Manufacturing method for semiconductor device

Organic insulating films with controlled polishing and bonding techniques address bonding defects in three-dimensional semiconductor chip mounting, enhancing precision and reducing costs by minimizing foreign particle impact.

JP2024152903AActive Publication Date: 2024-10-25RESONAC CORP

Patent Information

Application Number
JP2024139645
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-25
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

Three-dimensional mounting of semiconductor chips faces challenges due to foreign matter generated during singulation, which can cause bonding defects in the insulating film, and using clean rooms to prevent these defects is costly.

Method used

Using insulating films made of organic materials with lower elastic modulus for bonding, combined with precise polishing and controlled temperature bonding, to minimize the impact of foreign particles and reduce bonding defects.

Benefits of technology

This method enables fine bonding of semiconductor chips with reduced defects, eliminating the need for costly clean rooms and ensuring high precision and reliability in the bonding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152903000001_ABST
    Figure 2024152903000001_ABST
Patent Text Reader

Abstract

To provide a method of reducing poor bonding while performing fine bonding of a semiconductor chip in the case of performing three-dimensional packaging of a semiconductor chip.SOLUTION: A manufacturing method for a semiconductor device includes the steps of: polishing at least one of one surface side of a first semiconductor substrate and one surface side of a second semiconductor substrate; dividing the second semiconductor substrate into pieces and acquiring a plurality of semiconductor chips each including an insulating film part corresponding to a second insulating film and at least one second electrode; positioning the second electrode of at least one semiconductor chip among the semiconductor chips with respect to a first electrode of the first semiconductor substrate; attaching a first insulating film of the first semiconductor substrate and the insulating film part of the semiconductor chip to each other; and bonding the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip to each other. At least one insulating film of the first insulating film and the second insulating film includes an organic material. In this manufacturing method, the bonding step and the attaching step are performed at the same time.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor device, and more particularly to a method for manufacturing a semiconductor device in which an individual semiconductor chip is bonded to a semiconductor substrate (another semiconductor chip, a semiconductor wafer, or the like). [Background technology]

[0002] In recent years, three-dimensional packaging has been considered in order to improve the integration density of LSIs. Non-Patent Document 1 discloses an example of three-dimensional packaging of semiconductor chips. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] FC Chen et al., “Systemon Integrated Chips(SoIC TM) for 3D Heterogeneous Integration”, 2019IEEE 69th Electronic Components and Technology Conference (ECTC), p.594-599(2019) Summary of the Invention [Problem to be solved by the invention]

[0004] In the case of three-dimensional mounting of such semiconductor chips, the use of hybrid bonding technology used in wafer-to-wafer (W2W) bonding is being considered in order to prevent misalignment during fine bonding of wiring between devices and bonding. However, in the case of three-dimensional mounting of semiconductor chips, unlike W2W, foreign matter (cutting debris) may be generated during the process of dividing into semiconductor chips, and there is a risk that this foreign matter may adhere to the bonding interface (insulating film of hybrid bonding) of the semiconductor chips, etc. Inorganic materials such as silicon oxide (SiO2) are generally used for this insulating film, but since it is a hard material, the foreign matter that adheres to the insulating film creates large voids in the insulating film, for example, voids with a diameter nearly 1000 times the height of the foreign matter, in the direction of the bonding interface. For this reason, even if the hybrid bonding technology used in W2W is simply applied to three-dimensional mounting of semiconductor chips, there is a risk that such voids may cause bonding failures. On the other hand, if a clean room and equipment with a high level of cleanliness are used to prevent these bonding failures, a large amount of capital investment is required for the clean room, etc.

[0005] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide a method for reducing bonding defects while performing fine bonding of semiconductor chips when three-dimensional mounting of semiconductor chips is performed. [Means for solving the problem]

[0006] A method for manufacturing a semiconductor device according to one aspect of the present invention includes the steps of: preparing a first semiconductor substrate having a first substrate body, a first insulating film and a first electrode provided on one surface of the first substrate body; preparing a second semiconductor substrate having a second substrate body, a second insulating film and a plurality of second electrodes provided on one surface of the second substrate body; polishing at least one of the first and second semiconductor substrates; singulating the second semiconductor substrate to obtain a plurality of semiconductor chips, each of which has an insulating film portion corresponding to the second insulating film and at least one second electrode; aligning the second electrode of at least one of the plurality of semiconductor chips with the first electrode of the first semiconductor substrate; bonding the first insulating film of the first semiconductor substrate and the insulating film portion of the semiconductor chip to each other; and bonding the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip. In this manufacturing method, at least one of the first insulating film and the second insulating film contains an organic material.

[0007] In the above manufacturing method, at least one of the insulating films of the first semiconductor substrate and the second semiconductor substrate (semiconductor chip) is made of an organic material. Organic materials generally have a lower modulus of elasticity than inorganic materials, and by using such a soft material for the insulating film of hybrid bonding, even if foreign matter generated by dicing during the individualization into semiconductor chips adheres to the insulating film, the insulating film around the foreign matter is easily deformed, and the foreign matter can be contained in the organic material without generating a large gap in the insulating film. In other words, the influence of the foreign matter can be suppressed by the insulating film containing the organic material. Therefore, according to the above manufacturing method, it is possible to reduce bonding defects while performing fine bonding of semiconductor chips. Note that, according to this manufacturing method, although not limited thereto, since the above method can reduce bonding defects, it is not necessary to use a clean room and equipment with a high cleanliness level to prevent bonding defects, and the limitations on the manufacturing site of the above-mentioned semiconductor device are loosened.

