Power storage device and manufacturing method for power storage device

By arranging the negative electrode active material layer with a lower mass and density in its peripheral portion, the thickness of the edge is controlled, stabilizing the layer and facilitating smooth stacking in power storage devices.

JP2024154255AInactive Publication Date: 2024-10-30GS YUASA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023067990
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In conventional power storage devices, the negative electrode active material layer often becomes thicker at its peripheral edge due to its larger size compared to the positive electrode active material layer, leading to potential instability and difficulties in stacking and sealing.

Method used

The negative electrode active material layer is designed with a lower mass and density in its peripheral portion compared to the central portion, ensuring it is smaller and less dense, which is achieved by arranging it on the current collector foil such that the peripheral portion has a reduced amount of active material and is pressed simultaneously with the positive electrode active material layer to maintain stability.

Benefits of technology

This design effectively suppresses the thickness increase of the negative electrode active material layer's peripheral edge, preventing distortions and wrinkles, thereby enhancing the stability and ease of stacking, and reducing the risk of electrolyte leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154255000001_ABST
    Figure 2024154255000001_ABST
Patent Text Reader

Abstract

To provide a power storage device in which the increase in thickness of a peripheral part of a negative electrode active material layer can be suppressed, and a manufacturing method for the power storage device.SOLUTION: A power storage device includes a plurality of electrode units 100 stacked in a stacking direction. Each of the electrode units 100 includes at least a current collecting foil 110, a positive electrode active material layer 120 formed on one surface of the current collecting foil 110, and a negative electrode active material layer 130 formed on the other surface of the current collecting foil 110. The negative electrode active material layer 130 is larger than the positive electrode active material layer 120 when viewed from the stacking direction. The negative electrode active material layer 130 has lower density of the active material and smaller mass of the active material per unit area on the surface of the current collecting foil 110 in a peripheral part 131 than in a central part 132.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electricity storage device and a method for manufacturing an electricity storage device. [Background technology]

[0002] Conventionally, there is known a power storage device including an electrode unit in which active material layers (positive and negative active material layers) are formed on both sides of a current collector foil. For example, Patent Document 1 discloses a sheet battery including a bipolar electrode unit having a positive active material layer on one side of a composite current collector and a negative active material layer on the other side. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-100471 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the conventional electric storage device, the negative active material layer is generally larger than the positive active material layer among the active material layers formed on the current collector foil, and therefore, when the positive active material layer is formed on one side of the current collector foil and the negative active material layer is formed on the other side of the current collector foil, the thickness of the peripheral portion of the negative active material layer may become thick.

[0005] The present invention was made by the inventors of the present application by focusing on the above-mentioned problem, and aims to provide an energy storage device that can suppress an increase in thickness of the peripheral portion of a negative electrode active material layer, and a method for manufacturing the energy storage device. [Means for solving the problem]

[0006] An energy storage device according to one embodiment of the present invention includes a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one side of the current collecting foil, and a negative electrode active material layer formed on the other side of the current collecting foil, the negative electrode active material layer being larger in size than the positive electrode active material layer when viewed from the stacking direction, and the negative electrode active material layer having a smaller mass of active material per unit area on the surface of the current collecting foil and a lower active material density at its peripheral portion than at its central portion.

[0007] A manufacturing method for an electricity storage device according to one aspect of the present invention is a manufacturing method for an electricity storage device including a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one side of the current collecting foil, and a negative electrode active material layer formed on the other side of the current collecting foil, and the manufacturing method for the electricity storage device includes: arranging the negative electrode active material layer on the current collecting foil so that it is larger in size than the positive electrode active material layer when viewed from the stacking direction and so that a peripheral portion has a smaller mass of active material per unit area on a surface of the current collecting foil than a central portion; and forming the negative electrode active material layer by simultaneously pressing the negative electrode active material layer and the positive electrode active material layer so that the density of active material is lower in the peripheral portion than in the central portion. Effect of the Invention

[0008] According to the electricity storage device and the like of the present invention, it is possible to prevent the thickness of the peripheral portion of the negative electrode active material layer from increasing. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view showing the appearance of a power storage device according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an internal configuration of the electricity storage device according to the embodiment. [Diagram 3] FIG. 3 is a perspective view and a cross-sectional view showing a configuration of an electrode unit included in the power storage device according to the embodiment. [Figure 4]FIG. 4 is a flowchart showing the manufacturing steps in the manufacturing method for the electricity storage device according to the embodiment. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a manufacturing process in a manufacturing method for an electricity storage device according to an embodiment. [Figure 6] FIG. 6 is a cross-sectional view showing the configuration of the electricity storage pack. [Figure 7] FIG. 7 is a cross-sectional view showing another configuration of the electricity storage pack. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (1) An energy storage device according to one aspect of the present invention includes a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one side of the current collecting foil, and a negative electrode active material layer formed on the other side of the current collecting foil, the negative electrode active material layer being larger in size than the positive electrode active material layer when viewed in the stacking direction, and the negative electrode active material layer having a smaller mass of active material per unit area on the surface of the current collecting foil and a lower active material density at a peripheral portion than at a central portion.

[0011] According to this, in the electricity storage device, the mass of the active material in the peripheral portion of the negative electrode active material layer formed on the current collector foil (the mass of the active material per unit area on the surface of the current collector foil) is less than the mass of the active material in the central portion of the negative electrode active material layer. Furthermore, the density of the active material in the peripheral portion of the negative electrode active material layer is lower than the density of the active material in the central portion of the negative electrode active material layer. In other words, by pressing the negative electrode active material layer with the amount of active material arranged in the peripheral portion of the negative electrode active material layer, which is larger in size than the positive electrode active material layer, being less than the amount of active material arranged in the central portion, the mass of the active material in the peripheral portion of the negative electrode active material layer is less than that in the central portion, and the density of the active material is lower. This makes it possible to prevent the peripheral portion of the negative electrode active material layer from becoming thicker.

[0012] (2) In the energy storage device described in (1) above, the peripheral portion may be a portion of the negative electrode active material layer that protrudes from the positive electrode active material layer when viewed in the stacking direction, the negative electrode active material layer has an inner portion that is arranged inwardly and adjacent to the peripheral portion, and the peripheral portion may have a smaller mass of the active material and a lower density of the active material than the inner portion.

[0013] In many cases, the portion of the negative electrode active material layer that protrudes from the positive electrode active material layer (protruding portion) is thick. For this reason, in the negative electrode active material layer, the mass of the active material in the peripheral portion protruding from the positive electrode active material layer is made smaller than the mass of the active material in the inner portion inside the peripheral portion, and the density of the active material in the peripheral portion is made lower than the density of the active material in the inner portion. This makes it possible to prevent the thickness of the peripheral portion (protruding portion) protruding from the positive electrode active material layer from becoming thick.

[0014] (3) In the energy storage device described in (1) or (2) above, the negative electrode active material layer may be configured such that the mass of the active material is smaller and the density of the active material is lower in the peripheral portions at the ends in two directions perpendicular to the stacking direction and perpendicular to each other than in the central portion.

