Electrode, power storage device, and manufacturing method for the electrode
By optimizing the arrangement and distribution of conductive materials and pores in electrodes with cubic lithium composite oxides, the energy density per electrode volume is enhanced, addressing the conductivity and density challenges of existing cubic lithium composite oxide electrodes.
Patent Information
- Application Number
- JP2023068367
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing electrodes using cubic lithium composite oxides with layered rock salt structures have lower energy density per electrode volume due to lower conductivity, despite having higher capacity per mass, necessitating the use of large amounts of conductive materials which reduce density.
The electrode design incorporates a lithium composite oxide with a cubic crystal structure, controlled arrangement of conductive materials, and optimized manufacturing processes to ensure high contact between the active material and conductive materials, maintaining low conductive material content while enhancing electrode density and conductivity.
This approach significantly increases the energy density per electrode volume, achieving values over 700 Wh/L, while maintaining high discharge capacity per mass, by optimizing the distribution of conductive materials and pores around the active material.
Smart Images

Figure 2024154527000001_ABST
Abstract
Description
[Technical field]
[0001] This specification discloses an electrode, an electricity storage device, and a method for manufacturing the electrode. [Background technology]
[0002] Conventionally, LiMO2 (where M=Co, Ni, Mn) having a layered rock salt structure has been known as a positive electrode active material for lithium secondary batteries. The theoretical maximum discharge capacity with this composition is about 280 mAh / g, but the capacity that can be extracted from the viewpoint of potential and structural stability is about 70% of that. Therefore, a proposal has been made to increase the available discharge capacity by making the Li in the composition excessive. In particular, it is known that by making the active material into an irregular rock salt structure, Li can be charged and discharged three-dimensionally, and a high discharge capacity is exhibited (see, for example, Patent Documents 1 to 4, etc.). This is because the amorphous structure allows Li to move three-dimensionally, and Li can be reversibly inserted and removed even in a Li-excess composition. In addition, positive electrodes having a spinel structure and a layered rock salt structure have also been proposed (see, for example, Patent Document 5, etc.). In addition, a lithium composite oxide with the composition (1-α)LiMnO2·αLi3PO4 (α is 0.1, 0.2, or 0.3) has been proposed, in which layered LiMnO2 and Li3PO4 are mixed by mechanical milling (see Non-Patent Document 1). This lithium composite oxide has a disordered rock salt structure, and Mn 3+ / Mn 4+ It is said that this electrode exhibits a high capacity exceeding the theoretical capacity based on the oxidation-reduction of the lithium ion battery. In addition, the inventors of the present application have proposed a high-capacity positive electrode having a random rock salt structure, for example, with a discharge capacity exceeding 300 mAh / g (see, for example, Patent Document 6). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2018-92958 [Patent Document 2] Patent Publication No. 2017-202954 [Patent Document 3] Special table 2019-523532 [Patent Document 4] Patent Publication 2015-166291 [Patent Document 5] Patent Publication 2016-25009 [Patent Document 6] Patent Publication No. 2021-128880 [Non-patent literature]
[0004] [Non-Patent Document 1] M. Sawamura, et al., ACS Cent. Sci. 2020, 6, 2326-2338 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in electrodes using cubic active materials as in Patent Documents 1 to 6 and Non-Patent Document 1, the discharge capacity per active material mass is higher than that of electrodes using LiMO2 having a layered rock salt structure, but the energy density per electrode volume is sometimes lower. For this reason, it has been desired to further increase the energy density per electrode volume.
[0006] The present disclosure has been made to solve such problems, and has as its main object to provide an electrode, an electricity storage device, and a method for manufacturing an electrode that can further increase the energy density per electrode volume. [Means for solving the problem]
[0007] In order to achieve the above object, the present inventors have conducted extensive research and have found that, when a cross section of an electrode is observed by SEM and image analyzed, an average non-contact ratio, which is a ratio of the area of the boundary between the active material and pores to the area of the contour of the active material, is 8% or less, in an electrode containing a cubic lithium composite oxide active material, the energy density per electrode volume can be further increased, and the present inventors have completed the invention disclosed in this specification.
[0008] That is, the electrode disclosed in the present specification is The electrode comprises an active material of a lithium composite oxide containing Li and a metal element other than Li and having a cubic crystal structure, and a conductive material, and may contain a binder. The conductive material has pores, and the content of the conductive material is 20 mass% or less. When a cross section of the electrode is observed with a SEM and subjected to image analysis, the average non-contact ratio, which is the ratio of the area of the boundary line between the active material and the pores to the area of the outline of the active material, is 8% or less.
[0009] The electricity storage device disclosed in the present specification is The above-mentioned electrode, an ionically conductive medium in contact with the electrode and conducting lithium ions; It is equipped with the following:
[0010] The method for producing a lithium composite oxide disclosed in the present specification includes the steps of: The active material is a lithium composite oxide having a cubic crystal structure containing Li and metal elements other than Li, and a bulk density of 0.07 g / cm 3 An electrode is produced using an electrode mixture prepared by mixing a first conductive material described below, and then adding a second conductive material having a bulk density greater than that of the first conductive material and, if necessary, a binder. Effect of the Invention
[0011] In the present disclosure, it is possible to provide an electrode, an electricity storage device, and a method for manufacturing an electrode that can further increase the energy density per electrode volume. The reason for obtaining such an effect is presumed to be as follows. For example, an active material of a lithium composite oxide having a cubic crystal structure tends to have a high capacity per active material mass but a low conductivity compared to layered rock salt type active materials, and a large amount of conductive material is often used to extract the capacity of the active material. In contrast, in the present disclosure, conductive material and vacancies are appropriately arranged around the active material, so that it is possible to efficiently extract the capacity of the active material without using a large amount of conductive material, and it is presumed that the energy density per electrode volume can be increased. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram showing an example of the configuration of an electricity storage device 20. [Diagram 2] 4 shows discharge curves of half cells using the positive electrode active materials of Experimental Examples 1 to 6. [Diagram 3] 4 is a graph showing the relationship between electrode density and discharge capacity in Experimental Examples 1 to 6. [Figure 4] FIG. 13 is a diagram showing the process of deriving the non-contact ratio in Experimental Example 3. [Diagram 5] FIG. 13 is a diagram showing the process of deriving the non-contact ratio in Experimental Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [electrode] The electrode of this embodiment is an electrode used in an electricity storage device. The electricity storage device may be any one of a lithium secondary battery, a lithium ion secondary battery, a capacitor, a hybrid capacitor, an air battery, and the like. The electrode becomes either a positive electrode or a negative electrode based on the potential of the counter electrode relative to the potential of the active material. The active material absorbs and releases carrier ions of the electricity storage device. The carrier ions are not particularly limited as long as they are used in the electricity storage device, and examples thereof include alkali metal ions and Group 2 element ions. Examples of alkali metal ions include lithium ions, sodium ions, and potassium ions. Examples of Group 2 element ions include magnesium ions and calcium ions. Here, the following mainly describes a case where the electrode is a positive electrode of a lithium ion secondary battery using lithium ions as a carrier.
