Positive electrode active material, positive electrode plate, nonaqueous electrolyte secondary battery, and method of producing positive electrode active material
A positive electrode active material with high nickel content nickel-cobalt-manganese compounds, coated with phosphoric acid and lithium-containing oxides, addresses particle cracking and lithium extraction issues, enhancing energy density and cycle characteristics.
Patent Information
- Application Number
- JP2023067147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Positive electrode plates containing high nickel content nickel-cobalt-manganese compounds suffer from particle cracking during manufacturing and cycling, which affects energy density and cycle characteristics, and surface coatings to prevent cracking reduce thermal stability.
A positive electrode active material composed of single and aggregated particles containing a high nickel content nickel-cobalt-manganese compound, coated with a phosphoric acid compound and lithium-containing metal oxides or lithium borate, to enhance energy density and cycle characteristics.
The solution effectively suppresses particle cracking and lithium extraction, improving both energy density and cycle characteristics of the positive electrode active material.
Smart Images

Figure 2024153329000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material, and further to a positive electrode plate, a non-aqueous electrolyte secondary battery, and a method for producing the positive electrode active material. [Background technology]
[0002] Patent Document 1 discloses a lithium metal composite oxide composed of secondary particles formed by agglomerations of primary particles and single particles that exist independently of the secondary particles, and proposes improving the packing density by blending the single particles and secondary particles to make the circularity distribution of the active material bimodal (two-peak distribution). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-87879 A Summary of the Invention [Problem to be solved by the invention]
[0004] In positive electrode plates containing single particles and agglomerated particles containing nickel-cobalt-manganese compounds with a high nickel content (hereinafter also referred to as Hi-Ni NCM compounds) as positive electrode active materials, particle cracking of the agglomerated particles is likely to occur during the compression process in the manufacturing process, and the particle cracking may progress during cycle testing. On the other hand, in order to suppress particle cracking, coating of the particle surface with a different element has been considered, but the coating may extract lithium from inside the bulk of the positive electrode active material, reducing the thermal stability of the positive electrode active material and the cycle characteristics.
[0005] An object of the present disclosure is to provide a positive electrode active material that contains single particles and agglomerated particles containing a Hi-Ni-based NCM compound and that can achieve both energy density and cycle characteristics, a positive electrode plate containing the same, a nonaqueous electrolyte secondary battery, and a method for producing the positive electrode active material. [Means for solving the problem]
[0006] The present disclosure provides the following positive electrode active material, positive electrode plate, nonaqueous electrolyte secondary battery, and method for producing the positive electrode active material. [1] A positive electrode active material comprising single particles and aggregated particles, The single particles and the agglomerated particles contain a nickel-cobalt-manganese compound, The nickel content in the nickel-cobalt-manganese compound contained in the single particle is 70 mol % or more, The nickel content in the nickel-cobalt-manganese compound contained in the agglomerated particles is 75 mol % or more, The aggregated particles further include a phosphate compound and at least one selected from the group consisting of a lithium-containing metal oxide and a lithium borate, a molar ratio of the total mass of the lithium-containing metal oxide and lithium borate to the phosphate compound in the agglomerated particles is 5.0 or less. [2] The positive electrode active material according to [1], wherein a mass ratio of the single particles to the aggregated particles is 20:80 to 50:50. [3] The positive electrode active material according to [1] or [2], wherein the lithium-containing metal oxide contains at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, and lithium aluminate. [4] A positive electrode active material layer containing the positive electrode active material according to any one of [1] to [3], wherein the density of the positive electrode active material layer is 3.65 g / cm 3 That's all for the positive plate. [5] A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to [4]. [6] A method for producing a positive electrode active material according to any one of [1] to [3], a first treatment step of coating the aggregated particles with a phosphoric acid compound; a second treatment step of heat-treating the aggregated particles obtained after the first treatment step using at least one selected from the group consisting of metal oxides and boric acid, and a lithium salt; and A mixing step of mixing the aggregated particles after the second treatment step with the single particles. A method for producing a positive electrode active material comprising the steps of: Effect of the Invention
[0007] The present disclosure provides a positive electrode active material that contains single particles and agglomerated particles containing a Hi-Ni-based NCM compound and that can achieve both energy density and cycle characteristics, a positive electrode plate containing the same, a nonaqueous electrolyte secondary battery, and a method for producing the positive electrode active material. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic flow chart of a method for producing a positive electrode active material in this embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a battery according to this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of an electrode body in this embodiment. [Figure 4] FIG. 4 is a conceptual diagram showing the positive electrode plate in this embodiment. [Diagram 5] FIG. 5 is a schematic flowchart of a method for producing a positive electrode plate in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.