[0015] According to this, the mass of the active material in the peripheral portion at the two end portions of the negative electrode active material layer is made smaller than the mass of the active material in the central portion, and the density of the active material in the peripheral portion is made lower than the density of the active material in the central portion, thereby making it possible to prevent the thickness of the peripheral portion from increasing at the two end portions of the negative electrode active material layer.

[0016] (4) A manufacturing method for an electricity storage device according to one aspect of the present invention is a manufacturing method for an electricity storage device including a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil, the manufacturing method for the electricity storage device including: arranging the negative electrode active material layer on the current collecting foil such that it is larger in size than the positive electrode active material layer when viewed from the stacking direction and such that a peripheral portion has a smaller mass of active material per unit area on a surface of the current collecting foil than a central portion; and simultaneously pressing the negative electrode active material layer and the positive electrode active material layer to form the negative electrode active material layer such that the peripheral portion has a lower density of active material than the central portion.

[0017] According to this, in the method for producing an electricity storage device, the negative electrode active material layer is arranged on a current collector foil so that the mass of the active material is smaller at the periphery than at the center, and the negative electrode active material layer and the positive electrode active material layer are pressed simultaneously to form the negative electrode active material layer so that the density of the active material is lower at the periphery than at the center, thereby making it possible to prevent the thickness of the negative electrode active material layer from becoming thicker at the periphery.

[0018] (5) In the method for producing an electricity storage device described in (4) above, when the negative electrode active material layer is disposed on the current collector foil, the negative electrode active material layer may be disposed on the other surface of the current collector foil, and then the positive electrode active material layer may be disposed on the one surface of the current collector foil.

[0019] When placing a negative electrode active material layer, which is larger in size than a positive electrode active material layer, on a current collector foil, if the positive electrode active material layer is not placed on the current collector foil, the portion of the negative electrode active material layer that protrudes from the positive electrode active material layer will not have a support for the positive electrode active material layer. In this case, when placing the negative electrode active material layer on the current collector foil, the amount of the protruding portion may be unstable (may become large). For this reason, the negative electrode active material layer is placed on the current collector foil after the positive electrode active material layer is placed on the current collector foil. This allows the negative electrode active material layer to be placed on the current collector foil in a more stable state, making it easier to adjust the amount of negative electrode active material placed on the periphery of the negative electrode active material layer.

[0020] Hereinafter, a description will be given of an energy storage device and a manufacturing method thereof according to an embodiment (including its modified examples) of the present invention with reference to the drawings. Note that the embodiments described below all show comprehensive or specific examples. The numerical values, shapes, materials, components, arrangement and connection forms of the components, manufacturing processes, and the order of the manufacturing processes shown in the following embodiments are merely examples and are not intended to limit the present invention. In each drawing, the dimensions are not strictly shown. In each drawing, the same or similar components are given the same symbols.

[0021] In the following description and drawings, the longitudinal direction of the power storage device, or the opposing direction of a pair of short side surfaces of the power storage device, is defined as the X-axis direction. The opposing direction of a pair of long side surfaces of the power storage device is defined as the Y-axis direction. The thickness direction of the power storage device, the stacking direction of the multiple electrode units, the stacking direction of the current collecting foils and active material layers, the arrangement direction of a pair of end members, or the up-down direction is defined as the Z-axis direction. These X-axis, Y-axis, and Z-axis directions intersect with each other (orthogonal in this embodiment). Note that, depending on the mode of use, the Z-axis direction may not be the up-down direction, but for convenience of explanation, the following description will be given assuming that the Z-axis direction is the up-down direction.

[0022] In the following description, the positive X-axis direction refers to the direction of the X-axis arrow, and the negative X-axis direction refers to the opposite direction to the positive X-axis direction. When simply referring to the X-axis direction, it refers to both or either of the positive and negative X-axis directions. The same applies to the Y-axis and Z-axis directions. Expressions indicating relative directions or attitudes, such as parallel and perpendicular, also include cases where the directions or attitudes are not strictly speaking the same. For example, two directions being parallel not only means that the two directions are completely parallel, but also means that the directions are substantially parallel, that is, that there is a difference of, for example, about a few percent. In the following description, when the term "insulation" is used, it means "electrical insulation."

[0023] (Embodiment) [1 General Description of Power Storage Device 10] First, the general description of the energy storage device 10 in this embodiment will be given. FIG. 1 is a perspective view showing the appearance of the energy storage device 10 according to this embodiment. FIG. 2 is a cross-sectional view showing the internal configuration of the energy storage device 10 according to this embodiment. Specifically, FIG. 2 is a cross-sectional view of the energy storage device 10 in FIG. 1 cut along the YZ plane passing through the line II-II. FIG. 2 shows each component included in the energy storage device 10. FIG. 3 is a perspective view and a cross-sectional view showing the configuration of the electrode unit 100 included in the energy storage device 10 according to this embodiment. Specifically, FIG. 3(a) is a perspective view showing the appearance of the electrode unit 100. FIG. 3(b) is a cross-sectional view showing the configuration of the electrode unit 100 in FIG. 3(a) cut along the YZ plane passing through the line IIIb-IIIb. In FIG. 3, for convenience of explanation, the seal portion 210 included in the electrode unit 100 is omitted.

[0024] The power storage device 10 is a device that can charge electricity from an external source and discharge electricity to the outside. The power storage device 10 in this embodiment has a substantially rectangular parallelepiped shape. Specifically, the power storage device 10 is a bipolar battery. The power storage device 10 is used as a battery for driving or starting an engine of a moving body such as an automobile, a motorcycle, a watercraft, a ship, a snowmobile, an agricultural machine, a construction machine, an automatic guided vehicle (AGV), or a railway vehicle for an electric railway. Examples of the above-mentioned automobiles include electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and fossil fuel (gasoline, diesel, liquefied natural gas, etc.) vehicles. Examples of the above-mentioned railway vehicles for an electric railway include electric trains, monorails, linear motor cars, and hybrid trains equipped with both a diesel engine and an electric motor. The power storage device 10 can also be used as a stationary battery for home or business use.

[0025] As shown in FIG. 1 and FIG. 2, the energy storage device 10 includes a plurality of electrode units 100, end units 101 and 102, a plurality of separators 140, and a pair of end members 300. Each of the plurality of electrode units 100, the end units 101, and the end units 102 is a rectangular plate-like portion in a plan view, and is stacked in the Z-axis direction. In the present embodiment, the plan view refers to a view from the stacking direction (Z-axis direction). The direction in which the plurality of electrode units 100, the end units 101, and the end units 102 are stacked (Z-axis direction) is also referred to as the stacking direction. The separator 140 is disposed between each of the plurality of electrode units 100 and the end units 101 and 102. The pair of end members 300 are disposed on both sides of the plurality of electrode units 100 and the end units 101 and 102 in the stacking direction (Z-axis direction). In the present embodiment, two electrode units 100 are stacked in the stacking direction between the end unit 101 and the end unit 102, but the number of stacked electrode units 100 is not particularly limited. The shapes of the electrode unit 100, the end unit 101, the end unit 102, etc. in a plan view are also not particularly limited.