[0014] The electrode includes an active material and a conductive material, may include a binder, and has pores. The pores may be filled with an ion conductive medium or the like. The electrode may include a current collector and an electrode mixture formed on the current collector. In this case, the electrode mixture includes an active material and a conductive material, may include a binder, and may have pores.
[0015] The active material is a lithium composite oxide having a cubic crystal structure containing Li and a metal element other than Li. Examples of the cubic crystal structure include a rock salt structure and a spinel structure. The lithium composite oxide may have an XRD spectrum that shows a peak pattern of a cubic disordered rock salt structure (also called a random rock salt structure) or a cubic spinel structure. The lithium composite oxide having a disordered rock salt structure may have a peak pattern in the XRD spectrum having at least four diffraction peaks in the ranges of 2θ of 35° to 39°, 42° to 48°, 62° to 68°, and 80° to 84°. In addition, since it has a disordered structure, the diffraction peaks are relatively broad, and the half width of the main peak at 2θ=42° to 48° may be 1.5° or more, and the half width of the peak at 2θ=62° to 68° may be 2° or more. The lithium composite oxide having a spinel structure may also show a peak pattern in the XRD spectrum having at least five diffraction peaks in the ranges of 2θ from 15° to 22°, 33° to 39°, 42° to 48°, 62° to 68°, and 80° to 84°. In addition, in the spinel structure, the diffraction peaks may be relatively broad, and the half-width of the peak at 2θ=15° to 22° may be 1.5° or more, and the half-width of the main peak at 2θ=42° to 48° may be 1.5° or more. The lithium composite oxide preferably has a disordered rock salt crystal structure. The lithium composite oxide having a disordered rock salt structure is different from the layered positive electrodes that have been used in the past, in that Li can migrate three-dimensionally, and it is considered that more Li ions can be inserted and removed.
[0016] This lithium composite oxide may contain, as a metal element, for example, one or more of Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge, among which those containing Mn are preferred. This lithium composite oxide may contain, for example, one or more non-metal elements of B and P, and these may substitute for a part of the above-described metal elements. Further, this lithium composite oxide may contain one or more selected from the group consisting of F, Cl, Br, I, and S, and these may substitute for a part of oxygen.
[0017] This lithium composite oxide has the general formula Li a M x O 2-y A y and may be represented by this formula. However, in the general formula Li a M x O 2-y A y 0 < a < 2, 0 < x < 2, and 0 ≤ y < 2, where M is one or more selected from the group consisting of B, P, Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge, and A is one or more selected from the group consisting of F, Cl, Br, I, and S. The content a of Li in the general formula Li a M x O 2-y A y varies depending on the intercalation and deintercalation of lithium ions and can be any value, but for example, it may satisfy 1 ≤ a ≤ 1.25 in a state where charging and discharging are not performed. This lithium composite oxide may contain, as the element M, a metal element Me (one or more of Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Vu, Zn, Ga, and Ge), and among these, it may contain a transition metal element (one or more of Ti, V, Cr, Mn, Fe, Co, Ni, and Cu), and it is preferably at least Mn-containing. This lithium composite oxide may contain, as the element M, in addition to the metal element Me, a non-metal element Mx (one or more of B and P). At this time, the lithium composite oxide has the general formula Li a Mx x1 Me x2 O2-y A y The general formula Li a M x O 2-y A y In the formula, the content x of the element M may be 0.8 or more, 0.85 or more, or 0.90 or more. The content x may be less than 1, 0.98 or less, 0.96 or less, or 0.95 or less. The content x1 of the nonmetallic element Mx may be 0≦x1≦0.3. The content x2 of the metal element Me may be 0.5≦x2≦0.98. When the nonmetallic element Mx is P, the content x1 of the nonmetallic element Mx preferably satisfies 0.02≦x1≦0.08, and more preferably satisfies 0.03≦x1≦0.08. When the nonmetallic element Mx is P, the content x2 of the metal element Me preferably satisfies 0.65≦x2<1, and more preferably satisfies 0.7≦x2≦0.95. When the nonmetallic element Mx is B, the content x1 of the nonmetallic element Mx preferably satisfies 0.03≦x1≦0.27, and more preferably satisfies 0.05≦x1≦0.25. When the nonmetallic element Mx is B, the content x2 of the metallic element Me preferably satisfies 0.75≦x2<1, and more preferably satisfies 0.8≦x2≦0.95. a M x O 2-y A y In the formula, the element A may be, for example, one or more of F, Cl, Br, I, and S, among which a halogen element is preferable, and may be F. The content y of the element A preferably satisfies 0≦y<0.5, and may also satisfy 0.3≦y<0.5. This lithium composite oxide may have oxygen defects, but it is preferable to have fewer oxygen defects. It is presumed that the reduction of oxygen defects makes the electronic state of adjacent Mn ideal, and sufficient oxidation and reduction are performed, thereby further improving the discharge capacity. This lithium composite oxide is represented by the general formula Li a M x O 2-y A yin the formula Li that reflects the oxygen defect z a M x O 2-y-z A y wherein the oxygen defect z may satisfy 0 ≦ z ≦ 0.15. This oxygen defect z preferably satisfies z ≦ 0.10, more preferably satisfies z ≦ 0.05, and still more preferably satisfies z ≦ 0.03. When this lithium composite oxide contains P in element M, the oxygen defect may be reduced by PO4 ions. At this time, the lithium composite oxide may be represented by the general formula Li a P x1 Mn x2 O 2-z and may satisfy 0 < a < 2, 0 < x1 ≦ 0.09, 0 < x2 < 1, and 0 ≦ z ≦ 0.15.
[0018] This lithium composite oxide may be, for example, the lithium composite oxide disclosed in JP-A-2018-92958, JP-A-2017-202954, JP-T-2019-523532, JP-A-2015-166291, JP-A-2016-25009, JP-A-2021-128880, ACS Cent Sci, 6 (2020) 2326-2338, Nat. Commun., 2019, 10, 592, Energy Environ. Sci., 2018, 11, 926-932, Nature, 2018, 556, 185-190, Nature Energy, 2020, 5, 213-221, ACS Cent Sci, 2020, 6, 2326-2338, etc.
[0019] The electrode may be formed by forming an electrode mixture on a current collector, the electrode mixture being a mixture of an active material, a conductive material, and, if necessary, a binder. In forming the electrode, the electrode mixture may be used in the form of an electrode mixture slurry using an appropriate solvent, or the electrode mixture slurry may be applied to a current collector, dried, and, if necessary, compressed to increase the electrode density. In forming the electrode, the electrode mixture may be formed in a dry manner without being slurried. The electrode may have a conductive material content of 20% by mass or less, preferably 17% by mass or less, and more preferably 15% by mass or less. In the electrode, the conductive material content may be 5% by mass or more, 7% by mass or more, or 10% by mass or more. In the electrode, the active material content may be 75% by mass or more, 77% by mass or more, or 80% by mass or more. In the electrode, the active material content may be 90% by mass or less, 85% by mass or less, or 80% by mass or less. In the electrode, the content of the binder may be 1 mass% or more, 3 mass% or more, or 5 mass% or more. In the electrode, the content of the binder may be 10 mass% or less, or 8 mass% or less. Note that the contents of the conductive material, active material, and binder are values when the entire electrode mixture is taken as 100 mass%, even if the electrode has a current collector.
