Electrode active material composite particle, solid battery, manufacturing method for electrode active material composite particle, and manufacturing method for solid battery
By incorporating fibrous conductive materials within electrode active material composite particles, the expansion issue in negative electrodes is mitigated, enhancing the performance of solid-state batteries through reduced expansion and improved conductivity.
Patent Information
- Application Number
- JP2023067830
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-04-18
AI Technical Summary
Negative electrode active materials in batteries experience significant expansion during charging, which is not adequately addressed by existing technologies.
The use of electrode active material composite particles comprising silicon particles and a fibrous conductive material, where the fibrous conductive material is localized inside the composite particles, providing structural support and maintaining voids to suppress expansion, and the particles are produced through a spray-drying process.
The composite particles exhibit reduced expansion during charging, maintaining structural integrity and enhancing conductivity, thereby improving the performance of solid-state batteries.
Smart Images

Figure 2024154157000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrode active material composite particle, a solid-state battery, a method for producing an electrode active material composite particle, and a method for producing a solid-state battery. [Background technology]
[0002] 2. Description of the Related Art In recent years, there has been active development of batteries. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles and active materials for use in batteries is underway.
[0003] For example, Patent Document 1 discloses a negative electrode active material for use in a battery, the negative electrode active material being nonwoven particles containing silicon fibers, and the average particle diameter (D 50 ) is 0.2 μm or more and 3.6 μm or less, and the negative electrode active material is amorphous. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-022554 Summary of the Invention [Problem to be solved by the invention]
[0005] The negative electrode active material is required to have a small amount of expansion upon charging.
[0006] Therefore, an object of the present disclosure is to provide an electrode active material composite particle that exhibits small expansion upon charging, a solid-state battery having such an electrode active material composite particle, a method for producing such an electrode active material composite particle, and a method for producing a solid-state battery including producing such an electrode active material composite particle. [Means for solving the problem]
[0007] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> An electrode active material composite particle comprising silicon particles and a fibrous conductive material, The fibrous conductive material is localized inside the electrode active material composite particle. Electrode active material composite particles. <Aspect 2> 2. The electrode active material composite particle according to aspect 1, wherein the fiber diameter of the fibrous conductive material is 1000 nm or less. <Aspect 3> 3. The electrode active material composite particle according to aspect 1 or 2, wherein the fibrous conductive material is fibrous carbon. <Aspect 4> The electrode active material composite particle according to any one of aspects 1 to 3, further comprising a binder. <Aspect 5> An electrode active material layer is provided, and The electrode active material layer contains the electrode active material composite particle according to any one of aspects 1 to 4. solid state battery. <Aspect 6> A method for producing electrode active material composite particles, comprising spray drying a slurry containing silicon particles and a fibrous conductive material. Aspect 7 7. The method of claim 6, wherein the fibrous conductive material has a fiber diameter of 1000 nm or less. <Aspect 8> 8. The method of claim 6 or 7, wherein the fibrous conductive material is fibrous carbon. <Aspect 9> The method of any one of aspects 6 to 8, wherein the slurry further comprises a binder. Aspect 10 Producing an electrode active material composite particle by the method according to any one of aspects 6 to 9; and forming an electrode active material layer containing the electrode active material composite particles; How solid-state batteries are manufactured. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide an electrode active material composite particle that exhibits small expansion upon charging, a solid-state battery having such an electrode active material composite particle, a method for producing such an electrode active material composite particle, and a method for producing a solid-state battery that includes producing such an electrode active material composite particle. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is an SEM image of an electrode active material composite particle according to a reference example. [Diagram 2] FIG. 2 is an SEM-EDX image showing the cross-sectional structure of an electrode active material composite particle according to a reference example, measured using Ckα radiation. [Diagram 3] FIG. 3 is an SEM-EDX image showing the cross-sectional structure of an electrode active material composite particle according to a reference example, measured using Sikα radiation. [Figure 4] FIG. 4 is an SEM image showing the cross-sectional structure of the electrode active material composite particle according to Example 1. [Diagram 5] FIG. 5 is an SEM-EDX image showing the cross-sectional structure of the electrode active material composite particle according to Example 1, measured using Ckα rays. [Figure 6] FIG. 6 is an SEM-EDX image showing the cross-sectional structure of the electrode active material composite particle according to Example 1, measured using Sikα radiation. [Figure 7] FIG. 7 is a SEM image of the electrode active material composite particle according to Example 2. [Figure 8] FIG. 8 is an SEM-EDX image showing the cross-sectional structure of the electrode active material composite particle according to Example 2, measured using Ckα rays. [Figure 9] FIG. 9 is an SEM-EDX image showing the cross-sectional structure of the electrode active material composite particle according to Example 2, measured using Sikα radiation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0011] 《Electrode active material composite particles》 The electrode active material composite particle of the present disclosure contains silicon particles and a fibrous conductive material. In addition, in the electrode active material composite particle of the present disclosure, the fibrous conductive material is localized inside the electrode active material composite particle.
