MnBi-BASED MAGNET

By adding or substituting elements like chromium, germanium, or tellurium in MnBi-based magnets, the magnetic properties are enhanced, addressing the limitations of existing MnBi magnets and enabling cost-effective use in various applications.

JP2024153606APending Publication Date: 2024-10-29LG INNOTEK CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024066700
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing MnBi-based magnets have insufficient magnetic properties in the room temperature range, limiting their practical application, and they do not contain rare earth elements, which are expensive.

Method used

The MnBi-based magnets are modified by incorporating elements with atomic radii similar to or smaller than manganese or bismuth, such as chromium, germanium, or tellurium, to reduce the unit cell volume of the low-temperature phase, enhancing saturation magnetization.

Benefits of technology

The modified MnBi-based magnets exhibit higher saturation magnetization and improved magnetic properties at room temperature without the use of rare earth elements, making them cost-effective for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153606000001_ABST
    Figure 2024153606000001_ABST
Patent Text Reader

Abstract

To provide an MnBi-based magnet that can replace neodymium magnets, has high magnetic properties at room temperature, does not contain additional rare earth elements, and can be used as a magnet at low cost.SOLUTION: A MnBi-based magnet according to an embodiment has a composition of (MnBi)aMb, the M element is contained in an amount of more than 0 at% to 10 at% when the total atomic at% of (MnBi)aMb is taken as 100 at%, and the M element includes chromium, germanium, or tellurium. The MnBi magnet according to an embodiment has a composition of (MnBi)aMb, the atomic radius of the M element is smaller than the atomic radius of the manganese or bismuth element, and the difference between the atomic radius of the M element and the atomic radius of the bismuth element is 0.15 Å to 0.36 Å.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The examples relate to MnBi-based magnets. [Background technology]

[0002] The most powerful magnets used industrially are neodymium magnets (Nd-Fe-B). The neodymium magnets are applied to hard disk drives, speakers, mobile phones, automobiles, and robots. The coercive force of the neodymium magnets decreases as the temperature increases. For this reason, dysprosium (Dy) is added to the neodymium magnets. This allows the neodymium magnets to maintain a high coercive force even at high temperatures. However, dysprosium is an expensive substance. For this reason, there is a demand for permanent magnet materials that can replace the neodymium magnets but do not contain rare earth elements.

[0003] MnBi-based magnets are rare earth-free permanent magnet materials that were discovered over 60 years ago. At the time, MnBi-based magnets were not put to practical use due to their insufficient performance as permanent magnets or problems with corrosion resistance.

[0004] More specifically, the maximum energy product (BH)max is an index that represents the magnetic properties of a permanent magnet. The neodymium magnet has a maximum energy product (BH)max of 40 MGOe or more in the room temperature range. However, the coercive force and magnetization of the neodymium magnet decrease with increasing temperature. As a result, the maximum energy product (BH)max of the neodymium magnet decreases by 50% or more at a temperature of about 150°C.

[0005] On the other hand, the MnBi magnet has a unique property that the coercive force increases as the temperature rises. Theoretically, the MnBi magnet has a higher maximum energy product (BH)max than the neodymium magnet at a temperature of about 150°C. The MnBi magnet does not contain rare earth elements, and has recently been attracting renewed attention as a research subject.

[0006] However, theoretically, the MnBi magnet has a maximum energy product (BH)max of 17.7 MGOe in the room temperature range, which is much smaller than the maximum energy product (BH)max of the neodymium magnet. Also, the MnBi magnet has properties such as saturation magnetization, residual magnetization, and coercive force in the room temperature range that are smaller than those of the neodymium magnet.

[0007] Therefore, there is a demand for the MnBi-based magnets that have improved properties even in the normal temperature range.

[0008] Prior art relating to the MnBi-based magnet is disclosed in a Korean patent (KR10-1585478). Summary of the Invention [Problem to be solved by the invention]

[0009] The embodiment provides a MnBi-based magnet having improved magnetic properties in the room temperature range. [Means for solving the problem]

[0010] The MnBi-based magnet according to the embodiment is (MnBi) a M b The M element has a crystal grain having a composition of (MnBi) a M b When the total atomic percentage of is taken as 100 at%, the M element is contained in an amount of more than 0 at% to 10 at%. The M element includes a chromium element, a germanium element, or a tellurium element.

