Pure titanium wire rod and processing method thereof
A novel method combining MDF, rolling, and heat treatment creates a non-uniform microstructure in pure titanium wires, achieving high strength and low elasticity, addressing the challenges of existing technologies and improving processability and biocompatibility.
Patent Information
- Application Number
- JP2023068848
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing methods for producing pure titanium wires struggle to achieve a balance between high strength and low elasticity (Young's modulus) while maintaining processability and biocompatibility, particularly due to challenges in automating diameter reduction processes and the inability to maintain low Young's modulus after preliminary processing.
A method combining multi-directional forging (MDF) with rolling and specific heat treatment processes to create a non-uniform microstructure in pure titanium wires, featuring fibrous coarse grains with developed sub-grain boundaries and fine crystal grains surrounded by high-angle grain boundaries, along with subsequent grooved roll rolling to achieve the desired properties.
The method results in pure titanium wires with tensile strength exceeding 800 MPa and Young's modulus of 100 GPa or less, enhancing processability and suitability for biomaterial applications by improving ductility and reducing elastic modulus.
Smart Images

Figure 2024154788000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wire made of titanium with a purity of 99% or more (hereinafter referred to as "pure titanium") and a method for processing the same, and in particular to a wire-shaped material made of pure titanium having high strength and a low elastic modulus (low Young's modulus) and a method for processing the same. [Background technology]
[0002] In general, pure titanium has low strength, and therefore titanium alloys have been used to increase the strength of components that require strength. However, titanium alloys have a high elastic modulus (high Young's modulus), so cutting and other processes are not easy, and there have been reports of problems with biocompatibility, so there has been a demand for improving the properties of titanium alloys as medical materials (e.g., dental implants). Therefore, technologies have been reported for achieving high strength for pure titanium, which has better biocompatibility. One such technology is a combination of lateral extrusion (ECAP: Equal-Channel Angular Pressing) and 47% to 75% cold extrusion processing, which can be processed into a rod or wire shape of 1.1 GPa (see Non-Patent Document 1). This technology develops a uniform ultrafine grain structure (average grain boundary is 1 μm or less) and was excellent as an ultra-high strength biomaterial using a large strain processing method, but the elastic modulus (Young's modulus) is not different from that of ordinary pure titanium, and it lacks ductility and jawbone compatibility. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2014 / 038487 [Patent Document 2] JP 2018-069255 A [Non-patent literature]
[0004] [Non-Patent Document 1] VV Stolyarov, YT Zhu, TC Lowe, RZ Valiev, “Microstructure and Properties of Pure Ti Processed by ECAP and Cold Extrusion”, Mater. Sci. Eng. A, Vol.303 (2001) pp.82-89. Summary of the Invention [Problem to be solved by the invention]
[0005] Some of the inventors of this application have developed a massive deformation processing method using a multi-directional forging (MDF) method, and further developed a technology that enables uniform ultra-fine grain structure of pure titanium by combining this MDF method with rolling, and produces pure titanium with a maximum tensile strength of 1 GPa or more, a Young's modulus of 85 GPa or less, and an elongation of 10% or more (see Patent Document 1). With the above technology, it is possible to gradually increase the tensile strength by increasing the rolling ratio; for example, an additional rolling ratio of 65% can increase the Vickers hardness ratio by about 10%, and an additional rolling ratio of 86% can increase the Vickers hardness ratio by about 20%.
[0006] On the other hand, some of the inventors of the present application have developed a technique for processing pure titanium into a small diameter wire (see Patent Document 2). This technique combines the MDF method with wire forming processing to form fine crystal grains and process them into a wire (wire or rod shape). The crystal grains of the obtained pure titanium are long in the longitudinal direction of the wire, and both the major and minor axes have an average grain size of 0.5 μm or less. The maximum tensile strength in this case is 1050 MPa or more.
[0007] To manufacture the above-mentioned pure titanium, the preliminary processing involves a combination of the MDF method and flat roll rolling, and the deformation processing step involves reducing the diameter of pure titanium material maintained at 70°C or below by swaging or drawing.
[0008] The above processing steps are excellent in that they can produce pure titanium wire with at least high strength, but because the crystal grains are refined and high strength is achieved by the MDF method and flat roll rolling in the preliminary processing, swaging or drawing (diameter reduction process) cannot be easily performed. Therefore, it is difficult to automate the manufacturing process, and it is also difficult to shorten the time required for the diameter reduction process. Furthermore, since the purpose of the above pure titanium wire was to produce pure titanium in wire form while maintaining high strength (800 MPa or more), no consideration was given to ease of subsequent processing or a low elastic modulus (low Young's modulus) with an eye toward application to biomaterials. Therefore, the Young's modulus after the preliminary processing (MDF method and flat roll rolling) exceeded 100 GPa, and the Young's modulus of the pure titanium wire produced was about the same. Therefore, it was inevitable that the wire would lack subsequent processability and application to biomaterials.
[0009] The present invention has been made in consideration of the above points, and an object of the present invention is to provide a pure titanium wire having a low elastic modulus (low Young's modulus) while maintaining high strength, and a method for processing the same. [Means for solving the problem]
[0010] Therefore, as a result of intensive research, the inventors of the present application discovered that by combining a type of heat treatment process that utilizes processing heat at an appropriate temperature, coarse grains and ultrafine (sub)crystal grains become non-uniform, and that the above-mentioned non-uniform structure improves the mechanical properties, thereby completing the present invention.
[0011] In other words, the present invention relates to a pure titanium wire rod that exhibits a heterogeneous structure including coarse fibrous grains with developed subgrain boundaries and fine crystal grains or subgrains or a mixture of these with an average grain size of 1 μm or less, and the subgrain boundaries in the structure account for a ratio of 60% or more of all grain boundaries in EBSD measurement.
