Sm-Fe-N-BASED MAGNETIC MATERIAL AND METHOD FOR MANUFACTURING THE SAME
The Sm-Fe-N magnetic material with a tailored molar ratio composition enhances saturation magnetization and stabilizes the anisotropic magnetic field by using Co and Ni substitutions, addressing the limitations of Sm reduction in existing materials.
Patent Information
- Application Number
- JP2023067750
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-04-18
AI Technical Summary
Existing Sm-Fe-N magnetic materials face challenges in maintaining high saturation magnetization while reducing the amount of Sm, as substitutions with rare earth elements like La and Ce lead to decreased anisotropic magnetic fields.
The Sm-Fe-N magnetic material is formulated with a specific molar ratio composition (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 N h where x+y≦0.73, x/(x+y)≧0.80, p+q≧1.45(x+y)-0.5485, and 2.9≦h≦3.3, incorporating Co and Ni to stabilize the crystal structure and improve saturation magnetization.
This composition allows for improved saturation magnetization while minimizing the decrease in anisotropic magnetic field, even with reduced Sm usage, by maintaining the crystal structure and optimizing lattice volume and magnetic properties.
Smart Images

Figure 2024154109000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an Sm-Fe-N based magnetic material and a method for producing the same. 2 Zinc 17 Type and Th 2 Ni 17 The present invention relates to an Sm-Fe-N based magnetic material having a main phase with at least one of the crystal structures of the above types, and a method for producing the same. [Background technology]
[0002] As high-performance magnetic materials, Sm-Co magnetic materials and Nd-Fe-B magnetic materials have been put to practical use, but in recent years, other magnetic materials have been under study. 2 Zinc 17 Type and Th 2 Ni 17 Sm-Fe-N based magnetic materials (hereinafter sometimes simply referred to as "Sm-Fe-N based magnetic materials") having a main phase with at least one of the above crystal structures have been investigated.
[0003] Sm-Fe-N magnetic materials are 2 Zinc 17 Type and Th 2 Ni 17 The main phase has at least one of the following crystal structures: Sm-Fe-based crystal phase with nitrogen interstitially introduced therein.
[0004] For example, Patent Document 1 discloses a method for producing an Sm-Fe-N based magnetic material, which comprises reducing an oxide containing Sm, Fe, La, and W, and nitriding the reduced product to obtain an Sm-Fe-N based magnetic material.
[0005] Moreover, Patent Documents 2 and 3 disclose an Sm-Fe-N based magnetic material containing a light rare earth element in addition to Sm as a rare earth element, and a method for producing the same. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-117937 A [Patent Document 2] Public Relations, Patent Publication No. 2022-53187 [Patent Document 3] Public Relations, Patent Publication No. 2022-53207 Summary of the Invention [Problem to be solved by the invention]
[0007] The magnetic properties of Sm-Fe-N magnetic materials, especially the saturation magnetization, are achieved by selecting Sm as a rare earth element. As Sm-Fe-N magnetic materials become more widespread, the price of Sm, the main element in Sm-Fe-N magnetic materials, is expected to rise. For this reason, attempts have been made to replace part of Sm with rare earth elements other than Sm, especially light rare earth elements that are less rare than Sm.
[0008] In the Sm-Fe-N magnetic material of Patent Document 1, an attempt is made to replace part of Sm with La, but the amount of La is small, and the reduction in the amount of Sm used is limited. In the Sm-Fe-N magnetic material of Patent Document 2, the amount of Sm used is reduced by replacing part of Sm with La and / or Ce, but high saturation magnetization is not achieved, and the reduction in the anisotropic magnetic field is an issue. In the Sm-Fe-N magnetic material of Patent Document 3, high saturation magnetization is achieved by replacing part of Sm with La and / or Ce, but the amount of La and / or Ce is small, and the reduction in the amount of Sm used is limited.
[0009] For this reason, the inventors have discovered that there is a need for an Sm-Fe-N based magnetic material and a method for manufacturing the same that can improve saturation magnetization while minimizing the decrease in the anisotropic magnetic field even when the amount of Sm used is reduced.
[0010] The present disclosure has been made to solve the above problems. That is, the present disclosure aims to provide an Sm-Fe-N magnetic material and a manufacturing method thereof that can improve saturation magnetization while suppressing the decrease in anisotropic magnetic field as much as possible even if the amount of Sm used is reduced. In this specification, unless otherwise specified, "saturation magnetization" means saturation magnetization at room temperature. [Means for solving the problem]
[0011] In order to achieve the above object, the present inventors have conducted intensive research and have completed the disclosed Sm-Fe-N based magnetic material and its manufacturing method. The disclosed Sm-Fe-N based magnetic material and its manufacturing method include the following aspects. 1. Th 2 Zinc 17 Type and Th 2 Ni 17 A Sm-Fe-N based magnetic material having a main phase having at least one of the following crystal structures: The composition of the main phase is expressed by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 N h It is expressed as R 1 is one or more rare earth elements other than Sm, La, and Ce, and Zr; M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements; and 0.25≦x+y≦0.73, 0.25≦x≦0.73, x / (x+y)≧0.80, 0≦z≦0.10, 0.10≦p+q≦0.53, p+q≧1.45(x+y)-0.5485, 0≦s≦0.10, and 2.9≦h≦3.3 Satisfying Sm-Fe-N magnetic material. <2> The Sm-Fe-N based magnetic material according to <1>, wherein the p and the q satisfy 0.22≦p+q≦0.53. <3> The Sm-Fe-N based magnetic material according to <1> or <2>, wherein the lattice constant of the main phase is 1.4350 to 1.4460. <4> The Sm-Fe-N based magnetic material according to <1> or <2>, wherein the lattice volume of the main phase is 0.829 to 0.838 nm. <5> The Sm-Fe-N based magnetic material according to <1> or <2>, wherein a volume fraction of the main phase is 80 to 100%. <6> The density of the main phase is 7.40 to 7.76 g / cm 3 The Sm-Fe-N based magnetic material according to <1> or <2>, <7> A method for producing the Sm-Fe-N based magnetic material according to <1>, comprising the steps of: Molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 It is expressed as R 1 preparing a magnetic material precursor having a crystalline phase satisfying 0.25≦x+y≦0.73, 0.25≦x≦0.73, x / (x+y)≧0.80, 0≦z≦0.10, 0.10≦p+q≦0.53, p+q≧1.45(x+y)-0.5485, and 0≦s≦0.10; nitriding the magnetic material precursor; A method for producing a Sm-Fe-N based magnetic material, comprising: <8> The method for producing an Sm-Fe-N based magnetic material according to <7>, wherein the p and the q satisfy 0.22≦p+q≦0.53. <9> The method for producing a Sm-Fe-N based magnetic material according to <7> or <8>, further comprising pulverizing the magnetic material precursor to obtain a magnetic material precursor powder, and then nitriding the magnetic material precursor powder. <10> The method for producing the Sm-Fe-N based magnetic material according to <7> or <8>, further comprising melting and solidifying raw materials containing elements constituting the magnetic material precursor to obtain the magnetic material precursor. Effect of the Invention
[0012] According to the present disclosure, even if Sm is substituted with a predetermined ratio of La in order to reduce the amount of Sm used, by substituting a predetermined ratio of Co for Fe, it is possible to provide an Sm-Fe-N magnetic material capable of improving saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible.
