Rare earth sinter magnet and manufacturing method of them

By optimizing the composition and structure of R-T-B rare earth sintered magnets with specific phases and controlled sintering, the magnets exhibit improved high-temperature magnetic properties and reduced manufacturing time, addressing efficiency and environmental concerns.

JP2024154865APending Publication Date: 2024-10-31SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023069056
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing R-T-B rare earth sintered magnets face challenges in maintaining high-temperature magnetic properties due to prolonged sintering times, leading to increased power consumption, manufacturing costs, and environmental impact, while conventional methods fail to improve squareness and coercive force effectively.

Method used

Optimizing the composition and structure of R-T-B rare earth sintered magnets by incorporating specific phases (R2T14B, R6(T,M1)14, and R-rich 2(T,M1)17 phases, with controlled sintering conditions to achieve two magnetization bending points and improved heat resistance, while reducing sintering time and power consumption.

Benefits of technology

The solution results in a rare earth sintered magnet with excellent magnetic properties in high-temperature environments, maintaining high productivity and reducing manufacturing costs without compromising magnetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154865000001_ABST
    Figure 2024154865000001_ABST
Patent Text Reader

Abstract

SOLUTION: To provide a rare earth sinter magnet which contains R which is two or more rare earth elements and essentially contains Nd and Pr of 12.5 atom% to 16.0 atom%, B of 4.5 atom% to 5.3 atom%, M1 which is one or more kinds selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi of 0.5 atom% to 2.5 atom%, M2 which is one or more kinds selected from Ti, V, Zr, Nb, Hf, and Ta of 0.05 to 0.5 atom%, and a residual part T which is one or more kinds of Fe and Co, also contains a R2T14B phase as a main phase, and a R2(T and M1)17 phase coated by a R6(T and M1)14 phase and a R rich phase of more than 0 and 10% or less by an area fraction, and in which two magnetized bending points of a first knick point on a low magnetic field side and a second knick point on a high magnetic field side exist in a magnetic polarization curve second quadrant at 23°C.EFFECT: A rare earth sinter magnet having an excellent magnetic characteristic under a high temperature environment can be obtained with high productivity.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rare earth sintered magnet having excellent magnetic properties in a high-temperature environment, and a method for producing the same. [Background technology]

[0002] RTB rare earth sintered magnets are essential functional materials for energy conservation and high performance, and their range of applications and production volume are expanding year by year.Typical applications include motors used in electric and hybrid vehicles, and motors for various home appliances such as air conditioners.The high coercive force of RTB rare earth sintered magnets is an advantage for these applications, but there is a demand for improved heat resistance, i.e., improved magnetic properties.

[0003] In the past, in the development of RTB rare earth sintered magnets, much research has been done to improve the room temperature magnetic properties of the magnet products, and in particular to improve squareness, because these properties affect the actual demagnetization behavior in applied products. In particular, the deterioration of squareness is significant when the RTB rare earth sintered magnet has a composition with a low boron content, and to improve this, for example, WO 2022 / 209466 (Patent Document 1) proposes a method of extending the sintering time and carrying out a two-stage sintering process. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 209466 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the sintering conditions presented in Patent Document 1 are a maximum of 2 hours for the first sintering time and a maximum of 15 hours for the second sintering time, and the time required for the sintering process is significantly long when the cooling time between the first and second sintering processes is also taken into account, which not only reduces productivity but also increases the power consumption in the sintering process, significantly increasing manufacturing costs and posing an environmental problem by increasing carbon dioxide emissions.

[0006] The present invention has been made in light of the above circumstances, and has an object to provide an RTB rare earth sintered magnet that has excellent practical magnetic properties in high-temperature environments while reducing the power consumption required in the manufacturing process by optimizing the composition and structure of the magnet. [Means for solving the problem]

[0007] As a result of extensive research conducted by the present inventors in order to achieve the above object, R 2 T 14 In rare earth sintered magnets with the B phase as the main phase, the grain boundary phase is 6 (T, M1) 14 R phase and R-rich phase covered 2 (T, M1) 17 By incorporating this phase, the magnet will exhibit a demagnetization curve with two magnetization bending points at room temperature (23°C). However, because the temperature change of the magnetization bending point on the low magnetic field side is small, it has been discovered that in practical use it is not affected by the magnetization bending point and exhibits good heat resistance, leading to the completion of the present invention.

