Bonded body, method for manufacturing bonded body, and method for evaluating bonded body
The method addresses organic residue issues in semiconductor bonding by using plasma treatment and XPS analysis to reduce residues and enhance bonding strength, providing accurate evaluation.
Patent Information
- Application Number
- JP2023067063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
AI Technical Summary
Existing bonding methods using solder paste or silver paste for semiconductor elements result in organic residues that degrade bonding strength and are difficult to accurately evaluate, with formic acid treatment being corrosive and ineffective for residue assessment.
A bonded body manufacturing method involving plasma treatment in an oxygen atmosphere to reduce organic residues, combined with XPS analysis for precise residue evaluation, ensuring a carbon concentration ratio of 0.25 or less at specific distances from the bonding layer.
Effectively reduces organic residues without formic acid, enhancing bonding strength and enabling accurate residue evaluation at specific locations.
Smart Images

Figure 2024153275000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonded structure in which a second member is bonded to a portion of a surface of a first member via a bonding layer, a method for manufacturing the bonded structure, and a method for evaluating the bonded structure. [Background technology]
[0002] For example, various devices such as LEDs and power modules have a structure in which electronic components such as semiconductor elements are bonded via a bonding layer onto a circuit layer made of a metal material. Here, when bonding electronic components such as semiconductor elements onto a circuit layer, methods have been proposed that use bonding materials such as solder paste and silver paste, as shown in, for example, Patent Documents 1 and 2.
[0003] However, as described in Patent Documents 1 and 2, when an electronic component such as a semiconductor element is bonded to a circuit layer via a bonding layer using a bonding material such as a solder paste or a silver paste, residues of organic components (organic residues) contained in the bonding material may remain near the bonding layer, causing problems such as a decrease in bonding strength. There is also concern that the organic residues may adversely affect various devices such as LEDs and power modules.
[0004] Therefore, Patent Document 3 proposes a flux composition for solder paste and a solder paste that aim to reduce organic residues. Furthermore, Patent Document 4 proposes that in a bonded body using silver paste as a bonding material, the bonded body is immersed in a mixed liquid of alcohol and water to extract ion residues, and the content of the ion residues is specified. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-083809 A [Patent Document 2] International Publication No. 2007 / 034833 [Patent Document 3] Patent Publication No. 2022-022506 [Patent Document 4] JP 2022-167472 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, the solder paste described in Patent Document 3 requires reflow treatment in a formic acid atmosphere. Since formic acid is corrosive and irritating, there is a problem in that it deteriorates the working environment. In addition, in the bonded body described in Patent Document 4, the organic residue is evaluated by immersing the bonded body in a mixed liquid of alcohol and water to extract ion residues, but it is not possible to distinguish organic matter other than the organic residue caused by the bonding material, and there is a risk that the organic residue caused by the bonding material cannot be accurately evaluated. Also, although it is possible to evaluate the organic residue of the entire bonded body, it is not possible to accurately evaluate the organic residue at a specific location.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a bonded body in which organic residues are sufficiently and reliably reduced and which can suppress occurrence of defects such as a decrease in bonding strength caused by the organic residues; a method for producing a bonded body capable of sufficiently reducing the organic residues without using formic acid; and a method for evaluating a bonded body capable of accurately evaluating organic residues caused by bonding materials. [Means for solving the problem]
[0008] In order to solve the above problems, the bonded body of aspect 1 of the present invention is a bonded body in which a second member is bonded to a portion of a surface of a first member via a bonding layer, and is characterized in that a ratio C2 / C1 of a carbon concentration C1 at a position 1000 μm away from an end of the second member on the surface of the first member to a carbon concentration C2 at a position 500 μm away from the end of the second member on the second member is 0.25 or less.