[0013] Furthermore, according to the present disclosure, it is possible to provide a method for producing an Sm-Fe-N based magnetic material that can improve saturation magnetization while suppressing a decrease in the anisotropic magnetic field as much as possible, by nitriding a magnetic material precursor in which Sm is substituted with a predetermined ratio of La in order to reduce the amount of Sm used. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a graph showing the relationship between the molar ratio x of La and the molar ratio p of Co and the phase stability. [Diagram 2] FIG. 2 is a graph showing the relationship between the lattice constant and the saturation magnetization Ms. [Diagram 3] FIG. 3 is a graph showing the relationship between the sum of the molar ratio x of La and the molar ratio y of Ce and the anisotropic magnetic field Ha. [Figure 4] FIG. 4 is a graph showing the relationship between the molar ratio x of La and the saturation magnetization Ms when the molar ratio p of Co is 0.3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure will be described in detail. Note that the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure are not limited to the embodiments described below.
[0016] Without being bound by theory, the reasons why it is possible to provide an Sm-Fe-N based magnetic material and a manufacturing method thereof that can improve saturation magnetization while minimizing the decrease in the anisotropic magnetic field even when the amount of Sm used is reduced will be explained below.
[0017] As described above, the Sm-Fe-N magnetic material of the present disclosure has a Th 2 Zinc 17 Type and Th 2 Ni 17 The main phase of the Sm-Fe-N magnetic material of the present disclosure exhibits magnetism by being nitrided. 2 Zinc 17 Type and Th 2 Ni 17 When the main phase having at least one of the crystal structures of the above types is composed of Sm, Fe, and N, the most typical composition of the main phase is Sm 2 Fe 17 N 3 Hereinafter, the phase having such a composition will be referred to as "Sm 2 Fe 17 N 3 This is sometimes called "phase".
[0018] Sm 2 Fe 17 N 3 The phase is Sm 2 Fe 17 The phase is obtained by nitriding Sm 2 Fe 17 N 3 The phase is Sm 2 Fe 17 It has a crystal structure in which nitrogen (N) is interstitially introduced into the phase. 2 Fe 17 N 3 The lattice volume of the phase is approximately 0.838 nm 3 It is.
[0019] In order to reduce the amount of Sm used, 2 Fe 17 N 3 When part of the Sm in the phase is replaced with La, which is less expensive than Sm, the lattice volume of the main phase changes, and the change in the lattice volume of the main phase changes the magnetic properties, particularly the saturation magnetization.
[0020] Since the ionic radius of La is much larger than that of Sm, when part of Sm is replaced with La, the lattice volume of the main phase basically increases. If the amount of La is too large, the lattice volume becomes too large, and the lattice volume of Th 2 Zinc 17 Type and Th 2 Ni 17 Therefore, if a part of Fe is replaced with Co and / or Ni, which have a smaller ionic radius than Fe, the increase in lattice volume can be suppressed, and as a result, the crystal structure of Th 2 Zinc 17 Type and Th 2 Ni 17 It is possible to maintain the crystal structure of at least one of the types.
[0021] When a part of Sm is replaced by a light rare earth element such as Ce or La, the saturation magnetization and anisotropic magnetic field generally decrease by the amount of the replacement. However, even if a certain proportion of Sm is replaced by La, if a certain proportion of Fe is replaced by Co, the saturation magnetization and anisotropic magnetic field decrease by the amount of the replacement. 2 Zinc 17 Type and Th 2 Ni 17 Not only can it maintain at least one of the crystal structures, but also the magnetic properties are improved. That is, the inventors have found that even if Sm is substituted with a certain ratio of La, when Fe is substituted with a certain ratio of Co, it is possible to improve the saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible, more than expected from the amount of substitution with La.
[0022] Next, the constituent elements of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure, which have been completed based on the findings and the like described above, will be described.
[0023] 《Sm-Fe-N magnetic material》 The Sm-Fe-N magnetic material of the present disclosure has a Th 2 Zinc 17 Type and Th 2 Ni 17 The Sm-Fe-N based magnetic material of the present disclosure exhibits magnetism due to the main phase. The main phase will be described below.
[0024] <Crystal structure of the main phase> The main phase is Th 2 Zinc 17 Type and Th 2 Ni 17 The main phase has at least one of the following crystal structures: TbCu 7 The Sm-Fe-N magnetic material may include a crystal structure of the type. Th is thorium, Zn is zinc, Ni is nickel, Tb is terbium, and Cu is copper. The crystal structure of the main phase can be identified by subjecting the Sm-Fe-N magnetic material to, for example, X-ray diffraction analysis.
[0025] A phase having the above-mentioned crystal structure can be achieved by various element combinations (compositions), but the main phase of the Sm-Fe-N magnetic material of the present disclosure is achieved by the following element combination (composition): The composition of the main phase of the Sm-Fe-N magnetic material of the present disclosure will be described below.
[0026] <Composition of the main phase> The main phase is represented by the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 N h In the above formula, Sm is samarium, La is lanthanum, Ce is cerium, Fe is iron, Co is cobalt, and Ni is nickel. 1is one or more rare earth elements other than Sm, La, and Ce, and Zr, and M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements. Zr is zirconium. In the above formula, for the sake of convenience, Sm (1-x-y) La x Ce y R 1 z rare earth site, Fe (1-p-q-s) Co p Ni q M s are sometimes called iron group sites.
[0027] As can be seen from the above formula, the main phase contains 2 moles of one or more elements in the rare earth site, 17 moles of one or more elements in the iron group site, and h moles of nitrogen (N). That is, one or more elements in the rare earth site and one or more elements in the iron group site constitute a phase having the above-mentioned crystal structure, and h moles of nitrogen (N) are introduced interstitially into the phase. If the amount of nitrogen (N) introduced is h moles (where h is 2.9 to 3.1), the above-mentioned crystal structure can be maintained. Details of nitrogen (N) in the main phase will be described later.
[0028] The rare earth sites are Sm, La, Ce, and R. 1 Sm, La, Ce, and R 1 Each of them exists in a molar ratio of (1-xyz):x:y:z. Since (1-xyz)+x+y+z=1, a part of Sm is present in La, Ce, and R. 1 It means that the group consisting of one or more elements is substituted.
[0029] The iron group site consists of Fe, Co, Ni, and M, and Fe, Co, Ni, and M are present in a molar ratio of (1-pqs):p:q:s. Since (1-pqs)+p+q+s=1, this means that a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M.
[0030] The elements constituting the above formula and their content ratios (molar ratios) will be explained below.