[0008] Therefore, the present invention provides the following rare earth sintered magnet and method for producing the same. 1. R (R is two or more elements selected from rare earth elements, essentially consisting of Nd and Pr), T (T is one or more elements selected from Fe and Co), B, M1 (M1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi), and M2 (M2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta), R is 12.5 atomic % to 16.0 atomic %, B is 4.5 atomic % to 5.3 atomic %, M1 is 0.5 atomic % to 2.5 atomic %, M2 is 0.05 atomic % to 0.5 atomic %, and T is the remainder; R 2 T 14 Phase B is the main phase, R 6 (T, M1) 14 R phase and R-rich phase covered 2 (T, M1) 17 phase in an area fraction exceeding 0 and not exceeding 10%, and characterized in that in the second quadrant of the magnetic polarization curve at 23°C, there are two magnetization bending points, a first bending point on the low magnetic field side and a second bending point on the high magnetic field side. 2. The magnetic field at the first knickpoint [first knick magnetic field (H k1 2. The rare earth sintered magnet of claim 1, wherein the magnetization resistance (T) is 10 kOe or more. 3. The first knic magnetic field (H k1 Absolute value of the temperature change rate (|β 1 |) is the magnetic field at the second knickpoint [second knick magnetic field (H k2 )] absolute value of the temperature change rate (|β 2 3. The rare earth sintered magnet according to claim 1 or 2, characterized in that: |β 1 |<|β 2 |×0.94···(1) [Here, the first knick magnetic field (H k1 ) temperature change rate (β 1 ), the second knic magnetic field (H k2 ) temperature change rate (β 2 ) is expressed by the following formula: β 1 =(H k1 @90℃-H k1 @23℃) / (90-23) / (H k1 @23℃) β 2 =(H k2 @90℃-H k2 @23℃) / (90-23) / (H k2 @23℃)] 4. A rare earth sintered magnet according to any one of 1 to 3, wherein the first knickpoint disappears in the second quadrant of the magnetic polarization curve at least at 90° C. or higher. 5. In the second quadrant of the magnetic polarization curve in the temperature range of 23°C or higher and less than 90°C, the first knic magnetic field (H k1 5. The rare earth sintered magnet of any one of 1 to 4, wherein the resistivity is 8 kOe or more. 6. In the magnetic polarization curve at 23°C, the first knick magnetic field (H k1 ) and the second knic magnetic field (H k2 ) between the average relative permeability (μ 2 6. The rare earth sintered magnet of any one of 1 to 5, wherein the ratio of N to M is greater than 1.1 and smaller than 1.3. 7. In the magnetic polarization curve at any temperature, the first knic magnetic field (H k1 ) in a magnetic field lower than the average relative permeability (μ 1 7. The rare earth sintered magnet of any one of 1 to 6, wherein the ratio of 1.0 to 1.05 is satisfied. 8. A method for producing a rare earth sintered magnet for producing the magnet according to claim 1, comprising a heat treatment step of sintering a compact obtained by molding fine powder of a raw material alloy in a magnetic field, wherein the sintering temperature (T) in the heat treatment step is 1020°C or higher and 1080°C or lower, and the sintering time (t) is expressed by the following formula (2): t=200.45±1-0.185T···(2) and the heating time is from 1 hour to less than 11 hours. Effect of the Invention

[0009] According to the present invention, a rare earth sintered magnet having excellent magnetic properties even in a high temperature environment can be obtained with good productivity. [Brief description of the drawings]

[0010] [Figure 1] 2 is a graph showing the magnetic polarization curves from 23° C. to 140° C. of the rare earth sintered magnet obtained in Example 1. [Diagram 2]The graph shows the change in the second derivative of magnetization versus magnetic field for the rare earth sintered magnet, with the downward convex peak value designated Hk2. [Diagram 3] This is an enlarged graph of FIG. 2 in which Hk1 was calculated in a similar manner. [Figure 4] 4 is a photograph showing a backscattered electron composition image of a cross section parallel to the magnetization direction of the sintered body after low-temperature heat treatment in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The composition, structure, magnetic properties and production method of the highly heat-resistant rare earth sintered magnet of the present invention will be described in detail below.

[0012] The rare earth sintered magnet of the present invention has a composition of 12.5 atomic % to 16.0 atomic % of R element, 4.5 atomic % to 5.3 atomic % of B (boron), 0.5 atomic % to 2.5 atomic % of M1 element, 0.05 to 0.5 atomic % of M2 element, and the balance T.

[0013] R is two or more elements selected from rare earth elements, and Nd and Pr are essential. Preferable rare earth elements other than Nd and Pr are Y, La, Ce, Gd, Tb, Dy, and Ho. The content of R is 12.5 atomic % to 16.0 atomic % of the entire composition excluding unavoidable impurities of the magnet, and is preferably 13 atomic % or more, with the upper limit being 16 atomic % or less. If the content of R is less than 12.5 atomic %, the coercive force of the magnet will drop significantly, and if it exceeds 16 atomic %, the residual magnetic flux density B r The ratio of essential components Nd and Pr in R is preferably 80 to 100 atomic % in total of R. R may or may not contain Dy, Tb, and Ho, but if R contains them, the content of Dy, Tb, and Ho in total is preferably 5 atomic % or less of the total of R, more preferably 4 atomic % or less, further preferably 2 atomic % or less, and particularly preferably 1.5 atomic % or less.

[0014] M1 is composed of one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi. M1 is R 6 (T, M1) 14 It is an element necessary for the formation of the phase, and the same phase can be formed by adding a certain amount. If M1 is not contained, R 6 (T, M1) 14 As a result, the magnetic properties specific to the present invention, which will be described later, cannot be obtained. 1 The content of M1 is 0.5 atomic % to 2.5 atomic % with respect to the entire composition of the magnet excluding unavoidable impurities, and the lower limit is preferably 1.0 atomic % or more. If the content of M1 is less than 0.5 atomic %, the R in the grain boundary phase 6 (T, M1) 14 The amount of precipitated phase is small and sufficient magnetic properties do not appear. On the other hand, if it exceeds 2.5 atomic percent, the residual magnetic flux density B r This is not desirable because it reduces the

[0015] M2 is composed of one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta. The content of M2 is 0.05 to 0.5 atomic % or less, and within this content range, it forms a compound with boron and carbon during sintering, which is effective in suppressing abnormal grain growth and reducing variations in magnetic properties due to composition fluctuations.

