Substrate, method for manufacturing the same, and method for manufacturing liquid discharge head

By using a mask pattern layer and etching inhibitor layer with varying thicknesses, the method addresses the challenge of achieving precise recess shapes in silicon substrates for liquid ejection heads, resulting in high accuracy and reduced complexity.

JP2024154158APending Publication Date: 2024-10-30CANON KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023067831
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Existing methods for forming recesses in silicon substrates for liquid ejection heads face challenges in achieving precise control over the bottom shape, leading to issues such as insufficient volume, uneven depth, and increased complexity due to the use of etching stop layers.

Method used

A method involving the formation of a mask pattern layer and an etching inhibitor layer with varying thicknesses is employed to control the etching process, ensuring the bottom surface of recesses is flat and precise by adjusting the thickness of the etching inhibitor layer continuously or intermittently from the center to the edge of the opening.

Benefits of technology

This approach allows for the production of substrates with high depth accuracy and controlled bottom shapes, reducing manufacturing complexity and enhancing the suitability of the substrates for liquid ejection heads by preventing curvature and ensuring adequate volume.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154158000001_ABST
    Figure 2024154158000001_ABST
Patent Text Reader

Abstract

To manufacture a substrate having a recess highly accurately controlled in a bottom shape.SOLUTION: A method for manufacturing a substrate 1 comprises steps of: forming a mask pattern layer 4 having an opening 4a on one surface 1a of a substrate material 1c; forming an etching obstacle layer 5 on the one surface 1a on which the mask pattern layer 4 has been formed; and etching the etching obstacle layer 5 and the substrate material 1c inside the opening 4a to form a recess 2 in the substrate material 1c. The thickness of the etching obstacle layer 5 in a direction orthogonal to the one surface 1a inside the opening 4a before the step of forming the recess 2 gets continuously or intermittently thinner from a center position C of the opening 4a toward an inner peripheral edge E of the opening 4a.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate, a method for manufacturing the same, and a method for manufacturing a liquid ejection head. [Background technology]

[0002] In silicon substrates used as ejection port forming members of liquid ejection heads, fine structures such as flow paths are formed by the Bosch process, which alternates between dry etching and the formation of an etching inhibitor layer. When a recess is formed by anisotropic dry etching in the Bosch process, it is difficult to make the bottom and side (inner circumferential surface) of the recess completely perpendicular, and the bottom tends to be curved. In the invention described in Patent Document 1, part of the bottom of the supply path is intentionally formed to be curved. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-235828 Summary of the Invention [Problem to be solved by the invention]

[0004] When forming a recess by dry etching a silicon substrate, it is difficult to achieve the accuracy required for a flow path of a liquid ejection head. If at least a part of the bottom surface of the recess is curved, the recess may not be suitable for a flow path of a liquid ejection head due to insufficient volume of the recess or uneven depth within one recess. Therefore, it is possible to form an etching stop layer inside the silicon substrate in advance and then etch it to remove the area where the bottom surface is curved and make the bottom surface of the recess flat. However, in that case, the number of steps increases for forming and removing the etching stop layer, making the manufacturing method complicated. In the invention described in Patent Document 1, the curved part of the inner surface of the flow path is used to stabilize the displacement operation of the movable member and the growth of the bubble, but it is not easy to achieve high depth accuracy in a flow path having such a curved part.

[0005] SUMMARY OF THE PRESENTLY PREFERRED EMBODIMENTS An object of the present invention is to provide a substrate having a recess whose bottom shape is controlled with high precision, a method for manufacturing the same, and a method for manufacturing a liquid ejection head. [Means for solving the problem]

[0006] The method for manufacturing a substrate of the present invention includes the steps of forming a mask pattern layer having an opening on one side of a substrate material, forming an etching inhibitor layer on the one side on which the mask pattern layer is formed, and etching the etching inhibitor layer and the substrate material inside the opening to form a recess in the substrate material, and is characterized in that the thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one side prior to the step of forming the recess is continuously or intermittently thinner from the center position of the opening toward the inner peripheral edge of the opening. Effect of the Invention

[0007] According to the present invention, it is possible to obtain a substrate having a recess whose bottom surface shape is controlled with high precision, and a liquid ejection head having the same. [Brief description of the drawings]

[0008] [Figure 1] 1A and 1B are a schematic plan view and a cross-sectional view illustrating a substrate according to a first embodiment of the present invention. [Diagram 2] 2A to 2C are schematic cross-sectional views sequentially showing main steps of a method for manufacturing the substrate shown in FIG. [Diagram 3] 1A to 1C are schematic cross-sectional views sequentially showing main parts of a method for manufacturing a substrate according to a comparative example. [Figure 4] 5A and 5B are schematic plan and cross-sectional views illustrating a liquid ejection head according to a second embodiment of the present invention. [Diagram 5] 5A to 5C are schematic cross-sectional views sequentially showing main steps of a method for manufacturing the liquid ejection head shown in FIG. [Figure 6] 5A and 5B are schematic plan and cross-sectional views illustrating a liquid ejection head according to a third embodiment of the present invention. [Figure 7] 5A to 5C are schematic cross-sectional views sequentially showing main parts of a method for manufacturing a substrate according to a second embodiment of the present invention. [Figure 8] 10A to 10C are schematic cross-sectional views sequentially illustrating main steps of a manufacturing method for a liquid ejection head according to a third embodiment of the present invention. [Figure 9] 10A to 10C are schematic cross-sectional views sequentially illustrating main parts of a manufacturing method for a liquid ejection head according to a fourth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, several embodiments of the present invention will be described with reference to the drawings. However, the following description does not limit the scope of the present invention. The substrate of the present invention can be widely used in printers, copiers, facsimiles with communication systems, word processors and portable electronic devices with printer units, industrial devices combined with various processing devices, etc. In the embodiments described below, as an example, an example is shown in which the present invention is applied to a liquid ejection head that employs a thermal method, a piezoelectric method, or various other liquid ejection methods.

[0010] [First embodiment] Fig. 1(a) is a schematic plan view of a substrate 1 manufactured in a first embodiment of the present invention, and Fig. 1(b) is a schematic side cross-sectional view thereof. The substrate 1 is a silicon substrate, and a recess 2 is formed on one surface (first surface) 1a. The recess 2 is a bottomed hole that does not penetrate the substrate 1, and its depth is 100 µm or less. As shown in Fig. 1(b), the bottom surface 3 of the recess 2 is flat, not curved.

