Optical member and manufacturing method of the same
The laser lift-off technique combined with controlled adhesive lamination addresses the issues of scattered light and structural defects in light extraction layers, achieving high-directivity light extraction and enhanced light distribution.
Patent Information
- Application Number
- JP2023068023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing methods for forming a light extraction layer using an inkjet method result in significant scattered light and poor light distribution characteristics, leading to inadequate light extraction directivity, and the formation of cracks and air bubbles in the porous layer.
A method involving a laser lift-off technique to pattern the porous layer, followed by careful lamination of adhesive layers under specific strain and thickness conditions to prevent cracks and air bubbles, ensuring high directivity and efficient light extraction.
The method effectively suppresses cracks and air bubbles in the porous layer, enabling high-directivity light extraction with improved light distribution characteristics.
Smart Images

Figure 2024154277000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical member and a method for producing the same. [Background technology]
[0002] A method of utilizing a light extraction layer having two regions with different refractive indexes is known as a method for extracting light from a light guide layer. Such a light extraction layer is disclosed in, for example, Patent Document 1.
[0003] Patent Document 1 discloses a method using an inkjet method as an example of a method for forming a light extraction layer. In this method, ink (e.g., an ink-formed pressure-sensitive adhesive) is filled in a predetermined pattern into the voids of a porous layer by the inkjet method, thereby forming a light extraction layer including a low refractive index region in which voids remain and a high refractive index region in which the voids are filled with ink, arranged in a predetermined pattern.
[0004] The entire disclosure of Patent Document 1 is incorporated herein by reference. In this specification, the light extraction layer in Patent Document 1 may be referred to as an "optical coupling layer." In addition, "extracting light" in Patent Document 1 may be referred to as "taking out light" or "coupling light." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2019 / 182100 Summary of the Invention [Problem to be solved by the invention]
[0006] In the light extraction layer formed by the inkjet method as disclosed in Patent Document 1, the influence of scattered light (diffused light) from the surrounding area of the high refractive index area is large, and the desired light distribution characteristics may not be obtained. Specifically, there are cases where light with sufficiently high directivity cannot be extracted.
[0007] Therefore, the applicant of the present application considered using a method of removing a part of the porous layer by irradiating the porous layer with a laser light, that is, a method of patterning the porous layer by a laser lift-off method, as described below, and found that by adopting such a method, it is possible to form a light extraction layer that can extract light with sufficiently high directivity.
[0008] However, after detailed investigation, the inventors of the present application found that in an optical component including a light extraction layer formed in this manner, there is a risk that cracks will occur around the through holes formed by patterning in the porous layer, or that air bubbles will remain inside the through holes.
[0009] An embodiment of the present invention has been made in consideration of the above-mentioned problems, and its purpose is to provide an optical component and a manufacturing method thereof in which at least one of the occurrence of cracks around the through holes of the porous layer and the remaining of air bubbles inside the through holes of the porous layer is suppressed. [Means for solving the problem]
[0010] According to an embodiment of the present invention, there are provided solutions as described in the following items.
[0011] [Item 1] A step A of preparing a porous film having a substrate and a porous layer provided on the substrate and having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; A step B of bonding a first adhesive layer to the side of the porous film opposite the substrate side at a first nip pressure; After the step B, a step C of peeling the substrate from the porous layer, and then bonding a second adhesive layer to the opposite side of the porous layer from the first adhesive layer with a second nip pressure; Inclusive of When the strain obtained from the compressive stress-strain curve of the first adhesive layer and the first nip pressure is ε1 and the thickness of the first adhesive layer is t1, Da1 expressed as Da1=ε1×t1 is taken as a calculated value of a first deformation amount, which is the deformation amount of the first adhesive layer during bonding in step B, The method for producing an optical member, wherein the step B is performed under conditions in which the calculated value Da1 of the first deformation amount is 250% or less of a thickness of the porous layer.
[0012] [Item 2] When the strain obtained from the compressive stress-strain curve of the first adhesive layer and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer and the second nip pressure is ε2, and the thickness of the second adhesive layer is t2, Da2 expressed as Da2=ε1'×t1+ε2×t2 is taken as a calculated value of a second deformation amount which is the sum of the deformation amounts of the first adhesive layer and the second adhesive layer during bonding in step C, 2. The method for producing an optical member according to item 1, wherein the step C is performed under conditions such that the calculated value Da2 of the second deformation amount is 875% or more of a thickness of the porous layer.
[0013] [Item 3] A step A of preparing a porous film having a substrate and a porous layer provided on the substrate and having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; A step B of bonding a first adhesive layer to the side of the porous film opposite the substrate side at a first nip pressure; After the step B, a step C of peeling the substrate from the porous layer, and then bonding a second adhesive layer to the opposite side of the porous layer from the first adhesive layer with a second nip pressure; Inclusive of When the strain obtained from the compressive stress-strain curve of the first adhesive layer and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer and the second nip pressure is ε2, the thickness of the first adhesive layer is t1, and the thickness of the second adhesive layer is t2, Da2 expressed as Da2=ε1'×t1+ε2×t2 is taken as a calculated value of a second deformation amount which is the sum of the deformation amounts of the first adhesive layer and the second adhesive layer during bonding in step C, The method for producing an optical member, wherein the step C is performed under conditions in which the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer.
[0014] [Item 4] 4. The method for producing an optical member according to any one of items 1 to 3, wherein the first nip pressure is 0.1 MPa or more and 0.74 MPa or less, and the thickness t1 of the first adhesive layer is 1.25 μm or more and 215 μm or less.
[0015] [Item 5] 4. The method for producing an optical member according to any one of items 1 to 3, wherein the first nip pressure is 0.1 MPa or more and 0.24 MPa or less, and the thickness t1 of the first adhesive layer is 1.25 μm or more and 107 μm or less.
[0016] [Item 6] 6. The method for producing an optical member according to any one of items 1 to 5, wherein the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and a sum of the thickness t1 of the first adhesive layer and the thickness t2 of the second adhesive layer is 3.34 μm or more and 417 μm or less.
[0017] [Item 7] 6. The method for producing an optical member according to any one of items 1 to 5, wherein the second nip pressure is 0.32 MPa or more and 1.15 MPa or less, and a sum of the thickness t1 of the first adhesive layer and the thickness t2 of the second adhesive layer is 3.82 μm or more and 421 μm or less.
[0018] [Item 8] The step A comprises: a step a1 of preparing the porous layer supported on the substrate; a step a2 of forming the plurality of through holes in the porous layer by irradiating the porous layer with a laser beam; 8. The method for producing an optical member according to any one of items 1 to 7, comprising:
[0019] [Item 9] A porous layer having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; a first adhesive layer in contact with one of the two main surfaces of the porous layer; a second adhesive layer in contact with the other of the two main surfaces of the porous layer; having each of the plurality of through holes is filled with the first adhesive layer and the second adhesive layer; An optical member, wherein the rate of through holes having cracks around them is 20% or less among the plurality of through holes.
[0020] [Item 10] Item 10. The optical member according to item 9, wherein the rate of through holes containing air bubbles among the plurality of through holes is 25% or less.
[0021] [Item 11] A porous layer having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; a first adhesive layer in contact with one of the two main surfaces of the porous layer; a second adhesive layer in contact with the other of the two main surfaces of the porous layer; having each of the plurality of through holes is filled with the first adhesive layer and the second adhesive layer; An optical member, wherein the rate of the through holes containing air bubbles among the plurality of through holes is 25% or less.
[0022] [Item 12] The sum of the thickness of the first adhesive layer and the thickness of the second adhesive layer is 421 μm or less; 12. The optical member according to any one of items 9 to 11, wherein the thickness of the first adhesive layer is 215 μm or less.
[0023] [Item 13] Item 13. The optical member according to any one of items 9 to 12, wherein the second adhesive layer has a thickness of 2.09 μm or more and 202 μm or less.
[0024] [Item 14] Item 14. The method for producing an optical member according to any one of items 9 to 13, wherein the thickness of the porous layer is 100 nm or more and 5000 nm or less.