[0012] According to the above-mentioned configuration, by leaving a region of ultrafine grain structure in which fine crystal grains with an average grain size of 1 μm or less are surrounded by high-angle grain boundaries (grain boundary orientation of 15 degrees or more), a heterogeneous structure is formed as a whole by including fibrous coarse grains while maintaining a moderate strength. Such a structure can improve ductility and reduce the elastic modulus (Young's modulus). In addition, regarding the grain boundary orientation, in EBSD measurement (measurement by electron backscattered diffraction (EBSD): Electron Back Scattered Diffraction method), subgrain boundaries (grain boundary orientation of less than several degrees) account for 40% or more of all grain boundaries, so that a good balance is achieved between strength and ductility (low elastic modulus). In other words, a wire rod with a low elastic modulus (low Young's modulus) can be obtained while maintaining the strength of pure titanium. Although the ratio of subgrain boundaries is set to 60% or more, since the ultrafine grain structure remains, not all grain boundaries are subgrain boundaries (subgrain boundaries do not account for 100%). In other words, in addition to subgrain boundaries, there are also low-angle grain boundaries (with grain boundary orientations of a few degrees to 15 degrees), and if subgrain boundaries and low-angle grain boundaries are included, the proportion is 70% or more, but since 18% or more of high-angle grain boundaries remain, the upper limit of the proportion of subgrain boundaries is approximately 80%.
[0013] In the invention relating to the pure titanium wire rod having the above configuration, the structure can be a texture in which (10-10) columnar planes are accumulated in the longitudinal direction of the rod-like or wire-like rod, and the accumulation degree (development intensity) of the texture can be 9 or more in EBSD measurement.
[0014] According to the above-mentioned configuration, the (10-10) texture (meaning a texture in which (10-10) prismatic planes are accumulated; the same applies below) develops in the longitudinal direction of pure titanium, and the (10-10) prismatic planes of the texture function as slip planes, improving ductility, and since the perpendicular direction to the prismatic planes [10-10] is not the closest-packed direction, this contributes to a decrease in the elastic modulus (Young's modulus). On the other hand, the proportion of (0001) planes decreases relatively, and the longitudinal direction deviates from the closest-packed direction
[0001] , reducing the element of high Young's modulus.
[0015] In the invention of the above configuration relating to the pure titanium wire rod, the high-angle grain boundaries of the structure may have a higher concentration of oxygen segregated than the concentration of oxygen contained in the parent phase. Although the effect of impurity segregation to the grain boundaries of the ultrafine grain structure is related to other metals, some of the inventors of the present application have confirmed and reported that it increases strength (see Mater. Sci. Eng. A, Vol. 833 (2022) pp. 142531. "Age-Hardening Mechanisms of Heterogeneous-Nanostructured SUS316LN Stainless Steel Fabricated by Heavy Cold Rolling"). Therefore, even in pure titanium, the strength can be increased by segregating oxygen as an impurity to the grain boundaries.
[0016] In the invention of the pure titanium wire rod having the above-mentioned configuration, the oxygen concentration segregated at the high-angle grain boundaries of the structure is preferably at least twice the oxygen concentration contained in the parent phase. In pure titanium, impurities segregated at grain boundaries include carbon and nitrogen in addition to oxygen. However, since it is difficult to segregate these impurities other than oxygen at grain boundaries, the strength is increased by increasing the segregation concentration of oxygen as an impurity. The segregation concentration is compared with the concentration in the parent phase, and the effect of the segregation of the impurities can be significantly obtained by segregating with a concentration difference of at least two times. Segregation of oxygen is sufficient if it is at least two times, and it has been confirmed through experiments that a concentration of about three times can be segregated.
[0017] In the invention relating to the pure titanium wire rod having the above configuration, the tensile strength in the longitudinal direction of the rod-like or wire-like material is preferably 800 MPa or more. That is, by adjusting the proportion of high-angle grain boundaries among all grain boundaries in EBSD measurement to 18% or more and the proportion including subgrain boundaries and low-angle grain boundaries to 70% or more (the proportion of subgrain boundaries is 60% or more), the tensile strength in the longitudinal direction can be maintained at 800 MPa or more.
[0018] According to the above-mentioned configuration, the crystal grains are refined by the combined use of the MDF method and flat roll rolling, and the strength of the high-strength pure titanium is maintained, while a pure titanium wire rod having an appropriate low elastic modulus (low Young's modulus) and improved ductility due to the texture can be obtained. This makes it possible to provide pure titanium that can be easily processed as desired for applications requiring strength.
[0019] On the other hand, the invention relates to a method for processing pure titanium wire into a rod or wire shape using pure titanium, which includes a first step and a second step, and the first step includes a multi-axis forging step in which the pure titanium workpiece is forged at least once in each of the three dimensional directions so that the amount of strain per forging in the entire workpiece is within a range of 0.1 to 0.4, and a rolling step in which the workpiece after the multi-axis forging step is rolled by 50% or more using flat roll rolling, and the second step includes at least a diameter reduction step in which the workpiece is heated to 80°C to 500°C using processing heat of 70°C or more and reduced to a cross-sectional reduction rate of 40% or more by swaging.
[0020] According to the above configuration, the structure that has been made fine by the first step is restored by the second step, while fibrous coarse grains with developed subgrain boundaries appear, and a non-uniform structure can be formed. By setting the temperature of the pure titanium (workpiece material) at this time to 80°C to 500°C, it is possible to restore the material without recrystallization. As is well known, swaging is a processing method in which a die (metal mold) is struck at high speed while rotating in the circumferential direction to reduce the diameter, and generates relatively high processing heat. By utilizing this available heat, the material temperature can be increased, and the diameter can be reduced while the structure is restored. At this time, since the processing heat varies depending on the diameter of the workpiece material, it is difficult to set the material temperature uniformly, but by setting the temperature within a range that does not lead to recrystallization (500°C and 30 minutes), it is possible to contribute to recovery. In addition, since it is preferable that the workpiece material is softened to facilitate processing in the diameter reduction step, the temperature is preferably 150°C or higher, and more preferably 300°C or higher. Since the processing time was shortened even at temperatures above 150°C, it is assumed that softening occurred, and significant softening was confirmed at 300°C. Diameter reduction processing is possible even at low temperatures below 80°C, but in order to produce fibrous coarse grains with developed subgrain boundaries, a temperature of 80°C or higher is required. The proportion of fibrous coarse grains that appear changes depending on the temperature, and as the temperature increases, subgrain boundaries are more likely to appear and the proportion of developed fibrous coarse grains increases. In the low temperature range, subgrain boundaries appear locally, so the proportion of all grain boundaries decreases, approaching the lower limit of 40%.