[0011] The MnBi-based magnet according to the embodiment is (MnBi) a M b The atomic radius of the M element is smaller than that of the manganese element or the bismuth element, and the difference between the atomic radius of the M element and the atomic radius of the bismuth element is 0.15 Å to 0.36 Å.

[0012] In addition, when the total atomic at% of the MnBi is taken as 100 at%, the manganese element is contained at 45 at% to 65 at% and the bismuth element is contained at 35 at% to 55 at%, and the at% of the manganese element is greater than the at% of the bismuth element.

[0013] The MnBi-based magnet also contains 40% to 70% by weight of a low temperature phase (LTP).

[0014] The M element includes a chromium element, and the chromium element is contained in an amount of more than 0 at % to 6 at % or less.

[0015] Furthermore, the MnBi magnet has a saturation magnetization of 70 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

[0016] The M element includes a germanium element, and the germanium element is contained in an amount of more than 0 at % to 4 at % or less.

[0017] Furthermore, the MnBi magnet has a saturation magnetization of 70 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

[0018] The M element includes a tellurium element, and the tellurium element is contained in an amount of more than 0 at % and 3 at % or less.

[0019] Furthermore, the MnBi magnet has a saturation magnetization of 69 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

[0020] On the other hand, the embodiment is (MnBi) a M b In the MnBi-based magnet having crystal grains of this composition, the atomic radius of the M element is smaller than the atomic radius of the bismuth element, and the difference between the atomic radius of the M element and the atomic radius of the bismuth element is 0.15 Å to 0.36 Å.

[0021] In addition, the difference between the atomic radius of the M element and the atomic radius of the Mn element is 0.07 Å to 0.11 Å.

[0022] Moreover, the M element is substituted for the bismuth element.

[0023] Moreover, the M element includes a chromium element, a germanium element, or a tellurium element.

[0024] The MnBi-based magnet also contains 40% to 70% by weight of a low temperature phase (LTP).

[0025] The M element is (MnBi) a M b When the total atomic percentage of is 100 at%, it contains more than 0 at% or 10 at%. Effect of the Invention

[0026] The MnBi-based magnet according to the embodiment includes an element that is added to or substituted for the MnBi-based magnet. That is, the MnBi-based magnet is added to or substituted for the MnBi-based magnet (MnBi). a M b is formed.

[0027] The substitution or addition of the M element reduces the volume of the unit cell of the low temperature phase (LTP) which is the main component of the MnBi magnet and has a ferromagnetic phase, thereby increasing the saturation magnetization of the low temperature phase of the MnBi magnet.

[0028] Specifically, the atomic radius of the M element is similar to the atomic radius of the M element or the atomic radius of the bismuth element, and the at% of the M element is included within a set range.

[0029] Therefore, an MnBi magnet in which the MnBi magnet is added with the element M, or an MnBi magnet in which the manganese or bismuth of the MnBi magnet is replaced with the element M, has a low-temperature phase of 40% by weight or more. Also, the MnBi magnet has a higher saturation magnetization than the MnBi magnet in the room temperature range.

[0030] Therefore, the MnBi-based magnet according to the embodiment has high magnetic properties at room temperature. Therefore, the MnBi-based magnet according to the embodiment does not contain any additional rare earth elements and can be used at low cost. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a graph showing the atomic radii of elements for selecting substitution elements or additional elements for an MnBi based magnet according to an embodiment. [Diagram 2] FIG. 2 is a graph showing the magnetization characteristics of an MnBi-based magnet measured by DFT (Density Functional Theory) calculations in order to select substitution elements or additive elements for an MnBi-based magnet according to an embodiment. [Diagram 3] FIG. 3 is a graph showing the energy of formation of an MnBi-based magnet for selecting a substitution element or an additive element for an MnBi-based magnet according to an embodiment. [Figure 4] FIG. 4 is a graph of X-ray diffraction patterns when the amounts of chromium, germanium, and tellurium added to an MnBi magnet are changed. [Diagram 5] FIG. 5 is a graph of X-ray diffraction patterns when the amounts of chromium, germanium, and tellurium added to an MnBi magnet are changed. [Figure 6] FIG. 6 is a graph of X-ray diffraction patterns when the amounts of chromium, germanium, and tellurium added to an MnBi magnet are changed. [Figure 7] FIG. 7 is a graph showing the magnetic properties when the amount of chromium, germanium, and tellurium added to an MnBi magnet is changed. [Figure 8]FIG. 8 is a graph of magnetic properties when the addition amounts of chromium element, germanium element, and tellurium element are changed in the MnBi-based magnet. [Figure 9] FIG. 9 is a graph of magnetic properties when the addition amounts of chromium element, germanium element, and tellurium element are changed in the MnBi-based magnet.