[0025] [Item 15] Item 15. The method for producing an optical member according to any one of items 9 to 14, wherein the equivalent diameter of an isocircular ellipse of each of the plurality of through holes is 50 μm or more and 150 μm or less. Effect of the Invention
[0026] According to an embodiment of the present invention, an optical component and a manufacturing method thereof are provided in which at least one of the occurrence of cracks around the through holes of the porous layer and the remaining of air bubbles inside the through holes of the porous layer is suppressed. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of an optical element 100 having an optical member 1 obtained by a manufacturing method according to an embodiment of the present invention. [Diagram 2] 1 is a plan view showing an example of the arrangement of first regions 12 and second regions 14 in a first layer 10 of an optical member 1 (optical element 100). [Diagram 3] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of another optical element 200 having an optical member obtained by a manufacturing method according to an embodiment of the present invention. [Figure 4A] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Figure 4B] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Figure 4C] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Figure 4D] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Figure 4E] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Figure 4F] 1A to 1C are cross-sectional views illustrating a schematic diagram of one step of a manufacturing method according to an embodiment of the present invention. [Diagram 5] 1 is an optical microscope image of an optical member containing cracks and bubbles. [Figure 6A] FIG. 1 is a schematic diagram for explaining why cracks occur. [Figure 6B] FIG. 1 is a schematic diagram for explaining why cracks occur. [Figure 7] FIG. 1 is a schematic diagram for explaining why air bubbles are generated. [Figure 8] 1 is a graph showing evaluation results of the compression characteristics of adhesive layers formed using pressure sensitive adhesives A and B. [Figure 9] FIG. 13 shows examples of areas of a microscope image used to evaluate the incidence of cracks and bubbles. [Figure 10A] 1 is a graph in which the horizontal axis represents the calculated value Da1 of the first deformation amount, and the vertical axis represents the rate of crack occurrence. [Figure 10B] 13 is a graph in which the horizontal axis represents the calculated value Da2 of the second deformation amount, and the vertical axis represents the rate of bubble generation. [Figure 11A] This is a table showing the results of calculating the calculated value Da1 of the first deformation amount when adhesive A is used as the material of the first adhesive layer 20, the thickness t1 of the first adhesive layer 20 is in the range of 10 μm to 35 μm, and the first nip pressure is in the range of 0.1 MPa to 1.15 MPa. [Figure 11B] This is a table showing the results of calculating the calculated value Da1 of the first deformation amount when adhesive B is used as the material of the first adhesive layer 20, the thickness t1 of the first adhesive layer 20 is in the range of 10 μm to 28 μm, and the first nip pressure is in the range of 0.1 MPa to 1.15 MPa. [Figure 12A]This is a table showing the results of calculating the calculated value Da2 of the second deformation amount when adhesive A is used as the material for the first adhesive layer 20 and the second adhesive layer 30, the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 26 μm to 68 μm, and the second nip pressure is in the range of 0.1 MPa to 1.15 MPa. [Figure 12B] This is a table showing the results of calculating the calculated value Da2 of the second deformation amount when adhesive B is used as the material for the first adhesive layer 20 and the second adhesive layer 30, the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 21 μm to 54 μm, and the second nip pressure is in the range of 0.1 MPa to 1.15 MPa. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, an optical member and a manufacturing method thereof according to an embodiment of the present invention will be described with reference to the drawings. Note that the embodiment of the present invention is not limited to the examples given in the following description.
[0029] [Optical component configuration] Prior to the description of the manufacturing method according to the embodiment of the present invention, the configuration of an optical member manufactured using the manufacturing method according to the embodiment of the present invention will be described. The optical member described below can, for example, extract light propagating through the light guide layer from the main surface of the light guide layer, or guide it to an optical member arranged to be in contact with the main surface of the light guide layer. Guiding light propagating through the light guide layer to an optical member arranged to be in contact with the main surface of the light guide layer is called optical coupling, and a layer that acts in this way is called an optical coupling layer. The optical member described below is suitably used, for example, as an optical coupling layer of the light guide member described in WO 2022 / 025067. As described in WO 2022 / 025067, the optical coupling layer can be provided between the light guide layer and the direction conversion layer. The direction conversion layer has, for example, a plurality of internal spaces that form an interface that directs light toward the main surface side of the direction conversion layer by total internal reflection. Such a direction conversion layer having an internal space may be, for example, a light distribution structure disclosed in WO 2019 / 087118. The direction-changing layer may also be a known prism sheet. The entire disclosures of WO 2022 / 025067 and WO 2019 / 087118 are incorporated herein by reference.
[0030] 1 is a cross-sectional view that diagrammatically illustrates an optical element 100 having an optical member 1. As shown in FIG.
[0031] The optical member 1 has a first layer 10, a second layer 20 and a third layer 30 that face each other via the first layer 10, and a base layer 40 that supports the first layer 10, the second layer 20, and the third layer 30.
[0032] The second layer 20 and the third layer 30 are each adjacent to the first layer 10 in the layer normal direction, and the third layer 30 is located on the side opposite to the second layer 20 with respect to the first layer 10. That is, the second layer 20 is in contact with one of the two main surfaces of the first layer 10, and the third layer 30 is in contact with the other of the two main surfaces of the first layer 10. Each of the second layer 20 and the third layer 30 is an adhesive layer having adhesiveness. Hereinafter, the second layer 20 may be referred to as the "first adhesive layer", and the third layer 30 may be referred to as the "second adhesive layer". In the illustrated example, the first adhesive layer 20 is provided between the first layer 10 and the light guide layer 50, and the second adhesive layer 30 is provided between the first layer 10 and the base material layer 40.
[0033] The first layer 10 has a porous structure. Hereinafter, the first layer 10 is referred to as a "porous layer". The porous layer 10 has a plurality of through holes 14 in addition to the voids of the porous structure. The plurality of through holes 14 are discretely arranged in a plan view, and each is island-shaped. Hereinafter, in the porous layer 10, the region 12 other than the through holes 14, that is, the region 12 having a porous structure is referred to as the "first region". Also, the through holes 14, that is, the region having no porous structure may be referred to as the "second region". Each through hole 14 is filled with the first adhesive layer 20 and the second adhesive layer 30.
[0034] When the refractive index of the first region 12 is n1, the refractive index of the second region (through hole) 14 is n2, and the refractive index of the second layer (first adhesive layer) 20 is n3, n1 < n2 and n1 < n3. The refractive index n1 of the first region 12 is, for example, 1.30 or less. The refractive index n2 of the second region 14 and the refractive index n3 of the first adhesive layer 20 are each, for example, 1.43 or more. Also, when the refractive index of the third layer (second adhesive layer) 30 is n4, n1 < n4. The refractive index n2 of the second region 14, the refractive index n3 of the first adhesive layer 20, and the refractive index n4 of the second adhesive layer 30 may be substantially the same.
[0035] The first region 12 having a porous structure may be formed of, for example, a porous silica body. The porosity of the porous silica body is more than 0% and less than 100%. In order to obtain a low refractive index, the porosity of the porous silica body is preferably 40% or more, more preferably 50% or more, and even more preferably 55% or more. There is no particular upper limit to the porosity, but from the viewpoint of strength, it is preferably 95% or less, and even more preferably 85% or less. The refractive index of silica (the matrix portion of the porous silica body) is, for example, 1.41 or more and 1.43 or less.
[0036] In the present specification, the term "adhesive" is used to include pressure-sensitive adhesives (also called pressure-sensitive adhesives). Specific examples of adhesives for forming the first adhesive layer 20 and the second adhesive layer 30 include rubber-based adhesives, acrylic adhesives, silicone-based adhesives, epoxy adhesives, cellulose adhesives, and polyester adhesives. These adhesives may be used alone or in combination of two or more. From the viewpoint of suppressing embedding of the adhesive in the first region 12 of the porous layer 10 (i.e., in the voids of the porous structure), the first adhesive layer 20 and the second adhesive layer 30 are preferably formed from a highly elastic pressure-sensitive adhesive, and more specifically, are preferably formed from a pressure-sensitive adhesive having a nanoindentation hardness of 0.1 MPa or more and 1.0 MPa or less, as measured by pressing an indenter 2000 nm into the first region 12 of the porous layer 10. The nanoindentation hardness is expressed as Pmax / A, using the maximum load Pmax and the contact projected area A obtained by measuring a sample for measurement cut into a size of about 1 cm square and fixed to a predetermined support.
[0037] The first layer 10, which functions as a light coupling layer (light extraction layer), is obtained by arranging the first regions 12 and the second regions 14 in a predetermined pattern. The light coupling layer is disposed between two optical layers, for example between a light guide layer and a light redirecting layer, and directs a portion of the light propagating through the light guide layer to the light redirecting layer. The light redirecting layer has, for example, an interface (or surface) that imparts a layer normal component to the propagating light. The light redirecting layer can be, for example, a prism sheet.
[0038] The optical element 100 having the above-described configuration functions as follows.
[0039] 1 shows an X direction, a Y direction, and a Z direction which are perpendicular to each other. Here, each layer of the optical element 100 has a main surface parallel to the XY plane. Light emitted from the light source LS toward a light receiving end surface (not shown) of the light guide layer 50 propagates in the Y direction within the light guide layer 50 (guided light L P A part of the light incident on the light guide layer 50 is optically coupled (extracted) to the base layer 40 by the first layer 10, the second layer 20, and the third layer 30, and is output in the Z direction (output light L E ) Of course, the light propagation direction has variation (distribution) from the Y direction, and the light emission direction also has variation (distribution) from the Z direction.
[0040] Light L propagating in the light guide layer 50 P Of these, the light incident on the interface between the second layer 20 and the first region 12 of the first layer 10 is totally internally reflected. In contrast, the light incident on the interface between the second layer 20 and the second region 14 of the first layer 10 passes through the second region 14 of the first layer 10, the third layer 30, and the base layer 40 without being totally internally reflected, and is emitted from the optical element 100.
[0041] By adjusting the arrangement of the first region 12 and the second region 14 of the first layer 10 in the layer plane (plane parallel to the XY plane), it is possible to control the light distribution (emission intensity distribution, emission angle distribution, etc.) of the light extracted from the light guide layer 50 (coupled with the base layer 40) by the optical member 1. The arrangement of the first region 12 and the second region 14 in the first layer 10 is appropriately set according to the required light distribution.
[0042] FIG. 2 is a diagram showing an example of the arrangement of the first regions 12 and the second regions 14 in the first layer 10. In the example shown in FIG. 2, a plurality of circular second regions 14 are discretely arranged in the first layer 10. The diameter of the second regions 14 is, for example, about 1 μm or more and about 1000 μm or less. In addition, the pitch Px of the second regions 14 adjacent in the X direction and the pitch Py of the second regions 14 adjacent in the Y direction are, independently, for example, about 2 μm or more and about 5000 μm or less. The pitches Px and Py are the distances between the centers (area centers of gravity) of the second regions 14 adjacent in the X direction and the Y direction, respectively.