[0008] In the above manufacturing method, in the polishing step, one side of the first semiconductor substrate may be polished using a CMP method so that the surface of the first electrode is at the same height as the surface of the first insulating film or is recessed relative to the surface of the first insulating film. In addition, in the polishing step, one side of the second semiconductor substrate may be polished using a CMP method so that the surfaces of the second electrodes are at the same height as the surface of the second insulating film or are recessed relative to the surface of the second insulating film. By performing such polishing, the first electrode and the second electrode are prevented from coming into contact with each other in the step of bonding the insulating films, and the step of bonding the first insulating film of the first semiconductor substrate and the insulating film part of the semiconductor chip to each other can be more reliably performed.

[0009] In the above manufacturing method, in the bonding step, the insulating film portion of the semiconductor chip may be bonded to the first insulating film of the first semiconductor substrate at a temperature where the temperature difference between the semiconductor chip and the first semiconductor substrate is within 10° C. or at room temperature. In this case, the semiconductor chip can be bonded to the first semiconductor substrate while suppressing misalignment. Also, bonding is possible even if the first insulating film of the first semiconductor substrate and the insulating film portion of the semiconductor chip are made of different materials.

[0010] In the above manufacturing method, the modulus of elasticity of the organic material contained in at least one of the first insulating film and the second insulating film may be 7.0 GPa or less. In this case, even if foreign matter generated by dicing during the individualization into semiconductor chips adheres to the bonding interface, the foreign matter can be more reliably contained in the organic material without causing a large void, and bonding defects can be further reduced. The modulus of elasticity of the organic material is preferably 5.0 GPa or less, more preferably 2.0 GPa or less. The modulus of elasticity here means Young's modulus.

[0011] In the above manufacturing method, the thermal expansion coefficient in the thickness direction of the organic material contained in at least one of the first insulating film and the second insulating film may be 70 ppm / k or less, and more preferably 50 ppm / k or less. In this case, the thermal expansion coefficient of the organic material is equal to or close to the thermal expansion coefficient of the first electrode and the second electrode, and when heat is applied, the difference in thermal expansion between the insulating layer and the electrode becomes close, and bonding failure can be further reduced. Note that the organic material specified here may have the above-mentioned elastic modulus, or may have an elastic modulus different from the above-mentioned elastic modulus.

[0012] In the above manufacturing method, the organic material contained in the second insulating film may have a polishing rate that is 5 times or less than the polishing rate of the metal material constituting the second electrode. For example, when the polishing rate of the metal material constituting the second electrode is 50 nm / min, the polishing rate of the organic material contained in the second insulating film is preferably 200 nm / min or less (4 times or less), more preferably 100 nm / min or less (2 times or less), and even more preferably 50 nm / min or less (equal or less). When there is such a polishing rate relationship, the work of polishing the second insulating film containing the organic material and the second electrode becomes easier, and the polishing process can be simplified. The polishing rate relationship between the first insulating film and the first electrode may be the same as above.

[0013] In the above manufacturing method, the organic material contained in at least one of the first insulating film and the second insulating film may include polyimide, a polyimide precursor (e.g., polyimide ester or polyamic acid), polyamideimide, benzocyclobutene (BCB), polybenzoxazole (PBO), or a PBO precursor. The organic material contained in at least one of the first insulating film and the second insulating film may include a photosensitive resin, a thermosetting non-conductive film, or a thermosetting resin. When a photosensitive resin is used, it is possible to simplify the manufacturing process of the connection electrode. Furthermore, when a thermosetting non-conductive film is used, it is possible to shorten the time required for the manufacturing process of the insulating layer.

[0014] In the above manufacturing method, the thickness of the second insulating film may be thicker than the thickness of the first insulating film. In this case, most of the foreign matter that adheres to the bonding interface during separation into semiconductor chips or during chip mounting can be contained by the second insulating film, and bonding defects can be further reduced. On the other hand, the thickness of the second insulating film may be thinner than the thickness of the first insulating film. In this case, the height of the mounted semiconductor chip can be reduced. The thicknesses of the first insulating film and the second insulating film may be determined according to the height of the corresponding electrodes. Effect of the Invention

[0015] According to the present invention, it is possible to provide a method for reducing bonding defects while performing fine bonding of semiconductor chips in three-dimensional mounting of semiconductor chips. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a semiconductor device manufactured by a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 2] 2A to 2C are diagrams sequentially showing a method for manufacturing the semiconductor device shown in FIG. [Diagram 3] FIG. 3 is a diagram showing in more detail the bonding method in the method for manufacturing the semiconductor device shown in FIG. [Figure 4] 4A to 4C are views showing a method for manufacturing the semiconductor device shown in FIG. 1, sequentially illustrating steps subsequent to the step shown in FIG. [Diagram 5] FIG. 5 is a diagram showing an example in which the method for manufacturing a semiconductor device according to an embodiment of the present invention is applied to Chip-to-Wafer (C2W). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the following description, the same or corresponding parts are given the same reference numerals, and duplicated descriptions will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the illustrated ratios.

