Polyglycolic acid-containing resin composition and film containing the same

A polyglycolic acid resin composition with zinc-containing ionomer and ethylene-based terpolymer improves melt strength and processability, addressing PGA's processing challenges and enhancing biodegradability and gas barrier properties for eco-friendly films.

JP2024154373APending Publication Date: 2024-10-30SK INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024035256
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-03-07
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Polyglycolic acid (PGA) resin has high melting point and low melt strength, making film processing difficult due to ease of decomposition by heat and moisture, while maintaining biodegradability, gas barrier properties, and durability are essential.

Method used

A polyglycolic acid-containing resin composition comprising PGA, a zinc-containing ionomer, and an ethylene-based terpolymer, with specific weight ratios, to enhance molecular weight, impact resistance, and processability, thereby improving biodegradability and gas barrier properties.

Benefits of technology

The composition achieves improved melt strength, processability, and reduced gas permeability, allowing for the production of films with enhanced biodegradability and durability, suitable for eco-friendly applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154373000001_ABST
    Figure 2024154373000001_ABST
Patent Text Reader

Abstract

To provide a polyglycolic acid-containing resin composition which provides improved barrier characteristics, and a film containing the same.SOLUTION: A polyglycolic acid-containing resin composition according to an illustrative embodiment can contain a polyglycolic acid, a zinc-containing ionomer, and an ethylenic ternary copolymer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyglycolic acid-containing resin composition and a film containing the same. [Background technology]

[0002] Biodegradable resins are decomposed by other organic organisms such as bacteria and microorganisms, and as environmental regulations have been strengthened due to the worsening environmental pollution caused by conventional difficult-to-decompose polymers, demand for them as alternative materials to difficult-to-decompose resins is increasing. Recently, they have been used in a variety of fields, including the packaging materials industry, electronics industry, automobile industry, building materials industry, marine industry, stationery industry, and pulp and paper industry.

[0003] Examples of biodegradable resins include poly(glycolic acid) (PGA), poly(butylene succinate) (PBS), polyhydroxyalkanoate (PHA), polylactic acid (PLA), etc. Among them, PGA is a synthetic resin produced by polymerizing glycolic acid, and has excellent biodegradability and, as a resin with a linear structure, has excellent gas barrier properties.

[0004] In addition, PGA resin has ester bonds inside, high crystallinity, and excellent mechanical strength and brittleness. For this reason, there are attempts to develop barrier films using PGA resin that have high gas barrier properties, excellent biodegradability, and excellent durability.

[0005] However, PGA resin has a high melting point and low melt strength, and is easily decomposed by heat and moisture, making it difficult to process into a conventional film.

[0006] Therefore, it is necessary to develop a resin that is easy to process into a film while improving biodegradability, gas barrier properties, and durability by compounding or blending PGA resin with other polymers. Summary of the Invention [Problem to be solved by the invention]

[0007] One object of the present disclosure is to provide a polyglycolic acid-containing resin composition that provides improved barrier properties.

[0008] One object of the present disclosure is to provide a film formed from the resin composition and having improved barrier properties. [Means for solving the problem]

[0009] A polyglycolic acid-containing resin composition according to an exemplary embodiment may include poly(glycolic acid), a zinc-containing ionomer, and an ethylene-based terpolymer.

[0010] In some embodiments, the zinc-containing ionomer can include a terpolymer of ethylene, zinc (meth)acrylate, and (meth)acrylic acid.

[0011] In some embodiments, the ethylene-based terpolymer may include a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate.

[0012] In some embodiments, the content of the polyglycolic acid may be 60% by weight to 98% by weight based on the total weight of the polyglycolic acid-containing resin composition.

[0013] In some embodiments, the content of the zinc-containing ionomer may be 1 wt % to 39 wt % based on the total weight of the polyglycolic acid-containing resin composition.

[0014] In some embodiments, the content of the ethylene-based terpolymer may be 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.

[0015] In some embodiments, the sum of the content of the zinc-containing ionomer and the content of the ethylene-based terpolymer may be 2% by weight to 40% by weight based on the total weight of the polyglycolic acid-containing resin composition.