[0043] The arrangement of the first regions 12 and the second regions 14 in the first layer 10 may be modified in various ways. In addition, the shape of the second regions 14 is not limited to the circular shape exemplified, and may be various shapes.
[0044] The shape, size, density in the plane of the first layer 10, and occupancy rate in the first layer 10 of the second region 14 may be appropriately changed depending on the purpose and application of the optical member 1 (optical element 100). For example, when good visibility such as transparency is required, the major axis of each of the second regions 14 is preferably 100 μm or less, more preferably 70 μm or less. For example, when the second region 14 is circular as shown in FIG. 2, the diameter of the circle is preferably 100 μm or less. By making the major axis of the second region 14 100 μm or less, it is possible to suppress the second region 14 from being viewed in applications in which a device equipped with the optical member 1 is observed at a relatively close distance, such as a mobile display or a small signage. When the second region 14 is not circular, the size of the second region 14 can be evaluated, for example, by the equivalent diameter of an isocircular ellipse. The equivalent diameter of the isocircular ellipse of the second region (through hole) 14 is, for example, 50 μm or more and 150 μm or less.
[0045] The optical component (and the optical element having the same) manufactured by the manufacturing method according to the embodiment of the present invention need only include the above-mentioned first layer 10, second layer 20 and third layer 30, and various modifications are possible.
[0046] Fig. 3 shows another optical element 200 having an optical member manufactured by a manufacturing method according to an embodiment of the present invention. The optical element 200 shown in Fig. 3 differs from the optical element 100 shown in Fig. 1 in that it further has a light distribution control structure having a plurality of internal spaces IS.
[0047] In the illustrated example, the light distribution control structure having multiple internal spaces IS is formed in a direction changing layer 70 provided on a base layer 40. The direction changing layer 70 is composed of a shaped film 72 having a main surface with multiple recesses 74, and an adhesive layer 76 disposed between the shaped film 72 and the base layer 40. The multiple internal spaces IS of the light distribution control structure are defined by the multiple recesses 74 of the shaped film 72 and the adhesive layer 76, and form an interface that directs a portion of the light propagating within the base layer 40 toward the light output surface side by total internal reflection (TIR).
[0048] [Method of manufacturing optical components] A method for producing the optical member 1 according to an embodiment of the present invention will be described.
[0049] A manufacturing method according to an embodiment of the present invention includes step A of preparing a porous film having a substrate and a porous layer provided on the substrate and having a plurality of through holes; step B of bonding a first adhesive layer to the side of the porous film opposite the substrate side at a first nip pressure; and step C of peeling the substrate from the porous layer after step B, and then bonding a second adhesive layer to the side of the porous layer opposite the first adhesive layer at a second nip pressure.
[0050] Here, when the strain obtained from the compressive stress-strain curve of the first adhesive layer and the first nip pressure is ε1 and the thickness of the first adhesive layer is t1, Da1 expressed as Da1=ε1×t1 is taken as the calculated value of the first deformation amount, which is the deformation amount of the first adhesive layer during lamination in process B. In addition, when the strain obtained from the compressive stress-strain curve of the first adhesive layer and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer and the second nip pressure is ε2, and the thickness of the second adhesive layer is t2, Da2 expressed as Da2=ε1'×t1+ε2×t2 is taken as the calculated value of the second deformation amount, which is the sum of the deformation amounts of the first adhesive layer and the second adhesive layer during lamination in process C.
[0051] In a manufacturing method according to an embodiment of the present invention, step B is performed under conditions where the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer, and / or step C is performed under conditions where the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer, thereby suppressing at least one of the occurrence of cracks around the through holes of the porous layer and the remaining of air bubbles inside the through holes of the porous layer, as described below.
[0052] A specific example of a manufacturing method according to an embodiment of the present invention will be described with reference to FIGS. 4A to 4F.
[0053] First, as shown in FIG. 4A, a porous film PF having a substrate 40T and a porous layer 10 is prepared. For example, the porous layer 10 is formed on the substrate 40T. The porous layer 10 is provided on the substrate 40T (i.e., supported by the substrate 40T) and has a porous structure. The substrate 40T may be a film formed from a resin. For example, a polyimide (PI) film or a black polyethylene terephthalate (PET) film may be used as the substrate 40T. The porous layer 10 may be formed on the substrate 40T via another functional layer. For example, the porous layer 10 may be formed on the substrate 40T via a barrier layer for suppressing the penetration of the adhesive into the voids of the porous layer 10. The porous layer 10 may be formed, for example, by a method exemplified later.
[0054] In the illustrated example, a release layer 2 is provided on the substrate 40T, and the porous layer 10 is formed on the release layer 2. The release layer 2 is formed from a material (e.g., cycloolefin polymer) that has high releasability to the porous layer 10. The release layer 2 may be provided with laser light absorbency. The release layer 2 may be omitted. When the release layer 2 is provided, the transfer and peeling of the porous layer 10 (the step shown in FIG. 4D) described below can be performed more easily (i.e., the peelability of the porous layer 10 can be improved).
[0055] The thickness of the peeling layer 2 is, for example, 1000 nm or less. However, if the peeling layer 2 is relatively thick, cracks may occur in the porous layer 10 in the subsequent step of irradiating the porous layer 10 with laser light. From the viewpoint of suppressing cracks in the porous layer 10, the thickness of the peeling layer 2 is preferably 500 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less. Note that when a material from which the porous layer 10 is easily peeled (e.g., polyimide) is used as the material of the substrate 40T, the peeling layer 2 may be omitted.
[0056] The release layer 2 is preferably composed mainly of a polymer that does not contain a polar group (hereinafter also referred to as a "non-polar polymer"). Incidentally, "not containing a polar group" means that the main chain skeleton and the side chain skeleton, excluding the main chain terminals of the polymer, do not contain a polar group. The main chain terminals of the polymer may contain a polar group derived from an initiator or a quencher. Furthermore, "composed mainly of a polymer that does not contain a polar group" means that the non-polar polymer content of the release layer 2 is 50% by mass or more. The non-polar polymer content of the release layer 2 is preferably 80% by mass or more. Examples of non-polar polymers include polyolefin-based polymers, cycloolefin-based polymers such as polynorbornene-based polymers, and polystyrene-based polymers. Among these, cycloolefin-based polymers and polyolefin-based polymers are preferred, and cycloolefin-based polymers are particularly preferred.
[0057] 4B, the porous layer 10 is irradiated with laser light LB to form a plurality of through holes 14 in the porous layer 10. That is, in this step, the porous layer 10 is patterned by a laser lift-off method.
[0058] As the laser light LB, an ultraviolet laser light can be preferably used. Although laser light other than an ultraviolet laser light (e.g., an infrared laser light) can also be used, the use of an ultraviolet laser light allows the porous layer 10 to be preferably removed even in a fine pattern. The wavelength range of the ultraviolet laser light is preferably 150 nm or more and 380 nm or less, and more preferably 190 nm or more and 360 nm or less. For example, laser light with wavelengths of 193 nm, 248 nm, 308 nm, and 351 nm can be obtained from an ArF excimer laser light source, a KrF excimer laser light source, a XeCL excimer laser light source, and a XeF excimer laser light source, respectively.
[0059] The amount of light irradiation required to remove the porous layer 10 can be appropriately set by adjusting the intensity of the irradiated light, the irradiation time, etc. In addition, the removal of the porous layer 10 can be suitably performed by appropriately setting the absorption coefficient of the substrate 40T according to the wavelength range of the laser light LB used. Specifically, when the absorption coefficient of the substrate 40T for the laser light LB used is 500 cm -1 For example, when an ultraviolet laser beam having a wavelength of 355 nm is used as the laser beam LB, the absorption coefficient of the substrate 40T for the light having a wavelength of 355 nm is preferably 500 cm -1 If the thickness of the substrate 40T is L, the light intensity obtained by subtracting the intensity of the reflected light from the intensity of the incident light is I0, and the intensity of the light after passing through the substrate 40T is I, the absorption coefficient α is expressed as -αL=log 10 (I / I0) relationship (derived from the Beer-Lambert equation).
[0060] When using ultraviolet laser light, from the viewpoint of improving processing efficiency and productivity, it is preferable that the absorption coefficient of the substrate 40T for the ultraviolet laser light is 1000 cm -1It is more preferable that the above is the case. As the material for such substrate 40T, for example, polyethylene naphthalate (PEN) and polyimide can be suitably used, and from the viewpoint of cost, polyethylene naphthalate can be particularly suitably used.
[0061] The light intensity distribution of the laser light (beam) LB is, for example, a Gaussian type or a top hat type. If the light intensity distribution of the laser light LB is a top hat type, the energy provided by irradiation of the laser light LB can be easily made uniform within the irradiation region.
[0062] The beam shape may be circular or rectangular. The beam may be focused using a focusing optical system such as an objective lens. When the beam shape is circular, the focal spot diameter (spot diameter) is preferably in the range of 1 μm to 200 μm, more preferably 20 μm to 120 μm.