[0018] (Configuration of Semiconductor Device) Fig. 1 is a cross-sectional view showing an example of a semiconductor device manufactured by the manufacturing method according to the present embodiment. As shown in Fig. 1, the semiconductor device 1 is, for example, an example of a semiconductor package, and includes a first semiconductor chip 10 (first semiconductor substrate), a second semiconductor chip 20 (semiconductor chip), a pillar portion 30, a redistribution layer 40, a substrate 50, and a circuit substrate 60.

[0019] The first semiconductor chip 10 is a semiconductor chip such as an LSI (Large scale Integrated Circuit) chip or a CMOS (Complementary Metal Oxide Semiconductor) sensor, and the second semiconductor chip 20 is mounted vertically (downward in the height direction) to form a three-dimensional mounting structure. The second semiconductor chip 20 is a semiconductor chip such as an LSI or memory, and is a chip component having a smaller area in a plan view than the first semiconductor chip 10. The second semiconductor chip 20 is bonded to the back surface of the first semiconductor chip 10 by chip-to-chip (C2C) bonding. The first semiconductor chip 10 and the second semiconductor chip 20 are finely bonded to each other by hybrid bonding, the details of which will be described later, with their respective terminal electrodes and their surrounding insulating films firmly and without misalignment.

[0020] The pillar portion 30 is a connection portion in which a plurality of pillars 31 made of, for example, copper (Cu) are sealed with a resin 32. The plurality of pillars 31 are conductive members extending from the upper surface of the pillar portion 30 to the lower surface, and may be arranged so that the center pitch between the pillars 31 is 15 μm or less, and may have a cylindrical shape with a diameter of, for example, 3 μm to 20 μm (5 μm in one example). The plurality of pillars 31 flip-chip connect the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the rewiring layer 40. By using the pillar portion 30, the semiconductor device 1 can form a connection electrode without using a technique called TMV (Through mold via), which is a technique of drilling holes in a mold and soldering the mold. The pillar portion 30 has, for example, a thickness approximately equal to that of the second semiconductor chip 20, and is arranged on the lateral side of the second semiconductor chip 20 in the horizontal direction. In addition, instead of the pillar portion 30, this portion may be composed of a plurality of solder balls, and the solder balls may be used to electrically connect the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the redistribution layer 40.

[0021] The rewiring layer 40 is a wiring layer having a function of terminal pitch conversion, which is a function of the package substrate, and is a layer in which a rewiring pattern is formed of polyimide and copper wiring on the insulating film on the lower side of the second semiconductor chip 20 and on the lower surface of the pillar portion 30. The rewiring layer 40 is formed in a state in which the first semiconductor chip 10 and the second semiconductor chip 20 are turned upside down (see (d) of FIG. 4). The rewiring layer 40 electrically connects the terminal electrodes on the lower surface of the second semiconductor chip 20 and the terminal electrodes of the first semiconductor chip 10 via the pillar portion 30 to the terminal electrodes of the substrate 50. The terminal pitch of the substrate 50 is wider than the terminal pitch of the first semiconductor chip 10 (pillar 31) and the second semiconductor chip 20. Various electronic components 51 may be mounted on the substrate 50. In addition, when there is a large difference in the terminal pitch between the rewiring layer 40 and the substrate 50, an inorganic interposer or the like may be used here to electrically connect the rewiring layer 40 and the substrate 50.

[0022] The circuit board 60 is a board on which the first semiconductor chip 10 and the second semiconductor chip 20 are mounted, and has a plurality of through electrodes therein electrically connected to the board 50 connected to the first semiconductor chip 10, the second semiconductor chip 20, and electronic components 51, etc. In the circuit board 60, the terminal electrodes of the first semiconductor chip 10 and the second semiconductor chip are electrically connected to terminal electrodes 61 provided on the rear surface of the circuit board 60 by these through electrodes.

[0023] (Method of manufacturing a semiconductor device) Next, a method for manufacturing the semiconductor device 1 will be described with reference to Fig. 2 to Fig. 4. Fig. 2 is a diagram sequentially showing a method for manufacturing the semiconductor device shown in Fig. 1. Fig. 3 is a diagram showing in more detail a bonding method (hybrid bonding) in the method for manufacturing the semiconductor device shown in Fig. 2. Fig. 4 is a diagram sequentially showing steps subsequent to the steps shown in Fig. 2 in the method for manufacturing the semiconductor device shown in Fig. 1.

[0024] The semiconductor device 1 can be manufactured, for example, through the following steps (a) to (p). (a) A step of preparing a first semiconductor substrate 100 corresponding to a first semiconductor chip 10. (b) A step of preparing a second semiconductor substrate 200 corresponding to the second semiconductor chip 20. (c) polishing the first semiconductor substrate 100; (d) polishing the second semiconductor substrate 200; (e) A step of singulating the second semiconductor substrate 200 to obtain a plurality of semiconductor chips 205. (f) A step of aligning the terminal electrodes 203 of each of the plurality of semiconductor chips 205 with the terminal electrodes 103 of the first semiconductor substrate 100 . (g) A step of bonding the insulating film 102 of the first semiconductor substrate 100 and each of the insulating film portions 202b of the multiple semiconductor chips 205 to each other (see FIG. 3(b)). (h) A step of bonding the terminal electrodes 103 of the first semiconductor substrate 100 to the terminal electrodes 203 of each of the plurality of semiconductor chips 205 (see FIG. 3(c)). (i) A step of forming a plurality of pillars 300 (corresponding to pillars 31 ) between a plurality of semiconductor chips 205 on the connection surface of the first semiconductor substrate 100 . (j) A step of molding a resin 301 onto the connection surface of the first semiconductor substrate 100 so as to cover the semiconductor chip 205 and the pillar 300, thereby obtaining a semi-finished product M1. (k) A step of thinning the upper part of the semi-finished product M1 molded in step (j) by grinding to obtain a semi-finished product M2. (m) A step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in the step (k). (n) A step of cutting the semi-finished product M3 on which the wiring layer 400 has been formed in the step (m) along the cutting lines A into individual semiconductor devices 1. (p) A step of inverting the semiconductor device 1a individualized in the step (n) and placing it on the substrate 50 and the circuit board 60 (see FIG. 1).

