Negative electrode active material layer, and solid-state battery and method for manufacturing the same
By integrating silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes with controlled porosity and cracks, the negative electrode active material layer in solid-state batteries manages expansion during charging, maintaining performance and reducing resistance.
Patent Information
- Application Number
- JP2023069406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Existing solid-state batteries face challenges in suppressing the expansion of the negative electrode active material layer during charging without compromising battery performance.
Incorporating silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes into the negative electrode active material layer, with predetermined cracks and controlled porosity, and densifying the layer through roll pressing at a specific pressure to manage volume changes.
The solution effectively absorbs volume changes during charging, maintaining battery performance by generating cracks that allow for expansion while minimizing thickness expansion, thus enhancing the battery's structural integrity and reducing internal resistance.
Smart Images

Figure 2024155039000003 
Figure 2024155039000001 
Figure 2024155039000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode active material layer, a solid-state battery, and a method for producing the same. [Background technology]
[0002] A solid-state battery is a battery having a solid electrolyte layer between a positive electrode active material layer and a negative electrode active material layer, and has the advantage of being easy to simplify safety devices. Among solid-state batteries, solid-state lithium-ion batteries have been attracting attention because they can provide high energy density by utilizing a battery reaction involving the movement of lithium ions.
[0003] Regarding such solid-state batteries, Patent Documents 1 and 2 disclose an all-solid-state battery in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order, the negative electrode layer contains a negative electrode active material having a silicon clathrate II type crystal phase, and the all-solid-state battery is applied with a confining pressure of 0 MPa or more and less than 5 MPa in the lamination direction. The all-solid-state battery of Patent Document 1 is characterized in that, when the capacity ratio of the negative electrode capacity to the positive electrode capacity is A, the capacity ratio A is 2.5 or more and 4.8 or less, and the all-solid-state battery of Patent Document 2 is characterized in that the specific surface area of the negative electrode active material is 8 m 2 / g or more 17m 2 / g or less. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-92723 [Patent Document 2] Patent Publication No. 2022-92725 Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure provides a negative electrode active material layer that can suppress expansion in the thickness direction during charging without sacrificing battery performance. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by the following means, and have completed the present disclosure. That is, the present disclosure is as follows: <Aspect 1> Silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes, A negative electrode active material layer having, on average, one or more in-plane cracks having a length of 10 μm or more in a region of 50 μm in the thickness direction × 50 μm in the width direction in a cross section. Aspect 2: The negative electrode active material layer according to aspect 1, having a porosity of 7% or less during discharge. Aspect 3: The negative electrode active material layer according to aspect 1 or 2, wherein the content of the multi-walled carbon nanotubes is 8 mass% or more based on the mass of the negative electrode active material layer, the multi-walled carbon nanotubes have a fiber diameter of 100 nm or more, and a fiber length of 5 μm or more. <Aspect 4> The negative electrode active material layer according to any one of aspects 1 to 3, wherein the silicon active material particles are porous silicon active material particles, clathrate silicon active material particles, or porous clathrate silicon active material particles. A solid-state battery comprising the anode active material layer according to any one of Aspects 1 to 4, a solid electrolyte layer, and a cathode active material layer in this order. <Aspect 6> Providing a negative electrode active material layer, and densifying the negative electrode active material layer; Including, The negative electrode active material layer includes at least silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes; and The negative electrode active material layer is densified by a roll press with a linear pressure of 2 t / cm or more. How solid-state batteries are manufactured. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a negative electrode active material layer that can suppress expansion in the thickness direction during charging without sacrificing battery performance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a solid-state battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] 《Negative electrode active material layer》 The negative electrode active material layer of the present invention is Silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes; In the cross section, there is, on average, one or more in-plane cracks having a length of 10 μm or more in an area of 50 μm in the thickness direction × 50 μm in the width direction.
[0010] Here, the above-mentioned cracks may be present either immediately after the preparation of the negative electrode active material layer or after initial charge and discharge. In addition, in the above, the "width direction" means a direction perpendicular to the thickness direction in a thickness direction cross section of the negative electrode active material layer.
[0011] In solid-state batteries using silicon active material particles, the expansion of the silicon active material particles during charging causes the negative electrode active material layer to expand, which in turn causes the entire battery to expand. This expansion can be suppressed by lowering the load applied in the densification stage of the negative electrode active material layer and increasing the porosity of the negative electrode active material layer, but in this case, the performance of the battery, for example, the electrical resistance, can be deteriorated.