[0063] From the viewpoint of forming a pattern in a short time, it is preferable to use a pulsed laser, and it is preferable to use a laser having a pulse width on the order of nanoseconds to microseconds. The repetition frequency of the pulsed laser light is not particularly limited, but from the viewpoint of productivity, the higher the repetition frequency, the more preferable, and can be appropriately adjusted within the range of 10 kHz to 5000 kHz.
[0064] Examples of types of laser oscillators that satisfy the above requirements include excimer lasers, YAG lasers, YLF lasers, YVO4 lasers, fiber lasers, and semiconductor lasers.
[0065] The irradiation conditions of the laser light LB can be set to any appropriate conditions, but the energy density is, for example, 0.1 J / cm 2 More than 5J / cm 2 It is preferable that:
[0066] From the viewpoint of performing the desired pattern processing at high speed, it is preferable to use a scanner unit that is a galvano scanner or a polygon scanner, or a combination of them. By using such a scanner unit, it is possible to form a pattern at a scan speed in the range of 0.01 m / sec to 170 m / sec in the scanning direction of the laser light. The pitch of the pattern can be arbitrarily set by adjusting the repetition frequency of the laser pulse according to the scan speed, and can be set, for example, in the range of 10 μm to 500 μm.
[0067] The pattern pitch in the direction perpendicular to the scanning direction can be appropriately adjusted by controlling the relative positional relationship between the scanner unit and the object to be irradiated. Such control can be performed by using a precision stage having a drive shaft, for example, by adsorbing and fixing a sheet of the object to be irradiated on the stage surface, and irradiating it with laser light while feeding it at regular intervals in the direction perpendicular to the scanning direction, thereby forming a pattern at a desired pitch. Alternatively, a long roll of the original material that has been wound up can be intermittently or continuously transported by a roll-to-roll transport method, and a pattern can be formed using a scanner unit.
[0068] 4C, the first adhesive layer 20 is bonded to the side of the porous film PF opposite to the substrate 40T side. Specifically, the first adhesive layer 20 formed on the release sheet 61 is bonded by a roller. The nip pressure at this time is hereinafter referred to as the "first nip pressure."
[0069] 4D, the substrate 40T is peeled off from the porous layer 10 (it can be said that the porous layer 10 is transferred). In the illustrated example, since the release layer 2 is formed on the substrate 40T, the substrate 40T is peeled off together with the release layer 2 from the porous layer 10.
[0070] Next, as shown in FIG. 4E, the second adhesive layer 30 is attached to the opposite side of the porous layer 10 to the first adhesive layer 20. Specifically, the second adhesive layer 30 formed on the release sheet 62 is attached by a roller. The nip pressure at this time is hereinafter referred to as the "second nip pressure". At this time, the region of the porous layer 10 where the porous structure remains becomes the first region 12. Furthermore, the multiple through holes 14 formed in the porous layer 10 are filled with the first adhesive layer 20 and the second adhesive layer 30, so that each through hole 14 becomes the second region 14. In this way, the first layer 10 including the first region 12 and the second region 14 is obtained.
[0071] 4F, the release sheet 62 is peeled off, and the base layer 40 is attached to the second adhesive layer 30, thereby obtaining the optical member 1. After that, the release sheet 61 is peeled off, and the light guide layer 50 is attached to the first adhesive layer 20, thereby obtaining the optical element 100.
[0072] In the above-described manufacturing method, the first adhesive layer 20 deforms during lamination in the step shown in Fig. 4C, and the first adhesive layer 20 and the second adhesive layer 30 deform during lamination in the step shown in Fig. 4E. Hereinafter, the amount of deformation of the first adhesive layer 20 during the former lamination is referred to as the "first deformation amount," and the sum of the amounts of deformation of the first adhesive layer 20 and the second adhesive layer 30 during the latter lamination is referred to as the "second deformation amount."
[0073] Here, if the strain obtained from the compressive stress-strain curve of the first adhesive layer 20 and the first nip pressure is ε1 and the thickness of the first adhesive layer 20 is t1, the calculated value Da1 of the first deformation amount is expressed by the following formula (1). Da1 = ε1 × t1 (1)
[0074] Furthermore, if the strain obtained from the compressive stress-strain curve of the first adhesive layer 20 and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer 30 and the second nip pressure is ε2, and the thickness of the second adhesive layer 30 is t2, then the calculated value Da2 of the second deformation amount is expressed by the following equation (2). Da2=ε1'×t1+ε2×t2 (2)
[0075] In the manufacturing method according to the embodiment of the present invention, the first adhesive layer 20 is bonded under the condition that the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer 10, thereby suppressing the occurrence of cracks around the through-holes 14 of the porous layer 10. Alternatively, in the manufacturing method according to the embodiment of the present invention, the second adhesive layer 30 is bonded under the condition that the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer 10, thereby suppressing the remaining of air bubbles inside the through-holes 14 of the porous layer 10. Furthermore, in the manufacturing method according to the embodiment of the present invention, the first adhesive layer 20 may be bonded under the condition that the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer 10, and the second adhesive layer 30 may be bonded under the condition that the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer 10. As a result, both the occurrence of cracks and the remaining of air bubbles are suppressed. Hereinafter, the reason why the above-mentioned effects are obtained will be explained.
[0076] According to the research of the present inventors, it was found that in an optical component having a porous layer patterned by a laser lift-off method and a first adhesive layer and a second adhesive layer arranged on either side of the porous layer, cracks occur around the through holes in the porous layer and air bubbles remain inside the through holes.
[0077] Fig. 5 is a microscope image of an optical member in which such cracks and bubbles exist. Fig. 5 shows an area including six through holes. In the example shown in Fig. 5, cracks Cr have occurred around the through hole at the lower right. Also, bubbles Bu remain in the through holes at the upper left, upper right, and lower left.
[0078] In order to identify the process in which the cracks Cr and bubbles Bu occur, the inventors of the present application performed microscopic observations after each process was performed and found that the cracks Cr occurred in the process of transferring and peeling off the porous layer 10 (the process shown in FIG. 4D), and the bubbles Bu occurred in the process of bonding the second adhesive layer 30 (the process shown in FIG. 4E).
[0079] The cracks Cr are believed to occur due to the following mechanism. First, as shown in FIG. 6A, when the first adhesive layer 20 is bonded, the adhesive of the first adhesive layer 20 is compressed and embedded in the through holes 14 of the porous layer 10, and is attached to the substrate 40T. Then, as shown in FIG. 6B, when the porous layer 10 is transferred and peeled off, the adhesive attached to the substrate 40T is stretched, and the porous layer 10 is also stretched, which may cause cracks Cr. Since the cracks Cr are believed to occur due to such a mechanism, it is presumed that the more adhesive is embedded in the through holes 14 when the first adhesive layer 20 is bonded, that is, the greater the deformation amount of the first adhesive layer 20, the more likely cracks Cr will occur.
[0080] The air bubbles Bu are believed to be generated by the following mechanism. As shown in Fig. 7, air bubbles Bu may be generated due to an insufficient amount of adhesive (the adhesive of the first adhesive layer 20 and the second adhesive layer 30) that is compressed and embedded in the through-holes 14 of the porous layer 10 when the second adhesive layer 30 is attached. Since the air bubbles Bu are believed to be generated by such a mechanism, it is presumed that the less adhesive is embedded in the through-holes 14 when the second adhesive layer 30 is attached, that is, the smaller the deformation amount of the first adhesive layer 20 and the second adhesive layer 30, the more likely the air bubbles Bu will be generated.
[0081] Based on the above-mentioned assumption, the first deformation amount and the second deformation amount that suppress the occurrence of cracks and bubbles were verified. The results of the verification are described below.
[0082] First, two types of adhesives (referred to as "Adhesive A" and "Adhesive B") were prepared as materials for the first adhesive layer 20 and the second adhesive layer 30, and adhesive layers were formed using these adhesives, and their compression properties were evaluated. Preparation of Adhesive A and Adhesive B and formation of the adhesive layers were performed as follows.
[0083] [Preparation of adhesive A and formation of adhesive layer] An adhesive layer was formed using pressure sensitive adhesive A according to the following steps (1) to (3).
[0084] (1) Preparation of (meth)acrylic polymer A monomer mixture containing 79.5 parts by mass of butyl acrylate, 15 parts by mass of N-acryloylmorpholine, 5 parts by mass of acrylic acid, and 0.5 parts by mass of 4-hydroxybutyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 70 parts by mass of ethyl acetate per 100 parts by mass of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was carried out for 2 hours to prepare a solution of a (meth)acrylic polymer with a weight average molecular weight (Mw) of 3 million and Mw / Mn=2.5.
[0085] (2) Preparation of Pressure Sensitive Adhesive Composition 0.2 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate) and 0.2 parts by mass of an epoxy crosslinking agent 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (trade name "Tetrad C" manufactured by Mitsubishi Gas Chemical Company, Inc.) were blended with 100 parts by mass of the solid content of the obtained (meth)acrylic polymer solution to prepare a solution of an acrylic pressure-sensitive adhesive composition.
[0086] (3) Formation of adhesive layer The obtained solution of the acrylic pressure-sensitive adhesive composition was applied to one side of a polyethylene terephthalate film (separator film: MRF38, manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.) treated with a silicone-based release agent so that the adhesive layer would have a thickness of 10 μm after drying, and was dried at 155° C. for 1 minute to form an adhesive layer on the surface of the separator film.
[0087] [Preparation of adhesive B and formation of adhesive layer] An adhesive layer was formed using pressure sensitive adhesive B according to the following steps (1) to (3).