[0031] <Sm> Sm is a major element that constitutes the above-mentioned crystal structure together with Fe and N. A part of Sm is mixed with La, Ce, and R. 1 Hereinafter, La, Ce, and R are substituted with one or more elements selected from the group consisting of 1 This article explains:
[0032] 〈La〉 La belongs to the so-called light rare earth elements, and is abundant in reserves (resources) and inexpensive compared to Sm. Since the ionic radius of La is much larger than that of Sm, substituting a portion of Sm with La basically increases the lattice volume of the main phase.
[0033] As mentioned above, the ionic radius of La is much larger than that of Sm. Therefore, substituting part of Sm with La has a large effect on the change in the lattice volume of the main phase. However, if the amount of La substituted is too large, the main phase becomes a lattice volume of Th. 2 Zinc 17 Type and Th 2 Ni 17 Therefore, if a part of Fe is replaced with Co and / or Ni, which have a smaller ionic radius than Fe, the increase in lattice volume is suppressed, and as a result, the main phase becomes a crystal structure of Th. 2 Zinc 17 Type and Th 2 Ni 17 The substitution ratio when a part of Sm is substituted with La and the substitution ratio when a part of Fe is substituted with Co will be described later.
[0034] <Ce> Ce belongs to the so-called light rare earth elements, and is abundant in reserves (resources) and inexpensive compared to Sm. Since the ionic radius of Ce is slightly larger than that of Sm, substituting part of Sm with Ce basically increases the lattice volume of the main phase. However, because Ce ions can be trivalent or tetravalent, substituting part of Sm with Ce may increase or decrease the lattice volume of the main phase.
[0035] As described above, the ionic radius of Ce is slightly larger than that of Sm. Therefore, even if a part of Sm is replaced with Ce, the effect on the change in the lattice volume of the main phase is small, and therefore the effect on the saturation magnetization and anisotropic magnetic field is small. Therefore, Ce may be optionally contained in the Sm-Fe-N magnetic material of the present disclosure. As described above, La has a large effect on the change in the lattice volume of the main phase, so the replacement of a part of Sm with La must be performed simultaneously with the replacement of a part of Fe with Co, and since there is an upper limit to the replacement ratio of La, in order to increase the reduction amount of Sm, a part of Sm may be optionally replaced with Ce.
[0036] <R 1 〉 R 1 R is one or more rare earth elements other than Sm, La, and Ce, and Zr. 1 R is one or more elements that may be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. 1 Typically, R is one or more rare earth elements other than Sm, La, and Ce that are difficult to completely separate from Sm, La, and Ce when refining raw materials containing these elements, and remain in small amounts in the raw materials. 1 may contain Zr. Although Zr is not a rare earth element, a part of Sm may be substituted with Zr. Even if a part of Sm is substituted with Zr, as long as the amount of substitution is small, the magnetic properties of the Sm-Fe-N magnetic material are not significantly impaired.
[0037] In this specification, unless otherwise specified, the rare earth elements are 17 elements, namely, Sc (scandium), Y (yttrium), La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (eurobium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (ruthenium). Furthermore, among these, Sc, Y, La, and Ce are light rare earth elements, unless otherwise specified. Furthermore, Pr, Nd, Pm, Sm, and Eu are medium rare earth elements, unless otherwise specified. And, unless otherwise specified, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu are heavy rare earth elements. In general, heavy rare earth elements are highly rare, and light rare earth elements are less rare. The rarity of medium rare earth elements is between that of heavy rare earth elements and light rare earth elements.
[0038] <Fe> Fe is a main element that constitutes the above-mentioned crystal structure together with Sm and N. A part of Fe must be substituted with one or more elements selected from the group consisting of Co and Ni, and may further be substituted with M. Co, Ni, and M will be explained below.
[0039] <Co> A part of Fe is substituted with Co and / or Ni, and is preferably substituted with Co. Co belongs to the so-called iron group elements, and the ionic radius of Co is smaller than that of Fe. When a part of Sm is substituted with La, the lattice volume of the main phase basically increases, so by substituting a part of Fe with Co, it is possible to suppress an excessive increase in the lattice volume of the main phase.
[0040] Substituting a portion of Fe with Co is advantageous because it increases the Curie temperature of the main phase and makes it possible to suppress the decrease in saturation magnetization at high temperatures (403 to 473 K).
[0041] 〈Ni〉 A part of Fe is substituted with Co and / or Ni. Ni belongs to the so-called iron group element, and the ionic radius of Ni is smaller than that of Fe. When a part of Sm is substituted with La, the lattice volume of the main phase basically increases, so by substituting a part of Fe with Ni, it is possible to suppress an excessive increase in the lattice volume of the main phase.
[0042] When part of Fe is replaced with Ni, there is concern that the magnetic properties will deteriorate. However, since the ionic radius of Ni is smaller than that of Co, when part of Fe is replaced with Ni, the lattice volume of the main phase is significantly reduced even if the Ni substitution rate is not so high, compared to when part of Fe is replaced with Co. For this reason, when part of Sm is replaced with a large amount of La and the lattice volume of the main phase is excessively increased, the lattice volume of the main phase can be advantageously suppressed by using a relatively small amount of Ni. As a result, rather than the deterioration of the magnetic properties caused by replacing part of Fe with Ni, it is more effective to suppress the lattice volume of the main phase and increase the lattice volume of Th. 2 Zinc 17 Type and Th 2 Ni 17 Even when a part of Sm is replaced with La to increase the amount of Sm used, this contributes to improving the saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible.
[0043] <M> M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements. M is one or more elements and unavoidable impurity elements that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. An unavoidable impurity element refers to an impurity element whose inclusion cannot be avoided when manufacturing the Sm-Fe-N magnetic material of the present disclosure, or whose avoidance would lead to a significant increase in manufacturing costs. Examples of such unavoidable impurity elements include impurity elements in raw materials, or elements such as Cu (copper), Zn (zinc), Ga (gallium), Al (aluminum), and B (boron) that diffuse and / or penetrate into the surface of the main phase when forming a bonded compact. Other examples include elements contained in a lubricant used during molding that diffuse and / or penetrate into the surface of the main phase.
[0044] Examples of M excluding unavoidable impurity elements include one or more elements selected from the group consisting of Ti (titanium), Cr (chromium), Mn (manganese), V (vanadium), Mo (molybdenum), W (tungsten), and C (carbon). These elements form nuclei during the generation of the main phase, and contribute to promoting refinement of the main phase and / or suppressing grain growth of the main phase.
[0045] Also, Zr may be included as M. As mentioned above, Zr is not a rare earth element, but a part of Sm may be substituted with Zr, while a part of Fe may be substituted with Zr. In either case, if the amount of substitution is small, the magnetic properties of the Sm-Fe-N magnetic material are not significantly impaired.
[0046] <N> N is introduced interstitially into the main phase having the above-mentioned crystal structure. By introducing N to an extent that does not destroy the phase having the above-mentioned crystal structure, a magnetic moment appears in the main phase.