[0012] A technique using porous silicon particles is known to suppress the expansion of active materials in solid-state batteries during charging. This technique is based on the assumption that the voids inside the porous silicon particles absorb the expansion of the silicon particles, thereby suppressing the expansion.
[0013] The present inventors have found that even if porous silicon particles are used, the expansion of silicon particles may not be sufficiently suppressed. The reason for this is presumed to be as follows, without intending to be bound by any theory. That is, when manufacturing a solid-state battery, it is necessary to press an active material layer containing porous silicon for densification, and it is considered that the voids inside the porous silicon particles are partially crushed at that time. This is considered to be because there are cases where sufficient voids to absorb the expansion cannot be secured, and the expansion cannot be sufficiently suppressed.
[0014] In contrast, in the electrode active material composite particles of the present disclosure, the fibrous conductive material functions as pillars, thereby maintaining voids inside the electrode active material composite particles, which is thought to suppress expansion of the electrode active material composite particles during charging.
[0015] In addition, since the electrode active material composite particles of the present disclosure can provide high conductivity due to the fibrous conductive material, it is believed that the uniform expansion of the active material layer suppresses the expansion of the active material layer as a whole.
[0016] In the context of the present disclosure, an "electrode" may be a positive electrode or a negative electrode, and is particularly preferably a negative electrode.
[0017] <Silicon particles> The electrode active material composite particles contain silicon particles.
[0018] The composition of the silicon particles is not particularly limited. The proportion of silicon element in all elements contained in the silicon particles may be, for example, 50 mol % or more, 70 mol % or more, or 90 mol % or more.
[0019] The silicon particles may contain other elements such as Li in addition to the Si element. Examples of the other elements include Sn, Fe, Co, Ni, Ti, Cr, B, and P in addition to the Li element.
[0020] The silicon particles may contain impurities such as oxides.
[0021] The silicon particles may be amorphous or crystalline, and the crystal phase contained in the silicon particles is not particularly limited.
[0022] The shape and size of the silicon particles are not particularly limited. The average particle size of the silicon particles may be, for example, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average particle size can be determined by observation with an electron microscope such as an SEM, and is determined, for example, as the average value of the maximum Feret diameters of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. The average particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the silicon particles described later or by performing a classification process.
[0023] The silicon particles contained in the electrode active material composite particles may be porous silicon particles. The porous silicon particles contain silicon having a plurality of voids. There are no particular limitations on the shape of the voids in the porous silicon particles.
[0024] The porous silicon particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with pore diameters on the nanometer order (less than 1000 nm, preferably 100 nm or less).
[0025] The porous silicon particles may include pores having a diameter of 55 nm or less. Pores having a diameter of 55 nm or less are not easily crushed by pressing. In other words, porous silicon particles having pores having a diameter of 55 nm or less tend to maintain their porosity even after pressing. For example, 1 g of porous silicon particles may contain pores having a diameter of 55 nm or less in an amount of 0.21 cc or more, 0.22 cc / g or more, or 0.23 cc / g or more, or 0.30 cc / g or less, 0.28 cc / g or less, or 0.26 cc / g or less. The amount of pores having a diameter of 55 nm or less contained in the porous silicon particles can be determined, for example, from the pore size distribution by the nitrogen gas adsorption method or the DFT method. do.
[0026] The porous silicon particles may have a predetermined porosity. The porosity of the porous silicon particles may be, for example, 1% or more, 5% or more, 10% or more, or 20% or more, or 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less. The porosity of the silicon particles can be determined, for example, by observation using a scanning electron microscope (SEM). It is preferable that the number of samples is large, for example, 100 or more. The porosity can be an average value determined from these samples.