Embodiments for Carrying Out the Invention

[0032] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the technical idea of the present invention is not limited to the described partial embodiments, but can be embodied in various different forms, and within the scope of the technical idea of the present invention, one or more of the components between the embodiments can be selectively combined and replaced for use.

[0033] Also, the terms (including technical and scientific terms) used in the embodiments of the present invention are, unless specifically defined and described, interpreted as having a meaning generally understood by those having ordinary knowledge in the technical field to which the present invention belongs, and terms generally used like those defined in a dictionary can be interpreted considering their meaning in the context of the relevant technology.

[0034] Hereinafter, the MnBi-based magnet according to the embodiment will be described with reference to the drawings.

[0035] <MnBi-based Magnet> The MnBi-based magnet according to the embodiment contains (MnBi) a M b (a and b are positive numbers). Specifically, the MnBi-based magnet is formed by substituting or adding an M element to an MnBi magnet.

[0036] The MnBi magnet may contain 35 at% to 65 at% of manganese and 35 at% to 65 at% of bismuth. More specifically, the MnBi magnet may contain 45 at% to 65 at% of manganese and 35 at% to 55 at% of bismuth. The MnBi magnet may have a manganese at% greater than the bismuth at%. The at% of the manganese and bismuth elements is based on the total atomic at% of MnBi being 100 at%.

[0037] The MnBi magnet can contain a set range of M elements. a M b The MnBi-based magnet having crystal grains with the above composition can contain M element in an amount of more than 0 at% to 10 at% or less. More specifically, the MnBi-based magnet can contain M element in an amount of more than 0 at% to 8 at% or less. More specifically, the MnBi-based magnet can contain M element in an amount of more than 0 at% to 6 at% or less. The at% of M element is (MnBi) a M b The standard is based on the total atomic percentage of 100 at%.

[0038] The MnBi-based magnet may have a low temperature phase in a set weight % range. Specifically, the MnBi-based magnet may have a low temperature phase (LTP) of 40 weight % or more. More specifically, the MnBi-based magnet may have a low temperature phase of 40 weight % to 70 weight %. More specifically, the MnBi-based magnet may have a low temperature phase of 45 weight % to 68 weight %. Here, the weight % of the low temperature phase is based on the weight % of the entire phase of the MnBi-based magnet being 100 weight %.

[0039] The atomic radius of the M element has a set size, and is related to the atomic radius of the Mn element and the atomic radius of the Bi element.

[0040] The atomic radius of the M element is different from the atomic radius of the bismuth element, specifically, the atomic radius of the M element is smaller than the atomic radius of the bismuth element.

[0041] In addition, the atomic radius of the M element is different from the atomic radius of the M element. More specifically, the atomic radius of the M element is smaller than the atomic radius of the M element. Alternatively, the atomic radius of the M element is larger than the atomic radius of the M element.

[0042] Therefore, the atomic radius of the M element may be smaller than the atomic radius of the Mn element and the atomic radius of the B element, or may be between the atomic radius of the Mn element and the atomic radius of the B element.

[0043] The difference between the atomic radius of the M element and the atomic radius of the bismuth element may be 0.1 Å (angstroms) or more. Specifically, the difference between the atomic radius of the M element and the atomic radius of the bismuth element may be 0.1 Å to 0.5 Å. More specifically, the difference between the atomic radius of the M element and the atomic radius of the bismuth element may be 0.1 Å to 0.4 Å. More specifically, the difference between the atomic radius of the M element and the atomic radius of the bismuth element may be 0.15 Å to 0.36 Å.

[0044] In addition, the difference between the atomic radius of the M element and the atomic radius of the manganese element may be 0.2 Å (angstroms) or less. Specifically, the difference between the atomic radius of the M element and the atomic radius of the manganese element may be 0.05 Å to 0.2 Å. More specifically, the difference between the atomic radius of the M element and the atomic radius of the manganese element may be 0.06 Å to 0.15 Å. More specifically, the difference between the atomic radius of the M element and the atomic radius of the manganese element may be 0.07 Å to 0.11 Å.

[0045] Therefore, the atomic radius of the M element can be similar to the atomic radius of at least one of the manganese element and the bismuth element. In particular, the atomic radius of the M element can be similar to the atomic radius of the manganese element and the atomic radius of the bismuth element.