[0016] In some embodiments, the polyglycolic acid content may be greater than the sum of the zinc-containing ionomer content and the ethylene-based terpolymer content.

[0017] In some embodiments, the sum of the content of the polyglycolic acid, the content of the zinc-containing ionomer, and the content of the ethylene-based terpolymer may be 95% by weight or more based on the total weight of the polyglycolic acid-containing resin composition.

[0018] In some embodiments, the polyglycolic acid-containing resin composition may have a melt viscosity of 200 Pa·s to 10,000 Pa·s, measured under conditions of 230° C., 5% strain, and a vibration frequency of 0.1 Hz.

[0019] In some embodiments, the polyglycolic acid-containing resin composition may have a melt flow index of 1 g / 10 min to 200 g / 10 min measured at 230° C. under a load of 2.16 kg.

[0020] A film according to an exemplary embodiment can be formed from the polyglycolic acid-containing resin composition.

[0021] In some embodiments, the film may have a thickness of from 50 μm to 250 μm.

[0022] In some embodiments, the film has an oxygen transmission rate of 200 g / m2 or less, measured at 50% relative humidity and 25° C. 2 ·days or less is acceptable.

[0023] In some embodiments, the oxygen permeability of the film can satisfy Equation 1:

[0024] [Formula 1] OTR(PGA-Poly)<0.1(x OTR(PGA)+(1-x) OTR(Poly))

[0025] In the above formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only a zinc-containing ionomer or an ethylene-based terpolymer, and x is 0.6≦x<1. Effect of the Invention

[0026] The polyglycolic acid-containing resin composition according to the exemplary embodiment may include poly(glycolic acid, PGA), a zinc-containing ionomer (ZnIO), and an ethylene-based terpolymer, which may increase the molecular weight of the polyglycolic acid-containing resin composition to improve impact resistance and decrease the melt flow index to improve processability.

[0027] The polyglycolic acid-containing resin composition can contain PGA in a predetermined content, which can improve the biodegradability and gas barrier properties of a film containing the polyglycolic acid-containing resin composition while improving the processability.

[0028] The film according to the exemplary embodiment may include the polyglycolic acid-containing resin composition, which may complicate the gas permeation path inside the film and reduce the gas permeability.

[0029] The polyglycolic acid-containing resin composition and film of the present disclosure can be widely applied in the field of green technology such as biodegradable resins, biodegradable food packaging films, biodegradable sanitary products, and other biodegradable plastics in which the biodegradable composition is used. The polyglycolic acid-containing resin composition and film of the present disclosure can suppress land pollution, water pollution, air pollution, etc., and can be used as a material for disposable items that are eco-friendly. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a graph showing measured and estimated oxygen permeability of films according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] According to an exemplary embodiment, there is provided a polyglycolic acid-containing resin composition including poly(glycolic acid) (PGA), a zinc-containing ionomer (ZnIO) and an ethylene-based terpolymer, and a film including the polyglycolic acid-containing resin composition.

[0032] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. However, these embodiments are merely illustrative of the present disclosure and are not intended to limit the present disclosure.

[0033] According to an exemplary embodiment, the polyglycolic acid-containing resin composition can include PGA, ZnIO, and an ethylene-based terpolymer.

[0034] The PGA is a biodegradable polymer having a linear structure with ester bonds, and can have high biodegradability. In addition, due to hydrogen bonds between PGA polymers, it can have high crystallinity. This can improve the gas barrier properties of the polyglycolic acid-containing resin composition.

[0035] The ZnIO is a type of polymer containing zinc, a transition metal, and has low hygroscopicity and water content. In addition, the ZnIO can improve the structural stability of the polyglycolic acid-containing resin composition by forming a coordinate bond with the ester group of the PGA.

[0036] The ethylene-based terpolymer is a polymer obtained by copolymerizing three basic monomers including a monomer derived from ethylene, and the ethylene-based terpolymer can improve structural stability by cross-linking with the PGA and the ZnIO.