[0021] In the invention having the above-mentioned configuration relating to the processing method, it is preferable that the multi-axis forging step and the rolling step are both warm or cold processing at a temperature of 300° C. or less at which the material to be processed does not recrystallize.
[0022] In the case of the above-mentioned configuration, in the multi-axis forging process (when processing by MDF) and the rolling process (when rolling by flat rolls), an ultra-fine grain structure in which fine crystal grains with an average grain size of 1 μm or less are surrounded by high-angle grain boundaries can be produced, and high-strength pure titanium can be obtained, and the strength that is reduced by the process of improving the low elastic modulus (low Young's modulus) in the subsequent process can be compensated for. In other words, if recrystallization occurs during MDF processing or flat roll rolling, the proportion of the structure in which fine crystal grains are surrounded by high-angle grain boundaries decreases, making it difficult to increase the strength again in the subsequent process, so the temperature range in the first process where recrystallization does not occur (300°C or less) is required. At 300°C, there is a temperature range up to the temperature at which recrystallization occurs (500°C), but since it has been experimentally found that recovery and softening occur even at 300°C, 300°C is set as the upper limit. Naturally, when processing is performed while maintaining a low temperature (room temperature), the crystal grains become finer and the proportion of structures in which fine crystal grains are surrounded by high-angle grain boundaries increases, which is more favorable in terms of strength.
[0023] Furthermore, in the invention related to the processing method having the above-mentioned configuration, a heat treatment step of annealing at 300° C. to 500° C. can be included between the multi-axis forging step and the rolling step.
[0024] According to the above-mentioned configuration, the microstructure is not recrystallized but is restored, thereby reducing the internal energy, which reduces the occurrence of defects (cracks, etc.) when the cross-sectional area is changed in the subsequent process (diameter reduction process).
[0025] In addition, in the invention of each of the above configurations relating to the processing method, the second step can include a grooved roll rolling step in which grooved rolls are used to perform grooved roll rolling with a cross-sectional reduction rate of 20% or more.
[0026] Rolling using grooved rolls differs from swaging in that it allows for cold processing rather than processing at high temperatures caused by processing heat. As a result, it is possible to promote diameter reduction without reducing the strength of the pure titanium, which was strengthened in the first process by refining the structure, and while maintaining the low elastic modulus (low Young's modulus) achieved by swaging.
[0027] In the invention having the above-mentioned configuration relating to the processing method, the grooved roll rolling step can be performed either before or after the diameter reducing step, or both.
[0028] In the above configuration, grooved rolling is adopted to change the cross-sectional area (or cross-sectional shape) without significantly affecting the strength and elastic modulus, and it is possible to finish high-strength, low-elastic modulus (low Young's modulus) pure titanium into a desired diameter or shape. In particular, by carrying out grooved rolling after the diameter reduction process by swaging, it becomes easy to finish into a desired shape.
[0029] Furthermore, in the invention of each of the above configurations related to the processing method, the groove roll rolling process is at least carried out after the diameter reduction process, and the groove roll rolling process can include a cross-sectional flattening process for making the groove roll shape an ellipse, followed by a cross-sectional restoration process for making the groove roll shape a circle.
[0030] According to the above configuration, when a grooved roll is used to process a pure titanium wire rod into a round bar shape, radial compression can be repeated, and the strength of the pure titanium can be improved by the same logic as in a type of MDF. These flattening and restoration processes can be performed not only to reduce the diameter, but also to promote a decrease in the elastic modulus (Young's modulus) by applying a radial strain to the wire rod, accumulating the bottom faces ((0001) faces) of the crystal grains in the surface direction (ND direction) of the wire rod and accumulating the (10-10) prism faces in the longitudinal direction (RD direction). Effect of the Invention
[0031] According to the present invention relating to the pure titanium wire, a heterogeneous structure is formed with fibrous coarse grains (developed subgrain boundaries) and fine crystal grains (which may be subgrains surrounded by subgrain boundaries), and the subgrain boundaries account for 40% or more of the total grain boundaries (according to EBSD measurement), so that the proportion of the structure in which fine crystal grains are surrounded by high-angle grain boundaries can be kept small, resulting in a low modulus of elasticity (low Young's modulus).As a result, the workability when using the pure titanium wire of the present invention and its applicability to biomaterials are improved.
[0032] On the other hand, according to the present invention relating to the processing method of pure titanium wire, pure titanium wire with low elastic modulus (low Young's modulus) can be easily processed while maintaining sufficient strength. That is, when reducing the diameter of pure titanium to an appropriate diameter, the processing heat during swaging is utilized, and processing is performed in an appropriate temperature range, thereby making it possible to perform a diameter reduction process accompanied by recovery and softening. In addition, by combining this with grooved roll rolling, it becomes possible to deform the wire to a desired diameter and shape. When swaging is performed before grooved roll rolling, the material that has already been recovered and softened is deformed, so that it is also possible to easily change the diameter and shape by the grooved roll rolling. [Brief description of the drawings]
[0033] [Figure 1] FIG. 1 is an explanatory diagram showing an outline of a procedure according to an embodiment of a method for processing a pure titanium wire. [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a processing method in a grooved roll rolling process. [Diagram 3] 1A is a TEM image showing a first embodiment of the pure titanium wire, and FIG. 1B is a TEM image of a comparative example. [Figure 4] FIG. 2A is an EBSD measurement map of a pure titanium wire according to a first embodiment of the present invention, and FIG. 2B is a graph showing the distribution of (sub)grain size and the misorientation distribution of (sub)grain boundaries in the structure of FIG. 2A. [Diagram 5] (a) is an EBSD measurement map of a comparative example, and (b) is a graph showing the distribution of (sub)grain size and the misorientation distribution of (sub)grain boundaries in the structure of (a). [Figure 6] 1 is a photograph of a processed product made of pure titanium produced in Experimental Example 1. [Figure 7] 1 is a graph of a stress-strain curve showing the results of a tensile test according to Experimental Example 2. [Figure 8] 1 is a graph showing the results of three-dimensional atom probe analysis of high-angle grain boundaries in a manufactured pure titanium wire. [Figure 9] 13 is a graph showing the measurement results of a dynamic microhardness meter according to Experimental Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. For convenience of explanation, an embodiment of a processing method will be described first, followed by an embodiment of a pure titanium wire rod.
