Base paper for metallized paper, metallized paper, and packaging bag
The base paper for vapor-deposited paper, with a resin and pigment coating layer, addresses the need for improved printability and processability in packaging applications, ensuring excellent performance in automatic packaging and barrier properties.
Patent Information
- Application Number
- JP2023069150
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Metallized paper used for packaging materials requires excellent printability and processability, especially in automatic packaging applications, which existing technologies do not adequately address.
A base paper for vapor-deposited paper is designed with a resin layer on one side and a pigment coating layer on the other, containing specific amounts of pigment and having a smooth surface with controlled friction, along with additional layers to enhance barrier properties and adhesion.
The solution provides vapor-deposited paper with excellent printability and processability, suitable for automatic packaging, while maintaining effective barrier properties against gases and moisture.
Smart Images

Figure 2024154922000001 
Figure 2024154922000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a base paper for metallized paper, metallized paper using the same, and a packaging bag using the metallized paper. [Background technology]
[0002] Conventionally, packaging materials that have been imparted with a paper base material water vapor barrier property that provides a barrier against water vapor, gas barrier property that provides a barrier against gases other than water vapor, and in particular oxygen barrier property that provides a barrier against oxygen, have been used in packaging foods, medical products, electronic components, and the like to prevent deterioration of the contents.
[0003] Metallized paper is a paper substrate on which a metallized layer made of metal or the like is provided to improve the barrier properties of the paper substrate against oxygen and water vapor.
[0004] Patent Document 1 discloses a base paper for metallized paper for forming a vapor-deposited layer by vapor deposition, which has a coating layer on at least one side of a paper substrate, the coating layer having, from the paper substrate side, a clay coating layer and a resin layer containing a water-dispersible polyurethane resin, in this order, wherein the Cobb water absorbency of the coating layer side is in a specific range and the contact angle with water of the coating layer surface is not more than a specific value.Patent Document 2 discloses a base paper for metallized paper for forming a vapor-deposited layer by vapor deposition, which has a clay coating layer and a resin layer on at least one side of a paper substrate, in this order, wherein the wetting tension of the resin layer surface is not less than a specific value and the surface roughness is not more than a specific value. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6958756 [Patent Document 2] Patent No. 6958757 Summary of the Invention [Problem to be solved by the invention]
[0006] Metallized paper used as a packaging material for food and the like is required to have excellent printability on the printing surface, and particularly when used as a packaging bag, it is required to have excellent processability in automatic packaging.
[0007] Therefore, an object of the present invention is to provide a base paper for metallized paper that provides metallized paper with excellent printability and processability in automatic packaging, and to provide metallized paper made using the base paper. Another object of the present invention is to provide a packaging bag made using the metallized paper. [Means for solving the problem]
[0008] The inventors have found that the above-mentioned problems can be solved by providing a base paper for metallized paper with a pigment coating layer containing a specific pigment content on the other side of the paper substrate, and by providing the side with the pigment coating layer with an Oken smoothness of a specific value or more and a dynamic friction coefficient against stainless steel of a specific value or less.
[0009] That is, the present invention has the following configuration. <1> A base paper for metallized paper having a resin layer on one side of a paper substrate, on which a metallized layer is to be formed, and a pigment coating layer on the other side of the paper substrate, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, the side having the pigment coating layer having an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <2> A clay coating layer is provided between the paper substrate and the resin layer. <1> The base paper for metallized paper according to claim 1. <3> the resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin; <1> or <2> The base paper for metallized paper according to claim 1. <4> A metallized paper having a metallized layer on a resin layer of a base paper for metallized paper having a paper substrate and a pigment coating layer on the other side of the base paper, wherein the pigment content in the pigment coating layer is 50% by mass or more and 85% by mass or less, and the surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <5> a heat seal layer on the vapor deposition layer; <4> The metallized paper according to claim 1. <6> an overcoat layer between the vapor deposition layer and the heat seal layer; <5> The metallized paper according to claim 1. <7> A clay coating layer is provided between the paper substrate and the resin layer. <4> ~ <6> 1. The metallized paper according to any one of the above. <8> the resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin; <4> ~ <7> 1. The metallized paper according to any one of the above. <9> <4> ~ <8> A packaging bag made using the metallized paper described in any one of 1 to 3. [Effects of the Invention]
[0010] The present invention provides a base paper for metallized paper that provides metallized paper with excellent printability and processability in automatic packaging, and metallized paper made using the same.Furthermore, the present invention provides a packaging bag made using the metallized paper. DETAILED DESCRIPTION OF THE INVENTION
[0011] [Base paper for metallized paper] The base paper for metallized paper of this embodiment (hereinafter simply referred to as base paper for metallized paper) has a resin layer on one side of a paper substrate, and is a base paper for metallized paper on which a metallized layer is formed on the resin layer. The other side of the paper substrate has a pigment coating layer, and the pigment content in the pigment coating layer is 50% by mass or more and 85% by mass or less. The side having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The base paper for metallized paper of this embodiment provides metallized paper with excellent printability and processability in automatic packaging.
[0012] The structure and properties of the base paper for metallized paper of this embodiment will be described in more detail below. In this specification, a numerical range represented by "X to Y" means a numerical range including X as the lower limit and Y as the upper limit. When a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily. Furthermore, "(meth)acrylic" is a generic term that includes both acrylic and methacrylic.
[0013] The base paper for metallized paper of this embodiment has a resin layer on one side of a paper substrate, on which a metallized layer can be formed, and has a pigment coating layer on the other side of the paper substrate. From the viewpoint of smoothing the surface of the paper substrate, the base paper for metallized paper of this embodiment preferably has a clay coating layer between one side of the paper substrate and the resin layer. That is, the base paper for metallized paper of this embodiment preferably has a clay coating layer on one side of the paper substrate and a resin layer on the clay coating layer.
[0014] <Paper base material> In this embodiment, the pulp constituting the paper base material is preferably primarily composed of plant-derived pulp, and more preferably primarily composed of wood pulp. Examples of wood pulp include hardwood pulp and softwood pulp. Examples of non-wood pulp include cotton pulp, hemp pulp, kenaf pulp, and bamboo pulp. Materials other than pulp fibers, such as synthetic fibers such as rayon fiber and nylon fiber, may also be blended as secondary paper materials as long as they do not impair the effects of the present invention.
[0015] From the viewpoints of the formation, physical properties and recyclability of the metallized paper, the proportion of hardwood pulp in the pulp constituting the paper base material is preferably 65% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.
[0016] Examples of internal sizing agents include rosin-based, alkyl ketene dimer-based, alkenyl succinic anhydride-based, styrene-unsaturated carboxylic acid-based, higher fatty acid-based, petroleum resin-based, etc. The content of the internal sizing agent is not particularly limited, but is preferably 0 to 3 parts by mass per 100 parts by mass of pulp (bone dry mass) of the paper base material.
[0017] In addition to the internal sizing agent, other known internal additives may be added to the paper base material, such as fillers, paper strength agents, retention aids, pH adjusters, drainage aids, water-resistant agents, softeners, antistatic agents, antifoaming agents, slime control agents, dyes, and pigments.