[0046] The MnBi magnet contains a ferromagnetic low-temperature phase as a main component. The crystal structure of the low-temperature phase refers to a NiAs-type crystal structure having crystal grains with a stoichiometric composition of Mn:Bi=1:1.

[0047] The magnetization of the low-temperature phase of the MnBi magnet is calculated by the magnetic moment per unit cell volume. Therefore, when the volume of the unit cell of the crystal structure of the low-temperature phase of the MnBi magnet becomes smaller, the magnetization of the low-temperature phase of the MnBi magnet increases. Alternatively, when the magnetic moment of the low-temperature phase of the MnBi magnet becomes larger, the magnetization of the low-temperature phase of the MnBi magnet increases. Therefore, the magnetic properties of the MnBi magnet are improved.

[0048] When Mn is substituted with Mn, the volume of the unit cell of the crystal structure of the low-temperature phase of the MnBi magnet decreases, and the magnetization of the low-temperature phase of the MnBi magnet increases.

[0049] Alternatively, when the M element, which has an atomic radius smaller than that of the bismuth element, is substituted for the bismuth element, the volume of the unit cell of the crystal structure of the low-temperature phase of the MnBi magnet becomes smaller, thereby increasing the magnetization of the low-temperature phase of the MnBi magnet.

[0050] In the MnBi magnet according to the embodiment, the M element having an atomic radius smaller than that of the Mn element is substituted for the Mn atom. This reduces the volume of the unit lattice of the crystal structure of the low-temperature phase of the MnBi magnet. This increases the magnetization of the low-temperature phase of the MnBi magnet.

[0051] Alternatively, in the MnBi-based magnet according to the embodiment, an M element having an atomic radius smaller than that of the bismuth element replaces the bismuth atom. Thereby, the volume of the unit cell of the unit crystal of the low-temperature phase of the MnBi-based magnet becomes smaller. Thereby, the magnetization of the low-temperature phase of the MnBi-based magnet can be increased.

[0052] The M element is selected by the method for determining the substitution element or the addition element described below. For example, the M element can have an atomic radius smaller than the atomic radius of the manganese and the atomic radius of the bismuth. As an example, the M element includes a chromium element (Cr) and a germanium element (Ge).

[0053] Alternatively, the M element can have an atomic radius larger than the atomic radius of the manganese and smaller than the atomic radius of the bismuth. As an example, the M element includes a tellurium element (Te).

[0054] The chromium element (Cr), the germanium element (Ge), and the tellurium element (Te) can be replaced with at least one of the manganese element and the bismuth element.

[0055] Thus, the MnBi-based magnet having crystal grains of the composition of (MnBi) a M b can have crystal grains of the composition in which the added M element replaces the manganese element or the bismuth element and the low-temperature phase is Mn 1-x BiM x or MnBi 1-x M x Also, a, b, and x are positive numbers, and a > b is satisfied. Also, the M element can be replaced with at least one of the manganese element and the bismuth element. The M element includes a chromium element (Cr), a germanium element (Ge), or a tellurium element (Te).

[0056] <Determination of Substitution Element or Addition Element of MnBi-Based Magnet> The M element, which is a substitution element or additive element of the MnBi-based magnet, is determined by the atomic radius of the element, the magnetization characteristics of the MnBi-based magnet measured by DFT (Density Functional Theory) calculations, and the formation energy of the MnBi-based magnet.

[0057] FIG. 1 is a graph of atomic radii of elements for selecting the M element.

[0058] The atomic radius of the bismuth element is larger than the atomic radius of the manganese element.

[0059] Therefore, elements with an atomic radius larger than that of the bismuth element are excluded from the candidate group. In addition, elements with atomic radii similar to those of the bismuth element and the manganese element are selected as the candidate group. More specifically, elements with an atomic radius difference of 0.15 Å to 0.36 Å from that of the bismuth element are selected as the first candidate group elements. In addition, elements with an atomic radius difference of 0.07 Å to 0.11 Å from that of the manganese element are selected as the first candidate group elements.

[0060] Next, a second candidate group of elements, which are the final candidate group of elements, is selected from the first candidate group of elements based on the magnetization characteristics of the MnBi-based magnet measured by DFT (Density Functional Theory) calculations and the generation energy of the MnBi-based magnet.

