Seamless steel pipe
The seamless steel pipe with controlled chemical composition and oxide inclusions addresses the challenge of high strength and fracture toughness, achieving effective performance in cold regions through a balanced REM/Mg ratio and specific inclusion characteristics.
Patent Information
- Application Number
- JP2023069683
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Existing seamless steel pipes for line pipes do not adequately address high strength and low-temperature fracture toughness requirements, particularly in harsh environments, and existing technologies do not consider CTOD tests for evaluating fracture toughness.
A seamless steel pipe composition with specific chemical elements (C, Si, Mn, P, S, Al, Ti, Mg, REM, N, O, Mo, Nb, Ca, B, Cu, Ni, Cr, V) and controlled oxide inclusions (number density, aspect ratio, and hardness) to achieve high strength and excellent fracture toughness, satisfying the formula REM/Mg ratio of 0.3 to 2.0.
The seamless steel pipe achieves high tensile strength of 531 to 758 MPa with excellent fracture toughness, demonstrated by a CTOD value of 0.25 mm or more at -20°C, suitable for line pipes in cold regions.
Smart Images

Figure 2024155202000001 
Figure 2024155202000002 
Figure 2024155202000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a seamless steel pipe, and more particularly to a seamless steel pipe suitable for use as a line pipe. [Background technology]
[0002] A pipeline is a system that is installed on the ground or seabed to transport natural gas, crude oil, etc. A pipeline that is laid on the seabed is composed of multiple steel pipes (line pipes). A pipeline that is laid on the seabed is further subjected to high pressure from the production fluid passing through it. The pipeline is also subjected to repeated strain from waves and seawater pressure from the outside. Furthermore, in recent years, pipelines are sometimes laid in harsh environments such as low-temperature environments. Therefore, the steel pipes (line pipes) that make up the pipeline are required to have high strength and excellent low-temperature toughness.
[0003] Up to now, techniques for improving the strength and low-temperature toughness of seamless steel pipes for line pipe applications have been proposed in JP-A-2010-242222 (Patent Document 1) and JP-A-2004-124158 (Patent Document 2).
[0004] The seamless steel pipe proposed in Patent Document 1 contains C: 0.03-0.08%, Si: 0.15% or less, Mn: 0.3-2.5%, Al: 0.001-0.10%, Cr: 0.02-1.0%, Ni: 0.02-1.0%, Mo: 0.02-1.2%, Ti: 0.004-0.010%, N: 0.002-0.008%, and further contains one or more of Ca, Mg, and REM in total of 0.0002-0.005%, with the balance being Fe and impurities, and has a wall thickness of 30-50 mm. Patent Document 1 discloses that by containing an appropriate amount of one or more of Ca, Mg, and REM, this seamless steel pipe can obtain excellent low-temperature toughness even in a thick-walled seamless steel pipe.
[0005] The seamless steel pipe proposed in Patent Document 2 contains, by mass%, C: 0.02-0.15%, Si: 0.05-1.0%, Mn: 0.30-2.5%, P: 0.030% or less, S: 0.006% or less, Ti: 0.002-0.017%, Al: 0.001-0.100%, N: 0.008% or less, and O (oxygen): 0.004% or less, with the balance being Fe and impurities. The grain size number specified in JIS G 0551 is less than 7. Furthermore, the number of oxide-based inclusions with a diameter of more than 300 μm that exist in the steel is less than 1 cm. 2 The number of oxide inclusions with diameters of 5 to 300 μm is less than one per cm 2 The number density of oxide-based inclusions per size is limited to 200 or less. Patent Document 2 discloses that excellent low-temperature toughness can be obtained in this seamless steel pipe by limiting the number density of oxide-based inclusions per size. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-242222 A [Patent Document 2] JP 2004-124158 A Summary of the Invention [Problem to be solved by the invention]
[0007] The above Patent Documents 1 and 2 propose techniques for obtaining excellent low-temperature toughness in seamless steel pipes for line pipe applications. However, excellent low-temperature toughness may be obtained by techniques other than those disclosed in the above Patent Documents 1 and 2.
[0008] Recently, a CTOD (Crack Tip Opening Displacement) test has been used to evaluate fracture toughness. The CTOD test is a test that simulates the phenomenon in which a crack grows when a bending load is applied to a large structure such as a line pipe that has a crack. When a load is applied to a test piece having a crack, an "unstable fracture" occurs, which is a phenomenon in which the crack grows rapidly. The CTOD test uses the change in the opening just before the crack grows rapidly as an evaluation index. A high CTOD value is required especially for line pipes in cold regions. Patent Documents 1 and 2 do not consider such fracture toughness.
[0009] An object of the present disclosure is to provide a seamless steel pipe that has high strength and excellent fracture toughness. [Means for solving the problem]
[0010] The seamless steel pipe according to the present disclosure has In mass%, C: 0.03-0.08%, Si: 0.05 to 0.25%, Mn: 1.0-2.5%, P: 0.05% or less, S: 0.005% or less, Al: 0.030~0.100%, Ti: 0.001 to 0.050%, Mg: 0.0005~0.0050%, Rare earth elements: 0.0005~0.0050%, N: 0.0150% or less, O: 0.0050% or less, Mo: 0-0.3%, Nb: 0 to 0.020%, Ca: 0 to 0.0002%, B: 0~0.0002%, Cu: 0-0.50%, Ni: 0-0.50%, Cr: 0-0.50%, V: 0 to 0.08%, and the balance being Fe and impurities, satisfying formula (1); The tensile strength is 531 to 758 MPa. The density of specific oxide-based inclusions, which are oxide-based inclusions with a circle equivalent diameter of 2.0 μm or more, is 40 pieces / mm 2 is as follows: the aspect ratio of the specific oxide inclusions is 2.0 or less, The hardness of the specific oxide inclusions is 18 GPa or less. 0.3≦REM / Mg≦2.0 (1) Here, in the formula (1), the content of the rare earth element in mass% is substituted for "REM", and the content of Mg in mass% is substituted for "Mg". Effect of the Invention
[0011] The seamless steel pipe of the present disclosure has high strength and excellent fracture toughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] First, the inventors investigated seamless steel pipes that can provide high strength and excellent fracture toughness from the viewpoint of chemical composition. As a result, the inventors found that the composition is, in mass%, C: 0.03-0.08%, Si: 0.05-0.25%, Mn: 1.0-2.5%, P: 0.05% or less, S: 0.005% or less, Al: 0.030-0.100%, Ti: 0.001-0.050%, Mg: 0.0005-0.0050%, rare earth elements: 0.0005-0.0050%, N: 0.0150% or less, O: 0.005 It was believed that a seamless steel pipe consisting of 0% or less, Mo: 0-0.3%, Nb: 0-0.020%, Ca: 0-0.0002%, B: 0-0.0002%, Cu: 0-0.50%, Ni: 0-0.50%, Cr: 0-0.50%, V: 0-0.08%, and the balance being Fe and impurities, would have a high tensile strength of 531-758 MPa and would also have excellent fracture toughness.