[0047] In the Sm-Fe-N magnetic material of the present disclosure, a part of Sm is substituted, necessarily, by La, and optionally, by Ce, and a part of Fe is substituted, essentially, by Co and / or Ni, preferably by Co. In this regard, the composition of the main phase is represented by the formula (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 N h The following explanation will be given using the following.
[0048] 〈x+y〉 In the above formula representing the composition of the main phase, the value of x indicates the proportion (molar ratio) of a portion of Sm substituted with La, and the value of y indicates the proportion (molar ratio) of a portion of Sm substituted with Ce.
[0049] If the value of x+y is 0.25 or more, it is substantially recognized that the economic efficiency is improved by substituting a part of Sm with inexpensive La and / or Ce. In addition, if the value of x+y is 0.25 or more, it is substantially recognized that the saturation magnetization is improved while suppressing the decrease in the anisotropic magnetic field as much as possible. From these viewpoints, the value of x+y may be 0.28 or more, 0.30 or more, 0.35 or more, 0.40 or more, 0.47 or more, 0.51 or more, or 0.55 or more. On the other hand, if the value of x+y is 0.73 or less, it is substantially recognized that the main phase is composed of Th, taking into consideration that a part of Fe is substituted with Co and / or Ni. 2 Zinc 17 Type and Th 2 Ni 17 In this respect, the value of x+y may be 0.70 or less, 0.65 or less, or 0.58 or less.
[0050] Also, while the value of x+y satisfies the above-mentioned range, the value of x may be 0.25 or more, 0.28 or more, 0.30 or more, 0.35 or more, 0.40 or more, 0.47 or more, 0.48 or more, 0.51 or more, or 0.55 or more, and may be 0.73 or less, 0.70 or less, 0.65 or less, or 0.58 or less. Similarly, while the value of x+y satisfies the above-mentioned range, the value of y may be 0.26 or less, 0.24 or less, 0.22 or less, 0.20 or less, 0.19 or less, 0.18 or less, 0.16 or less, 0.14 or less, 0.12 or less, 0.10 or less, or 0.05 or less, or may be 0. When y is 0, it means that Ce is not intentionally contained, and that the presence of Ce cannot be practically measured.
[0051] 〈The relationship between x and x+y〉 When a part of Sm is replaced by La or Ce, it is better to have a high ratio of La in order to improve saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible. Therefore, x / (x+y) may be 0.80 or more, 0.82 or more, 0.85 or more, 0.90 or more, or 0.95 or more, or may be 1. x / (x+y) being 1 means that y is 0, that is, Ce is not intentionally contained, and the presence of Ce cannot be practically measured.
[0052] <z> In the above formula that represents the composition of the main phase, z is a part of Sm that is R. 1 As mentioned above, R 1 is one or more rare earth elements and Zr that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. For this reason, z may be 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less. On the other hand, when the Sm-Fe-N magnetic material of the present disclosure has R 1 In other words, z may be 0. However, when producing the Sm-Fe-N based magnetic material of the present disclosure, the raw material may contain R. 1 From this viewpoint, z may be 0.01 or more.
[0053] <p+q> In the above formula representing the composition of the main phase, the value of p indicates the proportion (molar ratio) of part of Fe substituted with Co, and the value of q indicates the proportion (molar ratio) of part of Fe substituted with Ni.
[0054] When a part of Sm is replaced by a small amount of La and / or Ce, a part of Fe is not replaced by Co and / or Ni, i.e., even if the value of p+q is 0, Th 2 Zinc 17 Type and Th 2 Ni 17 It is possible to maintain at least one of the crystal structures of the type.
[0055] However, when a part of Sm is replaced by La, or optionally Ce, in order to drastically reduce the amount of Sm used, as in the Sm-Fe-N magnetic material of the present invention, the amount of the replacement is large, and the lattice volume of the main phase basically increases. 2 Zinc 17 Type and Th 2 Ni 17 The crystal structure of at least one of the types is maintained.
[0056] If the value of p+q is 0.10 or more, Th 2 Zinc 17 Type and Th 2 Ni 17 At least one of the crystal structures of the above types can be maintained. From this viewpoint, the value of p+q may be 0.15 or more, 0.20 or more, 0.22 or more, or 0.30 or more. On the other hand, although Co and Ni are more expensive than Fe, as long as the value of p+q is 0.53 or less, the improvement in economy due to the substitution of a part of Sm with inexpensive La and / or Ce is not offset. From this viewpoint, the value of p+q may be 0.50 or less, 0.45 or less, 0.40 or less, 0.35 or less, or 0.33 or less.
[0057] Also, while the value of p+q satisfies the above-mentioned range, the value of p may be 0.10 or more, 0.15 or more, 0.20 or more, 0.22 or more, or 0.30 or more, and may be 0.53 or less, 0.50 or less, 0.45 or less, 0.40 or less, 0.35 or less, or 0.33 or less. Similarly, while the value of p+q satisfies the above-mentioned range, the value of q may be 0.20 or less, 0.15 or less, 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less, or may be 0. q being 0 means that Ni is not intentionally contained, and that the presence of Ni cannot be practically measured.
[0058] <The relationship between x+y and p+q> x+y and p+q satisfy the relationship p+q≧1.45(x+y)-0.5485. If this relationship is satisfied, then Th 2 Zinc 17 Type and Th 2 Ni 17 At least one of the crystal structures of the two types is maintained, and the saturation magnetization is improved while suppressing the decrease in the anisotropic magnetic field as much as possible.
[0059] As explained above, when a part of Sm is replaced with La or Ce, and when a part of Fe is replaced with Co or Ni, La and Co have a large effect on improving saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible. From this, in the relationship of p+q≧1.45(x+y)-0.5485, it can be roughly approximated that q and y are 0, and it can be considered that the relationship of p≧1.45x-0.5485 is approximately satisfied. According to this, the value of x indicates the ratio (molar ratio) of a part of Sm replaced with La, and the value of p indicates the ratio (molar ratio) of a part of Fe replaced with Co, so that the effect of substitution with La can be considered to be 1.45 times that of substitution with Co.
[0060] 〈s〉 In the above formula representing the composition of the main phase, s indicates the ratio (molar ratio) of Fe partially substituted with M. As described above, M is one or more elements and inevitable impurity elements that are permitted to be contained within a range that does not impair the magnetic properties of the Sm-Fe-N magnetic material of the present disclosure. For this reason, s may be 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less. On the other hand, the Sm-Fe-N magnetic material of the present disclosure may not contain M at all, that is, s may be 0, but it is difficult to completely prevent M from containing inevitable impurity elements. From this viewpoint, s may be 0.01 or more.