[0026] [1.1 Description of the electrode unit 100] The configuration of the electrode unit 100 will be described in detail below with reference to Fig. 3. The electrode unit 100 is a single unit in which active material layers are formed on both sides of a single current collector foil. Each of the multiple electrode units 100 has at least a current collector foil 110, a positive electrode active material layer 120 formed on one side of the current collector foil 110, a negative electrode active material layer 130 formed on the other side of the current collector foil 110, and a seal portion 210. In this embodiment, the thickness of the electrode unit 100 (thickness in the stacking direction) is about 135 µm to 190 µm.

[0027] The current collecting foil 110 is a plate-like member having a rectangular shape in a plan view. The current collecting foil 110 is a metal foil. As shown in FIG. 3, the current collecting foil 110 has two metal layers 111 and 112 arranged in the stacking direction (Z-axis direction). The metal layers 111 and 112 are plate-like parts having the same size and shape in a plan view. Hereinafter, of the metal layers 111 and 112, the metal layer 111 on which the positive electrode active material layer 120 is formed is also referred to as the positive electrode metal layer 111, and the metal layer 112 on which the negative electrode active material layer 130 is formed is also referred to as the negative electrode metal layer 112. The positive electrode metal layer 111 is a metal layer located in the positive direction of the current collecting foil 110 on the Z-axis, and the negative electrode metal layer 112 is a metal layer located in the negative direction of the current collecting foil 110 on the Z-axis. That is, the current collecting foil 110 is formed by laminating the positive electrode metal layer 111 and the negative electrode metal layer 112 in a lamination direction in a state in which the positive electrode metal layer 111 and the negative electrode metal layer 112 are connected (contacted or joined) to each other. One of the positive electrode metal layer 111 and the negative electrode metal layer 112 may be a metal foil, and the other may be a plated layer plated on the metal foil. Alternatively, both the positive electrode metal layer 111 and the negative electrode metal layer 112 may be metal foils. When both the positive electrode metal layer 111 and the negative electrode metal layer 112 are metal foils, the current collecting foil 110 may be a clad material formed by joining two metal foils together, or may have two metal foils in a state in which the two metal foils are connected (contacted) without being joined to each other.

[0028] The material of the positive electrode metal layer 111 may be a metal such as aluminum, titanium, tantalum, or stainless steel, or an alloy thereof. Among these, from the viewpoint of the balance between the electric potential resistance, the high conductivity, and the cost, the material of the positive electrode metal layer 111 is preferably aluminum or an aluminum alloy. The form of the positive electrode metal layer 111 may be a plated layer, but from the viewpoint of workability and cost, a foil is preferable. That is, the positive electrode metal layer 111 is preferably an aluminum foil. The material of the negative electrode metal layer 112 may be a metal such as copper, nickel, stainless steel, or nickel-plated steel, or an alloy thereof, and among these, it is preferable to use copper or a copper alloy. The form of the negative electrode metal layer 112 may be a plated layer or a foil (copper foil), and examples of the copper foil include rolled copper foil and electrolytic copper foil. The thickness (thickness in the lamination direction) of the current collector foil 110 is about 20 μm to 30 μm. The positive electrode metal layer 111 has a thickness (thickness in the stacking direction) of about 5 μm to 20 μm, and the negative electrode metal layer 112 has a thickness (thickness in the stacking direction) of about 5 μm to 15 μm.

[0029] The positive electrode active material layer 120 is a positive electrode active material layer formed on one surface (surface in the positive direction of the Z axis) of the current collector foil 110. Specifically, the positive electrode active material layer 120 is formed on the positive electrode metal layer 111 (the outer surface (surface in the positive direction of the Z axis) of the positive electrode metal layer 111). The positive electrode active material layer 120 is formed in a rectangular shape smaller in size than the positive electrode metal layer 111 in a planar view according to the shape of the positive electrode metal layer 111. Small size in a planar view means that the area in the XY plane is small. The same applies below. The thickness (thickness in the stacking direction) of the positive electrode active material layer 120 is about 70 μm to 100 μm.

[0030] The positive electrode active material layer 120 contains a positive electrode active material, and optionally contains a conductive agent, a binder, a thickener, a filler, and other optional components as necessary. Examples of the positive electrode active material include layered lithium transition metal oxides such as LiM1O2 (M1 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, and the like), spinel-type lithium transition metal oxides such as LiM22O4 (M2 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, and the like), and polyanion compounds such as LiM3PO4, LiM3SiO4, and LiM3BO3 (M3 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, and the like). As the positive electrode active material, one of these compounds may be used alone, or two or more may be used in combination. The conductive agent contained in the positive electrode active material layer 120 is not particularly limited as long as it has electrical conductivity. Examples of conductive agents include carbon black such as furnace black, acetylene black, and Ketjen black, and natural or artificial graphite. Examples of binders include fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), sulfonated EPDM, and styrene butadiene rubber (SBR). Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose (CMC), and methyl cellulose.

[0031] The negative electrode active material layer 130 is a negative electrode active material layer formed on the other surface (surface in the negative Z-axis direction) of the current collector foil 110. Specifically, the negative electrode active material layer 130 is formed on the negative electrode metal layer 112 (the outer surface (surface in the negative Z-axis direction) of the negative electrode metal layer 112). The negative electrode active material layer 130 is formed in a rectangular shape smaller than the negative electrode metal layer 112 in a planar view according to the shape of the negative electrode metal layer 112. The negative electrode active material layer 130 is formed in a larger size than the positive electrode active material layer 120 in a planar view. The larger size in a planar view means that the area in the XY plane is larger. The same applies below. In other words, the area in the XY plane of the negative electrode active material layer 130 is larger than that of the positive electrode active material layer 120. The thickness (thickness in the stacking direction) of the negative electrode active material layer 130 is about 45 μm to 60 μm.

[0032] The negative electrode active material layer 130 contains a negative electrode active material, and optionally contains optional components such as a conductive agent, a binder, a thickener, and a filler. The optional components such as the conductive agent, the binder, the thickener, and the filler can be the same as those in the positive electrode active material layer 120. As the negative electrode active material, a material capable of absorbing and releasing lithium ions is usually used. As the negative electrode active material, for example, metals or semi-metals such as Si and Sn; metal oxides or semi-metal oxides such as Si oxide and Sn oxide; and carbon materials such as graphite and non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon) can be used.