[0013] Therefore, the inventors further studied the fracture toughness of seamless steel pipes having the above-mentioned chemical composition. Here, the inventors focused on coarse oxide-based inclusions. Coarse oxide-based inclusions become the starting points of cracks. If the number density of coarse oxide-based inclusions is high, unstable fracture is more likely to occur. As a result, fracture toughness decreases. In the above-mentioned chemical composition, Ca is used as an impurity, and the Ca content is kept as low as possible. This makes it possible to keep the number density of coarse oxide-based inclusions low to a certain extent.
[0014] However, as a result of further investigation by the present inventors, even seamless steel pipes having the above-mentioned chemical composition still do not always have excellent fracture toughness in some cases. Therefore, the present inventors conducted further investigations and obtained the following findings.
[0015] Even if the number density of the coarse oxide-based inclusions is relatively low, if the coarse oxide-based inclusions are too hard, the coarse oxide-based inclusions may crack. In this case, the coarse oxide-based inclusions may become the starting point of cracks that cause a decrease in fracture toughness. On the other hand, if the coarse oxide-based inclusions are too soft, the coarse oxide-based inclusions are elongated in the steel material. If the aspect ratio of such coarse oxide-based inclusions is too large, the tip portion of the elongated coarse oxide-based inclusion may become the starting point of cracks that cause a decrease in fracture toughness. Therefore, the coarse oxide-based inclusions need to have an appropriate hardness that is neither too hard nor too soft.
[0016] Based on the above results, the present inventors further investigated the appropriate morphology of coarse oxide-based inclusions in seamless steel pipes that satisfy the above-mentioned chemical composition. As a result, it was found that the number density of oxide-based inclusions with a circle equivalent diameter of 2.0 μm or more was 40 pieces / mm 2 It has been found that excellent fracture toughness can be obtained if the aspect ratio of the oxide-based inclusions having an equivalent circle diameter of 2.0 μm or more is 2.0 or less and the hardness of the oxide-based inclusions having an equivalent circle diameter of 2.0 μm or more is 18 GPa or less. In the following description, the oxide-based inclusions having an equivalent circle diameter of 2.0 μm or more are also referred to as "specific oxide-based inclusions".
[0017] Furthermore, it was found that if the Mg content and REM content in the above-mentioned chemical composition satisfy formula (1), the number density, aspect ratio, and hardness of the specific oxide-based inclusions can be stably obtained. 0.3≦REM / Mg≦2.0 (1) Here, in formula (1), the content of rare earth elements (REM) in mass% is substituted for "REM", and the content of Mg in mass% is substituted for "Mg".
[0018] Fn is defined as REM / Mg. Fn is an index relating to the hardness of specific oxide-based inclusions in seamless steel pipes that satisfy the above-mentioned chemical composition. In the above-mentioned chemical composition, Mg softens the specific oxide-based inclusions. Meanwhile, rare earth elements (REM) harden the specific oxide-based inclusions. Therefore, in seamless steel pipes that satisfy the above-mentioned chemical composition, if Fn satisfies formula (1), the specific oxide-based inclusions will have an appropriate hardness that is neither too hard nor too soft. Therefore, the specific oxide-based inclusions can stably obtain an appropriate aspect ratio and appropriate hardness.
[0019] The seamless steel pipe of this embodiment, which has been completed based on the above findings, has the following configuration.
[0020] [1] A seamless steel pipe, In mass%, C: 0.03-0.08%, Si: 0.05 to 0.25%, Mn: 1.0-2.5%, P: 0.05% or less, S: 0.005% or less, Al: 0.030-0.100%, Ti: 0.001 to 0.050%, Mg: 0.0005~0.0050%, Rare earth elements: 0.0005~0.0050%, N: 0.0150% or less, O: 0.0050% or less, Mo: 0-0.3%, Nb: 0 to 0.020%, Ca: 0 to 0.0002%, B: 0~0.0002%, Cu: 0-0.50%, Ni: 0 to 0.50%, Cr: 0-0.50%, V: 0 to 0.08%, and the balance being Fe and impurities, satisfying formula (1); The tensile strength is 531 to 758 MPa. The density of specific oxide-based inclusions, which are oxide-based inclusions with a circle equivalent diameter of 2.0 μm or more, is 40 pieces / mm 2 is as follows: the aspect ratio of the specific oxide inclusions is 2.0 or less, The hardness of the specific oxide inclusions is 18 GPa or less. Seamless steel pipe. 0.3≦REM / Mg≦2.0 (1) Here, in the formula (1), the content of the rare earth element in mass% is substituted for "REM", and the content of Mg in mass% is substituted for "Mg".
[0021] [2] A seamless steel pipe according to [1], Al: 0.072-0.100%, Contains Seamless steel pipe.
[0022] [3] A seamless steel pipe according to [1] or [2], Cu: 0.01 to 0.50%, Ni: 0.01 to 0.50%, Cr: 0.01 to 0.50%, and V: 0.01 to 0.08%, Seamless steel pipe.
[0023] [4] A seamless steel pipe according to any one of [1] to [3], The seamless steel pipe is a seamless steel pipe for line pipe. Seamless steel pipe.
[0024] The seamless steel pipe according to the present embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.