[0012] In contrast, in the present invention, by forming predetermined planar cracks in the negative electrode active material layer, it is possible to efficiently absorb the volume change caused by the expansion of the silicon active material particles while maintaining the performance of the battery. In particular, such absorption of the volume change caused by the cracks can be achieved even when the porosity of the negative electrode active material layer is small.
[0013] In order to generate such cracks, for example, a predetermined amount of relatively thick and long carbon nanotubes, i.e., multi-walled carbon nanotubes, can be added to the negative electrode active material layer, and the negative electrode active material layer can be roll-pressed with an appropriate pressure. Specifically, with such multi-walled carbon nanotubes and roll-pressing, the negative electrode active material layer can be subjected to an appropriate springback after roll-pressing to generate such cracks.
[0014] The negative electrode active material layer of the present disclosure may have a porosity of 7% or less, 6% or less, or 5% or less during discharge. This porosity can be calculated by the following formula: Porosity (%)=(1-x / y)×100 x: The total volume of each material obtained by dividing the weight of each material constituting the negative electrode active material layer by the true density of each material y: Apparent volume obtained from the actual dimensions of the negative electrode active material layer
[0015] The negative electrode active material layer may further contain a conductive assistant and a binder, and may also contain other optional components.
[0016] Each component of the present disclosure will be described below.
[0017] Silicon active material particles Any silicon active material particles can be used as the silicon active material particles. Therefore, solid silicon active material particles or porous silicon active material particles can be used as the silicon active material particles. In addition, amorphous silicon active material particles or clathrate silicon active material particles can be used as the silicon active material particles.
[0018] Porous silicon active material particles are silicon active material particles having pores inside the primary particles, and these pores can suppress the expansion and contraction of the negative electrode active material particles during charging and discharging.
[0019] In this regard, for example, the amount of pores having a pore diameter of 100 nm or less in the porous silicon active material particles may be 0.01 cc / g or more, 0.05 cc / g or more, or 0.10 cc / g or more, and may be 0.50 cc / g or less, 0.40 cc / g or less, 0.30 cc / g or less, 0.20 cc / g or less, 0.15 cc / g or less, or 0.10 cc / g or less. The amount of pores having a pore diameter of 100 nm or less is the cumulative pore volume of pores having a pore diameter of 100 nm or less. The cumulative pore volume can be determined, for example, by mercury porosimeter measurement.
[0020] The porous silicon active material particles can be manufactured by any method. Specifically, the porous silicon active material particles can be manufactured by a known method. For example, the porous silicon active material particles can be manufactured by forming alloy particles of silicon and other metals such as magnesium and lithium, and dissolving and removing the other metals from the alloy particles.
[0021] The porous silicon active material particles may be porous clathrate silicon active material particles (porous clathrate silicon active material particles) having a clathrate structure. It is preferable that the porous silicon active material particles have a clathrate structure, since the expansion and contraction of the porous silicon active material particles accompanying the charging and discharging of the battery is further reduced. Whether the porous silicon active material particles have a clathrate structure or not can be easily determined from Raman spectrum, XRD, or the like. The porous silicon active material particles may have an oxide film, or may contain impurities such as carbon.
[0022] The porous clathrate silicon active material particles can be obtained by a known method, for example, by mixing the above-mentioned porous silicon active material particles with a sodium source, such as NaH, and then heat-treating the mixture in a non-oxidizing atmosphere to remove sodium.
[0023] The size of the silicon active material particles is not particularly limited. The median diameter (D50 particle diameter) of the porous silicon active material particles may be, for example, 0.1 μm or more, 0.3 μm or more, or 0.5 μm or more, and may be 50.0 μm or less, 30.0 μm or less, 10.0 μm or less, 5.0 μm or less, 3.0 μm or less, or 1.0 μm or less. The median diameter of the porous silicon active material particles is the particle diameter (D50 diameter) at an integrated value of 50% in the volume-based particle size distribution obtained by a laser diffraction / scattering method.