[0088] (1) Preparation of acrylic polymer solution In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 90.7 parts by mass of butyl acrylate, 6 parts by mass of N-acryloylmorpholine, 3 parts by mass of acrylic acid, 0.3 parts by mass of 2-hydroxybutyl acrylate, and 0.1 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator were placed together with 100 g of ethyl acetate. Next, nitrogen gas was introduced while gently stirring the contents in the flask to replace with nitrogen. Thereafter, the liquid temperature in the flask was kept at around 55°C and a polymerization reaction was carried out for 8 hours to prepare an acrylic polymer solution.
[0089] (2) Preparation of Pressure Sensitive Adhesive Composition An acrylic adhesive composition (acrylic adhesive solution) was prepared by blending 0.2 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate), 0.3 parts by mass of benzoyl peroxide (trade name "Niper BMT" manufactured by Nippon Oil & Fats Corporation), and 0.1 parts by mass of γ-glycidoxypropylmethoxysilane (trade name "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts by mass of the solid content of the obtained acrylic polymer solution.
[0090] (3) Formation of adhesive layer The obtained acrylic pressure-sensitive adhesive composition was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness: 38 μm) so that the adhesive layer would have a thickness of 10 μm after drying, and the coating was dried at 150° C. for 3 minutes to form an adhesive layer.
[0091] The compression characteristics of the two types of adhesive layers formed as described above were evaluated using a nanoindenter (Triboindenter manufactured by Hysitron). The evaluation results are shown in Figure 8. Figure 8 shows the measurement results of the adhesive layer formed using adhesive A and the adhesive layer formed using adhesive B using the nanoindenter, as well as the compressive stress-strain curves obtained by power approximation of the results.
[0092] The strain of the adhesive layer during lamination can be obtained from the compressive stress-strain curve for the adhesive layer and the nip pressure during lamination, and the amount of deformation of the adhesive layer during lamination can be calculated by multiplying the obtained strain by the thickness of the adhesive layer.
[0093] Next, the two types of pressure sensitive adhesives A and B prepared above were used as materials for the adhesive layer to fabricate various optical members (Examples 1 to 12) as described below.
[0094] [Example 1] (1) Preparation of substrate and formation of release layer As the substrate 40T, a PEN film (Q51 manufactured by Toyobo Co., Ltd.) having a thickness of 50 μm was prepared, and a release layer 2 was formed thereon in the following manner.
[0095] The coating liquid for forming the release layer 2 (coating liquid for forming the release layer) was prepared by adding cycloolefin polymer (COP) (ZEONEX T62R manufactured by Zeon Corporation) to ethylcyclohexane to a concentration of 8 mass %, and stirring and mixing with a stirrer at room temperature until the COP was dissolved by visual observation. The coating liquid for forming the release layer was applied to one side of a PEN film, and then dried at 120°C for 3 minutes to form a release layer 2 with a thickness of 144 nm. The thickness of the release layer 2 was measured using a microspectrophotometer (the same applies to other examples).
[0096] (2) Formation of porous layer The coating liquid for forming the porous layer 10 was prepared as follows.
[0097] (2-1) Gelation of silicon compounds 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a gel-like silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare mixed solution C. 0.5 g of 0.01 mol / L oxalic acid solution was added to this mixed solution C, and the mixture was stirred at room temperature for 30 minutes to hydrolyze MTMS, producing mixed solution D containing tris(hydroxy)methylsilane.
[0098] To 5.5 g of DMSO, 0.38 g of 28% by mass ammonia water and 0.2 g of pure water were added, and then the above mixed solution D was further added and stirred at room temperature for 15 minutes to gel tris(hydroxy)methylsilane, thereby obtaining mixed solution E containing a gel-like silicon compound (polymethylsilsesquioxane).
[0099] (2-2) Aging treatment The mixed solution E containing the gel-like silicon compound prepared as above was incubated as it was at 40° C. for 20 hours for maturation treatment.
[0100] (2-3) Crushing Next, the gel-like silicon compound aged as described above was crushed into granules of several mm to several cm in size using a spatula. Next, 40 g of isopropyl alcohol (IPA) was added to the mixed liquid E, and after light stirring, the mixture was left to stand at room temperature for 6 hours, and the solvent and catalyst in the gel were decanted. The same decantation process was performed three times to replace the solvent and obtain a mixed liquid F. Next, the gel-like silicon compound in the mixed liquid F was crushed (high-pressure media-less crushing). The crushing process (high-pressure media-less crushing) was performed using a homogenizer (manufactured by SMT Co., Ltd.: product name UH-50), and 1.85 g of the gel-like compound and 1.15 g of IPA in the mixed liquid F were weighed into a 5 cc screw bottle, and crushed for 2 minutes under the conditions of 50 W and 20 kHz.
[0101] The gel-like silicon compound in the mixed liquid F was pulverized by this pulverization process, and the mixed liquid F' became a sol liquid of the pulverized material. The volume average particle size indicating the particle size variation of the pulverized material contained in the mixed liquid F' was confirmed to be 0.50 to 0.70 by using a dynamic light scattering nanotrack particle size analyzer (UPA-EX150 type manufactured by Nikkiso Co., Ltd.). Furthermore, 0.062 g of a 1.5 mass % concentration MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd.: product name WPBG266) and 0.036 g of a 5% concentration MEK solution of bis(trimethoxysilyl)ethane were added to 0.75 g of this sol liquid (mixed liquid C') to obtain a coating liquid for forming a porous layer. The coating liquid for forming a porous layer contains a silica porous body containing silsesquioxane as a basic structure.
[0102] The coating solution for forming the porous layer was applied onto the release layer 2 so that the thickness of the coating film after drying would be 800 nm to form a coating film. The coating film was left to stand for 1 minute and then dried at 100°C for 2 minutes. The dried coating film was irradiated with 300 mJ / cm using light with a wavelength of 360 nm. 2 A laminate (porous film) PF was obtained in which a release layer 2 and a porous layer 10 (a silica porous body formed by chemical bonding between silica microporous particles) were formed on a black PET film. The refractive index of the porous layer 10 was 1.15.
[0103] (3) Patterning of the porous layer by laser lift-off method The obtained porous film PF was irradiated with ultraviolet laser light under the following conditions to form a plurality of through holes 14 in the porous layer 10. Laser oscillator: Spectra-Physics Talon355-20 Wavelength: 355nm Scanner: ScanLab IntelliScan14 (galvanometer scanner) Beam Intensity Distribution: Gaussian Focused spot size: φ80μm Repetition frequency: 50kHz Pattern pitch: 200μm Power: 2.0W Pulse energy: 40μJ
[0104] (4) Fabrication of optical components The porous film PF having the porous layer 10 patterned as described above was used to fabricate an optical member in the state shown in FIG. 4E. The first adhesive layer 20 and the second adhesive layer 30 were each formed to a thickness of 17 μm using the pressure sensitive adhesive A. The first nip pressure during lamination of the first adhesive layer 20 was 0.24 MPa, and the second nip pressure during lamination of the second adhesive layer 30 was 1.15 MPa. Each of the through holes 14 in the porous layer 10 was substantially circular (diameter approximately 93 μm) in plan view. The area ratio (design value) of the multiple through holes 14 in the porous layer 10 was 17.0%.
[0105] [Example 2] An optical member was produced in the same manner as in Example 1, except that the thickness of the first adhesive layer 20 was 10 μm.
[0106] [Example 3] An optical member was produced in the same manner as in Example 1, except that the first adhesive layer 20 had a thickness of 10 μm and the second adhesive layer 30 had a thickness of 20 μm.
[0107] [Example 4] An optical member was produced in the same manner as in Example 1, except that the thickness of the second adhesive layer 30 was 10 μm.
[0108] [Example 5] An optical member was produced in the same manner as in Example 1, except that the first nip pressure was 0.61 MPa and the thickness of the second adhesive layer 30 was 20 μm.
[0109] [Example 6] An optical member was produced in the same manner as in Example 1, except that the first nip pressure was 1.15 MPa and the thickness of the second adhesive layer 30 was 20 μm.
[0110] [Example 7] An optical member was produced in the same manner as in Example 1, except that the first adhesive layer 20 had a thickness of 10 μm and the second adhesive layer 30 had a thickness of 10 μm.
[0111] [Example 8] An optical member was produced in the same manner as in Example 1, except that the second nip pressure was 0.24 MPa, the first adhesive layer 20 had a thickness of 10 μm, and the second adhesive layer 30 had a thickness of 20 μm.
[0112] [Example 9] The optical component was produced in the same manner as in Example 1, except that the first adhesive layer 20 and the second adhesive layer 30 were each formed using adhesive B, and the first adhesive layer 20 had a thickness of 10 μm, and the second adhesive layer 30 had a thickness of 20 μm.
[0113] [Example 10] An optical member was produced in the same manner as in Example 9, except that the thickness of the second adhesive layer 30 was 10 μm.
[0114] [Example 11] An optical member was produced in the same manner as in Example 9, except that the second nip pressure was 0.61 MPa and the thickness of the first adhesive layer 20 was 20 μm.
[0115] [Example 12] An optical member was produced in the same manner as in Example 9, except that the second nip pressure was 0.24 MPa.