[0025] [Features of the seamless steel pipe of this embodiment] The seamless steel pipe of this embodiment satisfies the following characteristics. (Feature 1) The chemical composition, in mass%, is C: 0.03-0.08%, Si: 0.05-0.25%, Mn: 1.0-2.5%, P: 0.05% or less, S: 0.005% or less, Al: 0.030-0.100%, Ti: 0.001-0.050%, Mg: 0.0005-0.0050%, rare earth elements: 0.0005-0.0 050%, N: 0.0150% or less, O: 0.0050% or less, Mo: 0-0.3%, Nb: 0-0.020%, Ca: 0-0.0002%, B: 0-0.0002%, Cu: 0-0.50%, Ni: 0-0.50%, Cr: 0-0.50%, V: 0-0.08%, and the balance is Fe and impurities. (Feature 2) The above chemical composition further satisfies formula (1). 0.3≦REM / Mg≦2.0 (1) Here, in the formula (1), the content of the rare earth element in mass% is substituted for "REM", and the content of Mg in mass% is substituted for "Mg". (Feature 3) The tensile strength is 531 to 758 MPa. (Feature 4) The density of specific oxide-based inclusions, which are oxide-based inclusions with a circle equivalent diameter of 2.0 μm or more, is 40 pieces / mm 2 The following is the result. (Feature 5) The aspect ratio of the specific oxide inclusions is 2.0 or less. (Feature 6) The hardness of the specific oxide inclusions is 18 GPa or less.
[0026] In this specification, the term "oxide-based inclusion" refers to an inclusion containing an oxide. The oxide-based inclusion may be an inclusion consisting of only an oxide. The oxide-based inclusion may also be a composite inclusion in which an oxide and an inclusion other than the oxide (e.g., Mn sulfide, etc.) are crystallized adjacent to the oxide. That is, in this specification, the oxide-based inclusion may be a composite inclusion containing an oxide. The oxide and the inclusion other than the oxide in the composite inclusion are in contact with each other. When the oxide-based inclusion is a composite inclusion, the composite inclusion is regarded as one oxide-based inclusion. Features 1 to 6 will be explained below.
[0027] [(Feature 1) Chemical composition] The chemical composition of the seamless steel pipe according to this embodiment contains the following elements.
[0028] C: 0.03 to 0.08% Carbon (C) improves the hardenability of steel material and increases its strength. If the C content is less than 0.03%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the C content exceeds 0.08%, the strength of the steel material becomes too high and the toughness of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the C content is 0.03 to 0.08%. The lower limit of the C content is preferably 0.04%, and more preferably 0.05%. The upper limit of the C content is preferably 0.07%, and more preferably 0.06%.
[0029] Silicon: 0.05 to 0.25% Silicon (Si) deoxidizes steel. Si also increases the strength of steel. If the Si content is less than 0.05%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Si content exceeds 0.25%, the fracture toughness of the steel decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 0.05 to 0.25%. The lower limit of the Si content is preferably 0.07%, and more preferably 0.10%. The upper limit of the Si content is preferably 0.22%, more preferably 0.20%, further preferably 0.18%, and further preferably 0.15%.
[0030] Mn: 1.0-2.5% Manganese (Mn) improves the hardenability of steel material and increases its strength. Mn also improves the hot workability of steel material. If the Mn content is less than 1.0%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content exceeds 2.5%, the hardenability of the steel material becomes too high and the toughness of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mn content is 1.0 to 2.5%. The lower limit of the Mn content is preferably 1.1%, more preferably 1.2%, and further preferably 1.3%. The upper limit of the Mn content is preferably 2.3%, more preferably 2.0%, and further preferably 1.8%.
[0031] P:0.05% or less Phosphorus (P) is an unavoidable impurity. That is, the lower limit of the P content is more than 0%. If the P content exceeds 0.05%, even if the contents of other elements are within the range of this embodiment, P segregates at grain boundaries, and the toughness of the steel material decreases. Therefore, the P content is 0.05% or less. The lower the P content, the better. However, an extreme reduction in the P content increases the production cost. Therefore, in consideration of industrial production, the lower limit of the P content is preferably 0.01%, and more preferably 0.02%. The upper limit of the P content is preferably 0.04%, and more preferably 0.03%.
[0032] S: 0.005% or less Sulfur (S) is an impurity that is inevitably contained. That is, the lower limit of the S content is more than 0%. S combines with Mn to form MnS. If the S content exceeds 0.005%, coarse MnS is formed in the steel material even if the contents of other elements are within the range of this embodiment. As a result, the toughness of the steel material decreases. Therefore, the S content is 0.005% or less. The S content is preferably as low as possible. However, an extreme reduction in the S content increases the production cost. Therefore, in consideration of industrial production, the lower limit of the S content is preferably 0.001%, and more preferably 0.002%. The upper limit of the S content is preferably 0.004%, and more preferably 0.003%.
[0033] Al: 0.030~0.100% Aluminum (Al) deoxidizes steel. If the Al content is less than 0.030%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Al content exceeds 0.100%, even if the contents of other elements are within the range of this embodiment, cluster-shaped oxide-based inclusions are excessively generated, and the fracture toughness of the steel material decreases. Therefore, the Al content is 0.030 to 0.100%. The lower limit of the Al content is preferably 0.035%, more preferably 0.040%, still more preferably 0.050%, and still more preferably 0.072%. When the Al content is 0.072% or more, the fracture toughness is significantly increased. The upper limit of the Al content is preferably 0.090%, more preferably 0.085%, and further preferably 0.080%. The "Al" content in this specification means the content of "acid-soluble Al", that is, "sol. Al".
[0034] Ti: 0.001 to 0.050% Titanium (Ti) improves the hardenability of steel material, or combines with N to form nitrides to increase the strength of the steel material. If the Ti content is less than 0.001%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ti content exceeds 0.050%, coarse nitrides or carbides are formed, reducing the toughness of the steel material and the toughness of the weld heat affected zone (HAZ), even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ti content is 0.001 to 0.050%. The lower limit of the Ti content is preferably 0.002%, more preferably 0.003%, further preferably 0.005%, and further preferably 0.010%. The upper limit of the Ti content is preferably 0.040%, more preferably 0.030%, and further preferably 0.020%.
[0035] Mg: 0.0005~0.0050% Magnesium (Mg) combines with O to form oxides, which reduces the hardness of oxide-based inclusions. This increases the fracture toughness of the steel material. If the Mg content is less than 0.0005%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mg content exceeds 0.0050%, coarse oxide-based inclusions are excessively formed even if the contents of other elements are within the ranges of this embodiment. In this case, the fracture toughness of the steel material decreases. Therefore, the Mg content is 0.0005 to 0.0050%. The lower limit of the Mg content is preferably 0.0007%, more preferably 0.0010%, and further preferably 0.0015%. The upper limit of the Mg content is preferably 0.0045%, more preferably 0.0040%, still more preferably 0.0035%, and still more preferably 0.0030%.