[0016] The content of B (boron) is in the range of 4.5 atomic % to 5.3 atomic % of the total composition excluding inevitable impurities of the magnet. As mentioned above, boron forms a compound with a part of the M2 element, so the amount of boron added is adjusted within the range of 4.5 atomic % to 5.3 atomic % according to the amount of M2 added.

[0017] T is composed of one or more elements selected from Fe and Co. The content of T, which is the balance relative to the entire composition excluding inevitable impurities, is preferably 70 atomic % or more, more preferably 75 atomic % or more, and is preferably 85 atomic % or less, more preferably 80 atomic % or less.

[0018] Co can be contained as T as described above for the purpose of improving the Curie temperature and corrosion resistance. The content of Co is preferably 10 atomic % or less, and more preferably 5 atomic % or less, based on the entire composition excluding unavoidable impurities. If the Co content exceeds 10 atomic %, it will lead to a significant decrease in coercivity and an increase in costs.

[0019] The rare earth sintered magnet of the present invention may contain oxygen and nitrogen. However, since oxygen and nitrogen tend to form composite compounds containing carbon, the lower the content, the better. The content of these elements is preferably 1.5 atomic % or less, and more preferably 1.0 atomic % or less, for oxygen, and preferably 0.5 atomic % or less, and more preferably 0.2 atomic % or less, for nitrogen, based on the entire composition excluding unavoidable impurities.

[0020] The rare earth sintered magnet of the present invention may contain carbon. The carbon content is preferably 1.0 atomic % or less. Carbon remains in the sintered body as an impurity in the raw materials and as a decomposition residue of a lubricant added to improve the orientation of fine powder during compaction in a magnetic field. In the sintered body, carbon is dissolved in the R oxide or R-rich phase in the grain boundary phase, and in the composition range of boron in the present invention, it replaces part of the boron in the main phase and becomes the R oxide. 2 T 14 (B, C) 1 The carbon content suitable for the expression of magnetic properties is adjusted according to the boron and M2 element contents.

[0021] In addition to these elements, the inclusion of elements such as H, F, Mg, P, S, Cl, and Ca as unavoidable impurities is permitted, and the total amount of the unavoidable impurities is permitted to be up to 0.1% by mass of the total of the above-mentioned magnet constituent elements and unavoidable impurities, but it is preferable that the content of the unavoidable impurities is also low.

[0022] From the viewpoint of improving magnetic properties, the average grain size of the crystal grains of the rare earth sintered magnet of the present invention is preferably 1.5 μm or more and 5 μm or less. Furthermore, it is preferable to add a lubricant to improve the orientation during compaction in a magnetic field, so that the degree of orientation of the c-axis, which is the axis of easy magnetization of the main phase grains, is 98% or more. The residual magnetic flux density (B r ) is preferably 12 kG (1.2 T) or more at about 23° C., and the coercive force is preferably 20 kOe (1592 kA / m) or more at about 23° C.

[0023] In the rare earth sintered magnet of the present invention, the above-mentioned boron content is R 2 Fe 14 B 1 Since the stoichiometric composition is lower than that of ferromagnetic R 2 (T, M1) 17 In this case, the R phase is generated, which leads to a decrease in coercivity and a deterioration in squareness. 6 (T, M1) 14 R phase and R-rich phase 2 (T, M1) 17 By covering the phase, R 2 (T, M1) 17 This breaks the magnetic interaction between the phase and the main phase particles, and suppresses the propagation of magnetization reversal. Although this increase in coverage is effective in suppressing magnetization reversal, it is difficult to suppress the propagation of magnetization reversal above the magnetic phase transition point. 2 (T, M1) 17 After the phase becomes paramagnetic, the magnetic effect is reduced, and the decrease in coercive force and the deterioration of squareness can be suppressed. Therefore, although there is no particular limitation, the coverage is preferably 50% or more, and particularly 70% or more.

[0024] R of the cross section of a sintered magnet relative to the area of ​​the entire magnet 2 (T, M1) 17A smaller surface fraction of the phase is more effective in suppressing magnetization reversal, but for the same reasons as above, it is not necessary to completely eliminate the phase because the magnetic properties improve at high temperatures and have no practical effect. However, if it exceeds 10%, the effect on the magnetic properties cannot be ignored in practice even at high temperatures, so this is not desirable. Also, extending the sintering time and adding a homogenization process are effective in completely eliminating the phase, but these process changes are not desirable because they not only reduce productivity but also lead to increased manufacturing costs due to increased power consumption. Taking these factors into consideration, 2 (T, M1) 17 The area fraction of the phase is more than 0% and not more than 10%, with a preferred lower limit being 3% or more and a preferred upper limit being 5%.

[0025] The rare earth sintered magnet obtained by the present invention has two magnetization inflection points (knickpoints) in the second quadrant of the magnetic polarization curve at room temperature (23°C). In the present invention, the knickpoint located on the highest magnetic field side is called the second knickpoint, and the knickpoint located on the lower magnetic field side is called the first knickpoint.