[0020] The conductive material is not particularly limited as long as it is an electron conductive material that does not adversely affect the battery performance of the positive electrode, and can be, for example, one or a mixture of two or more of graphite such as natural graphite (scale graphite, flake graphite) and artificial graphite, acetylene black, carbon black, ketjen black, carbon whisker, needle coke, carbon fiber, metals (copper, nickel, aluminum, silver, gold, etc.), etc. Among these, from the viewpoint of electron conductivity and coatability, one or more of ketjen black, carbon black, and acetylene black are preferable as the conductive material.
[0021] The conductive material may include a first conductive material having a low bulk density and a second conductive material having a bulk density higher than that of the first conductive material. The bulk density of the first conductive material is 0.07 g / cm 3 It may be less than 0.06g / cm3 It may be less than 0.05 g / cm 3 The bulk density of the first conductive material may be 0.01 g / cm or less. 3 or more, 0.02 g / cm 3 or more, 0.03 g / cm 3 The bulk density of the second conductive material may be 0.07 g / cm or more. 3 It is acceptable to exceed 0.08g / cm 3 or more, 0.09 g / cm 3 The bulk density of the second conductive material may be 0.15 / cm or more. 3 It may be less than 0.12 g / cm 3 It may be less than 0.11 g / cm 3 It may be less than 100%. Of the first conductive material and the second conductive material, it is preferable that the first conductive material having a low bulk density is mostly distributed around the active material. The first conductive material having a low bulk density may be more conductive than the second conductive material. It is considered that the capacity of the active material can be efficiently drawn by disposing the first conductive material having a high conductivity around the active material. It is also considered that the capacity of the active material can be more efficiently drawn by disposing the high-density second conductive material around the first conductive material. As the first conductive material, ketjen black and acetylene black are preferable, and ketjen black is more preferable. As the second conductive material, carbon black, flake graphite, carbon nanotubes, rod-shaped graphite, etc. are preferable, and carbon black is more preferable. The first conductive material may be less than the second conductive material, and the first conductive material may be 90% by mass or less, 70% by mass or less, or 50% by mass or less of the second conductive material. The first conductive material may account for 30% by mass or more of the second conductive material, 40% by mass or more, or 50% by mass or more.
[0022] The binder plays a role of binding the active material particles and the conductive material particles, and can be, for example, fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, or thermoplastic resins such as polypropylene and polyethylene, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, natural butyl rubber (NBR), etc., used alone or as a mixture of two or more kinds. In addition, a cellulose-based aqueous binder or an aqueous dispersion of styrene butadiene rubber (SBR) can also be used. As a solvent for dispersing the active material, conductive material, and binder, for example, an organic solvent such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran can be used. In addition, a dispersant, a thickener, etc. can be added to water, and the active material can be slurried with latex such as SBR. As the thickener, for example, polysaccharides such as carboxymethylcellulose and methylcellulose can be used alone or as a mixture of two or more kinds. Examples of the coating method include roller coating such as an applicator roll, screen coating, doctor blade method, spin coating, bar coater, etc., and any of these can be used to obtain any thickness and shape. As the current collector, in addition to aluminum, titanium, stainless steel, nickel, iron, baked carbon, conductive polymer, conductive glass, etc., aluminum or copper whose surface is treated with carbon, nickel, titanium, silver, etc. for the purpose of improving adhesion, conductivity, and oxidation resistance can be used. The surface of these can also be subjected to oxidation treatment. Examples of the shape of the current collector include foil, film, sheet, net, punched or expanded, lath, porous, foamed, and fiber group formed bodies. The thickness of the current collector is, for example, 1 to 500 μm.
[0023] When the cross section of this electrode is observed with an SEM and image analyzed, the average non-contact ratio, which is the ratio of the area of the boundary between the active material and the pores to the area of the contour of the active material, is 8% or less. The average non-contact ratio is determined as follows. First, a scanning electron microscope (SEM) is used to observe a field of view of 5.9 μm × 4.5 μm to obtain an SEM image (backscattered electron image) of 927 pixels × 698 pixels. In the SEM image, the active material usually appears white, the mixture of the conductive material and the binder gray, and the pores black. Image analysis is performed on this SEM image using OpenCV, an open library for Python. Specifically, first, the SEM image is converted to a ternary value. The threshold value used for the ternary value conversion (here, the lower threshold value is L and the higher threshold value is H) is selected based on experience as an appropriate value according to the SEM image. The obtained ternary image is pre-processed by performing an open process (one contraction → one expansion) and a close process (one expansion → one contraction) twice in this order using morphological calculations. Next, the pre-processed image is subjected to a morphological gradient process to extract the contour line of the active material. In addition, the pre-processed image is subjected to a morphological gradient process to separate the area around the positive electrode active material into the area in contact with the conductive part (conductive material + binder part) and the area in contact with the pores, and the boundary line between the active material and the pores is extracted. Then, the area of the contour line of the active material and the area of the boundary line between the active material and the pores are calculated, and the non-contact ratio is calculated from the formula: non-contact ratio [%] = (area of the boundary line between the active material and the pores) × 100 / (area of the contour line of the active material). Note that a 3 × 3 square structuring element (kernel) is used for the morphological calculation and morphological gradient process. For each SEM image of one field of view, the non-contact ratio is calculated for a total of 49 patterns, including seven patterns of low thresholds, L-3, L-2, L-1, L, L+1, L+2, and L+3, and seven patterns of high thresholds, H-3, H-2, H-1, H, H+1, H+2, and H+3. This is performed for SEM images of five fields of view, and the average value and standard deviation of the non-contact ratio are calculated from a total of 245 data. The average value of the non-contact ratio may be 6.7% or less, 6.5% or less, or 6% or less.The average value of the non-contact ratio may be 2% or more, 3% or more, 4% or more, or 5% or more. The standard deviation of the non-contact ratio may be within ±1.5%, within ±1.2%, or within ±1.0%. The maximum value of the non-contact ratio may be 12% or less, 11% or less, or 8% or less. The maximum value of the non-contact ratio may be 6% or more, 6.5% or more, or 7% or more. The minimum value of the non-contact ratio may be 1% or more, 1.5% or more, or 2% or more. The minimum value of the non-contact ratio may be 5.5% or less, 5% or less, or 4% or less.
[0024] The electrode has an energy density per electrode volume of preferably 700 Wh / L or more, more preferably 800 Wh / L or more, even more preferably 900 Wh / L or more, and may be 1100 Wh / L or more. The energy density per electrode volume is the energy density per volume of the electrode mixture even when the electrode has a current collector. The energy density is the energy density at the first discharge when a charge / discharge measurement is performed on an electricity storage device including the electrode at a temperature environment of 20°C, a potential range of 4.8 to 1.5 V with respect to a lithium reference potential, and a current value of 20 mA / g.
[0025] The electrode has a discharge capacity per active material mass of preferably 300 mAh / g or more, more preferably 310 mAh / g or more, further preferably 320 mAh / g or more, and may be 330 mAh / g or more. Note that this discharge capacity is the initial discharge capacity when a charge / discharge measurement is performed on an electricity storage device including the electrode at a temperature of 20° C., in a potential range of 4.8 to 1.5 V with respect to a lithium reference potential, and at a current value of 20 mA / g.