[0036] Rare earth elements (REM): 0.0005~0.0050% Rare earth elements (REM) combine with O to form oxide-based inclusions, increase the hardness of the oxide-based inclusions, and decrease the aspect ratio of the oxide-based inclusions. If the REM content is less than 0.0005%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the REM content exceeds 0.0050%, even if the contents of other elements are within the ranges of this embodiment, excessive coarse oxide-based inclusions are formed or the hardness of the oxide-based inclusions becomes excessively high. In this case, the fracture toughness of the steel material decreases. Therefore, the REM content is 0.0005 to 0.0050%. The lower limit of the REM content is preferably 0.0007%, more preferably 0.0010%, and even more preferably 0.0015%. The upper limit of the REM content is preferably 0.0045%, more preferably 0.0040%, and even more preferably 0.0035%.
[0037] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and the lanthanides lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.
[0038] N: 0.0150% or less Nitrogen (N) is inevitably contained. That is, the lower limit of the N content is more than 0%. N combines with Ti to form nitrides and refines crystal grains. Even if even a small amount of N is contained, the above effect can be obtained to some extent. However, if the N content exceeds 0.0150%, blowholes are generated in the steel material, and cracks are likely to occur in the steel material, even if the contents of other elements are within the ranges of this embodiment. Therefore, the N content is 0.0150% or less. The lower limit of the N content is preferably 0.0001%, more preferably 0.0010%, further preferably 0.0020%, and further preferably 0.0025%. The upper limit of the N content is preferably 0.0100%, more preferably 0.0070%, more preferably 0.0050%, more preferably 0.0040%, and even more preferably 0.0035%.
[0039] O: 0.0050% or less Oxygen (O) is an unavoidable impurity. In other words, the O content is greater than 0%. If the O content exceeds 0.0050%, excessive coarse oxide-based inclusions are formed. In this case, the fracture toughness of the steel material decreases. Therefore, the O content is less than or equal to 0.0050%. The O content is preferably as low as possible. However, an extreme reduction in the O content increases the production cost. Therefore, in consideration of industrial production, the lower limit of the O content is preferably 0.0001%, more preferably 0.0003%, more preferably 0.0005%, more preferably 0.0007%, and more preferably 0.0010%. The upper limit of the O content is preferably 0.0045%, more preferably 0.0040%, and further preferably 0.0035%.
[0040] The balance of the seamless steel pipe of this embodiment is composed of Fe and impurities. Here, the impurities refer to those that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the seamless steel pipe of this embodiment, but are not intentionally contained and are permissible within a range that does not adversely affect the seamless steel pipe of this embodiment.
[0041] [Impurities or optional elements] The seamless steel pipe of this embodiment further contains, instead of a part of Fe, Mo: 0-0.3%, Nb: 0 to 0.020%, Ca: 0 to 0.0002%, B: 0~0.0002%, Cu: 0-0.50%, Ni: 0 to 0.50%, Cr: 0 to 0.50%, and V: 0 to 0.08%.
[0042] [Group 1 (Mo, Nb, Ca and B)] Mo, Nb, Ca and B are all impurities in the seamless steel pipe of this embodiment. The contents of these elements may be 0%. Each element will be described below.
[0043] Mo: 0 to 0.3% Molybdenum (Mo) is an impurity in the seamless steel pipe of this embodiment. Mo promotes the formation of island martensite and reduces the fracture toughness of the steel material. Therefore, it is preferable that Mo is not contained in the seamless steel pipe of this embodiment. Therefore, the Mo content is 0 to 0.3%. The Mo content is preferably as low as possible. However, an extreme reduction in the Mo content increases the production cost. Therefore, in consideration of industrial production, the preferred lower limit of the Mo content is 0.1%. The preferred upper limit of the Mo content is 0.2%.
[0044] Nb: 0 to 0.020% Niobium (Nb) is an impurity in the seamless steel pipe of this embodiment. Nb forms precipitates and makes the strength and toughness of the steel unstable. Therefore, it is preferable that Nb is not contained in the seamless steel pipe of this embodiment. Therefore, the Nb content is 0 to 0.020%. The Nb content is preferably as low as possible. However, an extreme reduction in the Nb content increases the manufacturing cost. Therefore, in consideration of industrial production, the lower limit of the Nb content is preferably 0.001%, more preferably 0.002%, and even more preferably 0.005%. The upper limit of the Nb content is preferably 0.018%, and more preferably 0.015%.
[0045] Ca: 0 to 0.0002% Calcium (Ca) is an impurity in the seamless steel pipe of this embodiment. Ca is contained in the oxide-based inclusions and excessively increases the hardness of the oxide-based inclusions. As a result, the fracture toughness of the steel material decreases. Therefore, it is preferable that Ca is not contained in the seamless steel pipe of this embodiment. Therefore, the Ca content is 0 to 0.0002%. The Ca content is preferably as low as possible. However, an extreme reduction in the Ca content increases the production cost. Therefore, in consideration of industrial production, the preferable lower limit of the Ca content is 0.0001%.
[0046] B: 0 to 0.0002% Boron (B) is an impurity in the seamless steel pipe of this embodiment. B excessively increases the strength of the steel material. As a result, the fracture toughness of the steel material decreases. B also decreases the toughness of the HAZ of the steel material after welding. Therefore, it is preferable that B is not contained in the seamless steel pipe of this embodiment. Therefore, the B content is 0 to 0.0002%. The B content is preferably as low as possible. However, an extreme reduction in the B content increases the production cost. Therefore, in consideration of industrial production, the preferred lower limit of the B content is 0.0001%.
[0047] [Group 2: Cu, Ni, Cr and V] The seamless steel pipe according to the present embodiment may contain, in place of a portion of Fe, one or more elements selected from the group consisting of Cu, Ni, Cr and V. All of these elements are optional elements, and increase the strength of the steel material.
