E.
[0507] Each sample in sample group E includes a transistor. See FIG. 3 for a cross-sectional view of the transistor included in each sample in sample group E. As shown in FIGS. 5A and 5B, the insulating layer 250 of the transistor included in each sample has a four-layer stacked structure consisting of an insulating layer 250d, an insulating layer 250c on insulating layer 250d, an insulating layer 250a on insulating layer 250c, and an insulating layer 250b on insulating layer 250a. The design values of the transistor included in each sample were a channel length of 30 nm and a channel width of 30 nm.
[0508] The following describes a method for producing Sample Group E. For details of the production method, refer to Embodiment 1.
[0509] The insulating layer 214a was made of silicon nitride with a thickness of 60 nm. The insulating layer 214a was formed by pulsed DC sputtering using a silicon target. The insulating layer 214b was made of aluminum oxide with a thickness of 40 nm. The insulating layer 214b was formed by pulsed DC sputtering using an aluminum target.
[0510] Silicon oxide having a thickness of 130 nm was used for the insulating layer 216. The insulating layer 216 was formed by pulse DC sputtering using a silicon target.
[0511] The insulating layer 214a, the insulating layer 214b, and the insulating layer 216 were successively formed using a multi-chamber sputtering apparatus without exposure to the outside air.
[0512] The conductive layer 215a was formed using a titanium nitride film deposited by metal CVD, and the conductive layer 215b was formed using a tungsten film deposited by metal CVD.
[0513] The insulating layer 222a was made of silicon nitride with a thickness of 5 nm and formed by the ALD method, and the insulating layer 222b was made of hafnium oxide with a thickness of 15 nm and formed by the ALD method.
[0514] The insulating layer 224 was formed using silicon oxide with a film thickness of 20 nm by sputtering.
[0515] The oxide semiconductor layer 230a was formed using an In-Ga-Zn oxide film with a thickness of 10 nm, which was deposited by RF sputtering. The oxide film that became the oxide semiconductor layer 230a was deposited using an oxide target with an atomic ratio of In:Ga:Zn=1:3:2.
[0516] The oxide semiconductor layer 230b was formed using an In-Ga-Zn oxide film with a thickness of 15 nm, which was deposited by RF sputtering. The oxide film that became the oxide semiconductor layer 230b was deposited using an oxide target with an atomic ratio of In:Ga:Zn=1:1:1.2.
[0517] The conductive layers 242a and 242b were formed using a tantalum nitride film with a thickness of 20 nm, which was deposited by a reactive sputtering method using a tantalum target and nitrogen (N) gas. For the tantalum nitride films, the target-substrate distance was 286 mm and the substrate temperature was room temperature, which were common to Samples 4E to 11E. The deposition conditions for the tantalum nitride films in Samples 4E to 11E can be found in Table 1 by replacing Samples 4A to 11A in Table 1 with Samples 4E to 11E, respectively.
[0518] The insulating layer 271a1 and the insulating layer 271b1 were formed using a silicon nitride film with a thickness of 5 nm. The insulating layer 271a2 and the insulating layer 271b2 were formed using a silicon oxide film with a thickness of 10 nm. The silicon nitride film and the silicon oxide film were formed successively using a multi-chamber sputtering apparatus without being exposed to the outside air.
[0519] The insulating layer 275 was made of silicon nitride having a film thickness of 5 nm and formed by the ALD method.
[0520] The insulating layer 280 was made of silicon oxide formed by sputtering.
[0521] The insulating layer 250d was formed using an aluminum oxide film with a thickness of 1 nm, which was deposited by the ALD method. The insulating layer 250c was formed using a silicon oxide film with a thickness of 1.5 nm, which was deposited by the ALD method. The insulating layer 250a was formed using a hafnium oxide film with a thickness of 1 nm, which was deposited by the ALD method. The insulating layer 250b was formed using a silicon nitride film with a thickness of 1 nm, which was deposited by the ALD method.