[0061] <h> Next, we will explain h, which indicates the degree of nitriding. 2 Fe 17 When the phase is nitrided, it basically becomes Sm 2 Fe 17 N h phase (where h=3). Nitriding is typically performed using Sm 2 Fe 17 This is done by exposing a precursor of the Sm-Fe-N magnetic material having a phase (hereinafter, sometimes simply referred to as the "precursor") to a nitrogen gas atmosphere at high temperature. Therefore, the degree of nitridation differs between the surface and the inside of the precursor, and h can vary within the range of 2.9 to 3.3. The same applies when part of Sm in the precursor is replaced with La and / or Ce, and part of Fe is replaced with Co and / or Ni. That is, (Sm, La, Ce) 2 (Fe, Co, Ni) 17 When the phase is nitrided, (Sm, La, Ce) 2 (Fe, Co, Ni) 17 N h phase (where h is 2.9 to 3.3).
[0062] When the main phase of the Sm-Fe-N magnetic material of the present disclosure has the composition described above and further has the following lattice volume, lattice constant, volume fraction, and density, the saturation magnetization is improved while suppressing the decrease in the anisotropic magnetic field as much as possible, with more stability. The lattice volume, lattice constant, volume fraction, and density are described below.
[0063] <Lattice volume> The lattice volume of the main phase is 0.829 to 0.838 nm 3 When the lattice volume of the main phase is in this range, Th 2 Zinc 17 Type and Th 2 Ni 17 This makes it easier to maintain the crystal structure of at least one of the molds.
[0064] As mentioned above, the saturation magnetization is derived from the magnetic moment that appears in the main phase due to the introduction of N in an interstitial manner into the main phase. For this reason, the saturation magnetization is significantly affected by the Fe-N distance in the lattice of the main phase (hereinafter, sometimes simply referred to as the "Fe-N distance"). Since Fe and N are arranged three-dimensionally in the lattice of the main phase, the lattice volume of the main phase is convenient for grasping the Fe-N distance.
[0065] In the Sm-Fe-N magnetic material of the present disclosure, a part of Sm is substituted, necessarily, by La and optionally by Ce, and a part of Fe is substituted by Co and / or Ni. 2 Fe 17 N 3 The lattice volume of the phase is changed. At this time, the Fe-N distance in the lattice of the main phase is changed by Sm 2 Fe 17 N 3 It is considered that it is best to approach the Fe-N distance in the lattice of the Sm phase. 2 Fe 17 N 3 The lattice volume of the phase is approximately 0.838 nm 3 Therefore, the lattice volume of the main phase of the Sm-Fe-N magnetic material of the present disclosure is set to 0.838 nm 3 It is considered good to approach Th 2 Zinc 17 Type and Th 2 Ni 17 In order to maintain at least one of the crystal structures of the Sm type and to improve the saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible, the lattice volume of the main phase should be within the range of Sm 2Fe 17 N 3 From these viewpoints, the lattice volume of the main phase is preferably equal to or slightly smaller than that of the lattice volume of the lattice of the main phase. 3 Above, 0.830nm 3 Above, 0.831nm 3 Above, 0.832nm 3 Above, 0.833nm 3 or more than 0.834 nm 3 or more, 0.838 nm 3 Below, 0.837nm 3 Below, 0.836nm 3 Less than or equal to 0.835 nm 3 It may be the following:
[0066] The lattice volume of the main phase can be obtained as follows. The Sm-Fe-N magnetic material is subjected to X-ray diffraction analysis, and the a-axis length and the c-axis length are obtained from the X-ray diffraction pattern based on the relationship between the plane index and the lattice spacing value (d value). When obtaining the a-axis length and the c-axis length, since the main phase of the Sm-Fe-N magnetic material of the present disclosure has the above-mentioned crystal structure, it may be assumed that the main phase is a rhombohedron. Therefore, the plane indexes that can be used are the (202) plane, the (113) plane, the (104) plane, the (211) plane, the (122) plane, and the (300) plane. Then, the lattice volume can be calculated according to the following formula. (Lattice volume) = {(a-axis length) / 2} 2 x6x3 0.5 ×{(c-axis length) / 3}
[0067] <Lattice constant> The lattice constant of the main phase is preferably 1.4350 to 1.4460. When the lattice constant of the main phase is in this range, the main phase is flattened, the saturation magnetization is improved, and the decrease in the anisotropic magnetic field is smaller than expected from the reduction in the amount of Sm used. From these viewpoints, the lattice constant of the main phase may be 1.4360 or more, 1.4370 or more, 1.4380 or more, 1.4390 or more, 1.4400 or more, 1.4410 or more, 1.4420 or more, or 1.4430 or more, or may be 1.4459 or less, 1.4458 or less, or 1.4457 or less.
[0068] The lattice constant of the main phase can be obtained as follows. The Sm-Fe-N magnetic material is subjected to X-ray diffraction analysis, and the a-axis length and the c-axis length are obtained from the X-ray diffraction pattern based on the relationship between the plane index and the lattice spacing value (d value). When obtaining the a-axis length and the c-axis length, since the main phase of the Sm-Fe-N magnetic material of the present disclosure has the above-mentioned crystal structure, it may be assumed that the main phase is a rhombohedron. Therefore, the plane indexes that can be used are the (202) plane, the (113) plane, the (104) plane, the (211) plane, the (122) plane, and the (300) plane. Then, the lattice constant can be calculated according to the following formula. Lattice constant (a / c) = (a-axis length) / (c-axis length)
[0069] <Volume ratio> The Sm-Fe-N magnetic material of the present disclosure includes a main phase represented by the above-mentioned composition formula. The magnetic properties of the Sm-Fe-N magnetic material of the present disclosure are expressed by the main phase. Therefore, it is preferable that the volume ratio of the main phase is high relative to the entire Sm-Fe-N magnetic material of the present disclosure. Specifically, the volume ratio of the main phase may be 80% or more, 81% or more, or 85% or more relative to the entire Sm-Fe-N magnetic material of the present disclosure. On the other hand, when manufacturing the Sm-Fe-N magnetic material of the present disclosure, there may be a process in which a phase other than the main phase represented by the above-mentioned composition formula is in a stable temperature range. In addition, it may be difficult to completely eliminate the inclusion of unavoidable impurity elements that do not constitute the main phase. For these reasons, the volume ratio of the main phase is ideally 100%, but as long as the volume ratio of the main phase is secured, there is no practical problem even if the volume ratio of the main phase is 99% or less, 98% or less, 97% or less, 96% or less, or 95% or less.
[0070] Phases other than the main phase are typically present at grain boundaries between the main phases, particularly at triple junctions. Phases other than the main phase are typically SmFe 3 phase and its nitride phase. 3 In the phase and its nitride phase, part of Sm is replaced by La, Ce, and R. 1a phase in which a part of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M, and a nitride phase thereof; and a phase in which a part of Sm is substituted with La, Ce, and R. 1 and a phase in which a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M, and a nitride phase thereof.