[0026] This electrode has an electrode density of 0.5 g / cm 3 or more, and may be 0.7 g / cm 3 or more, and may be 0.9 g / cm 3The electrode density may be 1.7 g / cm or more. 3 It may be 1.5 g / cm or less. 3 It may be less than or equal to 1.3 g / cm 3 The electrode density is defined as the density of the electrode mixture even in the case where the electrode has a current collector.
[0027] [Electrode manufacturing method] The method for producing an electrode according to the present embodiment is a method for producing an electrode used in an electricity storage device. This method may be a method for producing the above-mentioned electrode. In this electrode production method, an active material of a lithium composite oxide containing Li and a metal element other than Li and having a cubic crystal structure and a bulk density of 0.07 g / cm 3 After mixing the first conductive material described below, a second conductive material having a bulk density greater than that of the first conductive material and, if necessary, a binder are mixed to prepare an electrode composite material, and an electrode is produced using the electrode composite material. The manufacturing method of this electrode may include an active material step of preparing an active material, a mixing step of mixing the active material and the first conductive material, a mixing step of preparing an electrode composite material using the mixture obtained in the mixing step, and a forming step of forming an electrode using the electrode composite material obtained in the mixing step. In the manufacturing method of this electrode, for example, an active material of a lithium composite oxide may be separately prepared, and the active material step may be omitted. The materials, compounding ratios, compositions, and the like may be appropriately selected from those exemplified in the above-mentioned electrodes.
[0028] (Active material process) In the active material step, an active material of a lithium composite oxide containing Li and a metal element other than Li and having a cubic crystal structure is prepared. In the active material step, an active material of a lithium composite oxide containing Li and a metal element other than Li may be pulverized to prepare an active material of a lithium composite oxide having a cubic crystal structure. In the active material step, a raw material preparation process for preparing an orthorhombic lithium composite oxide and a pulverization process may be performed.
[0029] In the raw material preparation process, an orthorhombic lithium composite oxide containing Li and a metal element other than Li may be prepared while adjusting the firing conditions. The orthorhombic lithium composite oxide may contain one or more of Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge as a metal element. In this raw material preparation process, an orthorhombic LiMeO2 may be prepared. In the orthorhombic LiMeO2, Li2MeO3, and MeO described later, the metal element Me may be one or more of Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge. In the raw material preparation process, first, the raw material Li2MeO3 may be obtained by firing at 800°C to 1100°C for 6 hours to 15 hours. Orthorhombic LiMeO2 can be obtained, for example, by blending equimolar amounts of Li2MeO3 and MeO and firing them in an inert atmosphere (for example, in Ar) at a temperature in the range of 900°C to 1100°C for 6 hours to 24 hours.
[0030] In the pulverization process, a lithium composite oxide having a cubic crystal structure containing Li and metal elements other than Li may be prepared by pulverizing an orthorhombic lithium composite oxide. In the pulverization process, it is preferable to pulverize the orthorhombic lithium composite oxide by a mechanochemical method. The pulverization can be performed, for example, by a ball mill or a planetary ball mill, and is particularly preferably performed by a planetary ball mill. In the planetary ball mill, the rotation speed may be appropriately set according to the volume of the raw material to be contained, and is preferably, for example, in the range of 400 rpm to 1000 rpm, more preferably in the range of 500 rpm to 800 rpm, and more preferably in the range of 550 rpm to 650 rpm. The time of the pulverization process may be, for example, 2 hours to 40 hours. By performing such a pulverization process, a cubic lithium composite oxide can be prepared.
[0031] In the pulverization process, in addition to the orthorhombic lithium composite oxide obtained in the raw material preparation process, one or more of an Mx source containing a nonmetallic element Mx (one or more of B and P) and an A source containing an element A (one or more of F, Cl, Br, I and S) may be blended and mixed and pulverized. In the pulverization process, first, a lithium composite oxide having a cubic crystal structure is prepared without adding the Mx source or the A source, and then one or more of the Mx source and the A source are blended and mixed and pulverized. The Mx source may be a composite oxide containing Li and one or more of P and B, such as Li3PO4 and Li2B4O7. The A source may be a compound containing Li and element A, such as LiF, LiCl, LiBr, LiI, Li2S, and LiF is preferred. A lithium composite oxide having a cubic crystal structure is obtained by such a pulverization process.
[0032] After the crushing process, a heat treatment may be performed in an oxidizing atmosphere at 250°C to 500°C. The heat treatment can reduce oxygen defects, which is preferable. The heat treatment is more preferably performed under conditions that cause less transition from the disordered rock salt structure to the spinel structure, or less crystallization. In the heat treatment, the lithium composite oxide obtained by the crushing process is oxidized, so that oxygen defects can be further reduced. For example, the heat treatment is preferably performed under an oxygen atmosphere, or may be performed in an air atmosphere. The heat treatment may be performed at a temperature range of 275°C or higher, 300°C or higher, or 400°C or lower, 350°C or lower, or 325°C or lower. The heat treatment time may be 10 minutes or more, 20 minutes or more, 30 minutes or more, or 2 hours or less, 1 hour or less, or 45 minutes or less.
[0033] (Mixing process) In the mixing process, the active material and the sintered body having a bulk density of 0.07 g / cm 3 The first conductive material is mixed with the conductive material described below. As the first conductive material, a conductive material having a bulk density of 0.07 g / cm3 or more is selected from the conductive materials exemplified as the conductive material for the electrode described above. 3The following conductive materials may be appropriately selected. As the first conductive material, for example, Ketjen Black may be suitably used. A mortar, a mixer, a ball mill, a bead mill, or the like may be used to mix the active material and the first conductive material, and among these, a mortar is preferably used. The temperature during mixing is not particularly limited, and may be 0°C or higher and 50°C or lower, 10°C or higher and 40°C or lower, or 20°C or higher and 30°C or lower. The mixing time may be appropriately set depending on the mixing method. In the mixing step, the active material particles may be mixed under conditions such that the first conductive material adheres to or is compounded with the surface of the active material particles while maintaining their shape.
[0034] (Mixture process) In the combining step, an electrode mixture is prepared using the mixture obtained in the mixing step, a second conductive material having a bulk density greater than that of the first conductive material, and, if necessary, a binder. In the combining step, an electrode mixture slurry may be prepared by making the mixture into a slurry using a solvent. As the second conductive material, a conductive material having a bulk density greater than that of the first conductive material may be appropriately selected from the conductive materials exemplified as the conductive material for the electrode described above. The second conductive material has a bulk density of 0.07 g / cm 3 The amount of the second conductive material may be in excess of the amount of the binder. For example, carbon black may be suitably used as the second conductive material. The binder and the solvent may be appropriately selected from those exemplified as the binder and the solvent for the electrode described above. In the mixing step, the mixture obtained in the mixing step, the second conductive material, the binder, the solvent, etc. may be mixed by stirring or the like to prepare an electrode mixture.