[0018] Examples of fillers include titanium dioxide, kaolin, talc, calcium carbonate (heavy calcium carbonate, light calcium carbonate), calcium sulfite, gypsum, calcined kaolin, white carbon, amorphous silica, delaminated kaolin, diatomaceous earth, magnesium carbonate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, and zinc hydroxide.
[0019] The paper base material is obtained by papermaking from a papermaking raw material mainly composed of pulp slurry. The pulp slurry can be obtained from wood or non-wood raw material chips through processes such as cooking, washing, and bleaching. There are no particular limitations on the methods used in the cooking, washing, and bleaching processes. The pulp slurry obtained through these processes is preferably further beaten in the presence of water.
[0020] In the papermaking of paper substrates, a known wet paper machine can be appropriately selected and used. Examples of paper machines include a Fourdrinier paper machine, a gap former paper machine, a cylinder paper machine, and a short wire paper machine. The paper layer formed by the paper machine is preferably transported on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying in the dryer.
[0021] The paper substrate obtained as described above may be subjected to a surface treatment using a calendar to make the paper thickness and gloss profile uniform. For the calendar treatment, a known calendaring machine can be appropriately selected and used.
[0022] Specific examples of paper substrates used in the base paper for metallized paper of this embodiment include bleached kraft paper, unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-side glazed paper, glassine paper, graphene paper, etc. Among these, bleached kraft paper, unbleached kraft paper, fine paper, and one-side glazed paper are preferred.
[0023] (Stöckigt size) The paper substrate is not particularly limited, but from the viewpoint of improving barrier properties, the Stoeckigt sizing degree of at least the surface on which a resin layer (described later) is to be formed is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 5 seconds or more, and the upper limit is not particularly limited, but is preferably 100 seconds or less, more preferably 30 seconds or less. The Stoeckigt sizing degree of the paper substrate is measured in accordance with JIS P 8122:2004. The Stoeckigt sizing degree of the paper substrate can be controlled by the type and content of internal sizing agent, the type of pulp, smoothing treatment, etc.
[0024] (Basic weight) The basis weight of the paper substrate is not particularly limited, but from the viewpoint of strength when used as a packaging bag, it is preferably 20 g / m 2 More preferably, 30 g / m 2 More preferably, 40 g / m 2 From the viewpoint of economy and ease of production, it is preferably 500 g / m 2 Less than 400 g / m 2 More preferably, 200 g / m or less 2 More preferably, 100 g / m or less 2 The basis weight of the paper substrate is measured in accordance with JIS P 8124:2011.
[0025] (Thickness) The thickness of the paper substrate is not particularly limited, but from the viewpoint of strength when used as a packaging bag, it is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 30 μm or more, and even more preferably 50 μm or more, and from the viewpoint of economy and ease of production, it is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 75 μm or less. The thickness of the paper substrate is measured in accordance with JIS P 8118:2014.
[0026] (density) The density of the paper substrate is preferably 0.5 g / cm from the viewpoint of moldability. 3 More preferably, 0.6 g / cm 3 More preferably, 0.7 g / cm 3 and preferably 1.2 g / cm 3 or less, more preferably 1.0 g / cm 3 The density of the paper substrate is calculated from the basis weight and thickness of the paper substrate measured by the above-mentioned method.
[0027] (Oken type smoothness) To obtain a uniform vapor-deposited layer, the paper substrate preferably has an Oken smoothness of at least 5 seconds, more preferably 10 seconds, on the surface on which the vapor-deposited layer is to be formed (i.e., the resin layer surface), and the upper limit is not particularly limited, but is preferably 1000 seconds or less, for example. The Oken smoothness of the paper substrate is measured in accordance with JIS P 8155:2010.
[0028] <Resin layer> The base paper for metallized paper of this embodiment preferably has a resin layer on one side of the paper substrate, and has a resin layer on a clay coat layer described below. By providing a resin layer, adhesion between the metallized layer of the metallized paper and the paper substrate of the base paper for metallized paper is improved, improving barrier properties. In addition, the resin layer has oxygen barrier properties and water vapor barrier properties, and therefore also functions to improve barrier properties when made into metallized paper.
[0029] The resin layer preferably contains a water-suspendable polymer, and more preferably contains primarily a water-suspendable polymer. The phrase "the resin layer primarily contains a water-suspendable polymer" means that the content of the water-suspendable polymer in the resin layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The resin layer may further contain any optional components in addition to the water-suspendable polymer.
[0030] (Water-suspended polymer) The water-dispersible polymer contained in the resin layer is not particularly limited, but examples thereof include alkyd resins; (meth)acrylic (co)polymers, styrene-(meth)acrylic resins; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; polyvinyl alcohol resins such as polyvinyl alcohol and ethylene-vinyl alcohol copolymers (ethylene-modified polyvinyl alcohol); cellulose resins; polyurethane resins; and polyester resins. These may be used alone or in combination of two or more. Among these, the water-dispersible polymer is preferably one or more selected from the group consisting of water-dispersible polyvinyl alcohol resins, water-dispersible polyurethane resins, and water-dispersible polyester resins, and more preferably one or more selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.
[0031] <Water-dispersible polyurethane resin> The water-dispersible polyurethane resin contained in the resin layer is not particularly limited, and is preferably one that can be prepared into one or more selected from the group consisting of polyurethane resin dispersions and emulsions, more preferably one that can be prepared into a polyurethane resin dispersion or emulsion, and even more preferably one that can be prepared into a polyurethane resin dispersion.
[0032] The water-dispersible polyurethane resin contained in the resin layer preferably contains at least one selected from the group consisting of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate. When the polyurethane resin contains at least one of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate, the total content of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate relative to the total amount of structural units derived from polyisocyanate is preferably 50 mol% or more. Such polyurethane resins exhibit high cohesion due to hydrogen bonds and the stacking effect between xylylene groups, and therefore have excellent gas barrier properties. The above content is 1 It can be identified using known analytical techniques such as H-NMR.
[0033] -Oxygen permeability- The water-dispersible polyurethane resin contained in the resin layer preferably has an oxygen permeability of 100 mL / (m) at 23°C and 50% RH when converted into a 25 μm thick sheet. 2 ·day·atm) or less, more preferably 50mL / (m 2 ·day·atm) or less, more preferably 25mL / (m 2 ·day·atm) or less, and even more preferably 10 mL / (m 2 ·day·atm) or less, and even more preferably 5mL / (m 2 ·day·atm) or less. A low oxygen permeability of the resin layer is preferable because it imparts better gas barrier properties to the base paper for metallized paper. In this specification, oxygen permeability is measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) under conditions of 23°C and 50% RH.
[0034] -Glass transition temperature- The glass transition temperature of the water-dispersible polyurethane resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of improving film-forming properties in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyurethane resin is measured in accordance with JIS K 7122:2012.
[0035] As the water-dispersible polyurethane-based resin, a synthetic product may be used, and examples thereof include the polyurethane-based resins described in WO 2015 / 016069.
[0036] As the water-dispersible polyurethane resin, commercially available products may be used, such as "Takelac W series (trade name)," "Takelac WPB series (trade name)," and "Takelac WS series (trade name)" manufactured by Mitsui Chemicals, Inc., specifically "Takelac WPB-341 (trade name)." Other commercially available products include "HPU W-003 (trade name)" (hydroxyl value 235 mg KOH / g) manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.