[0011] <Substrate manufacturing method> Hereinafter, a method for manufacturing the substrate 1 of this embodiment, particularly a method for forming the bottom surface 3 of the recess 2 in a flat surface shape, will be described with reference to FIGS. 2(a) to 2(e), which are cross-sectional views seen from the same direction as FIG. 1(b). In this specification, the state before the completion of the substrate 1 is referred to as the substrate material 1c. As shown in FIG. 2(a), a mask pattern layer 4 including an opening 4a provided at a position where the recess 2 is to be formed is formed on one surface (first surface) 1a of the silicon substrate material 1c. The mask pattern layer 4 may be formed of a silicon oxide film or a silicon nitride film, but is preferably formed of a resist layer made of a photoresist so that the number of steps for patterning is not increased too much. Furthermore, as shown in FIG. 2(b), an etching inhibitor layer 5 is formed on the first surface 1a on which the mask pattern layer 4 is formed. The etching inhibitor layer 5 is formed both in the opening 4a of the mask pattern layer 4 and on the mask pattern layer 4. The etching inhibitor layer 5 is formed so that its thickness in the direction perpendicular to the first surface 1a decreases continuously or intermittently from the center position C in the opening 4a toward the outside, i.e., toward the inner periphery E of the opening 4a. As an example, the etching inhibitor layer 5 is a layer made of a material having a different composition from the mask pattern layer 4, such as a CF-based polymer film.

[0012] In this manner, etching is performed with the mask pattern layer 4 and the etching inhibitor layer 5 formed on the first surface 1a of the substrate material 1c to form the recess 2. During the process of forming the recess 2, the etching inhibitor layer 5 inside the opening is removed and the substrate material 1c is etched. In the opening 4a, the initial etching rate in the direction perpendicular to the first surface 1a changes depending on the thickness of the etching inhibitor layer 5, so that the amount of etching of the substrate material 1c varies depending on the position. In this embodiment, the shape of the bottom surface 3 of the recess 2 formed in the substrate material 1c is controlled by appropriately adjusting the thickness of the etching inhibitor layer 5. As shown in FIG. 2(b), the etching inhibitor layer 5 of this embodiment is thick at the center position C in the opening 4a and gradually becomes thinner toward the inner peripheral edge portion E located around it. That is, the thickness of the etching inhibitor layer 5 becomes thinner the further away from the center position C of the opening 4a. The bottom surface 3 of the recess 2 formed after removing the etching inhibitor layer 5 by etching is high at the center position C in the opening 4a and gradually lowers toward the inner peripheral edge E located around it, as shown in FIG. 2(c). Then, in the recess 2, a Bosch process is performed in which the deposition of the latter-stage etching inhibitor layer 6 (which may be a layer having a uniform thickness) shown in FIG. 2(d) and reactive ion etching are alternately repeated multiple times. As a result, the bottom surface 3 of the recess 2 becomes flat as shown in FIG. 2(e). In this embodiment, the shape of the bottom surface 3 of the recess 2 can be controlled in this way, and the bottom surface 3 can be flattened. After that, the mask pattern layer 4 is removed, and a substrate 1 having a recess 2 with high depth accuracy can be manufactured as shown in FIG. 1.

[0013] In this embodiment, the technical significance of forming the etching inhibitor layer 5 with an adjusted thickness will be described. When the Bosch process is performed by alternately repeating the formation of an etching inhibitor layer whose main component is carbon and whose thickness is uniform, and reactive ion etching, the etching rate varies depending on the position in the opening 4a. As a result, it is difficult to make the bottom surface 3 and the side surface (inner peripheral surface) 12 of the recess 2 perfectly perpendicular, and the bottom surface 3 of the recess 2 is likely to be curved rather than flat. If the bottom surface 3 of the recess 2 is curved, problems occur such as insufficient volume of the recess 2 and uneven depth within one recess 2. Therefore, in this embodiment, after etching using an etching inhibitor layer 5 with an appropriately adjusted thickness, the formation of the latter-stage etching inhibitor layer 6 and reactive ion etching are alternately repeated, so that the bottom surface 3 of the recess 2 of the substrate 1 can be easily flattened. As a result, the volume of the recess 2 is prevented from decreasing, and the area in which the bottom surface 3 is curved is eliminated or limited, thereby improving the depth precision of the recess 2.

[0014] In this embodiment, by using the etching inhibitor layer 5 whose thickness has been adjusted as described above, the bottom surface of the recess 2 is formed in a shape that cancels the difference in the amount of etching in the repeated formation of the latter-stage etching inhibitor layer 6 and the subsequent dry etching. For this purpose, the variation in the amount of etching in the repeated formation of the latter-stage etching inhibitor layer 6 and the subsequent dry etching is estimated in advance, and the difference in the thickness of the etching inhibitor layer 5 in the opening 4a is determined based on the estimation. Such a difference in the thickness of the etching inhibitor layer 5 in the opening 4a causes a difference in the etching rate of the substrate material 1c, and as shown in FIG. 2(c), a recess 2 is formed that is shallow at the center position C in the opening 4a and becomes deeper toward the inner periphery E. When the formation of the flat latter-stage etching inhibitor layer 6 and the dry etching are then alternately repeated, the amount of etching of the shallow part of the recess 2 at the center position C in the opening 4a is large and the amount of etching of the deep part of the inner periphery E is small, so that the bottom surface 3 of the recess 2 becomes flat. When the repetition of the formation of the latter-stage etching inhibitor layer 6 and the dry etching is stopped in this state, the recess 2 with the bottom surface 3 in a flat surface shape is completed. That is, in this embodiment, the difference in thickness of the etching inhibitor layer 5 inside the opening 4a is set so as to offset the difference in the amount of etching inside the opening 4a in the repetition of the formation of the latter-stage etching inhibitor layer 6 and the subsequent dry etching (Bosch process). The difference in thickness of the etching inhibitor layer 5 inside the opening 4a causes a difference in the etching rate of the substrate material 1c. As a result, the bottom surface 3 becomes flat after the Bosch process. The substrate 1 of this embodiment, which is manufactured in this way and has a flat bottom surface 3, can be suitably used as a substrate for a liquid ejection head, for example, as an ejection port forming member. However, the substrate 1 of this embodiment can also be widely used as a substrate for various other electronic devices, etc.

[0015] <Modification> In the above-mentioned example, as shown in Figures 2(d) to 2(e), reactive ion etching and the formation of a subsequent-stage etching inhibitor layer 6 are alternately repeated to flatten the bottom surface 3 of the recess 2. However, as shown in Figure 2(c), when the recess 2 is formed, which is shallow at the center position C in the opening 4a and gradually becomes deeper toward the inner peripheral edge portion E located around it, the process can be terminated without further etching or the formation of the subsequent-stage etching inhibitor layer 6. In this case, since the recess 2 has a bottom surface 3 with a characteristic shape, this recess 2 can be effectively used as an alignment mark for positioning, etc., which is intentionally improved in visibility and recognition rate.