[0026] In the present invention, the knickpoint is a point where the rate of change of magnetic polarization with respect to the magnetic field is locally maximum in the magnetic polarization curve, and the magnetic field that gives this knickpoint, specifically, the magnetic field that gives the minimum value of the second derivative of the magnetic polarization with respect to the magnetic field, is defined as the knick magnetic field. Figure 1 shows an example of a magnetic polarization curve, and in the magnetic polarization curve at room temperature (23°C) in the figure, the rate of magnetization change increases in a magnetic field of 13 to 14 kOe, and a remarkable increase in magnetization due to magnetization reversal is observed at about 20 kOe.

[0027] Figure 2 is a plot of the second derivative of the magnetic polarization curve in Figure 1 versus the magnetic field, showing a downward convex curve. The peak at approximately 20 kOe in the graph at room temperature (23°C) is the magnetic field at which the magnetization change rate associated with the simultaneous magnetization reversal of the main phase particles is maximized, and the second knick magnetic field (H k2 ) is defined as

[0028] Figure 3 is a plot of Figure 2 enlarged in the vertical direction. For example, the small peak at a magnetic field of about 13 kOe in the 23°C plot is a change in magnetization due to local magnetization reversal of the ferromagnetic phase remaining in the sintered compact structure and the surrounding main phase grains. This magnetic field is called the first knic field (H k1 ) is defined as

[0029] The first knic magnetic field of the rare earth sintered magnet of the present invention is preferably 10 kOe or more at 23° C. If it is 10 kOe or more, the magnetic flux amount at the operating point is less likely to decrease, making it suitable for practical use.

[0030] Here, the first knick magnetic field (H k1 ) temperature change rate (β 1 ) and the second knic magnetic field (H k2 ) temperature change rate (β 2 ) are expressed by the following formulas. In the formulas, "@23°C" means the value at 23°C. β 1 =(H k1 @90℃-H k1 @23℃) / (90-23) / (H k1 @23℃) β 2 =(H k2 @90℃-H k2 @23℃) / (90-23) / (H k2 @23℃)

[0031] At this time, the absolute value of the temperature change rate of the first knick magnetic field (|β 1 |) is the absolute value of the temperature gradient of the second knick magnetic field (|β 2 |) and preferably satisfies the relationship of the following formula (1). |β 1 |<|β 2 |×0.94···(1) That is, the first knic magnetic field (H k1 Absolute value of the temperature change rate (|β 1 |) is the second knic magnetic field (H k2 Absolute value of the temperature change rate (|β 2It is preferable that the magnetic flux amount at the operating point in a high-temperature environment is less likely to decrease if the magnetic flux amount is within this range.

[0032] First Knick magnetic field (H k1 ) is preferably 8 kOe or more at temperatures higher than 23° C. and lower than 90° C., and the first knickpoint preferably disappears at temperatures higher than 90° C. k1 ) in such a range is preferable because the amount of magnetic flux at the operating point in a high-temperature environment is unlikely to decrease.

[0033] The reason why the first knick point recognized at 23°C disappears at 90°C or higher and the absolute value of the temperature change rate of the first knick magnetic field (|β 1 |) is the absolute value of the temperature change rate of the second knic magnetic field (|β 2 The structural reason why the R is more than 6% smaller than the R (|) is unclear, but the R is likely to be due to the paramagnetization caused by the magnetic phase transition of the ferromagnetic phase remaining in the structure and the R distributed to cover the ferromagnetic phase. 6 (T, M1) 14 This is believed to be due to the disruption of the magnetic coupling between the ferromagnetic phase and the surrounding main phase grains due to the formation of the phase.

[0034] In addition, in the magnetic polarization curve of the rare earth sintered magnet of the present invention at 23° C., the first knic magnetic field (H k1 ) in a magnetic field lower than the average relative permeability (μ 1 ) is preferably 1.0 or more and 1.05 or less. On the other hand, the first knic magnetic field (H k1 ) and the second knic magnetic field (H k2 ) in a magnetic field up to 2 ) is preferably greater than 1.1 and smaller than 1.3. 1 If μ is 1.05 or less, the magnetic flux amount at the operating point is unlikely to decrease, which is preferable in practice. 2 If μ is smaller than 1.3, the magnetic flux amount at the operating point in a high-temperature environment is less likely to decrease, which is preferable. 2 If is larger than 1.1, the amount of excessive energy and time input to the sintering process can be reduced, as described later, and an increase in the manufacturing load and a decrease in productivity can be suppressed.

[0035] Next, a method for producing a rare earth sintered magnet of the present invention will be described. The method for producing the rare earth sintered magnet of the present invention, which produces the rare earth sintered magnet of the present invention, includes a heat treatment step of sintering a compact obtained by molding fine powder of a raw material alloy in a magnetic field. More specifically, the method includes a melting step of melting the raw material to obtain an alloy containing the elements R, T, B, M1, and M2, a crushing step of crushing the raw material alloy of a predetermined composition to obtain a fine powder, a molding step of molding the fine powder in a magnetic field to obtain a compact, and a heat treatment step of sintering and homogenizing the compact to form the above-mentioned structure.

