Method for deactivating nonlinear optical crystal

Hydrogen passivation and annealing methods enhance NLO crystal resistance to laser-induced damage, addressing material defects and extending device lifetime by repairing defects and reducing moisture content.

JP2024153787AActive Publication Date: 2024-10-29KLA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024122326
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2012-06-05
Filing Date
2024-07-29
Publication Date
2024-10-29
Estimated Expiration
2032-10-05

AI Technical Summary

Technical Problem

Laser-induced damage (LID) in nonlinear optical (NLO) devices, particularly those using shorter wavelengths, is exacerbated by material defects, leading to degradation of physical properties and reduced lifetime.

Method used

Utilizing hydrogen molecules or atoms to passivate crystal defects in NLO crystals through exposure to controlled hydrogen concentrations and temperatures, combined with annealing processes to reduce water and OH content, enhancing resistance to LID.

Benefits of technology

Improves the resistance of NLO devices to laser-induced damage, extending their lifetime and maintaining optimal physical properties by repairing defects and reducing moisture content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153787000001_ABST
    Figure 2024153787000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a system for optically inspecting one or more samples.SOLUTION: A laser system 400 comprises: NLO crystal 104 that is annealed within a selected temperature range and deactivated to a selected deactivation level with at least one of hydrogen, heavy hydrogen, a hydrogen-containing mixture, and a heavy hydrogen-containing mixture; at least one light source 402 configured to generate light with a selected wavelength and transmit the light through the NLO crystal 104; and a housing unit 406 configured to accommodate the NLO crystal 104.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application is related to the application(s) identified below ("Related Applications") and claims the benefit of the earliest available effective filing date(s) of those applications (e.g., claims the earliest available priority date other than a provisional patent application, or claims the benefit under 35 USC § 119 of a provisional patent application to any and all parent, grandfather, great-grandfather, etc. applications of the Related Applications).

[0002] For purposes of non-statutory requirements of the United States Patent and Trademark Office (USPTO), this application constitutes a regular (non-provisional) patent application of U.S. Provisional Patent Application No. 61 / 544,425, entitled NLO CRYSTAL PROPERTIES BY HYDROGEN PASSIVATION, filed on October 7, 2011, by Yung-Ho Chuang and Vladimir Dribinski as inventors.

[0003] The present invention relates to the field of nonlinear optical materials, and more particularly to a system and method for passivating nonlinear optical crystals to cure crystal defects. [Background technology]

[0004] Many modern laser systems require nonlinear optical (NLO) elements, which are commonly used in applications such as frequency mixing (e.g., harmonic generation, parametric oscillation / amplification, etc.), Raman amplification, Kerr lens mode-locking, electro-optic modulation, acousto-optic modulation, and others. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] U.S. Patent No. 6,667,828 [Patent Document 2] U.S. Patent Application Publication No. 2002 / 0109110 Summary of the Invention [Problem to be solved by the invention]

[0006] Laser-induced damage (LID) of NLO elements is a major limitation of many modern laser systems. LID occurs as a result of the interaction between the laser beam and the materials that make up a given NLO element. As a result, NLO elements suffer from LID over time, which can negatively affect physical properties such as transmittance, reflectance, and refractive index. In turn, this degradation of physical properties due to the occurrence of LID can ultimately lead to failure of NLO elements within a laser system.

[0007] LID is even more of a problem in laser systems that utilize shorter wavelengths of the electromagnetic spectrum, such as deep ultraviolet (DUV) light, with wavelengths less than 300 nm. Additionally, laser-induced damage rates are also affected by material defects present in the NLO elements, such as dislocations, impurities, vacancies, etc. In most cases, material defects in a given NLO element make the NLO element less resistant to LID. Thus, the NLO element has a shorter lifetime as a result of the material defects.

[0008] The present invention is directed to alleviating the above problems by improving the damage resistance of NLO elements utilizing the novel systems and methods disclosed herein. [Means for solving the problem]

[0009] Systems and methods are disclosed for repairing crystal defects in one or more nonlinear optical (NLO) crystals to improve performance or increase resistance to laser-induced damage. In one aspect, a system is provided for increasing the resistance of one or more nonlinear optical (NLO) crystals to laser-induced damage by utilizing hydrogen molecules or hydrogen atoms to passivate crystal defects, the system may include an exposure chamber configured to contain a passivation gas having a hydrogen concentration at or near a selected hydrogen concentration, the chamber further configured to contain at least one NLO crystal exposed to the passivation gas inside the chamber, a passivation gas source fluidly connected to the exposure chamber, the passivation gas source configured to supply a passivation gas inside the exposure chamber, and a substrate configured to hold the NLO crystal inside the chamber, the substrate further configured to maintain a temperature of the NLO crystal at or near a selected temperature, the selected temperature being a melting temperature of the NLO crystal.

[0010] In another aspect, a method is provided for increasing the resistance of an NLO crystal to laser-induced damage by utilizing hydrogen to passivate crystal defects, the method may include (i) maintaining a temperature of the NLO crystal at or near a selected temperature, where the selected temperature is below a melting temperature of the NLO crystal, and (ii) exposing the NLO crystal to a passivation gas having a selected hydrogen concentration at or near the selected hydrogen concentration.

[0011] In another aspect, a method is provided for increasing the resistance of a nonlinear optical (NLO) crystal to laser-induced damage by utilizing hydrogen molecules or atoms to passivate crystal defects, the method may include (i) performing an annealing process on the NLO crystal to reduce the moisture content or OH content of the NLO crystal, and (ii) exposing the NLO crystal to a passivation gas having a hydrogen concentration at or near a selected hydrogen concentration.

[0012] In another aspect, a system for optically inspecting one or more samples is provided, the system may include a sample stage; a laser system configured to illuminate a portion of a surface of one or more samples placed on the sample stage, the laser system including at least one passivated and annealed NLO crystal, the NLO crystal being annealed sufficiently to establish a moisture content below a selected level, the NLO crystal being further passivated sufficiently to establish a selected passivation level; at least one light source configured to generate light of a selected wavelength, the light source further configured to transmit light through the NLO crystal; and a crystal housing unit configured to house the NLO crystal; a detector configured to receive at least a portion of the illumination reflected from the surface of the sample; and a computing system communicatively coupled to the detector, the computing system configured to obtain information regarding at least a portion of the illumination received by the detector, the computing system further configured to utilize the information regarding at least a portion of the illumination received by the detector to determine the presence or absence of at least one defect in the sample.

[0013] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and do not necessarily restrict the invention as claimed. The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments of the invention and, together with the general description, serve to explain the principles of the invention.