[0024] <Sulfide solid electrolyte particles> Any sulfide solid electrolyte particles can be used. Specifically, sulfide solid electrolyte particles include, for example, Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5-GeS2. In particular, sulfide solid electrolyte particles, particularly sulfide solid electrolyte particles containing at least Li, S, and P as constituent elements, are preferred because of their high performance. The sulfide solid electrolyte particles may be amorphous or crystalline. Only one type of inorganic solid electrolyte particle may be used alone, or two or more types may be used in combination.
[0025] <Multi-walled carbon nanotubes> Any multi-walled carbon nanotube can be used. Here, a single-walled carbon nanotube is composed of one graphene sheet, whereas a multi-walled carbon nanotube is composed of multiple graphene sheets. The graphene sheets constituting the multi-walled carbon nanotube may be chiral (spiral) type, zigzag type, or armchair type. The multi-walled carbon nanotube in the present disclosure may also be composed of a single type of graphene sheet, or may be composed of multiple types of graphene sheets.
[0026] The content of the multi-walled carbon nanotubes may be 5 mass% or more, 6 mass% or more, 7 mass% or more, or 8 mass% or more, and may be 15 mass% or less, 14 mass% or less, 13 mass% or less, or 12 mass% or less, relative to the mass of the negative electrode active material layer. This mass of the negative electrode active material layer means the solid content.
[0027] The diameter (fiber diameter) of the multi-walled carbon nanotube is not particularly limited, and the average diameter may be, for example, 100 nm or more, 130 nm or more, or 150 nm or more, and may be 1000 nm or less, 500 nm or less, 300 nm or less, or 200 nm or less. The length of the multi-walled carbon nanotube is not particularly limited, and the average length may be, for example, 1000 nm or more, 2000 nm or more, 3000 nm or more, 4000 nm or more, or 5000 nm or more, and may be 20000 nm or less, 15000 nm or less, 12000 nm or less, 10000 nm or less, 9000 nm or less, 8000 nm or less, or 7000 nm or less. Multi-walled carbon nanotubes having an average diameter and an average length in such a range are preferable from the viewpoint of generating an appropriate springback after roll pressing of the negative electrode active material layer, thereby generating cracks.
[0028] The aspect ratio (ratio of average length to average diameter) of the multi-walled carbon nanotubes is not particularly limited and may be, for example, 10 or more, 20 or more, or 30 or more, and may be 1000 or less, 800 or less, 500 or less, 400 or less, 300 or less, 200 or less, 100 or less, 90 or less, 70 or less, or 50 or less.
[0029] The average diameter and average length of multi-walled carbon nanotubes can be determined by measuring the dimensions of 50 or more randomly selected multi-walled carbon nanotubes using a scanning electron microscope (SEM), transmission electron microscope (TEM), etc., and taking the arithmetic mean.
[0030] When single-walled carbon nanotubes are used in combination with multi-walled carbon nanotubes, the mass ratio of multi-walled carbon nanotubes to the total carbon nanotubes may be, for example, 1 mass% or more, 3 mass% or more, 5 mass% or more, 10 mass% or more, 20 mass% or more, 30 mass% or more, 40 mass% or more, 50 mass% or more, 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 95 mass% or more, or 99 mass% or more. Preferably, only multi-walled carbon nanotubes can be used as the carbon nanotubes.
[0031] <Conductive assistant> The conductive assistant is not particularly limited, and examples thereof include carbon materials such as VGCF (Vapor Grown Carbon Fiber), carbon nanofibers, and carbon black such as acetylene black and ketjen black, as well as metal materials.
[0032] <binder> The binder is not particularly limited, and may be, for example, polyvinylidene fluoride (PVDF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), styrene butadiene rubber (SBR), or a derivative thereof, or a combination thereof. As a derivative thereof, for example, polyvinylidene fluoride-hexafluoropropylene copolymer may be used.
[0033] Other Ingredients As the other component, for example, a conductive agent other than carbon nanotubes can be used. Such a conductive agent is not particularly limited, and for example,
[0034] 《Solid-state battery》 The solid-state battery of the present disclosure has the above-mentioned negative electrode active material layer, solid electrolyte layer, and positive electrode active material layer in this order.
[0035] The solid-state battery of the present disclosure may have an anode current collector layer on the side of the anode active material layer opposite the solid electrolyte layer, and may have a cathode current collector layer on the side of the cathode active material layer opposite the solid electrolyte layer. That is, the solid-state battery of the present disclosure may have an anode current collector layer, an anode active material layer, a solid electrolyte layer, a cathode active material layer, and a cathode current collector layer in this order.