[0033] The sealing portion 210 is a portion disposed around the positive electrode active material layer 120 or the negative electrode active material layer 130. In the present embodiment, the sealing portion 210 is an annular portion disposed around the positive electrode active material layer 120 and the negative electrode active material layer 130 over the entire circumference of the positive electrode active material layer 120 and the negative electrode active material layer 130. Specifically, the sealing portion 210 is formed in a quadrangular ring shape along the outer periphery of the current collector foil 110 so as to cover the outer periphery of the current collector foil 110. The sealing portion 210 is formed from an insulating material such as polycarbonate (PC), polypropylene (PP), polyethylene (PE), polystyrene (PS), polyphenylene sulfide resin (PPS), polyphenylene ether (PPE (including modified PPE)), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyether ether ketone (PEEK), tetrafluoroethylene-perfluoroalkyl vinyl ether (PFA), polytetrafluoroethylene (PTFE), polyethersulfone (PES), polyamide (PA), ABS resin, or a composite material thereof.

[0034] The seal parts 210 of two adjacent electrode units 100 are connected to each other. The seal parts 210 may be connected to each other by being integrally and continuously formed, or may be connected to each other by being joined to each other by heat sealing (thermal welding), ultrasonic welding, laser welding, adhesive, or the like. As a result, the seal part 210 is disposed around the positive electrode active material layer 120 of one of the two electrode units 100 and the negative electrode active material layer 130 of the other of the two electrode units 100, and the seal part 210 is provided between the current collector foils 110 of the two electrode units 100. In other words, the seal part 210 is provided continuously between the current collector foils 110 of the two electrode units 100, and the current collector foils 110 are sealed from each other.

[0035] An electrolyte layer (not shown) is formed on the inside of the seal portion 210 of each of the electrode units 100. In this embodiment, the electrolyte layer is a non-aqueous liquid electrolyte (electrolytic solution), but may be a solid electrolyte (solid electrolyte) or a gel electrolyte. Any known electrolyte may be used as the electrolyte. The electrolyte (non-aqueous electrolyte) may be a non-aqueous solvent in which an electrolyte salt is dissolved. Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate (EC) and propylene carbonate (PC), and chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, LiN(SO2F)2, and LiN(SO2CF3).

[0036] [1.2 Description of end units 101 and 102] Next, the configuration of the end units 101 and 102 will be described in detail. The end unit 101 is disposed at the end of the multiple electrode units 100 in the negative direction of the Z axis. The end unit 102 is disposed at the end of the multiple electrode units 100 in the positive direction of the Z axis. The end units 101 and 102 are portions that sandwich the multiple electrode units 100 in the Z axis direction.

[0037] The end unit 101 has at least a positive electrode metal layer 111, a positive electrode active material layer 120 formed on a surface of the positive electrode metal layer 111 in the Z-axis positive direction, and a seal portion 220. The positive electrode metal layer 111 and the positive electrode active material layer 120 of the end unit 101 have the same configuration as the positive electrode metal layer 111 and the positive electrode active material layer 120 of the current collector foil 110 of the electrode unit 100 described above.

[0038] The sealing portion 220 is a portion disposed around the positive electrode active material layer 120. In the present embodiment, the sealing portion 220 is an annular portion disposed around the positive electrode active material layer 120 over the entire circumference of the positive electrode active material layer 120. Specifically, the sealing portion 220 is formed in a quadrangular ring shape along the outer periphery of the positive electrode metal layer 111 and the end member 300 so as to cover the outer periphery of the positive electrode metal layer 111 and the end member 300. The sealing portion 220 is formed of the same material as the sealing portion 210 of the electrode unit 100.

[0039] The seal portion 220 is connected to the seal portion 210 of the electrode unit 100 adjacent to the end unit 101. The connection between the seal portion 220 and the seal portion 210 is similar to the connection between the seal portions 210 described above, and therefore a detailed description will be omitted. This provides a seal between the positive electrode metal layer 111 of the end unit 101 and the current collecting foil 110 of the electrode unit 100. The above-mentioned electrolyte layer (not shown) is formed inside the seal portion 220.

[0040] The end unit 102 has at least a current collecting foil 110, a negative electrode active material layer 130 arranged on a surface of the current collecting foil 110 in the negative Z-axis direction, and a seal portion 230. The current collecting foil 110 and the negative electrode active material layer 130 of the end unit 102 have the same configuration as the current collecting foil 110 and the negative electrode active material layer 130 of the electrode unit 100 described above.

[0041] The sealing portion 230 is a portion disposed around the negative electrode active material layer 130. In the present embodiment, the sealing portion 230 is an annular portion disposed around the negative electrode active material layer 130 over the entire circumference of the negative electrode active material layer 130. Specifically, the sealing portion 230 is formed in a quadrangular ring shape along the outer periphery of the current collector foil 110 and the end member 300 so as to cover the outer periphery of the current collector foil 110 and the end member 300. The sealing portion 230 is formed of the same material as the sealing portion 210 of the electrode unit 100.

[0042] The seal portion 230 is connected to the seal portion 210 of the electrode unit 100 adjacent to the end unit 102. The connection between the seal portion 230 and the seal portion 210 is similar to the connection between the seal portions 210 described above, and therefore a detailed description will be omitted. This provides a seal between the current collecting foil 110 of the end unit 102 and the current collecting foil 110 of the electrode unit 100. The above-mentioned electrolyte layer (not shown) is formed inside the seal portion 230.

[0043] In this manner, the seal portions 210, 220, and 230 are connected to one another to form the seal member 200. The seal member 200 is a cylindrical (rectangular cylindrical) member that is disposed so as to surround the entire periphery of the positive electrode metal layer 111, the negative electrode metal layer 112, the positive electrode active material layer 120, the negative electrode active material layer 130, the separator 140, and the end member 300, and seals these members from the outside.

[0044] [1.3 Description of the separator 140 and the end member 300] The separator 140 is a microporous sheet made of resin. The separator 140 is disposed between the electrode units 100, between the end unit 101 and the electrode unit 100, and between the end unit 102 and the electrode unit 100. Specifically, the separator 140 is disposed between the positive electrode active material layer 120 and the negative electrode active material layer 130. For example, a woven fabric, a nonwoven fabric, a porous resin film, or the like is used as the material of the separator 140. Among these, a porous resin film is preferable. From the viewpoint of strength, a polyolefin such as polyethylene or polypropylene is preferable as the main component of the porous resin film. The separator 140 may be a multilayer film in which a layer containing a filler is formed on the surface of the porous resin film. The separator 140 is formed in a rectangular shape larger than the negative electrode active material layer 130 in a planar view. In this embodiment, the size of the separator 140 is smaller than that of the current collector foil 110 in a planar view, but may be larger than the current collector foil 110 in a planar view. The thickness of the separator 140 (thickness in the stacking direction) is about 15 μm to 20 μm.