[0027] <Fibrous conductive material> The electrode active material composite particle of the present disclosure contains a fibrous conductive material, and the fibrous conductive material is localized inside the electrode active material composite particle.
[0028] The fiber diameter of the fibrous conductive material is preferably 1000 nm or less. When the fiber diameter of the fibrous conductive material is within the above range, sufficient voids can be maintained inside the electrode active material composite particles, and the fibrous conductive material is deformable, so that the expansion caused by charging is further reduced. In addition, the fiber diameter may be 1 nm or more, 3 nm or more, 5 nm or more, or 10 nm or more, and may be 750 nm or less, 500 nm or less, 300 nm or less, 200 nm or less, or 150 nm or less.
[0029] The fibrous conductive material is not particularly limited, but examples thereof include fibrous carbon and metal fibers. Examples of fibrous carbon include carbon nanotubes (CNTs) and vapor grown carbon fibers (VGCFs). Examples of metals constituting the metal fibers include nickel, aluminum, copper, iron, and stainless steel. The fibrous conductive material is preferably fibrous carbon, more preferably carbon nanotubes and vapor grown carbon fibers, and even more preferably carbon nanotubes. Only one type of fibrous conductive material may be used alone, or two or more types may be used in combination.
[0030] In the present disclosure, the fibrous conductive material is localized inside the electrode active material composite particle. The fact that the fibrous conductive material is localized inside the electrode active material composite particle can be confirmed by, for example, observing the cross-sectional structure by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX).
[0031] <binder> The electrode active material composite particle of the present disclosure may further contain a binder. The binder bonds a plurality of silicon particles together. The type of binder is not particularly limited. For example, the binder may be selected from butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, carboxymethyl cellulose (CMC)-based binders, polyacrylate-based binders, polyacrylic acid ester-based binders, and the like. In particular, the performance of the PVdF-based binder is high. The PVdF-based binder may be a copolymer having a unit derived from a monomer other than VdF. Only one type of binder may be used alone, or two or more types may be used in combination.
[0032] The mass ratio of the silicon particles, fibrous conductive material, and binder contained in the electrode active material composite particles (silicon particles:fibrous conductive material:binder) is not particularly limited as long as it is sufficient to form the electrode active material composite particles. For example, the ratio of silicon particles:fibrous conductive material:binder may be 100:5-15:0.1-10.
[0033] The average particle diameter of the electrode active material composite particles is not particularly limited. The average particle diameter of the electrode active material composite particles may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 20 μm or less, 15 μm or less, or 10 μm or less. The average particle diameter of the electrode active material composite particles can be obtained by observation with an electron microscope such as SEM, and is obtained, for example, as the average value of the maximum Feret diameters of a plurality of electrode active material composite particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. Alternatively, the average particle diameter (D50, median diameter) of the electrode active material composite particles measured by taking out only the electrode active material composite particles and using a laser diffraction type particle distribution measuring device may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 20 μm or less, 15 μm or less, or 10 μm or less.
[0034] <<Method for producing electrode active material composite particles>> The disclosed method of making electrode active material composite particles includes spray drying a slurry containing silicon particles and a fibrous conductive material.
[0035] For the silicon particles and the fibrous conductive material, reference can be made to the above descriptions regarding the electrode active material composite particles of the present disclosure.
[0036] The slurry may further contain a binder. For the binder, reference may be made to the above description regarding the electrode active material composite particles of the present disclosure.
[0037] As the method for spray drying, a conventional method can be adopted.
[0038] For example, the slurry may be sprayed into a spray dryer into which an inert gas at 100° C. to 180° C. has been introduced, and dried.
[0039] In this case, the temperature may be 110°C or more, 120°C or more, or 130°C or more, and may be 170°C or less, 160°C or less, or 150°C or less.
[0040] Examples of the inert gas include, but are not limited to, nitrogen and argon.
[0041] 《Solid-state battery》 The solid-state battery of the present disclosure has an electrode active material layer. The electrode active material layer contains the electrode active material composite particle of the present disclosure. In particular, the solid-state battery of the present disclosure preferably contains the electrode active material composite particle of the present disclosure as the negative electrode active material. In this case, the solid-state battery may have a negative electrode current collector layer, a negative electrode active material layer containing the electrode active material composite particle of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer in this order. A solid-state battery refers to a battery in which an electrolyte having carrier ion conductivity is mainly composed of a solid electrolyte. However, a liquid component may be included at the additive level. Alternatively, the solid-state battery may be an all-solid-state battery that does not substantially contain a liquid component.