[0036] Furthermore, the solid-state battery of the present disclosure may be restrained by restraining members such as end plates from both sides in the stacking direction of each of the above-mentioned layers.
[0037] <Solid electrolyte layer> The solid electrolyte layer may contain a solid electrolyte.
[0038] The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in a lithium ion battery can be used. For example, the solid electrolyte may be, but is not limited to, a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer electrolyte. In addition, one type of these solid electrolytes may be used alone, or two or more types may be used in combination.
[0039] As the sulfide solid electrolyte, for example, the sulfide solid electrolyte particles mentioned in relation to the negative electrode active material layer can be used.
[0040] As an example of an oxide solid electrolyte, Li7La3Zr2O 12、 Li 7-x La3Zr 1-x Nb x O 12、 Li 7-3x La3Zr2Al x O 12 , Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4, or Li 3+x PO 4-x N x(LiPON), etc., but are not limited to these. These may be amorphous or crystalline.
[0041] Examples of the polymer electrolyte include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.
[0042] <Cathode active material layer> The positive electrode active material layer used in the solid-state battery of the present disclosure includes a positive electrode active material, and may further include an electrolyte, a conductive assistant, a binder, etc. In addition, the positive electrode active material layer may also include various other additives. The contents of the positive electrode active material, electrolyte, conductive assistant, binder, etc. in the positive electrode active material layer may be appropriately determined according to the desired battery performance.
[0043] As the positive electrode active material, a known positive electrode active material, particularly a positive electrode active material used in lithium ion batteries, can be used. For example, the positive electrode active material can be selected from metal oxides containing lithium and at least one transition metal selected from manganese, cobalt, nickel, and titanium, such as lithium cobalt oxide, lithium nickel oxide, lithium manganate, or lithium nickel cobalt manganate (NCM), a different element-substituted Li-Mn spinel, lithium titanate, lithium metal phosphate, or a combination thereof.
[0044] The electrolyte that can be contained in the positive electrode active material layer may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination thereof.
[0045] <Negative electrode current collector layer> The negative electrode layer used in the solid-state battery of the present disclosure may include a negative electrode current collector layer in contact with the negative electrode active material layer. Any of the negative electrode current collector layers commonly used for battery negative electrode current collector layers can be used. The negative electrode current collector layer may be in the form of a foil, a plate, a mesh, a punched metal, a porous, or a foam. The negative electrode current collector layer may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, metal foil is excellent in terms of ease of handling. The negative electrode current collector layer may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector layer include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector layer may contain at least one metal selected from Cu, Ni, and stainless steel.
[0046] <Positive electrode current collector layer> The positive electrode collector layer used in the solid-state battery of the present disclosure can be any of those commonly used as a positive electrode collector layer for secondary batteries. The positive electrode collector layer may be in the form of a foil, a plate, a mesh, a punched metal, a porous, or a foam. The positive electrode collector layer may be a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector layer may be made of a plurality of metal foils. Examples of metals constituting the positive electrode collector layer include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel.
[0047] <<Method for manufacturing solid-state batteries>> The disclosed method of making a solid-state battery includes: Providing a negative electrode active material layer; and densifying the negative electrode active material layer; Including, The negative electrode active material layer includes at least silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes; and The negative electrode active material layer is densified by roll pressing at a linear pressure of 2 t / cm or more.
[0048] In particular, the methods of the present disclosure may include providing an anode active material layer, providing a solid electrolyte layer, and providing a cathode active material layer.
[0049] Each step of the method of the present disclosure and the materials used therein will be described below.
[0050] <Providing the negative electrode active material layer> The negative electrode active material layer can be provided by a known method, for example, by applying a slurry for forming the negative electrode active material layer to the negative electrode current collector layer.
[0051] The negative electrode active material layer forming slurry can be obtained by mixing the components constituting the negative electrode active material layer in a dispersion medium. For each of these components, the description regarding the negative electrode active material layer can be referred to.
[0052] The dispersion medium may be, for example, water or various organic solvents, including non-polar organic solvents, polar organic solvents, or a combination thereof.