[0010] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."
[0011] <Cathode active material> The positive electrode active material includes single particles and aggregated particles. This makes it easier to increase the packing density of the positive electrode active material layer of the positive electrode plate. The positive electrode active material may be substantially composed of single particles and aggregated particles. The positive electrode active material of this embodiment may be a non-aqueous electrolyte secondary battery. Details of the non-aqueous electrolyte secondary battery will be described later.
[0012] The single particles and the aggregated particles may have any size. The average particle size D50 of the single particles may be, for example, 1 μm or more and 20 μm or less, preferably 1 μm or less and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. The average particle sizes D50, D70, and D30 of the aggregated particles may be, for example, 1 μm or less and 40 μm or less, preferably 1 μm or less and 30 μm or less, and more preferably 1 μm or more and 20 μm or less. The average particle sizes D50, D70, and D30 represent particle sizes at which the cumulative particle volume from the small particle size side in the volume-based particle size distribution is 50%, 70%, and 30% of the total particle volume, respectively. The average particle size can be measured by a laser diffraction / scattering method.
[0013] The aggregated particles may be aggregates of primary particles. The primary particles are particles in which grain boundaries cannot be visually confirmed in an SEM image of the particles, and have an average primary particle size of less than 0.5 μm. The average primary particle size refers to the distance between the two most distant points on the contour line of the primary particle. The average primary particle size of the primary particles may be, for example, 0.05 μm to 0.2 μm or 0.1 μm to 0.2 μm. When 10 or more primary particles randomly extracted from an SEM image of one aggregated particle have an average primary particle size of 0.05 μm to 0.2 μm, all of the primary particles contained in the aggregated particle are considered to have an average primary particle size of 0.05 μm to 0.2 μm. The primary particles may have an average primary particle size of, for example, 0.1 μm to 0.2 μm.
[0014] The single particles and agglomerated particles (primary particles) contain a nickel-cobalt-manganese compound (hereinafter also referred to as an NCM compound). The nickel content in the NCM compound contained in the single particles is 70 mol% or more, preferably 73 mol% or more, and more preferably 76 mol% or more. The nickel content in the NCM compound contained in the agglomerated particles (primary particles) is 75 mol% or more, preferably 78 mol% or more, and more preferably 81 mol% or more. The nickel content is the content ratio of nickel to metal elements other than lithium.
[0015] The NCM compound preferably contains nickel-cobalt-manganese composite hydroxide, more preferably lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained by, for example, a coprecipitation method. The nickel-cobalt-manganese composite hydroxide is, for example, a compound represented by the general formula: Ni x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.
[0016] The single particle may be, for example, a particle represented by the following formula (1): Li 1-a1 Ni x1 Me 1 1-x1 O2(1) [In formula (1), “a1” satisfies the relationship: −0.3≦a1≦0.3. “x1” satisfies the relationship 0.7≦x1<1.0. "Me 1 " represents at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W. The layered metal oxide may contain one or more first layered metal oxides represented by the following formula:
[0017] The primary particles are, for example, represented by the following formula (2): Li 1-a2 Ni x2 Me 2 1-x2 O2(2) [In Formula (2), "a2" satisfies the relationship of -0.3 ≤ a2 ≤ 0.3. "x2" satisfies the relationship of 0.75 ≤ x2 ≤ 1.0. "Me 2 " represents at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W.] It may contain one or more of the second-layered metal oxides represented by the formula.
[0018] In Formulas (1) and (2), for example, the relationship of "x1 < x2" may be satisfied.