[0522] The conductive layer 260a was formed using a titanium nitride film with a thickness of 5 nm, which was deposited by metal CVD, and the conductive layer 260b was formed using a tungsten film, which was deposited by metal CVD.
[0523] Aluminum oxide was used for the insulating layer 282. The insulating layer 282 was formed by pulse DC sputtering using an aluminum target.
[0524] The insulating layer 283 was made of silicon nitride having a film thickness of 20 nm and formed by sputtering.
[0525] In the above manner, Samples 4E to 11E including transistors were fabricated.
[0526] [Id-Vg characteristics] The electrical characteristics of selected transistors in each of sample group E were evaluated. Here, the drain current (Id)-gate voltage (Vg) characteristics were measured as the electrical characteristics. The Id-Vg characteristics were measured by setting the drain voltage to 1.2 V or 0.1 V, the source voltage to 0 V, and sweeping the gate voltage Vg from -4 V to +4 V in 0.1 V steps. The measurements were performed at room temperature. A Keysight Technologies semiconductor parameter analyzer was used to measure the Id-Vg characteristics.
[0527] From the obtained Id-Vg characteristics, the threshold voltage V th In this example, the threshold voltage V th In the Id-Vg characteristics when the drain voltage is 1.2V, Id=1.0×10 -12 A. Also, the on-current I on , Vg=V th This is the value of the drain current Id at +2.5V. Also, σ(V th ) is the threshold voltage V th is the deviation.
[0528] 35(A) to 36(D) show the Id-Vg characteristics of the transistors included in each of Sample Group E. In FIGS. 35(A) to 36(D), the horizontal axis represents Vg [V], the first vertical axis (left vertical axis) represents Id [A], and the second vertical axis (right vertical axis) represents field-effect mobility μ FE [cm 2 / Vs]. Figure 35(A) shows the Id-Vg characteristics of the transistor included in Sample 4E, Figure 35(B) shows the Id-Vg characteristics of the transistor included in Sample 5E, Figure 35(C) shows the Id-Vg characteristics of the transistor included in Sample 6E, and Figure 35(D) shows the Id-Vg characteristics of the transistor included in Sample 7E. Figure 36(A) shows the Id-Vg characteristics of the transistor included in Sample 8E, Figure 36(B) shows the Id-Vg characteristics of the transistor included in Sample 9E, Figure 36(C) shows the Id-Vg characteristics of the transistor included in Sample 10E, and Figure 36(D) shows the Id-Vg characteristics of the transistor included in Sample 11E. In Figures 35(A) to 36(D), the Id-Vg characteristics when the drain voltage is 1.2 V are shown by a thick solid line, the Id-Vg characteristics when the drain voltage is 0.1 V are shown by a thin solid line, the field effect mobility is shown by a dashed line, and the gate leakage current is shown by a dotted line.
[0529] In addition, the on-current I on Average value of threshold voltage V th Average value of σ(V th ) are shown in Table 2. The threshold voltage V th median of σ(V th ), on-current I on Median of , median of subthreshold swing S, field-effect mobility μ FE The median values of the threshold voltage V and the median values of the drain-induced barrier lowering (DIBL) are shown in Table 5. Note that DIBL is the change in the threshold voltage V when the drain voltage (Vd) is changed by 1 V. th Note that since transistors using tantalum nitride formed under the film formation conditions of Samples 1A to 3A were not fabricated, the I values corresponding to Index 1 to Index 3 in Tables 2 and 5 wereon , V th , σ(V th ), S, μ FE , DIBL is marked as not applicable (n / a).
[0530] [Table 5]
[0531] 35A to 35C, the threshold voltage V th was greater than 0 V, and the normally-off characteristics were obtained. In addition, as the DC power increased from 0.5 kW to 1.0 kW, the on-current I on A trend was observed in which the average value of on-current increased from 3.91 μA to 6.33 μA (see Table 2). The increase in on-current is similar to the decrease in resistivity of tantalum nitride.