[0042] <Negative electrode current collector layer> As the negative electrode current collector, any common negative electrode current collector for solid-state batteries can be used.
[0043] The negative electrode current collector may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, a metal foil is excellent in terms of ease of handling. The negative electrode current collector may be made of a plurality of foils or sheets.
[0044] Examples of metals constituting the negative electrode current collector include copper, nickel, chromium, gold, platinum, silver, aluminum, iron, titanium, zinc, cobalt, stainless steel, etc. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector may contain at least one metal selected from copper, nickel, and stainless steel.
[0045] The negative electrode current collector may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. The negative electrode current collector may be a metal foil or a base material on which the above-mentioned metal is plated or vapor-deposited. When the negative electrode current collector is made of multiple sheets of metal foil, some kind of layer may be present between the multiple sheets of metal foil.
[0046] The thickness of the negative electrode current collector is not particularly limited and may be, for example, 0.1 μm or more, or 1 μm or more, and may be 1 mm or less, or 100 μm or less.
[0047] <Negative electrode active material layer> The negative electrode active material layer contains at least electrode active material composite particles as a negative electrode active material, and may further contain, optionally, a negative electrode active material other than the electrode active material composite particles, a solid electrolyte, a conductive assistant, a binder, etc. The negative electrode active material layer may also contain various other additives.
[0048] (Negative electrode active material)
[0049] The negative electrode active material layer contains electrode active material composite particles as a negative electrode active material. For the electrode active material composite particles, the above description of the electrode active material composite particles of the present disclosure can be referred to.
[0050] The negative electrode active material layer may contain a negative electrode active material other than the electrode active material composite particles. In this case, the proportion of the electrode active material composite particles in the total negative electrode active material may be, for example, 50% by weight or more, 70% by weight or more, or 90% by weight or more.
[0051] The proportion of the negative electrode active material in the negative electrode active material layer may be, for example, 20% by weight or more, 30% by weight or more, or 40% by weight or more, and may be 80% by weight or less, 70% by weight or less, or 60% by weight or less.
[0052] (solid electrolyte) Typical examples of the solid electrolyte include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes, and organic polymer electrolytes such as polymer electrolytes.
[0053] Examples of sulfide solid electrolytes having lithium ion conductivity include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and halogen elements. Examples of halogen elements include F, Cl, Br, and I.
[0054] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is P, Si, Ge, B, Al, Ga, or In.)
[0055] Examples of oxide solid electrolytes having lithium ion conductivity include solid electrolytes containing Li, Y (Y is at least one of Nb, B, Al, Si, P, Ti, Zr, Mo, W, and S), and O. A specific example is Li7La3Zr2O 12 , Li 7-x La3(Zr 2-x Nb x )O 12 (0≦x≦2), Li5La3Nb2O 12perovskite-type solid electrolytes such as (Li,La)TiO3, (Li,La)NbO3, (Li,Sr)(Ta,Zr)O3; Nasicon-type solid electrolytes such as Li(Al,Ti)(PO4)3 and Li(Al,Ga)(PO4)3; Li-PO-based solid electrolytes such as Li3PO4 and LIPON (a compound in which some of the O in Li3PO4 is replaced with N); and Li-BO-based solid electrolytes such as Li3BO3 and a compound in which some of the O in Li3BO3 is replaced with C.
[0056] The proportion of the solid electrolyte in the negative electrode active material layer may be 1 wt % or more, 10 wt % or more, or 20 wt % or more, and may be 60 wt % or less, or 50 wt % or less.
[0057] (Conductive assistant) Examples of the conductive assistant include carbon materials and metal particles. Specific examples of the carbon materials include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF). Examples of the metal particles include nickel, copper, iron, and stainless steel. The proportion of the conductive assistant in the negative electrode active material layer may be 1% by weight or more, or 5% by weight or more, and may be 30% by weight or less, or 20% by weight or less.