[0037] In some embodiments, the ZnIO can include an ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer.

[0038] The ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer contains zinc ions (Zn 2+ ) and carboxylate anion (-COO - ) is an ionic bonded polymer. The zinc ion of the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer is a transition metal ion, and can form a coordinate bond with the ester group of the PGA. By including the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer in the polyglycolic acid-containing resin composition, durability and melt strength can be improved.

[0039] In one embodiment, the content of the ethylene monomer in the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer is not limited, and may be, for example, 70% by weight to 98% by weight, 73% by weight to 95% by weight, or 76% by weight to 92% by weight, based on the total weight of the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer.

[0040] In one embodiment, the content of the zinc (meth)acrylate monomer in the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer is not limited, and may be, for example, 1 wt % to 20 wt %, 1 wt % to 17 wt %, or 1 wt % to 14 wt % based on the total weight of the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer.

[0041] In one embodiment, the content of the (meth)acrylic acid monomer in the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer is not limited, and may be, for example, 1 wt % to 29 wt %, 4 wt % to 26 wt %, or 7 wt % to 23 wt % based on the total weight of the ethylene-zinc (meth)acrylate-(meth)acrylic acid terpolymer.

[0042] In some embodiments, the ethylene-based terpolymer can include a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate (EAG).

[0043] The EAG is an ethylene-based polymer containing a glycidyl group, and the glycidyl group of the EAG is contained in the polyglycolic acid-containing resin composition and can bond to at least one carboxyl group of the PGA and ZnIO.

[0044] This allows the polyglycolic acid-containing resin composition to be elongated and the polymer structure to be made complex, thereby improving the melt strength and durability of the polyglycolic acid-containing resin composition and improving the processability.

[0045] In one embodiment, the ethylene monomer content of the EAG is not limited, but may be, for example, 50% by weight to 88% by weight, 55% by weight to 82% by weight, or 57% by weight to 78% by weight, based on the total weight of the EAG.

[0046] In one embodiment, the content of the glycidyl methacrylate monomer in the EAG is not limited, but may be, for example, 1 wt % to 30 wt %, 3 wt % to 25 wt %, or 5 wt % to 20 wt % relative to the total weight of the EAG.

[0047] In one embodiment, the content of the alkyl acrylate monomer in the EAG is not limited, but may be, for example, 10% by weight to 48% by weight, 15% by weight to 42% by weight, or 17% by weight to 38% by weight relative to the total weight of the EAG.

[0048] In some embodiments, the content of the PGA may be 60% by weight to 98% by weight, 60% by weight to 93% by weight, 60% by weight to 88% by weight, or 65% by weight to 85% by weight, based on the total weight of the polyglycolic acid-containing resin composition.

[0049] In the above content range, PGA can be distributed throughout the entire region of the polyglycolic acid-containing resin composition. This allows the polyglycolic acid-containing resin composition to maintain low gas permeability while improving the melt strength, durability, and processability of the polyglycolic acid-containing resin composition. In addition, PGA can improve the biodegradability of the polyglycolic acid-containing resin composition.

[0050] In some embodiments, the content of the ZnIO may be 1 wt % to 39 wt %, 5 wt % to 38 wt %, 7 wt % to 30 wt %, or 8 wt % to 20 wt %, based on the total weight of the polyglycolic acid-containing resin composition.

[0051] Within the above content range, the increase in the gas permeability of the polyglycolic acid-containing resin composition due to the increase in the ZnIO and the decrease in the PGA can be prevented. In addition, the zinc ions of the ZnIO coordinate with the ester groups of the PGA to improve the durability of the polyglycolic acid-containing resin composition. In addition, the hygroscopicity of the polyglycolic acid-containing resin composition is reduced, and the polymer structure is prevented from collapsing due to the high biodegradability of the polyglycolic acid-containing resin composition. This improves the structural stability of the polyglycolic acid-containing resin composition.

[0052] In some embodiments, the content of the ethylene-based terpolymer (e.g., EAG) may be 1 wt % to 39 wt %, 2 wt % to 35 wt %, 5 wt % to 33 wt %, or 7 wt % to 27 wt %, based on the total weight of the polyglycolic acid-containing resin composition.