[0025] [Step (a) and Step (b)] Step (a) is a step of preparing a first semiconductor substrate 100, which is a silicon substrate on which an integrated circuit composed of semiconductor elements and wiring connecting the semiconductor elements is formed, corresponding to a plurality of first semiconductor chips 10. In step (a), as shown in FIG. 2(a), a plurality of terminal electrodes 103 (first electrodes) made of copper or aluminum are provided at predetermined intervals on one surface 101a of a first substrate body 101 made of silicon or the like, and an insulating film 102 (first insulating film) made of an organic material is provided. The insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103, or the insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103. A predetermined interval is provided between the plurality of terminal electrodes 103 in order to form pillars 300 in a step described later, and another terminal electrode (not shown) connected to the pillars 300 is formed between the plurality of terminal electrodes 103.

[0026] Step (b) is a step of preparing a second semiconductor substrate 200, which is a silicon substrate on which an integrated circuit composed of semiconductor elements and wiring connecting the semiconductor elements is formed, corresponding to a plurality of second semiconductor chips 20. In step (b), as shown in (a) of Fig. 2, a plurality of terminal electrodes 203 (a plurality of second electrodes) made of copper, aluminum, or the like are continuously provided on one surface 201a of a second substrate body 201 made of silicon or the like, and an insulating film 202 (a second insulating film) made of an organic material is also provided. The insulating film 202 may be provided on the one surface 201a of the second substrate body 201, and then the plurality of terminal electrodes 203 may be provided, or the insulating film 202 may be provided on the one surface 201a of the second substrate body 201.

[0027] The insulating films 102 and 202 used in steps (a) and (b) are made of an organic material as described above. The organic material is made of, for example, polyimide, a polyimide precursor (for example, polyimide ester or polyamic acid), polyamideimide, benzocyclobutene (BCB), polybenzoxazole (PBO), or a PBO precursor, and has a lower elastic modulus than inorganic materials such as silicon oxide (SiO2). The elastic modulus of the organic material constituting the insulating films 102 and 202 is, for example, 7.0 GPa or less, preferably 5.0 GPa or less or 3.0 GPa or less, and more preferably 2.0 GPa or less or 1.5 GPa or less. The elastic modulus here means Young's modulus.

[0028] Furthermore, the organic material constituting the insulating films 102 and 202 may preferably have a thermal expansion coefficient of 70 ppm / k or less, and more preferably 50 ppm / k or less.

[0029] Furthermore, the organic material constituting the insulating films 102 and 202 may have a polishing rate that is 5 times or less than the polishing rate of the metal material (e.g., copper or aluminum) constituting the corresponding terminal electrode 103 or 203. For example, when the metal material constituting the terminal electrode 103 or 203 is copper and has a polishing rate of 50 nm / min, the polishing rate of the organic material constituting the insulating films 102 and 202 is preferably 200 nm / min or less (4 times or less), more preferably 100 nm / min or less (2 times or less), and even more preferably 50 nm / min or less (the same or less).

[0030] The organic material constituting the insulating films 102 and 202 may be a photosensitive resin, a thermosetting non-conductive film (NCF: Non Conductive Film), or a thermosetting resin. This organic material may be an underfill material. The organic material constituting the insulating films 102 and 202 may be a heat-resistant resin.

[0031] [Step (c) and step (d)] Step (c) is a step of polishing the first semiconductor substrate 100. In step (c), as shown in FIG. 3(a), the surface 101a of the first semiconductor substrate 100 can be polished using a chemical mechanical polishing (CMP) method so that each surface 103a of the terminal electrodes 103 is at the same position as or slightly lower (recessed) than the surface 102a of the insulating film 102. In step (c), the first semiconductor substrate 100 can also be polished by the CMP method under conditions that selectively and deeply polish the terminal electrodes 103 made of, for example, copper. In step (c), the CMP method may be used to polish each surface 103a of the terminal electrodes 103 so that they coincide with the surface 102a of the insulating film 102.

[0032] Step (d) is a step of polishing the second semiconductor substrate 200. In step (d), as shown in (a) of FIG. 3, the surface 201a of the second semiconductor substrate 200 may be polished by using the CMP method so that the surfaces 203a of the terminal electrodes 203 are at the same position or slightly lower (recessed) than the surface 202a of the insulating film 202. In step (d), the second semiconductor substrate 200 is polished by the CMP method under conditions for selectively and deeply polishing the terminal electrodes 203 made of, for example, copper. In step (d), the surfaces 203a of the terminal electrodes 203 may be polished by the CMP method so that they coincide with the surface 202a of the insulating film 202.