[0037] <Water-dispersible polyester resin> The water-dispersible polyester resin contained in the resin layer is not particularly limited, and is preferably one that can be prepared into one or more types selected from the group consisting of polyester resin dispersions and emulsions, more preferably one that can be prepared into a polyester resin dispersion or emulsion, and even more preferably one that can be prepared into a polyester resin dispersion.
[0038] -Acid value- From the viewpoint of achieving superior adhesion to a vapor-deposited layer described below, the acid value of the water-dispersible polyester resin is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, even more preferably 5 mgKOH / g or more, and even more preferably 6 mgKOH / g or more, and although there is no particular upper limit, it is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and even more preferably 15 mgKOH / g or less. The acid value of the water-dispersible polyester resin is measured in accordance with JIS K 0700:1992.
[0039] -Hydroxyl value- From the viewpoint of achieving superior adhesion to a vapor-deposited layer described below, the hydroxyl value of the water-dispersible polyester resin is preferably 0.5 mgKOH / g or more, more preferably 1 mgKOH / g or more, even more preferably 1.5 mgKOH / g or more, and even more preferably 2 mgKOH / g or more. The upper limit is not particularly limited, but is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and even more preferably 10 mgKOH / g or less. The hydroxyl value of the water-dispersible polyester resin is measured in accordance with JIS K 0700:1992.
[0040] -Glass transition temperature- The glass transition temperature of the water-dispersible polyester resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of improving film-forming properties in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyester resin is measured in accordance with JIS K 7122:2012.
[0041] As the water-dispersible polyester resin, commercially available products may be used, such as the "Elite KT Series (product name)" manufactured by Unitika Ltd. and the "Landy PL Series (product name)" manufactured by Miyoshi Oil & Fats Co., Ltd., and specific examples include "Elite KT-8803 (product name)" and "Landy PL-3000 (product name)."
[0042] (Silane coupling agent) From the viewpoint of improving the flex resistance of the resin layer, the resin layer may be one which contains a silane coupling agent in addition to the water-dispersible polymer.
[0043] The silane coupling agent is a compound having at least one alkoxysilyl group and at least one reactive functional group other than the alkoxysilyl group in the molecule. The alkoxysilyl group may be any of a monoalkoxysilyl group, a dialkoxysilyl group, and a trialkoxysilyl group, but from the viewpoint of reactivity, a trialkoxysilyl group is preferred.
[0044] Examples of reactive functional groups other than alkoxysilyl groups include vinyl groups, epoxy groups, styryl groups, (meth)acryloyloxy groups, amino groups, isocyanato groups, ureido groups, and acid anhydride groups. Among these, amino groups, epoxy groups, and acid anhydride groups are preferred, and amino groups are more preferred.
[0045] Examples of epoxy group-containing silane coupling agents include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0046] Examples of amino group-containing silane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane, and among these, 3-aminopropyltriethoxysilane is preferred.
[0047] An example of an acid anhydride group-containing silane coupling agent is 3-trimethoxysilylpropylsuccinic anhydride.
[0048] As the silane coupling agent, commercially available products may be used, and examples thereof include KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, and X-12-967C manufactured by Shin-Etsu Chemical Co., Ltd.
[0049] The amount of the silane coupling agent to be added is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, particularly preferably 0.3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less, particularly preferably 5 parts by mass or less, relative to 100 parts by mass of the water-suspendable polymer.
[0050] (optional ingredient) Optional components that may be contained in the resin layer include other resins and additives, such as antifoaming agents, surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and mold release agents.
[0051] The coating amount of the resin layer is not particularly limited, but is preferably 0.1 g / m in terms of solid content. 2 More preferably, 0.5 g / m 2 More preferably, 0.7 g / m2 and preferably 10 g / m 2 Less than 5g / m, more preferably 2 Less than 3 g / m, more preferably 2 The method for forming the resin layer is not particularly limited, but it is preferable to form the resin layer by applying an aqueous coating liquid containing a water-dispersible polymer and drying it.
[0052] <Clay court layer> As described above, the base paper for metallized paper of this embodiment preferably has a clay coating layer between the paper substrate and the resin layer, which seals the paper substrate and smooths the surface on which the resin layer is formed, forming a flatter resin layer. As a result, when metallized paper (described later) is formed, a uniform metallized layer can be formed, improving barrier properties.
[0053] The clay coat layer preferably contains an inorganic pigment and a binder, and more preferably is composed mainly of an inorganic pigment and a binder. The phrase "the clay coat layer is composed mainly of an inorganic pigment and a binder" means that the total content of the inorganic pigment and the binder in the clay coat layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The clay coat layer may further contain any optional components in addition to the inorganic pigment and the binder.
[0054] (inorganic pigments) The inorganic pigment contained in the clay coating layer is not particularly limited, but examples thereof include kaolin, talc, mica, etc., and preferably kaolin. The content of the inorganic pigment in the clay coating layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and preferably 98% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less.
[0055] <Aspect ratio> From the viewpoint of forming a uniform and smooth resin layer, the aspect ratio of the inorganic pigment is preferably 50 or less, more preferably 45 or less, and the lower limit thereof is not particularly limited, but is preferably 1 or more, more preferably 5 or more. The aspect ratio of the inorganic pigment can be measured by observation with an electron microscope or X-ray diffraction measurement.
[0056] ≪Average particle size≫ From the viewpoint of forming a uniform and smooth resin layer, the average particle size of the inorganic pigment is preferably 5 μm or less, more preferably 3 μm or less, even more preferably 1 μm or less, and even more preferably 0.50 μm or less, and the lower limit is not particularly limited, but is preferably 0.05 μm or more, more preferably 0.10 μm or more. The average particle size of the inorganic pigment means the median diameter (d50) measured by laser diffraction / scattering particle size distribution measurement.
[0057] (binder) The binder contained in the clay coating layer is not particularly limited, but examples thereof include styrene-butadiene resins; (meth)acrylic (co)polymers; styrene-(meth)acrylic resins; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; and polylactic acid. These may be used alone or in combination of two or more. Among these, one or more selected from the group consisting of styrene-butadiene resins, styrene-(meth)acrylic resins, olefin-unsaturated carboxylic acid copolymers, and polylactic acid are preferred, one or more selected from the group consisting of styrene-(meth)acrylic resins, ethylene-(meth)acrylic acid copolymers, and polylactic acid are more preferred, and one or more selected from the group consisting of styrene-acrylic resins, ethylene-acrylic resins, and polylactic acid are even more preferred.
[0058] The (meth)acrylic (co)polymer is a (co)polymer of one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters. The (meth)acrylic acid ester is not particularly limited, but is preferably an alkyl ester of (meth)acrylic acid having 1 to 12 carbon atoms.
[0059] The styrene-(meth)acrylic resin is a copolymer of styrene and one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters, and is preferably a styrene-acrylic resin or a styrene-methacrylic resin, and more preferably a styrene-acrylic acid copolymer or a styrene-acrylic acid ester copolymer.
[0060] The binder content in the clay coating layer is preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less.
[0061] (optional ingredient) Optional components that can be contained in the clay coating layer include adhesives, dispersants, thickeners, water retention agents, antifoaming agents, waterproofing agents, colorants, surfactants, etc. Adhesives include proteins such as casein, soy protein, and synthetic protein; starches such as oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, and dextrin; and cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose.