[0035] <Embodiments Related to Processing Method> Fig. 1 shows an outline of the procedure for the processing method of pure titanium wire. As shown in this figure, the processing method of this embodiment is divided into a first step and a second step. The first step is a processing step mainly for improving strength, and the second step is a processing step mainly for forming pure titanium into a wire and at the same time reducing the elastic modulus (Young's modulus).
[0036] Here, the first step is a multi-axis forging step using a multi-axis forging (MDF) method and a rolling step using flat roll rolling, which are carried out in sequence. The multi-axis forging step involves forging the material to be processed (pure titanium ingot with a purity of 99% or more) at least once in each of the three dimensional directions (a total of three times: one pass is one pass with one pass in each of the three dimensional directions (a total of three times)), with the amount of strain in the entire material to be processed per pass being within the range of 0.1 to 0.4. The strain rate is 1×10 -3The range of the forging speed is from 1 / sec to 10 / sec. By repeating the above, the total strain amount applied can be from 1.2 (for example, 0.2×2 passes (i.e., 0.2 forging twice in each of the three directions)) to 7.2 (for example, 0.2×12 passes). The amount of strain per pass and the number of passes can be changed as appropriate, and the above-mentioned exemplary amounts of strain and number of passes can be increased or decreased. Note that by multi-axis forging with a total strain amount of about 2.4, it is possible to realize an appropriate refinement of the crystal grains.
[0037] The rolling process using flat rolls applies massive strain to the material being worked, which also promotes the refinement of crystal grains. The rolling reduction is 50% or more, and the material is rolled in multiple passes, resulting in a total rolling reduction of 50% or more. This massive strain processing refines the crystal grains, but at the same time, high-angle grain boundaries also appear. The strength of pure titanium is achieved by the refinement of these crystal grains and the appearance of high-angle grain boundaries.
[0038] The multi-axis forging process and rolling process described above are both performed at a temperature of 300°C or less, at which the material to be processed does not recrystallize, and are performed in a warm or cold state. In the case of processing in a high temperature environment, such as 500°C, which exceeds 300°C, recrystallization occurs as described below, and the fine crystal grains may become coarse due to recrystallization, resulting in a decrease in strength. The upper limit is set at 300°C because the material to be processed is not significantly softened, and even if the temperature is within the range of 150°C to 300°C, recrystallization of the crystal structure does not occur for a short period of time, and only recovery can be used for property control. In order to suitably perform grain refinement, cold rolling is preferable.
[0039] The central step in the second step is the diameter reduction step. The material used in the diameter reduction process is the plate-shaped pure titanium rolled in the first step, cut into rod-shaped material of an appropriate size. For this reason, a cutting step is carried out between the first and second steps. As will be described in detail later, in the second step, a grooved roll rolling step is carried out as a pre-step to the diameter reduction step, in order to make the material into a round bar shape for use in swaging (diameter reduction step).
[0040] The diameter reduction process is a process for reducing the diameter of the material to be processed by swaging at a high temperature range of 80°C to 500°C to a cross-sectional reduction rate of 40% or more. Heating of the material to be processed is done mainly by using the processing heat (70°C or more) generated by swaging. Since processing is done at a specified temperature, the die of the swaging machine or the material to be processed may be heated directly in the initial stage, but when the material to be processed starts to be struck (the die striking the material to be processed), the temperature of the material to be processed rises and processing heat of 70°C or more is generated. By conserving this processing heat rather than eliminating it by cooling or the like, the temperature of the material to be processed rises to a range exceeding 80°C. However, the temperature of the material to be processed that rises is adjusted so as to be kept within a range not exceeding 500°C (the temperature at which the material recrystallizes).
[0041] If the temperature in the diameter reduction step by swaging is 150°C or higher, preferably 300°C or higher, the material to be processed (pure titanium) will soften, making diameter reduction by swaging easier. Also, by carrying out swaging at a temperature range of 150°C or higher, it is possible to improve the structure of the high-angle grain boundaries that have been refined and formed in the first step. That is, in addition to fine crystal grains, subgrains, or a mixture of these, fibrous coarse grains with developed subgrains can appear. These become non-uniform, and the ratio of subgrains can be developed at a desired ratio.
[0042] The second step may be completed by the above-mentioned swaging, but if the pure titanium is to be made into a wire of a desired shape and finished to a desired size (cross-sectional area), a grooved roll rolling step may be carried out again as a finishing step. In particular, because swaging processes the wire into a circular cross-section (round bar or cylinder) due to its processing method, if a wire is to be finished into a polygonal cross-section, it is required to use a grooved roll with a polygonal groove cross-section.
[0043] In the above-mentioned processing procedure, annealing may be performed between the first and second steps by heating the workpiece to 500°C or less. This is because the workpiece should be subjected to diameter reduction processing at a high temperature range of 150°C or more (preferably 300°C or more) by utilizing the processing heat generated by swaging. However, when the workpiece is not expected to be heated by the processing heat, the workpiece is pre-annealed for a short time at a temperature below the recrystallization temperature (500°C) in advance, so that the workpiece can be restored without recrystallization and the internal energy can be reduced. This annealing can suppress the occurrence of defects (cracks, etc.) when the cross-sectional area changes during the diameter reduction process, etc. When the temperature of the workpiece during swaging is 300°C or more, the internal energy can be reduced at the same time as the above-mentioned structure is improved.