[0116] Table 1 shows the calculated values of the first deformation amount and the second deformation amount for Examples 1 to 8 in which adhesive A was used, and Table 2 shows the calculated values of the first deformation amount and the second deformation amount for Examples 9 to 12 in which adhesive B was used.
[0117] [Table 1]
[0118] [Table 2]
[0119] [Evaluation of cracks and bubbles] The incidence rates of cracks and bubbles were evaluated for Examples 1 to 12. Specifically, from a microscope image of an area including 165 through holes 14 (11 rows and 15 columns) as shown in Fig. 9, the through holes 14 with cracks occurring around them and the through holes 14 with bubbles remaining inside were confirmed, and the incidence rates of cracks and bubbles were calculated. The incidence rate of cracks is the percentage of the number of through holes 14 with cracks occurring around them to the total number of through holes 14 (165). The incidence rate of bubbles is the percentage of the number of through holes 14 with bubbles remaining inside to the total number of through holes 14 (165).
[0120] Table 3 shows the crack occurrence rate and the bubble occurrence rate for Examples 1 to 12. Table 3 also shows the percentage of the calculated value Da1 of the first deformation amount relative to the thickness of the porous layer and the percentage of the calculated value Da2 of the second deformation amount relative to the thickness of the porous layer for Examples 1 to 12. Table 3 also shows the evaluation results for the suppression of crack occurrence and the suppression of bubble occurrence for Examples 1 to 12. When the crack occurrence rate was 20% or less, it was evaluated that the crack occurrence was sufficiently suppressed (represented as "◯" in Table 3), and when the crack occurrence rate was more than 20%, it was evaluated that the crack occurrence was not sufficiently suppressed (represented as "△" in Table 3). When the bubble occurrence rate was 25% or less, it was evaluated that the remaining bubbles were sufficiently suppressed (represented as "◯" in Table 3), and when the bubble occurrence rate was more than 25%, it was evaluated that the remaining bubbles were not sufficiently suppressed (represented as "△" in Table 3). FIG. 10A shows a graph with the calculated value Da1 of the first deformation amount on the horizontal axis and the crack occurrence rate on the vertical axis, and FIG. 10B shows a graph with the calculated value Da2 of the second deformation amount on the horizontal axis and the bubble occurrence rate on the vertical axis.
[0121] [Table 3]
[0122] From Table 3 and Fig. 10A, it can be seen that the occurrence of cracks is sufficiently suppressed in Examples 1 to 4, 7 to 10, and 12 in which the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer (here, the calculated value Da1 of the first deformation amount is 2 μm or less), and from Table 3 and Fig. 10B, it can be seen that the occurrence of bubbles is sufficiently suppressed in Examples 1 to 6, 9, and 11 in which the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer (here, the calculated value Da2 of the second deformation amount is 7 μm or more). It can also be seen that both the occurrence of cracks and the remaining of bubbles are sufficiently suppressed in Examples 1 to 4 and 9 in which the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer and the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer.
[0123] In this way, it was confirmed that the occurrence of cracks around the through-holes 14 of the porous layer 10 was suppressed by performing the lamination of the first adhesive layer 20 under conditions where the calculated value Da1 of the first deformation amount was 250% or less of the thickness of the porous layer 10. It was also confirmed that the remaining of air bubbles inside the through-holes 14 of the porous layer 10 was suppressed by performing the lamination of the second adhesive layer 30 under conditions where the calculated value Da2 of the second deformation amount was 875% or more of the thickness of the porous layer 10.
[0124] From the viewpoint of suppressing the occurrence of cracks, it is more preferable that the first adhesive layer 20 is bonded under conditions in which the calculated value Da1 of the first deformation amount is 125% or less of the thickness of the porous layer 10. Even in the examples shown in Table 3, when the calculated value Da1 of the first deformation amount is 125% or less of the thickness of the porous layer 10, the occurrence rate of cracks tends to be further suppressed than when the calculated value Da1 of the first deformation amount is more than 125% and 250% or less of the thickness of the porous layer 10.
[0125] Moreover, from the viewpoint of suppressing residual air bubbles, it is more preferable that the bonding of the second adhesive layer 30 is performed under conditions in which the calculated value Da2 of the second deformation amount is 1000% or more of the thickness of the porous layer 10. Even in the examples shown in Table 3, when the calculated value Da2 of the second deformation amount is 1000% or more of the thickness of the porous layer 10, the rate of air bubble generation tends to be further suppressed compared to when the calculated value Da2 of the second deformation amount is 875% or more and less than 1000% of the thickness of the porous layer 10.
[0126] The thickness of the porous layer 10 is not limited to the exemplified thickness of 800 nm, and is, for example, 100 nm to 5000 nm.
[0127] Fig. 11A is a table showing the results of calculating the calculated first deformation amount Da1 when the thickness t1 of the first adhesive layer 20 is 10 μm to 35 μm and the first nip pressure is in the range of 0.1 MPa to 1.15 MPa when adhesive A is used as the material of the first adhesive layer 20. Fig. 11B is a table showing the results of calculating the calculated first deformation amount Da1 when the thickness t1 of the first adhesive layer 20 is 10 μm to 28 μm and the first nip pressure is in the range of 0.1 MPa to 1.15 MPa when adhesive B is used as the material of the first adhesive layer 20. In Figs. 11A and 11B, the region above the dotted ruled line is the region where the calculated first deformation amount Da1 is 2 μm or less, that is, the calculated first deformation amount Da1 is 250% or less of the thickness of the porous layer 10. In the region above the dashed ruled line, the calculated first deformation amount Da1 is 1 μm or less, that is, the calculated first deformation amount Da1 is 125% or less of the thickness of the porous layer 10.
[0128] 11A, in the case where the thickness of the porous layer 10 is 800 nm and the adhesive A is used, the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer 10 when the first nip pressure is 0.1 MPa or more and 0.74 MPa or less and the thickness t1 of the first adhesive layer 20 is 10 μm or more and 34 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the first nip pressure is 0.1 MPa or more and 0.74 MPa or less and the thickness t1 of the first adhesive layer 20 is 1.25 μm or more and 215 μm or less. In other words, it can be said that the suitable ranges of the first nip pressure and the thickness t1 of the first adhesive layer 20 for making the calculated value Da1 of the first deformation amount 250% or less of the thickness of the porous layer 10 are 0.1 MPa or more and 0.74 MPa or less and 1.25 μm or more and 215 μm or less, respectively.
[0129] Similarly, when the thickness of the porous layer 10 is 800 nm and the adhesive A is used, the calculated value Da1 of the first deformation amount is 125% or less of the thickness of the porous layer 10 when the first nip pressure is 0.1 MPa or more and 0.24 MPa or less and the thickness t1 of the first adhesive layer 20 is 10 μm or more and 17 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the first nip pressure is 0.1 MPa or more and 0.24 MPa or less and the thickness t1 of the first adhesive layer 20 is 1.25 μm or more and 107 μm or less. In other words, it can be said that the suitable ranges of the first nip pressure and the thickness t1 of the first adhesive layer 20 for making the calculated value Da1 of the first deformation amount 125% or less of the thickness of the porous layer 10 are 0.1 MPa or more and 0.24 MPa or less and 1.25 μm or more and 107 μm or less, respectively.
[0130] 11B, in the case where the thickness of the porous layer 10 is 800 nm and adhesive B is used, the calculated value Da1 of the first deformation amount is 250% or less of the thickness of the porous layer 10 when the first nip pressure is 0.1 MPa or more and 0.52 MPa or less and the thickness t1 of the first adhesive layer 20 is 10 μm or more and 27 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the first nip pressure is 0.1 MPa or more and 0.52 MPa or less and the thickness t1 of the first adhesive layer 20 is 1.25 μm or more and 173 μm or less. In other words, it can be said that the suitable ranges of the first nip pressure and the thickness t1 of the first adhesive layer 20 for making the calculated value Da1 of the first deformation amount 250% or less of the thickness of the porous layer 10 are 0.1 MPa or more and 0.52 MPa or less and 1.25 μm or more and 173 μm or less, respectively.
[0131] Similarly, in the case where the thickness of the porous layer 10 is 800 nm and adhesive B is used, the calculated value Da1 of the first deformation amount is 125% or less of the thickness of the porous layer 10 when the first nip pressure is 0.1 MPa or more and 0.17 MPa or less and the thickness t1 of the first adhesive layer 20 is 10 μm or more and 13 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the first nip pressure is 0.1 MPa or more and 0.17 MPa or less and the thickness t1 of the first adhesive layer 20 is 1.25 μm or more and 86 μm or less. In other words, it can be said that the suitable ranges of the first nip pressure and the thickness t1 of the first adhesive layer 20 for making the calculated value Da1 of the first deformation amount 125% or less of the thickness of the porous layer 10 are 0.1 MPa or more and 0.17 MPa or less and 1.25 μm or more and 86 μm or less, respectively.
[0132] Fig. 12A is a table showing the results of calculating the calculated value Da2 of the second deformation amount when the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 26 μm to 68 μm, the second nip pressure is in the range of 0.1 MPa to 1.15 MPa, and the adhesive A is used as the material for the first adhesive layer 20 and the second adhesive layer 30. Fig. 12B is a table showing the results of calculating the calculated value Da2 of the second deformation amount when the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 21 μm to 54 μm, the second nip pressure is in the range of 0.1 MPa to 1.15 MPa, and the adhesive B is used as the material for the first adhesive layer 20 and the second adhesive layer 30. 12A and 12B, the region below the dotted line is a region where the calculated value Da2 of the second deformation amount is 7 μm or more, that is, the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer 10. Moreover, the region below the chain line is a region where the calculated value Da2 of the second deformation amount is 8 μm or more, that is, the calculated value Da2 of the second deformation amount is 1000% or more of the thickness of the porous layer 10.