[0033] In steps (c) and (d), the insulating film 102 and the insulating film 202 may be polished to have the same thickness, or may be polished to have a thickness greater than that of the insulating film 102. On the other hand, the insulating film 202 may be polished to have a thickness less than that of the insulating film 102. When the insulating film 202 is thicker than the insulating film 102, most of the foreign matter adhering to the bonding interface during dicing into the semiconductor chip 205 or during chip mounting can be contained by the insulating film 202, and bonding defects can be further reduced. On the other hand, when the insulating film 202 is thinner than the insulating film 102, the height of the mounted semiconductor chip 205, that is, the semiconductor device 1, can be reduced.

[0034] [Step (e)] Step (e) is a step of dividing the second semiconductor substrate 200 into individual semiconductor chips 205. In step (e), as shown in FIG. 2(b), the second semiconductor substrate 200 is divided into multiple semiconductor chips 205 by a cutting means such as dicing. When dicing the second semiconductor substrate 200, the insulating film 202 may be covered with a protective material or the like and then divided into individual chips. In step (e), the insulating film 202 of the second semiconductor substrate 200 is divided into insulating film portions 202b corresponding to each semiconductor chip 205. As a dicing method for dividing the second semiconductor substrate 200, for example, plasma dicing, stealth dicing, or laser dicing can be used. In addition, as a surface protective material for the second semiconductor substrate 200 during dicing, for example, an organic film that can be removed with water or TMAH, or a thin film such as a carbon film that can be removed with plasma, may be provided.

[0035] [Process (f)] Step (f) is a step of aligning the terminal electrodes 203 of each of the multiple semiconductor chips 205 with the terminal electrodes 103 of the first semiconductor substrate 100. In step (f), as shown in (c) of Fig. 2, each semiconductor chip 205 is aligned so that the terminal electrodes 203 of each semiconductor chip 205 face the corresponding multiple terminal electrodes 103 of the first semiconductor substrate 100. For this alignment, an alignment mark or the like may be provided on the first semiconductor substrate 100.

[0036] [Process (g)] Step (g) is a step of bonding the insulating film 102 of the first semiconductor substrate 100 and each insulating film portion 202b of the multiple semiconductor chips 205 to each other. In step (g), after removing organic matter or metal oxide attached to the surface of each semiconductor chip 205, the semiconductor chip 205 is aligned with the first semiconductor substrate 100 as shown in FIG. 2(c), and when this is completed, the insulating film portion 202b of each of the multiple semiconductor chips 205 is bonded to the insulating film 102 of the first semiconductor substrate 100 as hybrid bonding (see FIG. 3(b)). At this time, the insulating film portions of the multiple semiconductor chips 205 and the insulating film 102 of the first semiconductor substrate 100 may be uniformly heated before bonding. The temperature difference between the semiconductor chips 205 and the first semiconductor substrate 100 during bonding is preferably, for example, 10° C. or less. By such heat bonding at a uniform temperature, the insulating film 102 and the insulating film portion 202b are bonded to form an insulating bond portion S1, and the multiple semiconductor chips 205 are mechanically and firmly attached to the first semiconductor substrate 100. Furthermore, since the heat bonding is performed at a uniform temperature, positional deviation or the like is unlikely to occur at the bonding portion, and high-precision bonding can be performed. At this attachment stage, the terminal electrodes 103 of the first semiconductor substrate 100 and the terminal electrodes 203 of the semiconductor chip 205 are separated from each other and are not connected (but are aligned). Note that the bonding of the semiconductor chip 205 to the first semiconductor substrate 100 may be performed by other bonding methods, such as room temperature bonding.

[0037] [Process (h)] Step (h) is a step of bonding the terminal electrode 103 of the first semiconductor substrate 100 and each of the terminal electrodes 203 of the semiconductor chips 205. In step (h), as shown in FIG. 2(d), after the bonding in step (g) is completed, a predetermined heat H or pressure or both are applied to bond the terminal electrode 103 of the first semiconductor substrate 100 and each of the terminal electrodes 203 of the semiconductor chips 205 as hybrid bonding (see FIG. 3(c)). When the terminal electrodes 103 and 20 are made of copper, the annealing temperature in step (g) is preferably 150° C. or higher and 400° C. or lower, and more preferably 200° C. or higher and 300° C. or lower. By such bonding process, the terminal electrode 103 and the corresponding terminal electrode 203 are bonded to each other to form an electrode bonding portion S2, and the terminal electrodes 103 and 203 are bonded mechanically and electrically firmly. The electrode bonding in step (h) is carried out after the bonding in step (g), but may be carried out simultaneously with the bonding in step (g).

[0038] As a result, multiple semiconductor chips 205 are electrically and mechanically mounted at predetermined positions with high precision on the first semiconductor substrate 100. Note that, for example, a reliability test (connection test, etc.) of the product may be performed at the stage of the semi-finished product shown in Fig. 2(d) and only non-defective products may be used in the subsequent steps. Next, an example of a method for manufacturing a semiconductor device using such a semi-finished product will be described with reference to Fig. 4.