[0071] The volume fraction of the main phase was determined by measuring the overall composition of the precursor before nitriding using inductively coupled plasma atomic emission spectroscopy (ICP-AES). From the measured value, it was found that the precursor before nitriding contained the following elements: (Sm, La, Ce, R 1 ) 2 (Fe, Co, Ni, M) 17 Phase and (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3 Assuming that the phase is separated into two phases, calculate the volume fraction of the main phase. Specifically, after obtaining the mass concentration (mass fraction) of each element from the ICP measurement results, Sm 2 Fe 17 phase and SmFe 3 The mass ratio of each phase is first calculated, and then the volume fraction is calculated from the density of each phase. 1 ) 2 (Fe, Co, Ni, M) 17 The phase is Sm 2 Fe 17 Phase, Sm 2 Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of Sm 2 Fe 17 A phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and Sm 2 Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm2 Fe 17 It represents a phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M. Also, (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3 The phase is SmFe 3 Phase, SmFe 3 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of SmFe 3 A phase in which part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and SmFe 3 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm 2 Fe 17 The Fe in the phase is partially substituted with one or more elements selected from the group consisting of Co, Ni, and M.
[0072] The overall composition (total of the main phase and phases other than the main phase) of the Sm-Fe-N magnetic material of the present disclosure is such that, from the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase and its nitride phase during the production of the Sm-Fe-N magnetic material of the present disclosure, the main phase contains Sm, La, Ce, and R. 1 That is, the overall composition of the Sm-Fe-N magnetic material of the present disclosure can be set to be equal to or greater than the total mole number of (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 N h(wherein w is 2.00 to 3.00). In this case, x, y, z, p, q, s, and h may be the same as x, y, z, p, q, s, and h in the formula expressing the composition of the main phase described above. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is more preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more, or 2.50 or more. On the other hand, in the case of the above-mentioned (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3 From the viewpoint of reducing the volume fraction of the phase, w is more preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.
[0073] <Density of the main phase> The density of the main phase is 7.40 g / cm 3 More than 7.45g / cm 3 or more than 7.50g / cm 3 More than 7.76 g / cm is preferable. 3 Below, 7.70g / cm 3 or less than 7.65g / cm 3 The following is preferable: When the density of the main phase is within this range, it contributes to improving the saturation magnetization.
[0074] The density of the main phase is obtained by pulverizing the Sm-Fe-N magnetic material to obtain a powder, and measuring the density of the powder by a pycnometer method. As described above, in the Sm-Fe-N magnetic material of the present disclosure, the volume fraction of the main phase is preferably 80%. 2 Fe 17 N 3 phase and SmFe 3 The density of each phase is 7.65 g / cm 3 and 8.25 g / cm 3 Therefore, the density of the main phase can be approximated by the value obtained by the above-mentioned measurement method.
[0075] 《Manufacturing method》 Next, a method for producing the Sm-Fe-N based magnetic material of the present disclosure (hereinafter sometimes referred to as the "production method of the present disclosure") will be described.
[0076] The manufacturing method of the present disclosure includes a magnetic material precursor preparation step and a nitriding step. Each step will be described below.
[0077] <Magnetic material precursor preparation process> In the manufacturing method of the present disclosure, the molar ratio formula (Sm (1-x-y-z) La x Ce y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 A magnetic material precursor having a crystalline phase with a composition represented by the following formula is prepared.
[0078] In the formula that represents the composition of the crystal phase, Sm, La, Ce, R 1 , Fe, Co, Ni, and M, as well as x, y, z, p, q, and s are as explained in “Sm—Fe—N based magnetic material.”
[0079] The crystalline phase of the magnetic material precursor is Th 2 Zinc 17 Type and Th 2 Ni 17 The magnetic material precursor has at least one of the crystal structures of the Th type. When the magnetic material precursor is nitrided, the crystal phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N magnetic material of the present disclosure. The main phase of the Sm-Fe-N magnetic material of the present disclosure is a Th 2 Zinc 17 Type and Th 2 Ni 17 The nitriding has at least one of the crystal structures of the Th 2 Zinc 17 Type and Th 2 Ni 17 The annealing is carried out to such an extent that at least one of the crystal structures of the two types is maintained, and a main phase having a lattice volume and a lattice constant in the above-mentioned ranges can be obtained.
[0080] As described above, the crystalline phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N magnetic material of the present disclosure, so the volume fraction of the crystalline phase in the magnetic material precursor may be considered to be equivalent to the volume fraction of the main phase in the Sm-Fe-N magnetic material of the present disclosure. For this reason, the volume fraction of the crystalline phase in the magnetic material precursor may be 80% or more, 81% or more, or 85% or more with respect to the entire magnetic material precursor. When manufacturing the magnetic material precursor, there may be a process in which a phase other than the crystalline phase represented by the above-mentioned composition formula is in a stable temperature region. In addition, it may be difficult to completely eliminate the inclusion of unavoidable impurity elements that do not constitute the crystalline phase. Although the volume fraction of the crystalline phase is ideally 100%, as long as the volume fraction of the above-mentioned crystalline phase is secured, there is no practical problem even if the volume fraction of the main phase is 99% or less, 98% or less, 97% or less, 96% or less, or 95% or less.
[0081] Phases other than the crystalline phase are typically present at grain boundaries between crystalline phases, particularly at triple junctions. Phases other than the crystalline phase are typically SmFe 3 etc. 3 In the phase, part of Sm is replaced by La, Ce, and R. 1 a phase in which a portion of Fe is replaced by one or more elements selected from the group consisting of Co, Ni, and M; and a phase in which a portion of Sm is replaced by La, Ce, and R. 1 and a phase in which a portion of Fe is substituted with one or more elements selected from the group consisting of Co, Ni, and M.
[0082] The volume fraction of the crystalline phase was determined by measuring the overall composition of the precursor before nitridation using inductively coupled plasma atomic emission spectroscopy (ICP-AES). From the measured value, it was determined that the precursor before nitridation contained the following elements: (Sm, La, Ce, R 1 ) 2 (Fe, Co, Ni, M) 17 Phase and (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3Assuming that the crystal phase is separated into two phases, the volume fraction of the crystal phase is calculated. Specifically, after obtaining the mass concentration (mass fraction) of each element from the ICP measurement results, Sm 2 Fe 17 phase and SmFe 3 The mass ratio of each phase is first calculated, and then the volume fraction is calculated from the density of each phase. 1 ) 2 (Fe, Co, Ni, M) 17 The phase is Sm 2 Fe 17 Phase, Sm 2 Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of Sm 2 Fe 17 A phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and Sm 2 Fe 17 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of Sm 2 Fe 17 It represents a phase in which a part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M. Also, (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3 The phase is SmFe 3 Phase, SmFe 3 Part of the Sm in the phase is Sm, La, Ce, and R. 1 A phase substituted with one or more elements selected from the group consisting of SmFe 3 A phase in which part of the Fe in the phase is replaced with one or more elements selected from the group consisting of Co, Ni, and M, and SmFe 3 Part of the Sm in the phase is Sm, La, Ce, and R. 1 and is substituted with one or more elements selected from the group consisting of SmFe 3 The Fe in the phase is partially substituted with one or more elements selected from the group consisting of Co, Ni, and M.