[0014] Many advantages of the present disclosure can be better understood by those skilled in the art by reference to the following drawings. [Brief description of the drawings]

[0015] [Figure 1A] 1 is a block diagram illustrating a system for passivating an NLO crystal, in accordance with one embodiment of the present invention. [Figure 1B]1 is a schematic diagram of an exposure chamber of a system for passivating NLO crystals, in accordance with one embodiment of the present invention. [Figure 2A] 1 is a flow diagram illustrating a method for passivating an NLO crystal in accordance with one embodiment of the present invention. [Figure 2B] 1 is a flow diagram illustrating a method for passivating an NLO crystal in accordance with one embodiment of the present invention. [Figure 2C] 1 is a flow diagram illustrating a method for passivating an NLO crystal in accordance with one embodiment of the present invention. [Figure 2D] 1 is a flow diagram illustrating a method for passivating an NLO crystal in accordance with one embodiment of the present invention. [Figure 3A] 1 is a flow diagram illustrating a method for annealing and passivating an NLO crystal in accordance with one embodiment of the present invention. [Figure 3B] 1 is a flow diagram of a method for annealing and passivating an NLO crystal, in accordance with one embodiment of the present invention. [Figure 3C] 1 is a flow diagram of a method for annealing and passivating an NLO crystal, in accordance with one embodiment of the present invention. [Figure 3D] 1 is a flow diagram of a method for annealing and passivating an NLO crystal, in accordance with one embodiment of the present invention. [Figure 4] FIG. 1 is a block diagram illustrating a laser system including an annealed and passivated NLO crystal in accordance with one embodiment of the present invention. [Diagram 5] 1 is a block diagram illustrating a system for inspecting a wafer or photomask in accordance with one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Reference will now be made in detail to the disclosed subject matter, which is illustrated in the accompanying drawings.

[0017] 1A-5, systems and methods for passivating nonlinear optical (NLO) crystals are described in accordance with the present disclosure. Laser systems typically utilize NLO crystals for many applications, such as frequency mixing, Raman amplification, Kerr lens mode locking, electro-optic modulation, acousto-optic modulation, among others. Exposure to electromagnetic radiation within a laser system affects the physical properties (e.g., transmittance, reflectance, refractive index, etc.) of the NLO crystal. The resulting changes to the physical properties of the NLO crystal, typically referred to as laser-induced damage (LID), tend to prevent the NLO crystal from functioning properly. NLO crystals are less resistant to LID when they have a large or large amount of crystal defects, such as dislocations, impurities, vacancies, etc. The present invention is directed to systems and methods for repairing NLO crystal defects utilizing hydrogen activation and / or crystal annealing.

[0018] As used throughout this disclosure, the terms "crystal", "NLO crystal" or "nonlinear crystal" generally refer to nonlinear optical crystals suitable for frequency conversion. For example, the nonlinear optical crystals of the present invention may be configured to frequency convert incident illumination at a first wavelength (e.g., 532 nm) to output illumination at a shorter wavelength (e.g., 266 nm). Furthermore, the nonlinear optical crystals of the present invention may include, but are not limited to, beta-type barium borate (BBO), lithium triborate (LBO), lithium tetraborate (LTB), lithium cesium borate (CLBO), cesium borate (CBO), oxide-type nonlinear crystals, and the like.

[0019] As used throughout this disclosure, the term "wafer" generally refers to a substrate formed from a semiconductor or non-semiconductor material. For example, semiconductor or non-semiconductor materials include, but are not limited to, monocrystalline silicon, gallium arsenide, and indium phosphide. A wafer may include one or more layers. For example, such layers may include, but are not limited to, resist, dielectric materials, conductive materials, and semiconductor materials. Many different types of such layers are known in the art, and the term wafer as used herein is intended to encompass wafers upon which all types of such layers may be formed.

[0020] 1A and 1B show a system 100 for passivating an NLO crystal 104 to repair crystal defects within the crystal. These defects may be repaired by attaching hydrogen atoms to dangling bonds or broken chemical bonds within the crystal 104. For example, the dangling bonds or broken chemical bonds may include oxygen dangling bonds, which are often the primary type of defect that affects the NLO crystal lifetime as well as physical / optical properties. In one embodiment, the system 100 may include an exposure chamber 101 configured to contain a volume of a passivation gas. The exposure chamber 101 may be further configured to contain the NLO crystal 104 such that the NLO crystal 104 may be exposed to the passivation gas contained within the exposure chamber 101. The exposure chamber 101 may also be further configured to include a substrate 102 configured to hold the NLO crystal 104 while the NLO crystal 104 is exposed to the passivation gas contained within the exposure chamber 101. Alternatively, the substrate 102 may be a portion of the interior surface of the chamber 101.

[0021] The inert gas of the present invention may include two or more gaseous mixtures having a selected hydrogen concentration. In one embodiment, the gas mixture may include molecular hydrogen (H2). In another embodiment, the inert gas may include a low molecular weight gas that may generate hydrogen during a chemical reaction or upon decomposition. Such low molecular weight gases may include, but are not limited to, NH3 or CH4. The desired hydrogen concentration may include a concentration that exceeds the natural abundance of hydrogen present under normal atmospheric conditions. In this regard, the hydrogen concentration of the inert gas may comprise a concentration that exceeds the hydrogen concentration naturally present in air. In another aspect, the desired concentration of hydrogen may be a concentration selected by a user or a concentration determined utilizing one or more physical attributes of the NLO crystal 104. The inert gas mixture may further include an inert gas, such as argon, nitrogen, helium, etc.

[0022] In additional embodiments, the passivation gas of the present invention may include a gas mixture having a hydrogen concentration in the range of 5-10%. It is noted herein that this hydrogen concentration range is presented merely for illustration and not limitation. It is contemplated that the hydrogen concentration level of the passivation gas may include any range appropriate for a given application. In additional embodiments, the hydrogen concentration of the passivation gas mixture may include a heavy isotope of hydrogen, deuterium, to improve the passivation results. The exact amount of deuterium in the mixture may be determined by optimizing the passivation results and may range from a portion of the total hydrogen coverage to 100% of the total hydrogen in the mixture.

[0023] In one embodiment, the system may further include an inerting gas source 108 fluidly coupled to the exposure chamber 101 and configured to supply an inerting gas to the exposure chamber. The exposure chamber 101 may include a gas inlet port 105 configured to receive the inerting gas from the inerting gas source 108 and further configured to transfer the inerting gas received from the inerting gas source 108 to the interior of the exposure chamber 101. The exposure chamber 101 may further include a gas outlet port 106 configured to release the inerting gas from the interior of the exposure chamber 101.