[0058] (binder) Examples of the binder include rubber-based binders such as butadiene rubber, hydrogenated butadiene rubber, styrene butadiene rubber (SBR), hydrogenated styrene butadiene rubber, nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, and ethylene propylene rubber; fluoride-based binders such as polyvinylidene fluoride (PVDF), polyvinylidene fluoride-polyhexafluoropropylene copolymer (PVDF-HFP), polytetrafluoroethylene, and fluorine-containing rubber; thermoplastic polyolefin resins such as polyethylene, polypropylene, and polystyrene; imide resins such as polyimide and polyamideimide; amide resins such as polyamide; acrylic resins such as polymethyl acrylate and polyethyl acrylate; and methacrylic resins such as polymethyl methacrylate and polyethyl methacrylate. The proportion of the binder in the negative electrode active material layer is, for example, 1% by weight or more and 30% by weight or less.
[0059] The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0060] <Solid electrolyte layer> The solid electrolyte layer contains at least a solid electrolyte, and may further contain, optionally, a binder and the like.
[0061] For the solid electrolyte and the binder, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.
[0062] The thickness of the solid electrolyte layer is, for example, not less than 0.1 μm and not more than 1000 μm.
[0063] <Cathode active material layer> The positive electrode active material layer contains at least a positive electrode active material, and may further contain, optionally, a solid electrolyte, a conductive assistant, a binder, and the like.
[0064] Examples of the positive electrode active material include oxide active materials. Examples of oxide active materials used in lithium ion batteries include LiCoO2, LiMnO2, Li2NiMn3O8, LiVO2, LiCrO2, LiFePO4, LiCoPO4, LiNiO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc. Also, on the surface of these active materials, for example, a coating layer containing a Li-ion conductive oxide such as LiNbO3, etc. may be formed.
[0065] The proportion of the positive electrode active material in the positive electrode active material layer may be 20% by weight or more, 30% by weight or more, or 40% by weight or more, and may be 80% by weight or less, 70% by weight or less, or 60% by weight or less.
[0066] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0067] <Positive electrode current collector layer> The positive electrode current collector can be any of those generally used as a positive electrode current collector for solid-state batteries. The positive electrode current collector may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The positive electrode current collector may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode current collector may be made of a plurality of foils.
[0068] Examples of metals constituting the positive electrode current collector include copper, nickel, chromium, gold, platinum, silver, aluminum, iron, titanium, zinc, cobalt, stainless steel, etc. In particular, from the viewpoint of ensuring oxidation resistance, etc., the positive electrode current collector may contain aluminum.
[0069] The positive electrode current collector may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. The positive electrode current collector may be a metal foil or a substrate on which the above-mentioned metal is plated or vapor-deposited. When the positive electrode current collector is made of multiple sheets of metal foil, some kind of layer may be present between the multiple sheets of metal foil.
[0070] The thickness of the positive electrode current collector is not particularly limited and may be, for example, 0.1 μm or more, or 1 μm or more, and may be 1 mm or less, or 100 μm or less.
[0071] <Other configurations> The solid-state battery may be one in which each of the above-mentioned components is housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. In addition, a plurality of solid-state batteries may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The solid-state battery may also have other obvious components such as necessary terminals. Examples of the shape of the solid-state battery include a coin type, a laminate type, a cylindrical type, and a square type.
[0072] <<Method for manufacturing solid-state batteries>> A method of the present disclosure for producing a solid-state battery includes producing an electrode active material composite particle of the present disclosure, and forming a negative electrode active material layer containing the electrode active material composite particle.
[0073] For the method for producing the electrode active material composite particles of the present disclosure, the above description regarding the method for producing the electrode active material composite particles of the present disclosure can be referred to.
[0074] An example of a method for forming a negative electrode active material layer containing electrode active material composite particles is a method in which constituent materials such as the electrode active material composite particles are mixed to obtain a negative electrode mixture, and the obtained negative electrode mixture is compacted into a powder form.