[0016] <Comparative Example> Next, a comparative example to be compared with the present invention will be described with reference to FIG. 3. FIGS. 3(a) to 3(c) are cross-sectional views seen from the same direction as FIG. 1(b), showing a method for forming a recess 2 having a flat bottom surface 3 in this comparative example. In this comparative example, in order to flatten the bottom surface 3 of the recess 2, a protective layer (etching stop layer) 7 is formed in advance inside the substrate material 1c, as shown in FIG. 3(a). The protective layer 7 is made of a material having a high etching selectivity with respect to silicon constituting the substrate material 1c, and may be, for example, a silicon oxide film or a silicon nitride film. A mask pattern layer 4 having an opening 4a is formed on one surface (first surface) 1a of this substrate material 1c. Then, reactive ion etching and the formation of an etching inhibitor layer (not shown, but may be a layer having a uniform thickness) are alternately repeated. During this repetition, the bottom surface 3 of the recess 2 is curved, as shown in FIG. 3(b). Thereafter, when reactive ion etching and the formation of an etching inhibitor layer are repeated until the region where the bottom surface 3 is curved is removed, the bottom surface 3 of the recess 2 becomes flat as shown in FIG. 3(c). The bottom surface 3 at this time is a part of the protective layer 7. In this way, the recess 2 with the flat bottom surface 3 can be formed in the substrate material 1c in this comparative example as well. However, there is a problem that the number of steps increases due to the formation and removal of the protective layer 7, and the manufacturing method becomes complicated especially due to the step of forming the protective layer 7. In addition, the protective layer 7 is also etched to a certain extent and becomes thin. When this protective layer 7 is used as a layer that exerts some function (for example, a protective layer for a vibration plate in a pressure chamber of a liquid ejection head), the function may be deteriorated by the thinning of the protective layer 7. Thus, according to this comparative example, even if a certain degree of high depth accuracy is realized, it is not preferable because new problems such as an increase in the number of steps and a thinning of the protective layer arise.

[0017] [Second embodiment] The second embodiment of the present invention relates to a liquid ejection head 8 incorporating a substrate 1 similar to that of the first embodiment. FIG. 4(a) is a schematic plan view showing the ejection port forming surface of the liquid ejection head 8 of this embodiment, and FIG. 4(b) is a schematic cross-sectional view cut along the line AA in FIG. 4(a). FIG. 5 is a schematic cross-sectional view showing in order some steps of a manufacturing method of the liquid ejection head 8. The main part of the liquid ejection head 8 shown in FIG. 4 has a laminated structure of three substrates (a first substrate 1, a second substrate 9, and a third substrate 10). The first to third substrates 1, 9, and 10 are all mainly made of silicon substrates. The first substrate 1 shown in FIG. 5(a) is an example of the substrate of the present invention, and is a member having the aforementioned recess 2 formed as a flow path 2a and a clearance groove 2b on one surface (a first surface) 1a, and an ejection port 11 formed thereon that communicates with the flow path 2a and opens to the other surface (a second surface) 1b. The depth of the discharge port 11 is 30 μm or less, and the depth of the flow path 2a and the escape groove 2b is 100 μm or less. The manufacturing method of the first substrate 1 is as described above. As shown in FIG. 2(a), a mask pattern layer 4 having an opening 4a is formed on one surface 1a of the substrate material 1c. Then, as shown in FIG. 2(b), an etching inhibitor layer 5 is formed, which is thick at the center position C in the opening 4a and gradually becomes thinner toward the inner periphery E. Then, etching is performed to form the recess 2 (flow path 2a and escape groove 2b) as shown in FIG. 2(c). Furthermore, the formation of a flat rear-stage etching inhibitor layer 6 shown in FIG. 2(d) and reactive ion etching are alternately repeated multiple times to make the bottom surface 3 of the recess 2 (flow path 2a and escape groove 2b) flat as shown in FIG. 2(e). Then, a discharge port 11 is formed that communicates with the flow path 2a and opens on the other surface. In this manner, the first substrate 1 shown in FIG. 5(a) is manufactured.

[0018] The second substrate 9 shown in FIG. 5(b) has a silicon substrate 20, which is a main part, a vibration plate 13 made of, for example, silicon, a protective layer 7 made of, for example, a silicon oxide film, and a piezoelectric element 14, which are located on one surface (first surface) 9a side. The piezoelectric element 14 is a type of energy generating element that generates energy for ejecting liquid, and is made of, for example, lead zirconate titanate, and is fixed to the vibration plate 13. A second supply path 15, which is a through hole, is formed in the protective layer 7 and the vibration plate 13. Furthermore, although not shown, wiring connected to the piezoelectric element 14, and a drive circuit and a connection terminal 29 (see FIG. 4(a)) connected to the wiring are formed on the first surface 9a side of the second substrate 9. A pressure chamber 16 communicating with the second supply path 15 is formed on the other surface (second surface) 9b of the second substrate 9. The depth of the pressure chamber 16 is 200 μm or less.

[0019] 5(c) is formed with a first supply path 17, which is a through hole penetrating from one surface (first surface) 10a to the other surface (second surface) 10b. A recess 18 is formed on the second surface 10b of the third substrate 10, facing a portion of the vibration plate 13 of the second substrate 9 where the piezoelectric element 14 is fixed.

[0020] As shown in FIG. 5(d), the first surface 9a of the second substrate 9 and the second surface 10b of the third substrate 10 are bonded by an adhesive 19, and the second supply path 15 of the second substrate 9 and the first supply path 17 of the third substrate 10 are connected to each other. The layer of the adhesive 19 has an opening 19a in an area surrounding the piezoelectric element 14, and the piezoelectric element 14 is not covered by the adhesive 19. As shown in FIG. 4(b), the first surface 1a of the first substrate 1 and the second surface 9b of the second substrate 9 are bonded by an adhesive 19, and the pressure chamber 16 of the second substrate 9 and the flow path 2a of the first substrate 1 are connected to each other. With this configuration, the liquid supplied from the outside of the liquid ejection head 8 is supplied to the pressure chamber 16 from the first supply path 17 of the third substrate 10 through the second supply path 15 of the second substrate 9. The liquid in the pressure chamber 16 is pressurized by the vibration of the vibration plate 13, which is vibrated by energy (vibration energy) generated by the piezoelectric element 14 electrically driven via a drive circuit and wiring not shown, and is ejected to the outside through the flow path 2a and the ejection port 11 of the first substrate 1.