[0062] The coating amount of the clay coating layer is not particularly limited, but is preferably 5 g / m2 in terms of solid content. 2 More preferably, 8g / m 2 More preferably, 10 g / m 2 and preferably 30 g / m 2 Less than 20 g / m, more preferably 2 or less, more preferably 15 g / m 2 The following is the result.
[0063] The method for forming the clay coating layer is not particularly limited, but a method of forming the clay coating layer by coating a dispersion containing an inorganic pigment and a binder on a paper substrate and drying it is preferred. The dispersion containing an inorganic pigment and a binder is preferably one that uses an aqueous medium containing water as the main component as the solvent.
[0064] <Pigment coating layer> The base paper for metallized paper of this embodiment has a pigment coating layer on the other side of the paper substrate, i.e., the side opposite the side bearing the resin layer. By providing the pigment coating layer and then calendering the coated surface under specified conditions, the smoothness of the coated surface can be improved and the coefficient of dynamic friction against stainless steel can be reduced, resulting in metallized paper with excellent printability and processability. The pigment coating layer is preferably composed primarily of a pigment and a binder. Note that "the pigment coating layer is composed primarily of a pigment and a binder" means that the total content of the pigment and binder in the pigment coating layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The pigment coating layer may contain any optional components in addition to the pigment and binder.
[0065] (pigment) The pigment contained in the pigment coating layer is not particularly limited and may include, for example, inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, calcined clay, heavy calcium carbonate, light calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, and satin white; and organic pigments such as solid, hollow, and core-shell pigments. These may be used alone or in combination of two or more. Among these, at least one pigment selected from the group consisting of kaolin and calcium carbonate is preferred, and a combination of kaolin and calcium carbonate is even more preferred, with a combination of kaolin, heavy calcium carbonate, and light calcium carbonate being even more preferred. From the perspective of further improving printability, the mass ratio of kaolin to calcium carbonate in the pigment (kaolin / calcium carbonate) is preferably 10 / 90 to 50 / 50, more preferably 20 / 80 to 40 / 60.
[0066] The pigment content in the pigment coating layer is 50% by mass or more, preferably 60% by mass or more, and 85% by mass or less, preferably 83% by mass or less, from the viewpoint of preventing the ink from peeling off and achieving excellent printability when forming metallized paper and printing on the metallized paper.
[0067] (binder) The binder contained in the pigment coating layer is not particularly limited, but includes styrene-butadiene resins; acrylic resins such as methyl (meth)acrylate copolymers and styrene-(meth)acrylic copolymers; olefin-unsaturated carboxylic acid copolymers such as ethylene-(meth)acrylic acid copolymers; dextrin, mannan, chitosan, arabinogalactan, glycogen, inulin, pectin, hyaluronic acid, hydroxyethylated starch, oxidized starch, etherified starch, phosphated starch, enzyme-modified starch, and modified starch obtained by flash drying thereof, as well as natural polysaccharides and their oligomers and modified forms. Among these, one or more selected from the group consisting of acrylic resins, styrene-butadiene resins, and modified starches are preferred, one or more selected from the group consisting of styrene-(meth)acrylic copolymers, styrene-butadiene resins, and oxidized starches are more preferred, one or more selected from the group consisting of styrene-butadiene resins and oxidized starches is even more preferred, and a combination of both is even more preferred.
[0068] The content of the binder in the pigment coating layer is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 50% by mass or less, more preferably 45% by mass or less. When oxidized starch is used as the binder, the content of the oxidized starch in the pigment coating layer is preferably 1% by mass or more, more preferably 2% by mass or more, and preferably 12% by mass or less, more preferably 8% by mass or less.
[0069] (optional ingredient) Optional components that may be contained in the pigment coating layer include adhesives, dispersants, thickeners, water retention agents, antifoaming agents, waterproofing agents, colorants, surfactants, etc. Adhesives include proteins such as casein, soy protein, and synthetic protein; starches such as oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, and dextrin; and cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose.
[0070] The coating amount of the pigment coating layer is not particularly limited, but is preferably 3 g / m2 in terms of solid content. 2 More preferably, 5 g / m 2 More preferably, 7 g / m 2 and preferably 30 g / m 2 Less than 20 g / m, more preferably 2 or less, more preferably 15 g / m 2 The following is the result.
[0071] The method for forming the pigment coating layer is not particularly limited, but a method of forming the layer by coating a dispersion containing a pigment and a binder on a paper substrate and drying it is preferred. The dispersion containing a pigment and a binder is preferably one that uses an aqueous medium containing water as the main component as the solvent.
[0072] <Physical properties of base paper for metallized paper> (Oken type smoothness) From the viewpoint of obtaining a base paper for metal-deposited paper with excellent printability, the Oken smoothness of the pigment-coated surface of the base paper for metal-deposited paper is 300 seconds or more, preferably 350 seconds or more, more preferably 450 seconds or more, even more preferably 650 seconds or more, and even more preferably 850 seconds or more. The upper limit is not particularly limited, but is preferably 5000 seconds or less, more preferably 3000 seconds or less. The Oken smoothness of the pigment-coated surface of the base paper for metal-deposited paper does not change even after undergoing a process such as providing a metal-deposited layer to obtain metal-deposited paper, so if the Oken smoothness is within the above range, metal-deposited paper with excellent printability can be obtained. The Oken smoothness of the pigment-coated surface is measured in accordance with JIS P 8155:2010. The Oken smoothness of the surface having the pigment coating layer can be adjusted to the above range by adjusting the Oken smoothness of the paper base material used, or by performing a calendar treatment under the following conditions after forming the pigment coating layer. As for the calendering conditions, the linear pressure is preferably 10 kg / cm or more, more preferably 30 kg / cm or more, even more preferably 50 kg / cm or more, and is preferably 1000 kg / cm or less, more preferably 500 kg / cm or less, even more preferably 200 kg / cm or less. Furthermore, when heating is performed in the calendering process, the heating temperature is not particularly limited, but from the viewpoint of enhancing the effect of the process while preventing thermal deterioration of the paper base material or pigment coating layer and sticking of the pigment coating layer, the heating temperature is preferably 20°C or higher, more preferably 30°C or higher, even more preferably 35°C or higher, and is preferably 80°C or lower, more preferably 70°C or lower, even more preferably 60°C or lower. The calendering may be carried out in one or more stages. From the viewpoint of further improving printability and / or automatic packaging suitability, however, it is preferably carried out in multiple stages (two or more stages), more preferably five or more stages, and even more preferably ten or more stages. There is no particular upper limit, but it is preferably 15 stages or less.
[0073] (Kinematic friction coefficient against stainless steel) The dynamic friction coefficient of the pigment-coated surface of the base paper for metal-deposited paper against stainless steel is 0.35 or less, more preferably 0.32 or less, from the viewpoint of obtaining a base paper for metal-deposited paper with excellent processability. From the viewpoint of further improving processability (ease of transport in an automatic packaging machine), it is even more preferably 0.22 or less, even more preferably 0.20 or less. The lower limit is not particularly limited, but is preferably 0.10 or more. The dynamic friction coefficient of the pigment-coated surface of the base paper for metal-deposited paper against stainless steel does not change even after the process of providing the metal-deposited layer, so a value within the above range ensures excellent processability. The dynamic friction coefficient of the pigment-coated surface against stainless steel is measured in accordance with JIS P 8147:2010, specifically, by the method described in the Examples. The dynamic friction coefficient of the surface having the pigment coating layer against stainless steel can be adjusted to the above range by adjusting the Oken smoothness of the paper base material used, or by performing a calendar treatment under the above conditions after forming the pigment coating layer.