[0019] For example, the single particle may contain at least one selected from the group consisting of LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2O2, and LiNi 0.8 Co 0.1 Mn 0.1 O2. For example, the primary particle may contain at least one selected from the group consisting of LiNi 0.75 Co 0.15 Mn 0.1 O2, and LiNi 0.75 Co 0.1 Mn 0.15 O2, and LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0020] For example, both the single particle and the primary particle may consist essentially of LiNi 0.75 Co 0.15 Mn 0.1 O2. For example, both the single particle and the primary particle may consist essentially of LiNi 0.75 Co 0.1 Mn0.15 For example, both the single particles and the primary particles may be substantially composed of LiNiO2. 0.8 Co 0.1 Mn 0.1 For example, a single particle may be substantially composed of LiNiO2. 0.7 Co 0.2 Mn 0.1 O2, and the primary particles are essentially LiNi 0.75 Co 0.1 Mn 0.15 For example, a single particle may be substantially composed of LiNiO2. 0.7 Co 0.2 Mn 0.1 O2, and the primary particles are essentially LiNi 0.75 Co 0.15 Mn 0.1 It may consist of O2.
[0021] When the single particle contains a lithium nickel cobalt manganese composite oxide, the single particle can be obtained by mixing a lithium source such as lithium hydroxide and a nickel cobalt manganese composite hydroxide, firing the mixture, and then wet-pulverizing the mixture using a ball mill or the like and drying the mixture. The single particle may be surface-treated.
[0022] The agglomerated particles further contain a phosphate compound and at least one selected from the group consisting of lithium-containing metal oxides and lithium borate (Li3BO3). This suppresses particle cracking of the agglomerated particles, making it easier to achieve a desired energy density, and also suppresses extraction of lithium from the inside of the agglomerated particles, making it easier to suppress deterioration of cycle characteristics. The degree of extraction of lithium from the inside of the agglomerated particles can be evaluated by the DTG peak value of a TG curve obtained by differential thermogravimetry (DTG) measurement described in the Examples section.
[0023] The phosphate compound may include, for example, lithium phosphate (Li3PO4) and the like. The lithium-containing metal oxide may include, for example, at least one selected from the group consisting of lithium tungstate (Li2WO4), lithium zirconate (Li2ZrO3), lithium titanate (Li2TiO3) and lithium aluminate (LiAlO2). From the viewpoints of energy density and cycle characteristics, the aggregated particles preferably include lithium borate.
[0024] When the agglomerated particles are lithium nickel cobalt manganese composite oxides, the agglomerated particles can be obtained by, for example, mixing a lithium source such as lithium hydroxide with a nickel cobalt manganese composite hydroxide and calcining to obtain an agglomerated lithium nickel cobalt manganese composite oxide (hereinafter also referred to as lithium composite oxide), surface-treating the agglomerated lithium composite oxide with a phosphoric acid compound, and then heat-treating it with at least one selected from the group consisting of metal oxides and boric acid, and a lithium salt. Usually, when the surface of a Hi-Ni-based NCM active material is coated with a metal oxide or boric acid, lithium is extracted from the inside of the agglomerated particles, and the agglomerated particles are converted into compounds such as lithium-containing metal oxides and lithium borate. In order to suppress this reaction, the surface of the Hi-Ni-based NCM active material is subjected to mechanochemical treatment using a phosphate compound such as lithium phosphate, and then heat treatment is performed using a metal oxide, boric acid, and a lithium salt. This forms a barrier layer of the phosphate compound that suppresses the diffusion of lithium between the surface of the Hi-Ni-based NCM active material and the coating layer, thereby suppressing the extraction of lithium from inside the agglomerated particles, and is presumably helpful in suppressing the deterioration of cycle characteristics.
[0025] Examples of methods for surface-treating the lithium composite oxide having an aggregated structure with a phosphate compound include mechanochemical treatment. Mechanochemical treatment can facilitate the formation of a phosphate compound layer on the surface of the aggregated particles. The mechanochemical treatment can be, for example, a dry treatment in which a base material (particles made of lithium composite oxide having an aggregated structure) and coating material particles (lithium phosphate) are rotated at high speed in a container together with media (zirconia beads), and the coating material particles are crushed and bonded to the surface of the base material to coat it. The molar ratio of the coating material particles to the base material may be, for example, 0.01 mol% or more and 2.0 mol% or less.
[0026] A method of heat treating an aggregated lithium composite oxide (also called a surface-treated lithium composite oxide) surface-treated with a phosphoric acid compound using at least one selected from the group consisting of metal oxides and boric acid (H3BO3) and a lithium salt includes, for example, a method of mixing the surface-treated lithium composite oxide with at least one selected from the group consisting of metal oxides and boric acid and a lithium salt, and heating at a temperature of 200°C or higher and 400°C or lower for 3 minutes to 120 minutes. An example of the lithium salt is lithium carbonate. An example of the metal oxide is tungstic acid (H3BO3), zirconate (H4O4Zr), titanate (H4TiO4), aluminate (HAlO2), etc. The heat treatment time is preferably 10 minutes to 60 minutes from the viewpoint of energy density and cycle characteristics.