[0053] Examples of the non-polar organic solvent that can be used include aliphatic hydrocarbons such as hexane and heptane, and aromatic hydrocarbons such as xylene and toluene. Examples of the polar organic solvent that can be used include ketone-based solvents such as diisobutyl ketone, tertiary amine-based solvents such as triethylamine, ether-based solvents such as cyclopentyl methyl ether, thiol-based solvents such as ethane mercaptan, and ester-based solvents such as butyl butyrate.
[0054] The negative electrode active material layer forming slurry can be applied by a known method, such as a doctor blade method, a metal mask printing method, an electrostatic coating method, a dip coating method, a spray coating method, a roll coating method, a gravure coating method, a screen printing method, etc. These methods may be used alone or in combination.
[0055] <Densification of the negative electrode active material layer> The negative electrode active material layer is densified by roll pressing at a linear pressure of 2 t / cm or more.
[0056] The negative electrode active material layer may be densified alone, or simultaneously with other layers. For example, the negative electrode active material layer and the solid electrolyte layer may be densified as a single unit.
[0057] The densification is performed at a linear pressure of 2.0 t / cm or more, 2.5 t / cm or more, 3.0 t / cm or more, 3.5 t / cm or more, 4.0 t / cm or more, or 4.5 t / cm or more. This linear pressure may be 10.0 t / cm or less, 9.0 t / cm or less, 8.0 t / cm or less, 7.0 t / cm or less, 6.0 t / cm or less, or 5.5 t / cm or less. By densifying the negative electrode active material layer containing multi-walled carbon nanotubes at the above linear pressure, the negative electrode active material layer after densification can be appropriately spring-backed, thereby generating the above cracks.
[0058] <Provision of solid electrolyte layer> The solid electrolyte layer can be provided by a known method, for example, by applying a slurry for forming a solid electrolyte layer to a substrate to be transferred, for example, a metal foil such as a stainless steel foil.
[0059] The provided solid electrolyte layer can be laminated and integrated with a negative electrode active material layer and / or a positive electrode active material layer.
[0060] <Providing a positive electrode active material layer> The positive electrode active material layer can be provided by a known method, for example, by applying a positive electrode active material layer forming slurry to the positive electrode current collector layer.
[0061] The slurry for forming the positive electrode active material layer can be obtained by mixing the positive electrode active material, the solid electrolyte, and an optional binder, conductive assistant, etc., in a dispersion medium. As the positive electrode active material and the solid electrolyte, those listed for the positive electrode active material layer can be used. As the silicon active material particles, the sulfide solid electrolyte particles, and the multi-walled carbon nanotubes, those listed for the negative electrode active material layer can be used.
[0062] For the coating method and dispersion medium of the positive electrode active material forming slurry, the description of the negative electrode active material forming slurry can be referred to. EXAMPLES
[0063] The present disclosure will be specifically described with reference to examples and comparative examples, but the present disclosure is not limited thereto.
[0064] The solid-state battery of Example 1 was fabricated as follows.
[0065] (Preparation of negative electrode active material layer) To diisobutyl ketone (2.7 g) as a dispersion medium, multi-walled carbon nanotubes (MWCNT) (0.33 g), silicon active material (1.0 g), sulfide solid electrolyte (1.2 g), and 5 mass% diisobutyl ketone solution of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) (0.8 g (PVDF-HFP: 0.04 g, diisobutyl ketone: 0.76 g)) were added, and the mixture was dispersed for 10 minutes with ultrasonic waves of 40 μm amplitude and 20 kHz frequency to obtain a slurry for forming a negative electrode active material layer. The multi-walled carbon nanotubes (SWCNT) used had an average fiber diameter of about 150 nm and an average fiber length of about 6000 nm.
[0066] The negative electrode active material layer forming slurry obtained as described above was applied to a roughened nickel foil serving as a negative electrode current collector layer using a blade with a gap of 100 μm to obtain a negative electrode active material layer.
[0067] The ratio of the single-walled carbon nanotubes to the total solid content was about 13 mass % (0.33 g / (2.7 g+0.33 g+1.0 g+0.8 g×0.05)). Li2S-P2S5-based glass ceramic was used as the sulfide solid electrolyte.