[0053] Within the above content range, the ethylene-based terpolymer (e.g., EAG) can be stably cross-linked with the carboxyl groups of the PGA and the ZnIO, which can further improve the melt strength and processability of the polyglycolic acid-containing resin composition.

[0054] In one embodiment, the sum of the content of the ZnIO and the content of the ethylene-based terpolymer may be 2 wt % to 40 wt %, 5 wt % to 40 wt %, 10 wt % to 35 wt %, or 10 wt % to 30 wt % based on the total weight of the polyglycolic acid-containing resin composition.

[0055] Within the above content range, the content of PGA in the polyglycolic acid-containing resin composition may be 60% by weight or more, 65% by weight or more, or 70% by weight or more, which can reduce gas permeability and improve processability without reducing the biodegradability of the polyglycolic acid-containing resin composition.

[0056] In some embodiments, the content of the PGA may be greater than the sum of the content of the ZnIO and the content of the ethylene-based terpolymer, thereby improving the biodegradability, gas barrier property, and durability of the polyglycolic acid-containing resin composition.

[0057] As described above, the melt viscosity and melt flow index can be adjusted by adjusting the contents of PGA, ZnIO, and the ethylene-based terpolymer contained in the polyglycolic acid-containing resin composition.

[0058] In some embodiments, the sum of the polyglycolic acid content, the zinc-containing ionomer content, and the ethylene-based terpolymer content may be 95 wt % or more, 98 wt % or more, or 99 wt % or more, based on the total weight of the polyglycolic acid-containing resin composition. In one embodiment, the polyglycolic acid-containing resin composition can be composed of the polyglycolic acid, the zinc-containing ionomer, and the ethylene-based terpolymer. For example, the total content of the polyglycolic acid, the zinc-containing ionomer, and the ethylene-based terpolymer may be 100% by weight based on the total weight of the polyglycolic acid-containing resin composition.

[0059] In some embodiments, the melt viscosity of the polyglycolic acid-containing resin composition may be 50 Pa·s to 10,000 Pa·s, 100 Pa·s to 8,000 Pa·s, or 200 Pa·s to 6,000 Pa·s.

[0060] The melt viscosity was measured by pressing the polyglycolic acid-containing resin composition at 230° C. to a thickness of 2 mm into a test piece, and measuring the melt viscosity at a strain of 5% and a frequency of 0.1 Hz.

[0061] In one embodiment, the melt flow index of the polyglycolic acid-containing resin composition may be 1 g / 10 min to 200 g / 10 min, 1 g / 10 min to 100 g / 10 min, or 2 g / 10 min to 50 g / 10 min.

[0062] The melt flow index was calculated according to ASTM D1238, measured at a temperature of 230° C. under a load of 2.16 kg.

[0063] By maintaining the melt viscosity and melt flow index within the above ranges, the flexibility of the polyglycolic acid-containing resin composition can be improved compared to that of PGA. This can improve the processability in processes such as foaming-expansion molding, injection molding, compression molding, casting filming process, and inflation film process. This can improve the processability of the polyglycolic acid-containing resin composition into a film.

[0064] The polyglycolic acid-containing resin composition described above can be formed by drying and kneading a mixture of PGA, ZnIO, and an ethylene-based terpolymer.

[0065] In an exemplary embodiment, PGA, ZnIO and an ethylene-based terpolymer can be charged to a Hopper Dryer.

[0066] PGA can be dried, for example, by being placed in a hopper dryer maintained at a temperature of 60°C to 100°C, 70°C to 90°C, or 75°C to 85°C. ZnIO can be dried, for example, by being placed in a hopper dryer maintained at a temperature of 30°C to 70°C, 40°C to 60°C, or 45°C to 55°C. Ethylene-based terpolymers (e.g., EAG) can be dried, for example, by being placed in a hopper dryer maintained at a temperature of 20°C to 60°C, 30°C to 50°C, or 35°C to 45°C.