[0061] Fig. 2 is a graph showing the magnetization characteristics of the MnBi magnet measured by DFT (Density Functional Theory) calculations when the MnBi magnet is replaced with the first candidate group elements, and Fig. 3 is a graph showing the formation energy of the MnBi magnet when the MnBi magnet is replaced with the first candidate group elements.

[0062] 2 and 3, ◯ indicates the magnetization characteristics and formation energies when the first candidate group elements are substituted with manganese, and □ indicates the magnetization characteristics and formation energies when the first candidate group elements are substituted with bismuth.

[0063] Referring to FIG. 2, the magnetization characteristics of MnBi-based magnets in which lithium (Li), magnesium (Mg), gallium (Ga), germanium (Ge), selenium (Se), silver (Ag), and tellurium (Te) are substituted for bismuth are greater than those of MnBi magnets.

[0064] Furthermore, the magnetization characteristics of MnBi-based magnets in which aluminum (Al), indium (In), and tin (Sn) are substituted for bismuth are smaller than those of MnBi magnets.

[0065] In addition, the magnetic properties of MnBi-based magnets in which vanadium (V), chromium (Cr), iron (Fe), cobalt (Co), gallium (Ga), molybdenum (Mo), palladium (Pd), and silver (Ag) are substituted for manganese are smaller than those of MnBi magnets.

[0066] Referring to FIG. 3, the formation energy of MnBi-based magnets in which lithium (Li), magnesium (Mg), aluminum (Al), gallium (Ga), silver (Ag), and indium (In) are substituted for bismuth is greater than the formation energy of MnBi magnets.

[0067] In addition, the formation energy of MnBi-based magnets in which germanium (Ge), selenium (Se), tin (Sn), and tellurium (Te) are substituted for bismuth is smaller than the formation energy of MnBi magnets.

[0068] In addition, the formation energy of MnBi-based magnets in which vanadium (V), chromium (Cr), iron (Fe), cobalt (Co), gallium (Ga), molybdenum (Mo), and silver (Ag) are substituted for manganese is greater than the formation energy of MnBi magnets.

[0069] Furthermore, the formation energy of an MnBi-based magnet, in which palladium (Pd) is replaced with manganese, is smaller than that of an MnBi magnet.

[0070] With reference to FIGS. 1 to 3, germanium element (Ge), tellurium element (Te), and chromium element (Cr) are selected as the second candidate group elements that are the final candidate group elements.

[0071] When the germanium element (Ge) and the tellurium element (Te) are substituted for the bismuth element, the magnetization characteristics of the MnBi-based magnet are high and the generation energy is small, so they are selected as the second candidate group elements.

[0072] When the chromium element (Cr) is substituted for the manganese element, the magnetization characteristics of the MnBi-based magnet are low and the generation energy is large. However, since the atomic radius of the chromium element (Cr) is smaller than the atomic radius of the germanium element (Ge) and the atomic radius of the tellurium element (Te), it is selected as the second candidate group element.

[0073] Since the lithium element (Li), the gallium element (Ga), and the silver element (Ag) have a large generation energy for the MnBi-based magnet, they are excluded from the second candidate group elements.

[0074] Since the selenium element (Se) is toxic, it is excluded from the second candidate group elements.

[0075] Since the magnesium element (Mg) has a high generation energy, it is excluded from the second candidate group elements.

[0076] <Experimental Example of MnBi-based Magnet> The saturation magnetization of the MnBi-based magnet in which the element selected as the second candidate group element is substituted for the MnBi magnet was calculated.

[0077] <Experimental Example 1> Mn, Bi, and Cr were used as raw materials and mixed. Subsequently, the mixture was put into a ceramic crucible, heated and melted at a temperature of about 1200° C. in an Ar atmosphere, and then the molten metal was transferred to a metal mold to obtain an ingot. The ingot was annealed and homogenized at a temperature range of 280° C. to 320° C. for 48 hours. Subsequently, the annealed ingot was pulverized into powder.