[0532] From FIG. 35(D), in the transistor included in sample 7E, the threshold voltage V th Although the value was smaller than 0 V and a normally-on characteristic was obtained, good switching characteristics were obtained.
[0533] 36A to 36D, the transistors included in Samples 8E to 11E were normally on or did not exhibit switching characteristics and were always on. This is presumably because the DC power used during tantalum nitride film formation was high, causing significant damage to the channel. Since Sample 10E and Sample 11E each included a transistor that was always on, the I values of Sample 10E and Sample 11E in Tables 2 and 5 were on , V th , σ(V th ), S, μ FE , DIBL is marked with a hyphen (-) to indicate that it could not be calculated.
[0534] Here, FIG. 37 shows the result in which the horizontal axis of FIG. 20 is changed to DC power (Plasma power). In FIG. 37, the first vertical axis (left vertical axis) represents resistivity [Ωcm]. The first vertical axis is also shown on a linear scale. FIG. 37 shows the resistivity of each of Samples 4A to 11A, Samples 4B to 11B, Samples 4C to 11C, and Samples 4D to 11D. Furthermore, FIG. 37 does not show the N / Ta ratio, but shows the σ(V th ) In FIG. 37, the second vertical axis (the vertical axis on the right) represents σ(V th ) is shown.
[0535] σ(V when DC power is 1.0kW or less th ) is the σ(V th ) Therefore, it was suggested that the highest DC power that the channel can withstand without loss of transistor properties is in the range of 1.0 kW to 1.3 kW.
[0536] From the above, it was found that the tantalum nitride films formed under the film formation conditions of Samples 3A to 7A shown in Table 1 are suitable for electrodes of transistors.
[0537] Here, the contact resistance when a conductive layer is provided in contact with an oxide semiconductor layer was evaluated by a transfer length method (TLM).
[0538] The contact resistance can be calculated simply by adding up the individual resistances of the FET. Here, we assume that the total resistance of the FET is as shown in equation (1).
[0539]
number
[0540] In number (1), R FET is the total resistance of the FET, and R channel is the channel resistance, and ρ channelis the channel resistivity and σ channel is the cross-sectional area of the channel, L is the channel length, and R S / D is the resistance of the source electrode (resistance of the drain electrode), and R contact is the contact resistance between the source electrode and the channel (contact resistance between the drain electrode and the channel). In this example, it was assumed that the resistance of the source electrode and the resistance of the drain electrode were the same.
[0541] When the channel length L in equation (1) is approximated to 0 nm, equation (2) is obtained.
[0542]
number
[0543] R in equation (2) intercept is the total resistance of the FET when the channel length L is approximately 0 nm. R intercept corresponds to the intercept obtained by calculating the total resistance of the FET with different channel lengths and performing linear regression of the calculated total resistance of the FET.
[0544] From the above, the contact resistance R contact is R intercept and R S / D This can be obtained by calculating
[0545] Introduction, R intercept was calculated.
[0546] In this embodiment, the drain voltage Vd is set to the on-current I on The value divided by R FET In addition, the gate voltage is set to the threshold voltage V th When the drain current is equal to the on-current I on It was decided.
[0547] The results obtained using the TLM method for each of Samples 4E to 7E are shown in Table 6 and FIG.
[0548] [Table 6]
[0549] W in Table 6 is the channel width. Table 6 also shows the channel length L and channel width W measured using SEM images. The linear equation in Table 6 is a linear equation approximated for each sample.
[0550] In Fig. 38, the horizontal axis represents channel length L, and the vertical axis represents total FET resistance. The circles in Fig. 38 represent the results for sample 4E, the squares in Fig. 38 represent the results for sample 5E, the triangles in Fig. 38 represent the results for sample 6E, and the diamonds in Fig. 38 represent the results for sample 7E. The dotted lines in Fig. 38 are approximate straight lines for each sample.