[0035] (Formation process) In the forming step, an electrode is formed using the electrode mixture prepared in the mixing step. In the forming step, the electrode mixture may be formed on a current collector. In the forming step, the electrode mixture slurry may be applied to the surface of the current collector and dried, and the electrode density may be compressed as necessary to form an electrode. In the forming step, the electrode mixture may be formed into a pellet shape or the like in a dry manner and pressed together with the current collector to form the electrode. By carrying out such steps, for example, the above-mentioned electrode can be formed.
[0036] [Electricity storage device] The electric storage device of this embodiment includes the above-mentioned electrode and an ion conductive medium that contacts the electrode and conducts lithium ions. This electric storage device may include a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, and an ion conductive medium that is interposed between the positive electrode and the negative electrode and conducts lithium ions. This electric storage device may include the above-mentioned electrode as a positive electrode. In addition, this electric storage device may be a lithium secondary battery that uses metallic lithium or a lithium alloy as a negative electrode active material, a lithium ion secondary battery that has a negative electrode active material that absorbs and releases lithium ions, or a hybrid capacitor that has a negative electrode active material that absorbs and desorbs ions.
[0037] The positive electrode is the electrode described above, that is, an electrode that contains an active material of a lithium composite oxide containing Li and metal elements other than Li and having a cubic crystal structure, a conductive material, and may contain a binder, has pores, has a conductive material content of 20 mass% or less, and when the cross section of the electrode is observed with an SEM and image analyzed, the average non-contact ratio, which is the ratio of the area of the boundary line between the active material and the pores to the area of the outline of the active material, is 8% or less.
[0038] The negative electrode may be formed by bonding a negative electrode active material and a current collector, or may be formed by mixing a negative electrode active material, a binder, and optionally a conductive material, adding an appropriate solvent to form a paste-like negative electrode material, applying it to the surface of a current collector, drying it, and compressing it to increase the electrode density as necessary. Examples of the negative electrode active material include inorganic compounds such as lithium, lithium alloys, and tin compounds, carbonaceous materials capable of absorbing and releasing lithium ions, composite oxides containing multiple elements, and conductive polymers. Examples of the carbonaceous material include cokes, glassy carbons, graphites, non-graphitizable carbons, pyrolytic carbons, and carbon fibers. Among these, graphites such as artificial graphite and natural graphite are preferred because they have an operating potential close to that of metallic lithium, can be charged and discharged at a high operating voltage, and can suppress self-discharge when a lithium salt is used as a supporting salt, and can reduce irreversible capacity during charging. Examples of the composite oxide include lithium titanium composite oxide and lithium vanadium composite oxide. Of these, carbonaceous materials are preferred as the negative electrode active material from the viewpoint of safety. The conductive material, binder, solvent, etc. used in the negative electrode can be the same as those exemplified in the above-mentioned electrodes. In addition to copper, nickel, stainless steel, titanium, aluminum, baked carbon, conductive polymer, conductive glass, Al-Cd alloy, etc., the negative electrode current collector can also be one in which the surface of, for example, copper, etc. is treated with carbon, nickel, titanium, silver, etc. for the purpose of improving adhesion, conductivity, and reduction resistance. The surfaces of these can also be oxidized. The shape of the current collector can be the same as those exemplified in the above-mentioned electrodes.
[0039] The ion-conducting medium may be a non-aqueous electrolyte solution containing a supporting salt containing lithium and a non-aqueous solvent. Examples of the solvent for the non-aqueous electrolyte solution include carbonates, esters, ethers, nitriles, furans, sulfolanes, and dioxolanes, which may be used alone or in combination. Specific examples of carbonates include cyclic carbonates such as ethylene carbonate, propylene carbonate, vinylene carbonate, butylene carbonate, and chloroethylene carbonate; chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl-n-butyl carbonate, methyl-t-butyl carbonate, di-i-propyl carbonate, and t-butyl-i-propyl carbonate; cyclic esters such as γ-butyl lactone and γ-valerolactone; chain esters such as methyl formate, methyl acetate, ethyl acetate, and methyl butyrate; ethers such as dimethoxyethane, ethoxymethoxyethane, and diethoxyethane; nitriles such as acetonitrile and benzonitrile; furans such as tetrahydrofuran and methyltetrahydrofuran; sulfolanes such as sulfolane and tetramethylsulfolane; and dioxolanes such as 1,3-dioxolane and methyldioxolane. Of these, a combination of a cyclic carbonate and a chain carbonate is preferred.
[0040] Examples of the supporting salt include LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiSbF6, LiSiF6, LiAlF4, LiSCN, LiClO4, LiCl, LiF, LiBr, LiI, and LiAlCl4. Among these, it is preferable to use one or more salts selected from the group consisting of inorganic salts such as LiPF6, LiBF4, LiAsF6, and LiClO4, and organic salts such as LiCF3SO3, LiN(CF3SO2)2, and LiC(CF3SO2)3 in combination from the viewpoint of electrical properties. The concentration of this supporting salt in the non-aqueous electrolyte is preferably 0.1 mol / L or more and 5 mol / L or less, more preferably 0.5 mol / L or more and 2 mol / L or less. When the concentration of the supporting salt is 0.1 mol / L or more, a sufficient current density can be obtained, and when the concentration is 5 mol / L or less, the electrolyte can be more stable. The ion-conducting medium is not limited to a non-aqueous electrolyte containing a supporting salt and a non-aqueous solvent, and may be, for example, an ionic liquid, an aqueous electrolyte, or a solid electrolyte.
[0041] The electric storage device may have a separator between the negative electrode and the positive electrode. The separator is not particularly limited as long as it has a composition that can withstand the range of use of the electric storage device, and examples thereof include polymer nonwoven fabrics such as polypropylene nonwoven fabrics and polyphenylene sulfide nonwoven fabrics, and thin microporous films of olefin resins such as polyethylene and polypropylene. These may be used alone or in combination.
[0042] The shape of the electricity storage device is not particularly limited, and examples thereof include coin type, button type, sheet type, laminated type, cylindrical type, flat type, and square type. In addition, a plurality of such electricity storage devices may be connected in series to be applied to a large-sized device used in an electric vehicle or the like. FIG. 1 is a schematic diagram showing an example of an electricity storage device 20 of this embodiment. The electricity storage device 20 includes a positive electrode sheet 23 in which a positive electrode mixture 22 is formed on a current collector 21, a negative electrode sheet 26 in which a negative electrode mixture 25 is formed on the surface of a current collector 24, a separator 28 provided between the positive electrode sheet 23 and the negative electrode sheet 26, and a non-aqueous electrolyte solution 29 that fills the space between the positive electrode sheet 23 and the negative electrode sheet 26. In the electricity storage device 20, the separator 28 is sandwiched between the positive electrode sheet 23 and the negative electrode sheet 26, which are wound and inserted into a cylindrical case 32, and a positive electrode terminal 34 connected to the positive electrode sheet 23 and a negative electrode terminal 36 connected to the negative electrode sheet 26 are disposed. The positive electrode mixture 22 contains an active material of a lithium composite oxide containing Li and metal elements other than Li and having a cubic crystal structure, a conductive material, and may contain a binder. The positive electrode mixture 22 has pores, and the conductive material content is 20 mass% or less. When the cross section of the electrode is observed with an SEM, the average non-contact ratio, which is the ratio of the area of the boundary line between the active material and the pores to the area of the outline of the active material, is 8% or less.