[0074] (Thickness) The thickness of the base paper for metallized paper is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less. The thickness of the base paper for metallized paper is measured in accordance with JIS P 8118:2014.
[0075] There are no particular limitations on the method for producing the base paper for metallized paper of this embodiment, but it is preferable to, for example, coat and dry a clay coating layer coating liquid containing an inorganic pigment and a binder as needed on one side of the paper substrate, then coat and dry a resin layer coating liquid containing a water-dispersible polymer, and coat and dry a pigment coating layer coating liquid containing a pigment and a binder on the other side of the paper substrate to form the base paper, and then perform a calendering treatment under the above conditions. Note that, as long as the base paper for metallized paper of this embodiment can be obtained, after forming a pigment coating layer on one side of the paper substrate, a clay coating layer and a resin layer may be formed on the other side of the paper substrate as needed. Each layer can be formed by coating as described above.
[0076] [Metallic paper] The metallized paper of this embodiment has a resin layer on one side of a paper substrate and a pigment coating layer on the other side of a base paper for metallized paper, and the metallized paper has a metallized layer on the resin layer, and the pigment coating layer has a pigment content of 50% by mass or more and 85% by mass or less, and the side with the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The metallized paper of this embodiment has excellent printability and processability in automatic packaging. Note that the Oken smoothness and dynamic friction coefficient against stainless steel of the side with the pigment coating layer of the metallized paper do not change even if a metallized layer is provided on the resin layer of the base paper for metallized paper.
[0077] The paper substrate used in the metallized paper of this embodiment can be any of the paper substrates exemplified for the base paper for metallized paper described above. The resin layer provided on one side of the paper substrate can also be any of the resin layers exemplified for the base paper for metallized paper described above. The pigment coating layer provided on the other side of the paper substrate can also be any of the pigment coating layers exemplified for the base paper for metallized paper described above.
[0078] <Vapour-deposited layer> The metallized paper of this embodiment has a metallized layer on the resin layer of the base paper for metallized paper. The metallized layer is at least one of a layer made of metal and a layer made of ceramic. That is, the metallized layer may be a layer made of metal, a layer made of ceramic, or a laminate of a metal layer and a ceramic layer. When the metallized layer is a laminate of a metal layer and a ceramic layer, the metal layer may be on the resin layer side of the base paper for metallized paper, or the ceramic layer may be on the resin layer side of the base paper for metallized paper, and there are no particular restrictions.
[0079] The vapor-deposited layer may be a layer made of a metal, a layer made of a ceramic, or a laminate thereof, but is preferably a layer made of a metal. When the vapor-deposited layer is a layer made of a metal, specific examples of the metal include aluminum and titanium. When the vapor-deposited layer is a layer made of a ceramic, specific examples of the ceramic include silicon oxide, titanium oxide, aluminum oxide, and diamond-like carbon. These may be used alone or in combination of two or more.
[0080] Among these, the vapor deposition layer is preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, silicon oxide, and diamond-like carbon, and from the viewpoint of ease of production, it is more preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, and diamond-like carbon, and even more preferably a layer made of one or more materials selected from the group consisting of aluminum and aluminum oxide.
[0081] (Thickness) The thickness of the vapor-deposited layer is preferably 1 nm or more, more preferably 2 nm or more, and even more preferably 3 nm or more, and preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 100 nm or less. From the viewpoint of barrier properties, the thickness of the vapor-deposited layer is preferably 10 nm or more, more preferably 15 nm or more, and preferably 80 nm or less, and even more preferably 70 nm. From the viewpoints of adhesion to other layers and cost, the thickness of the vapor-deposited layer is preferably 4 nm or more, more preferably 5 nm or more, and preferably 100 nm or less, more preferably 70 nm or less, and even more preferably 60 nm or less.
[0082] <Heat seal layer> The metallized paper of this embodiment preferably has a heat seal layer on the metallized layer. The heat seal layer is a layer that melts and adheres by heating, ultrasonic waves, or the like. Methods for forming the heat seal layer include coating a thermoplastic resin solution or thermoplastic resin dispersion and drying it, and extrusion lamination. Among these, coating a thermoplastic resin solution or thermoplastic resin dispersion and drying it is preferred. The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves the thermoplastic resin, a dispersion using an organic solvent that disperses the thermoplastic resin, or a dispersion using an aqueous medium. From the standpoints of coatability and environmental impact, a dispersion using an aqueous medium is preferred.
[0083] (thermoplastic resin) Thermoplastic resins suitable for dispersions using aqueous media may be either natural resins or synthetic resins, and examples thereof include starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, acrylic resins, ionomer resins, maleic acid resins, urethane resins, polyester resins, styrene-butadiene resins, vinyl chloride resins, and polyolefin resins. More specifically, examples of acrylic resins include acrylic resins copolymerized with (meth)acrylic acid and its alkyl ester or styrene as monomer components, styrene-maleic acid resins, styrene-acrylic acid-maleic acid resins, water-soluble polyurethane resins, and water-soluble polyester resins. Preferred examples of ionomer resins include ethylene-acrylic acid copolymer ionomers and ethylene-methacrylic acid ionomers. Here, ionomers are polymers neutralized with cations, and the cations include metal ions and ammonium ions (NH4 + ), and organic ammonium ions. Metal ions include lithium ions (Li + ), sodium ions (Na + ), potassium ions (K + ), magnesium ions (Mg 2+ ), calcium ions (Ca 2+ ), alkaline earth metal ions such as zinc ions (Zn 2+ ), copper ions (Cu 2+ Among these, sodium ions are preferred as metal ions from the viewpoint of availability. Among these, from the viewpoints of the stability of the coating liquid and the solvent resistance of the coating layer, the thermoplastic resin is preferably one or more selected from the group consisting of starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, ionomer resins, acrylic resins, polyolefin resins, and maleic acid resins, more preferably one or more selected from the group consisting of starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer resins, acrylic resins, polyolefin resins, and maleic acid resins, even more preferably at least one selected from starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer resins, acrylic resins, and polyolefin resins, even more preferably one or more selected from the group consisting of polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer resins, and polyolefin resins, and even more preferably one or more selected from the group consisting of ionomer resins and polyolefin resins.
[0084] Examples of methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used.
[0085] The coating amount of the heat seal layer is not particularly limited, but from the viewpoint of ensuring sufficient heat sealability, it is preferably 0.5 g / m 2 More preferably, 1 g / m 2 More preferably, 1.5 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 15 g / m 2 Less than 10 g / m, more preferably 2 Less than 7 g / m, more preferably 2 or less, even more preferably 5 g / m 2 The following is the result.