[0551] R intercept corresponds to the intercept of the linear equation shown in Table 6 or the intercept of the approximate line shown in FIG.
[0552] Next, R S / D The calculation was performed. S / D is calculated from the resistivity of the tantalum nitride film included in sample 4C, and R S / D is calculated from the resistivity of the tantalum nitride film included in sample 5C, and R S / D is calculated from the resistivity of the tantalum nitride film included in sample 6C, and R S / D is calculated from the resistivity of the tantalum nitride film included in sample 7C. Table 2 can be referred to for the resistivity of the tantalum nitride film of each sample.
[0553] R of each sample calculated from the resistivity of the tantalum nitride film S / D is shown in Table 7.
[0554] [Table 7]
[0555] The length shown in Table 7 is the film thickness of the source electrode or the drain electrode, and the cross-section shown in Table 7 is the area where the source electrode and the oxide semiconductor layer contact each other, or the area where the drain electrode and the oxide semiconductor layer contact each other.
[0556] R S / D can be calculated by multiplying the resistivity of the tantalum nitride film by the film thickness and dividing the result by the area. S / D is shown in Table 7.
[0557] The calculated R intercept and R S / D Using the contact resistance R contact The results are shown in Table 7.
[0558] From Table 7, it was found that among samples 4E to 7E, sample 7E had the smallest contact resistance. It was also found that reducing the DC power from 1.3 kW to 0.5 kW increased the contact resistance by approximately four times.
[0559] Here, the contact conductance was calculated. The contact conductance is calculated by multiplying the contact resistance R contact It can be calculated by taking the inverse of
[0560] The calculated contact conductance results are shown in Figures 39(A) and 39(B).
[0561] In Figure 39(A), the vertical axis represents contact conductance, and the horizontal axis represents conducting chemical surroundings. The conducting chemical surroundings were assumed to be the same as those in the XPS analysis results for sample group A. As explained in [Sample Preparation 2], the conductive layers that would become the source and drain electrodes were deposited under oxygen-free conditions. Furthermore, we assumed that oxidation of the source and drain electrodes could occur on the surface but not in the bulk. In other words, we assumed that oxygen was not present in the bulk of the source and drain electrodes. Therefore, we assumed that nitrides (Ta(N<1), Ta(N=1), and Ta(N>1)) contribute to the tantalum bonding state in the source and drain electrodes, while oxides (TaON and Ta2O5) do not. In this case, the conductive chemical environment is the ratio of the sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N=1) to the sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N=1) to the sum of the abundance ratio of Ta(N<1) and the abundance ratio of Ta(N>1). Figure 39(A) shows the results for samples with indices 4 to 7.
[0562] In FIG. 39(B), the horizontal axis indicates the index, and the first vertical axis (left vertical axis) indicates the contact conductance (Conductance) 1 / R contact , and the line graph indicates the contact conductance. FIG. 39(B) also shows the abundance ratio for each bonding state of tantalum. In FIG. 39(B), the second vertical axis (the vertical axis on the right) indicates the abundance ratio (Fraction) for each bonding state of tantalum, and the bar graph indicates the abundance ratio for each bonding state of tantalum. FIG. 39(B) also shows the abundance ratio of Ta(N<1), the abundance ratio of Ta(N=1), and the abundance ratio of Ta(N>1).