[0036] In the melting step, the metal or alloy that is the raw material for each element is weighed so as to obtain the predetermined composition in the present invention described above, and the raw material is melted, for example, by high-frequency melting, and cooled to produce a raw material alloy. The raw material alloy is generally cast by a melting casting method in which the alloy is poured into a flat mold or a book mold, or a strip casting method. In addition, the R, which is the main phase of the RTB alloy, is also cast by a melting casting method. 2 Fe 14 The present invention can also be applied to the so-called two-alloy method, in which an alloy close to the B compound composition and a low-melting alloy that melts at the sintering temperature are weighed and mixed as sintering aids after coarse grinding. The sintering aid is preferably a composition containing a large amount of R components in order to lower the melting point. There is no particular restriction on the casting method, but in addition to the above, a liquid quenching method can also be used.

[0037] The pulverization step may include a plurality of steps including a coarse pulverization step and a fine pulverization step depending on the form of the raw material to be input. In this case, for example, a jaw crusher, a Brown mill, a pin mill, or hydrogen pulverization is used in the coarse pulverization step. In industrial practice, a method is preferably adopted in which a ribbon-shaped alloy obtained by strip casting is used, and then hydrogen pulverization is performed to obtain a coarse powder having an average particle size of 0.05 to 3 mm, particularly 0.05 to 1.5 mm. After the coarse pulverization, a lubricant can be appropriately added to increase the orientation of the powder in the molding step. Examples of the types of lubricants include saturated fatty acids such as stearic acid, decanoic acid, and lauric acid, or saturated fatty acid salts such as zinc stearate, and further compounds having a polar functional group and a cyclohexane skeleton such as cyclohexanol, cyclohexylamine, cyclohexanone, and cyclohexylcarboxylic acid, and further cyclic terpenes having a cyclohexane skeleton in the molecule such as menthol, menthone, and camphor, and it is also possible to add them in a mixed state.

[0038] The fine pulverization step can suitably employ a method of pulverizing the coarse powder using a jet mill with an inert gas stream such as nitrogen, helium, or argon. The average particle size after pulverization is preferably 0.2 μm to 10 μm, more preferably 0.5 μm to 5 μm, in terms of volume-based median diameter D50. In addition, in order to reduce the impurity oxygen concentration in the sintered body, it is preferable that the moisture content in the atmosphere during pulverization is 100 ppm or less. The volume-based median diameter D50 is the particle size when the cumulative volume frequency is 50%.

[0039] The compacting step may employ a method in which a magnetic field of 400 to 1600 kA / m is applied to the fine powder to orient it in the direction of the easy magnetization axis, and the powder is compressed and compacted to obtain a green compact. In this case, the green compact density is 2.8 to 4.2 g / cm. 3 That is, from the viewpoint of securing the strength of the molded body and obtaining good handling properties, the molded body density is preferably 2.8 g / cm. 3 On the other hand, in order to obtain sufficient compact strength and to suppress disturbance of the particle orientation when pressed, the compact density is preferably 4.2 g / cm. 3It is preferable that the compaction is carried out in an inert gas atmosphere such as nitrogen gas or Ar gas in order to suppress oxidation of the alloy fine powder.

[0040] In the heat treatment step, the compact obtained in the compacting step is sintered in a high vacuum or in a non-oxidizing atmosphere such as Ar gas. The sintering temperature (T) is in the range of 1020°C or higher and 1080°C or lower, and the holding time (t) is 1 hour or higher and less than 11 hours. If the holding time is less than 1 hour, the sintered body will not follow the temperature sufficiently, and there is a possibility that uneven sintering will occur in the furnace and inside the sintered body. On the other hand, a holding time of 11 hours or more is not preferable because it significantly deteriorates productivity. Furthermore, within the above holding time, the preferable holding time is a function of the sintering temperature (T), i.e., the following formula (2): t=200.45±1-0.185T···(2) By holding the magnet for a time within this range, it is possible to obtain the rare earth sintered magnet of the present invention having the above-mentioned characteristics. If the time is shorter than that given by formula (2), the coercive force decreases and the average relative permeability (μ 2 Conversely, if the time is long, abnormal grain growth will occur at high temperatures, resulting in a decrease in the strength of the sintered body and deterioration of the magnetic properties, while at low temperatures productivity will decrease, leading to increased costs. After sintering, it is preferable to quickly cool the material to 400°C or less by gas quenching (cooling rate: 20°C / min or more).