[0043] In the electrode, the manufacturing method of the electrode, and the power storage device of the present embodiment described above in detail, the energy density per electrode volume can be further increased. The reason for obtaining such an effect is presumed to be as follows. For example, an active material of a lithium composite oxide having a cubic crystal structure tends to have a high capacity per active material mass but a low conductivity compared to a layered rock salt type active material, and a large amount of conductive material is often used to extract the capacity of the active material. In contrast, in the present disclosure, since the conductive material and vacancies around the active material are appropriately arranged, it is possible to efficiently extract the capacity of the active material without using a large amount of conductive material, and it is presumed that the energy density per electrode volume can be increased. For this reason, it can be suitably used in power storage devices arranged in a limited space, such as automobile on-board batteries and batteries for electronic devices such as smartphones.
[0044] In addition, the theoretical maximum capacity of layered rock salt type active materials expressed by the general formula LiMO2 (where M=Co, Ni, Mn) is about 280mAh / g per active material mass, but from the viewpoint of potential and structural stability, the capacity that can be extracted is about 70% of that. In contrast, in cubic active materials, Li can be charged and discharged three-dimensionally, so that a high discharge capacity can be realized. On the other hand, electrodes using cubic active materials tend to have a lower energy density per electrode volume than those using layered rock salt type active materials. This is presumably because cubic active materials have low electronic conductivity and a high surface area, and require a relatively large amount of conductive material. Since the conductive carbon has a lower density than the active material, if there is a lot of conductive material, the electrode becomes low density, and as a result, it is presumed that the energy density per electrode volume also decreases. In order to densify the electrode, it is possible to use high-density carbon with high density, but this alone cannot ensure electronic conductivity, and there is a risk of the capacity decreasing. In this embodiment, for example, by arranging Ketjen black, which has high electronic conductivity, close to the active material and arranging carbon black, which has a relatively high density, in its surroundings, the arrangement of the conductive material and voids is optimized, and it is presumed that the energy density per electrode volume can be increased.
[0045] It goes without saying that the present disclosure is in no way limited to the above-described embodiment, and can be embodied in various forms as long as it falls within the technical scope of the present disclosure.
[0046] The present disclosure may be any one of the following [1] to
[10] . [1] An electrode comprising: an active material of a lithium composite oxide containing Li and a metal element other than Li and having a cubic crystal structure; a conductive material; and optionally a binder; the electrode has pores, the conductive material content being 20 mass% or less; and when a cross section of the electrode is observed by SEM and image analyzed, the average non-contact ratio, which is the ratio of the area of the boundary line between the active material and the pores to the area of the outline of the active material, is 8% or less. [2] The lithium composite oxide has the general formula Li aM x O 2-y A y (However, 0 < a < 2, 0 < x < 2, 0 ≤ y < 2, M is one or more selected from the group consisting of B, P, Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge, and A is one or more selected from the group consisting of F, Cl, Br, I, and S), and the electrode according to [1], which contains P. [3] The electrode according to [1] or [2], which contains Mn as the metal element. [4] The electrode according to any one of [1] to [3], wherein the energy density per unit volume of the electrode is 700 Wh / L or more. [5] The electrode according to any one of [1] to [4], wherein the average value of the non-contact ratio is 7% or less. [6] The electrode according to any one of [1] to [5], wherein the content of the conductive material is 15% by mass or less. [7] The electrode according to any one of [1] to [6], wherein the discharge capacity per unit mass of the active material is 300 mAh / g or more. [8] The electrode according to any one of [1] to [7], and an ion conduction medium that contacts the electrode and conducts lithium ions, A power storage device comprising the same. [9] An active material of a lithium composite oxide containing a metal element other than Li and having a cubic crystal structure, and a first conductive material having a bulk density of 0.07 g / cm 3 or less are mixed, and then a second conductive material having a larger bulk density than the first conductive material and, if necessary, a binder are blended to prepare an electrode mixture, and an electrode is manufactured using the electrode mixture. A method for manufacturing an electrode.
[10] The method for manufacturing an electrode according to [9], wherein the total content of the first conductive material and the second conductive material in the electrode mixture is 20% by mass or less.
Examples
[0047] Hereinafter, examples of specifically manufacturing the electrode and the power storage device of the present disclosure will be described as experimental examples. Note that Experimental Examples 5 to 6 correspond to Examples, and Experimental Examples 1 to 4 correspond to Comparative Examples.
[0048] [Li 0.90 P 0.04 Mn 0.84 Synthesis of O2 cathode active material] Orthorhombic LiMnO2 was placed in a 500 mL zirconia pot together with 5 mm diameter zirconia balls as the raw material, and ground in a planetary ball mill at 560 rpm for 28 h to obtain LiMnO2 powder with a disordered rock salt phase. The LiMnO2 and Li3PO4 obtained by the above method as raw materials were mixed in an agate bowl so that Li3PO4 was 5 mass%, and then placed in a zirconia pot together with zirconia balls and ground in a planetary ball mill at 600 rpm for 36 h. The collected powder was fired in a tubular firing furnace in an air atmosphere at 300 °C for 30 minutes to obtain LiMnO2 powder with a cubic phase. 0.90 P 0.04 Mn 0.84 We synthesized an O2 positive electrode active material. In this positive electrode active material, both rock salt type and spinel type cubic crystal phases were confirmed.
[0049] [Preparation of positive electrode] (Experimental Example 1) Li 0.90 P 0.04 Mn 0.84 70 parts by mass of O2 positive electrode active material, Ketjen Black (KB, ECP-600JP, Lion, bulk density = 0.04 gcm -3 The mixture was crushed in a mixer to prepare a dry composite. The obtained composite was made into a circular pellet having a diameter of 10 mm, and pressed on an Al expand metal to obtain a positive electrode of Experimental Example 1. The weight of the composite layer was 19.8 mg / cm. 2 It was. (Experimental Example 2) Li 0.90 P 0.04 Mn 0.84The positive electrode active material of O2 was mixed in a ratio of 85 parts by mass, 10 parts by mass of Ketjen Black, and 5 parts by mass of a binder (polyvinylidene fluoride (PVDF)), and the mixture was made into a slurry using N-methyl-2-pyrrolidone (NMP) as a solvent. The slurry was applied to an Al current collector foil, dried, and cut into a circle of φ16 mm to obtain a positive electrode of Experimental Example 2. The weight of the mixture layer was 2.7 mg / cm. 2 It was. (Experimental Example 3) Li 0.90 P 0.04 Mn 0.84 85 parts by mass of O2 positive electrode active material, carbon black (CB, TB5500, manufactured by Tokai Carbon, bulk density = 0.10 g / cm 3 The mixture was mixed in a ratio of 10 parts by mass of the mixture (aluminum fluoride) and 5 parts by mass of a binder (PVDF), and slurried using NMP as a solvent. The mixture was applied to an Al current collector foil, dried, and cut into a circle with a diameter of 16 mm to obtain a positive electrode of Experimental Example 3. The weight of the mixture layer was 8.6 mg / cm. 2 It was. (Experimental Example 4) Li 0.90 P 0.04 Mn 0.84 The positive electrode of Experimental Example 4 was obtained by mixing 85 parts by mass of O2 positive electrode active material, 10 parts by mass of conductive carbon, and 5 parts by mass of binder (PVDF), forming a slurry using NMP as a solvent, coating and drying an Al current collector foil, and cutting out a circle of φ16 mm. In addition to CB and KB, fibrous graphite (FG) and carbon nanotubes (CNT) were used as conductive carbon. CB, KB, FG, and CNT were mixed in a mass ratio of 2:1:1:1. The weight of the composite layer was 6.1 mg / cm. 2 It was. (Experimental Example 5) Li 0.90 P 0.04 Mn 0.84 77 parts by mass of O2 positive electrode active material and 7 parts by mass of Ketjen Black were mixed in an agate bowl. Then, 8 parts by mass of carbon black and 8 parts by mass of a binder (PVDF) were mixed with a solvent of NMP to form a slurry, which was then applied to an Al current collector foil, dried, and cut into a circle of φ16 mm to obtain a positive electrode of Experimental Example 5. The weight of the mixture layer was 4.0 mg / cm. 2 It was. (Experimental Example 6) Li 0.90 P 0.04 Mn 0.84 85 parts by mass of O2 positive electrode active material and 3 parts by mass of Ketjen black were mixed in an agate bowl. Then, 7 parts by mass of carbon black, 5 parts by mass of a binder (PVDF), and a solvent of NMP were mixed to form a slurry, which was then applied to an Al current collector foil, dried, and cut into a circle of φ16 mm to obtain a positive electrode of Experimental Example 6. The weight of the mixture layer was 4.7 mg / cm. 2 It was.