[0086] <Overcoat layer> The metallized paper of this embodiment may have an overcoat layer between the metallized layer and the heat seal layer. The overcoat layer is a layer for protecting the metallized layer. The metallized paper of this embodiment has a certain level of barrier property due to the metallized layer, but by having an overcoat layer on the metallized layer, the oxygen barrier property can be further improved. In addition, the metallized layer is less likely to be damaged by processing such as bending, and even if it is damaged, the overcoat layer can ensure the oxygen barrier property, allowing the excellent oxygen barrier property to be maintained.
[0087] The overcoat layer is not particularly limited and may contain an organic compound, an inorganic compound, or both. That is, the overcoat layer may be an organic layer, an inorganic layer, or an organic-inorganic hybrid layer. Examples of organic compounds include vinyl alcohol-based resins such as polyvinyl alcohol, polyurethane-based resins, (meth)acryloyl compounds, and reaction products of (meth)acryloyl compounds. Examples of inorganic compounds include oxides of silicon, aluminum, and the like.
[0088] Among these, the overcoat layer is preferably one of the resins exemplified as being contained in the resin layer of the base paper for metallized paper, more preferably contains at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins, even more preferably is capable of being prepared into one or more resins selected from the group consisting of polyurethane resin dispersions and emulsions, even more preferably is capable of being prepared into a polyurethane resin dispersion or emulsion, and even more preferably is capable of being prepared into a polyurethane resin dispersion.
[0089] The water-dispersible polyurethane resin or water-dispersible polyester resin that can be contained in the overcoat layer may be the same type as or a different type from the resin contained in the resin layer of the base paper for metallized paper described above, but it is preferable that they are the same type. Furthermore, the synthetic products or commercially available products listed as usable for the resin layer of the base paper for metallized paper may also be used.
[0090] The content of the water-dispersible polyurethane resin or water-dispersible polyester resin in the overcoat layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 99% by mass or more, and the upper limit is not particularly limited, but is 100% by mass.
[0091] The overcoat layer may contain other resins or additives as long as the effects of the present invention are not impaired. Examples of additives include surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and release agents. When the polyurethane resin is used as an aqueous dispersion, it is preferable to use a dispersant to disperse the polyurethane resin in an aqueous medium and obtain a uniform overcoat layer film.
[0092] The coating amount of the overcoat layer is preferably 0.1 g / m in terms of solid content from the viewpoint of protecting the vapor deposition layer. 2 More preferably, 0.2 g / m 2 More preferably, 0.3 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 10 g / m 2 Less than 7g / m, more preferably 2 or less, more preferably 5 g / m 2 The following is the result.
[0093] From the viewpoint of protecting the vapor-deposited layer, the thickness of the overcoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more, and from the viewpoint of recyclability of the vapor-deposited paper, the thickness is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 4 μm or less.
[0094] The method for forming the overcoat layer is not particularly limited, but it is preferable to form the overcoat layer by applying an aqueous medium of an organic compound or inorganic compound that constitutes the overcoat layer and drying it.
[0095] In the metallized paper of this embodiment, the overcoat layer may be the outermost layer, but even if the overcoat layer is the outermost layer, it does not impair the design of the glossy metallized layer.
[0096] [Metal-deposited paper manufacturing method] Although there are no limitations on the method for producing the metal-deposited paper of this embodiment, it is preferable to include the steps of forming a metal-deposited layer by vapor-depositing at least one of metal and ceramic on the resin layer-covered surface of a base paper for metal-deposited paper, which has a clay coating layer and a resin layer, in that order, as needed, on one surface of a paper substrate, and applying a coating liquid for a heat-sealing layer onto the metal-deposited layer and drying it to form a heat-sealing layer. In this case, an overcoat layer may be formed on the metal-deposited layer by coating before forming the heat-sealing layer.
[0097] The preferred method for depositing metal or ceramic is to vacuum-deposit the metal or ceramic directly onto the surface of the resin layer of the base paper for metallized paper.
[0098] From the viewpoint of efficiently protecting the vapor-deposited layer and enhancing the barrier properties, the overcoat layer is preferably formed directly on the vapor-deposited layer. The overcoat layer is preferably formed by applying a liquid for the overcoat layer and drying it. By applying a coating liquid for the overcoat layer to form the overcoat layer, a relatively thin overcoat layer of 10 μm or less can be formed.
[0099] The coating liquid for the overcoat layer used here may be an aqueous medium for an organic compound or an inorganic compound that constitutes the overcoat layer. Among these, a solution using an organic solvent that dissolves a polyurethane resin, a dispersion using an organic solvent that disperses a polyurethane resin, or a dispersion using an aqueous medium is preferred, and from the viewpoints of coatability and environmental load, a dispersion using an aqueous medium is more preferred.
[0100] Examples of methods for applying the coating liquid for the overcoat layer include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used. The coated metal-deposited paper coated with the coating liquid for the overcoat layer is dried to remove the organic solvent or aqueous medium, thereby obtaining a metal-deposited paper having an overcoat layer on the metal-deposited layer.
[0101] A heat seal layer containing a thermoplastic resin can be formed on the vapor deposition layer or the overcoat layer. Methods for forming the heat seal layer include coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it, and extrusion lamination. Among these, coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it is preferred.
[0102] The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves the thermoplastic resin, a dispersion using an organic solvent that disperses the thermoplastic resin, or a dispersion using an aqueous medium, and from the standpoints of coatability and environmental impact, a dispersion using an aqueous medium is preferred.
[0103] Examples of methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used.
[0104] The coated metallized paper coated with a thermoplastic resin solution or thermoplastic resin dispersion can be dried to remove the organic solvent or aqueous medium, thereby obtaining a metallized paper having a heat seal layer on the metallized layer or overcoat layer.
[0105] <Physical properties of metallized paper> (Thickness) The thickness of the metallized paper is preferably 20 μm or more, more preferably 50 μm or more, and preferably 200 μm or less, more preferably 150 μm or less. The thickness of the metallized paper is measured in accordance with JIS P 8118:2014.
[0106] (oxygen permeability) The oxygen permeability of the metallized paper at 23°C and 50% RH is preferably 1.5 mL / (m 2 ·day·atm) or less, more preferably 1.0mL / (m 2 ·day·atm), and its lower limit is 0 mL / (m 2 The oxygen permeability of the metallized paper is measured in accordance with JIS K 7126-2:2006, specifically by the method described in the examples.
[0107] (Water vapor permeability) The water vapor permeability of the metallized paper at 40°C and 90% RH is preferably 1.0 g / (m 2 ·day) or less, more preferably 0.7g / (m 2 ·day) or less, and the lower limit is 0g / (m 2 The water vapor permeability of the metallized paper is measured in accordance with JIS K 7129-2:2019, specifically by the method described in the examples.
[0108] Taking advantage of the excellent printability and processability, as well as the gas barrier properties, the metallized paper of this embodiment can be suitably used as a packaging material, particularly as a packaging bag, for foods such as coffee, confectionery, and milk, as well as pharmaceuticals, medical supplies, and electronic components.