[0044] In addition, the inventors of the present application have found that when annealing is performed at or below the recrystallization temperature and for a short annealing time, the material is hardened (strengthened) in the Vickers hardness measurement. For this reason, in the case of pure titanium only, if the annealing temperature is 500°C or less, the material is hardened (strengthened) for an annealing time of 100 to 5000 seconds, so that annealing can be performed to increase strength without changing the crystal structure. Annealing for this purpose may be additionally performed after the completion of all processing (second process) in order to impart strength (hardness).
[0045] In addition, when the grooved roll rolling process is performed before and after swaging, these grooved roll rolling processes are different from each other. That is, the grooved roll rolling process before swaging (pre-rolling process) is for enabling processing by swaging, and is intended to make the cross-sectional shape circular. Therefore, the area reduction rate is hardly taken into consideration. Therefore, if the cross-sectional shape can be processed into a circular shape by cutting, it can be omitted. On the other hand, the grooved roll rolling process after swaging (post-rolling process) is intended to finish the wire into a desired shape and size, so it is processed with an area reduction rate in order to adjust the wire into a desired diameter. In the case of the grooved roll rolling process (post-rolling process), grooved roll rolling with an area reduction rate of 20% or more is performed, and if the diameter of the finished wire is smaller than the diameter of the wire rod after swaging, the area reduction rate may exceed 80%. In addition, if the pre-rolling process is also performed and a moderate area reduction is involved during the pre-rolling process, the total area reduction rate in both grooved roll rolling processes is adjusted to be 20% or more. The purpose of setting the cross-sectional reduction rate to 20% or more in the grooved roll rolling process is to accumulate the bottom faces ((0001) faces) of the crystal grains in the surface direction (ND direction) of the wire rod and accumulate the (10-10) columnar faces in the longitudinal direction (RD direction), as described later.
[0046] In addition, when the final wire shape is other than a circular cross section, the groove shape of the groove roll is processed to match the desired shape, and the area reduction ratio is also taken into consideration in order to adjust the diameter at the same time. In addition, when the wire has a circular cross section and the diameter after swaging does not need to be changed, the groove rolling step as a post-rolling step can be omitted, but even in this case, as described later, there are cases where the groove rolling step as a post-rolling step is performed.
[0047] FIG. 2 illustrates an example of the grooved roll rolling process as a post-rolling process during processing of a wire rod with a circular cross section. In this grooved roll rolling process, pressure is applied to the initial circular material A in a biased direction (see (a-1) and (a-2) in FIG. 2) to form a flat material B with an elliptical cross section (see (b-1) and (b-2) in FIG. 2). This is the cross section flattening process. After that, pressure is applied to the flat material B in a direction rotated 90 degrees in the circumferential direction (see (c-1) and (c-2) in FIG. 2), and the cross section is restored to a circular shape to form a circular material C (see (d-1) and (d-2) in FIG. 2). This is the cross section restoration process. The grooved roll rolling using the circular groove and the elliptical groove has the advantage of effectively suppressing surface cracks at the corners that occur during normal grooved roll rolling using a diamond-shaped groove.
[0048] Both of these cross-section flattening process and cross-section restoring process are performed by rolling with grooved rolls. In the cross-section flattening process, the groove shape of the grooved roll is made elliptical (only one side is semi-elliptical, and both grooves together form an elliptical shape), the pressure of the roll is concentrated in one direction (X direction in the figure), and the roll is processed so as to bulge in the perpendicular direction (Y direction in the figure). On the other hand, in the cross-section restoring process, the groove shape of the grooved roll is made circular (only one side is semi-circular, and both grooves together form a circle), and the pressure is concentrated in the bulged direction (Y direction in the figure) by the cross-section flattening process, thereby restoring the circular cross section. Since both of these processes are a pair, they may be repeated two or more times. When repeated multiple times, the direction of pressure concentration by the cross-section flattening process from the second time onwards may be a different direction from the first time (for example, halfway between the X direction and the Y direction in the figure).
[0049] Both of these flattening and restoration processes may be performed with the aim of reducing the cross-sectional area in order to reduce the diameter, but even if there is no need to reduce the cross-sectional area, both processes may be performed while maintaining the same diameter. That is, the process is performed with the aim of accumulating the bottom faces ((0001) faces) of the crystal grains in the surface direction (ND direction) of the wire rod and accumulating the (10-10) prism faces in the longitudinal direction (RD direction) of the wire rod by applying a strain in the radial direction to the wire rod. This change in the orientation of the crystal grains can promote a decrease in the elastic modulus (Young's modulus). In addition, the above-mentioned processing method can change the crystal orientation even in a wire rod with a polygonal cross section by applying pressure in two orthogonal directions, so that the flattening process and restoration process may be performed as post-rolling processes for polygonal wire rods after the grooved roll rolling process to form the desired shape. Furthermore, in cases where the desired ductility can be obtained by reducing the elastic modulus (Young's modulus) solely through the accumulation of such crystal grain faces, it may be possible to consider using only the grooved roll rolling process and omitting swaging, and it may also be possible to consider introducing a short-term heat treatment in place of the heat treatment during swaging.
[0050] <First embodiment of pure titanium wire rod> A first embodiment of the present invention relating to a pure titanium wire rod will be described with reference to Fig. 3. Fig. 3(a) is a TEM image in the RD direction (longitudinal direction) of a wire rod that has been subjected to only swaging after the above-mentioned first step (MDF and flat roll rolling), and Fig. 3(b) is a TEM image in the RD direction of a wire rod that has been subjected to only grooved roll rolling after the first step for comparison.