[0009] According to the bonded body of the first aspect of the present invention, the ratio C2 / C1 between the carbon concentration C1 at a position 1000 μm away from the end of the second member on the surface of the first member and the carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member is set to 0.25 or less, so that the carbon concentration near the bonding layer is not significantly increased compared to the carbon concentration at a position sufficiently away from the bonding layer, and the organic residue near the bonding layer is sufficiently reduced. Therefore, it is possible to suppress the occurrence of defects such as a decrease in bonding strength caused by organic residue.
[0010] The bonded body of aspect 2 of the present invention is characterized in that, in the bonded body of aspect 1 of the present invention, in the plasma treatment process, the ratio C2 / C1 of the carbon concentration C1 at a position 1000 μm away from the end of the second member on the surface of the first member to the carbon concentration C2 at a position 500 μm away from the end of the second member on the second member is 0.20 or less. According to the bonded body of aspect 2 of the present invention, the ratio C2 / C1 of the carbon concentration C1 at a position 1000 μm away from the end of the second member on the surface of the first member to the carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member is 0.20 or less. This further reduces organic residues in the vicinity of the bonding layer, making it possible to further suppress the occurrence of defects such as a decrease in bonding strength caused by organic residues.
[0011] The method for producing a bonded body of aspect 3 of the present invention is a method for producing a bonded body in which a second member is bonded to a portion of a surface of a first member via a bonding layer, and is characterized by comprising a lamination process for obtaining a laminate in which the first member and the second member are laminated via a bonding material, a bonding process for heat-treating the laminate and bonding the first member and the second member via the bonding layer, and a plasma treatment process for performing plasma treatment on the bonded first member and second member.
[0012] According to the method for producing a bonded body of aspect 3 of the present invention, after the bonding step of bonding the first member and the second member via a bonding layer, a plasma treatment step of performing plasma treatment on the bonded first member and the second member is included. Therefore, organic residues can be removed by the plasma treatment, and organic residues in the vicinity of the bonding layer can be sufficiently reduced without performing reflow in a formic acid atmosphere, so that a bonded body can be produced in which the occurrence of defects such as a decrease in bonding strength caused by organic residues is suppressed.
[0013] A fourth aspect of the present invention relates to a method for producing a bonded body, and is characterized in that in the plasma treatment step, the plasma treatment is carried out in an oxygen atmosphere. According to the method for producing a bonded body of the fourth aspect of the present invention, in the plasma treatment step, the plasma treatment is performed in an oxygen atmosphere. This makes it possible to effectively remove organic residues, and thus to produce a bonded body with even less organic residues in the vicinity of the bonding layer.
[0014] A method for evaluating a bonded body according to a fifth aspect of the present invention is a method for evaluating a bonded body in which a second member is bonded to a part of a surface of a first member via a bonding layer, the method comprising the steps of: performing a plasma treatment on a laminate in which the second member is laminated on a part of the surface of the first member without using a bonding material; performing an XPS analysis at a position on the surface of the first member that is 1000 μm away from an end of the second member, and determining a carbon concentration measured as a first standard carbon concentration C0=0; and bonding the second member to a part of the surface of the first member via a bonding material, not performing a plasma treatment, and performing an XPS analysis at a portion of a residue that is visually observed, and determining a carbon concentration measured as a second standard carbon concentration C0=0. 100 = 100, and the carbon concentrations of the surface of the first member and the second member are calculated based on the first standard carbon concentration C0 and the second standard carbon concentration C 100 It is characterized by relative evaluation using
[0015] According to the method for evaluating a bonded body of the fifth aspect of the present invention, the first standard carbon concentration C0 in a laminated body formed without using a bonding material and the second standard carbon concentration C 100Since the carbon concentration on the surface of the bonded body (first member and second member) is evaluated based on the above, it is possible to accurately evaluate the organic residues caused by the bonding material. In addition, it is possible to accurately evaluate the organic residues at specific locations of the bonded body.