[0050] [Positive electrode density] For the positive electrodes of Experimental Examples 1 to 6, the thickness and mass of the electrode were measured, and the volume of the electrode mixture was calculated to measure the electrode density.
[0051] [Charge and discharge of positive half-cell] A half cell was fabricated using the positive electrodes of Experimental Examples 1 to 6, metallic Li for the negative electrode, a separator (E20MMS manufactured by Tonen Chemical Co., Ltd.) and an electrolyte. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1M in a mixed solvent containing 30 volume % ethylene carbonate (EC), 40 volume % dimethyl carbonate (DMC), and 30 volume % ethyl methyl carbonate (EMC). Using the fabricated half cell, a test was performed at 4.8 to 1.5 V vs. Li + Constant current and constant voltage charge / discharge measurements were performed at a current value of 20 mA / g per mass of positive electrode active material in the potential range of 1000 V / Li. From the measurement results, the initial discharge capacity and volumetric energy density were calculated. The initial discharge capacity was taken as the discharge capacity per mass of positive electrode active material. The volumetric energy density was taken as the energy density per volume of the electrode mixture of the positive electrode during the initial discharge.
[0052] [Non-contact ratio in positive electrode] The cross-section of the positive electrode was taken and observed at Melco Semiconductor Engineering Co., Ltd. A scanning electron microscope (SEM) was used to observe the reflected electron microscope image at a magnification of 20,000 times. The cross-sectional SEM image of the positive electrode obtained by the above method (a field of view of 5.9 μm × 4.5 μm displayed in 927 pixels × 698 pixels) was used to calculate the non-contact ratio in the positive electrode by morphological analysis. Specifically, the SEM image was converted to a ternary value using OpenCV, an open library for Python, and divided into three parts: the positive electrode active material part (white), the conductive material + binder part (gray), and the void part (black). The threshold value for the ternary value conversion was determined after checking each cross-sectional SEM image, and the appropriate value was used for each, and the values of -3, -2, -1, +1, +2, and +3 were also used for the analysis. The obtained ternary image was pre-processed by performing expansion and contraction processing using morphological calculations, and then morphological gradient processing was performed to separate the area around the positive electrode active material into areas in contact with the conductive material (conductive material + binder area) and areas in contact with pores. This analysis allowed the calculation of the non-contact ratio, which indicates the ratio of areas not in contact with the conductive material (conductive material + binder area) on the surface of the positive electrode active material. The analysis was performed using five cross-sectional SEM images at a magnification of 20,000 times, and the average and standard deviation of all 245 data were calculated for 49 patterns with different ternary conversion conditions.
[0053] [Results and Discussion] Table 1 summarizes the types and composition ratios of the positive electrode active material, conductive material, and binder, electrode density, initial discharge capacity, non-contact ratio, and energy density per volume for Experimental Examples 1 to 6. Figure 2 shows the discharge curves of half cells using the positive electrode active materials of Experimental Examples 1 to 6. Figure 3 shows the relationship between electrode density and discharge capacity for Experimental Examples 1 to 6. Figure 4 shows the process of deriving the non-contact ratio for Experimental Example 3. Figure 5 shows the process of deriving the non-contact ratio for Experimental Example 5.
[0054] (Relationship between electrode density and charge / discharge capacity) In Experimental Example 1, in which the composition ratio of Ketjen Black was sufficiently high, an extremely high discharge capacity of 359 mAh / g was shown. However, while Ketjen Black has high electronic conductivity, it is bulky and has low density, so the electrode density of Experimental Example 1 was 0.32 g / cm 3 This was lower than the positive electrodes of the other experimental examples. Therefore, the energy density per electrode volume of Experimental Example 1 was low at 244 Wh / L.
[0055] In Experimental Example 2, in which the proportion of Ketjen Black was reduced, the discharge capacity was 297 mAh / g, a value lower than that of Experimental Example 1. This was presumably because the electronic conductivity could not be secured as compared to Experimental Example 1. On the other hand, in Experimental Example 2, the energy density per electrode volume was improved to 542 Wh / L. This was due to the fact that the electrode density was 0.70 g / cm 3 It was presumed that this was because the
[0056] In Experimental Example 3, in which carbon black was used instead of bulky Ketjen black, the discharge capacity was 272 mAh / g, which was even lower than that of Experimental Example 2. This was presumably because the electronic conductivity could not be secured as compared to Experimental Example 2. On the other hand, in Experimental Example 3, the energy density per electrode volume was further improved to 945 Wh / L. This was due to the fact that the electrode density was 1.32 gcm -3 It was presumed that this was because the
[0057] In experimental example 4, which mixed Ketjen black, which has high electronic conductivity but low density, with carbon black, which has low electronic conductivity but high density, the discharge capacity was 277 mAh / g and the energy density per volume was 653 Wh / L.
[0058] For the four positive electrodes of Experimental Examples 1 to 4, as shown in FIG. 2, the electrode density and the discharge capacity have a mutually exclusive relationship, and it was presumed that there is a limit to the energy density per volume.
[0059] Therefore, the electrode manufacturing process and raw materials were improved to manufacture the positive electrodes of Experimental Examples 5 and 6. The improvement in the manufacturing process was that the positive electrode active material was mixed with Ketjen black, which has high electronic conductivity, in advance, and then mixed with carbon black to form a slurry and apply it. It was presumed that this process would make it possible to densify the electrode while ensuring the conductivity of the positive electrode as much as possible.