[0024] In an additional embodiment, the system 100 may include a flow controller 110 fluidly connected between the inerting gas source 108 and the exposure chamber 101. The flow controller 110 may be configured to control the rate at which the inerting gas is supplied to the exposure chamber 101. The flow controller 110 may include a valve, regulator, or other means for regulating the pressure or rate at which the inerting gas passes through at least one conduit fluidly connecting the flow controller 110 to the exposure chamber 101. The flow controller may be further configured to be fluidly connected to the gas inlet port 105 of the exposure chamber and further configured to control the rate at which the inerting gas is supplied to the interior of the exposure chamber 101 through the gas inlet port 105. In another embodiment, the flow controller 110 or an additional flow controller (not shown) may be configured to be fluidly connected to the gas outlet port 106 of the exposure chamber 101 and further configured to control the rate at which the inerting gas is removed from the interior of the exposure chamber 101.

[0025] In another embodiment, the system 100 may further include one or more computing systems 112 communicatively coupled to the flow controller 110. The computing system 112 may be configured to provide instructions to the flow controller 110 to control the rate at which the inerting gas is supplied to the exposure chamber 101. The computing system 112 may be further configured to provide instructions to the flow controller 110 or additional flow controllers (not shown) to control the rate at which the inerting gas is removed from the exposure chamber 101. The computing system may include a carrier medium 114, such as a flash memory device, solid state storage device, optical storage device, random access memory device, or other static or dynamic storage device, configured with program instructions 116 including a flow control algorithm 118. The flow control algorithm 118, such as an algorithm for configuring a pressure valve, may be included in the flow controller 110, and is known to the art. For example, the flow control algorithm 118 may instruct the flow controller 110 to operate a pressure valve based on a correlation between a mechanical property of the pressure valve and a desired flow rate. In some embodiments, the flow control algorithm 118 may be configured ... 3 A user-selected flow rate of 1000 cm / min may be the desired flow rate for passivating the NLO crystal 104 contained within the exposure chamber 101. However, depending on the composition of the passivation gas mixture or the NLO crystal 104, a flow rate of 10-200 cm / min may be used. 3 Flow rates other than 100 / min may be desired. The above flow rate ranges are exemplary only and are not intended to limit the invention in any way.

[0026] In additional embodiments, the substrate 102 configured to hold the NLO crystal 104 inside the exposure chamber 101 may be further configured to control the temperature of the NLO crystal 104. In one aspect, a user may select a temperature that is higher than ambient or room temperature, but below the melting temperature of the NLO crystal 104. For example, the substrate 102 may be configured to heat the NLO crystal to a range of 300-350° C. or some other selected temperature to improve hydrogen permeation into the crystal interior, reduce decomposition of molecular hydrogen (e.g., H2) or other hydrogen-containing molecules into atomic hydrogen, or eliminate undesirable reaction products between hydrogen and the NLO crystal (e.g., weak OH bonds, water, etc.). It is contemplated herein that the substrate 102 may be configured to increase, decrease, and / or maintain the temperature of the NLO crystal 104 at any feasible temperature or range of temperatures desired for successful passivation of the NLO crystal 104. Thus, the temperature ranges discussed above are merely exemplary and are not intended to limit the invention in any way.

[0027] In accordance with the above-described system 100, Figures 2A-2D show a flow diagram of a method 200 for passivating an NLO crystal 104 with hydrogen to repair crystal defects caused by dangling bonds or broken chemical bonds. With reference to Figure 2A, the method 200 may include one or more of the following steps: (i) step 202, maintaining the temperature of the NLO crystal 104 at or near a selected temperature, which may be a user selected temperature or a temperature determined utilizing one or more attributes of the NLO crystal 104 (e.g., composition, moisture content, defect level, etc.); and (ii) step 204, exposing the NLO crystal 104 to an inert gas having a selected hydrogen concentration, which may be a user selected hydrogen concentration or a hydrogen concentration determined utilizing one or more attributes of the NLO crystal 104.

[0028] In step 202, the temperature of the NLO crystal 104 may be controlled by any heating and / or cooling elements (hereinafter "heating elements"), such as the substrate 102 configured to hold the NLO crystal 104 in the exposure chamber 101 of the system 100. The heating elements may be configured to heat or cool the NLO crystal 104 to a selected temperature, which may be a user-selected temperature, a temperature determined utilizing one or more attributes of the NLO crystal 104, or any temperature that improves hydrogen permeation into the crystal, reduces decomposition of H2 molecules into H atoms, or eliminates undesirable products (e.g., weak O-H bonds, water, etc.) from one or more reactions between hydrogen and the NLO crystal 104. For example, in one embodiment, the selected temperature may be a temperature in the range of approximately 300-350° C. The heating elements may be further configured to maintain the temperature of the NLO crystal 104 at or near the selected temperature for a selected period of time, such as the time required to adequately passivate the NLO crystal 104. For example, the time required to adequately deactivate the NLO crystal 104 may range from about 100-200 hours. Thus, in one embodiment, the heating element may be configured to maintain the temperature of the NLO crystal 104 at or near a selected temperature for a selected period of time within the range of about 100-200 hours. The temperatures and time periods discussed above are included by way of example only, and it is intended that these parameters may be significantly altered without departing from the essence of the present disclosure. Thus, nothing herein should be construed as limiting the present invention in any way.

[0029] In step 204, the NLO crystal 104 may be exposed to a passivation gas within an atmospherically controlled vessel, such as the exposure chamber 101 of the system 100. The passivation gas may be a gas mixture having a selected hydrogen concentration. The selected hydrogen concentration may be a user-selected concentration, a concentration determined utilizing one or more attributes of the NLO crystal 104, or any concentration acceptable for repairing crystal defects in the NLO crystal 104 by attaching hydrogen atoms from the passivation gas to broken or dangling chemical bonds in the NLO crystal 104. For example, in one embodiment, the selected hydrogen concentration of the passivation gas may be a hydrogen concentration in the range of approximately 5-10% of the passivation gas mixture. However, the above hydrogen concentrations are included by way of example only and are not intended to limit the invention in any way.

[0030] 2B, step 204 may include step 206 of maintaining a flow rate at which the passivation gas may flow through the vessel at or near a selected flow rate, such as a flow rate selected by a user, a flow rate determined utilizing one or more attributes of the NLO crystal 104, an acceptable flow rate to maintain a hydrogen concentration of the passivation gas in the vessel at or near a selected hydrogen concentration, or any flow rate sufficient to repair crystal defects in the NLO crystal 104 by attaching hydrogen atoms from the passivation gas to broken chemical bonds or dangling bonds in the NLO crystal 104. The flow rate may be regulated by a flow controller 110 of the system 100 or by any valve, regulator, or other means for controlling the pressure or rate at which the gas passes through one or more conduits. For example, in one embodiment, the flow controller 110 regulates the flow rate of the passivation gas flowing through the exposure chamber at or near a selected flow rate of about 10 to 200 cm. 3 1 / min, although the above ranges of flow rates are included by way of example only and should not be construed as limiting the invention in any way.