[0083] The overall composition of the magnetic material precursor (the sum of the crystalline phase and the phases other than the crystalline phase) is, from the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase during the production of the magnetic material precursor, Sm, La, Ce, and R in the crystalline phase. 1 That is, the overall composition of the magnetic material precursor can be set to be equal to or greater than the total mole number of (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 (wherein w is 2.00 to 3.00). In this case, x, y, z, p, q, and s may be the same as x, y, z, p, q, and s in the formula expressing the composition of the above-mentioned crystal phase. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is more preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more, or 2.50 or more. On the other hand, when (Sm, La, Ce, R 1 )(Fe, Co, Ni, M) 3 From the viewpoint of reducing the volume fraction of the phase, w is more preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.
[0084] The magnetic material precursor can be obtained by using a well-known manufacturing method. For example, a method for obtaining the magnetic material precursor includes melting and solidifying raw materials containing elements constituting the magnetic material precursor. For example, a method for melting the raw materials includes charging the raw materials into a container such as a crucible, and melting the raw materials in the container by arc melting or high frequency melting to obtain a molten metal, and then pouring the molten metal into a mold such as a book mold, or solidifying the molten metal in a crucible. From the viewpoint of suppressing the coarsening of the crystalline phase in the magnetic material precursor and homogenizing the crystalline phase, it is preferable to increase the cooling rate of the molten metal. From this viewpoint, it is preferable to pour the molten metal into a mold such as a book mold. Furthermore, from the viewpoint of suppressing the coarsening of the crystalline phase in the magnetic material precursor and enhancing the homogenization of the crystalline phase, for example, the following method may be adopted. That is, the raw materials are melted by high frequency or arc in a container, solidified, and the resulting ingot is melted again by high frequency melting or the like, and the resulting melt is quenched using a strip casting method, a liquid quenching method, or the like to obtain a flake, which may then be used as the magnetic material precursor.
[0085] Prior to nitriding, which will be described later, the magnetic material precursor may be heat-treated (hereinafter, such heat treatment may be referred to as "homogenization heat treatment") in order to homogenize the crystal grains in the magnetic material precursor. The temperature of the homogenization heat treatment may be, for example, 1273K or more, 1323K or more, or 1373K or more, and may be 1523K or less, 1473K or less, or 1423K or less. The homogenization heat treatment time may be, for example, 6 hours or more, 12 hours or more, 18 hours or more, or 24 hours or more, and may be 48 hours or less, 42 hours or less, 36 hours or less, or 30 hours or less.
[0086] In order to suppress oxidation of the magnetic material precursor, the homogenization heat treatment is preferably performed in an inert gas atmosphere. The inert gas atmosphere does not include a nitrogen gas atmosphere. When the homogenization heat treatment is performed in a nitrogen gas atmosphere, the Th 2 Zinc 17 Type and / or Th 2 Ni 17 This is because the phase having the crystal structure of this type is easily decomposed.
[0087] <Nitriding process> The above-mentioned magnetic material precursor is nitrided, whereby the crystal phase in the magnetic material precursor is nitrided to form the main phase of the Sm—Fe—N based magnetic material of the present disclosure.
[0088] As long as the desired main phase can be obtained, the nitriding method is not particularly limited, but typically includes, for example, exposing the magnetic material precursor to an atmosphere containing nitrogen gas while heating, or exposing it to a gas atmosphere containing nitrogen (N). Examples of the atmosphere containing nitrogen gas include a nitrogen gas atmosphere, a mixed gas atmosphere of nitrogen gas and an inert gas, and a mixed gas atmosphere of nitrogen gas and hydrogen gas. Examples of the gas atmosphere containing nitrogen (N) include an ammonia gas atmosphere, or a mixed gas atmosphere of ammonia gas and hydrogen gas. The atmospheres exemplified above may be combined. From the viewpoint of nitriding efficiency, an ammonia gas atmosphere, a mixed gas atmosphere of ammonia gas and hydrogen gas, and a mixed gas atmosphere of nitrogen gas and hydrogen gas are preferred.
[0089] The magnetic material precursor may be pulverized before nitriding to obtain a magnetic material precursor powder, which may then be nitrided. By pulverizing the magnetic material precursor and then nitriding it, the crystal phase present inside the magnetic material precursor can be sufficiently nitrided. The magnetic material precursor is preferably pulverized in an inert gas atmosphere. The inert gas atmosphere may include a nitrogen gas atmosphere. This makes it possible to suppress oxidation of the magnetic material precursor during pulverization. The particle size of the magnetic material precursor powder is D 50 and may be 5 μm or more, 10 μm or more, or 15 μm or more, and may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less.
[0090] The nitriding temperature may be, for example, 673 K or more, 698 K or more, 723 K or more, or 748 K or more, and may be 823 K or less, 798 K or less, or 773 K or less. In addition, the nitriding time may be, for example, 4 hours or more, 8 hours or more, 12 hours or more, or 16 hours or more, and may be 48 hours or less, 36 hours or less, 24 hours or less, 20 hours or less, or 18 hours or less.
[0091] 《Transform》 The Sm-Fe-N magnetic material and its manufacturing method of the present disclosure are not limited to the embodiments described above, and may be modified as appropriate within the scope of the claims. For example, the Sm-Fe-N magnetic material of the present disclosure may be a powder or a compact of the powder. The compact may be a bonded compact or a sintered compact. In the case of a compact, a bonded compact is preferred from the viewpoint of easily avoiding a temperature at which nitrogen (N) in the main phase is separated (decomposed) during the molding process. Examples of the bond include resin and low-melting-point metal bond. Examples of the low-melting-point metal bond include metal zinc or zinc alloy, and combinations thereof. EXAMPLES
[0092] The Sm-Fe-N magnetic material and the manufacturing method thereof according to the present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the Sm-Fe-N magnetic material and the manufacturing method thereof according to the present disclosure are not limited to the conditions used in the following examples.
[0093] Sample preparation A sample of the Sm-Fe-N magnetic material was prepared in the following manner.
[0094] Metal Sm, metal La, metal Ce, metal Fe, metal Co, and metal Ni were mixed so that the main phase had the composition shown in Table 1, and this was melted at high frequency at 1673K (1400°C) and solidified to obtain a magnetic material precursor. During mixing, the total number of moles of Sm, La, and Ce mixed was made larger than the total number of moles of Sm, La, and Ce in the main phase so that the volume fraction of the main phase was 80 to 100%. In this specification, for example, "metal Sm" means unalloyed Sm. Of course, metal Sm, metal La, metal Ce, metal Fe, metal Co, and metal Ni may contain unavoidable impurities.
[0095] The magnetic material precursor was homogeneously heat-treated in an argon gas atmosphere at 1373 K for 24 hours.
[0096] The magnetic material precursor after the homogeneous heat treatment was placed in a glove box and pulverized in a nitrogen gas atmosphere using a cutter mill. The particle size of the pulverized magnetic material precursor powder was D 50 The average particle size was less than 20 μm.