[0078] The powder was measured with an X-ray diffractometer (Rigaku, Smart-lab). Figure 4 shows the X-ray diffraction pattern when chromium element was added. It can be confirmed from the X-ray diffraction pattern that the manufactured MnBi-based magnet contains a Bi phase and a small amount of Mn phase in addition to the low-temperature phase that exhibits ferromagnetism. The weight ratio of the low-temperature phase, which is a magnetic phase, was calculated by Rietveld analysis of the X-ray diffraction pattern. In addition, the lattice volume of the low-temperature phase was calculated from the lattice constant of the low-temperature phase obtained from the Rietveld analysis. In addition, the magnetization of the powder was measured with a SQUID (Quantum Design, Magnetic Property Measurement System). Figure 7 shows the magnetic measurement results when chromium element was added. At this time, the magnetization in a magnetic field (5T) was used as the actual value of saturation magnetization, and in order to eliminate the difference in saturation magnetization due to the difference in the ratio of the low-temperature phase, the saturation magnetization was calculated by multiplying the actual saturation magnetization value by the reciprocal of the low-temperature phase ratio and converting it to 100 wt% low-temperature phase. Table 1 shows the low-temperature phase weight ratio, lattice volume and saturation magnetization of each composition. It can be confirmed that the saturation magnetization of the composition to which chromium element is added up to 6 at% is improved compared to MnBi. It can also be confirmed that the lattice volume of the low-temperature phase of the composition to which chromium element is added up to 6 at% is smaller than that of MnBi. The atomic radii of manganese, bismuth and chromium elements are 1.35A, 1.60A and 1.25A, respectively. As a result of substituting chromium element with either manganese element or bismuth element, the lattice volume becomes smaller, and it is presumed that the saturation magnetization improves due to the effect of reducing the lattice volume. When the amount of addition is 7 at% or more, the lattice volume becomes larger than MnBi and the saturation magnetization turns to a decrease, so that the amount of chromium element is preferably 6 at% or less.

[0079] <Experimental Example 2> A powder was produced in the same manner as in Experimental Example 1, except that Mn, Bi, and Ge were used and mixed as raw materials. The saturation magnetization and lattice volume of the powder were then calculated. Figures 5 and 8 show the X-ray diffraction pattern and magnetic measurement results when germanium element was added. It can be confirmed that the lattice volume of the low-temperature phase of the composition to which germanium element was added up to 4 at% is smaller than the lattice volume of the low-temperature phase of MnBi, and the saturation magnetization is improved. The atomic radii of manganese, bismuth, and germanium elements are 1.35A, 1.60A, and 1.24A, respectively. It is presumed that the lattice volume is reduced as a result of replacing germanium element with one of manganese element and bismuth element, and the saturation magnetization is improved due to the effect of reducing the lattice volume. When the amount of germanium added is 5 at% or more, the lattice volume becomes larger than that of MnBi, and the saturation magnetization is converted to a decrease, so that the germanium element is preferably 4 at% or less.

[0080] <Experimental Example 3> A powder was produced in the same manner as in Experimental Example 1, except that Mn, Bi and Te were used and mixed as raw materials. The saturation magnetization and lattice volume of the powder were then calculated. Figures 6 and 9 show the X-ray diffraction pattern and magnetic measurement results when tellurium element was added. It can be confirmed that the lattice volume of the low-temperature phase of the composition with tellurium element added up to 3 at% is smaller than that of the low-temperature phase of MnBi, and the saturation magnetization is improved. The atomic radii of manganese, bismuth and tellurium elements are 1.35A, 1.60A and 1.45A, respectively. It is presumed that the lattice volume is reduced as a result of tellurium element replacing bismuth element, and the saturation magnetization is improved due to the effect of reducing the lattice volume. When the amount of tellurium added is 4 at% or more, the lattice volume becomes larger than that of MnBi, and the saturation magnetization is converted to a decrease, so that the amount of tellurium element is preferably 3 at% or less.

[0081] <Experimental Example 4> Except for using and mixing Mn and Bi as raw materials, powder was produced in the same manner as in Experimental Example 1. Then, the saturation magnetization and lattice volume of the powder were calculated.

[0082] [Table 1] Table 1 shows the weight percentage of the low temperature phase (LTP) and saturation magnetization of an MnBi magnet according to the atomic percentage of the substituting or added element when chromium (Cr), germanium (Ge), or tellurium (Te) is added to the MnBi magnet.

[0083] Referring to Table 1, it can be seen that when chromium (Cr), germanium (Ge) or tellurium (Te) is substituted or added to the MnBi magnet, it has improved saturation magnetization compared to the MnBi magnet.