[0045] The end member 300 is a member disposed at an end of the power storage device 10 in the stacking direction (Z-axis direction) relative to the plurality of electrode units 100. In this embodiment, a pair of end members 300 are disposed at the end closest to the negative Z-axis direction and the end closest to the positive Z-axis direction of the power storage device 10. The pair of end members 300 are connected to the end units 101 and 102 (the positive electrode metal layers 111 of the end units 101 and 102). As a result, the pair of end members 300 sandwich the plurality of electrode units 100 and the end units 101 and 102 located therebetween from both sides in the stacking direction (Z-axis direction). The end member 300 is a flat plate-shaped member (end plate). The end member 300 is electrically connected to another end member 300 of another power storage device 10 via another conductive member (bus bar, cooling plate, etc., not shown). The end member 300 is formed of a conductive member made of metal such as aluminum, aluminum alloy, copper, copper alloy, nickel, etc., or a combination thereof, or a conductive member other than metal. Since the end member 300 is connected to the positive electrode metal layer 111, it is preferably formed of the same material as the positive electrode metal layer 111, such as aluminum. The end member 300 has a thickness (thickness in the stacking direction) of about 0.5 mm to 3 mm. The electricity storage device 10 may have another conductive member on the outside of the end member 300 (outside in the Z-axis direction).

[0046] In the above configuration, the separator 140, the positive electrode active material layer 120 and the negative electrode active material layer 130 sandwiching the separator 140 in the Z-axis direction, and the positive electrode metal layer 111 and the negative electrode metal layer 112 sandwiching them in the Z-axis direction may be referred to as one energy storage element. In this case, the energy storage device 10 can also be said to be a group of energy storage elements having a configuration in which a plurality of energy storage elements stacked in the Z-axis direction are sandwiched between a pair of end members 300 in the Z-axis direction and are surrounded by a sealing member 200.

[0047] [2. Description of negative electrode active material layer 130] Next, the configuration of the negative electrode active material layer 130 of the electrode unit 100 will be described in more detail.

[0048] As shown in Fig. 3, a region (outer periphery) of the negative electrode active material layer 130 including the periphery (outer periphery) of the negative electrode active material layer 130 and having a width of 0.5 mm to 3 mm from the periphery is referred to as a peripheral portion 131. The peripheral portion 131 is a ring-shaped (quadrangle-shaped) portion arranged to surround the periphery of the negative electrode active material layer 130 (the entire circumference of the end portion in the positive direction of the X-axis, the end portion in the negative direction of the X-axis, the end portion in the positive direction of the Y-axis, and the end portion in the negative direction of the Y-axis). A portion of the negative electrode active material layer 130 that is located at the center of the negative electrode active material layer 130 in a plan view is referred to as a central portion 132. The central portion 132 is a portion within a predetermined region including the center of the negative electrode active material layer 130 in a plan view. The specified region is a region that is centered at the center of the negative electrode active material layer 130 and is located within a range of 1 / 3 to 1 / 2 of the length of the negative electrode active material layer 130 in the X-axis direction and within a range of 1 / 3 to 1 / 2 of the length of the negative electrode active material layer 130 in the Y-axis direction.

[0049] In the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass of active material per unit area on the surface of the current collector foil 110 than the central portion 132, and the density of the active material is lower. That is, the negative electrode active material layer 130 formed on the surface of the current collector foil 110 is divided into unit areas on the surface of the current collector foil 110 in a plan view, and the mass and density of the negative electrode active material contained in the negative electrode active material layer 130 are compared for each divided portion. In this case, the mass of the negative electrode active material contained in the divided portion located in the peripheral portion 131 is smaller than the mass of the negative electrode active material contained in the divided portion located in the central portion 132. Also, the density of the negative electrode active material contained in the divided portion located in the peripheral portion 131 is lower than the density of the negative electrode active material contained in the divided portion located in the central portion 132. The masses of the active materials are compared by taking out and measuring each of the portions to be compared. The density of the active material is compared by taking out portions of each material to be compared and measuring the density by Archimedes' method.

[0050] Specifically, in the negative electrode active material layer 130, the peripheral portion 131 at the end portions in two directions perpendicular to the stacking direction (Z-axis direction) and perpendicular to each other has a smaller mass of the active material and a lower density of the active material than the central portion 132. That is, in the negative electrode active material layer 130, the peripheral portion 131 at the end portions in the X-axis direction and the Y-axis direction has a smaller mass of the negative electrode active material and a lower density of the negative electrode active material than the central portion 132. In this embodiment, in the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass of the negative electrode active material and a lower density of the negative electrode active material than the central portion 132 at all end portions (entire circumference) in the X-axis positive direction, the X-axis negative direction, the Y-axis positive direction, and the Y-axis negative direction. It is preferable that the peripheral portion 131 at the end in the X-axis direction of the negative electrode active material layer 130 satisfies the above condition (the mass of the negative electrode active material is smaller and the density is lower than that of the central portion 132) from one end to the other end in the Y-axis direction, but a part of the portion from one end to the other end in the Y-axis direction may not satisfy the above condition. The same applies to the peripheral portion 131 at the end in the Y-axis direction of the negative electrode active material layer 130.

[0051] In this embodiment, the peripheral portion 131 is a portion of the negative electrode active material layer 130 that protrudes from the positive electrode active material layer 120 when viewed from the stacking direction (Z-axis direction). That is, the peripheral portion 131 is an annular (quadrangle-shaped) portion of the negative electrode active material layer 130 that includes a portion that protrudes from the positive electrode active material layer 120 in the X-axis positive direction, a portion that protrudes from the positive electrode active material layer 120 in the X-axis negative direction, a portion that protrudes from the positive electrode active material layer 120 in the Y-axis positive direction, and a portion that protrudes from the positive electrode active material layer 120 in the Y-axis negative direction. In this embodiment, the width of the peripheral portion 131 (the amount of protrusion from the positive electrode active material layer 120) is about 2 to 3 mm.

[0052] A portion disposed inside the peripheral portion 131 and adjacent to the peripheral portion 131 is referred to as an inner portion 133. The inner portion 133 is disposed adjacent to the peripheral portion 131 in the negative X-axis direction of the peripheral portion 131 protruding from the positive X-axis direction from the positive electrode active material layer 120. The inner portion 133 is disposed adjacent to the peripheral portion 131 in the positive X-axis direction of the peripheral portion 131 protruding from the positive X-axis direction from the positive electrode active material layer 120. The same applies to the Y-axis direction. In this way, the inner portion 133 is an annular (quadrangle-shaped) portion disposed adjacent to the peripheral portion 131 inside (inward) of the peripheral portion 131 when viewed from the Z-axis direction. The peripheral portion 131 does not face the positive electrode active material layer 120 in the Z-axis direction, whereas the inner portion 133 faces the positive electrode active material layer 120 in the Z-axis direction. In other words, the central portion 132 faces the central portion of the positive electrode active material layer 120 in the Z-axis direction, and the inner portion 133 faces the end portion (outer periphery) of the positive electrode active material layer 120 in the Z-axis direction.

[0053] In the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass of the active material and a lower density of the active material than the inner portion 133. That is, at the end in the positive direction of the X-axis of the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass of the negative electrode active material and a lower density of the negative electrode active material than the inner portion 133. The same is true for the end in the negative direction of the X-axis, the end in the positive direction of the Y-axis, and the end in the negative direction of the Y-axis of the negative electrode active material layer 130. In this way, at all ends (entire circumference) in the X-axis and Y-axis directions of the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass of the negative electrode active material and a lower density than the inner portion 133. It is preferable that the peripheral portion 131 at the end in the X-axis direction of the negative electrode active material layer 130 satisfies the above condition (the mass of the negative electrode active material is smaller and the density is lower than the inner portion 133) from one end to the other end in the Y-axis direction, but a part from one end to the other end in the Y-axis direction may not satisfy the above condition. The same applies to the peripheral portion 131 at the end portion in the Y-axis direction of the negative electrode active material layer 130.