[0067] The PGA, ZnIO, and ethylene-based terpolymer can be dried for, for example, 10 hours to 14 hours, 11 hours to 13 hours, or 11 hours 30 minutes to 12 hours 30 minutes. By drying the PGA, ZnIO, and ethylene-based terpolymer sufficiently within the above range, side reactions in the kneading process of the PGA, ZnIO, and ethylene-based terpolymer can be suppressed.

[0068] The dried PGA, ZnIO, and ethylene-based terpolymer can be introduced into the chamber of an internal mixer, which can be maintained at, for example, 220°C to 260°C, 225°C to 250°C, or 230°C to 240°C.

[0069] When the dried PGA, ZnIO, and ethylene-based terpolymer are charged into an internal mixer, the rotor in the internal mixer can rotate at, for example, 10 rpm to 70 rpm, 20 rpm to 60 rpm, or 30 rpm to 50 rpm.

[0070] Within the above range, kneading can be started without the PGA, ZnIO, and ethylene-based terpolymer agglomerating with each other.

[0071] After the addition of the dried PGA, ZnIO, and ethylene-based terpolymer is completed, the rotor speed can be maintained at, for example, 60 rpm to 100 rpm, 70 rpm to 90 rpm, or 75 rpm to 85 rpm while kneading. The kneading can be performed for, for example, 1 minute to 5 minutes, 2 minutes to 4 minutes, or 2 minutes 30 seconds to 3 minutes 30 seconds.

[0072] Within this range, the PGA, ZnIO and ethylene-based terpolymer can be uniformly distributed and kneading can be completed.

[0073] The kneaded product obtained as described above can be recovered to obtain a polyglycolic acid-containing resin composition.

[0074] Although the above-mentioned kneading step is described as being performed by an internal mixer, the means for the kneading step is not limited to an internal mixer. For example, the dried PGA, ZnIO and ethylene-based terpolymer may be put into a single-screw extruder or a twin-screw extruder, melted and kneaded to complete the kneading. The kneaded resin composition discharged from the outlet of the single-screw extruder or the twin-screw extruder can be cut by a pelletizer to obtain a polyglycolic acid-containing resin composition in the form of pellets.

[0075] According to an exemplary embodiment, a film can be formed from the polyglycolic acid-containing resin composition described above, which can reduce the gas permeability of the film and improve its biodegradability and durability.

[0076] In some embodiments, the thickness of the film may be 50 μm to 250 μm, 100 μm to 200 μm, or 120 μm to 180 μm, which is sufficient to reduce the gas permeability of the film.

[0077] In one embodiment, the oxygen permeability of the film is 200 g / m 2 ·day or less, 100g / m2 day or less, or 30g / m 2 The lower limit of the oxygen permeability of the film is not limited, but for example, the oxygen permeability of the film may be 1 g / m 2 ·day or more, 2g / m 2 ·day or more, 5g / m 2 day or more, or 10g / m 2 · days or more is acceptable.

[0078] The oxygen permeability may be measured under conditions of 50% relative humidity and 25°C temperature.

[0079] Within this range, when the film is used as a barrier film, the barrier properties against gases (for example, oxygen) are improved, and products within the barrier film can be sufficiently protected.

[0080] When the polyglycolic acid-containing resin composition contains 60% by weight or more of PGA, the PGA can be uniformly distributed throughout the entire region of the polyglycolic acid-containing resin composition, and the high gas barrier properties of the PGA can thereby be maintained at a high level for the film containing the polyglycolic acid-containing resin composition.

[0081] Therefore, by including 60% by weight or more of PGA in the polyglycolic acid-containing resin composition, the oxygen permeability of the polyglycolic acid-containing resin composition can be kept low. For example, the oxygen permeability of the polyglycolic acid-containing resin composition can be measured to be lower than the arithmetic average value of the oxygen permeability of each of the polymer components contained in the polyglycolic acid-containing resin composition.