[0021] In this embodiment, the bottom surface 3 of the flow path 2a and the clearance groove 2b of the first substrate 1 is formed in a flat surface shape by using an etching inhibitor layer 5 whose thickness is adjusted in the same manner as in the first embodiment shown in FIG. 2. The clearance groove 2b will be described. If the adhesive 19 overflows and infiltrates into the flow path 2a or the pressure chamber 16 when the first surface 1a of the first substrate 1 and the second surface 9b of the second substrate 9 are bonded, it is undesirable because it may affect the flow and discharge of the liquid. Therefore, the clearance groove 2b is provided to suppress the overflow of the adhesive 19. However, if the bottom surface 3 of the clearance groove 2b is curved, the capillary phenomenon is unlikely to occur, so the adhesive 19 does not enter the clearance groove 2b very much, and the adhesive 19 may overflow and infiltrate into the flow path 2a or the pressure chamber 16. Therefore, in this embodiment, the bottom surface 3 of the clearance groove 2b is made flat and the bottom surface 3 of the clearance groove 2b and the side surface 12 are in a perpendicular relationship, so that the capillary phenomenon is likely to occur. As a result, the infiltration of the adhesive 19 into the relief groove 2b is promoted, and the infiltration of the adhesive 19 into the flow path 2a and the pressure chamber 16 can be suppressed.

[0022] In this embodiment, it is required to form the depth of the pressure chamber 16 with high accuracy, and a depth accuracy higher than the etching accuracy is required. Therefore, the pressure chamber 16 is formed in the same manner as in the comparative example shown in FIG. 3. That is, the pressure chamber 16 is formed by performing dry etching from the second surface 9b of the second substrate 9. At this time, the protective layer 7 formed on the first surface 9a of the second substrate 9 is formed of a silicon oxide film or the like having a high etching selectivity with respect to silicon, and functions as an etching stop layer. Therefore, the etching is terminated when the etching progresses to a position where the protective layer 7 is reached. However, when the pressure chamber 16 is formed by dry etching, as described above, the bottom surface 22 of the pressure chamber 16 may become curved, resulting in a decrease in depth accuracy. Therefore, in order to reliably remove the curved area of ​​the bottom surface 22 of the pressure chamber 16 and flatten the bottom surface 22, the protective layer 7 is over-etched until it becomes thin. In this way, the pressure chamber 16 with high depth accuracy is formed. However, the protective layer 7 has the role of protecting the diaphragm 13 and controlling the thickness, and there are cases where a very high thickness accuracy is required. For example, if the required tolerance for the thickness accuracy of the protective layer 7 is very narrow, about 0.5 μm, it is not preferable to make the protective layer 7 thinner even if the tolerance is several nm. In such a case, it is preferable to form the bottom surface 22 of the pressure chamber 16 into a flat surface by using an etching inhibitor layer 5 (see FIG. 2) whose thickness is adjusted in the same manner as the flow path 2a and the escape groove 2b of the first substrate 1. In this way, a region in which the bottom surface 22 is curved is unlikely to occur in the pressure chamber 16 during etching, and there is no need to etch the protective layer 7 excessively to remove that region, and thus it is possible to prevent the protective layer 7 from becoming thinner.

[0023] [Third embodiment] FIG. 6(a) is a schematic plan view showing a liquid ejection head 23 according to a third embodiment of the present invention, and FIG. 6(b) is a schematic cross-sectional view taken along the line AA in FIG. 6(a). As shown in FIG. 6(b), the liquid ejection head 23 of this embodiment includes a substrate 1 made of, for example, silicon, and an ejection port forming member 25 made of, for example, negative epoxy resin. A first supply path 26 is formed on a first surface 1a of the substrate 1. A second supply path 27 communicating with the first supply path 26 is formed on a second surface 1b of the substrate 1, and an energy generating element (for example, a heat generating element made of a TaSiN film) 28, a driving circuit, wiring, a connection terminal 29, and the like (not shown) are formed. The depth of the first supply path 26 is 500 μm or less. Even if the first supply path 26 is deep, it is not preferable that the depth is non-uniform. In this embodiment, similar to the recess 2 of the substrate 1 in the first embodiment and the flow path 2a and the escape groove 2b of the first substrate 1 in the second embodiment, the bottom surface 30 of the first supply path 26 is formed into a flat surface by using an etching inhibitor layer 5 (see FIG. 2(b)) with an adjusted thickness.

[0024] An ejection port forming member 25 is formed on the second surface 1b of the substrate 1. A flow path 2a and a pressure chamber 16 are formed between the ejection port forming member 25 and the substrate 1. The ejection port forming member 25 constitutes a top plate portion 31 facing the substrate 1 at a distance, and a side wall portion 32 located between the top plate portion 31 and the substrate 1. The space surrounded by the top plate portion 31, the substrate 1, and the side wall portion 32 is the pressure chamber 16 and the flow path 2a. The flow path 2a communicates with the pressure chamber 16. The top plate portion 31 is formed with an ejection port 11 that is a through hole and communicates with the pressure chamber 16. The flow path 2a communicates with a second supply path 27 formed in the substrate 1. In this embodiment, liquid supplied from the outside of the liquid ejection head 23 is supplied to the pressure chamber 16 from the first supply path 26 of the substrate 1 through the second supply path 27 and the flow path 2a. The liquid in the pressure chamber 16 is boiled by energy (thermal energy) generated by the energy generating element 28 electrically driven via a drive circuit and wiring (not shown), and is discharged to the outside through the discharge port 11. In this embodiment, too, the bottom surfaces 3 and 22 of the flow channel 2a and the pressure chamber 16 are formed into flat surfaces by using an etching inhibitor layer 5 (see FIG. 2) whose thickness is adjusted, as in the first embodiment. EXAMPLES

[0025] [Example 1] As Example 1 of the present invention, a method for manufacturing the substrate 1 according to the first embodiment shown in FIG. 1 will be described in detail. As the substrate material 1c, a silicon substrate having a thickness of about 20 μm and a circular planar shape with a diameter of about 200 mm was prepared. In order to facilitate the transportation of such a thin substrate material 1c, the substrate material 1c may be processed in a state in which it is temporarily attached to a support substrate or support tape having a thickness of about 725 μm (not shown). As shown in FIG. 2(a), a positive photoresist was applied to the first surface 1a of the substrate material 1c by a spin coat method, and then baked to form a resist layer having a thickness of about 10 μm, which becomes the mask pattern layer 4. Then, by a photolithography method, an opening 4a having a planar shape of a square with one side of about 100 μm was formed in the resist layer to complete the mask pattern layer 4. Next, as shown in FIG. 2(b), an etching inhibitor layer 5 was formed on the mask pattern layer 4 on the first surface 1a of the substrate material 1c and in the opening 4a. The etching inhibitor layer 5 was formed by injecting C4F8 gas at a flow rate of 500sccm for 5 seconds in a vacuum device set at a pressure of 6 Pa and a coil power of 2000W. The formed etching inhibitor layer 5 was a CF-based polymer film, and was formed thickly at the location where the film-forming species was frequently incident. The locations where the film-forming species was frequently incident were the surface corner D of the opening 4a and the center position C of the opening 4a. As a result, the etching inhibitor layer 5 formed on the first surface 1a of the substrate material 1c was approximately continuously thinner in the direction perpendicular to the first surface 1a from the center position C of the opening 4a toward the inner peripheral edge E. It is preferable that the etching inhibitor layer 5 is a material that can be etched at the same time when the silicon substrate material 1c is etched in a later process. If a material with a very high etching selectivity to silicon, such as a silicon oxide film or a silicon nitride film, is used as the etching inhibitor layer 5, it may function as an etching stop layer, preventing etching of silicon from proceeding, and the effect of the present invention may not be obtained. Therefore, the etching inhibitor layer 5 is preferably made of a CF-based polymer film or the like, which is a material with a low etching selectivity to silicon, rather than a silicon oxide film or silicon nitride film, which has a high etching selectivity to silicon.