[0051] As shown in the TEM image in FIG. 3(a), this embodiment presents a non-uniform structure of fibrous coarse grains and fine crystal grains. The total processing rate (ratio of area reduction after area reduction to area reduction before area reduction) of both swaging (FIG. 3(a)) and grooved roll rolling (FIG. 3(b)) is the same, that is, 5.1%. Comparing the two structures, both have fine structures developed. However, when comparing the bright field image and the selected area diffraction image, the diffraction spot that was arc-shaped in grooved roll rolling (FIG. 3(b)) can be confirmed as a clear diffraction spot in swaging (FIG. 3(a)), and at the same time, the developed substructure also approaches equiaxed. In addition, the black and white contrast in the grains caused by processing strain has almost disappeared in swaging (FIG. 3(a)).
[0052] In particular, the characteristic of the swaging shown in Fig. 3(a) is that, even though it is observed from the longitudinal direction (RD), the (sub)grain structure is connected to form a long and thin band-like structure (fibrous coarse grains). Generally, when a wire is processed into a rod (wire) by a large cross-sectional reduction, the structure in the longitudinal direction (RD) of the wire is considered to be an equiaxed granular structure, but in Fig. 3(a), it is completely different from such a structure. The formation of such a structure makes it possible to reduce the elastic modulus (Young's modulus), as shown in the experimental results described later.
[0053] <Second embodiment of pure titanium wire rod> A second embodiment of the present invention relating to a pure titanium wire rod will be described with reference to FIG. 4. FIG. 4(a) shows a map obtained by EBSD measurement, and FIG. 4(b) shows the distribution of (sub)grain size and the orientation difference distribution of (sub)grain boundaries in the structure of (a). However, this embodiment is a wire rod obtained by performing flat roll rolling (area reduction rate of 68%) after MDF (total strain amount of 2.4) (first step), then performing grooved roll rolling (area reduction rate of 25%) as a pre-rolling step, swaging (area reduction rate of 40%), and then performing grooved roll rolling (area reduction rate of 80%) as a post-rolling step (second step). The total area reduction rate of the above steps was set to 97%.
[0054] For comparison with the above, a wire rod was obtained without swaging and only grooved roll rolling (area reduction rate: 91%) was used as the second process, resulting in a total area reduction rate of 97%. As in Fig. 4, Fig. 5(a) shows a map obtained by EBSD measurement, and Fig. 5(b) shows the distribution of (sub)grain grain size and the misorientation distribution of (sub)grain boundaries.
[0055] Comparing Figures 4(a) and 5(a), there is no significant difference in the structure of the longitudinal cross section (RD surface) along the length of the wire, but the cross section (ND surface) has a significantly increased area that can be analyzed by EBSD measurement due to the effect of recovery by swaging, and it is clear that there is a mixture of fibrous coarse grains extending in the length direction and fine granular structure. This is also clear from the difference in the average grain size on the "ND surface" shown in the figure, which is 0.38 μm (Figure 4(a)) and 0.30 μm (Figure 5(a)). Note that the figure is a little difficult to understand because it was converted from a color map to black and white, but the above can be confirmed by looking at the white parts.
[0056] This indicates that the bottom faces ((0001) planes) of the crystal grains are accumulated in the surface (radial) direction (ND direction) of the wire, and the (10-10) planes are strongly accumulated in the longitudinal direction (RD direction).
[0057] In addition, when comparing FIG. 4(b) and FIG. 5(b), the (sub)crystal grain distributions (both graphs on the left) show a wide distribution of 0.02 μm to 1 μm. However, when comparing the distribution of (sub)grain boundary orientation differences (both graphs on the right), the subgrain boundaries (indicated as "SGB" in the figure) are 48% in FIG. 5(b) and 63% (60% or more) in FIG. 4(b). Even when low-angle grain boundaries (indicated as "LAGB" in the figure) are included, the one is 61%, while the present embodiment is 82% (70% or more). Furthermore, the high-angle grain boundaries (indicated as "HAGB" in the figure) are only 18% in the present embodiment. In addition, the average grain boundary orientations tend to be low-angle, at 10 degrees (less than 20 degrees), in the present embodiment. This is less than half the average orientation of the comparative example, which is 21 degrees.
[0058] This is clearly different from the state that is said to be formed mainly by high-angle grain boundaries in the definition of an ultrafine-grained structure, and is also clearly different from conventional structures that have been able to achieve high strength (Patent Documents 1 and 2). EXAMPLES
[0059] <Experimental Example 1> Pure titanium wires were produced under various conditions. Figure 6 is a photograph of the produced pure titanium wires. Of the pure titanium wires shown in Figure 6, from the top, there is one processed by MDF (total strain 3.6) and then grooved roll rolling (area reduction rate 90%) to produce a wire, one processed by MDF (total strain 3.6) followed by flat roll rolling (area reduction rate 90%), one processed by MDF (total strain 2.4) followed by flat roll rolling (area reduction rate 68%) and grooved roll rolling (area reduction rate 91%) to produce a wire (total area reduction rate 97%), and the last one at the bottom is one processed by MDF (total strain 2.4) followed by flat roll rolling (area reduction rate 68%) and then swaging (area reduction rate 40%) followed by grooved roll rolling (area reduction rate 80%) to produce a wire (total area reduction rate 97%).
[0060] In the above manufacturing process, the grooved roll rolling adopted a method of repeating the cross-section flattening process and the cross-section restoration process. In addition, when MDF with an initial total strain of 3.6 was adopted and flat roll rolling with a cross-section reduction rate of 90% was performed, end cracks occurred (second row from the top of Fig. 6) and the yield was poor, so the total strain by MDF was set to 2.4 and the cross-section reduction rate by flat roll rolling was set to 68%. Even in this case, when a wire rod was manufactured with a cross-section reduction rate of 91% by grooved roll rolling, it became in a state where cracks were likely to occur, as shown in the third row from the top of Fig. 6. Therefore, by performing swaging (processing at a high temperature range (150 °C) using processing heat), it was possible to manufacture a suitable wire rod (bottom row of Fig. 6). From this, it is judged that the effect of recovery was obtained by processing in a high temperature range using the processing heat during swaging. It is presumed that the same result can be obtained when annealing is performed at 300 °C or less, which is a level at which recrystallization does not occur.