[0039] [Step (i)] Step (i) is a step of forming a plurality of pillars 300 between a plurality of semiconductor chips 205 on the connection surface 100a of the first semiconductor substrate 100. In step (i), as shown in (a) of FIG. 4, a large number of pillars 300 made of, for example, copper are formed between a plurality of semiconductor chips 205. The pillars 300 can be formed, for example, from copper plating, conductive paste, or copper pins. The pillars 300 are formed so that one end is connected to a terminal electrode of the first semiconductor substrate 100 that is not connected to the terminal electrode 203 of the semiconductor chip 205, and the other end extends upward. The pillars 300 have a diameter of, for example, 10 μm or more and 100 μm or less, and a height of, for example, 10 μm or more and 1000 μm or less. For example, 1 to 10,000 pillars 300 may be provided between a pair of semiconductor chips 205.

[0040] [Process (j)] Step (j) is a step of molding resin 301 on the connection surface 100a of the first semiconductor substrate 100 so as to cover the semiconductor chips 205 and the pillars 300. In step (j), as shown in FIG. 4B, for example, epoxy resin or the like is molded to entirely cover the semiconductor chips 205 and the pillars 300. As a molding method, for example, compression molding or transfer molding can be used, or a film-like epoxy film may be laminated. By this resin molding, the spaces between the pillars 300 and between the pillars 300 and the semiconductor chips 205 are filled with resin. As a result, a semi-finished product M1 filled with resin is formed. Note that a curing process may be performed after molding the epoxy resin or the like. In addition, when steps (i) and (j) are performed substantially simultaneously, that is, when the pillars 300 are also formed at the same time as the resin molding, the pillars may be formed using imprinting, which is a fine transfer, and conductive paste or electrolytic plating.

[0041] [Process (k)] In step (k), the semi-finished product M1 consisting of the resin 301, the pillars 300, and the semiconductor chips 205 molded in step (j) is ground and thinned to obtain the semi-finished product M2. In step (k), as shown in FIG. 4(c), the upper part of the semi-finished product M1 is polished with a grinder or the like to thin the resin-molded first semiconductor substrate 100 and the like to obtain the semi-finished product M2. By polishing in step (k), the thicknesses of the semiconductor chips 205, the pillars 300, and the resin 301 are thinned to, for example, about several tens of μm, the semiconductor chips 205 have a shape corresponding to the second semiconductor chip 20, and the pillars 300 and the resin 301 have a shape corresponding to the pillar portion 30.

[0042] [Process (m)] Step (m) is a step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in step (k). In step (m), as shown in Fig. 4(d), a rewiring pattern is formed of polyimide and copper wiring on the second semiconductor chip 20 and pillar portion 30 of the ground semi-finished product M2. This forms a semi-finished product M3 having a wiring structure in which the terminal pitch of the second semiconductor chip 20 and the pillar portion 30 is widened.

[0043] [Step (n) and step (p)] Step (n) is a step of cutting the semi-finished product M3 on which the wiring layer 400 has been formed in step (m) along the cutting line A to obtain each semiconductor device 1. In step (n), as shown in (d) of Fig. 4, the semiconductor device substrate is cut along the cutting line A by dicing or the like to obtain each semiconductor device 1. Thereafter, in step (p), the semiconductor device 1a separated in step (n) is inverted and placed on the substrate 50 and the circuit board 60 to obtain a plurality of semiconductor devices 1 shown in Fig. 1.

[0044] As described above, according to the manufacturing method of the semiconductor device of this embodiment, the insulating film 102 of the first semiconductor substrate 100 and the insulating film 202 (insulating film portion 202b) of the second semiconductor substrate 200 (semiconductor chip 205) are configured to contain an organic material. Organic materials generally have a lower elastic modulus than inorganic materials, and by using such a soft material for the insulating film of the hybrid bonding, even if a foreign substance generated by dicing when dividing the second semiconductor substrate 200 into the semiconductor chips 205 adheres to the insulating film, the insulating film around the foreign substance is easily deformed, and the foreign substance can be contained in the organic material without generating a large void in the insulating film. That is, the influence of the foreign substance can be suppressed by the insulating film containing the organic material. Therefore, according to the manufacturing method of this embodiment, it is possible to reduce the bonding failure while performing fine bonding between the first semiconductor substrate 100 and the semiconductor chip 205. Note that, when the organic material used for the insulating film is made of a material with a low elastic modulus or has a resin composition with high toughness, it is possible to more reliably prevent damage to the semiconductor device 1 manufactured by the above manufacturing method.

[0045] In the manufacturing method of the semiconductor device according to the present embodiment, in the polishing steps (c) and (d), the first surface 101a side of the first semiconductor substrate 100 is polished by using the CMP method so that the surfaces 103a of the terminal electrodes 103 are at the same height as the surface 102a of the insulating film 102 or are recessed relative to the surface 102a of the insulating film 102. In addition, the first surface 201a side of the second semiconductor substrate 200 is polished by using the CMP method so that the surfaces 203a of the terminal electrodes 203 are at the same height as the surface 202a of the insulating film 202 or are recessed relative to the surface 202a of the insulating film 202. By performing such polishing, the step (g) of bonding the insulating film 102 of the first semiconductor substrate 100 and the insulating film portions 202b of the semiconductor chip 205 to each other can be performed more reliably, and positional deviation between the electrodes bonded by hybrid bonding can be prevented.

