Manufacturing method of silicon clathrate active material, and manufacturing method of lithium-ion battery

By oxidizing the surface of sodium-containing silicon clathrate and acid washing, the method addresses the issue of expansion in silicon clathrate active materials, resulting in a low-expansion material for lithium ion batteries.

JP2024153364AInactive Publication Date: 2024-10-29TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023067217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon clathrate active materials, while effective in reducing expansion during charging, still require further suppression of expansion to enhance battery performance.

Method used

A method involving partial oxidation of the surface of sodium-containing silicon clathrate followed by acid washing to improve the removal of by-products and reduce voids in the clathrate structure, resulting in a silicon clathrate active material with reduced expansion.

Benefits of technology

The method produces a silicon clathrate active material with minimal expansion during charging, suitable for use in lithium ion batteries, enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153364000001
    Figure 2024153364000001
Patent Text Reader

Abstract

To provide a manufacturing method of silicon clathrate active material with small expansion, and a manufacturing method of lithium-ion battery including manufacture of such a silicon clathrate active material.SOLUTION: A disclosed manufacturing method of a silicon clathrate active material includes: oxidizing at least partially the surface of the sodium-containing silicon clathrate; and washing the oxidized silicon clathrate with acid. A disclosed manufacturing method of a lithium-ion battery includes: manufacturing the silicon clathrate active material using the disclosed method: and forming a negative electrode active material layer by using the silicon clathrate active material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a silicon clathrate active material and a method for producing a lithium ion battery. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as an active material for batteries, particularly lithium ion batteries.

[0003] Silicon active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate active material as the silicon active material.

[0004] For example, Patent Document 1 discloses a silicon clathrate active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]

[0006] Although silicon clathrate active materials can suppress expansion during charging as compared with ordinary silicon active materials, there is a demand for further suppression of the expansion of silicon clathrate active materials during charging.

[0007] An object of the present disclosure is to provide a method for producing a silicon clathrate active material with low expansion, and a method for producing a lithium ion battery that includes producing such a silicon clathrate active material. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a silicon clathrate active material, comprising the steps of: at least partially oxidizing the surface of the sodium-containing silicon clathrate; and washing the oxidized sodium-containing silicon clathrate with an acid. <Aspect 2> 2. The method of embodiment 1, wherein the surface of the sodium-containing silicon clathrate is at least partially oxidized by exposing the sodium-containing silicon clathrate to an air atmosphere. <Aspect 3> 3. The method of any one of the preceding claims, wherein the sodium-containing silicon clathrate has at least a partial clathrate II structure. <Aspect 4> The method according to any one of aspects 1 to 3, wherein the sodium-containing silicon clathrate has a porous structure. <Aspect 5> The method according to any one of aspects 1 to 4, wherein the silicon clathrate active material is for use as a negative electrode active material in a lithium ion battery. Aspect 6 Producing a silicon clathrate active material by the method according to any one of aspects 1 to 5; and forming a negative electrode active material layer using the silicon clathrate active material; How lithium-ion batteries are manufactured. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a method for producing a silicon clathrate active material that exhibits small expansion during charging, and a method for producing a lithium ion battery that includes producing such a silicon clathrate active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] <<Method for producing silicon clathrate active material>> The disclosed method of making a silicon clathrate active material includes at least partially oxidizing a surface of a sodium-containing silicon clathrate and washing the oxidized sodium-containing silicon clathrate with an acid.

[0012] The sodium-containing silicon clathrate used as a raw material in the present disclosure can be obtained by any method. Generally, the sodium-containing silicon clathrate can be formed by removing sodium from NaSi alloy (sodium silicon alloy).

[0013] For example, in the production of sodium-containing silicon clathrate, first, silicon and sodium hydride are reacted to prepare NaSi alloy, and then the thus-prepared NaSi alloy is reacted with aluminum fluoride as a sodium trapping agent to prepare sodium-containing silicon clathrate.

[0014] At this time, in addition to the sodium-containing silicon clathrate, by-products such as sodium fluoride and aluminum are generated. These by-products are removed by washing the reaction product with an acid.