[0041] Following the above heat treatment for sintering, a heat treatment may be performed at a temperature lower than the sintering temperature, although this is not particularly limited, in order to increase the coercive force. This post-sintering heat treatment may be a two-stage heat treatment of a high-temperature heat treatment and a low-temperature heat treatment, or only a low-temperature heat treatment may be performed. In the high-temperature heat treatment in the post-sintering heat treatment, the sintered body is preferably heat-treated at a temperature of 900 to 1000°C, and in the low-temperature heat treatment, the sintered body is preferably heat-treated at a temperature of 400 to 600°C. Cooling after the high-temperature heat treatment is preferably performed by gas quenching (cooling rate: 5°C / min or more) to 400°C or less quickly. On the other hand, the cooling rate after the low-temperature heat treatment has no effect on the magnetic properties and is not particularly specified, but it is preferable to cool the sintered body quickly to 40°C or less in order to suppress surface oxidation and to carry it out of the furnace in a short time. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0043] [Example 1] The alloy composition is Di 15.0 Fe bal. Co 1.0 B 5.3 Al 0.2 Cu 0.2 Ga 0.9 S 0.2 Zr 0.2 (Here, Di is a mixture of Nd and Pr, and the composition ratio was Nd:Pr = 78:22.) The raw metal or alloy was melted in an Ar gas atmosphere in a high-frequency melting furnace, and an alloy ribbon with an average thickness of about 300 μm was produced by strip casting. The alloy ribbon was coarsely pulverized by hydrogenation and dehydrogenation treatment, and then 0.15 mass% of stearic acid was added to obtain a coarse powder with an average particle size of about 100 μm. Next, fine pulverization was performed in a jet mill in a nitrogen stream so that the average particle size would be 3 μm or less. At this time, the oxygen concentration in the jet mill was controlled to 50 ppm or less.

[0044] The resulting fine powder was filled into the die of a molding machine in a nitrogen atmosphere, and pressed vertically while applying a horizontal static magnetic field of 15 kOe to orient the fine powder. The resulting molded body was sintered by heat treatment at 1050°C for 5.5 hours in a vacuum, and then cooled to below 200°C. It was then heated and held at 900°C for 2 hours, cooled at a rate of 20°C / min in an Ar gas atmosphere, and further subjected to low-temperature heat treatment at 470°C for 2 hours.

[0045] A rectangular sample measuring 18 mm x 15 mm x 12 mm was cut out from the center of the obtained sintered body, and the magnetic properties were measured using a BH tracer manufactured by Toei Kogyo Co., Ltd. The measurement temperatures were room temperature (23°C), as well as 50°C, 75°C, 95°C, 110°C, and 140°C.

[0046] Figure 1 shows the magnetic polarization curves from 23°C to 140°C, and Table 1 shows the magnetic property measurement results. From these, the first knickpoint was observed at 13.5 kOe in the magnetic polarization curve at 23°C, and the magnetization began to decrease at magnetic fields above that. k and squareness ratio (H k / H cJ On the other hand, at temperatures above 90°C, the first knickpoint disappeared, and the H k In addition, an improvement in squareness ratio is observed.

[0047] [Table 1]

[0048] In addition, β from 23℃ to 80℃ 1 and β 2 , H calculated from the magnetic polarization curve at 23°C in Figure 1 k1 The average relative permeability in the lower magnetic field (μ 1 ), and H k1 and H k2 The average relative permeability (μ 2 ) are shown in Table 2.

[0049] [Table 2]

[0050] From the results in Table 2, H k1 The absolute value of the temperature change rate (|β 1 |) is H k2 The absolute value of the temperature change rate (|β 2 It can be seen that the relative permeability is approximately 27% smaller than that of the first knickpoint. It was also confirmed that the average relative permeability differs on either side of the first knickpoint, and that the average relative permeability between the first and second knickpoints increased to 1.17. Figure 2 shows a graph plotting the change in the second derivative of magnetization against the magnetic field. In this figure, the downward convex peak value is H k2 In addition, the same H k1 The graph showing the results is shown in Figure 3.

[0051] In addition, the cross section of the sintered body after low-temperature heat treatment was observed with a scanning electron microscope (SEM). The backscattered electron composition image of the cross section parallel to the magnetization direction is shown in Figure 4. In the center of the figure, (Nd, Pr) 6 (Fe, Ga, Si, Al) 14 phase and R-rich phase covered (Nd,Pr) 2 (Fe, Co, Ga, Si) 17 The phase was observed, and its area fraction relative to the entire cross section was 3%.

[0052] [Examples 2 to 4] The raw metal or alloy was melted in an Ar gas atmosphere in a high-frequency melting furnace so that the alloy composition was as shown in Table 3 below, and an alloy ribbon with an average thickness of about 300 μm was produced by strip casting. The alloy ribbon was coarsely pulverized by hydrogenation and dehydrogenation treatment, and then 0.15 mass% of stearic acid was added to obtain a coarse powder with an average particle size of about 100 μm. Next, fine pulverization was performed in a jet mill in a nitrogen stream so that the average particle size was 3 μm or less. At this time, the oxygen concentration in the jet mill was controlled to 50 ppm or less.

[0053] [Table 3]

[0054] The resulting fine powder was filled into the die of a molding machine in a nitrogen atmosphere, and pressed vertically while applying a horizontal static magnetic field of 15 kOe to orient the fine powder. The resulting compact was sintered by heat treatment at 1050°C in a vacuum for 5.5 hours, and then cooled to below 200°C. It was then heated and held at 900°C for 2 hours, cooled at 20°C / min in an Ar gas atmosphere, and further subjected to low-temperature heat treatment at 470°C for 2 hours.

[0055] A rectangular sample measuring 18 mm x 15 mm x 12 mm was cut out from the center of the obtained sintered body, and the magnetic properties were measured using a BH tracer manufactured by Toei Kogyo Co., Ltd. The measurement temperatures were room temperature (23°C), as well as 50°C, 65°C, 70°C, 80°C, and 95°C. The results are shown in Tables 4 and 5. Details will be described later.