[0061] <Experimental Example 2> Next, tensile tests were conducted on the pure titanium wires produced under various conditions. The results (stress-strain curves) are shown in Figure 7. In the figure, "MDF2.4" indicates processing with a total strain of 2.4 using MDF, "flat 68%" indicates rolling processing with a cross-sectional reduction rate of 68% using flat roll rolling, "SW68%" indicates processing with a cross-sectional reduction rate of 68% using swaging, and "groove 44%" indicates processing with a cross-sectional reduction rate of 44% using groove roll rolling. Each number indicates the total strain or cross-sectional reduction rate during processing, so when the individual numbers are different, it indicates that processing was performed according to the content of that number. The order of each processing is indicated by connecting them with "+". The same notation method will be adopted below.
[0062] As shown in Experimental Example 1, when MDF with a total strain of 3.6 was used and flat roll rolling with a cross-sectional reduction rate of 90% was performed, edge cracks occurred. In consideration of this, the total strain by MDF was set to 2.4 and the cross-sectional reduction rate by flat roll rolling was set to 68%. In addition, the grooved roll rolling was performed by repeating a cross-sectional flattening process and a cross-sectional restoration process.
[0063] As a result, as shown in FIG. 7, in the case of MDF2.4+flat 68%, the strength exceeded 800 MPa and the ductility exceeded 15%. This is the same as the content described in the above-mentioned Patent Document 1. Next, in the case of MDF2.4+flat 68%+SW68% (total area reduction rate 90%), the strength did not increase, but the stress drop after the peak stress became slightly gentler, and the local shrinkage became smaller. This is thought to be due to recovery by swaging in the high temperature range (150°C or higher). In contrast, when SW was replaced with groove 68% (MDF2.4+flat 68%+groove 68%), a tensile strength of about 1 GPa was achieved. This is the same as the content described in the above-mentioned Patent Document 2.
[0064] Next, in the case of MDF2.4 + flat 68% + SW44% + groove 44% (total area reduction rate 90%), a tensile strength slightly below 1 GPa (almost 1 GPa) was obtained and ductility was restored.
[0065] In addition, when MDF2.4+flat 68%+groove 91% (total area reduction rate 97%) was used, the tensile strength was 1.1GPa and the elongation was 12%, but cracks occurred during processing (see Experimental Example 1), resulting in poor yield. In contrast, in the case of MDF2.4+flat 68%+groove 25%+SW40%+groove 80% (total area reduction rate 97%), the tensile strength was 1.15GPa and excellent wire rod with no decrease in ductility was obtained.
[0066] In addition, in the results of the above tensile test, the tensile strength in the case of MDF2.4+flat 68%+groove 25%+SW40%+groove 80% (total area reduction rate 97%) was 1.15GPa, which is greater than the materials under other conditions. This is because impurities (oxygen) segregated at the high angle grain boundaries due to the grooved roll rolling with a large area reduction rate (80%) after heating during swaging (processing in a high temperature range at a temperature where recrystallization does not occur). As mentioned above, when impurities are segregated at the grain boundaries, the strength increases, so it is judged that this is due to the segregation of oxygen at a higher concentration than the concentration of oxygen contained in the parent phase.
[0067] To confirm the above, the elements segregated at the grain boundaries were analyzed using a 3D atom probe for a material processed with MDF2.4 + flat 68% + SW40% + groove 80% (total area reduction rate 97%). The results are shown in Figure 8.
[0068] According to the above results, the oxygen concentration as an impurity is segregated at a higher concentration than the oxygen concentration in the parent phase. The material used for the measurement was processed under the above-mentioned conditions, and the ratio of the segregated oxygen concentration is about three times that of the oxygen concentration in the parent phase. Considering this together with the results of the tensile test described above, the tensile strength was 800 MPa with only swaging (MDF2.4 + flat 68% + SW68%) and about 1 GPa with only grooved roll rolling (MDF2.4 + flat 68% + groove 68%), while it reached about 1 GPa when grooved roll rolling was performed slightly after swaging (MDF2.4 + flat 68% + SW44% + groove 44%), and it can be understood that this is also due to oxygen segregation at the grain boundaries. In this case, the segregation concentration ratio of oxygen (ratio of concentration in the parent phase to concentration at the grain boundaries) is estimated to be about twice. From these considerations, it was found that in the case of pure titanium, if the segregation concentration ratio of oxygen at the grain boundaries is twice or more, the strength can be increased. It has also been found that such a state can be obtained by carrying out grooved roll rolling after swaging in a high temperature range utilizing processing heat.
[0069] <Experimental Example 3> Finally, we conducted experiments to examine the degree of decrease in Young's modulus when swaging was performed using processing heat and when rolling was performed using grooved rolls that repeat the cross-section flattening and cross-section restoration processes. In other words, we confirmed the tendency for Young's modulus (elastic modulus) to decrease due to the improvement of the structure by swaging in the high temperature range using processing heat, and the tendency for Young's modulus (elastic modulus) to decrease due to changes in the accumulation of crystal planes caused by repeating flattening and restoration.
[0070] Young's modulus was measured by a dynamic microhardness tester, and the results of measurements under different processing conditions are shown in Figure 9. The materials used were hot forged material as the "initial material," which had a total strain of 3.6 set by MDF (denoted as "MDF3.6"), the initial material was flat-rolled to a cross-sectional reduction of 68% after a total strain of 2.4 set by MDF (denoted as 1 in a circle, hereafter referred to as "rolled material 1"), the material "○1" was swaged (high temperature range) to a cross-sectional reduction of 68% (denoted as 2 in a circle, hereafter referred to as "rolled material 2"), and the material "○1" was grooved-rolled (repeated flattening and restoration) to a cross-sectional reduction of 68% (denoted as 3 in a circle, hereafter referred to as "rolled material 3"). For materials that had been rolled, the Young's modulus was measured in the rolling direction (longitudinal direction (RD)), and only for the "○3" items, the Young's modulus was also measured in the surface (radial) direction (ND) to confirm.