[0016] The method for evaluating a bonded body according to a sixth aspect of the present invention is the method for evaluating a bonded body according to the fifth aspect of the present invention, further comprising the steps of: measuring carbon concentrations by performing XPS analysis at a position on the surface of the first member that is 1000 μm away from an end of the second member and at a position on the second member that is 500 μm away from the end of the second member; and comparing the measured carbon concentrations with the first standard carbon concentration C0 and the second standard carbon concentration C1. 100 to determine a carbon concentration C1 at a position 1000 μm away from the end of the second member on the surface of the first member and a carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member, and calculate C2 / C1.
[0017] According to the method for evaluating a bonded body of the sixth aspect of the present invention, the carbon concentration C1 at a position 1000 μm away from the end of the second member on the surface of the first member and the carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member are defined as a first standard carbon concentration C0 and a second standard carbon concentration C2. 100 Since a relative evaluation is performed using the above and C2 / C1 is calculated, the amount of organic residue in the vicinity of the bonding layer can be accurately evaluated. Effect of the Invention
[0018] According to the present invention, it is possible to provide a bonded body in which organic residues are sufficiently and reliably reduced and which can suppress occurrence of defects such as a decrease in bonding strength caused by organic residues, a method for producing a bonded body which can sufficiently reduce organic residues without using formic acid, and a method for evaluating a bonded body which can accurately evaluate organic residues caused by bonding materials. [Brief description of the drawings]
[0019] [Figure 1]1A and 1B are explanatory diagrams of a bonded body according to an embodiment of the present invention, in which (a) is a top view and (b) is a cross-sectional view taken along line XX. [Diagram 2] FIG. 2 is a flow diagram of a method for producing a bonded body according to an embodiment of the present invention. [Diagram 3] 4 is a temperature profile of a reflow process in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, a bonded structure, a method for producing the bonded structure, and a method for evaluating the bonded structure according to embodiments of the present invention will be described with reference to the drawings.
[0021] 1, the bonded body 10 according to this embodiment is formed by bonding a first member 11 and a second member 12 via a bonding layer 13. In this embodiment, the bonded body 10 is a semiconductor device in which a circuit layer (first member 11) of an insulating circuit board and a semiconductor element (second member 12) are bonded via the bonding layer 13.
[0022] In the joined body 10 of this embodiment, as shown in FIG. 1 , the ratio C2 / C1 of the carbon concentration C1 at a position A on the surface of the first member 11 that is 1000 μm away from the end of the second member 12 to the carbon concentration C2 at a position B on the second member 12 that is 500 μm inward from the end of the second member 12 is 0.25 or less. Incidentally, C2 / C1 is preferably 0.20 or less, and more preferably 0.02 or less.
[0023] In this embodiment, the carbon concentration on the surface of the joined body 10 (the first member 11 and the second member 12) is evaluated as follows. First, a plasma treatment was performed on a laminate in which a second member 12 was laminated on a part of the surface of a first member 11 without using any bonding material, and the carbon concentration measured by XPS analysis at a position 1000 μm away from the end of the second member 12 on the surface of the first member 11 was defined as the first reference carbon concentration C0 = 0. Next, the second member 12 is bonded to a part of the surface of the first member 11 via a bonding material, and the plasma treatment is not performed. The carbon concentration measured by XPS analysis on the part of the residue that is visually observed is designated as the second reference carbon concentration C. 100 =100.
[0024] Then, XPS analysis is performed at a position A on the surface of the first member 11 that is 1000 μm away from the end of the second member 12, and at a position B on the surface of the second member 12 that is 500 μm away from the end of the second member 12, to measure the carbon concentration. The measured carbon concentrations are referred to as a first standard carbon concentration C0 and a second standard carbon concentration C1. 100 A relative evaluation was performed using the above to determine the carbon concentration C1 at a position A on the surface of the first member 11 that was 1000 μm away from the end of the second member 12, and the carbon concentration C2 at a position B on the second member 12 that was 500 μm inward from the end of the second member 12, and the ratio C2 / C1 was calculated.