[0109] [Packaging bag] A packaging bag according to another embodiment of the present disclosure is a packaging bag made using the above-mentioned metallized paper. Examples of packaging bags include a standing pouch type, a side seal type, a two-sided seal type, a three-sided seal type, a four-sided seal type, an envelope seal type, a palm seal type (pillow seal type), a pleated seal type, a flat bottom seal type, a square bottom seal type, and a gusset type. The packaging bag of the present embodiment may be formed by folding one of the above-mentioned metal-deposited papers having a heat seal layer or by overlapping two sheets of the metal-deposited paper so that the heat seal layers face each other, and then heat-sealing the peripheral edges of the paper to form the above-mentioned shape, or by folding one of the above-mentioned metal-deposited papers or by overlapping two sheets of the metal-deposited paper and then bonding the peripheral edges of the paper with an adhesive to form the above-mentioned shape.
[0110] The metallized paper of this embodiment may be used for purposes other than packaging bags, such as flexible packaging materials such as lids and labels; liquid containers such as milk cartons (hereinafter also referred to as liquid paper containers); packaging containers such as cups, trays, dishes, lids and laminated tubes; etc. In this case, the contents to be packaged may be liquids, solids (granular materials, powdery materials, etc.), or gels. [Example]
[0111] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Furthermore, unless otherwise specified, "%" and "parts" represent "% by mass" and "parts by mass," respectively. Furthermore, the operations of the examples and comparative examples were carried out at room temperature (20-25°C) and normal humidity (40-50% RH) unless otherwise specified.
[0112] [Measurement and Evaluation] The metallized paper base paper, metallized paper (packaging material), and packaging bags according to the examples and comparative examples were analyzed and evaluated as follows.
[0113] <Base paper for metallized paper> (Oken type smoothness) The Oken smoothness of the surface having the pigment coating layer was measured in accordance with JIS P 8155:2010.
[0114] (Kinematic friction coefficient against stainless steel) The coefficient of dynamic friction of the surface having the pigment coating layer against stainless steel was measured in accordance with JIS P 8147:2010 by fixing a stainless steel plate to the sled side and placing the test piece on the table side so that the surface having the pigment coating layer was in contact with the stainless steel.
[0115] <Metal-deposited paper> (oxygen permeability) The oxygen permeability of the metallized paper was measured using an oxygen permeability measuring device (trade name "OX-TRAN2 / 22" manufactured by MOCON) under conditions of a temperature of 23°C and a relative humidity of 50%. Specifically, an isocyanate-based adhesive (manufactured by DIC Corporation, a mixture of 10 parts by mass of Dickdry LX-500 and 1 part by mass of Dickdry KW-75) was applied at a rate of 5 g / m2 to the surface of the heat seal layer of the metallized paper obtained in the examples and comparative examples. 2 After coating, a 20 μm thick CPP film (GP-32, manufactured by Hokuetsu Chemicals Co., Ltd.) was attached to form a laminate sheet. The oxygen permeability of the laminate sheet was measured at a temperature of 23°C and a relative humidity of 50% in accordance with JIS K7126-2:2006. The lower the oxygen permeability value, the better the oxygen barrier property.
[0116] (Water vapor permeability) The water vapor permeability of metallized paper was measured in accordance with JIS Z 7129-2:2019 (temperature 40°C ± 0.5°C, relative humidity 90% ± 2%) by positioning the overcoat layer or metallized layer of the metallized paper on the inner side (low humidity side). The lower the water vapor permeability value, the better the water vapor barrier property.
[0117] (printability) Test printing was carried out in four colors using a gravure printing machine, and the print density was evaluated using a Gretag Macbeth portable reflection densitometer RD-19A. A: Print density is 1.0 or higher for all four colors B: Print density is less than 1.0 for one or more colors, but white spaces are not noticeable C: Print density is less than 1.0 for one or more colors, and white spots are noticeable
[0118] (Processability) <Cracks and scrapes in the pigment coating layer> Using a horizontal pillow packaging machine (manufactured by Fujikikai Co., Ltd., product name "α8 Series FW3410"), empty bags measuring 150 mm in width and 250 mm in length were continuously produced at a speed of 60 bags / minute without any contents inside, and the condition of the pigment coating layer of the resulting empty bags was evaluated according to the following criteria. A: There are no cracks or chips. B: There are cracks and chips, but they are barely noticeable. C: Cracks and chipping are present and noticeable.
[0119] <Transportability in automatic packaging machines> Using a horizontal pillow packaging machine (manufactured by Fujikikai Co., Ltd., product name "α8 Series FW3410"), empty bags measuring 150 mm wide and 250 mm long were continuously produced at a speed of 60 bags per minute without any contents inside. The transportability of the packaging material unwound from the reel before being made into packaging bags was evaluated according to the following criteria. A: The packaging material is pulled smoothly and does not meander. B: The packaging catches slightly, but does not meander. C: The packaging material cannot be pulled continuously or it meanders.
[0120] <Packaging bag> (exterior) The appearance of the empty packaging bags produced in the above-mentioned evaluation of processability was evaluated according to the following criteria. A: The bag is not distorted and there are no seal defects. B: The bag is slightly warped, but the seal is not faulty. C: The bag is significantly distorted or a seal defect has occurred.
[0121] (gas barrier properties) The empty packaging bags produced for the above-mentioned evaluation of processability were measured using an oxygen permeability measuring device (manufactured by MOCON under the trade name "OX-TRAN2 / 22") at a temperature of 23°C and a relative humidity of 50%, and evaluated according to the following criteria. Note that "pkg" stands for "package." A: Oxygen permeability is less than 0.1 mL / (day·pkg·0.2 atm) B: Oxygen permeability is 0.1 mL / (day·pkg·0.2 atm) or more and less than 1 mL / (day·pkg·0.2 atm) C: Oxygen permeability is 1mL / (day·pkg·0.2atm) or more
[0122] Example 1 <Preparation of base paper for metallized paper> A coating solution for the clay coating layer was prepared by mixing 70 parts of kaolin (Imerys' product name "Contour Xtreme", aspect ratio 33, average particle size d50: 0.26 μm) and 30 parts (solids) of a styrene-acrylic copolymer aqueous dispersion (BASF's product name "ACRONAL S504"). 2 , thickness 60μm, density 0.83g / cm 3 The clay coating layer coating solution was applied to the glossy surface of the glass substrate (12 g / m2, Stockigt sizing degree (glossy surface) 9 seconds, Oken smoothness (glossy surface) 430 seconds) using a Mayer bar, and dried at 120°C for 1 minute to form a clay coating layer (12 g / m2). 2 Next, a 25 μm thick film with an oxygen permeability (23° C., 50% RH) of 2.0 mL / (m 2 The resin layer coating solution containing 100 parts of an aqueous dispersion of a polyurethane resin binder (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content concentration 30%) was diluted with water to a solid content concentration of 10%, and then coated with a Mayer bar and dried at 120°C for 1 minute to form a resin layer (1 g / m 2 , thickness 1 μm) was formed. Next, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added to an aqueous solution containing 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd.) as a dispersant per 100 parts of kaolin to be dispersed, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 25 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as binders per 70 parts (solids) of pigment, to prepare Coating Solution A for the pigment coating layer, which had a final solids concentration of 60%. This was applied to the side opposite the resin layer in a concentration of 10 g / m2 in terms of solids. 2 After coating using a Mayer bar so that the coating was as shown above, the paper was dried for 1 minute in a 120°C air dryer. Finally, a linear pressure of 90 kg / cm was applied, with a chilled roll in contact with the resin layer coated surface and a cotton roll in contact with the pigment layer coated surface. The rolls were heated to 40°C and a 12-stage supercalendering treatment was carried out to obtain base paper for metallized paper (thickness 65 μm, smoothness of the resin layer side: 7000 sec, smoothness of the reverse pigment coating side: 2400 sec, dynamic friction coefficient of the pigment coating side against stainless steel: 0.188). The obtained base paper for metallized paper was subjected to the above-mentioned analyses and evaluations. The results are shown in Table 1. <Preparation of metallized paper> An aluminum vapor deposition layer (50 nm thick) was formed on the resin layer of the base paper for metallized paper using a batch-type vacuum deposition device. Next, an aqueous dispersion of ethylene-methacrylic acid copolymer sodium salt (active ingredient 35% by mass, trade name "Chemipearl S-300" manufactured by Mitsui Chemicals, Inc.) was diluted with water to an active ingredient content of 20% by mass to prepare a coating solution for the heat-seal layer. This was applied with a Mayer bar and dried at 120°C for 1 minute to form a heat-seal layer (3 g / m 2 ) was formed to obtain metallized paper. The obtained metallized paper was subjected to the above-mentioned analysis and evaluation. The results are shown in Table 1.