[0031] 2C and 2D, an embodiment of the method 200 may further include step 208 of monitoring the degree of passivation of the NLO crystal 104. Since the amount of OH bonds generally increases as the NLO crystal 104 is passivated as a result of attaching hydrogen atoms to the oxygen dangling bonds of the NLO crystal 104, the degree of passivation may be correlated to the amount of OH bonds or the change in the amount of OH bonds of the NLO crystal 104. Thus, the degree of passivation may be monitored by analyzing one or more absorption bands of the NLO crystal 104, which are affected by the change in the number of OH bonds of the NLO crystal 104. The absorption bands may be analyzed by using any method known in the art for detecting the level at which the NLO crystal 104 absorbs illumination having one or more wavelengths. In one embodiment, the degree of passivation may be monitored utilizing Fourier transform infrared spectroscopy (FTIR). For example, utilizing Fourier transform infrared spectroscopy (FTIR), the degree of passivation of the NLO crystal 104 may be monitored by observing at least one absorption band in the infrared (IR) spectrum of the NLO crystal 104. An FTIR process for monitoring the degree of passivation of the NLO crystal 104 may include one or more of the following steps: (i) transmitting illumination having one or more wavelengths through the NLO crystal 104, (ii) detecting the illumination transmitted through the NLO crystal 104, and (iii) utilizing information about the illumination transmitted through the NLO crystal 104 to determine an amount of illumination absorbed by the NLO crystal 104 at one or more wavelengths, and (iv) utilizing a correlation between the illumination absorbed by the NLO crystal 104 at one or more wavelengths and the amount of OH bonds or a change in the amount of OH bonds of the NLO crystal 104 to determine the degree of passivation of the NLO crystal 104.

[0032] In an additional embodiment of method 200, the NLO crystal 104 may be exposed to the inert gas in step 204 until the NLO crystal 104 is sufficiently passivated. Step 208 of monitoring the degree of passivation of the NLO crystal 104 may be utilized to determine whether the NLO crystal 104 has been sufficiently passivated. For example, the degree of passivation of the NLO crystal 104 may be determined to be between about 3200 and 4000 cm. -1 The amplitude or intensity of the absorption bands that appear or change in intensity at one or more wavelengths in the IR spectrum in the range of 3580 cm to 3590 cm may be determined by observing the amplitude or intensity of the absorption bands that appear or change in intensity at one or more wavelengths in the IR spectrum in the range of 3580 cm to 3590 cm, where the amplitude or intensity of the absorption bands that appear or change in intensity at the wavelengths correlates to the amount of O-H bonds or the change in the amount of O-H bonds in the NLO crystal 104. For example, FTIR can be used to measure the amount of O-H bonds in the infrared spectrum in the range of 3580 cm to 3590 cm. -1 A passivation spectrum may be used to monitor the absorption of nearby -OH bonds (including HO). For example, FTIR monitoring may be performed in situ, where the crystal is monitored with FTIR while it is undergoing passivation. Step 208 may further determine whether the NLO crystal 104 has been sufficiently passivated by monitoring a relative change in integrated peak intensity of one or more selected peaks in the FTIR absorption spectrum. For example, step 208 may determine sufficient passivation when a 5% decrease in the -OH absorption peak is observed.

[0033] The above-mentioned ranges of absorption band wavelengths and percentage changes for sufficient inactivation are included by way of example only, and it is contemplated that one or more absorption bands may occur at other wavelengths in the IR, visible, and / or UV spectra, and thus the above ranges of wavelengths are not intended to limit the invention in any way.

[0034] The above steps are not necessarily sequential and may occur in any order or parallel to one another. For example, in one embodiment of method 200, NLO crystal 104 may be exposed to a passivation gas as defined in step 204 while the degree of passivation of NLO crystal 104 may be monitored utilizing FTIR as defined in step 208. In some instances, it may be advantageous to combine some or all of the steps and to arrange the steps in a sequence that deviates from the order described herein. The description herein is merely illustrative and is not intended to limit one or more methods disclosed herein to any particular sequence, order, or combination of steps.

[0035] 3A-3D illustrate a method 300 for passivating and annealing an NLO crystal 104. With reference to FIG. 3A, the method 300 may include one or more of the following steps: (i) step 302, performing an annealing process on the NLO crystal 104 to reduce the moisture or OH content of the NLO crystal 104; and (ii) step 304, exposing the NLO crystal 104 to a passivation gas having a selected hydrogen concentration, which may be a user-selected hydrogen concentration or a hydrogen concentration determined utilizing one or more attributes of the NLO crystal 104.

[0036] In step 302, the NLO crystal 104 may undergo an annealing process in a dry atmosphere (e.g., clean dry air or dry inert gas) to remove at least a portion of the water or OH molecules from the NLO crystal 104. The annealing process is known to the art and may include one or more of the following steps: (i) raising or lowering the temperature of the NLO crystal 104 to a selected temperature, such as a value high enough to remove the water molecules from the NLO crystal without melting or damaging the NLO crystal 104, (ii) maintaining the temperature of the NLO crystal 104 at or near the selected temperature for a selected period of time, such as a period of time sufficient to reduce the moisture content of the NLO crystal 104 to a selected level, and (iii) raising or lowering the temperature of the NLO crystal 104 to a selected final temperature, such as ambient or room temperature, when the moisture content of the NLO crystal 104 has been reduced to the selected level. The selected level of moisture content may be a level selected by a user, a moisture content level determined utilizing one or more attributes of the NLO crystal 104, or any moisture content level that correlates to desired optical / physical performance or increased crystal lifetime.

[0037] In one embodiment, the annealing process of step 302 may further include increasing or decreasing the temperature of the NLO crystal 104 to the selected temperature over a selected time interval. For example, the NLO crystal 104 may be gradually heated to a selected temperature of about 150° C. over a selected period of about 2 hours. The temperature of the NLO crystal 104 may be increased, decreased, or maintained by any known heating or cooling device. For example, the substrate 102 may be equipped with a heating or cooling device suitable for heating or cooling the NLO crystal 104. In another example, the chamber 101 may be configured as a furnace or cooling device. The heating or cooling device may be further configured to maintain the temperature of the NLO crystal 104 at or near the selected temperature for a selected period of time, such as a user-selected period of time or a period of time determined utilizing one or more attributes of the NLO crystal 104. For example, the temperature of the NLO crystal 104 may be maintained at or near 150° C. for about 10 hours. Alternatively, the temperature of the NLO crystal 104 may be maintained at or near the selected temperature until the moisture content or OH content of the NLO crystal 104 is sufficiently reduced. The temperatures, durations, and time intervals described above are included by way of example only, and it is intended that these parameters may be significantly altered without departing from the essence of the present disclosure. Thus, nothing herein should be construed as limiting the present invention in any way.