[0025] As described above, by evaluating the ratio C2 / C1 of the carbon concentration C1 at position A on the surface of the first member 11 that is 1000 μm away from the end of the second member 12 to the carbon concentration C2 at a position on the second member 12 that is 500 μm away from the end of the second member 12, it is possible to evaluate the organic residues caused by the bonding material.
[0026] Next, a method for producing the bonded body 10 according to this embodiment will be described with reference to the flow chart of FIG.
[0027] (Paste application process S01) 3, a bonding material is applied to one or both of the bonding surface of the first member 11 and the bonding surface of the second member 12. There are no particular limitations on the bonding material used, and solder paste, Ag paste, etc. can be used. The application method is not particularly limited, but for example, a metal mask method, a screen printing method, a dispensing method, or the like can be used.
[0028] (Lamination process S02) Next, the first member 11 and the second member 12 are laminated together with the bonding material interposed therebetween.
[0029] (Joining process S03) Next, the first member 11 and the second member 12 laminated with the bonding material therebetween are subjected to a reflow treatment to form a bonding layer 13, thereby bonding the first member 11 and the second member 12 together. The heating temperature and holding time in the bonding step S03 are preferably set appropriately depending on the bonding material used. The atmosphere in the bonding step S03 is not particularly limited, but it is preferable to perform the bonding step in a nitrogen gas atmosphere or the like without using formic acid.
[0030] (Plasma treatment step S04) Next, the first member 11 and the second member 12 bonded via the bonding layer 13 are subjected to a plasma treatment. By removing organic residues present around the bonding layer 13 through the plasma treatment step S04, the bonded body 10 of this embodiment is obtained. The plasma treatment step S04 is preferably performed in an oxygen atmosphere, and the output of the plasma treatment step S04 is preferably set within a range of 1400 W or more and 1600 W or less.
[0031] According to the bonded body 10 of the present embodiment configured as described above, the ratio C2 / C1 between the carbon concentration C1 at position A on the surface of the first member 11, which is 1000 μm away from the end of the second member 12, and the carbon concentration C2 at position B on the second member 12, which is 500 μm away from the end of the second member 12, is set to 0.25 or less, so that the carbon concentration in the vicinity of the bonding layer 13 is not significantly increased compared to the carbon concentration at a position sufficiently away from the bonding layer, and the organic residue in the vicinity of the bonding layer 13 is sufficiently reduced. Therefore, it is possible to suppress the occurrence of defects such as a decrease in bonding strength caused by organic residue.
[0032] In the manufacturing method of the bonded body 10 of this embodiment, after the bonding step S03 of bonding the first member 11 and the second member 12 via the bonding layer 13, a plasma treatment step S04 of performing plasma treatment on the first member 11 and the second member 12 bonded via the bonding layer 13 is included. Therefore, organic residues can be removed by the plasma treatment, and the organic residues in the vicinity of the bonding layer 13 can be sufficiently reduced without performing reflow in a formic acid atmosphere, so that a bonded body 10 can be manufactured in which the occurrence of defects such as a decrease in bonding strength caused by organic residues is suppressed.
[0033] Moreover, in the manufacturing method of the bonded body of the present embodiment, when the plasma treatment step S04 is performed in an oxygen atmosphere, the organic residues can be effectively removed, and a bonded body can be manufactured in which the organic residues in the vicinity of the bonding layer are further reduced.
[0034] In this embodiment, a plasma treatment is performed on a laminate in which a second member 12 is laminated on a part of the surface of a first member 11 without using a bonding material, and the carbon concentration measured by performing an XPS analysis at a position on the surface of the first member 11 that is 1000 μm away from the end of the second member 12 is set as a first standard carbon concentration C0=0. A carbon concentration measured by performing an XPS analysis on a part of the surface of the first member 11 without using a bonding material and without performing a plasma treatment is set as a second standard carbon concentration C0=0. 100 = 100, and the carbon concentrations on the surfaces of the first member 11 and the second member 12 are evaluated relatively, so that the organic residues originating from the bonding material can be accurately evaluated. Also, the organic residues at specific locations of the bonded body 10 can be accurately evaluated.