[0068] The silicon active material is porous clathrate silicon (PC-Si) produced as follows. Specifically, Si powder (Si powder having no voids inside the primary particles) was prepared as the Si source. This Si source and Li metal were weighed out in a molar ratio of Li / Si=4.0 and mixed in a mortar in an Ar atmosphere to obtain an alloy compound. The obtained alloy compound was reacted with ethanol in an Ar atmosphere to obtain silicon having voids inside the primary particles, i.e., porous silicon having a porous structure.
[0069] Next, a NaSi alloy was produced using the porous silicon powder and NaH as a Na source. The NaH used was washed with hexane in advance. The Na source and the Si source were weighed out to a molar ratio of 1.05:1.00, and mixed using a cutter mill. The mixture was heated in a heating furnace under an Ar atmosphere at 400°C for 40 hours to obtain a powdered NaSi alloy.
[0070] The obtained NaSi alloy was heated in an Ar atmosphere at 270°C for 120 hours to remove Na, and porous clathrate silicon having a clathrate II crystal phase was obtained.
[0071] (Preparation of solid electrolyte layer) The above sulfide solid electrolyte (0.4 g) and a 5 mass% heptane solution (0.05 g) of acrylonitrile butadiene rubber (ABR) were added to heptane (0.8 g) as a dispersion medium, and dispersed for 10 minutes with ultrasonic waves of 40 μm amplitude and 20 kHz frequency to obtain a slurry for forming a solid electrolyte layer. The slurry for forming a solid electrolyte layer thus obtained was applied to a stainless steel foil for transfer with a blade with a gap of 50 μm to obtain a solid electrolyte layer.
[0072] (Preparation of Positive Electrode Active Material Layer) NCM (2g), VGCF-H (0.03g), sulfide solid electrolyte (0.3g), and 5 mass% butyl butyrate solution (0.3g) of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) copolymer were added to butyl butyrate (1g) as a dispersion medium, and dispersed for 10 minutes with ultrasonic waves of 40μm amplitude and 20kHz frequency to obtain a positive electrode active material layer forming slurry. The positive electrode active material layer forming slurry thus obtained was applied to an aluminum foil as a positive electrode current collector layer with a blade having a gap of 100μm to obtain a positive electrode active material layer.
[0073] (Fabrication of solid-state batteries) A solid electrolyte layer was superposed on the negative electrode active material layer, and roll-pressed at room temperature with a linear pressure of 5 t / cm to obtain a negative electrode laminate 20 having a negative electrode current collector layer 21, a negative electrode active material layer 22, and a solid electrolyte layer 23 in this order. A solid electrolyte layer was superposed on the positive electrode active material layer, and roll-pressed at 170°C with a linear pressure of 4 t / cm to obtain a positive electrode laminate 10 having a positive electrode current collector layer 11, a positive electrode active material layer 12, and a solid electrolyte layer 13 in this order. Each was cut to a thickness of 1 cm. 2 The solid electrolyte layer 23 of the negative electrode laminate 20 and the solid electrolyte layer 13 of the positive electrode laminate 10 were then overlapped and bonded to obtain a solid battery 100 having a laminate of the negative electrode current collector layer 21, the negative electrode active material layer 22, the solid electrolyte layer 23, the solid electrolyte layer 13, the positive electrode active material layer 12, and the positive electrode current collector layer 11. That is, the obtained battery laminate has a laminate configuration as shown in FIG.
[0074] <evaluation> The solid-state battery of Example 1 obtained as described above was evaluated as follows. The evaluation results are shown in Table 2.
[0075] (Number of cracks and porosity) The number of cracks in the negative electrode active material layer of the obtained battery laminate was evaluated. Specifically, the produced solid-state battery was cut in the stacking direction, and the cut cross section was observed at a magnification of 2000 times using an FE-SEM to count the number of cracks in a range of 40 μm in the stacking direction (thickness direction) × 60 μm in the width direction of the solid-state battery. Three fields of view were observed for each sample, and the average of the three fields of view was taken as the number of cracks. Note that a void that is long in the horizontal direction and has a width of 2 μm or more in the stacking direction of the solid-state battery and an aspect ratio of 5 or more was determined to be a crack. Regardless of the length of the crack, a continuous crack was counted as one crack. In addition, the porosity of the negative electrode active material layer was calculated using the total volume of each material obtained from the weight and true density of each material constituting the negative electrode active material layer, and the apparent volume obtained from the dimensions of the actual negative electrode active material.