[0075] The method of the present disclosure for manufacturing a solid-state battery may further include stacking an anode current collector, an anode active material layer, a solid electrolyte layer, a cathode active material layer, and a cathode current collector in this order. Here, the laminate may be press-molded. Other members such as terminals may be attached to the laminate as necessary. The laminate is housed in a battery case and sealed to obtain a solid-state battery. EXAMPLES
[0076] Preparation of nanoporous silicon particles 0.65g of silicon (Si) particles (particle size 0.5μm, manufactured by Kojundo Chemical) and 0.60g of metallic lithium (Li) (manufactured by Honjo Metal) were mixed in an agate mortar under an argon (Ar) atmosphere to obtain a lithium silicon (LiSi) precursor. In a glass reactor under an Ar atmosphere, 1.0g of the obtained LiSi precursor and 125ml of 1,3,5-trimethylbenzene (manufactured by Nacalai Tesque) as a dispersion medium were mixed using an ultrasonic homogenizer (UH-50, manufactured by SMT). The obtained LiSi precursor dispersion was then cooled to 0°C, and 125ml of ethanol (manufactured by Nacalai Tesque) was dripped and reacted for 120 minutes. After the reaction, 50ml of acetic acid (manufactured by Nacalai Tesque) was further dripped and reacted for 60 minutes. After the reaction, the liquid and solid reactants were separated by suction filtration. The obtained solid reactant was vacuum dried at 120°C for 2 hours to obtain nanoporous silicon particles.
[0077] <Preparation of Electrode Active Material Composite Particles> (Reference example) The nanoporous silicon particles, PVDF-HFP (Kureha) as a binder, and carbon black (CB) as a conductive material were dispersed in dimethyl carbonate (Nacalai Tesque) to obtain a ratio (mass ratio) of silicon particles: binder: CB = 100: 13.3: 20 to obtain a slurry. This slurry was sprayed and dried in a spray dryer in a nitrogen gas atmosphere under the condition of 140 ° C. As a result, the electrode active material composite particles of the reference example were obtained.
[0078] Example 1 The nanoporous silicon particles, PVDF-HFP (Kureha) as a binder, and carbon nanotubes (CNT) (fiber diameter: about 10 nm) as a fibrous conductive material were dispersed in dimethyl carbonate (Nacalai Tesque) to obtain a ratio (mass ratio) of silicon particles: binder: CNT = 100: 13.3: 0.4 to obtain a slurry. This slurry was sprayed and dried in a spray dryer in a nitrogen gas atmosphere under a condition of 140 ° C. As a result, the electrode active material composite particles of Example 1 were obtained.
[0079] Example 2 The nanoporous silicon particles, PVDF-HFP (Kureha) as a binder, and vapor grown carbon fiber (VGCF) (fiber diameter: 150 nm) as a fibrous conductive material were dispersed in dimethyl carbonate (Nacalai Tesque) to obtain a ratio (mass ratio) of silicon particles: binder: VGCF = 100: 13.3: 8 to obtain a slurry. This slurry was sprayed and dried in a spray dryer in a nitrogen gas atmosphere under the condition of 140 ° C. As a result, the electrode active material composite particles of Example 2 were obtained.
[0080] Comparative Example 1 The nanoporous silicon particles and PVDF-HFP (Kureha) as a binder were dispersed in dimethyl carbonate (Nacalai Tesque) so that the ratio (mass ratio) of silicon particles to binder was 100:13.3 to obtain a slurry. The slurry was sprayed and dried in a spray dryer in a nitrogen gas atmosphere under a condition of 140°C. Thus, the electrode active material composite particles of Comparative Example 1 were obtained.
[0081] (Preparation of solid electrolyte) 0.550g of lithium sulfide (Li2S) (Furuuchi Chemical), 0.887g of phosphorus pentasulfide (P2S5) (Aldrich), 0.285g of lithium iodide (LiI) (Nippo Chemical), and 0.277g of lithium bromide (LiBr) (Kojundo Chemical) were mixed in an agate mortar for 5 minutes. 4g of n-heptane (dehydrated grade, Kanto Chemical) was added to the resulting mixture, and mechanical milling was performed for 40 hours using a planetary ball mill to obtain a solid electrolyte.
[0082] (Preparation of evaluation battery) Lithium Nickel Cobalt Manganese Oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A cathode active material was obtained by surface-treating lithium niobate (LiNbO3) on a cathode active material. 1.5 g of this cathode active material, 0.023 g of a conductive additive (VGCF, Showa Denko), 0.239 g of the above solid electrolyte, 0.011 g of a binder (PVdF, Kureha), and 0.8 g of butyl butyrate (Kishida Chemical) were mixed using an ultrasonic homogenizer (UH-50, SMT) to obtain a cathode composite.
[0083] 1.0 g of the electrode active material composite particles of each of the above examples, 0.04 g of a conductive additive (VGCF, manufactured by Showa Denko), 0.776 g of the above solid electrolyte, 0.02 g of a binder (PVdF, manufactured by Kureha), and 1.7 g of butyl butyrate (manufactured by Kishida Chemical) were mixed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a negative electrode mixture.