[0054] In the negative electrode active material layer 130, the mass of the negative electrode active material in the peripheral portion 131 is preferably 0.1 to 0.9 times, more preferably 0.3 to 0.7 times, and even more preferably about 0.5 times, the mass of the negative electrode active material in the central portion 132 and the inner portion 133. The density of the negative electrode active material in the peripheral portion 131 is preferably 0.1 to 0.9 times, more preferably 0.3 to 0.7 times, and even more preferably about 0.5 times, the density of the negative electrode active material in the central portion 132 and the inner portion 133.

[0055] [3. Description of Manufacturing Method of Electricity Storage Device 10] Next, a method for manufacturing the energy storage device 10 will be described. FIG. 4 is a flowchart showing manufacturing steps in the method for manufacturing the energy storage device 10 according to the present embodiment. Specifically, FIG. 4 is a flowchart showing manufacturing steps in the method for manufacturing the electrode unit 100 in the method for manufacturing the energy storage device 10. FIG. 5 is a cross-sectional view showing manufacturing steps in the method for manufacturing the energy storage device 10 according to the present embodiment. Specifically, (a) of FIG. 5 shows a first arrangement step in the arrangement step in the method for manufacturing the energy storage device 10 (the method for manufacturing the electrode unit 100), and (b) of FIG. 5 shows a second arrangement step in the arrangement step in the method for manufacturing the energy storage device 10 (the method for manufacturing the electrode unit 100). (c) of FIG. 5 shows a pressing step in the method for manufacturing the energy storage device 10 (the method for manufacturing the electrode unit 100). FIG. 5 corresponds to (b) of FIG. 3, and the seal portion 210 of the electrode unit 100 is omitted.

[0056] First, an arrangement step is performed in which the negative electrode active material layer 130 is arranged on the current collector foil 110 so that it is larger in size than the positive electrode active material layer 120 when viewed from the stacking direction and so that the peripheral portion 131 has a smaller mass of active material per unit area on the surface of the current collector foil 110 than the central portion 132. In the arrangement step (when arranging the negative electrode active material layer 130 on the current collector foil 110), the negative electrode active material layer 130 is arranged on the other surface of the current collector foil 110, and then the positive electrode active material layer 120 is arranged on one surface of the current collector foil 110.

[0057] 4 and 5(a), in a first arrangement step of the arrangement steps, a current collector foil 110 is prepared, and the negative electrode active material layer 130 is arranged on the other surface (the surface in the negative Z-axis direction) of the current collector foil 110. At this time, the negative electrode active material layer 130 is arranged on the current collector foil 110 such that a peripheral portion 131 of the negative electrode active material layer 130 has a smaller mass of active material per unit area on the surface of the current collector foil 110 than a central portion 132.

[0058] Specifically, the negative electrode active material layer 130 is disposed on the current collector foil 110 so that the amount of the negative electrode active material disposed (applied) on the current collector foil 110 is smaller in the peripheral portion 131 than in the central portion 132. In other words, the negative electrode active material layer 130 is disposed on the current collector foil 110 so that the amount of the negative electrode active material applied to the current collector foil 110 is smaller around the entire circumference of the peripheral portion 131 than in the central portion 132. When applying the negative electrode active material, the amount of the negative electrode active material at both ends in the traveling direction during application can be reduced by applying using a tapered shim on the die head, and the amount of the negative electrode active material in the middle of the traveling direction can be reduced by applying intermittently. As a result, as shown in (a) of FIG. 5, the peripheral portion 131 is thinner in the Z-axis direction than the central portion 132. In this embodiment, the peripheral portion 131 has a shape in which the surface in the negative Z-axis direction is inclined so that the thickness in the Z-axis direction becomes thinner toward the outside (toward the outer edge (outer periphery) of the negative electrode active material layer 130).

[0059] Next, as shown in S104 of Fig. 4 and (b) of Fig. 5, as a second arrangement step of the arrangement steps, after the first arrangement step, the positive electrode active material layer 120 is arranged on one surface (the surface in the positive direction of the Z axis) of the current collector foil 110. Specifically, after the negative electrode active material layer 130 is arranged on the current collector foil 110 and dried in the first arrangement step, the positive electrode active material layer 120 is arranged on the current collector foil 110 so that the negative electrode active material layer 130 is larger in size than the positive electrode active material layer 120 when viewed from the Z axis direction. As a result, the negative electrode active material layer 130 is arranged on the current collector foil 110 so that the negative electrode active material layer 130 is larger in size than the positive electrode active material layer 120 when viewed from the stacking direction, and the peripheral portion 131 protrudes from the positive electrode active material layer 120 when viewed from the stacking direction.

[0060] Next, as shown in S106 of FIG. 4 and (c) of FIG. 5, the negative electrode active material layer 130 and the positive electrode active material layer 120 are pressed simultaneously in a pressing step, so that the negative electrode active material layer 130 is formed so that the peripheral portion 131 has a lower density of the active material than the central portion 132. Specifically, when the central portion 132 and the peripheral portion 131 of the negative electrode active material layer 130 are pressed, the thick central portion 132 is compressed more than the peripheral portion 131. As a result, the density of the negative electrode active material becomes higher in the central portion 132 than in the peripheral portion 131 (the density of the negative electrode active material becomes lower in the peripheral portion 131 than in the central portion 132). In other words, the central portion 132 and the peripheral portion 131 are compressed to approximately the same thickness, so that the density of the negative electrode active material becomes lower in the peripheral portion 131, which has a smaller amount of coating, than in the central portion 132.

[0061] As a result, in the negative electrode active material layer 130, the mass of active material per unit area on the surface of the current collector foil 110 is smaller and the density of the active material is lower in the peripheral portion 131 than in the central portion 132. Similarly, in the negative electrode active material layer 130, the mass of active material is smaller and the density of the active material is lower in the peripheral portion 131 than in the inner portion 133. That is, in the negative electrode active material layer 130, the mass of active material is smaller and the density of the active material is lower in the peripheral portion 131 at the ends in two directions perpendicular to the stacking direction (Z-axis direction) and perpendicular to each other than in the central portion 132 and the inner portion 133.

[0062] Thus, the manufacturing method of the electricity storage device 10 (the manufacturing method of the electrode unit 100) includes an arrangement step (first arrangement step and second arrangement step) and a pressing step. In the arrangement step (first arrangement step and second arrangement step), the end portion (portion including the peripheral portion 131) of the negative electrode active material layer 130 has a surface in the negative Z-axis direction that is inclined linearly (flat), but may be inclined curvedly (curved). After the pressing step (after the electrode unit 100 is manufactured), the multiple electrode units 100 and the end units 101 and 102 are stacked in the stacking direction with the separator 140 sandwiched therebetween, and are sandwiched between a pair of end members 300, thereby manufacturing the electricity storage device 10.