[0082] In some embodiments, the oxygen permeability of the film can satisfy Equation 1:

[0083] [Formula 1] OTR(PGA-Poly)<0.1(x OTR(PGA)+(1-x) OTR(Poly))

[0084] In the above formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only a zinc-containing ionomer or an ethylene-based terpolymer, and x is 0.6≦x<1.

[0085] The film can be used as a barrier film for packaging materials for various products, such as food packaging materials and battery packaging materials.

[0086] The aforementioned films can be produced from polyglycolic acid-containing resin compositions.

[0087] According to an exemplary embodiment, the polyglycolic acid-containing resin composition can be compressed by a press to produce a film.

[0088] In some embodiments, the press can be maintained at 200° C. to 260° C., 210° C. to 250° C., 220° C. to 240° C., or 225° C. to 235° C. The above ranges allow for forming and deforming a film comprising the polyglycolic acid-containing resin composition.

[0089] In some embodiments, the polyglycolic acid-containing resin composition can be compressed to a pressure of 10 MPa to 30 MPa, 15 MPa to 25 MPa, or 18 MPa to 22 MPa for 1 minute to 3 minutes, or 1 minute 30 seconds to 2 minutes 30 seconds.

[0090] In the above range, the film can be manufactured to the above thickness, which reduces the oxygen permeability of the film and allows the film to be manufactured to a small thickness.

[0091] Although the above-mentioned film production is performed by applying pressure by a press, the film production method is not limited thereto. For example, the polyglycolic acid-containing resin composition melted in an extruder can be extruded through a chill roll in a t-die and cooled to produce a film (for example, a cast film production method). For example, the polyglycolic acid-containing resin composition can be cooled by contacting air with an air ring in a ring-shaped die (for example, a spiral die) to produce a film (for example, a blown film production method).

[0092] Below, preferred examples are presented to aid in understanding the present invention. However, these examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope of the scope and technical spirit of the present invention, and it is natural that such changes and modifications also fall within the scope of the appended claims.

[0093] Examples and Comparative Examples Example 1 (1) Preparation of raw materials for polyglycolic acid-containing resin composition Poly(glycolic acid, PGA) was dried in a hopper dryer set at 80° C. for 12 hours to prepare dried PGA.

[0094] The ethylene-zinc acrylate-acrylic acid terpolymer was dried for 12 hours in a hopper dryer set at 50° C. to prepare a dried ethylene-zinc acrylate-acrylic acid terpolymer. The contents of ethylene monomer, zinc acrylate monomer and acrylic acid monomer in the ethylene-zinc acrylate-acrylic acid terpolymer were about 86.5 wt%, 6.75 wt% and 6.75 wt%, respectively.

[0095] An ethylene-glycidyl methacrylate-methyl acrylate terpolymer (EAG) was dried for 12 hours in a hopper dryer set at 40° C. to prepare a dried EAG. The contents of ethylene monomer, glycidyl methacrylate monomer, and methyl acrylate monomer in the EAG were 68 wt %, 8 wt %, and 24 wt %, respectively.

[0096] As the hopper dryer, a Mitsui hot air dryer was used.

[0097] (2) Production of polyglycolic acid-containing resin composition The dried PGA, dried ethylene-zinc acrylate-acrylic acid terpolymer, and dried EAG were placed in the chamber of an internal mixer at 80 wt%, 10 wt%, and 10 wt%, respectively, and the temperature in the chamber of the internal mixer was maintained at 230° C., and the rotor of the internal mixer rotated at a speed of 40 rpm.

[0098] Thereafter, the rotor speed was increased to 80 rpm and kneading was continued for 3 minutes, after which a kneaded product, a polyglycolic acid-containing resin composition, was produced and collected.

[0099] As the internal mixer, a Brabender Measuring Mixer W50 was used.

[0100] (3) Film manufacturing The polyglycolic acid-containing resin composition was pressed at a pressure of 20 MPa for 2 minutes using a press set at 230° C. to produce a film.