[0035] Then, XPS analysis was performed at a position A on the surface of the first member 11 that was 1000 μm away from the end of the second member 12, and at a position B on the surface of the second member 12 that was 500 μm away from the end of the second member 12, to measure the carbon concentration. The measured carbon concentrations were designated as a first standard carbon concentration C0 and a second standard carbon concentration C1. 100A relative evaluation is performed using the above to determine the carbon concentration C1 at position A on the surface of the first member 11 that is 1000 μm away from the end of the second member 12, and the carbon concentration C2 at a position on the second member 12 that is 500 μm away from the end of the second member 12, and C2 / C1 is calculated, so that the amount of organic residue in the vicinity of the bonding layer 13 can be accurately evaluated.
[0036] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0037] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0038] A substrate (Au (0.05 μm) / Ni (0.5 μm) / Kovar plate) and a dummy chip (Si, Au plating 0.05 μm) were prepared. As a joining material, a paste using RMA type flux manufactured by Mitsubishi Materials Corporation was prepared. Furthermore, a printing mask made of SUS with an opening diameter of 6.5 mm and a thickness of 200 μm was prepared.
[0039] First, a dummy chip was placed on the surface of the above-mentioned newly prepared substrate without applying any paste. Using a reflow simulator (N2 atmosphere), reflow is performed according to the temperature profile shown in Figure 3. Without separating the chip from the substrate after reflow, the carbon concentration was measured by XPS. The carbon concentration was measured at position A on the substrate, 1000 μm away from the edge of the chip, and the reference carbon concentration C0 = 0 was set.
[0040] Next, a bonding material was printed on the surface of the newly prepared substrate using a mask by a manual printer. The bonding material used is shown as Paste A in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. After reflow, the carbon concentration is measured by XPS by visually focusing on the center of the paste residue (an ointment-like organic substance that does not contain metal powder). The measured value is taken as the reference carbon concentration C 100 =100.
[0041] (Example 1 of the present invention) Using a manual printer, the adhesive material is printed on the surface of the newly prepared substrate described above using a mask. The adhesive materials used are shown in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. After reflow, the bonded body was subjected to plasma treatment under the following conditions. Equipment: Nordson MRACH, RF power: 1500W, base pressure: 100mTorr, process pressure: 200mTorr, gas: O2 240sccm, plasma time: 300 s
[0042] The carbon concentration C of the obtained bonded body was measured by XPS analysis at a position A 1000 μm away from the end of the chip on the substrate surface. A , and the measured carbon concentration C at position B 500 μm from the tip of the chip on the chip surface B The carbon concentrations C0 and C 100 Using these, the carbon concentration C1 at position A and the carbon concentration C2 at position B were calculated using the following formulas (1) and (2), and the ratio C2 / C1 was obtained. The evaluation results are shown in Table 1. (1) Formula: C1=(100×(C A -C0)) / C 100 (2) Formula: C2=(100×(C B -C0)) / C 100
[0043] (Example 2 of the present invention) Using a manual printer, the adhesive material is printed on the surface of the newly prepared substrate described above using a mask. The adhesive materials used are shown in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. After reflow, the bonded body was subjected to plasma treatment under the following conditions. Equipment: Nordson MRACH, RF power: 1500W, base pressure: 100mTorr, process pressure: 200mTorr, gas: Ar 240sccm, plasma time: 300s
[0044] For the obtained bonded body, the carbon concentration C1 at position A 1000 μm away from the chip end on the substrate surface and the carbon concentration C2 at position B 500 μm away from the chip end on the chip surface were calculated, and the ratio C2 / C1 was determined, in the same manner as in Invention Example 1. The evaluation results are shown in Table 1.