[0026] If the etching inhibitor layer is not formed or if an etching inhibitor layer with a uniform thickness is formed, the bottom surface 3 of the recess 2 will be curved. This is because, if a difference in etching rate occurs in the first etching step and the bottom surface 3 is formed in a curved shape, and a similar difference in etching rate occurs in the subsequent etching step, the shape of the bottom surface 3 will be maintained or the curve will be enlarged. Therefore, in this embodiment, the thickness of the etching inhibitor layer 5 in the opening 4a is made different in parts to change the etching rate in the direction perpendicular to the first surface 1a of the substrate 1, so that the shape of the bottom surface 3 can be controlled. That is, assuming that a difference in etching rate occurs in the subsequent etching step and the bottom surface 3 will be curved, the difference in thickness of the etching inhibitor layer 5 is set so that a bottom surface having a shape complementary to the assumed curved shape is formed in the first etching step. The etching inhibitor layer 5 is preferably thinner than the mask pattern layer 4. If a relatively thick film (several μm to several tens of μm thick) made of photoresist or the like is used as the etching inhibitor layer 5, etching does not proceed well, and the formation of the recess 2 itself is difficult. If the exposure dose of the photoresist is reduced to the limit sensitivity of the resist, it is possible to form a resist layer with a thickness of about 0.5 μm in the opening 4a, but it is difficult to control the difference in thickness of the resist layer in the opening 4a. In this embodiment, a CF-based polymer film that can be formed to a thickness of 0.5 μm or less, thinner than the mask pattern layer 4 (about 10 μm thick), is used as the etching inhibitor layer 5 so that the thickness difference in the opening 4a can be set to a degree that allows the shape of the bottom surface 3 of the recess 2 to be formed to be controlled.

[0027] Next, as shown in FIG. 2(c), a recess 2 was formed by dry etching from the first surface 1a of the substrate material 1c using a Bosch process including reactive ion etching, which is a type of dry etching. The depth of the recess 2 formed was about 10 μm. The Bosch process is a method of anisotropically etching silicon by alternately repeating the formation of an etching inhibitor layer mainly composed of carbon and etching with SF6 gas or the like. In the Bosch process of this embodiment, SF6 gas was sprayed when etching was performed, and C4F8 gas was sprayed when forming the latter-stage etching inhibitor layer 6. Since the first etching inhibitor layer 5 formed in the opening 4a has a thickness difference in parts, a difference occurred in the etching rate in the direction perpendicular to the first surface 1a, and the bottom surface 3 of the recess 2 became curved. Thereafter, as shown in FIG. 2(d), when etching was performed after forming the latter-stage etching inhibitor layer 6 with a substantially uniform thickness, a difference occurred in the etching rate in the direction perpendicular to the first surface 1a. However, the difference in the etching rate at this time was different from the difference in the etching rate at the first etching, and offset the difference in the etching rate at the first etching. Therefore, after the Bosch process, the bottom surface 3 of the recess 2 was flat instead of curved, as shown in FIG. 2(e). In this way, in this embodiment, the final shape of the bottom surface 3 of the recess 2 could be arbitrarily controlled by appropriately adjusting the thickness of the etching inhibitor layer 5 in the opening 4a. Next, the latter etching inhibitor layer 6 in the Bosch process was removed using hydrofluoroether, and then the mask pattern layer 4 was removed using an alkaline stripping solution. In this way, the substrate 1 shown in FIG. 1 was completed.

[0028] As described above, according to this embodiment, the bottom surface 3 of the recess 2 can be formed into a flat surface, not a curved surface as formed by only the conventional Bosch process. As a result, a sufficient volume of the recess 2 can be secured, and the depth precision of the recess 2 can be increased. Specifically, the flatness of the bottom surface 3 of the recess 2 is 0.5% or less, which is an improvement of about 1.1% over the comparative example shown in FIG. 3, for example.

[0029] [Example 2] As Example 2 of the present invention, a method for manufacturing a substrate 1 of a modified example of the first embodiment will be described. In this example, a mask pattern layer 4 and an etching inhibitor layer 5 were formed on the first surface 1a of the substrate material 1c in the same manner as in Example 1. The etching inhibitor layer 5 was formed by injecting C4F8 gas at a flow rate of 500 sccm for 10 seconds in a vacuum device set at a pressure of 6 Pa and a coil power of 2000 W. Since the injection time of C4F8 gas is 5 seconds longer than in Example 1, as shown in FIG. 7(a), the partial film thickness difference of the etching inhibitor layer 5 in the opening 4a of the mask pattern layer 4 is large. Next, the substrate material 1c was subjected to reactive ion etching to form a recess 2 as shown in FIG. 7(b). The depth of the formed recess 2 was about 5 μm. In this example, the shape of the bottom surface 3 of the recess 2 could be arbitrarily controlled by appropriately adjusting the thickness of the etching inhibitor layer 5 in the opening 4a. Due to the large difference in thickness of the etching inhibitor layer 5, the bottom surface 3 of the recess 2 was not a downward convex curved surface toward the second surface 1b, but an upward convex curved surface toward the first surface 1a. Specifically, a characteristic shape with an upward protrusion of about 0.5 μm toward the first surface 1a was obtained. Thereafter, the mask pattern layer 4 was removed using an alkaline stripping solution, and the substrate 1 shown in FIG. 7(c) was completed. According to this embodiment, the recess 2 having the above-mentioned characteristic upward convex bottom shape can be used as an alignment mark for positioning, and the visibility and recognition rate of the mark can be intentionally improved.

[0030] [Example 3] As Example 3 of the present invention, a method for manufacturing a liquid ejection head 8 according to the second embodiment shown in FIG. 4 will be described in detail. First, as shown in FIG. 8(a), a third substrate 10 was prepared in which a first supply path 17, which is a through hole, and a recess 18 located on a second surface 10b were formed on a silicon substrate having a thickness of about 500 μm and a circular shape with a diameter of about 200 mm in plan view. In addition, as shown in FIG. 8(b), a second substrate 9 was prepared in which a vibration plate 13, a protective layer 7, and a piezoelectric element 14, which constitute a first surface 9a, were formed on a silicon substrate 20 having a thickness of about 200 μm and a circular shape with a diameter of about 200 mm in plan view. The vibration plate 13 was made of silicon, the protective layer 7 was made of a silicon oxide film, and the piezoelectric element 14 was made of lead zirconate titanate. Although not shown, a driving circuit, wiring, connection terminals, and the like were also formed on the first surface 9a side of the second substrate 9.