[0038] In additional embodiments, the annealing process of step 302 may be repeated to further reduce the moisture content of the NLO crystal 104. The annealing process may be repeated utilizing the same or different parameters, such as one or more different temperatures or different durations or intervals, if necessary. For example, the NLO crystal 104 may be heated to about 200° C. for about 1 hour. Similarly, the temperature of the NLO crystal 104 may be maintained at or near 200° C. for about 100 hours, or until the moisture content or OH content of the NLO crystal 104 is sufficiently reduced. The temperatures, durations, and time intervals described above are included by way of example only, and it is intended that these parameters may be significantly altered without departing from the essence of the present disclosure. Thus, nothing herein should be construed as limiting the present invention in any way.

[0039] The annealing process of step 302 may further include gradually increasing or decreasing the temperature of the NLO crystal 104 to a selected final temperature (e.g., ambient or room temperature) over a selected time interval. For example, the NLO crystal 104 may be gradually cooled or allowed to cool to ambient or room temperature over about three hours or any other acceptable time interval. In one embodiment, the NLO crystal 104 may be cooled by gradually removing heat such that the temperature of the NLO crystal 104 gradually decreases to ambient temperature over a selected time interval. In another embodiment, the NLO crystal 104 may be cooled utilizing a cooling device to decrease the temperature of the NLO crystal 104 to the selected final temperature. The selected time interval may be any time interval selected by a user or determined utilizing one or more attributes of the NLO crystal 104. Thus, any time intervals included herein are included by way of example only and are not intended to limit the invention in any way.

[0040] 3B and 3D, the annealing process of step 302 may further include step 310 of monitoring the moisture or OH content of the NLO crystal by analyzing one or more absorption bands of the NLO crystal 104, the absorption bands being affected by changes in the number of OH bonds of the NLO crystal 104. The absorption bands may be analyzed by using any method known in the art for detecting the level at which the NLO crystal 104 absorbs illumination having one or more wavelengths. For example, utilizing FTIR, the moisture or OH content of the NLO crystal 104 may be monitored by observing at least one absorption band in the infrared (IR) spectrum of the NLO crystal 104. The FTIR process for monitoring the moisture or OH content of the NLO crystal 104 may include one or more of the following steps: (i) transmitting illumination having one or more wavelengths through the NLO crystal 104; (ii) detecting the illumination transmitted through the NLO crystal 104; and (iii) utilizing information about the illumination transmitted through the NLO crystal 104 to determine an amount of illumination absorbed by the NLO crystal 104 at one or more wavelengths; and (iv) utilizing a correlation between the illumination absorbed by the NLO crystal 104 at one or more wavelengths and the amount of OH bonds or a change in the amount of OH bonds in the NLO crystal 104 to determine a moisture content or OH content of the NLO crystal 104 or a change in the moisture content or OH content of the NLO crystal 104.

[0041] In an additional embodiment, the annealing process of step 302 may further include step 312 of performing one or more steps of the annealing process until a determination is made that the moisture or OH content of the NLO crystal has been sufficiently reduced, utilizing the monitoring process of step 310. For example, the moisture or OH content of the NLO crystal 104 may be reduced to between about 3200 and 4000 cm. -1The amplitude or intensity of the absorption band occurring at one or more wavelengths in the IR spectrum in the range of 100 nm to 100 nm may be determined by observing one or more absorption bands of the NLO crystal occurring at one or more wavelengths in the IR spectrum in the range of 100 nm to 100 nm, where the amplitude or intensity of the absorption band occurring at the wavelength correlates to the amount of O-H bonds or the change in the amount of O-H bonds in the NLO crystal 104. The above-mentioned ranges of absorption band wavelengths are included by way of example only, and it is contemplated that one or more absorption bands may occur at other wavelengths in the IR spectrum. Thus, the above-mentioned wavelength ranges are not intended to limit the invention in any way.

[0042] The above-mentioned steps of the annealing process of step 302 are not sequential or required. The steps may occur in any order or in parallel with one another. For example, it is contemplated that the NLO crystal 104 may be maintained at a selected temperature. At the same time, the moisture or OH content of the NLO crystal 104 may be monitored with the aid of FTIR as defined by step 310. It is further contemplated that the temperature of the NLO crystal 104 may be maintained at a selected temperature until the moisture or OH content of the NLO crystal 104 is sufficiently reduced as defined by step 312. In some instances, it may be advantageous to combine some or all of the steps and to arrange the steps in a sequence that deviates from the order described herein. The description herein is merely illustrative and is not intended to limit one or more methods disclosed herein to any particular sequence, order, or combination of steps.

[0043] After the NLO crystal 104 has been annealed to reduce the moisture content or OH bonds of the NLO crystal, it may be advantageous to passivate the NLO crystal 104 with hydrogen to repair crystal defects caused by one or more dangling bonds or broken chemical bonds, some of which may have resulted from the annealing process of step 302. Thus, in step 304 of method 300, the NLO crystal 104 may be exposed to a passivation gas within a vessel, such as the exposure chamber 101 of the system 100. The passivation gas may be a gas mixture having a selected hydrogen concentration. The hydrogen concentration may be a user-selected concentration, a concentration determined utilizing one or more attributes of the NLO crystal 104, or any concentration acceptable for repairing crystal defects in the NLO crystal 104 by attaching hydrogen atoms from the passivation gas to the broken chemical bonds or dangling bonds of the NLO crystal 104. For example, in one embodiment, the selected hydrogen concentration of the passivation gas may be a hydrogen concentration in the range of about 5-10% of the passivation gas mixture. However, the above hydrogen concentrations are included by way of example only and are not intended to limit the invention in any way. In some embodiments, step 304 may further include one or more steps or elements from method 200 of passivating NLO crystal 104 described above.

[0044] 3C and 3D, the passivation process of step 304 may further include step 320 of monitoring the degree of passivation of the NLO crystal 104. The degree of passivation may be monitored by analyzing one or more absorption bands of the NLO crystal 104, which are affected by changes in the number of O-H bonds of the NLO crystal 104. The absorption bands may be analyzed by using any method known in the art for detecting the level at which the NLO crystal 104 absorbs illumination having one or more wavelengths. For example, utilizing FTIR, the degree of passivation of the NLO crystal 104 may be monitored by observing at least one absorption band in the infrared (IR) spectrum of the NLO crystal 104. The FTIR process for monitoring the degree of passivation of the NLO crystal 104 may include one or more of the following steps: (i) transmitting illumination having one or more wavelengths through the NLO crystal 104; (ii) detecting the illumination transmitted through the NLO crystal 104; and (iii) utilizing information about the illumination transmitted through the NLO crystal 104 to determine an amount of illumination absorbed by the NLO crystal 104 at one or more wavelengths; and (iv) utilizing a correlation between the illumination absorbed by the NLO crystal 104 at one or more wavelengths and the amount of OH bonds or a change in the amount of OH bonds in the NLO crystal 104 to determine the degree of NLO crystal 104 deactivation.