[0060] The positive electrode of Experimental Example 5, which was produced by the improved method, showed a discharge capacity of 334 mAh / g and the energy density per electrode volume increased to 749 Wh / L. This is because the electrode density was increased to 0.94 g / cm while the conductivity was ensured by Ketjen black. 3 It was speculated that this was because the
[0061] Furthermore, the positive electrode of Experimental Example 6, which was produced by optimizing the raw material ratio, exhibited a discharge capacity of 322 mAh / g and an energy density per electrode volume of 1103 Wh / L, both of which were very high values.
[0062] As shown in FIG. 2, the positive electrodes of Experimental Examples 5 to 6 deviated from the mutually exclusive trend lines obtained in Experimental Examples 1 to 4, and it was found that the discharge capacity could be increased even with the same electrode density.
[0063] (Quantification of active material conductive paths through image analysis of SEM observations) To evaluate the electronic conductivity of the electrode, we performed scanning electron microscope (SEM) observations and analyzed the collected images to attempt to quantify the conductive paths of the pseudo positive electrode active material. As a representative example, Figure 4A shows a cross-sectional SEM image (backscattered electron image) of the positive electrode of Experimental Example 3. The whiter and brighter areas are the positive electrode active material (Li 0.90 P 0.04 Mn 0.84O2), and it was confirmed that the gray parts represent the mixture of conductive material and binder, and the black parts represent voids. From Figure 4A, it was found that the positive electrode active material has parts that are in contact with the mixture of conductive material and binder, and parts that are not in contact (in contact with voids). It was thought that the capacity of the positive electrode active material in contact with voids was not extracted in the half cell. Therefore, it was presumed that quantifying how much of the positive electrode active material is in contact with voids would provide an index of whether or not capacity can be extracted. Therefore, the extent to which the positive electrode active material is in contact with voids was quantified by image processing of the SEM images.
[0064] The process of analyzing the positive electrode of Experimental Example 3 is shown in Figures 4A to 4F. Figure 4B is a diagram in which the cross-sectional SEM image of Figure 4A is ternarized with thresholds L = 96 and H = 130, and is divided into a mixture containing a positive electrode active material and a conductive material, and voids. In this figure, the noise of each element was significant, so open processing and close processing were performed in image processing to clarify each part. The result is shown in Figure 4C. It was found that the separation of each element was better in Figure 4C than in Figure 4B. By performing morphological gradient processing on this figure, an image of the periphery of the positive electrode active material (Figure 4D) and an image of the part in contact with the void part were calculated. When this area ratio was calculated as the non-contact ratio in the positive electrode, it was 10.9% as shown in Figure 4F. For the positive electrode of Experimental Example 3, a similar analysis was performed on 49 patterns with different threshold values for five cross-sectional SEM images including FIG. 4A, and the non-contact rate was 8.5±1.7%.
[0065] The process of analyzing the positive electrode of Experimental Example 5 is shown in Figures 5A to 5F. Figure 5B is a diagram in which the cross-sectional SEM image of Figure 5A is ternarized with thresholds L = 71 and H = 134, and is divided into a mixture containing a positive electrode active material and a conductive material, and voids. In this figure, the noise of each element was significant, so open processing and close processing were performed as in Experimental Example 3, and the results are shown in Figure 5C. For this figure, a morphology gradient processing was performed to calculate an image around the positive electrode active material (Figure 5D) and an image of the part in contact with the void part (Figure 5E). When this area ratio was calculated as the non-contact ratio in the positive electrode, it was 3.3% as shown in Figure 5F. When the same analysis was performed on 49 patterns with different thresholds for five cross-sectional SEM images including Figure 5A, the non-contact ratio was 4.2 ± 0.8%, which was smaller than the value of the positive electrode of Experimental Example 3. It was presumed that a small value of the non-contact ratio means that the positive electrode active material and the conductive material are in closer contact with each other. The average values of the non-contact ratios in Experimental Examples 5 and 6 were 4.2% and 6.5%, respectively, which were smaller than the average values of the non-contact ratios in the positive electrodes in Experimental Examples 1 to 4. From this, it was presumed that the positive electrodes in Experimental Examples 5 and 6 had good contact between the positive electrode active material and the conductive material, and thus were able to extract high capacity. In particular, it was found that Experimental Example 6 was preferable because it was able to achieve an energy density per electrode volume of more than 1100 Wh / L.
[0066] [Table 1]
[0067] It goes without saying that the present disclosure is in no way limited to the above-described embodiments, and can be embodied in various forms as long as they fall within the technical scope of the present disclosure. [Industrial Applicability]
[0068] The electrode, the electricity storage device, and the method for producing a lithium composite oxide disclosed in this specification can be used in the technical field of secondary batteries. [Explanation of symbols]
[0069] 20 electricity storage device, 21 current collector, 22 positive electrode mixture, 23 positive electrode sheet, 24 current collector, 25 negative electrode mixture, 26 negative electrode sheet, 28 separator, 29 non-aqueous electrolyte, 32 cylindrical case, 34 positive electrode terminal, 36 negative electrode terminal.
Claims
1. An electrode comprising: an active material of a lithium composite oxide containing Li and a metal element other than Li and having a cubic crystal structure; a conductive material; and optionally containing a binder; the electrode has pores, the conductive material content being 20 mass% or less; and when a cross section of the electrode is observed with a SEM and image analyzed, the average non-contact ratio, which is the ratio of the area of the boundary line between the active material and the pores to the area of the outline of the active material, is 8% or less.
2. The lithium composite oxide has the general formula Li a M x O 2-y A y (wherein 0<a<2, 0<x<2, 0≦y<2, M is one or more selected from the group consisting of B, P, Al, Si, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, and Ge, and A is one or more selected from the group consisting of F, Cl, Br, I, and S), and containing P.
3. The electrode according to claim 1 , comprising Mn as the metallic element.
4. 3. The electrode according to claim 1, wherein the energy density per electrode volume is 700 Wh / L or more.
5. The electrode according to claim 1 or 2, wherein the average non-contact rate is 7% or less.
6. 3. The electrode according to claim 1, wherein the conductive material is present in an amount of 15% by mass or less.
7. 3. The electrode according to claim 1, wherein the discharge capacity per mass of the active material is 300 mAh / g or more.
8. The electrode according to claim 1 or 2; an ionically conductive medium in contact with the electrode and conducting lithium ions; The power storage device includes:
9. A lithium composite oxide active material containing Li and metal elements other than Li and having a cubic crystal structure and a bulk density of 0.07 g / cm 3 A method for manufacturing an electrode, comprising: mixing a first conductive material described below; and then blending a second conductive material having a bulk density greater than that of the first conductive material and, if necessary, a binder to prepare an electrode mixture, and then producing an electrode using the electrode mixture.
10. The method for producing an electrode according to claim 9 , wherein the electrode mixture contains the first conductive material and the second conductive material in a total amount of 20 mass % or less.
Citation Information
Patent Citations
Lithium composite oxide
JP2015166291A
Positive electrode active material for lithium secondary batteries and its use
JP2016025009A
Composite oxide, cathode active material for nonaqueous electrolyte secondary battery, cathode for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, method for producing composite oxide and method for producing nonaqueous electrolyte secondary battery
JP2017202954A
High capacity cathode active material
JP2018092958A
Oxides for high-energy cathode materials
JP2019523532A
Cited By
Liquid crystal display apparatus, method of controlling liquid crystal display apparatus, and electronic apparatus
EP4749608A2