[0097] The magnetic material precursor powder was heated to 748 K in a nitrogen gas atmosphere and nitrided for 16 hours. The amount of nitridation was determined by the change in mass of the magnetic material precursor powder before and after nitriding.
[0098] "evaluation" The composition, lattice volume, lattice constant, density, and volume fraction of the main phase were determined for each sample by the above-mentioned measurement method. In addition, the magnetic properties of each sample were measured by applying a maximum magnetic field of 9 T using a physical property processing system PPMS (registered trademark)-VSM. Regarding the measurement of magnetic properties, each sample powder after nitriding was solidified while being magnetically oriented in an epoxy resin, and the magnetic properties of each sample after solidification were measured in the easy axis direction and the hard axis direction at 300 to 453 K. The saturation magnetization was calculated from the measured value for the easy axis direction using the saturation asymptotic law. Then, the saturation magnetization Ms was calculated by dividing the saturation magnetization obtained using the saturation asymptotic law by the volume fraction of the main phase. In addition, the anisotropic magnetic field Ha was obtained from the intersection of the hysteresis curve in the easy axis direction and the hysteresis curve in the hard axis direction.
[0099] The results are shown in Table 1. In Table 1, "-" indicates that the crystal structure, density, and volume fraction of the main phase, as well as the saturation magnetization and anisotropy field, could not be measured due to poor phase stability.
[0100] [Table 1-1]
[0101] [Table 1-2]
[0102] [Table 1-3]
[0103] [Table 1-4]
[0104] FIG. 1 is a graph showing the relationship between the molar ratio x of La and the molar ratio p of Co and the phase stability. In this specification, unless otherwise specified, the phase stability means that the main phase is 2 Zinc 17 Type and Th 2 Ni17 The term "good phase stability" refers to whether or not the crystal structure of at least one of the types can be maintained. 2 Zinc 17 Type and Th 2 Ni 17 It means that the crystal structure of at least one of the two types can be maintained. 2 Zinc 17 Type and Th 2 Ni 17 This means that it is difficult to maintain at least one of the crystal structures of the two types. Fig. 2 is a graph showing the relationship between the lattice constant and the saturation magnetization Ms. Fig. 3 is a graph showing the relationship between the sum of the molar ratio x of La and the molar ratio y of Ce, and the anisotropic magnetic field Ha. Fig. 4 is a graph showing the relationship between the molar ratio x of La and the saturation magnetization Ms when the molar ratio p of Co is 0.3.
[0105] From Table 1 and Fig. 1, it can be seen that the samples of Examples 1 to 6 have improved saturation magnetization while suppressing the decrease in the anisotropic magnetic field as much as possible. On the other hand, it can be seen that the samples of Comparative Examples 1 to 14 have good phase stability but have not yet improved saturation magnetization. And the samples of Comparative Examples 15 to 33 have poor phase stability.
[0106] It can be seen from Table 1 and FIG. 2 that when the lattice constant of the main phase is 1.4350 to 1.4460, the saturation magnetization Ms is high.
[0107] As shown by the dashed line in Fig. 3, when a part of Sm is replaced with La and Ce, the anisotropy field Ha is predicted to decrease as the substitution ratio of La and Ce increases. However, it can be seen from Table 1 and Fig. 3 that the samples of Examples 1 to 6 have anisotropy field Ha higher than the anisotropy field Ha predicted from the substitution ratio of La and Ce.
[0108] From Table 1 and FIG. 4, it can be seen that when the molar ratio of Co is 0.3, in the samples of Examples 2 and 3 in which the molar ratio x of La is 0.25 or more, the decrease in the anisotropy field Ha is within a range that does not cause practical problems.
[0109] These results confirm the effects of the Sm-Fe-N based magnetic material and the manufacturing method thereof according to the present disclosure.
Claims
1. Th 2 Zinc 17 Type and Th 2 Ni 17 A Sm-Fe-N based magnetic material having a main phase having at least one of the following crystal structures: The composition of the main phase is expressed by the molar ratio formula (Sm (1-x-y-z) La x C.E. y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 N h It is expressed as R 1 is one or more rare earth elements other than Sm, La, and Ce, and Zr; M is one or more elements other than Fe, Co, Ni, and rare earth elements, and unavoidable impurity elements; and 0.25≦x+y≦0.73, 0.25≦x≦0.73, x / (x+y)≧0.80, 0≦z≦0.10, 0.10≦p+q≦0.53, p+q≧1.45(x+y)−0.5485, 0≦s≦0.10, and 2.9≦h≦3.3 Satisfying Sm-Fe-N magnetic material.
2. 2. The Sm-Fe-N based magnetic material according to claim 1, wherein said p and said q satisfy 0.22≦p+q≦0.
53.
3. 3. The Sm-Fe-N based magnetic material according to claim 1, wherein the lattice constant of the main phase is 1.4350 to 1.4460.
4. 3. The Sm—Fe—N based magnetic material according to claim 1, wherein the lattice volume of the main phase is 0.829 to 0.838 nm.
5. 3. The Sm-Fe-N based magnetic material according to claim 1, wherein the volume fraction of the main phase is 80 to 100%.
6. The density of the main phase is 7.40 to 7.76 g / cm 3 3. The Sm-Fe-N based magnetic material according to claim 1, wherein
7. A method for producing the Sm-Fe-N based magnetic material according to claim 1, Molar ratio formula (Sm (1-x-y-z) La x C.E. y R 1 z ) 2 (Fe (1-p-q-s) Co p Ni q M s ) 17 and R 1 preparing a magnetic material precursor having a crystalline phase satisfying 0.25≦x+y≦0.73, 0.25≦x≦0.73, x / (x+y)≧0.80, 0≦z≦0.10, 0.10≦p+q≦0.53, p+q≧1.45(x+y)−0.5485, and 0≦s≦0.10; nitriding the magnetic material precursor; The method for producing a Sm-Fe-N based magnetic material includes the steps of:
8. 8. The method for producing an Sm-Fe-N based magnetic material according to claim 7, wherein said p and said q satisfy 0.22≦p+q≦0.
53.
9. 9. The method for producing a Sm-Fe-N based magnetic material according to claim 7, further comprising the steps of: pulverizing the magnetic material precursor to obtain a magnetic material precursor powder; and nitriding the magnetic material precursor powder.
10. 9. The method for producing a Sm-Fe-N based magnetic material according to claim 7, wherein raw materials containing elements constituting the magnetic material precursor are melted and solidified to obtain the magnetic material precursor.
Citation Information
Patent Citations
Heterogeneous single crystal magnetic powder as well as preparation method and application thereof
CN115083715A
Magnetic material
JP1996191006A
Magnetic anisotropic agglomerate of r2t17nx magnet material, its manufacturing method, and bonded magnet
JP2002043110A
Bond magnet
JP2010062326A
Sm-Fe-N-BASED MAGNETIC MATERIAL AND MANUFACTURING METHOD THEREOF
JP2022053187A