[0045] In an additional embodiment, step 304 may further include step 322 of exposing NLO crystal 104 to a passivation gas until NLO crystal 104 is sufficiently passivated. Step 320 of monitoring the degree of passivation of NLO crystal 104 may be utilized to determine whether NLO crystal 104 has been sufficiently passivated. For example, the degree of passivation of NLO crystal 104 may be determined to be between about 3200-4000 cm -1The amplitude or intensity of the absorption bands may be determined by observing one or more absorption bands of the NLO crystal 104 appearing or varying in intensity at one or more wavelengths in the IR spectrum in the range of 100 nm to 100 nm, where the amplitude or intensity of the absorption bands appearing or varying in intensity at the wavelengths correlates to the amount of O-H bonds or the change in the amount of O-H bonds in the NLO crystal 104. The above-mentioned absorption band wavelength ranges are included by way of example only, and it is contemplated that one or more absorption bands may appear at other wavelengths in the IR spectrum. Thus, the above-mentioned wavelength ranges are not intended to limit the invention in any way.

[0046] The steps described above are not necessarily sequential, and the steps may occur in any order or in parallel with each other. For example, in one embodiment of step 304, it is contemplated that the NLO crystal 104 may be exposed to a passivation gas having a selected hydrogen concentration, and at the same time, the degree of passivation of the NLO crystal 104 may be monitored utilizing FTIR as defined in step 320. It is further contemplated that the NLO crystal 104 may be exposed to the passivation gas until the NLO crystal 104 is sufficiently passivated as defined in step 322, and the monitoring technique of step 320 may be utilized to determine whether the NLO crystal 104 has been sufficiently passivated. In some instances, it may be advantageous to combine some or all of the steps, and to arrange the steps in a sequence that deviates from the order described herein. The description herein is merely illustrative and is not intended to limit one or more methods disclosed herein to any particular sequence, order, or combination of steps.

[0047] It may be advantageous to incorporate a fully annealed and passivated NLO crystal 104 into a laser system for better physical / optical performance or longer crystal life than can be achieved utilizing an unmodified NLO crystal 104. The laser system configurations of the present disclosure may include, but are not limited to, configurations such as mode-locked, CW, or Q-switched, and any other laser or laser system that include one or more nonlinear crystals. The description herein is further intended to include a wide range of possible laser spectra, including, but not limited to, deep ultraviolet (DUV), ultraviolet (UV), infrared, visible, and other electromagnetic spectrums. As used herein, the terms "laser system" and "laser" may be used interchangeably to describe one or more laser configurations.

[0048] 4 illustrates a laser system 400 with a passivated and / or annealed NLO crystal 104. The laser system 400 of the present invention may include, but is not limited to, a light source 402, a first set of beam shaping lenses 404, the passivated / annealed crystal 104 described herein above, a housing unit 406, a set of harmonic separation elements 408, and a second set of beam shaping lenses 410.

[0049] In one aspect, the output of the light source 402 may be focused using a beam shaping lens 404 into an elliptical cross-section Gaussian beam waist at or proximate to the passivated / annealed NLO crystal 104. As used herein, the term "proximate" is preferably less than half the Rayleigh range from the center of the crystal 104. In one embodiment, the aspect ratio between the Gaussian widths of the major axes of the ellipse may be intermediate between about 2:1 and about 6:1. In other embodiments, the ratio between the major axes of the ellipse may be between about 2:1 and about 10:1. In one embodiment, the wider Gaussian width is substantially aligned with the departure direction of the NLO crystal (e.g., within about 10° of alignment).

[0050] In another aspect, the housing unit 406 may protect the NLO crystal 104 from ambient atmospheric conditions and other impurities, thereby facilitating the maintenance of its passivated / annealed state. It is noted that a crystal exposed to atmospheric water or other impurities may begin to degrade over time and revert to an unpassivated or unannealed state. Crystal housing units are generally described in U.S. patent application Ser. No. 12 / 154,337, filed May 6, 2008, entitled "Enclosure For Controlling The Environment of Optical Crystals," which is incorporated herein by reference in its entirety. In some embodiments, the housing unit 406 may include a large structure suitable for housing the crystal 104 and other components of the laser system 400. In other embodiments, the housing 406 may be large enough to house all of the components of the laser system 400. It is noted that the larger the housing, the more precautions are required for maintenance and repair of the laser system (to protect the crystal 104 from degradation and maintain its passivated / annealed state). Thus, in an additional embodiment, the housing unit 406 may consist primarily of a small housing structure suitable for enclosing only the NLO crystal 406 .

[0051] The beam shaping lens 404 may include an anamorphic lens that may change the cross section of the output from the light source 402. The anamorphic lens may include at least one of a prism, a cylindrically curved element, a radially symmetric curved element, and a diffractive element, for example. In one embodiment, the light source 402 may include a laser that produces a frequency in the visible range (e.g., 532 nm) that is doubled inside the crystal 104. In other embodiments, the light source 402 may include a laser source that produces two or more frequencies that are combined inside the crystal 402 to produce a sum or difference frequency. Frequency conversion and associated lenses and hardware are described in U.S. Patent Application Serial No. 13 / 412,564, filed March 6, 2012, Dribinski et al., which is incorporated herein by reference in its entirety.

[0052] 5 illustrates an inspection system 500 configured to measure or analyze defects on one or more specimens 510, such as a photomask (i.e., reticle), wafer, or any other specimen that may be analyzed with the aid of an optical inspection system. Inspection system 500 may include laser system 400 as described above. Laser system 400 may include one or more of the passivated / annealed NLO crystals 104 described throughout this disclosure. In one embodiment, the NLO crystals 104 of laser system 400 may be annealed sufficiently to reduce the moisture content of the NLO crystals 104 to a selected moisture content level.

[0053] In additional embodiments, the NLO crystal 104 of the laser system 400 may be passivated sufficiently to repair crystal defects caused by dangling bonds or broken chemical bonds, such as oxygen dangling bonds. The dangling bonds or broken chemical bonds of the NLO crystal 104 may be repaired by passivation by bonding hydrogen atoms to the broken chemical bonds or dangling bonds of the NLO crystal 104. In some cases, some of the dangling bonds or broken chemical bonds may be products of an annealing process performed on the NLO crystal 104. The NLO crystal 104 may be passivated to a selected degree of passivation that is acceptable to achieve a desired physical / optical performance, improved LID resistance, improved output beam quality, improved output stability, increased crystal lifetime, or higher operating power.