[0084] MnBi magnets mainly contain a low-temperature phase that exhibits ferromagnetism. The low-temperature phase can mean crystal grains with a stoichiometric composition of Mn:Bi=1:1. For example, it has a NiAs-type crystal structure. When a different element is added to an MnBi magnet, the different element may replace the manganese element or the bismuth element in the low-temperature phase crystal structure, or the different element may invade the crystal structure. Here, since the atomic radius of the added element M is relatively close to the atomic radius of the manganese element and the bismuth element, it is presumed that the added element M is highly likely to be replaced. In the embodiment, it is presumed that the manganese element or the bismuth element that constitutes the low-temperature phase may have been replaced by the added element M, and a change has occurred in the lattice volume, so that the saturation magnetization of the low-temperature phase of the MnBi magnet has changed.

[0085] For example, manganese or bismuth is replaced by chromium (Cr) to form Mn 1-x BiCr x (x is any number) or MnBi 1-x Cr x A low-temperature phase crystal structure of a MnBi-based magnet having a composition (x is an arbitrary number) is formed. (MnBi) having the above crystal structure a Cr b The low temperature phase of the magnet has improved saturation magnetization compared to the low temperature phase of MnBi magnets. a Cr bWhen the chromium element is contained in a magnet between 0 at% and 6 at% or less, the above (MnBi) a Cr b has a low temperature phase of 40% by weight or more, and has improved saturation magnetization compared to the low temperature phase of MnBi magnet. a Cr b The low-temperature phase of the magnet has a saturation magnetization of 70 emu / g or more in the normal temperature range (300K). a Cr b The low-temperature phase of the magnet has a saturation magnetization of 70 emu / g to 80 emu / g at room temperature (300K). Here, the at% of chromium is (MnBi) a Cr b The total at% is taken as 100 at%.

[0086] Or, the manganese or bismuth element is replaced by germanium (Ge) to form Mn 1-x BiGe x (x is any number) or MnBi 1-x Ge x A low-temperature phase crystal structure of a MnBi-based magnet having a composition (x is an arbitrary number) is formed. (MnBi) having the above crystal structure a Ge b The low temperature phase of the magnet has improved saturation magnetization compared to the low temperature phase of MnBi magnets. a Ge b When the germanium element is contained in a magnet in an amount of more than 0 at% or less than 4 at% (MnBi) a Ge b has a low temperature phase of 60% by weight or more, and has improved saturation magnetization compared to the low temperature phase of MnBi magnet. a Ge b The magnet has a saturation magnetization of 70 emu / g or more at room temperature (300K). a Ge b The magnet has a saturation magnetization of 70 emu / g to 80 emu / g at room temperature (300K). Here, the at% of germanium is (MnBi) a Ge bThe total at% is taken as 100 at%.

[0087] Or, the element bismuth is replaced with the element tellurium (Te) to form MnBi 1-x Te x A low-temperature phase crystal structure of a MnBi-based magnet having a composition (x is an arbitrary number) is formed. (MnBi) having the above crystal structure a Te b The low temperature phase of the magnet has improved saturation magnetization compared to the low temperature phase of MnBi magnets. a Te b When the tellurium element is contained in a magnet in an amount of more than 0 at% or less than 3 at% (MnBi) a Te b has a low temperature phase of 60% by weight or more, and has improved saturation magnetization compared to the low temperature phase of MnBi magnet. a Te b The magnet has a saturation magnetization of 69 emu / g or more at room temperature (300K). a Te b The magnet has a saturation magnetization of 69 emu / g to 80 emu / g at room temperature (300K). Here, the at% of tellurium is (MnBi) a Te b The total at% is taken as 100 at%.

[0088] The MnBi magnet according to the embodiment contains an element that can replace the manganese or bismuth element of the MnBi magnet. That is, the low-temperature phase crystal structure of the MnBi magnet contains Mn, which is substituted for the M element. 1-x BiM x (x is any number) or MnBi 1-x M x (x is an arbitrary number) has a low-temperature phase crystal structure with the composition (MnBi) a M b is formed.

[0089] The substitution of the M element reduces the volume of the unit cell of the low temperature phase of the MnBi magnet, thereby increasing the magnetization of the MnBi magnet.

[0090] Specifically, the atomic radius of the M element is similar to the atomic radius of the M element or the atomic radius of the bismuth element, and the at% of the M element is included within a set range.

[0091] Therefore, the MnBi magnet in which the manganese or bismuth element is replaced with the M element or to which the manganese or bismuth element is added has a low temperature phase of 40% by weight or more. Also, the low temperature phase of the MnBi magnet has a higher saturation magnetization than the low temperature phase of the MnBi magnet in the room temperature range. Therefore, the MnBi magnet has a saturation magnetization of 69 emu / g or more at room temperature.