[0048] Cu: 0-0.50% Copper (Cu) is an optional element and may not be contained. In other words, the Cu content may be 0%. When contained, Cu improves the hardenability of the steel material and increases the strength of the steel material. If even a small amount of Cu is contained, the above effects can be obtained to a certain extent. However, if the Cu content exceeds 0.50%, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cu content is 0 to 0.50%. The lower limit of the Cu content is preferably 0.01%, more preferably 0.03%, further preferably 0.05%, and further preferably 0.10%. The upper limit of the Cu content is preferably 0.40%, more preferably 0.30%, further preferably 0.25%, and further preferably 0.20%.
[0049] Ni: 0 to 0.50% Nickel (Ni) is an optional element and may not be contained. In other words, the Ni content may be 0%. When contained, Ni increases the hardenability of the steel material and increases the strength of the steel material. Even if even a small amount of Ni is contained, the above effects can be obtained to a certain extent. However, if the Ni content exceeds 0.50%, the hardenability of the steel material becomes too high and the toughness of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ni content is 0 to 0.50%. The lower limit of the Ni content is preferably 0.01%, more preferably 0.05%, and further preferably 0.10%. The upper limit of the Ni content is preferably 0.40%, more preferably 0.30%, and further preferably 0.25%.
[0050] Cr: 0~0.50% Chromium (Cr) is an optional element and may not be contained. In other words, the Cr content may be 0%. When contained, Cr improves the hardenability of the steel material and increases the strength of the steel material. Even if even a small amount of Cr is contained, the above effects can be obtained to a certain extent. However, if the Cr content exceeds 0.50%, even if the contents of other elements are within the ranges of this embodiment, the hardenability becomes too high and the toughness of the steel material decreases. Therefore, the Cr content is 0 to 0.50%. The lower limit of the Cr content is preferably 0.01%, more preferably 0.05%, and further preferably 0.10%. The upper limit of the Cr content is preferably 0.40%, more preferably 0.30%, and further preferably 0.25%.
[0051] V: 0~0.08% Vanadium (V) is an optional element and may not be contained. In other words, the V content may be 0%. When contained, V generates V carbides to increase the strength of the steel material. Even if even a small amount of V is contained, the above effect can be obtained to some extent. However, if the V content exceeds 0.08%, even if the contents of other elements are within the range of this embodiment, excessive V carbides are generated, and the toughness of the steel material decreases. Therefore, the V content is 0 to 0.08%. The lower limit of the V content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the V content is preferably 0.07%, more preferably 0.06%, and further preferably 0.05%.
[0052] [(Feature 2) Regarding formula (1)] The above chemical composition further satisfies formula (1). 0.3≦REM / Mg≦2.0 (1) Here, in the formula (1), the content of the rare earth element in mass% is substituted for "REM", and the content of Mg in mass% is substituted for "Mg".
[0053] Let Fn be defined as follows: Fn=REM / Mg Fn is an index relating to the hardness of specific oxide-based inclusions in a seamless steel pipe satisfying characteristic 1. As described above, Mg softens the specific oxide-based inclusions. On the other hand, REM hardens the specific oxide-based inclusions. Therefore, the hardness of the specific oxide-based inclusions can be adjusted by adjusting Fn.
[0054] In a seamless steel pipe satisfying the characteristic 1, if Fn is less than 0.3, the REM content is too low relative to the Mg content. In this case, the specific oxide-based inclusions become excessively soft. As a result, the specific oxide-based inclusions become more likely to elongate, and the aspect ratio of the specific oxide-based inclusions may exceed 2.0. On the other hand, if Fn exceeds 2.0, the REM content is too high relative to the Mg content. In this case, the specific oxide-based inclusions become excessively hard. As a result, the hardness of the specific oxide-based inclusions exceeds 18 GPa. Therefore, Fn is 0.3 to 2.0. Fn is calculated by rounding off the obtained numerical value to one decimal place.
[0055] The lower limit of Fn is preferably 0.4, more preferably 0.5, still more preferably 0.6, and still more preferably 0.7. The upper limit of Fn is preferably 1.9, more preferably 1.8, even more preferably 1.7, and even more preferably 1.6.
[0056] [Feature 3: Tensile strength] The seamless steel pipe of this embodiment has a tensile strength of 531 to 758 MPa. The seamless steel pipe of this embodiment has excellent fracture toughness while satisfying the above-mentioned high strength.
[0057] The lower limit of the tensile strength of the seamless steel pipe of this embodiment is preferably 535 MPa, and more preferably 540 MPa. The upper limit of the tensile strength of the seamless steel pipe of this embodiment is preferably 740 MPa, more preferably 730 MPa, and even more preferably 720 MPa.
[0058] [Yield ratio] In the seamless steel pipe of this embodiment, the yield ratio is preferably 0.75 or more. If the yield ratio is 0.75 or more, excellent fracture toughness can be obtained while maintaining high strength. Specifically, the fracture toughness is increased by setting the tensile strength within the range of 531 to 758 MPa, while the yield ratio is set to 0.75 or more to increase the yield strength relative to the tensile strength. This allows the seamless steel pipe to maintain high strength while obtaining excellent fracture toughness. The lower limit of the yield ratio is preferably 0.78, and more preferably 0.80. The upper limit of the yield ratio is preferably 0.90, more preferably 0.88, and even more preferably 0.86.
[0059] [How to determine mechanical properties (tensile strength, yield ratio, etc.)] The tensile strength of the seamless steel pipe of this embodiment can be determined by the following method. A tensile test specimen is prepared from the seamless steel pipe. When the wall thickness of the seamless steel pipe is 20 mm or more, a No. 4 test specimen (round bar test specimen) specified in JIS Z 2241 (2011) is prepared as a tensile test specimen from the center of the wall thickness. When the wall thickness of the seamless steel pipe is less than 20 mm, the thickness is taken as the total wall thickness, and any one of No. 12A, No. 12B, and No. 12C test specimens (arc-shaped test specimens) specified in JIS Z 2241 (2011) is prepared as a tensile test specimen according to the outer diameter of the steel pipe. The longitudinal direction of the tensile test specimen is the axial direction of the steel pipe. A tensile test is performed at room temperature (25°C) in the air using the prepared tensile test specimen to determine the yield strength (MPa) and tensile strength (MPa). The 0.2% offset proof stress is taken as the yield strength (MPa). Based on the obtained yield strength and tensile strength, the yield ratio is calculated by the following formula. Yield ratio = Yield strength / Tensile strength The yield strength and tensile strength are calculated by rounding off the obtained values to the nearest one decimal place, and the yield ratio is calculated by rounding off the obtained values to the nearest two decimal places.