[0045] (Example 3 of the present invention) Using a manual printer, the adhesive material is printed on the surface of the newly prepared substrate described above using a mask. The adhesive materials used are shown in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. After reflow, the bonded body was subjected to plasma treatment under the following conditions. Equipment: Nordson MRACH, RF power: 1400W, base pressure: 100mTorr, process pressure: 200mTorr, gas: Ar 240sccm, plasma time: 300s
[0046] For the obtained bonded body, the carbon concentration C1 at position A 1000 μm away from the chip end on the substrate surface and the carbon concentration C2 at position B 500 μm away from the chip end on the chip surface were calculated, and the ratio C2 / C1 was determined, in the same manner as in Invention Example 1. The evaluation results are shown in Table 1.
[0047] Comparative Example 1 Using a manual printer, the adhesive material is printed on the surface of the newly prepared substrate described above using a mask. The adhesive materials used are shown in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. After reflow, the bonded body was heated to 50°C in cleaning solution (Pine Alpha, Arakawa Chemical) and ultrasonically cleaned for 5 minutes. It was then washed with 70°C hot water for 5 minutes. After cleaning, it was dried in a dryer for 5 minutes. For the obtained bonded body, the carbon concentration C1 at position A 1000 μm away from the chip end on the substrate surface and the carbon concentration C2 at position B 500 μm away from the chip end on the chip surface were calculated, and the ratio C2 / C1 was determined, in the same manner as in Invention Example 1. The evaluation results are shown in Table 1.
[0048] Comparative Example 2 Using a manual printer, the adhesive material is printed on the surface of the newly prepared substrate described above using a mask. The adhesive materials used are shown in Table 1. A dummy chip was mounted on the printed bonding material, and reflow was performed using a reflow simulator (N2 atmosphere) with the temperature profile shown in Figure 3. No plasma treatment or cleaning treatment was performed on the bonded body after reflow. For the obtained bonded body, the carbon concentration C1 at position A 1000 μm away from the chip end on the substrate surface and the carbon concentration C2 at position B 500 μm away from the chip end on the chip surface were calculated, and the ratio C2 / C1 was determined, in the same manner as in Invention Example 1. The evaluation results are shown in Table 1.
[0049] (Wire bondability evaluation) The bonded body obtained as described above was subjected to a wire bonding test as follows. Using an ultrasonic thermocompression bonding multi-board (7KE manufactured by WEST BOND), ten 25μmφ gold wires were wire-bonded under the following conditions, and the number of gold wires that were successfully bonded was evaluated. The evaluation results are shown in Table 1. Ultrasonic: 30ms Load: 25g Temperature: 150℃ Distance between WB foot and chip: 500~1000μm Distance on chip: Within 200μm from the feet
[0050] [Table 1]
[0051] In Comparative Example 1, reflow was performed in an N2 atmosphere, and cleaning was performed after reflow. C2 / C1 was 0.33, which means that the organic residue was not sufficiently reduced, and only 5 out of 10 wires were bonded in the wire bonding test. In Comparative Example 2, reflow was performed in an N2 atmosphere and cleaning was not performed after reflow. C2 / C1 was 0.70, a large amount of organic residue was generated, and wire bonding was not possible in the wire bonding test.
[0052] In contrast, in Example 1 of the present invention, reflow was performed in an N2 atmosphere, and plasma treatment (1500 W) was performed in an oxygen atmosphere after reflow. As a result, C2 / C1 became 0.02, the organic residue was sufficiently removed, and all 10 wires were bonded in the wire bonding test.
[0053] In the present invention example 2, reflow was performed in a N2 atmosphere, and plasma treatment (1500 W) was performed in an argon atmosphere after reflow. As a result, C2 / C1 became 0.19, organic residues were sufficiently removed, and all 10 wires were bonded in the wire bonding test.