[0027] The molar ratio of the total mass of the lithium-containing metal oxide and lithium borate to the phosphate compound in the aggregated particles (hereinafter also referred to as the covering ratio) is 5.0 or less. The lower limit of the covering ratio may be, for example, 0.5 or more, 0.8 or more, or 1.0 or more. The upper limit of the covering ratio may be, for example, 4.0 or less, 3.0 or less, 2.0 or less, or 1.8 or less.
[0028] The mass ratio of the single particles to the aggregated particles in the positive electrode active material may be, for example, 20:80 to 50:50, and preferably 30:70 to 50:50. When the mass ratio of the single particles to the aggregated particles in the positive electrode active material is within the above range, the filling property tends to be easily improved.
[0029] The DTG peak value of the positive electrode active material may be, for example, less than 3.2% / min, preferably 3.0% / min or less, more preferably 2.0% / min or less, and further preferably 1.5% / min or less. The DTG peak value of the positive electrode active material is measured according to the method described in the Examples section below.
[0030] <Method of manufacturing positive electrode active material> The method for producing a positive electrode active material includes a first treatment step (A) of coating aggregated particles with a phosphate compound by, for example, mechanochemical treatment, a second treatment step (B) of heat-treating the aggregated particles after the first treatment step using at least one selected from the group consisting of metal oxides and boric acid and a lithium salt, and a mixing step (C) of mixing the aggregated particles after the second treatment step with single particles, as shown in Fig. 1. The above explanations apply to the single particles, the aggregated particles, the phosphate compound, the mechanochemical treatment, and the heat treatment.
[0031] <Nonaqueous electrolyte secondary battery> Fig. 2 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery in this embodiment. The battery 100 shown in Fig. 2 may be, for example, a lithium ion battery used as a main power source or a power assist power source for an electric vehicle.
[0032] The battery 100 includes an exterior body 90. The exterior body 90 houses an electrode assembly 50 and an electrolyte (not shown). The electrode assembly 50 is connected to a positive terminal 91 by a positive current collecting member 81. The electrode assembly 50 is connected to a negative terminal 92 by a negative current collecting member 82. FIG. 3 is a schematic diagram showing an example of an electrode assembly in this embodiment. The electrode assembly 50 is of a wound type. The electrode assembly 50 includes a positive electrode plate 20, a separator 40, and a negative electrode plate 30. That is, the battery 100 includes a positive electrode plate 20. The positive electrode plate 20 includes a positive electrode active material layer 22 and a positive electrode substrate 21. The negative electrode plate 30 includes a negative electrode active material layer 32 and a negative electrode substrate 31.
[0033] <Positive electrode plate> As shown in Fig. 4, the positive electrode plate 20 may have a positive electrode active material layer 22 formed directly or indirectly on one or both sides of a positive electrode substrate 21. The positive electrode substrate 21 may be a conductive sheet made of, for example, an Al alloy foil, a pure Al foil, or the like. The positive electrode active material layer 22 contains a positive electrode active material containing single particles 11 and agglomerated particles 12. The positive electrode active material layer 22 contains the above-mentioned positive electrode active material. The positive electrode active material layer 22 may further contain a conductive material, a binder, and the like.
[0034] The positive electrode active material layer 22 may have a thickness of, for example, 10 μm or more and 200 μm or less. The positive electrode active material layer 22 may have a high density. The density of the positive electrode active material layer 22 is, for example, 3.65 g / cm 3 or more, 3.7 g / cm 3 or more than 3.8g / cm 3 The positive electrode active material layer 22 may have a density of, for example, 4.0 g / cm 3 It may have the following densities:
[0035] <Manufacturing method of positive electrode plate> The manufacturing method of the positive electrode plate 20 in this embodiment includes the preparation of a positive electrode slurry (A), application (B), and rolling (C) as shown in FIG. 5. In the preparation of the positive electrode slurry (A), a positive electrode slurry containing the above-mentioned positive electrode active material is prepared. The positive electrode slurry is prepared by dispersing the positive electrode active material in a dispersion medium. The dispersion medium may be an organic solvent, such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK), and dimethyl sulfoxide (DMSO). The positive electrode slurry may contain a conductive material and a binder. Examples of the conductive material include carbon nanotubes, carbon black such as acetylene black (AB), and other carbon materials (e.g., graphite, etc.). Examples of the binder include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide (PA), polyamideimide (PAI), butadiene rubber (BR), styrene butadiene rubber (SBR), nitrile-butadiene rubber (NBR), styrene-ethylene-butylene-styrene block copolymer (SEBS), carboxymethyl cellulose (CMC), or a combination thereof. The slurry may have a solids concentration of, for example, 40% to 80%. Any stirring device, mixing device, or dispersing device may be used for mixing.