[0101] Examples 2 to 7 and Comparative Examples 1 to 6 The polyglycolic acid-containing resin compositions and films of Examples 2 to 7 and Comparative Examples 1 to 6 were produced in the same manner as in Example 1, except that the type of PGA used and the weight ratios of the dried PGA, dried ethylene-zinc acrylate-acrylic acid terpolymer, and dried EAG charged into the chamber of the internal mixer were adjusted as shown in Table 1 below.

[0102] [Table 1]

[0103] The types of PGAs shown in Table 1 are as follows: Types of PGA A: Polyglycolic acid having a number average molecular weight (Mn) of 35,000 to 45,000 and a weight average molecular weight (Mw) of 80,000 to 95,000 as measured by gel permeation chromatography (GPC). B: Polyglycolic acid having a number average molecular weight (Mn) of 70,000 to 80,000 and a weight average molecular weight (Mw) of 160,000 to 180,000 as measured by gel permeation chromatography (GPC).

[0104] The gel permeation chromatography was carried out by dissolving polyglycolic acid in hexafluoroisopropyl alcohol (HFIP), filtering the solution through a polytetrafluoroethylene (PTFE) filter, and injecting the solution into EcoSEC HLC-8320 GPC manufactured by Tosoh Corporation for measurement. Poly(methyl methacrylate, PMMA) was used as a standard substance.

[0105] Experimental Example 1 FIG. 1 is a graph showing the measured and estimated oxygen permeabilities of films depending on the total content of ethylene-zinc acrylate-acrylic acid terpolymer and EAG contained in a polyglycolic acid-containing resin composition.

[0106] The estimated oxygen permeability is the arithmetic average of the oxygen permeability of the PGA, the oxygen permeability of the ethylene-zinc acrylate-acrylic acid terpolymer, and the oxygen permeability of the EAG contained in the polyglycolic acid-containing resin composition, based on their weight ratios.

[0107] The measured oxygen permeability indicates a value obtained by measuring the oxygen permeability of a film containing the polyglycolic acid-containing resin composition. The measured values ​​of the oxygen permeability of the film were those of Example 1, Example 2, Example 5, and Example 6.

[0108] Referring to FIG. 1, the estimated oxygen permeability of the films was calculated to increase linearly with the sum of the ethylene-zinc acrylate-acrylic acid terpolymer content and the EAG content.

[0109] However, the measured oxygen permeability of the film remained low when the total content of the ethylene-zinc acrylate-acrylic acid terpolymer and the EAG content was 40% by weight or less (PGA was more than 60% by weight), and it was measured that the oxygen permeability increased in proportion to the content when the total content of the ethylene-zinc acrylate-acrylic acid terpolymer and the EAG content exceeded 40% by weight.

[0110] Experimental Example 2 (1) Measurement of melt viscosity The polyglycolic acid-containing resin compositions prepared in the above examples and comparative examples were pressed to a thickness of 2 mm at a temperature of 230° C., and then the melt viscosity was measured using a viscometer (TA ARES).

[0111] The viscosity meter was set under the conditions of 230° C., 5% strain, and a frequency of 0.1 Hz to 400 Hz, and the viscosity value measured at a frequency of 0.1 Hz was taken as the melt viscosity.

[0112] The evaluation results are shown in Table 2 below.

[0113] (2) Measurement of Melt Flow Index The melt flow index of each of the polyglycolic acid-containing resin compositions produced in the above-mentioned Examples and Comparative Examples was measured at a temperature of 230° C. under a load of 2.16 kg in accordance with ASTM D1238.

[0114] The evaluation results are shown in Table 2 below.

[0115] (3) Measurement of oxygen permeability The films prepared in the above examples and comparative examples were attached to an oxygen permeability meter (MOCON OX TRANS model 2 / 61) to measure the oxygen permeability.

[0116] The oxygen permeability was measured at a relative humidity of 50% and a temperature of 25° C. for 12 hours, and then the value at which the permeability stabilized was measured.

[0117] The upper limit of the oxygen permeability measurement is 1,200 g / m 2 The oxygen permeability of the film which could not be measured exceeding the upper limit was expressed as "Ultra".

[0118] The evaluation results are shown in Table 2 below.