[0092] Therefore, the MnBi-based magnet according to the embodiment has high magnetic properties at room temperature. Therefore, the MnBi-based magnet according to the embodiment does not contain any additional rare earth elements and can be used at low cost.

[0093] Therefore, due to their excellent magnetic properties, the MnBi-based magnets according to the embodiments can be used in motors for refrigerators and air conditioner compressors, washing machine drive motors, vibration motors for mobile handsets, speakers, voice coil motors, linear motors for determining the position of computer hard disk heads, camera zooms, apertures, shutters, actuators for micromachining machines, automotive electrical components such as DCT (Dual Clutch Transmission), ABS (Anti-lock Brake System), EPS (Electric Power Steering) motors, and fuel pumps.

[0094] The features, structures, effects, etc. described in the above-mentioned embodiments are included in at least one embodiment of the present invention, and are not necessarily limited to one embodiment. In addition, the features, structures, effects, etc. exemplified in each embodiment can be combined or modified in other embodiments by a person having ordinary skill in the art to which the embodiment belongs. Therefore, the contents related to such combinations and modifications should be interpreted as being included in the scope of the present invention.

[0095] In addition, the above description has been centered on the embodiments, but these are merely examples and do not limit the present invention. A person having ordinary skill in the art to which the present invention pertains may make various modifications and applications not exemplified above within the scope of the essential characteristics of the present embodiments. For example, each component specifically presented in the embodiments may be modified and implemented. The differences related to such modifications and applications should be interpreted as being included in the scope of the present invention defined in the appended claims.

Claims

1. (MnBi) a M b As an MnBi-based magnet having crystal grains with the composition The M element is (MnBi) a M b When the total atomic at% of the element is taken as 100 at%, it contains more than 0 at% to 10 at%. The MnBi-based magnet includes a chromium element, a germanium element, or a tellurium element.

2. When the total atomic at% of the MnBi is taken as 100 at%, The manganese element in the MnBi is contained in an amount of 45 at% to 65 at%; The bismuth element in the MnBi is contained in an amount of 35 at % to 55 at %; 2. The MnBi system magnet according to claim 1, wherein the at% of said manganese element is greater than the at% of said bismuth element.

3. 2. The MnBi-based magnet according to claim 1, wherein the MnBi-based magnet contains 40% to 70% by weight of a low temperature phase (LTP).

4. The M element includes a chromium element, 2. The MnBi system magnet according to claim 1, wherein the chromium element is contained in an amount of more than 0 at % and not more than 6 at %.

5. 5. The MnBi system magnet according to claim 4, wherein the MnBi system magnet has a saturation magnetization of 70 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

6. The M element includes a germanium element, 2. The MnBi based magnet according to claim 1, wherein the germanium element is contained in an amount of more than 0 at % and less than or equal to 4 at %.

7. 7. The MnBi system magnet according to claim 6, wherein the MnBi system magnet has a saturation magnetization of 70 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

8. The M element includes a tellurium element, 2. The MnBi based magnet according to claim 1, wherein the tellurium element is contained in an amount of more than 0 at % and not more than 3 at %.

9. 9. The MnBi system magnet according to claim 8, wherein the MnBi system magnet has a saturation magnetization of 69 emu / g to 80 emu / g at a temperature of 300K when the low temperature phase is converted to 100% by weight.

10. (MnBi) a M b As an MnBi-based magnet having crystal grains with the composition the atomic radius of the M element is smaller than the atomic radius of the bismuth element, A MnBi-based magnet, wherein the difference between the atomic radius of the M element and the atomic radius of the bismuth element is 0.15 Å to 0.36 Å.

11. 11. The MnBi-based magnet according to claim 10, wherein the difference between the atomic radius of the M element and the atomic radius of the manganese element is 0.07 Å to 0.11 Å.

12. The MnBi based magnet according to claim 10 , wherein the M element is substituted for the bismuth element.

13. The MnBi-based magnet according to claim 10 , wherein the M element includes a chromium element, a germanium element, or a tellurium element.

14. The MnBi-based magnet according to claim 10, wherein the MnBi-based magnet comprises 40% to 70% by weight of a Low Temperature Phase (LTP).

15. The M element is (MnBi) a M b 11. The MnBi system magnet according to claim 10, wherein the content of said MnBi is more than 0 at % and 10 at %, where the total atomic at % is taken as 100 at %.

Citation Information

Cited By

  • Tire-wheel assembly, tire, and wireless power receiving system

    US12420598B2