[0046] Moreover, in the manufacturing method of the semiconductor device according to this embodiment, in the bonding step (g), the insulating film portion 202b of the semiconductor chip 205 is bonded to the first insulating film 102 of the first semiconductor substrate 100 at a temperature where the temperature difference between the semiconductor chip 205 and the first semiconductor substrate 100 is within 10° C., or at room temperature. Since such temperature control is performed, it is possible to bond the multiple semiconductor chips 205 to the first semiconductor substrate 100 while suppressing misalignment.

[0047] In the method for manufacturing a semiconductor device according to this embodiment, the elastic modulus of the organic material constituting the insulating film 102 and the insulating film 202 may be 7.0 GPa or less. In this case, even if foreign matter adheres to the bonding interface during singulation into the semiconductor chip 205 or during chip mounting, the foreign matter can be contained in the organic material without further generating large voids, thereby further reducing bonding defects.

[0048] Furthermore, in the method for manufacturing a semiconductor device according to this embodiment, the thermal expansion coefficient of the organic material constituting the insulating film 102 and the insulating film 202 may be 70 ppm / k or less. In this case, the thermal expansion coefficient of the organic material constituting the insulating film becomes equal to or close to the thermal expansion coefficient of the terminal electrodes 103 and 203, and even if heat is generated during use of the semiconductor device 1, the thermal expansion of the insulating layer and the terminal electrodes becomes approximately the same, and damage to the semiconductor device 1 due to the difference in thermal expansion coefficient can be prevented.

[0049] Furthermore, in the method for manufacturing a semiconductor device according to this embodiment, the organic material contained in the insulating film 102 may have a polishing rate that is 5 times or less than the polishing rate of the metal material constituting the terminal electrode 103, and the organic material contained in the insulating film 202 may have a polishing rate that is 5 times or less than the polishing rate of the metal material constituting the terminal electrode 203. In this case, the operations in steps (c) and (d) of polishing the insulating film and the terminal electrode are facilitated, and the polishing steps (c) and (d) can be simplified.

[0050] Although an embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment. For example, in the above embodiment, after the step (i) of forming the pillar 300, the step (j) of molding the resin 301 and the step (k) of grinding and thinning the resin 301 and the like are performed in this order in the process shown in FIG. 4, the step (j) of molding the resin 301 on the connection surface of the first semiconductor substrate 100 may be performed first, followed by the step (k) of grinding and thinning the resin 301 to a predetermined thickness, and then the step (i) of forming the pillar 300. In this case, the work of grinding the pillar 300 can be reduced, and since the part of the pillar 300 that is to be ground is not necessary, the material cost can be reduced.

[0051] In the above embodiment, an example of bonding by C2C has been described, but the present invention may be applied to bonding by Chip-to-Wafer (C2W) shown in FIG. 5. In C2W, a semiconductor wafer 410 (first semiconductor substrate) having a substrate body 411 (first substrate body), an insulating film 412 (first insulating film) provided on one surface of the substrate body 411, and a plurality of terminal electrodes 413 (first electrodes) is prepared, and a semiconductor substrate (second semiconductor substrate) before being singulated into a plurality of semiconductor chips 420 having a substrate body 421 (second substrate body), an insulating film portion 422 (second insulating film) provided on one surface of the substrate body 421, and a plurality of terminal electrodes 423 (second electrodes) is prepared. Then, one surface side of the semiconductor wafer 410 and one surface side of the second semiconductor substrate before being singulated into the semiconductor chips 420 are polished by a CMP method or the like, similar to the above steps (c) and (d). Thereafter, the second semiconductor substrate is subjected to a singulation process similar to that in step (e) to obtain a plurality of semiconductor chips 420.

[0052] 5(a), the terminal electrodes 423 of the semiconductor chip 420 are aligned with the terminal electrodes 413 of the semiconductor wafer 410 (step (f)). Then, the insulating film 412 of the semiconductor wafer 410 and the insulating film portion 422 of the semiconductor chip 420 are attached to each other (step (g)), and the terminal electrodes 413 of the semiconductor wafer 410 and the terminal electrodes 423 of the semiconductor chip 420 are bonded to each other (step (h)), to obtain a semi-finished product shown in FIG. 5(b). As a result, the insulating film 412 and the insulating film portion 422 are bonded to each other to form an insulating bonding portion S3, and the semiconductor chip 420 is attached to the semiconductor wafer 410 mechanically and with high accuracy. Also, the terminal electrodes 413 and the corresponding terminal electrodes 423 are bonded to each other to form an electrode bonding portion S4, and the terminal electrodes 413 and 423 are bonded to each other mechanically and electrically.

[0053] 5(c) and 5(d), a plurality of semiconductor chips 420 are bonded to a semiconductor wafer 410, which is a semiconductor wafer, in a similar manner to obtain a semiconductor device 401. Note that the plurality of semiconductor chips 420 may be bonded to the semiconductor wafer 410 one by one by hybrid bonding, or may be bonded to the semiconductor wafer 410 collectively by hybrid bonding.

[0054] In the manufacturing method of the semiconductor device 401, as in the manufacturing method of the semiconductor device 1 described above, the insulating film 412 of the semiconductor wafer 410 and the insulating film portion 422 of the semiconductor chip 420 are made of organic material. By using such a soft material for the insulating film of the hybrid bonding, even if a foreign substance generated by dicing during the individualization into the semiconductor chips 420 adheres to the insulating film, the insulating film around the foreign substance is easily deformed, and the foreign substance can be contained in the organic material without generating a large void in the insulating film. In other words, the influence of the foreign substance can be suppressed by the insulating film containing the organic material. Therefore, in the manufacturing method related to C2W described above, as in C2C, the semiconductor wafer 410 and the semiconductor chip 420 can be finely bonded while bonding failure can be reduced.