[0076] (confining pressure, cell volume, and internal resistance) A solid-state battery prepared different from the one evaluated for the number of cracks and porosity was restrained at a restraining pressure of 5 MPa using a restraining jig, CCCV charged (constant current constant voltage charging) at 1 / 10C to 4.35V, and then CCCV discharged at 1 / 3C to 3.35V. Then, CCCV charged again at 1 / 10C to 4.35V, the restraining pressure was measured, and this was used as the restraining pressure after charging to calculate the increase in the restraining pressure. Then, CCCV discharged at 1 / 3C to 3.35V to measure the cell capacity. Then, CCCV charged again at 1 / 10C to 4.35V, and discharged at 7C, and the internal resistance was calculated from the change in voltage and current value for 10 seconds.
[0077] Examples 2 to 4 and Comparative Examples 1 to 4 Except for changing the conductive assistant used as shown in Tables 1 and 2 below and changing the densification load of the negative electrode active material layer as shown in Table 2, the solid-state batteries of Examples 2 to 4 and Comparative Examples 1 to 4 were obtained and evaluated in the same manner as in Example 1.
[0078] In Table 1, "MWCNT" refers to multi-walled carbon nanotubes with an average fiber diameter of about 150 nm and an average fiber length of about 6000 nm, and "SWCNT" refers to single-walled carbon nanotubes with an average fiber diameter of about 2 nm and an average fiber length of about 5000 nm. In Table 1, "AB" refers to acetylene black with an average particle diameter of 35 nm.
[0079] The outlines and evaluation results of the Examples and Comparative Examples are shown in Tables 1 and 2 below. [Table 1]
[0080] [Table 2]
[0081] From Table 1, it can be seen that the secondary battery of the embodiment having the negative electrode active material layer of the present disclosure, which has, on average, one or more planar cracks with a length of 10 μm or more in a cross-section in an area of 50 μm in the thickness direction × 50 μm in the width direction, can suppress expansion and has low resistance.
[0082] In addition, regarding the number of cracks, the number of cracks was counted in an area of 40 μm in the thickness direction × 60 μm in the width direction this time. Since this area is narrower than 50 μm in the thickness direction × 50 μm in the width direction, even when converted to an area of 50 μm in the thickness direction × 50 μm in the width direction, the number of cracks in the negative electrode active material of the solid-state battery of the example is naturally one or more on average. [Explanation of symbols]
[0083] 10 Positive electrode laminate 11 Positive electrode current collector layer 12 Cathode active material layer 13, 23 Solid electrolyte layer 20 Negative electrode laminate 21 Negative electrode current collector layer 22 Negative electrode active material layer 100 solid state battery
Claims
1. Silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes; A negative electrode active material layer having, on average, one or more in-plane cracks having a length of 10 μm or more in a region of 50 μm in the thickness direction×50 μm in the width direction in a cross section.
2. The negative electrode active material layer according to claim 1 , which has a porosity of 7% or less during discharge.
3. 3. The negative electrode active material layer according to claim 1, wherein the content of the multi-walled carbon nanotubes is 8 mass% or more relative to the mass of the negative electrode active material layer, the fiber diameter of the multi-walled carbon nanotubes is 100 nm or more, and the fiber length of the multi-walled carbon nanotubes is 5 μm or more.
4. The negative electrode active material layer according to claim 1 or 2, wherein the silicon active material particles are porous silicon active material particles, clathrate silicon active material particles, or porous clathrate silicon active material particles.
5. A solid-state battery comprising the anode active material layer according to claim 1 or 2, a solid electrolyte layer, and a cathode active material layer in this order.
6. Providing a negative electrode active material layer; and densifying the negative electrode active material layer; Including, The negative electrode active material layer includes at least silicon active material particles, sulfide solid electrolyte particles, and multi-walled carbon nanotubes; and The negative electrode active material layer is densified by a roll press with a linear pressure of 2 t / cm or more. How solid-state batteries are manufactured.
Citation Information
Patent Citations
Anode active material for secondary battery, conductive composition for secondary battery, anode material including the same, anode structure including the same and secondary battery, and methods for producing the same
JP2016509739A
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158003A
All-solid battery
JP2022092723A
All-solid battery
JP2022092725A
Composite active material for lithium secondary battery and manufacturing method for the same
JP2022190387A