[0084] 1cm 2 0.065 g of the above solid electrolyte was placed in a ceramic mold at 1 ton / cm 2 The solid electrolyte layer was prepared by pressing the positive electrode mixture (0.018 g) on one side of the solid electrolyte layer at a pressure of 1 ton / cm. 2 The positive electrode active material layer was prepared by pressing the negative electrode mixture (0.0054 g) at a pressure of 4 ton / cm. 2 The negative electrode active material layer was prepared by pressing the positive electrode current collector with a pressing machine. An aluminum foil was used as the positive electrode current collector, and a copper foil was used as the negative electrode current collector. In this manner, an all-solid-state battery was prepared as a battery for evaluation.
[0085] <evaluation> (Microscopic Observation) The cross-sectional structures of the electrode active material composite particles obtained in the Reference Example and Examples 1 and 2 were observed by a scanning electron microscope (SEM) and a scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX).
[0086] (Increase in confining pressure) The obtained evaluation battery was CC / CV charged at 0.245 mA to 4.55 V, and then CC / CV discharged at 0.245 mA to 3.0 V. In the first charge, the battery's restraint pressure was monitored, and the restraint pressure at 4.55 V was measured. The increase in the restraint pressure was used as an index of the magnitude of expansion. The restraint pressure in Comparative Example 1 was set to 1.00, and a relative evaluation was performed.
[0087] <result> Images of the electrode active material composite particles of each example observed by SEM are shown in Figures 1, 4, and 7, and images showing the cross-sectional structure of the electrode active material composite particles of each example observed by SEM-EDX are shown in Figures 2, 3, 5, 6, 8, and 9. Table 1 also shows the results of the increase in confining pressure of the all-solid-state batteries produced using the electrode active material composite particles of each example.
[0088] [Table 1]
[0089] As shown in Figures 1 to 3, in the electrode active material composite particles of the Reference Example in which the conductive material is particulate, the silicon particles and the conductive material were uniformly dispersed. In contrast, as shown in Figures 4 to 6 and Figures 7 to 9, in the electrode active material composite particles of the Examples in which the conductive material is fibrous, the conductive material was localized inside the electrode active material composite particles.
[0090] Furthermore, as shown in Table 1, the batteries of Examples 1 and 2 had a smaller increase in confining pressure, i.e., a smaller expansion, than the battery of Comparative Example 1. In particular, the battery of Example 1, in which the fiber diameter of the fibrous conductive material was smaller, had the smallest expansion.
Claims
1. An electrode active material composite particle comprising silicon particles and a fibrous conductive material, The fibrous conductive material is localized inside the electrode active material composite particle. Electrode active material composite particles.
2. 2. The electrode active material composite particle according to claim 1, wherein the fiber diameter of the fibrous conductive material is 1000 nm or less.
3. 2. The electrode active material composite particle according to claim 1, wherein the fibrous conductive material is fibrous carbon.
4. The electrode active material composite particle according to claim 1 , further comprising a binder.
5. An electrode active material layer is provided, and The electrode active material layer contains the electrode active material composite particle according to any one of claims 1 to 4. solid state battery.
6. A method for producing electrode active material composite particles, comprising spray drying a slurry containing silicon particles and a fibrous conductive material.
7. The method according to claim 6 , wherein the fiber diameter of the fibrous conductive material is 1000 nm or less.
8. The method of claim 6 wherein the fibrous conductive material is fibrous carbon.
9. The method of claim 6 , wherein the slurry further comprises a binder.
10. Producing an electrode active material composite particle by the method according to any one of claims 6 to 9; and forming an electrode active material layer containing the electrode active material composite particles; How solid-state batteries are manufactured.
Citation Information
Patent Citations
Silicon-carbon composite, a method for preparing said composite, and an electrode material and a battery comprising said composite
CN107112504A
Nanometer silicon / carbon nanotube microsphere / graphite composite structure negative electrode material and preparation method thereof
CN111180712A
Electrode material and method of manufacturing the same, and negative electrode for nonaqueous secondary battery and nonaqueous secondary battery
JP2003303588A
Electrode material and its manufacturing method, and nonaqueous secondary battery and its manufacturing method
JP2005135925A
Lithium-ion cell and anode therefor
JP2019511103A
Cited By
Hydrogen generating device
CN121648844A