[0060] [(Features 4 to 6) Specific oxide inclusions] The seamless steel pipe of this embodiment further satisfies the following characteristics 4 to 6. (Feature 4) The density of specific oxide-based inclusions, which are oxide-based inclusions with a circle equivalent diameter of 2.0 μm or more, is 40 pieces / mm 2 The following is the result. (Feature 5) The aspect ratio of the specific oxide inclusions is 2.0 or less. (Feature 6) The hardness of the specific oxide inclusions is 18 GPa or less. Here, the circle equivalent diameter means the diameter of a circle having the same area as the area of the inclusion. As described above, oxide-based inclusions having a circle equivalent diameter of 2.0 μm or more are also called specific oxide-based inclusions. Features 4 to 6 will be described below.
[0061] [(Feature 4) Number density of specific oxide inclusions] In the seamless steel pipe of this embodiment, the density of specific oxide-based inclusions is 40 pieces / mm 2 The specific oxide-based inclusions become the starting points of cracks and reduce the fracture toughness of seamless steel pipes. In seamless steel pipes that satisfy Features 1 to 3, the number density of the specific oxide-based inclusions is 40 pieces / mm 2 If the density exceeds 40 / mm, excellent fracture toughness cannot be obtained. 2 The following is the result.
[0062] The preferred upper limit of the density of specific oxide inclusions is 38 pieces / mm 2 and more preferably 36 pieces / mm 2 and more preferably 34 pieces / mm 2 and more preferably 32 pieces / mm 2 It is. The preferred lower limit of the density of the specific oxide-based inclusions is not particularly limited. The lower limit of the density of the specific oxide-based inclusions is, for example, 3 pieces / mm 2 For example, 5 pieces / mm 2 It is.
[0063] [(Feature 5) Aspect ratio of specific oxide inclusions] Furthermore, in the seamless steel pipe of this embodiment, the specific oxide-based inclusions have an appropriate aspect ratio. Specifically, the aspect ratio of the specific oxide-based inclusions is 2.0 or less. Even if the number density of the specific oxide-based inclusions satisfies characteristic 4, if the aspect ratio of the specific oxide-based inclusions exceeds 2.0, the specific oxide-based inclusions are excessively soft. Therefore, the specific oxide-based inclusions extend excessively in the axial direction of the tube. In this case, cracks are likely to occur from the ends of the specific oxide-based inclusions extending in the axial direction of the tube. This reduces the fracture toughness of the seamless steel pipe. Therefore, the aspect ratio of the specific oxide-based inclusions is 2.0 or less.
[0064] The upper limit of the aspect ratio of the specific oxide inclusions is preferably 1.9, more preferably 1.8, and even more preferably 1.7. The lower limit of the aspect ratio of the specific oxide inclusions is preferably 1.2, more preferably 1.1, and most preferably 1.0.
[0065] [(Feature 6) Hardness of specific oxide inclusions] Furthermore, in the seamless steel pipe of this embodiment, the specific oxide-based inclusions have an appropriate hardness. Specifically, the hardness of the specific oxide-based inclusions is 18 GPa or less. Even if the number density and aspect ratio of the specific oxide-based inclusions satisfy Features 4 and 5, if the specific oxide-based inclusions are excessively hard, the specific oxide-based inclusions are likely to crack. The cracked specific oxide-based inclusions are likely to become the starting point of cracks in the steel material. Therefore, the fracture toughness of the seamless steel pipe is reduced. If the hardness of the specific oxide-based inclusions is 18 GPa or less, the specific oxide-based inclusions are appropriately soft. Therefore, cracks in the specific oxide-based inclusions are sufficiently suppressed. As a result, it is possible to suppress the specific oxide-based inclusions from becoming the starting point of cracks, and excellent fracture toughness is obtained in the seamless steel pipe. The hardness of the specific oxide-based inclusions means the hardness of the oxides contained in the specific oxide-based inclusions.
[0066] The upper limit of the hardness of the specific oxide inclusions is preferably 17 GPa, more preferably 16 GPa, and even more preferably 15 GPa. The lower limit of the hardness of the specific oxide-based inclusion is not particularly limited. However, in a seamless steel pipe having a chemical composition that satisfies Features 1 and 2, the lower limit of the hardness of the specific oxide-based inclusion is, for example, 5 GPa, for example, 8 GPa, or for example, 10 GPa.
[0067] There is no particular upper limit to the circle-equivalent diameter of the specific oxide-based inclusions in Features 4 to 6. However, in a seamless steel pipe satisfying Features 1 and 2, the upper limit to the circle-equivalent diameter of the specific oxide-based inclusions is, for example, 10.0 μm.
[0068] [Method for measuring the number density of specific oxide inclusions] The number density of the specific oxide inclusions can be determined by the following method. A test piece for microstructural observation is prepared from the center of the wall thickness of the seamless steel pipe. The surface of the test piece that includes the wall thickness direction and tube axis direction of the seamless steel pipe is used as the observation surface. The observation surface of the test piece is mirror polished. An observation field is arbitrarily set on the polished observation surface. The set observation field is observed at 1000x magnification using a scanning electron microscope (SEM) to generate a photographic image. The size of the observation field is 2000 μm in the wall thickness direction and 5000 μm in the tube axis direction. The observation field is set so that the center position of the observation field in the wall thickness direction coincides with the wall thickness center of the seamless steel pipe.
[0069] In the photographic image of the observation field, particles (inclusions or precipitates) are identified based on the contrast. The area of each identified particle is calculated, and the equivalent circle diameter is calculated based on the area. Among the identified particles, particles with an equivalent circle diameter of 2.0 μm or more are identified.
[0070] The identified particles are subjected to point analysis by energy dispersive X-ray spectrometry (EDS). The content of elements contained in each particle is determined by the EDS point analysis. In the EDS point analysis, the acceleration voltage is set to 20 kV, and the target elements are quantified as Mg, REM, Al, Ti, V, Cr, Mn, Fe, Ni, Mo, and Nb, N, and O. When the specific oxide-based inclusion includes multiple different contrast regions, the EDS point analysis is performed on each contrast region to determine the content of elements contained in each region. Based on the EDS analysis results for each particle with a circle equivalent diameter of 2.0 μm or more, the region with an O content of 5% or more by mass is recognized as an oxide. Then, the particle containing the oxide is identified as a "specific oxide-based inclusion."