[0063] [4. Description of Effects] As described above, according to the electricity storage device 10 of the embodiment of the present invention, in the negative electrode active material layer 130 formed on the current collector foil 110, the mass of the active material in the peripheral portion 131 (the mass of the active material per unit area on the surface of the current collector foil 110) is smaller than the mass of the active material in the central portion 132. Furthermore, the density of the active material in the peripheral portion 131 is lower than the density of the active material in the central portion 132. That is, the amount of active material to be disposed in the peripheral portion 131 of the negative electrode active material layer 130, which is larger in size than the positive electrode active material layer 120, is made smaller than the amount of active material to be disposed in the central portion 132, and the negative electrode active material layer 130 is pressed. As a result, the mass of the active material in the peripheral portion 131 of the negative electrode active material layer 130 is smaller than that in the central portion 132, and the density of the active material is lower. Therefore, it is possible to prevent the thickness of the peripheral portion 131 of the negative electrode active material layer 130 from becoming thicker.

[0064] Specifically, it is as follows. Since the portion of the negative electrode active material layer 130 that protrudes from the positive electrode active material layer 120 does not have a support for the positive electrode active material layer 120, when the negative electrode active material layer 130 is arranged (applied) on the current collector foil 110, the amount (application amount) of the protruding portion may not be stable (may become large). When the negative electrode active material layer 130 is pressed, since the positive electrode active material layer 120 does not face the protruding portion, the protruding portion may not be pressed sufficiently. As a result, the thickness of the protruding portion becomes thick, and there is a risk of problems such as a large pressure being applied to the current collector foil 110 and the separator 140 when stacking the electrode units 100, or the current collector foil 110 being distorted and wrinkled, making stacking difficult. These wrinkles may cause the thickness of the seal portion 210 to become uneven when the electrode units 100 are stacked, or may cause gaps to form between the seal portion 210 and the current collecting foil 110, resulting in leakage of the electrolyte.

[0065] For this reason, the peripheral portion 131 of the negative electrode active material layer 130 is pressed with a smaller amount of active material than the central portion 132. As a result, the mass of the active material per unit area of ​​the peripheral portion 131 of the negative electrode active material layer 130 is smaller than that of the central portion 132, and the density of the active material is lower, so that the thickness of the peripheral portion 131 of the negative electrode active material layer 130 can be prevented from becoming thicker. There was also a problem that the pressing of the negative electrode active material layer 130 generates a stress difference between the portion where the negative electrode active material layer 130 is disposed and the portion where the negative electrode active material layer 130 is not disposed, causing distortion and forming wrinkles. In response to this, by reducing the mass of the active material and lowering the density of the active material in the peripheral portion 131 of the negative electrode active material layer 130, the distortion is gradually alleviated, and thus the occurrence of wrinkles can be prevented.

[0066] In many cases, the portion (protruding portion) of the negative electrode active material layer 130 that protrudes from the positive electrode active material layer 120 becomes thick. For this reason, in the negative electrode active material layer 130, the mass of the active material in the peripheral portion 131 that protrudes from the positive electrode active material layer 120 is made smaller than the mass of the active material in the inner portion 133 inside the peripheral portion 131, and the density of the active material in the peripheral portion 131 is made lower than the density of the active material in the inner portion 133. This makes it possible to prevent the thickness of the peripheral portion 131 (protruding portion) that protrudes from the positive electrode active material layer 120 in the negative electrode active material layer 130 from becoming thicker.

[0067] The mass of the active material in peripheral portion 131 at the ends in two directions (X-axis direction and Y-axis direction) of negative electrode active material layer 130 is made smaller than the mass of the active material in central portion 132, and the density of the active material in peripheral portion 131 is made lower than the density of the active material in central portion 132. This makes it possible to prevent peripheral portion 131 from becoming thicker at the ends in those two directions of negative electrode active material layer 130.

[0068] According to the method for manufacturing the electricity storage device 10 according to the embodiment of the present invention, the negative electrode active material layer 130 is disposed on the current collector foil 110 such that the mass of the active material is smaller in the peripheral portion 131 than in the central portion 132. Thereafter, the negative electrode active material layer 130 and the positive electrode active material layer 120 are pressed simultaneously to form the negative electrode active material layer 130 such that the density of the active material is lower in the peripheral portion 131 than in the central portion 132. This makes it possible to prevent the peripheral portion 131 of the negative electrode active material layer 130 from becoming thicker.

[0069] When the negative electrode active material layer 130, which is larger in size than the positive electrode active material layer 120, is arranged on the current collector foil 110, if the positive electrode active material layer 120 is not arranged on the current collector foil 110, the portion of the negative electrode active material layer 130 that protrudes from the positive electrode active material layer 120 will not receive the positive electrode active material layer 120. In this case, when the negative electrode active material layer 130 is arranged (applied) on the current collector foil 110, the amount (application amount) of the protruding portion may not be stable (become large). For this reason, after the negative electrode active material layer 130 is arranged on the current collector foil 110, the positive electrode active material layer 120 is arranged on the current collector foil 110. This allows the negative electrode active material layer 130 to be arranged on the current collector foil 110 in a more stable state, making it easier to adjust the amount of negative electrode active material arranged on the peripheral portion 131 of the negative electrode active material layer 130.

[0070] [5. Explanation of Variations] Although the electricity storage device 10 and the manufacturing method thereof according to the present embodiment have been described above, the present invention is not limited to the above embodiment. The embodiment disclosed herein is illustrative and not restrictive in all respects, and the scope of the present invention includes all modifications within the meaning and scope of the claims.

[0071] In the above embodiment, the current collecting foil 110 is formed of multiple layers (two layers) of the positive electrode metal layer 111 and the negative electrode metal layer 112, but the current collecting foil 110 may be formed of one layer (one metal foil). In other words, the current collecting foil 110 may be formed of a single sheet of stainless steel foil or the like, and the single sheet of stainless steel foil or the like may have the functions of both the positive electrode metal layer and the negative electrode metal layer.

[0072] In the above embodiment, the negative electrode active material layer 130 has a lower mass and density of the negative electrode active material in the peripheral portion 131 than in the central portion 132 at all ends (whole circumference) on both sides in the X-axis direction and both sides in the Y-axis direction, but is not limited thereto. The negative electrode active material layer 130 may have a lower mass and density of the negative electrode active material in the peripheral portion 131 than in the central portion 132 only at one end in the X-axis direction. The same applies to the Y-axis direction. The negative electrode active material layer 130 may have a lower mass and density of the negative electrode active material in the peripheral portion 131 than in the central portion 132 only at the end in the X-axis direction or only at the end in the Y-axis direction. When the negative electrode active material layer 130 does not have a quadrangular shape in plan view, it is sufficient that the negative electrode active material in the peripheral portion 131 is lower in mass and density than in the central portion 132 at the end in any direction in the XY plane.