[0119] [Table 2]

[0120] Referring to Table 2, the film according to the embodiment has a thickness of 200 g / m 2 The oxygen permeability was less than 100%.

[0121] In Examples 4 and 5, in which the PGA content was reduced to 60 wt%, the oxygen permeability increased.

[0122] In Example 6, where the PGA content was reduced to less than 60 wt%, the oxygen permeability increased.

[0123] In Example 7, where the molecular weight of the PGA was increased, the melt viscosity increased and the melt flow index decreased.

[0124] In Comparative Example 1, in which only PGA was used, the melt viscosity of the polyglycolic acid-containing resin composition decreased and the melt flow index increased.

[0125] In Comparative Example 2, which used only a terpolymer of ethylene-zinc acrylate-acrylic acid, the oxygen permeability was 1,200 g / m 2 ·day has passed.

[0126] In Comparative Example 3, in which only EAG was used, the oxygen permeability was 1,200 g / m 2 ·day has passed.

[0127] In Comparative Example 4, which did not contain PGA and used a resin composition containing an ethylene-zinc acrylate-acrylic acid terpolymer and EAG, the oxygen permeability was 1,200 g / m 2 ·day has passed.

Claims

1. Poly(glycolic acid) A zinc-containing ionomer (Zn ionomer); and an ethylene-based terpolymer.

2. 2. The polyglycolic acid-containing resin composition of claim 1, wherein the zinc-containing ionomer comprises a terpolymer of ethylene, zinc (meth)acrylate, and (meth)acrylic acid.

3. 2. The polyglycolic acid-containing resin composition of claim 1, wherein the ethylene-based terpolymer comprises a copolymer of ethylene, glycidyl methacrylate, and an alkyl acrylate.

4. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the polyglycolic acid is 60% by weight to 98% by weight based on the total weight of the polyglycolic acid-containing resin composition.

5. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the zinc-containing ionomer is 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.

6. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the ethylene-based terpolymer is 1% by weight to 39% by weight based on the total weight of the polyglycolic acid-containing resin composition.

7. The polyglycolic acid-containing resin composition according to claim 1, wherein the sum of the content of the zinc-containing ionomer and the content of the ethylene-based terpolymer is 2% by weight to 40% by weight based on the total weight of the polyglycolic acid-containing resin composition.

8. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the content of the polyglycolic acid is greater than the sum of the content of the zinc-containing ionomer and the content of the ethylene-based terpolymer.

9. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the total content of the polyglycolic acid, the zinc-containing ionomer, and the ethylene-based terpolymer is 95% by weight or more based on the total weight of the polyglycolic acid-containing resin composition.

10. 2. The polyglycolic acid-containing resin composition according to claim 1, wherein the melt viscosity of the polyglycolic acid-containing resin composition measured under conditions of 230° C., 5% strain and 0.1 Hz is 200 Pa·s to 10,000 Pa·s.

11. The polyglycolic acid-containing resin composition according to claim 1, wherein the polyglycolic acid-containing resin composition has a melt flow index of 1 g / 10 min to 200 g / 10 min measured at 230° C. under a load of 2.16 kg.

12. A film formed from the polyglycolic acid-containing resin composition according to claim 1.

13. The film of claim 12, wherein the thickness of the film is from 50 μm to 250 μm.

14. The oxygen permeability of the film measured at 50% relative humidity and 25° C. is 200 g / m 2 14. The film of claim 13, wherein the film has a viscosity of 0.05 to 1.0 s.

15. The film according to claim 12, wherein the oxygen permeability of the film satisfies the following formula 1: [Formula 1] OTR(PGA-Poly)<0.1(x・OTR(PGA)+(1-x)・OTR(Poly)) (In formula 1, OTR(PGA-Poly) is the oxygen permeability of a film formed from the polyglycolic acid-containing resin composition, OTR(PGA) is the oxygen permeability of a film containing only polyglycolic acid, OTR(Poly) is the oxygen permeability of a film containing a resin containing only a zinc-containing ionomer or an ethylene-based terpolymer, and x is 0.6≦x<1.)