[0031] As shown in FIG. 8(c), the first surface 9a of the second substrate 9 and the second surface 10b of the third substrate 10 were joined via an adhesive 19, and then the adhesive 19 was hardened by heat treatment. The adhesive 19 was spin-coated on a dry film (not shown) and then transferred in advance to the second surface 10b of the third substrate 10. At this time, the adhesive 19 was not transferred to the positions of the first supply path 17 and the recess 18. The method of applying the adhesive 19 is not limited to spin-coating and transfer, and patterning may be performed using screen printing or a photolithography method using a photosensitive adhesive.

[0032] Thereafter, a mask pattern layer 4 having an opening 4a was formed on the second surface 9b of the second substrate 9 in the same manner as in the steps shown in Fig. 2(a) to Fig. 2(e), and an etching inhibition layer 5 having a thickness that varies from place to place was formed in the opening 4a. Then, as shown in Fig. 8(d), a pressure chamber 16 communicating with the second supply path 15 was formed on the second surface 9b of the second substrate 9 by a Bosch process using reactive ion etching. In the Bosch process, the etching of the pressure chamber 16 was performed by injecting SF6 gas, and the formation of an etching inhibition layer (not shown) on the bottom surface 22 and side surface 24 of the pressure chamber 16 was performed by injecting C4F8 gas. The depth of the formed pressure chamber 16 was about 200 µm, and when viewed from the second surface 9b side, the bottom surface was etched and flattened until the protective layer 7 was exposed. As described above, it is not preferable that the bottom surface of the pressure chamber 16 is curved or the protective film 7 is thin. Therefore, in this embodiment, an etching inhibitor layer 5 having a non-constant thickness in the opening 4a (thickness is continuously or intermittently reduced from the center position C toward the inner periphery E) is formed, and the initial etching rate in the direction perpendicular to the second surface 9b is changed. This makes it possible to flatten the bottom surface of the pressure chamber 16 formed through the subsequent Bosch process, and to suppress excessive etching that would thin the protective layer 7, thereby suppressing a reduction in the thickness of the protective layer 7 by about 50 nm. Next, the latter-stage etching inhibitor layer 6 formed in the Bosch process was removed with hydrofluoroether, and the mask pattern layer 4, which is a resist layer, was removed with an alkaline stripping solution.

[0033] Next, the first substrate 1 was formed by substantially the same method as in Example 1. That is, on the first surface 1a of the substrate material 1c made of a silicon substrate having a thickness of about 130 μm and a circular planar shape with a diameter of about 200 mm, as shown in FIG. 2(a) to FIG. 2(e), a mask pattern layer 4 having an opening 4a was formed, and an etching inhibitor layer 5 was further formed. The etching inhibitor layer 5 was continuously or intermittently thinned from the center position C to the inner periphery E in the opening 4a. Then, reactive ion etching was performed on the first surface 1a to form the flow path 2a and the escape groove 2b, which are recesses. Furthermore, the Bosch process was performed to make the bottom surface 3 of the flow path 2a and the escape groove 2b flat. The etching in the Bosch process was performed by injecting SF6 gas onto the first surface 1a, and the formation of the latter-stage etching inhibitor layer 6 was performed by injecting C4F8 gas onto the first surface 1a. The depth of the flow path 2a and the escape groove 2b thus formed was about 100 μm, and the depth precision was good. Specifically, the flatness of the bottom surface 3 of the flow path 2a was 0.5% or less, which was improved by about 1.1% compared to the comparative example shown in FIG. 3. The flatness of the bottom surface 3 of the escape groove 2b was also good, similar to that of the bottom surface 3 of the flow path 2a. Next, the rear-stage etching inhibitor layer 6 in the Bosch process was removed using hydrofluoroether, and then the mask pattern layer 4 was removed using an alkaline stripping solution, as shown in FIG. 8(e). Note that the above steps may be performed in a state in which the substrate material 1c is temporarily attached to a support substrate or support tape having a thickness of about 725 μm (not shown) in order to facilitate the transportation and handling of the thin substrate material 1c. Next, in the Bosch process, an outlet 11 having a depth of about 30 μm that communicates with the flow path 2a on the first surface 1a was formed on the second surface 1b of the substrate material 1c. In the step of forming the outlet 11, the etching in the Bosch process was performed by spraying SF6 gas, and the formation of the rear-stage etching inhibitor layer 6 was performed by spraying C4F8 gas. Then, the subsequent etching inhibitor layer 6 was removed with hydrofluoroether, and the mask pattern layer 4 was removed with an alkaline stripping solution, thus forming the first substrate 1 shown in FIG.

[0034] The first surface 1a of the first substrate 1 and the second surface 9b of the second substrate 9 formed as described above were bonded together via the adhesive 19 as shown in FIG. 4(b), and the adhesive 19 was cured by heat treatment. The adhesive 19 was spin-coated on a dry film (not shown) and then transferred to the second surface 9b of the second substrate 9. At this time, the adhesive 19 was not transferred to the position of the pressure chamber 16. The method of applying the adhesive 19 is not limited to spin-coating and transfer, and the adhesive 19 may be patterned by screen printing or photolithography using a photosensitive adhesive. When the first surface 1a of the first substrate 1 and the second surface 9b of the second substrate 9 are bonded together in this manner, the adhesive 19 penetrates into the escape groove 2b, thereby preventing the adhesive 19 from overflowing and entering the flow path 2a or the pressure chamber 16. As described above, the bottom surface 3 of the escape groove 2b in this embodiment is formed in a flat surface shape, so that the capillary phenomenon is likely to occur and the adhesive 19 is likely to enter the escape groove 2b. As a result, it was possible to prevent the adhesive 19 from penetrating into the flow paths 2a and the pressure chambers 16. Then, by connecting the drive circuit and the connection terminals to the piezoelectric elements 14 via wiring, the liquid ejection head 8 of this embodiment shown in FIG.