[0015] The present inventors have unexpectedly discovered that by at least partially oxidizing the surface of a sodium-containing silicon clathrate, a silicon clathrate active material can be produced that exhibits low expansion upon charging.

[0016] Although not intending to be bound by any theory, the reason for this is believed to be that by oxidizing the surface of the sodium-containing silicon clathrate, the efficiency of removing by-products in the subsequent acid washing is improved, making it easier to maintain voids in the clathrate structure.

[0017] The method for at least partially oxidizing the surface of the sodium-containing silicon clathrate is not particularly limited, but an example thereof is a method in which the silicon clathrate is exposed to the air atmosphere. Specifically, the method includes a method in which the silicon clathrate is placed in an apparatus capable of reducing pressure and replacing gas, and after reducing the pressure inside the apparatus, the air is introduced.

[0018] The sodium-containing silicon clathrate in the method of the present disclosure may at least partially have a clathrate II structure. When the silicon clathrate has a clathrate II structure, the expansion during charging is further reduced.

[0019] The sodium-containing silicon clathrate in the method of the present disclosure may have a porous structure. When the silicon clathrate has a porous structure, the expansion during charging is further reduced.

[0020] <Application> The silicon clathrate active material in the method of the present disclosure can be used as an anode active material in a lithium ion battery.

[0021] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making a silicon clathrate active material by the disclosed method and forming a negative electrode active material layer using the silicon clathrate active material.

[0022] By using the silicon clathrate active material produced by the method of the present disclosure, a battery with small expansion during charging can be obtained.

[0023] For the method for producing the silicon clathrate active material, reference can be made to the above description regarding the method for producing the silicon clathrate active material of the present disclosure.

[0024] The method for forming the negative electrode active material layer is not particularly limited, and a known method can be adopted. For example, a slurry containing a silicon clathrate active material is applied to a negative electrode current collector and dried to obtain a negative electrode active material layer formed on the negative electrode current collector layer.

[0025] The method for forming the battery is not particularly limited, and any known method can be used.

[0026] In addition to producing a silicon clathrate active material and forming a negative electrode active material layer using the silicon clathrate active material, the battery manufacturing method according to the present disclosure may also include forming a solid electrolyte layer, forming a positive electrode active material layer, and arranging a negative electrode current collector layer, a negative electrode active material layer, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer in this order.

[0027] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0028] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0029] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally a solid electrolyte, a conductive assistant, and a binder.

[0030] (Negative electrode active material) The negative electrode active material includes a silicon clathrate active material of the present disclosure.

[0031] (solid electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0032] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li7- x PS6 - x Cl x etc.; or combinations thereof, but are not limited to these.

[0033] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0034] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate active material:mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0035] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0036] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0037] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.

[0038] <Solid electrolyte layer> The solid electrolyte layer includes at least a solid electrolyte. In addition to the solid electrolyte, the solid electrolyte layer may include a binder, etc., as necessary. For the solid electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.

[0039] The thickness of the solid electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0040] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.

[0041] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-yLi-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.

[0042] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.

[0043] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0044] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.

[0045] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0046] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0047] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0048] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred. EXAMPLES

[0049] 《Synthesis of silicon clathrate active material》 Comparative Example 1 Si powder (Kojundo Kagaku, SIEPB32) was prepared as a silicon (Si) source. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and further treated with hydrogen fluoride (HF) to obtain a powder having voids inside the primary particles, i.e., a Si powder having a porous structure.

[0050] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0051] The obtained NaSi alloy and aluminum fluoride (AlF3) were weighed out to a molar ratio of 1:0.35, and the weighed NaSi alloy and AlF3 were mixed with a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 310°C for 60 hours to obtain a reaction product containing sodium-containing silicon clathrate. The obtained reaction product was acid washed using a mixed solvent of HNO3 and H2O in a volume ratio of 90:10 to remove by-products in the reaction product. After washing, it was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a powdered silicon clathrate active material. The obtained material was further washed with a 3 wt% HF solution, filtered, and then dried at 120°C for 3 hours or more to obtain a silicon clathrate active material of Comparative Example 1.