[0563] 39(A) and 39(B) suggest that the abundance ratio of each bonding state of tantalum is related to the contact conductance. [Explanation of symbols]
[0564] BGL: wiring, BIL: wiring, CA: capacitance element, CAL: wiring, CB: capacitance element, CC: capacitance element, GNDL: wiring, LL: wiring, MC: memory cell, RBL: wiring, RWL: wiring, SL: wiring, WBL: wiring, WOL: wiring, WWL: wiring, 100: capacitance element, 110: conductive layer, 112: conductive layer, 115: conductive layer, 120: conductive layer, 125: conductive layer, 132: insulating layer, 140: conductive layer, 142: insulating layer, 145: insulating layer, 150: insulating layer, 151: insulating layer, 153: conductive layer, 154: insulating layer, 156: insulating layer, 168: opening, 200: transistor, 210: insulating layer, 214a: insulating layer, 214b: insulating layer, 214: insulating layer, 215a: conductive layer, 215b: conductive layer, 215: conductive layer, 216: insulating layer, 217: insulating layer, 218: conductive layer, 222a: insulating layer, 222b: insulating layer, 222: insulating layer, 224: insulating layer, 230a: oxide semiconductor layer, 230b: oxide semiconductor layer, 230i: region, 230na: region, 230nb: region, 230: oxide semiconductor layer, 240a: conductive layer, 240b: conductive layer, 240: conductive layer, 241a: insulating layer, 241b: insulating layer, 241: insulating layer, 242_1: conductive layer, 242_2: Conductive layer, 242a: conductive layer, 242b: conductive layer, 242: conductive layer, 250a: insulating layer, 250b: insulating layer, 250c: insulating layer, 250d: insulating layer, 250: insulating layer, 260a: conductive layer, 260b: conductive layer, 260: conductive layer, 271a: insulating layer, 271a1: insulating layer, 271a2: insulating layer, 271b: insulating layer, 271b1: insulating layer, 271b2: insulating layer, 271: insulating layer, 275: insulating layer, 280: insulating layer, 282: insulating layer, 283: insulating layer, 285: insulating layer, 300: transistor, 311: substrate, 313: semiconductor region, 314a: low resistance region, 314b: Low resistance region, 315: insulating layer, 316: conductive layer, 320: insulating layer, 322: insulating layer, 324: insulating layer, 326: insulating layer, 328: conductive layer, 330: conductive layer, 350: insulating layer, 352: insulating layer, 354: insulating layer, 356: conductive layer, 700: electronic component, 702: printed circuit board, 704: mounting board, 710: semiconductor device, 711: mold, 712: land, 713: electrode pad, 714: wire, 715: drive circuit layer, 716: memory layer, 730: electronic component, 731: interposer, 732: package substrate, 733: electrode, 735: semiconductor device, 901: layer,902: Layer, 903: Layer, 904: Layer, 1001: Wiring, 1002: Wiring, 1003: Wiring, 1004: Wiring, 1005: Wiring, 1006: Wiring, 1007: Wiring, 1400: Memory device, 1411: Peripheral circuit, 1420: Row circuit, 1430: Column circuit, 1440: Output circuit, 1460: Control logic circuit, 1470: Memory cell array, 1471: Memory cell, 1472: Memory cell, 1473: Memory cell, 1474: Memory cell, 1475: Memory cell, 1476: Memory cell, 1477: Memory cell, 1478: Memory cell, 1479: Memory cell, 1480: Peripheral circuit, 1481: Peripheral circuit, 1482: Peripheral circuit, 1483: Peripheral circuit, 1484: Peripheral circuit, 1485: Peripheral circuit, 1486: Peripheral circuit, 1487: Peripheral circuit, 1488: Peripheral circuit, 1489: Peripheral circuit, 1490: Peripheral circuit, 1491: Peripheral circuit, 1492: Peripheral circuit, 1493: Peripheral circuit, 1494: Peripheral circuit, 1495: Peripheral circuit, 1496: Peripheral circuit, 1497: Peripheral circuit, 1498: Peripheral circuit, 1499: Peripheral circuit, 1500: Peripheral circuit, 1501: Peripheral circuit, 1502: Peripheral circuit, 473: Memory cell, 1474: Memory cell, 1475: Memory cell, 1476: Memory cell, 1477: Memory cell, 1478: Memory cell, 1479: Memory cell, 5600: Mainframe computer, 5610: Rack, 5620: Computer, 5621: PC card, 5622: Board, 5623: Connection terminal, 5624: Connection terminal, 5625: Connection terminal, 5626: Semiconductor device, 5627: Semiconductor device, 5 628: semiconductor device, 5629: connection terminal, 5630: motherboard, 5631: slot, 6500: electronic device, 6501: housing, 6502: display unit, 6503: power button, 6504: button, 6505: speaker, 6506: microphone, 6507: camera, 6508: light source, 6509: control device, 6600: electronic device, 6611: housing, 6612: keyboard, 6613: pointing device device, 6614: external connection port, 6615: display unit, 6616: control device, 6800: artificial satellite, 6801: aircraft, 6802: solar panel, 6803: antenna, 6804: planet, 6805: secondary battery, 6807: control device, 7000: storage system, 7001sb: server, 7001: host, 7002: storage control circuit, 7003md: storage device, 7003: storage,