[0035] [Example 4] As Example 4 of the present invention, a method for manufacturing a liquid ejection head 23 according to the third embodiment shown in FIG. 6 will be described in detail. FIGS. 9(a) to 9(d) are cross-sectional views seen from the same direction as FIG. 1(b), sequentially showing each step of the manufacturing method of the substrate 1. First, as shown in FIG. 9(a), a substrate material 1c was prepared, which was made of a circular silicon substrate having a thickness of about 725 μm and a planar shape with a diameter of about 200 mm, and on which an energy generating element (heat generating element) 28 made of a TaSiN film and a driving circuit, wiring, connection terminals, etc. (not shown) were formed. Then, the substrate 1 was formed by substantially the same method as in Example 1 (see FIGS. 2(a) to 2(e)). That is, a mask pattern layer 4 having an opening 4a was formed on a first surface 1a of the substrate material 1c, and an etching inhibitor layer 5 was further formed. The etching inhibitor layer 5 was continuously or intermittently thinner in thickness from a center position C toward an inner periphery E in the opening 4a. Then, reactive ion etching was performed on the first surface 1a to form a first supply path 26, which is a recess. Further, the Bosch process was performed to flatten the bottom surface of the first supply path 26. Etching in the Bosch process was performed by injecting SF6 gas onto the first surface 1a, and the formation of the subsequent etching inhibitor layer 6 was performed by injecting C4F8 gas onto the first surface 1a. The depth of the first supply path 26 thus formed was about 500 μm, and the depth precision was good. Specifically, the flatness of the bottom surface of the first supply path 26 was 0.5% or less, which was improved by about 1.1% compared to the comparative example shown in FIG. 3. Next, as shown in FIG. 9(b), the subsequent etching inhibitor layer 6 formed in the Bosch process was removed with hydrofluoroether, and the mask pattern layer 4, which was a resist layer, was removed with an alkaline stripping solution.

[0036] Next, as shown in FIG. 9(c), a second supply path 27 was formed on the second surface 1b of the substrate 1 by a Bosch process including reactive ion etching. The second supply path 27 was connected to the first supply path 26. Etching in the Bosch process was performed by injecting SF6 gas onto the second surface 1b, and the subsequent etching inhibitor layer 6 was formed by injecting C4F8 gas onto the second surface 1b. The depth of the second supply path 27 thus formed was about 225 μm. Next, the subsequent etching inhibitor layer 6 formed in the Bosch process was removed with hydrofluoroether, and the mask pattern layer 4, which was a resist layer, was removed with an alkaline stripping solution.

[0037] As shown in FIG. 6, the discharge port forming member 25 was formed on the second surface 1b of the substrate 1. The discharge port forming member 25 was formed with a side wall portion 32 and a top plate portion 31 by photolithography, and the discharge port 11 was formed in the top plate portion 31. The flow path 2a and the pressure chamber 16 were formed between the top plate portion and the substrate 1. The discharge port forming member 25 may be formed by laminating a layer forming the top plate portion 31 and a layer forming the side wall portion 32, each made of different photosensitive resins. In this embodiment, the discharge port forming member 25 was formed with two types of dry films made of epoxy resin to which a photoacid generator was added. Specifically, the first layer of dry film that will become the side wall portion 32 was laminated on the second surface 1b of the substrate 1, and then the first layer of dry film was exposed to light, and the second layer of dry film that will become the top plate portion 31 was laminated thereon. After the second layer of dry film was exposed to light, the first layer of dry film and the second layer of dry film were developed together. After that, each dry film was cured by heat treatment. Finally, the energy generating element 28 was connected to a drive circuit, wiring, connection terminals, etc. (not shown), thereby completing the liquid ejection head 23 of this embodiment.

[0038] Disclosure of embodiments of the present invention includes the following methods and compositions. (Method 1) forming a mask pattern layer having an opening on one surface of a substrate material; forming an etching inhibitor layer on the surface on which the mask pattern layer is formed; and etching the etching inhibitor layer and the substrate material within the opening to form a recess in the substrate material, A method for manufacturing a substrate, characterized in that, before the step of forming the recess, the thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface becomes thinner continuously or intermittently from the center position of the opening toward the inner peripheral edge of the opening. (Method 2) The method for producing a substrate according to method 1, wherein the mask pattern layer and the etch inhibitor layer are made of materials having different compositions. (Method 3) The method for producing a substrate according to Method 2, wherein the etching inhibitor layer is made of a CF-based polymer film. (Method 4) The method for manufacturing a substrate according to method 3, wherein the step of forming the etching inhibitor layer includes spraying C4F8 gas onto the one surface on which the mask pattern layer is formed. (Method 5) 5. The method for manufacturing a substrate according to any one of Methods 1 to 4, wherein the etching inhibitor layer has a thickness smaller than a thickness of the mask pattern layer in a direction perpendicular to the one surface. (Method 6) 6. The method for manufacturing a substrate according to any one of Methods 1 to 5, wherein the step of forming the recess includes performing dry etching after forming the etching inhibitor layer. (Method 7) The method for producing a substrate according to Method 6, wherein the step of forming the recess includes, after forming the etching inhibitor layer, alternately repeating dry etching and formation of a subsequent etching inhibitor layer. (Method 8) The method for producing a substrate according to Method 7, wherein the subsequent etch inhibitor layer has a constant thickness in a direction perpendicular to the one surface. (Method 9) a difference in thickness of the etching inhibitor layer in the opening in a direction perpendicular to the one surface is set so that a difference in the amount of etching in the opening caused by the repetition of the formation of the subsequent etching inhibitor layer and the subsequent dry etching is offset, and the bottom surface becomes flat after the repetition of the formation of the subsequent etching inhibitor layer and the subsequent dry etching; The method for manufacturing a substrate according to method 7 or 8, wherein a difference in thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface causes a difference in etching rate of the substrate material. (Method 10) A method for manufacturing a substrate according to any one of methods 1 to 9, wherein a difference in thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface is used to create a difference in etching rate of the substrate material, thereby controlling the shape of the bottom surface of the recess that is formed. (Method 11) 11. The method for manufacturing a substrate according to any one of methods 1 to 10, further comprising removing the etching inhibitor layer inside the opening midway through the step of forming the recess. (Method 12) a flow path and a relief groove are formed on the one surface of the recess, 12. The method for manufacturing a substrate according to any one of methods 1 to 11, further comprising the step of forming a discharge port that communicates with the flow path and opens to the other surface. (Method 13) A method for manufacturing a liquid ejection head having at least two substrates, comprising the steps of: Each step of the method for producing a substrate according to method 12, which is performed on a first substrate; and laminating a second substrate having pressure chambers and energy generating elements on the first substrate so that the pressure chambers communicate with the flow paths. (Method 14) The method for manufacturing a liquid ejection head according to Method 13, further comprising the step of laminating a third substrate having a first supply path onto the second substrate such that the first supply path communicates with the pressure chamber. (Method 15) the energy generating element is a piezoelectric element, the piezoelectric element, a vibration plate, a protective layer, and a second supply path communicating with the pressure chamber are formed on one surface of the second substrate, and the piezoelectric element is fixed to a part of the vibration plate; the first supply path is a through hole penetrating the third substrate in a thickness direction, and a recess is provided in the third substrate; the third substrate is laminated on the second substrate such that the first supply path is connected to the second supply path and the recessed portion faces a portion of the vibration plate to which the piezoelectric element is fixed; The method for manufacturing a liquid ejection head according to Method 14, further comprising laminating the second substrate on the first substrate so that the pressure chamber communicates with the flow path. (Method 16) forming a mask pattern layer having an opening on one surface of the second substrate, forming an etching inhibitor layer on the one surface on which the mask pattern layer is formed, and etching the etching inhibitor layer and the substrate material inside the opening to form the pressure chamber in the second substrate; A method for manufacturing a liquid ejection head described in any one of Methods 13 to 15, wherein a thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface before forming the pressure chamber becomes thinner continuously or intermittently from a center position of the opening toward an inner peripheral edge of the opening. (Method 17) forming a first supply path, which is the recess, on the one surface of the substrate material by the substrate manufacturing method according to any one of methods 1 to 12; A method for manufacturing a liquid ejection head, further comprising the step of forming an ejection port forming member on the one surface of the substrate, the ejection port forming member having a pressure chamber communicating with the first supply path and an ejection port communicating with the pressure chamber. (Configuration 1) A substrate having a recess on one surface, the recess being shallowest at a center position of the recess and becoming deeper continuously or discontinuously away from the center position. (Configuration 2) 2. The substrate according to claim 1, wherein the recess is an alignment mark for positioning. (Configuration 3) 3. The substrate according to claim 1 or 2, wherein the substrate is a silicon substrate. [Explanation of symbols]