[0133] 12A, when the thickness of the porous layer 10 is 800 nm and adhesive A is used, the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer 10 when the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 27 μm or more and 68 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 3.34 μm or more and 417 μm or less. In other words, the preferred ranges of the second nip pressure and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 for making the calculated value Da2 of the second deformation amount 875% or more of the thickness of the porous layer 10 are 0.26 MPa or more and 1.15 MPa or less and 3.34 μm or more and 417 μm or less, respectively. In this case, since the preferred range of the thickness t1 of the first adhesive layer 20 is 1.25 μm or more and 215 μm or less, the preferred range of the thickness t2 of the second adhesive layer 30 is 2.09 μm or more and 202 μm or less.
[0134] Similarly, when the thickness of the porous layer 10 is 800 nm and adhesive A is used, the calculated value Da2 of the second deformation amount is 1000% or more of the thickness of the porous layer 10 when the second nip pressure is 0.32 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 31 μm or more and 68 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the second nip pressure is 0.32 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 3.82 μm or more and 421 μm or less. In other words, the preferred ranges for the second nip pressure to make the calculated value Da2 of the second deformation amount 1000% or more of the thickness of the porous layer 10 and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 are 0.32 MPa or more and 1.15 MPa or less and 3.82 μm or more and 421 μm or less, respectively.
[0135] 12B, when the thickness of the porous layer 10 is 800 nm and adhesive B is used, the calculated value Da2 of the second deformation amount is 875% or more of the thickness of the porous layer 10 when the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 22 μm or more and 54 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 2.68 μm or more and 337 μm or less. In other words, the preferred ranges for the second nip pressure to make the calculated value Da2 of the second deformation amount 875% or more of the thickness of the porous layer 10 and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 are 0.26 MPa or more and 1.15 MPa or less and 2.68 μm or more and 337 μm or less, respectively.
[0136] Similarly, when the thickness of the porous layer 10 is 800 nm and adhesive B is used, the calculated value Da2 of the second deformation amount is 1000% or more of the thickness of the porous layer 10 when the second nip pressure is 0.33 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 25 μm or more and 54 μm or less. When this range is converted to the case where the thickness of the porous layer 10 is 100 nm or more and 5000 nm or less, the second nip pressure is 0.33 MPa or more and 1.15 MPa or less, and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 is 3.06 μm or more and 332 μm or less. In other words, the preferred ranges for the second nip pressure to make the calculated value Da2 of the second deformation amount 1000% or more of the thickness of the porous layer 10 and the sum of the thickness t1 of the first adhesive layer 20 and the thickness t2 of the second adhesive layer 30 are 0.33 MPa or more and 1.15 MPa or less and 3.06 μm or more and 332 μm or less, respectively.
[0137] Next, examples of components that can be suitably used in the optical element according to the embodiment of the present invention will be described.
[0138] [Light guiding layer] A wide variety of known light guide layers (light guides) can be used for the light guide layer 50. The light guide layer 50 can be typically made of a film or plate-like material of resin (preferably transparent resin). The resin may be a thermoplastic resin or a photocurable resin. Examples of the thermoplastic resin include (meth)acrylic resins such as polymethylmethacrylate (PMMA) and polyacrylonitrile, polycarbonate (PC) resins, polyester resins such as PET, cellulose resins such as triacetyl cellulose (TAC), cyclic polyolefin resins, and polystyrene resins. Examples of the photocurable resin include photocurable resins such as epoxy acrylate resins and urethane acrylate resins. These resins may be used alone or in combination of two or more.
[0139] The thickness of the light guide layer 50 can be, for example, 100 μm or more and 100 mm or less. The thickness of the light guide layer 50 is preferably 50 mm or less, more preferably 30 mm or less, and further preferably 10 mm or less.
[0140] The refractive index n of the light guide layer 50 GP is, for example, a value in the range of −0.1 to +0.1 with respect to the refractive index n3 of the second layer 20, and the lower limit is preferably 1.43 or more, and more preferably 1.47 or more. On the other hand, the upper limit of the refractive index of the light guide layer 50 is 1.7.
[0141] Although a conventional light guide layer having an uneven surface can be used as the light guide layer 50, a light guide layer having a substantially flat surface, such as the light guide layer 50 shown in Fig. 1, can be preferably used. The optical member 1 functioning as the optical coupling layer can have a substantially flat main surface, and therefore can be easily laminated with the light guide layer 50 having a substantially flat surface, and can also be easily laminated with other optical elements having substantially flat surfaces. A substantially flat surface means that the uneven surface does not refract or diffusely reflect light.
[0142] [Porous layer] The porous layer 10 preferably includes silica particles, silica particles having micropores, approximately spherical particles such as hollow silica nanoparticles, fibrous particles such as cellulose nanofibers, alumina nanofibers, and silica nanofibers, and flat particles such as nanoclay composed of bentonite. In one embodiment, the porous layer 10 is a porous body formed by direct chemical bonding of particles (e.g., microporous particles). In addition, at least a part of the particles constituting the porous layer 10 may be bonded to each other via a small amount (e.g., equal to or less than the mass of the particles) of a binder component. The porosity and refractive index of the porous layer 10 can be adjusted by the particle size, particle size distribution, etc. of the particles constituting the porous layer 10.
[0143] Examples of methods for obtaining the porous layer 10 include the method for forming a low refractive index layer described in WO 2019 / 146628, as well as the methods described in JP 2010-189212 A, JP 2008-040171 A, JP 2006-011175 A, WO 2004 / 113966 A, JP 2017-054111 A, JP 2018-123233 A, and JP 2018-123299 A, and references thereto. The entire disclosures of these publications are incorporated herein by reference.
[0144] A porous silica body can be suitably used as the porous layer 10. The porous silica body can be produced, for example, by the following methods. Examples of the methods include a method of hydrolyzing and polycondensing at least one of silicon compounds, hydrolyzable silanes and / or silsesquioxane, and their partial hydrolyzates and dehydration condensates, a method of using porous particles and / or hollow fine particles, a method of producing an aerogel layer by utilizing the springback phenomenon, a method of using a crushed gel in which a gel-like silicon compound obtained by a sol-gel method is crushed and the resulting crushed body, that is, microporous particles, are chemically bonded to each other by a catalyst or the like. However, the porous layer 10 is not limited to a porous silica body, and the production method is not limited to the exemplified production method, and any production method may be used. The silsesquioxane is (RSiO 1.5 Silsesquioxane is a silicon compound whose basic structural unit is a silsesquioxane (R is a hydrocarbon group). Strictly speaking, it is different from silica whose basic structural unit is SiO2. However, it has something in common with silica in that it has a network structure cross-linked by siloxane bonds. Therefore, here, porous materials containing silsesquioxane as a basic structural unit are also referred to as porous silica materials or silica-based porous materials.
[0145] The silica porous body can be composed of microporous particles of gel-like silicon compound bonded together. The microporous particles of gel-like silicon compound include pulverized bodies of gel-like silicon compound. The silica porous body can be formed, for example, by applying a coating liquid containing pulverized bodies of gel-like silicon compound to a substrate. The pulverized bodies of gel-like silicon compound can be chemically bonded (for example, siloxane bonded) by, for example, the action of a catalyst, light irradiation, heating, etc.
[0146] The lower limit of the thickness of the porous layer 10 (first layer 10) may be, for example, greater than the wavelength of the light used. Specifically, the lower limit is, for example, 100 nm or more. There is no particular limitation on the upper limit of the thickness of the first layer 10, but it is, for example, 5000 nm or less, and more preferably 3000 nm or less. If the thickness of the first layer 10 is within the above range, the surface irregularities will not be so large as to affect lamination, making it easy to combine or laminate with other members.
[0147] The refractive index n1 of the first region 12 of the porous layer 10 is preferably 1.30 or less. Total internal reflection is likely to occur at the interface in contact with the first region 12, that is, the critical angle can be made small. The refractive index n1 of the first region 12 is more preferably 1.25 or less, further preferably 1.18 or less, and particularly preferably 1.15 or less. The lower limit of the refractive index n1 of the first region 12 is not particularly limited, but from the viewpoint of mechanical strength, it is preferably 1.05 or more.
[0148] The lower limit of the porosity of the first region 12 of the porous layer 10 is, for example, 40% or more, preferably 50% or more, more preferably 55% or more, and even more preferably 70% or more. The upper limit of the porosity of the first region 12 of the porous layer 10 is, for example, 90% or less, more preferably 85% or less. By having the porosity within the above range, the refractive index of the first region 12 can be set to an appropriate range. The porosity can be calculated, for example, from the value of the refractive index measured by an ellipsometer using the Lorentz-Lorenz's formula.
[0149] The film density of the first region 12 of the porous layer 10 is, for example, 1 g / cm 3 or more, preferably 10 g / cm 3 or more, more preferably 15 g / cm 3 or more. On the other hand, the film density is, for example, 50 g / cm 3 or less, preferably 40 g / cm 3 or less, more preferably 30 g / cm 3 or less, still more preferably 2.1 g / cm 3 or less. The range of the film density is, for example, 5 g / cm 3 or more and 50 g / cm 3 or less, preferably 10 g / cm 3 or more and 40 g / cm 3 or less, more preferably 15 g / cm 3 or more and 30 g / cm 3 or less. Alternatively, the range is, for example, 1 g / cm 3 or more and 2.1 g / cm 3 or less. The film density can be measured by a known method.