[0054] In Example 3 of the present invention, reflow was performed in an N2 atmosphere, and plasma treatment (1400 W) was performed in an argon atmosphere after reflow. As a result, C2 / C1 became 0.24, organic residues were sufficiently removed, and 8 out of 10 wires were bonded in the wire bonding test.
[0055] In addition, in Example 1 of the present invention, in which the plasma treatment was carried out in an oxygen atmosphere, C2 / C1 was lower than in Example 2 of the present invention, in which the plasma treatment was carried out in an argon atmosphere, and organic residues were able to be removed more efficiently.
[0056] From the results of the above confirmatory experiments, it was confirmed that the present invention can provide a bonded body in which organic residues are sufficiently and reliably reduced and which can suppress the occurrence of defects such as a decrease in bonding strength caused by organic residues, a method for manufacturing a bonded body that can sufficiently reduce organic residues without using formic acid, and a method for evaluating a bonded body that can accurately evaluate organic residues caused by bonding materials. [Explanation of symbols]
[0057] 10 zygote 11 First member 12 Second member 13 Bonding layer
Claims
1. A bonded body in which a second member is bonded to a part of a surface of a first member via a bonding layer, A joint body, characterized in that a ratio C2 / C1 of a carbon concentration C1 at a position 1000 μm away from an end of the second member on the surface of the first member to a carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member is 0.25 or less.
2. The joined body according to claim 1, characterized in that a ratio C2 / C1 of a carbon concentration C1 at a position 1000 μm away from an end of the second member on the surface of the first member to a carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member is 0.20 or less.
3. A method for producing a bonded body in which a second member is bonded to a part of a surface of a first member via a bonding layer, comprising the steps of: a lamination step of obtaining a laminate by laminating a first member and a second member via a bonding material; a bonding step of heat-treating the laminate and bonding the first member and the second member via a bonding layer; and a plasma treatment step of performing a plasma treatment on the bonded first member and the second member. A method for manufacturing a bonded body, comprising:
4. 4. The method for producing a bonded body according to claim 3, wherein the plasma treatment is carried out in an oxygen atmosphere in the plasma treatment step.
5. A method for evaluating a bonded structure in which a second member is bonded to a part of a surface of a first member via a bonding layer, comprising the steps of: A plasma treatment is performed on a laminate in which the second member is laminated on a part of the surface of the first member without using a bonding material, and the carbon concentration measured by performing an XPS analysis at a position on the surface of the first member that is 1000 μm away from the end of the second member is defined as a first reference carbon concentration C 0 = 0, The second member is bonded to a part of the surface of the first member via a bonding material, and the plasma treatment is not performed. The carbon concentration measured by XPS analysis of the part of the residue that is visually observed is defined as the second reference carbon concentration C. 100 = 100, The carbon concentration of the surface of the first member and the second member is determined as the first reference carbon concentration C 0 and the second reference carbon concentration C 100 A method for evaluating a bonded body, comprising the steps of:
6. The carbon concentration is measured by performing XPS analysis at a position on the surface of the first member that is 1000 μm away from the end of the second member and at a position on the surface of the second member that is 500 μm away from the end of the second member, and the measured carbon concentration is referred to as the first reference carbon concentration C 0 and the second reference carbon concentration C 100 Relative evaluation is performed using The method for evaluating a joint body according to claim 5, characterized in that a carbon concentration C1 at a position 1000 μm away from an end of the second member on the surface of the first member and a carbon concentration C2 at a position 500 μm away from the end of the second member on the surface of the second member are obtained, and C2 / C1 is calculated.
Citation Information
Patent Citations
Flux, solder paste and joined part
JP2011083809A
Flux composition for solder paste
JP2022022506A
Joint body and method for producing joint body
JP2022167472A
Pasty silver particle composition, process for producing solid silver, solid silver, joining method, and process for producing printed wiring board