[0071] The total number of specific oxide-based inclusions identified in the observation field is calculated. Based on the total number of specific oxide-based inclusions obtained and the total area of the observation field, the number density of the specific oxide-based inclusions (pieces / mm 2 In this embodiment, the number density of the specific oxide-based inclusions is determined by rounding off the obtained value to one decimal place.
[0072] The number density of the specific oxide-based inclusions can be determined using a scanning electron microscope equipped with a composition analysis function (SEM-EDS device). For example, an inclusion automatic analyzer manufactured by FEI (ASPEX) under the trade name Metals Quality Analyzer can be used as the SEM-EDS device.
[0073] [Method for measuring the aspect ratio of specific oxide inclusions] The major axis and minor axis of each specific oxide-based inclusion in the observation field obtained by the above-mentioned [Method for measuring the number density of specific oxide-based inclusions] are obtained by the following method. The boundary between the specific oxide-based inclusion and the parent phase, i.e., the contour line of the specific oxide-based inclusion is sandwiched between two parallel line segments, and the maximum distance between the two line segments (distance between the lines) is defined as the major axis (μm). In addition, the distance between the two line segments when the contour line of the specific oxide-based inclusion is sandwiched between two line segments parallel to the major axis is defined as the minor axis (μm). The aspect ratio of the specific oxide-based inclusion is calculated from the obtained major axis and minor axis by the following formula. Aspect ratio = major axis / minor axis The maximum value of the aspect ratios of the specific oxide-based inclusions in the observed field of view is defined as the aspect ratio of the specific oxide-based inclusions. Note that in this embodiment, the aspect ratio of the specific oxide-based inclusions is determined by rounding off the obtained numerical value to one decimal place.
[0074] [Method for measuring hardness of specific oxide inclusions] The hardness of the specific oxide inclusions can be determined by the nanoindentation method as follows. Each specific oxide-based inclusion in the observation field obtained by the above-mentioned [Method for measuring the number density of specific oxide-based inclusions] is observed at a magnification of 5000. In order to identify the position of each specific oxide-based inclusion, an indentation is made in advance by an indenter near the specific oxide-based inclusion as a marker, and the positional relationship between the indentation and the specific oxide-based inclusion is recorded.
[0075] The hardness (GPa) of the oxide contained in each of the specific oxide-based inclusions is determined by a nanoindentation method. For example, a nanoindenter (product name: TI-950) manufactured by Bruker Japan is used as the nanoindenter. The oxide contained in each of the specific oxide-based inclusions is identified based on the positional relationship between the above-mentioned indentation and the specific oxide-based inclusion. The indenter is pressed into the identified oxide to measure the hardness. At this time, the test force is set to 500 μN. The pressing position is adjusted so that the center position of the indenter is pressed into the center of gravity of the identified oxide. The maximum value of the obtained hardness of each specific oxide-based inclusion is defined as the hardness (GPa) of the specific oxide-based inclusion. In this embodiment, the hardness of the specific oxide-based inclusion is determined by rounding off the obtained numerical value to one decimal place.
[0076] [Effects of the seamless steel pipe of this embodiment] The seamless steel pipe of this embodiment satisfies Features 1 to 6. Therefore, the seamless steel pipe of this embodiment has high strength and excellent fracture toughness.
[0077] Here, excellent fracture toughness means excellent fracture toughness at low temperatures, and is defined as follows.
[0078] [Method of measuring fracture toughness] A CTOD test is performed according to a method conforming to ISO 12135 (2021) to obtain a CTOD value at -20°C. Specifically, a three-point bending CTOD test piece is prepared from a seamless steel pipe according to a method conforming to ISO 15653 (2018). In this embodiment, a single edge notched bend (SENB: Single Edge Notched Bend) test piece is used as the CTOD test piece. The CTOD test piece has a thickness of B, a width W of 2B, and a length L of 10B. The CTOD test piece is further prepared so that the thickness B is as large as possible. The notch of the CTOD test piece has a width of 2 mm and a tip shape of 60°.
[0079] A fatigue test for introducing a pre-crack is performed on the prepared CTOD test piece. In this embodiment, the initial relative crack length a0 / W is set to 0.50. Specifically, a fatigue test is performed at room temperature (25 ° C), a fatigue pre-crack of 2 mm is introduced at the tip of the notch, and the initial crack length a0 is set to B. A CTOD test is performed at -20 ° C in accordance with ISO 12135 (2021) on the CTOD test piece in which the fatigue pre-crack is introduced. The CTOD value (mm) is obtained based on ISO 12135 (2021) from the load at break in the load-opening amount curve and the plastic component amount of the clip gauge opening displacement obtained by the CTOD test. Note that the same test is performed six times, and the minimum CTOD value (mm) is defined as the CTOD value (mm) of the seamless steel pipe at -20 ° C. Note that in this embodiment, the CTOD value is obtained by rounding off the obtained numerical value to two decimal places.
[0080] In this embodiment, if the CTOD value at -20°C obtained by the above method is 0.25 mm or more, it is determined that the specimen has excellent fracture toughness.
[0081] [Microstructure] Preferably, the microstructure of the seamless steel pipe according to this embodiment is mainly composed of tempered bainite. More specifically, the microstructure of the seamless steel pipe according to this embodiment has a volume fraction of tempered bainite of 90% or more. The remainder of the microstructure is, for example, ferrite or pearlite. Note that the microstructure of the seamless steel pipe according to this embodiment may contain minute amounts of precipitates, inclusions, etc. in addition to tempered bainite, ferrite, and pearlite. However, in the microstructure of the seamless steel pipe according to this embodiment, the volume fraction of precipitates, inclusions, etc. is negligibly small compared to the volume fractions of tempered bainite, ferrite, and pearlite.