[0054] The NLO crystal 104 of the laser system 400 may have at least one absorption band in the IR spectrum of the NLO crystal 104 that correlates to the presence, absence, or amount of OH bonds of the NLO crystal 104. The absorption band of the NLO crystal 104 may be measured utilizing FTIR to determine the degree of passivation or moisture content level of the NLO crystal 104. A specified amplitude or intensity of the absorption band of the NLO crystal 104 may correspond to a sufficient annealing level or a sufficient passivation level of the NLO crystal 104. The specified amplitude or intensity of the absorption band may be a value selected by a user or a value determined utilizing one or more attributes of the NLO crystal 104. Thus, the absorption band of the NLO crystal 104 of the laser system 400 may have an amplitude or intensity at or near a specified amplitude or intensity. The laser system 400 may further include at least one electromagnetic source, such as a diode-pumped solid-state (DPS) source or a fiber IR source, configured to provide illumination to the NLO crystal 104. At least a portion of the illumination provided by the electromagnetic source may be transmitted directly or indirectly through NLO crystal 104 in a frequency conversion process of crystal 104 .

[0055] The inspection system 500 may further include a sample stage 512 configured to hold the sample 510 during the inspection process. The sample stage 512 may be configured to hold the sample 510 at a location where the sample 510 may receive at least a portion of the illumination transmitted from the laser system 400. The sample stage 512 may be further configured to actuate the sample 510 to a user selected location. The sample stage 512 may be further communicatively coupled to one or more computing systems and configured to actuate the sample 510 to a location selected by a user or determined by the computing systems, where the sample 510 may receive at least a portion of the illumination transmitted from the laser system 400.

[0056] The inspection system 500 may further include a detector 504 configured to directly or indirectly receive at least a portion of the illumination reflected from the surface of the specimen 510. The detector 504 may include any suitable detector known to the art, such as a charge-coupled device (CCD) or a time-delay integration (TDI) CCD-based detector. The inspection system 500 may further include one or more computing systems 514 communicatively coupled to the detector 504. The computing system 514 may be configured to receive information from the detector 504 regarding characteristics of the illumination reflected from the surface of the specimen 510. The computing system 514 may be further configured to execute an inspection algorithm from program instructions 518 on the carrier medium 516. The inspection algorithm may be any inspection algorithm known to the art for utilizing information regarding characteristics of the illumination reflected from the surface of the specimen 510 to measure one or more defects of the specimen 510. Thus, the computing system 514 may utilize information regarding the illumination reflected from the surface of the specimen 510 to perform measurements such as the presence, absence, amount, and / or type of defects of the specimen 510.

[0057] The inspection system 500 may include one or more illumination optics 503 (e.g., retarders, quarter wave plates, focusing lenses, phase modulators, polarizers, mirrors, beam splitters, reflectors, converging / diverging lenses, prisms, etc.). The illumination optics 503 may be configured to directly or indirectly receive illumination emanating from the laser system 400. The illumination optics 403 may further be configured to transmit and / or guide at least a portion of the illumination received directly or indirectly along an illumination path of the inspection system 500 from the laser system 400 to the surface of the sample 510. The illumination path may be any path along which illumination may travel from the laser system 400 to the surface of the sample 510, such as a direct line of sight between the laser system 400 and the surface of the sample 510. In some embodiments, the illumination path may be a path described by a configuration of one or more optical elements, including but not limited to the illumination optics or any other optical elements disclosed herein.

[0058] In one embodiment, the illumination path of the inspection system 400 may include a beam splitter 508 configured to transmit at least a portion of the illumination received directly or indirectly from the laser system 400 to the surface of the specimen 510 or to additional components in the illumination path. The beam splitter 508 may be any optical device capable of splitting one beam of illumination into two or more beams of illumination. The illumination path may further include inspection optics 505 (e.g., retarders, quarter wave plates, focusing lenses, phase modulators, polarizers, mirrors, beam splitters, reflectors, converging / diverging lenses, prisms, etc.) configured to transmit at least a portion of the illumination received directly or indirectly from the laser system 400 to the surface of the specimen 510.

[0059] In an embodiment, the inspection system 500 may include collection optics 505 (e.g., retarders, quarter wave plates, focusing lenses, phase modulators, polarizers, mirrors, beam splitters, reflectors, converging / diverging lenses, prisms, etc.) configured to directly or indirectly receive at least a portion of the illumination reflected from the surface of the sample 510. The collection optics 506 may be further configured to transmit at least a portion of the illumination received directly or indirectly from the surface of the sample 510 to the detector 504 along a collection path of the inspection system 500. The collection path may be any path along which illumination may travel from the surface of the sample 510 to the detector 504, such as a direct line of sight between the surface of the sample 510 and the detector 504. In some embodiments, the collection path may be a path described by an arrangement of one or more optical elements, including but not limited to collection optics or any other optical elements disclosed herein.

[0060] Although this disclosure describes inspection system 400 in the context of generically inspecting one or more specimens, it is contemplated that the inventive aspects of inspection system 400 may extend to a broad range of inspection or metrology systems utilized in the fabrication or analysis of semiconductors or semiconductor components. Inspection system 400 may be configured for one or more operational configurations known to the art. For example, inspection system 400 may be configured for brightfield inspection, darkfield inspection, or any other configuration or configuration known to the art now or in the future. Inspection system 400 may be further configured for one or more inspection functions known to the art. For example, inspection system 400 may be configured to inspect one or more photomasks, patterned wafers, unpatterned wafers, or any other inspection function known to the art now or in the future.

[0061] It should be appreciated that the various steps described throughout this disclosure may be performed by a single computing system or, alternatively, by multiple computing systems. Furthermore, different subsystems of the system may include computing systems suitable for performing at least some of the steps described above. Thus, the above description should not be construed as a limitation on the present invention, but merely as an example. Furthermore, one or more computing systems may be configured to perform any other step(s) of any of the method embodiments described herein.

[0062] A computing system may include, but is not limited to, a personal computing system, a mainframe computing system, a workstation, a graphics computer, a parallel processor, or any other device known in the art. In general, the term "computing system" may be broadly defined to encompass any device having one or more processors that executes instructions from a memory medium.

[0063] Program instructions implementing methods such as those described herein may be transmitted on or stored on a carrier medium. The carrier medium may be a transmission medium such as a wired, cabled, or wireless transmission link. The carrier medium may also include a storage medium such as a read-only memory, a random access memory, a magnetic or optical disk, or a magnetic tape.