[0055] Furthermore, in the above-mentioned method for manufacturing a semiconductor device, the insulating film 102 of the semiconductor substrate 110 and the insulating film 202 of the semiconductor chip 205 are made of organic materials, but these insulating films may contain inorganic materials as part of them. In other words, if there is a part of an organic material that can contain the above-mentioned foreign matter, the remaining part of the insulating film may be made of an inorganic material. [Explanation of symbols]

[0056] Reference Signs List 1, 1a, 401...semiconductor device, 10...first semiconductor chip, 20...second semiconductor chip, 30...pillar portion, 40...rewiring layer, 50...substrate, 60...circuit board, 61...terminal electrode, 100...first semiconductor substrate, 101...first substrate body, 101a...one surface, 102...insulating film (first insulating film), 103...terminal electrode (first electrode), 103a...surface, 200...second semiconductor substrate, 201...second substrate body, 201a...one surface, 202...insulating film (second insulating film), 203...terminal electrode (second electrode), 203a...surface, 205... Semiconductor chip, 300... pillar, 301... resin, 410... semiconductor wafer (first semiconductor substrate), 411... substrate main body (first substrate main body), 412... insulating film (first insulating film), 413... terminal electrode (first electrode), 420... semiconductor chip (second semiconductor substrate), 421... substrate main body (second substrate main body), 422... insulating film portion (second insulating film), 423... terminal electrode (second electrode), A... cutting line, H... heat, M1 to M3... semi-finished product, S1... insulating joint portion, S2... electrode joint portion, S3... insulating joint portion, S4... electrode joint portion.

Claims

1. A step of preparing a first semiconductor substrate having a first substrate body and a first insulating film and a first electrode provided on one surface of the first substrate body; preparing a second semiconductor substrate having a second substrate body, and a second insulating film and a plurality of second electrodes provided on one surface of the second substrate body; polishing at least one of the one surface side of the first semiconductor substrate and the one surface side of the second semiconductor substrate; a step of singulating the second semiconductor substrate to obtain a plurality of semiconductor chips, each of which includes an insulating film portion corresponding to the second insulating film and at least one of the second electrodes; aligning the second electrodes of at least one semiconductor chip among the plurality of semiconductor chips with the first electrodes of the first semiconductor substrate; a step of bonding the first insulating film of the first semiconductor substrate and the insulating film portion of the semiconductor chip to each other; and bonding the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip, at least one of the first insulating film and the second insulating film contains an organic material; A method for manufacturing a semiconductor device, wherein the joining step is carried out simultaneously with the laminating step.

2. In the polishing step, at least one of the one surface side of the first semiconductor substrate and the one surface side of the second semiconductor substrate is polished by using a CMP method. The method for manufacturing a semiconductor device according to claim 1 .

3. In the bonding step, the insulating film portion of the semiconductor chip is bonded to the first insulating film of the first semiconductor substrate at a temperature where a temperature difference between the semiconductor chip and the first semiconductor substrate is within 10° C. or at room temperature. The method for manufacturing a semiconductor device according to claim 1 or 2.

4. the modulus of elasticity of the organic material contained in at least one of the first insulating film and the second insulating film is 7.0 GPa or less; The method for manufacturing a semiconductor device according to any one of claims 1 to 3.

5. the thermal expansion coefficient of the organic material contained in at least one of the first insulating film and the second insulating film is 70 ppm / k or less; The method for manufacturing a semiconductor device according to any one of claims 1 to 4.

6. the organic material contained in the second insulating film has a polishing rate that is 5 times or less than a polishing rate of a metal material constituting the second electrode; The method for manufacturing a semiconductor device according to any one of claims 1 to 5.

7. the organic material contained in at least one of the first insulating film and the second insulating film includes polyimide, a polyimide precursor, polyamideimide, benzocyclobutene (BCB), polybenzoxazole (PBO), or a PBO precursor; The method for manufacturing a semiconductor device according to any one of claims 1 to 6.

8. The organic material contained in at least one of the first insulating film and the second insulating film includes a photosensitive resin, a thermosetting non-conductive film, or a thermosetting resin. The method for manufacturing a semiconductor device according to any one of claims 1 to 7.

9. The second insulating film has a thickness greater than a thickness of the first insulating film. The method for manufacturing a semiconductor device according to any one of claims 1 to 8.

10. The thickness of the second insulating film is thinner than the thickness of the first insulating film. The method for manufacturing a semiconductor device according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Semiconductor device and its manufacturing method

    JP2001135663A

  • Semiconductor device, and manufacturing method thereof

    JP2009071045A

  • Semiconductor device and method for manufacturing semiconductor device

    JP2013229415A

  • Method of manufacturing semiconductor device, method of manufacturing flip-chip semiconductor device, semiconductor device and flip-chip semiconductor device

    JP2017152602A

  • Polishing agent, storage liquid for polishing agent and polishing method

    JP2018012752A

Cited By

  • Semiconductor device manufacturing method, slurry, and resin material

    JP7732619B1

  • Semiconductor device production method, slurry, and resin material

    WO2026186132A1