Claims
1. A first conductive layer; and a first insulating layer on the first conductive layer; an oxide semiconductor layer on the first insulating layer; a second conductive layer, a third conductive layer, and a second insulating layer on the oxide semiconductor layer; a third insulating layer on the second conductive layer and the third conductive layer; a fourth conductive layer on the second insulating layer; and having the third insulating layer is provided with an opening reaching the oxide semiconductor layer; the second insulating layer and the fourth conductive layer are disposed in the opening; a height of an upper surface of the third insulating layer coincides with a height of an upper surface of the fourth conductive layer; each of the second conductive layer and the third conductive layer comprises tantalum and nitrogen; an abundance ratio of tantalum in a first bonding state is 3% or less and an abundance ratio of tantalum in a second bonding state is 5% or more in each of the second conductive layer and the third conductive layer; the first bonding state is a metallic tantalum bonding state and a tantalum nitride bonding state having a stoichiometrically small amount of nitrogen per tantalum; The semiconductor device wherein the second bonding state is a tantalum nitride bonding state having equal stoichiometric amounts of nitrogen per tantalum.
2. In claim 1, the abundance ratio of the first bonding state and the abundance ratio of the second bonding state are calculated by performing a waveform analysis of an XPS spectrum of tantalum 4f obtained by X-ray photoelectron spectroscopy.
3. In claim 1 or 2, Each of the second conductive layer and the third conductive layer has a first peak having a peak position in a range of 2θ=35.5±1.0 deg and a second peak having a peak position in a range of 2θ=41.2±2.0 deg in an XRD spectrum; A semiconductor device, wherein a ratio of a peak height of the second peak to a peak height of the first peak is not less than 0.2 and not more than 1.
0.
4. In claim 3, The semiconductor device, wherein the oxide semiconductor layer contains one or both of indium and zinc.
5. A first conductive layer; and a first insulating layer on the first conductive layer; an oxide semiconductor layer on the first insulating layer; a second conductive layer, a third conductive layer, and a second insulating layer on the oxide semiconductor layer; a third insulating layer on the second conductive layer and the third conductive layer; a fourth conductive layer on the second insulating layer; and having the third insulating layer is provided with an opening reaching the oxide semiconductor layer; the second insulating layer and the fourth conductive layer are disposed in the opening; a height of an upper surface of the third insulating layer coincides with a height of an upper surface of the fourth conductive layer; Each of the second conductive layer and the third conductive layer has a first peak having a peak position in a range of 2θ=35.5±1.0 deg and a second peak having a peak position in a range of 2θ=41.2±2.0 deg in an XRD spectrum; A semiconductor device, wherein a ratio of a peak height of the second peak to a peak height of the first peak is not less than 0.2 and not more than 1.
0.
6. In claim 5, The semiconductor device, wherein the second conductive layer and the third conductive layer each contain tantalum and nitrogen.
7. In claim 6, The semiconductor device, wherein the oxide semiconductor layer contains one or both of indium and zinc.
Citation Information
Patent Citations
Semiconductor device
JP2011151383A
Semiconductor integrated circuit
JP2012257187A
Cited By
Semiconductor device
WO2026190621A1