[0064] All of the methods described herein may include storing results of one or more steps of the method embodiments in a storage medium. The results may include any of the results described herein and may be stored in any manner known in the art. The storage medium may include any storage medium described herein or other suitable storage medium known in the art. After the results are stored, they may be accessed and used in the storage medium by any of the method or system embodiments described herein, may be formatted for display to a user, may be used by another software module, method, or system, etc. Furthermore, the results may be stored "permanently," "semi-permanently," temporarily, or for some period of time. For example, the storage medium may be a random access memory (RAM), and the results may not necessarily persist indefinitely in the storage medium.

[0065] It is further contemplated that each of the method embodiments described above may include any other step(s) of any other method(s) described herein. Moreover, each of the method embodiments described above may be performed by any of the systems described herein.

[0066] Those skilled in the art will appreciate that there are a variety of means (e.g., hardware, software, and / or firmware) by which the processes and / or systems and / or other techniques described herein can be accomplished, and that the preferred means will vary depending on the context in which the processes and / or systems and / or other techniques are deployed. For example, if the implementer determines that speed and accuracy are paramount, the implementer may choose a primarily hardware and / or firmware means. Alternatively, if flexibility is paramount, the implementer may choose a primarily software implementation. Yet again, the implementer may choose some combination of hardware, software, and / or firmware. Thus, there are several possible means by which the processes and / or apparatus and / or other techniques described herein can be accomplished, none of which is inherently better than the others, in that any means utilized is a choice depending on the context in which the means is deployed, and the particular concerns of the implementer (e.g., speed, flexibility, or predictability), any of which may vary. Those skilled in the art will appreciate that the optical aspects of the implementations typically utilize optically oriented hardware, software, and / or firmware.

[0067] Those skilled in the art will recognize that it is common in the art to describe devices and / or processes in the manner set forth herein and then integrate such described devices and / or processes into a data processing system using engineering standards. That is, at least a portion of the devices and / or processes described herein can be integrated into a data processing system through a reasonable amount of experimental work. Those skilled in the art will recognize that a typical data processing system generally includes one or more of a system unit housing, a video display device, memory such as volatile and non-volatile memory, a processor such as a microprocessor and a digital signal processor, a computing entity such as an operating system, a driver, a graphic user interface, and an application program, one or more interaction devices such as a touchpad or screen, and / or a control system including feedback loops and control motors (e.g., feedback for sensing position and / or velocity, control motors for moving and / or adjusting components and / or quantities). A typical data processing system may be implemented utilizing any suitable commercially available components, such as components typically found in data computing / communication systems and / or network computing / communication systems.

[0068] The subject matter described herein may depict different components that are included within or connected to different other components. It should be understood that such depicted architectures are merely exemplary, and that in fact many other architectures that achieve the same functionality can be implemented. In a conceptual sense, any arrangement of components to achieve the same functionality is effectively "associated" such that the desired functionality is achieved. Thus, any two components that are combined herein to achieve a particular functionality can be viewed as "associated" with each other such that the desired functionality is achieved regardless of the architecture or intermediate components. Similarly, any two components that are so associated can also be considered to be "connected" or "coupled" with each other to achieve the desired functionality, and any two components that can be so associated can also be considered to be "combinable" with each other to achieve the desired functionality. Particular examples of combineable include, but are not limited to, components that can be physically coupled together and / or components that physically interact, and / or components that can wirelessly interact and / or components that wirelessly interact, and / or components that logically interact and / or components that are capable of logically interacting.

[0069] While particular embodiments of the present subject matter described herein have been shown and described, it will be apparent to those skilled in the art that, based on the teachings herein, changes and modifications may be made without departing from the subject matter described herein and its broader aspects, and therefore the appended claims should encompass within their scope all such changes and modifications as are within the true spirit and scope of the subject matter described herein.

[0070] Furthermore, it should be understood that the invention is defined by the appended claims.

[0071] While specific embodiments of the present invention have been described, it will be apparent that various modifications and embodiments of the present invention may be made by those skilled in the art without departing from the scope and spirit of the above disclosure. Accordingly, the scope of the present invention should be limited only by the claims appended hereto.

[0072] It will be appreciated that the present disclosure and many of its attendant advantages will be understood from the foregoing description, and that various changes may be made in the form, construction, and arrangement of the elements without departing from the disclosed subject matter or sacrificing all of its important advantages. The forms described are exemplary only, and it is the intent of the following claims to encompass and include such modifications.

Claims

1. 1. A method comprising: Providing a nonlinear optical (NLO) crystal; annealing the NLO crystal by maintaining the temperature within a selected temperature range below the melting temperature of the NLO crystal; exposing the NLO crystal to a passivation gas having a concentration of at least one of hydrogen and deuterium necessary to repair crystal defects caused by the annealing process, the hydrogen concentration being in the range of 5% to 10% of the passivation gas, and monitoring the passivation level using Fourier transform infrared spectroscopy (FTIR) to achieve a selected passivation level in the NLO crystal; A method for providing the above.

2. 2. The method of claim 1, wherein maintaining the temperature of the NLO crystal within the selected temperature range comprises maintaining the temperature of the NLO crystal between room temperature and the melting point of the NLO crystal.

3. 3. The method of claim 2, wherein maintaining the temperature of the NLO crystal within the selected temperature range comprises maintaining the temperature of the NLO crystal between 300.degree. C. and 350.degree.

4. 10. The method of claim 1, wherein the NLO crystal comprises at least one of beta-barium borate (BBO), lithium triborate (LBO), lithium tetraborate (LTB), lithium cesium borate (CLBO), or cesium borate (CBO).

5. The method of claim 1 , further comprising housing the NLO crystal in a crystal housing unit.

6. The method of claim 1 further comprising the step of passing a light beam from a light source through the NLO crystal.

7. 7. The method of claim 6, further comprising the step of passing a light beam from a light source through said NLO crystal to generate deep ultraviolet light in said NLO crystal.

8. The method of claim 6 further comprising shaping the light beam from the light source with one or more beam shaping optics.

Citation Information

Patent Citations

  • Cesium lithium borate crystal

    JP1997328395A

  • Method of preventing decrease in transmittance due to coloring of nonlinear optical crystal for wavelength conversion

    JP2001109027A

  • Wavelength conversion optical element, method for manufacturing wavelength conversion optical element, wavelength converter, ultraviolet laser irradiation device and laser machining system

    JP2007249092A

  • Wavelength conversion element, wavelength conversion device, and lithium tantalate single crystal used for the same

    JP2010256659A

  • Apparatus and method using a nonlinear optical crystal

    US20030011872A1