[0052] Example 1 The silicon clathrate active material of Example 1 was obtained in the same manner as in Comparative Example 1, except that before the reaction product was washed with a mixed solvent of HNO3 and HO, it was placed in an apparatus capable of reducing pressure and replacing gas, the pressure inside the apparatus was reduced to room temperature, and then air was introduced to oxidize it.

[0053] 《Making a lithium-ion battery》 Using the silicon clathrate active material of each example, a lithium ion battery was fabricated as follows.

[0054] <Formation of negative electrode active material layer> Butyl butyrate, 5wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, vapor grown carbon fiber (VGCF) as a conductive additive, synthesized silicon clathrate active material, and Li2S-P2S5 glass ceramic as a sulfide solid electrolyte were added to a polypropylene container, and the mixture was stirred for 30 seconds with an ultrasonic dispersing device (UH-50 manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a negative electrode composite slurry.

[0055] The obtained negative electrode composite slurry was applied onto a copper (Cu) foil serving as a negative electrode current collector layer by the blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C to form a negative electrode active material layer on the negative electrode current collector layer.

[0056] <Formation of solid electrolyte layer> Heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li2SP2S5-based glass ceramic as a sulfide solid electrolyte were added to a polypropylene container and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.

[0057] The obtained solid electrolyte slurry was applied onto an aluminum (Al) foil as a release sheet by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100° C. to form a solid electrolyte layer. Three solid electrolyte layers were produced.

[0058] <Formation of Positive Electrode Active Material Layer> A polypropylene container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and VGCF as a conductive additive were added to a container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT).

[0059] Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), further stirred with an ultrasonic dispersing device for 30 seconds, and then shaken for 3 minutes with the shaker to obtain a positive electrode composite slurry.

[0060] The obtained positive electrode mixture slurry was applied onto an Al foil serving as a positive electrode current collector layer by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C, thereby forming a positive electrode active material layer on the positive electrode current collector layer.

[0061] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.

[0062] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.

[0063] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.

[0064] The positive electrode laminate and the negative electrode laminate were laminated on top of each other so that the solid electrolyte layer of each laminate faced the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed at a pressure of 200 MPa and a press temperature of 120° C. for 1 minute, thereby obtaining an all-solid-state battery.

[0065] "evaluation" <Measurement of increase in confining pressure> The fabricated cell was restrained at a predetermined restraining pressure using a restraining jig, and the increase in restraining pressure was measured when the cell was charged at a constant current and constant voltage at a 10-hour rate (1 / 10C) up to 4.55 V. The increase in restraining pressure is the difference between the maximum and minimum restraining pressures, and the value for Example 1 is shown as a relative value when the value for Comparative Example 1 is taken as 1.00.

[0066] "result" The increase in confining pressure for each example of the silicon clathrate active material is shown in Table 1.

[0067] [Table 1]

[0068] As shown in Table 1, the silicon clathrate active material of Example 1 in which the surface of the sodium-containing silicon clathrate was oxidized before the acid washing had a small increase in confining pressure, that is, a small expansion.

Claims

1. A method for producing a silicon clathrate active material, comprising the steps of: at least partially oxidizing the surface of the sodium-containing silicon clathrate; and washing the oxidized sodium-containing silicon clathrate with an acid.

2. 2. The method of claim 1, wherein the surface of the sodium-containing silicon clathrate is at least partially oxidized by exposing the sodium-containing silicon clathrate to an air atmosphere.

3. 2. The method of claim 1, wherein the sodium-containing silicon clathrate has at least a partial clathrate II structure.

4. The method of claim 1 , wherein the sodium-containing silicon clathrate has a porous structure.

5. 10. The method of claim 1, wherein the silicon clathrate active material is for use as an anode active material in a lithium ion battery.

6. Producing a silicon clathrate active material by the method according to any one of claims 1 to 5; and forming a negative electrode active material layer using the silicon clathrate active material; How lithium-ion batteries are manufactured.

Citation Information

Patent Citations

  • METHOD FOR PRODUCING Si CLATHRATE

    JP2012224488A

  • Production method for producing silicon clathrate ii

    JP2021031349A

  • Negative electrode active material including silicon clathrate ii

    JP2021034279A

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158004A

  • Method for manufacturing negative electrode active material

    JP2023043948A