[0056] In addition, when SEM observation was performed in the same manner as in Example 1, (Nd, Pr) contained in the sintered body was 6 (Fe, Ga, Si, Al) 14 phase and R-rich phase covered (Nd,Pr) 2 (Fe, Co, Ga, Si) 17 The area fraction of the phase relative to the entire cross section was 3 to 5% for all magnets.

[0057] [Comparative Example 1] The alloy composition is Di 14.0 Dy 1.0 Fe bal. Co 1.0 B 6.2 Al 0.2 Cu 0.1 Zr 0.1 (Here, Di is a mixture of Nd and Pr, and the composition ratio was Nd:Pr = 78:22.) The raw metal or alloy was melted in an Ar gas atmosphere in a high-frequency melting furnace, and an alloy ribbon with an average thickness of about 500 μm was produced by strip casting. The alloy ribbon was coarsely pulverized by hydrogenation and dehydrogenation treatment, and then 0.05 mass% of stearic acid was added to obtain a coarse powder with an average particle size of about 100 μm. Next, fine pulverization was performed in a jet mill in a nitrogen stream so that the average particle size would be 3.5 μm or less. At this time, the oxygen concentration in the jet mill was controlled to 500 ppm or less.

[0058] The resulting fine powder was filled into the die of a molding machine in a nitrogen atmosphere, and pressed vertically while applying a horizontal static magnetic field of 15 kOe to orient the fine powder. The resulting compact was sintered by heat treatment at 1100°C in a vacuum for 3 hours, and then cooled to below 200°C. It was then heated and held at 900°C for 2 hours, slowly cooled in an Ar gas atmosphere, and then subjected to a low-temperature heat treatment at 470°C for 2 hours.

[0059] A rectangular sample measuring 18 mm x 15 mm x 12 mm was cut out from the center of the obtained sintered body, and the magnetic properties were measured using a BH tracer manufactured by Toei Kogyo Co., Ltd. The measurement temperatures were room temperature (23°C), as well as 50°C, 65°C, 70°C, 80°C, and 95°C. The results are shown in Tables 4 and 5.

[0060] In addition, SEM observation was performed in the same manner as in Example 1, and it was found that (Nd, Pr, Dy) 2 (Fe,Co) 17 The precipitation of the R phase was observed, but the B content was high. 6 (T, M1) 14 No phase precipitation was observed.

[0061] [Table 4]

[0062] [Table 5]

[0063] As shown in Table 4, the rare earth sintered magnets of Examples 2 to 4 had the first knickpoints at 23° C. and deteriorated squareness, but the first knickpoints disappeared and squareness improved at 70 to 95° C. As shown in Table 5, the rare earth sintered magnets of Examples 2 to 4 had the first knickpoints at 23° C. and deteriorated squareness. k1 The absolute value of the temperature change rate (|β 1 |) is H k2 The absolute value of the temperature change rate (|β 2It can be seen that the average permeability is different on either side of the first knickpoint, and the average relative permeability (μ 2 ) was confirmed to have increased to 1.16-1.26.

[0064] On the other hand, in the rare earth sintered magnet of Comparative Example 1, the first knickpoint was present even at 95° C., and the squareness was not sufficiently improved. This is because, as mentioned above, the precipitation of Fe in the alloy causes the (Nd, Pr, Dy) in the sintered compact structure to become weak. 2 (Fe,Co) 17 The precipitation of the R phase was observed, but the B content was high. 6 (T, M1) 14 It is presumed that this is because the phase did not precipitate and was magnetically coupled with the main phase.

[0065] [Examples 5 and 6, Comparative Examples 2 to 6] The alloy composition is Di 15.0 Fe bal. Co 1.0 B 5.0 Al 0.2 Cu 0.2 Ga 0.9 S 0.2 Zr 0.2 (Here, Di is a mixture of Nd and Pr, and the composition ratio was Nd:Pr=78:22.) The raw metal or alloy was melted in an Ar gas atmosphere in a high-frequency melting furnace, and an alloy ribbon with an average thickness of about 300 μm was produced by strip casting. The obtained alloy ribbon was coarsely pulverized by hydrogenation and dehydrogenation treatment, and then 0.20 mass% of stearic acid was added to obtain a coarse powder with an average particle size of about 100 μm. Next, fine pulverization was performed in a jet mill in a nitrogen stream so that the average particle size would be 2.5 μm or less. At this time, the oxygen concentration in the jet mill was controlled to 50 ppm or less.

[0066] The resulting fine powder was filled into the die of a molding machine in a nitrogen atmosphere, and pressed vertically while applying a horizontal static magnetic field of 15 kOe to orient the fine powder. The resulting molded body was heat-treated and sintered in a vacuum under the sintering conditions shown in Table 6. After cooling to below 200°C, it was heated and held at 900°C for 2 hours, cooled at 20°C / min in an Ar gas atmosphere, and then subjected to a low-temperature heat treatment at 470°C for 2 hours.