[0071] From the results in Fig. 9, a decrease in Young's modulus was expected for the MDF3.6 material because the ductility improves as described in the above-mentioned Patent Document 1. In addition, the Young's modulus of the rolled material 1, which was subjected to additional flat roll rolling, increases because the aim of the material was to increase strength as described in the above-mentioned Patent Document 2.
[0072] In contrast to this Rolled Material 1, Rolled Material 2 and Rolled Material 3 both had a Young's modulus of 100 GPa or less, which was lower than the Young's modulus of Rolled Material 1. These values are lower than the Young's modulus of general pure titanium (105 GPa to 115 GPa). Looking at them individually, the Young's modulus for Rolled Material 2 was 98 GPa, and for Rolled Material 3 it was 82 GPa, and in the case of Rolled Material 3 it was possible to obtain a result in which the Young's modulus was lower than that of the MDF3.6 material.
[0073] As mentioned above, these are believed to be due to the effect of recovery accompanying the rise in temperature during swaging (rolled material 2), as well as changes in the crystal planes caused by the repeated flattening and restoration during grooved roll rolling (rolled material 3). Therefore, it was found that a low elastic modulus (low Young's modulus) can be achieved by recovering the structure through swaging in a moderate temperature range, and it was also found that an even lower elastic modulus (low Young's modulus) can be achieved by suppressing the occurrence of cracks and the like and by expressing a unique accumulation of crystal planes during grooved roll rolling after the structure has been recovered.
[0074] Furthermore, since the Young's modulus in the surface (radial) direction (ND direction) of the rolled material 3 exceeds 100 GPa, it was also found that the specific accumulation of the above-mentioned crystal planes makes it possible to reduce the elastic modulus (Young's modulus) in a specific direction (longitudinal direction). [Explanation of symbols]
[0075] A Initial circular material B Flat material C. Restoration materials
Claims
1. A rod-shaped or wire-shaped pure titanium wire made of pure titanium with a purity of 99% or more, The steel has a heterogeneous structure including fibrous coarse grains with developed subgrain boundaries, and fine crystal grains or subgrains or a mixture of these grains with an average grain size of 1 μm or less, The sub-boundaries in the structure are those that show a ratio of 60% or more of all grain boundaries in EBSD measurement.
1. A pure titanium wire material characterized by:
2. 2. The pure titanium wire according to claim 1, wherein the structure is a texture in which (10-10) cylindrical planes are accumulated in the longitudinal direction of the rod-like or wire-like shape, and an accumulation intensity of the texture is 9 or more in EBSD measurement.
3. 2. The pure titanium wire rod according to claim 1, wherein oxygen is segregated at the high-angle grain boundaries of the structure at a concentration higher than the concentration of oxygen contained in the matrix.
4. 4. The pure titanium wire rod according to claim 3, wherein the concentration of oxygen segregated at the high-angle grain boundaries of the structure is at least twice the concentration of oxygen contained in the matrix.
5. 5. The pure titanium wire according to claim 1, wherein the rod-like or wire-like material has a tensile strength in the longitudinal direction of 800 MPa or more.
6. A method for processing pure titanium wire into a rod or wire shape using pure titanium with a purity of 99% or more, comprising the steps of: The method includes a first step and a second step, The first step includes a multi-axis forging step in which a workpiece made of pure titanium is forged once or more in each of the three-dimensional directions, so that the amount of strain per forging in the entire workpiece is within a range of 0.1 to 0.4, and a rolling step in which the workpiece after the multi-axis forging step is rolled by 50% or more by flat roll rolling. The second step includes at least a diameter reduction step of reducing the diameter of the processed material to a cross-sectional reduction rate of 40% or more by swaging while heating the processed material to a temperature of 80°C to 500°C using processing heat of 70°C or more. A method for processing pure titanium wire, comprising the steps of:
7. 7. The method for processing a pure titanium wire rod according to claim 6, wherein the multi-axis forging step and the rolling step are both warm or cold processing at a temperature of 300° C. or less at which the material to be processed does not undergo recrystallization.
8. 7. The method for processing a pure titanium wire according to claim 6, further comprising a heat treatment step of annealing at 300° C. to 500° C. between the multi-axis forging step and the rolling step.
9. The method for processing a pure titanium wire rod according to any one of claims 6 to 8, wherein the second step includes a grooved roll rolling step of performing grooved roll rolling using grooved rolls to achieve a cross-sectional reduction rate of 20% or more.
10. 10. The method for processing a pure titanium wire rod according to claim 9, wherein the grooved roll rolling step is performed either before or after the diameter reducing step, or both.
11. 10. The processing method for a pure titanium wire rod according to claim 9, wherein the grooved roll rolling step is at least performed after the diameter reducing step, and the grooved roll rolling step includes a cross-section flattening step of making the grooved roll shape an ellipse, followed by a cross-section restoring step of making the grooved roll shape a circle.
12. A method for processing pure titanium wire into a rod or wire shape using pure titanium with a purity of 99% or more, comprising the steps of: The method includes a first step and a second step, The first step includes a multi-axis forging step in which a workpiece made of pure titanium is forged once or more in each of the three-dimensional directions, so that the amount of strain per forging in the entire workpiece is within a range of 0.1 to 0.4, and a rolling step in which the workpiece after the multi-axis forging step is rolled by 50% or more by flat roll rolling. The second step includes a diameter reduction step by rolling with a grooved roll, and the diameter reduction step includes a cross-sectional flattening step for making the grooved roll shape an ellipse, followed by a cross-sectional restoration step for making the grooved roll shape a circle. A method for processing pure titanium wire, comprising the steps of:
Citation Information
Patent Citations
Pure titanium metal wire and processing method thereof
JP2018069255A
Member-manufacturing process and biomaterial
WO2014038487A1