[0039] 1. Board (first board) 1a One side (first side) 1c board material 2 Recess 4 Mask Pattern Layer 4a aperture 5 Etch inhibitor layer C center position E Inner edge

Claims

1. forming a mask pattern layer having an opening on one surface of a substrate material; forming an etching inhibitor layer on the surface on which the mask pattern layer is formed; and etching the etching inhibitor layer and the substrate material within the opening to form a recess in the substrate material, A method for manufacturing a substrate, characterized in that, before the step of forming the recess, the thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface becomes thinner continuously or intermittently from the center position of the opening toward the inner peripheral edge of the opening.

2. The method of claim 1 , wherein the mask pattern layer and the etch inhibitor layer are made of materials having different compositions.

3. The method for manufacturing a substrate according to claim 2 , wherein the etching inhibitor layer is made of a CF-based polymer film.

4. The step of forming the etching inhibitor layer may include forming a layer of C 4 F 8 The method for manufacturing a substrate according to claim 3 , further comprising injecting a gas.

5. The method for manufacturing a substrate according to claim 1 , wherein a thickness of the etching inhibitor layer is smaller than a thickness of the mask pattern layer in a direction perpendicular to the one surface.

6. The method for manufacturing a substrate according to claim 1 , wherein the step of forming the recess includes performing dry etching after forming the etching inhibitor layer.

7. The method for manufacturing a substrate according to claim 6 , wherein the step of forming the recess includes alternately repeating dry etching and formation of a subsequent etch inhibitor layer after forming the etch inhibitor layer.

8. The method for manufacturing a substrate according to claim 7 , wherein the subsequent-stage etch inhibitor layer has a constant thickness in a direction perpendicular to the one surface.

9. a difference in thickness of the etching inhibitor layer in the opening in a direction perpendicular to the one surface is set so that a difference in the amount of etching in the opening caused by the repetition of the formation of the subsequent etching inhibitor layer and the subsequent dry etching is offset, and the bottom surface becomes flat after the repetition of the formation of the subsequent etching inhibitor layer and the subsequent dry etching; The method for manufacturing a substrate according to claim 7 , wherein a difference in thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface causes a difference in etching rate of the substrate material.

10. 5. The method for manufacturing a substrate according to claim 1, further comprising the steps of: generating a difference in an etching rate of the substrate material by controlling a thickness difference of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface, thereby controlling a shape of a bottom surface of the recess formed.

11. The method for manufacturing a substrate according to claim 1 , further comprising removing the etching inhibitor layer inside the opening during the step of forming the recess.

12. a flow path and a relief groove are formed on the one surface of the recess, The method for manufacturing a substrate according to claim 1 , further comprising the step of forming a discharge port that communicates with the flow path and opens on the other surface.

13. A method for manufacturing a liquid ejection head having at least two substrates, comprising the steps of: Each step of the method for manufacturing a substrate according to claim 12 is performed on a first substrate; and laminating a second substrate having pressure chambers and energy generating elements on the first substrate so that the pressure chambers communicate with the flow paths.

14. The method for manufacturing a liquid ejection head according to claim 13, further comprising the step of laminating a third substrate having a first supply path on the second substrate such that the first supply path communicates with the pressure chamber.

15. the energy generating element is a piezoelectric element, the piezoelectric element, a vibration plate, a protective layer, and a second supply path communicating with the pressure chamber are formed on one surface of the second substrate, and the piezoelectric element is fixed to a part of the vibration plate; the first supply path is a through hole penetrating the third substrate in a thickness direction, and a recess is provided in the third substrate; the third substrate is laminated on the second substrate such that the first supply path is connected to the second supply path and the recessed portion faces a portion of the vibration plate to which the piezoelectric element is fixed; The method for manufacturing a liquid ejection head according to claim 14 , wherein the second substrate is laminated on the first substrate so that the pressure chamber communicates with the flow path.

16. forming a mask pattern layer having an opening on one surface of the second substrate, forming an etching inhibitor layer on the one surface on which the mask pattern layer is formed, and etching the etching inhibitor layer and the substrate material inside the opening to form the pressure chamber in the second substrate; 14. A method for manufacturing a liquid ejection head as described in claim 13, wherein a thickness of the etching inhibitor layer inside the opening in a direction perpendicular to the one surface before forming the pressure chamber becomes thinner continuously or intermittently from a center position of the opening toward an inner peripheral edge of the opening.

17. 5. The method for manufacturing a substrate according to claim 1, further comprising forming a first supply path, which is the recess, on the one surface of the substrate material; The method for manufacturing a liquid ejection head further includes a step of forming an ejection port forming member on the one surface of the substrate, the ejection port forming member having a pressure chamber communicating with the first supply path and an ejection port communicating with the pressure chamber.

18. A substrate having a recess on one surface, the recess being shallowest at a center position of the recess and becoming deeper continuously or discontinuously away from the center position.

19. 20. The substrate according to claim 18, wherein the recess is an alignment mark for positioning.

20. 20. The substrate according to claim 18 or 19, wherein the substrate is a silicon substrate.

Citation Information

Patent Citations

  • Liquid ejection head, method for ejecting liquid, head cartridge, and liquid ejection device

    JP1999235828A