[0067] A rectangular sample measuring 18 mm x 15 mm x 12 mm was cut out from the center of each of the obtained sintered bodies, and the magnetic properties were measured using a BH tracer manufactured by Toei Kogyo Co., Ltd. The measurement temperatures were room temperature (23°C), as well as 50°C, 80°C, 100°C, 110°C, and 130°C. The measurement results and the calculated β1, β2, μ1, and μ2 are shown in Tables 7 and 8. In addition, each rare earth sintered magnet was observed with an SEM in the same manner as in Example 1 to measure the R 2 (T, M1) 17 The area fraction of the phase and the presence or absence of abnormal grain growth were confirmed, and the results are shown in Table 6.

[0068] [Table 6]

[0069] [Table 7]

[0070] [Table 8]

[0071] The magnets of Comparative Examples 2 to 4 had a R of more than 10% in the cross section of the sintered magnet because the sintering time was shorter than the sintering time given by formula (2). 2 (T, M1) 17 The precipitation of the phase was observed (Table 6). As a result, the squareness (H k / H cJ) deteriorated to 0.79 or less, and the squareness did not improve sufficiently even at high temperatures (Table 7). Furthermore, the average relative permeability (μ 2 ) was as high as 1.32 to 2.04 (Table 8). On the other hand, the magnets of Comparative Examples 5 and 6 had a longer sintering time than the sintering time given by formula (2), so that the cross section of the obtained sintered magnet had a large R 2 (T, M1) 17 No phase precipitation was observed (Table 6), and no first knickpoint was observed below 90°C (Table 7). However, in the magnet of Comparative Example 6, abnormal grain growth was observed after sintering because the sintering temperature was relatively high (Table 6). In addition, the productivity of the magnet of Comparative Example 5 was significantly reduced because the sintering time exceeded 11 hours (Table 6).

Claims

1. R (R is two or more elements selected from rare earth elements, essentially consisting of Nd and Pr), T (T is one or more elements selected from Fe and Co), B, M1 (M1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi), and M2 (M2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta), R is 12.5 atomic % to 16.0 atomic %, B is 4.5 atomic % to 5.3 atomic %, M1 is 0.5 atomic % to 2.5 atomic %, M2 is 0.05 to 0.5 atomic %, and T is the balance; R 2 T 14 Phase B is the main phase, R 6 (T, M1) 14 R phase and R-rich phase covered 2 (T, M1) 17 phase in an area fraction exceeding 0 and not exceeding 10%, and in the second quadrant of a magnetic polarization curve at 23°C, there are two magnetization inflection points, a first inflection point on the low magnetic field side and a second inflection point on the high magnetic field side.

2. The magnetic field at the first knickpoint [first knick magnetic field (H k1 2. The rare earth sintered magnet according to claim 1, wherein the magnetic moment (Mn) is 10 kOe or more.

3. The first knic magnetic field (H k1 Absolute value of the temperature change rate (|β 1 |) is the magnetic field at the second knickpoint [second knick magnetic field (H k2 ) ] absolute value of the temperature change rate (|β 2 3. The rare earth sintered magnet according to claim 1, wherein the sintered rare earth magnet has a length smaller than |(x,y) and satisfies the following formula (1): |β 1 |<|β 2 |×0.94・・・(1) [Here, the first knick magnetic field (H k1 ) temperature change rate (β 1 ), the second knic magnetic field (H k2 ) temperature change rate (β 2 ) is expressed by the following formula: β 1 =(H k1 @90℃-H k1 @23℃) / (90-23) / (H k1 @23℃) β 2 =(H k2 @90℃-H k2 @23℃) / (90-23) / (H k2 @23℃)]

4. 3. The rare earth sintered magnet according to claim 1, wherein the first knickpoint disappears in the second quadrant of the magnetic polarization curve at least at 90° C. or higher.

5. In the second quadrant of the magnetic polarization curve in the temperature range of more than 23° C. and less than 90° C., the first knic magnetic field (H k1 3. The rare earth sintered magnet according to claim 1, wherein the magnet strength is 8 kOe or more.

6. In the magnetic polarization curve at 23° C., the first knic magnetic field (H k1 ) and the second knic magnetic field (H k2 ) between the average relative permeability (μ 2 3. The rare earth sintered magnet according to claim 1, wherein the ratio of the sintered rare earth magnet to the total rare earth magnet mass is greater than 1.1 and smaller than 1.

3.

7. In the magnetic polarization curve at any temperature, the first knic magnetic field (H k1 ) in a magnetic field lower than the average relative permeability (μ 1 3. The rare earth sintered magnet according to claim 1, wherein the value of n is 1.0 or more and 1.05 or less.

8. A method for producing a rare earth sintered magnet for producing the magnet according to claim 1, comprising a heat treatment step of sintering a compact obtained by molding fine powder of a raw material alloy in a magnetic field, wherein the sintering temperature (T) in the heat treatment step is 1020° C. or higher and 1080° C. or lower, and the sintering time (t) is expressed by the following formula (2): t=200.45±1-0.185T...(2) and the heating time is from 1 hour to less than 11 hours.

Citation Information

Patent Citations

  • Permanent magnet with high thermal stability

    JP1989007503A

  • R-t-b-based sintered magnet

    JP2016149397A

  • R-t-b based sintered magnet

    JP2017183318A

  • R-t-b-based sintered magnet

    JP2019169621A

  • Sintered magnet

    WO2013191276A1