[0036] In coating (B), the positive electrode slurry is coated on the surface of the positive electrode substrate 21 to form a positive electrode active material layer 22. In rolling (C), the positive electrode active material layer 22 and the positive electrode substrate 21 are rolled to produce the positive electrode plate 20. A raw sheet of the positive electrode plate 20 is produced by rolling. The raw sheet can be cut to a predetermined planar size according to the specifications of the battery 100. EXAMPLES
[0037] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0038] <Example 1> [Preparation of single particles] Obtained by coprecipitation, with the composition Ni 0.78 Co 0.11 Mn 0.11 The nickel-cobalt-manganese composite hydroxide of (OH)2 was calcined at 500°C to obtain a nickel-cobalt-manganese composite oxide (Z1). Next, lithium hydroxide and the nickel-cobalt-manganese composite oxide (Z1) were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.05:1, and the mixture was calcined at 900°C for 72 hours in an oxygen atmosphere, and then wet-pulverized in a ball mill and dried to form a single particle structure. The mixture was then heat-treated again at 750°C for 10 hours in an oxygen atmosphere to obtain a lithium composite oxide (composite oxide A) with a single particle structure. When the particle size distribution of the composite oxide A was measured, the particle diameter (D50) was 3.6 μm, and when the structure was observed by SEM, the composite oxide A was almost a particle with a single particle structure, and the particle diameter was 2.5 to 3.8 μm.
[0039] [Preparation of aggregated particles] Obtained by coprecipitation, with the composition Ni 0.83 Co 0.05 Mn 0.12 The nickel-cobalt-manganese composite hydroxide of (OH)2 was calcined together with lithium hydroxide in an oxygen atmosphere at a temperature of 800°C for 10 hours, and then crushed to obtain a lithium composite oxide. 0.2 mol% of lithium phosphate was added to this and mechanochemically treated for a predetermined time with φ2 mm zirconia balls using a P5 planetary mill manufactured by Flitch, to obtain a lithium composite oxide (composite oxide B1) with an aggregated structure coated with lithium phosphate (first treatment step). Next, the composite oxide B1 was added with 0.6 wt% boric acid and an equal molar amount of lithium carbonate, and heat-treated at a temperature of 300°C to obtain a lithium composite oxide B1 (composite oxide B) with an aggregated structure coated with lithium borate (Li3PO4) as a surface-coating compound (second treatment step). The coating ratio and heat treatment time are shown in Table 1.
[0040] The particle size distribution of composite oxide B was D50 12 μm, D70 14 μm, and D30 10 μm. The cross section of composite oxide B after CP processing was observed by SEM, and the average primary particle diameter of composite oxide B was 0.13 μm.
[0041] [Preparation of positive electrode active material] The composite oxide A and the composite oxide B2 were mixed in a mass ratio of 1:1 (mixing step) to obtain the positive electrode active material of Example 1.
[0042] <Examples 2 to 10> A positive electrode active material was prepared in the same manner as in Example 1, except that the additive compounds and surface coating compounds shown in Table 1 were used in amounts so as to obtain the coating ratios shown in Table 1, and that the treatment time in the second treatment step was shown in Table 1.
[0043] <Comparative Example 1> A positive electrode active material was produced in the same manner as in Example 1, except that the aggregated particles were produced by the following procedure. Obtained by coprecipitation, with the composition Ni 0.83 Co 0.05 Mn 0.12 The nickel-cobalt-manganese composite hydroxide (OH)2 was baked together with lithium hydroxide in an oxygen atmosphere at 800°C for 10 hours, and then crushed to obtain a lithium composite oxide. To this, the lithium composite oxide coated with lithium phosphate, 0.6 wt% boric acid, and an equal molar amount of lithium carbonate were added, and the mixture was heat-treated at a temperature of 300°C for 5 minutes to obtain a lithium composite oxide coated with lithium borate (Li3PO4). The heat treatment time is shown in Table 1.