[0123] Example 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that Coating Solution B for pigment coating layer was used, with the blending amounts of 80 parts pigment, 5 parts oxidized starch, and 15 parts by mass of styrene-butadiene copolymer latex being changed from Coating Solution A for pigment coating layer in Example 1.
[0124] Example 3 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that Coating Solution C for pigment coating layer was used, with the blending amounts of pigment, oxidized starch, and styrene-butadiene copolymer latex changed from Coating Solution A for pigment coating layer in Example 1 to 60 parts by mass.
[0125] Example 4 To an aqueous solution containing 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") as a dispersant per 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 15 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as binders relative to 80 parts (solids) of pigment, to prepare Coating Solution D for the pigment coating layer with a final solids concentration of 60%. 2 to 10g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that the thickness was changed to 3.8 μm.
[0126] Example 5 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that instead of using aluminum as the deposition source, a mixture of aluminum and oxygen was vacuum-deposited, and the deposited layer was made of alumina (AlOx) and had a thickness of 20 nm.
[0127] Example 6 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the deposition source was changed from aluminum to a silica (SiOx) deposition layer using electron beam deposition, with a thickness of 20 nm.
[0128] Example 7 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that chemical vapor deposition was performed using acetylene instead of aluminum as the deposition source, and the deposited layer was made of diamond-like carbon (DLC) and had a thickness of 20 nm.
[0129] Example 8 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the coating liquid for the heat seal layer was changed to a polyolefin dispersion (active content 43 mass%, product name "Rhobarr 320" manufactured by Dow Chemical Japan Co., Ltd.).
[0130] Example 9 After aluminum deposition, the oxygen permeability (23°C, 50% RH) of a 25 μm thick film was 2.0 mL / (m 2 An overcoat layer coating solution containing 100 parts by mass of an aqueous dispersion of a polyurethane resin binder (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content concentration 30%) was applied using a Mayer bar and dried at 120°C for 1 minute to form an overcoat layer (0.5 g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that a 0.5 μm thick film (0.5 μm thick) was formed.
[0131] Example 10 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 stages to 6 stages.
[0132] Example 11 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 to 2.
[0133] Example 12 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the resin layer coating liquid was changed to a resin layer coating liquid containing 100 parts of polyester resin (trade name "Elitel KT-8803" manufactured by Unitika Ltd., acid value 8 mg KOH / g, hydroxyl value 3 mg KOH / g, glass transition temperature 65°C). The results of Examples 1 to 12 are shown in Table 1 below.
[0134] [Table 1]
[0135] Comparative Example 1 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that a pigment coating layer was not formed.
[0136] Comparative Example 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Comparative Example 1, except that the 12-stage supercalendering was not performed.
[0137] Comparative Example 3 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that a resin coating solution containing 100 parts by mass (solid content) of a styrene-(meth)acrylic resin (product name "ACRONAL S504" manufactured by BASF) was used instead of coating solution A for the pigment coating layer.
[0138] Comparative Example 4 A pigment slurry was prepared by adding 30 parts of fine kaolin (BASF's Milagros J), 40 parts of light calcium carbonate (Okutama Kogyo Co., Ltd.'s TP-123CS), and 30 parts of heavy calcium carbonate (Bihoku Funka Kogyo Co., Ltd.'s Hydrocarb 90) to an aqueous solution containing 0.1 parts of sodium polyacrylate (Toagosei Co., Ltd.'s Aron T-50) as a dispersant per 100 parts of kaolin to be dispersed, and dispersing the mixture using a Coles disperser. A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that 5 parts (solids) of oxidized starch (Oji Ace A, Oji Cornstarch Co., Ltd.'s Oji Ace A) and 75 parts (solids) of styrene-butadiene copolymer latex (JSR Corporation's OJ1000H) were added as binders per 20 parts (solids) of pigment to this pigment slurry.
[0139] Comparative Example 5 To an aqueous solution containing 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") as a dispersant per 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (manufactured by Oji Cornstarch Co., Ltd. under the trade name "Oji Ace A") and 5 parts (solids) of styrene-butadiene copolymer latex (manufactured by JSR Corporation under the trade name "OJ1000H") were added as binders per 90 parts (solids) of pigment, to prepare Coating Solution F for the pigment coating layer having a final solids concentration of 60%. Except for this, a base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4. The results of Comparative Examples 1 to 5 are shown in Table 2.
[0140] [Table 2]
[0141] The metallized paper produced using the base paper for metallized paper of the examples was excellent in printability and processability. In addition, the metallized paper produced using the base paper for metallized paper of the examples also produced packaging bags with good appearance.
Claims
1. A base paper for metallized paper having a resin layer on one side of a paper substrate, the base paper being used to form a metallized layer on the resin layer, A pigment coating layer is provided on the other side of the paper base material, The content of the pigment in the pigment coating layer is 50% by mass or more and 85% by mass or less, The surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less.
2. The base paper for metallized paper according to claim 1 , further comprising a clay coating layer between the paper substrate and the resin layer.
3. 3. The base paper for metallized paper according to claim 1, wherein the resin layer comprises at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.
4. A metal-deposited paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate, the metal-deposited paper having a metal-deposited layer on the resin layer, The content of the pigment in the pigment coating layer is 50% by mass or more and 85% by mass or less, The surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less.
5. The metal-deposited paper according to claim 4 , further comprising a heat seal layer on the metal-deposited layer.
6. The metal-deposited paper according to claim 5 , further comprising an overcoat layer between the metal-deposited layer and the heat seal layer.
7. The metallized paper according to claim 4 or 5, further comprising a clay coating layer between the paper substrate and the resin layer.
8. 6. The metallized paper according to claim 4, wherein the resin layer contains at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.
9. A packaging bag made using the metallized paper according to claim 4 or 5.
Citation Information
Patent Citations
Paper for metal vacuum deposited label and production thereof
JP1989221593A
Biodegradable paper sheet and paper container
JP2003013391A
Antenna paper sheet, sheet-like antenna using the same, and RFID tag
JP2009239817A
Support for inkjet recording material and its manufacturing method
JP2010030231A
Base paper for container and production method thereof
JP2015030955A