[0150] When the refractive index of the material constituting the matrix portion (the portion other than the voids) of the first region 12 of the porous layer 10 is n M , the refractive index n1 of the first region 12 of the porous layer 10 is determined by n M , the porosity, and the refractive index of air. For example, as described above, when a silica porous body is used as the porous layer 10, n M is, for example, 1.41 or more and 1.43 or less.
[0151] The refractive index n2 of the second region 14 of the porous layer 10 satisfies the relationship n1 < n2 and n1 < n3 with the refractive index n1 of the first region 12 and the refractive index n3 of the first adhesive layer (the second layer) 20. By the refractive index n2 of the second region 14 satisfying this relationship, light scattering due to reflection and refraction at the interface between the first region 12 and the second region 14 in the plane direction of the porous layer 10 can be suppressed. The lower limit value of the refractive index n2 of the second region 14 is, for example, more than 1.30, preferably 1.35 or more, and more preferably 1.40 or more.
[0152] Since the through-holes 14 of the porous layer 10 are filled with adhesive from both the second layer 20 and the third layer 30, the second region 14 has a structure in which a region made of adhesive from the second layer 20 and a region made of adhesive from the third layer 30 are laminated along the thickness direction. From the viewpoint of suppressing reflection, refraction, etc. at the interface between the former region and the latter region, it is preferable that the difference between the refractive index n3 of the second layer 20 and the refractive index n4 of the third layer 30 is small. Specifically, the difference between the refractive index n3 of the second layer 20 and the refractive index n4 of the third layer 30 is preferably 0.05 or less, more preferably 0.03 or less, and even more preferably 0.02 or less.
[0153] [Base material layer] The thickness of the base layer 40 is, for example, 1 μm to 1000 μm, preferably 10 μm to 100 μm, and more preferably 20 μm to 80 μm. The refractive index of the base layer 40 is preferably 1.40 to 1.70, and more preferably 1.43 to 1.65.
[0154] [Adhesive layer] The thicknesses of the first adhesive layer 20, the second adhesive layer 30, and the adhesive layer 76 are each independently, for example, 0.1 μm or more and 100 μm or less, preferably 0.3 μm or more and 100 μm or less, and more preferably 0.5 μm or more and 50 μm or less. The refractive indexes of the first adhesive layer 20, the second adhesive layer 30, and the adhesive layer 76 are each independently, preferably 1.42 or more and 1.60 or less, more preferably 1.47 or more and 1.58 or less. In addition, the refractive indexes of the first adhesive layer 20, the second adhesive layer 30, and the adhesive layer 76 are preferably close to the refractive index of the light guide layer 50, the base layer 40, or the shaping film 72 to which they are in contact, and the absolute value of the difference in refractive index is preferably 0.2 or less. [Industrial Applicability]
[0155] The optical member obtained by the manufacturing method according to the embodiment of the present invention is, for example, an optical element (light distribution element) together with a light guide layer or the like, and can be applied to public or general lighting such as frontlight, backlight, window / facade lighting, signage, signal lighting, window lighting, wall lighting, table lighting, solar applications, decorative illumination, light shield, light mask, roof lighting, etc. The optical member obtained by the manufacturing method according to the embodiment of the present invention is also suitably used as a component of the frontlight of a reflective display, which is an example of signage. By using the optical member obtained by the manufacturing method according to the embodiment of the present invention, it becomes possible to view images or graphics on a reflective display without optical defects such as visible blur caused by scattered or diffracted light. [Explanation of symbols]
[0156] 1 Optical components 2. Peel layer 10 Porous layer (first layer) 12 The First Area 14 Through hole (second region) 20 First adhesive layer (second layer) 30 Second adhesive layer (third layer) 40 Base material layer 40T Base Material 50 Light guiding layer 61, 62 Release sheet 70 Directional Change Layer 72 Forming film 74 Recess 76 Adhesive layer 100, 200 Optical elements IS interior space PF Porous Film Cr Crack Bu bubbles
Claims
1. A step A of preparing a porous film having a substrate and a porous layer provided on the substrate and having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; A step B of bonding a first adhesive layer to the side of the porous film opposite the substrate side at a first nip pressure; a step C of peeling the substrate from the porous layer after the step B, and then bonding a second adhesive layer to the porous layer on the side opposite to the first adhesive layer with a second nip pressure; Inclusive of When the strain calculated from the compressive stress-strain curve of the first adhesive layer and the first nip pressure is ε1 and the thickness of the first adhesive layer is t1, Da1 expressed as Da1=ε1×t1 is taken as a calculated value of a first deformation amount, which is the deformation amount of the first adhesive layer during bonding in step B. The method for producing an optical member, wherein the step B is performed under conditions in which the calculated value Da1 of the first deformation amount is 250% or less of a thickness of the porous layer.
2. When the strain obtained from the compressive stress-strain curve of the first adhesive layer and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer and the second nip pressure is ε2, and the thickness of the second adhesive layer is t2, Da2 expressed as Da2=ε1'×t1+ε2×t2 is taken as a calculated value of a second deformation amount which is the sum of the deformation amounts of the first adhesive layer and the second adhesive layer during lamination in step C, The method for producing an optical member according to claim 1 , wherein the step C is performed under conditions in which the calculated value Da2 of the second deformation amount is 875% or more of a thickness of the porous layer.
3. A step A of preparing a porous film having a substrate and a porous layer provided on the substrate and having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; A step B of bonding a first adhesive layer to the side of the porous film opposite the substrate side at a first nip pressure; a step C of peeling the substrate from the porous layer after the step B, and then bonding a second adhesive layer to the porous layer on the side opposite to the first adhesive layer with a second nip pressure; Inclusive of When the strain obtained from the compressive stress-strain curve of the first adhesive layer and the second nip pressure is ε1', the strain obtained from the compressive stress-strain curve of the second adhesive layer and the second nip pressure is ε2, the thickness of the first adhesive layer is t1, and the thickness of the second adhesive layer is t2, Da2 expressed as Da2=ε1'×t1+ε2×t2 is taken as a calculated value of a second deformation amount which is the sum of the deformation amounts of the first adhesive layer and the second adhesive layer during lamination in step C, The method for producing an optical member, wherein the step C is performed under conditions in which the calculated value Da2 of the second deformation amount is 875% or more of a thickness of the porous layer.
4. 4. The method for producing an optical member according to claim 1, wherein the first nip pressure is 0.1 MPa or more and 0.74 MPa or less, and the thickness t1 of the first adhesive layer is 1.25 μm or more and 215 μm or less.
5. 4. The method for producing an optical member according to claim 1, wherein the first nip pressure is 0.1 MPa or more and 0.24 MPa or less, and the thickness t1 of the first adhesive layer is 1.25 μm or more and 107 μm or less.
6. 4. The method for manufacturing an optical member according to claim 1, wherein the second nip pressure is 0.26 MPa or more and 1.15 MPa or less, and a sum of the thickness t1 of the first adhesive layer and the thickness t2 of the second adhesive layer is 3.34 μm or more and 417 μm or less.
7. 4. The method for manufacturing an optical member according to claim 1, wherein the second nip pressure is 0.32 MPa or more and 1.15 MPa or less, and a sum of the thickness t1 of the first adhesive layer and the thickness t2 of the second adhesive layer is 3.82 μm or more and 421 μm or less.
8. The step A comprises: a step a1 of preparing the porous layer supported on the substrate; a step a2 of forming the plurality of through holes in the porous layer by irradiating the porous layer with a laser beam; The method for producing the optical member according to claim 1 , comprising:
9. A porous layer having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; a first adhesive layer in contact with one of the two main surfaces of the porous layer; a second adhesive layer in contact with the other of the two main surfaces of the porous layer; having each of the plurality of through holes is filled with the first adhesive layer and the second adhesive layer; An optical member, wherein the rate of through holes having cracks around them is 20% or less among the plurality of through holes.
10. The optical member according to claim 9 , wherein the rate of through holes containing air bubbles among the plurality of through holes is 25% or less.
11. A porous layer having a porous structure, the porous layer having a plurality of through holes in addition to the voids of the porous structure; a first adhesive layer in contact with one of the two main surfaces of the porous layer; a second adhesive layer in contact with the other of the two main surfaces of the porous layer; having each of the plurality of through holes is filled with the first adhesive layer and the second adhesive layer; An optical member, wherein the rate of through holes containing air bubbles among the plurality of through holes is 25% or less.
12. The sum of the thickness of the first adhesive layer and the thickness of the second adhesive layer is 421 μm or less; 12. The optical member according to claim 9, wherein the first adhesive layer has a thickness of 215 μm or less.
13. 12. The optical member according to claim 9, wherein the second adhesive layer has a thickness of 2.09 μm or more and 202 μm or less.
14. The method for producing an optical member according to claim 9 , wherein the porous layer has a thickness of 100 nm or more and 5000 nm or less.
15. The method for producing an optical member according to claim 9 , wherein the equivalent diameter of an isocircumferential ellipse of each of the plurality of through holes is 50 μm or more and 150 μm or less.
Citation Information