[0044] [Preparation of positive electrode plate] The positive electrode active material obtained in the examples and comparative examples, acetylene black, and polyvinylidene fluoride (PVdF) were further mixed to a solid content mass ratio of 96.3:2.5:1.2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, followed by kneading to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a 13 μm thick aluminum foil core of No. 1N30, the coating was dried, and then the coating was rolled using a rolling machine until the composite density of the coating was 3.7 g / cm. 3 Then, the positive electrode core was compressed so as to have a predetermined electrode size, and then cut to obtain a positive electrode plate having a positive electrode mixture layer formed on both sides of the positive electrode core.
[0045] [Production and evaluation of small lithium-ion batteries] A separator was placed between the electrode and the carbon anode, which was then placed in a laminated outer bag, and the electrolyte was added and sealed to produce a small laminated battery. Batteries of the examples and comparative examples shown in the table were produced to obtain positive electrode active materials with different coating treatments. The size of the battery was determined by stacking eight layers of electrode bodies to obtain a charge capacity of 600 mAh. The measurement results of charge capacity (mAh / g) and discharge capacity (mAh / g) are shown in Table 1.
[0046] [Evaluation of DTG peak value] The battery after charging was disassembled, washed and dried, and the powder mixture active material powder was scraped off from the positive electrode plate, and 10 mg was loaded into an Al pan in an Ar atmosphere glove box. The thermogravimetric change was measured at a rate of 5°C / min up to 500°C using a TG-DTA device (Shimadzu DTA-60AH), and the DTG peak value (% / min) associated with oxygen release from the active material was obtained from the differential curve. The results are shown in Table 1.
[0047] [Table 1]
[0048] As shown in Table 1, the results showed that the DTG peak values were lower in Examples 1 to 10 than in Comparative Example 1. It is clear that the positive electrode active material of the present disclosure can achieve both good energy density and good cycle characteristics. [Explanation of symbols]
[0049] 11 single particle, 12 agglomerated particle, 20 positive electrode plate, 21 positive electrode substrate, 22 positive electrode active material layer, 30 negative electrode plate, 31 negative electrode substrate, 32 negative electrode active material layer, 40 separator, 50 electrode body, 81 positive electrode current collector, 82 negative electrode current collector, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 100 battery.
Claims
1. A positive electrode active material including single particles and aggregated particles, The single particles and the agglomerated particles contain a nickel-cobalt-manganese compound, The nickel content in the nickel-cobalt-manganese compound contained in the single particle is 70 mol % or more, The nickel content in the nickel-cobalt-manganese compound contained in the agglomerated particles is 75 mol % or more, The aggregated particles further include a phosphate compound and at least one selected from the group consisting of a lithium-containing metal oxide and a lithium borate, a molar ratio of a total mass of the lithium-containing metal oxide and lithium borate to the phosphate compound in the agglomerated particles is 5.0 or less.
2. 2. The positive electrode active material according to claim 1, wherein a mass ratio of the single particles to the aggregated particles is 20:80 to 50:
50.
3. 2. The positive electrode active material according to claim 1, wherein the lithium-containing metal oxide comprises at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, and lithium aluminate.
4. A cathode active material layer containing the cathode active material according to claim 1, wherein the density of the cathode active material layer is 3.65 g / cm 3 That's all for the positive plate.
5. A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to claim 4.
6. A method for producing a positive electrode active material according to claim 1, A first treatment step of coating the aggregated particles with a phosphoric acid compound; a second treatment step of heat-treating the aggregated particles obtained after the first treatment step using at least one selected from the group consisting of metal oxides and boric acid, and a lithium salt; and a mixing step of mixing the aggregated particles after the second treatment step with the single particles; A method for producing a positive electrode active material comprising the steps of:
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
JP2019212400A
Positive electrode active material for lithium ion secondary battery, and method for manufacturing the same
JP2021064598A
Nonaqueous electrolyte secondary battery
JP2022112207A
Positive electrode material and preparation method thereof, lithium ion secondary battery
JP2023502845A
Non-aqueous electrolyte secondary battery
WO2016157735A1
Cited By
Secondary battery positive electrode and secondary battery
WO2026140578A1