[0073] In the above embodiment, the negative electrode active material layer 130 has a lower mass and density of the negative electrode active material in the peripheral portion 131 than the inner portion 133 at all ends (whole circumference) on both sides in the X-axis direction and both sides in the Y-axis direction, but is not limited thereto. The negative electrode active material layer 130 may have a lower mass and density of the negative electrode active material in the peripheral portion 131 than the inner portion 133 only at one end in the X-axis direction. The same applies to the Y-axis direction. The negative electrode active material layer 130 may have a lower mass and density of the negative electrode active material in the peripheral portion 131 than the inner portion 133 only at the end in the X-axis direction or only at the end in the Y-axis direction. When the negative electrode active material layer 130 does not have a quadrangular shape in plan view, it is sufficient that the negative electrode active material in the peripheral portion 131 is lower in mass and density than the inner portion 133 at the end in any direction in the XY plane.

[0074] In the above embodiment, in the negative electrode active material layer 130, the peripheral portion 131 has a smaller mass and a lower density of the negative electrode active material than the inner portion 133, but this is not limited thereto. It is sufficient that the peripheral portion 131 has a smaller mass and a lower density of the negative electrode active material than the central portion 132, and the mass and density of the negative electrode active material in the inner portion 133 are not particularly limited.

[0075] In the above embodiment, in the arrangement step of the manufacturing method of the electricity storage device 10 (the manufacturing method of the electrode unit 100), the negative electrode active material layer 130 is arranged on the current collector foil 110, and then the positive electrode active material layer 120 is arranged on the current collector foil 110, but this is not limited to the above. The positive electrode active material layer 120 may be arranged on the current collector foil 110, and then the negative electrode active material layer 130 may be arranged on the current collector foil 110. The positive electrode active material layer 120 and the negative electrode active material layer 130 may be arranged on the current collector foil 110 at the same time.

[0076] In the above embodiment, all of the electrode units 100 have the above configuration, but it is not necessary that any of the electrode units 100 have the above configuration. Although all of the electrode units 100 are manufactured by the above method, it is not necessary that any of the electrode units 100 are manufactured by the above method.

[0077] The electricity storage device 10 may be used in an electricity storage pack 1 as shown in FIG. 6. FIG. 6 is a cross-sectional view showing the configuration of the electricity storage pack 1. In FIG. 6, the internal configuration of the electricity storage device 10 is omitted. As shown in FIG. 6, the electricity storage pack 1 includes an electricity storage device stack 2 in which a plurality of electricity storage devices 10 are stacked, and a conductive member 3. In this case, the technology of the present invention may be applied to at least one electricity storage device 10 included in the electricity storage pack 1. Two adjacent electricity storage devices 10 in the electricity storage device stack 2 are electrically connected by contact or joining (welding, etc.). The conductive member 3 is made of a metal such as stainless steel, and the electricity storage device 10 located at the end in the stacking direction (Z-axis direction) and the conductive member 3 are electrically connected by contact or joining (welding, etc.). An adhesive may be used for the joining. The plurality of electricity storage devices 10 in the electricity storage device stack 2 are connected in series, and charging and discharging are performed via the conductive member 3. The electricity storage pack 1 may be restrained in the stacking direction (Z-axis direction) by using a restraining member such as a screw, a resin band, or a metal band. The electricity storage device stack 2 and the conductive member 3 may be housed in a metal case or a resin case.

[0078] As another example of the electricity storage pack 1, a configuration in which individual electricity storage devices 10 are housed in an exterior body 4 is shown in FIG. 7. FIG. 7 is a cross-sectional view showing the configuration of an electricity storage pack 1a. As shown in FIG. 7, the electricity storage device 10 of this configuration has a connection portion 5 exposed from the exterior body 4. A laminate film or the like can be used as the exterior body 4. The connection portions 5 of adjacent electricity storage devices 10 are electrically connected to each other by contact or bonding (welding, etc.). The connection portion 5 of the electricity storage device 10 located at the end in the stacking direction (Z-axis direction) and the conductive member 3 are electrically connected to each other by contact or bonding (welding, etc.). The other configuration is similar to that of the above-mentioned electricity storage pack 1, so a description thereof will be omitted.

[0079] Any combination of the components included in the above-described embodiment and its modified examples is also included within the scope of the present invention. [Industrial Applicability]

[0080] The present invention can be applied to electricity storage devices such as bipolar batteries. [Explanation of symbols]

[0081] 1, 1a storage pack 2. Electricity storage device laminate 3 Conductive materials 4 Exterior body 5 Connection part 10. Energy storage device 100 electrode units 101, 102 End unit 110 Current collecting foil 111 Positive electrode metal layer (metal layer) 112 Negative electrode metal layer (metal layer) 120 Cathode active material layer 130 Negative electrode active material layer 131 Periphery 132 Central part 133 Inner part 140 Separator 200 Sealing material 210, 220, 230 Seal part 300 End member

Claims

1. A plurality of electrode units are stacked in a stacking direction, each of the plurality of electrode units includes at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil; the negative electrode active material layer is larger in size than the positive electrode active material layer when viewed from the stacking direction, In the negative electrode active material layer, the mass of the active material per unit area on the surface of the current collector foil is smaller in the peripheral portion than in the central portion, and the density of the active material is also lower. Energy storage device.

2. the peripheral portion is a portion of the negative electrode active material layer that protrudes from the positive electrode active material layer when viewed from the stacking direction, the negative electrode active material layer has an inner portion disposed inside the peripheral portion and adjacent to the peripheral portion, The peripheral portion has a smaller mass of the active material and a lower density of the active material than the inner portion. The power storage device according to claim 1 .

3. In the negative electrode active material layer, the mass of the active material is smaller and the density of the active material is lower in the peripheral portion at the ends in two directions perpendicular to the stacking direction and perpendicular to each other than in the central portion. The power storage device according to claim 1 or 2.

4. A method for manufacturing an electricity storage device including a plurality of electrode units stacked in a stacking direction, comprising the steps of: each of the plurality of electrode units includes at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil; The method for manufacturing the electricity storage device includes: disposing the negative electrode active material layer on the current collector foil so that the negative electrode active material layer is larger in size than the positive electrode active material layer when viewed from the stacking direction and so that a mass of active material per unit area on a surface of the current collector foil is smaller at a peripheral portion than at a central portion; and pressing the negative electrode active material layer and the positive electrode active material layer simultaneously to form the negative electrode active material layer such that the peripheral portion has a lower active material density than the central portion. A method for manufacturing an electricity storage device.

5. When the negative electrode active material layer is disposed on the current collector foil, the negative electrode active material layer is disposed on the other surface of the current collector foil, and then the positive electrode active material layer is disposed on the one surface of the current collector foil. A method for manufacturing the electricity storage device according to claim 4.

Citation Information

Patent Citations

  • Sheet battery

    JP2000100471A