[0082] When the volume fraction of tempered bainite is determined by observation, it can be determined by the following method. First, a test piece is prepared from the center of the wall thickness of a seamless steel pipe according to this embodiment, with the observation surface being a plane including the pipe axis direction and the wall thickness direction. The observation surface of the test piece is polished to a mirror finish, and then immersed in a nital etching solution for about 10 seconds to reveal the structure by etching. The etched observation surface is observed in 10 fields of view using an optical microscope. The field area is, for example, 0.04 mm. 2 (magnification: 500x). In each field of view, ferrite and pearlite are identified based on the contrast. The total area ratio of the identified ferrite and pearlite is determined. The method for determining the area ratio is not particularly limited, and any well-known method may be used. For example, the total area ratio of ferrite and pearlite can be determined by image analysis. The area ratio (%) of tempered bainite is determined using the obtained total area ratio (%) of ferrite and pearlite and the following formula. Area ratio of tempered bainite (%) = 100 - (total area ratio of ferrite and pearlite) (%) The arithmetic mean value of the area fraction (%) of tempered bainite obtained from 10 fields of view is defined as the volume fraction (%) of tempered bainite.
[0083] [Seamless steel pipe shape] The shape of the seamless steel pipe according to the present embodiment is not particularly limited as long as it is a seamless steel pipe. That is, the outer diameter, wall thickness, and length are not particularly limited. When the seamless steel pipe according to the present embodiment is a seamless steel pipe for line pipe, the preferred outer diameter is 60 to 425 mm. When the seamless steel pipe according to the present embodiment is a seamless steel pipe for line pipe, the preferred wall thickness is less than 50 mm. The lower limit of the wall thickness is, for example, 5 mm. In particular, even if the wall thickness is 20 mm or more, excellent fracture toughness can be obtained.
[0084] [Manufacturing method] A method for producing a seamless steel pipe according to the present embodiment will be described below. The method for producing a seamless steel pipe described below is one example of a method for producing a seamless steel pipe according to the present embodiment. That is, the seamless steel pipe according to the present embodiment may be produced by a production method other than the production method described below. An example of a method for manufacturing a seamless steel pipe according to this embodiment includes the following steps. (Process 1) Steelmaking process (Process 2) Hot processing process (Step 3) Quenching process (Process 4) Tempering process Each step will be described below.
[0085] [(Process 1) Steelmaking process] The steelmaking process includes the following steps: (Step 11) Refining step (Step 12) Casting process In the refining process, molten steel with adjusted composition is produced. In the casting process, the molten steel produced in the refining process is used to produce a cast material (bloom or billet). Each process will be described below.
[0086] [(Step 11) Refining process] The refining process includes primary refining and secondary refining. In the primary refining, refining is performed in a converter on molten steel produced by a known method. Specifically, oxygen is blown onto the molten iron to remove carbon. In the secondary refining, elements are added to adjust the composition, and molten steel whose chemical composition satisfies Features 1 and 2 is produced. Specifically, after the primary refining process, deoxidation is performed on the molten steel tapped from the converter. After the deoxidation, slag removal is performed. After the slag removal, secondary refining is performed. In the secondary refining, composition adjustment is performed by LT (Ladle Treatment). Specifically, in LT, alloy elements are added to the molten steel in the ladle to adjust the composition of the molten steel. The molten steel temperature during composition adjustment is preferably maintained at, for example, 1500 to 1700°C.
[0087] The composition adjustment in the secondary refining satisfies the following conditions: (Condition 1) Al, REM, and Mg are added to the molten steel in this order, and the holding time t0 from the addition of Al to the addition of REM is set to 300 seconds (5 minutes) or more. (Condition 2) The holding time from the time τ of uniform mixing after adding REM to the time Mg is added is defined as holding time t1. The holding time from the time τ of uniform mixing after adding Mg to the time Mg is tapped is defined as holding time t2. In this case, holding time t1 and holding time t2 satisfy formula (A). t1 / t2≧1.0 (A)
[0088] Here, the uniform mixing time τ means the time from when elemental components are added to molten steel until the added elemental components are uniformly dispersed in the molten steel. The uniform mixing time τ can be calculated by the following formula (B). τ=800×ε -0.4 (B) Here, ε is the stirring power density of the molten steel in the LT and is defined by equation (C). ε=28.5(Q / W)×T×log(1+H / 1.48) (C) Here, Q is the top blown gas flow rate (Nm 3 / min). W is the mass of molten steel (t). T is the temperature of molten steel (K). H is the depth of the molten steel in the ladle (steel bath depth) (m).
[0089] Conditions 1 and 2 will be explained below.
[0090] [(Condition 1) Regarding the order of element addition and retention time t0] In this embodiment, deoxidizing elements are added to the molten steel in the secondary refining in the order of Al, REM, and Mg. By adding Al, Al oxides are generated in the molten steel. If REM is added after the addition of Al, hard oxides containing Al and REM are generated. If Mg is further added after the addition of REM, the hard oxides containing Al and REM are reduced by Mg. As a result, the hard oxides containing Al and REM are modified to soft oxides containing Al, REM, and Mg. By the above steps, the specific oxide-based inclusions in the manufactured seamless steel pipe satisfy Features 5 and 6.
[0091] On the other hand, if Mg is added without adding REM after adding Al, soft oxides containing Al and Mg are generated. In this case, even if REM is added afterwards, the soft oxides containing Al and Mg are not easily reduced by REM. Therefore, the aspect ratio of the specific oxide-based inclusions in the seamless steel pipe after production becomes excessively large. Therefore, in the secondary refining, the deoxidizing elements are added in the order of Al, REM, and Mg.
[0092] Furthermore, the holding time t0 from the addition of Al to the addition of REM is set to 300 seconds or more. If the holding time t0 is less than 300 seconds, Al2O3 generated in the molten steel after the addition of Al does not rise sufficiently. In this case, the number density of the specific oxide-based inclusions becomes excessively high. Therefore, the holding time t0 is set to 300 seconds or more. The upper limit of the holding time t0 is not particularly limited, but is, for example, 1200 seconds.
[0093] [(Condition 2) Regarding formula (A)] The holding time from when the uniform mixing time τ has elapsed after adding REM until when Mg is added is defined as holding time t1 (seconds). Also, the holding time from when the uniform mixing time τ has elapsed after adding Mg until when steel is tapped is defined as holding time t2 (seconds). In this case, holding time t1 (seconds) and holding time t2 (seconds) satisfy the following formula (A). t1 / t2≧1.0 (A)
[0094] FA is defined as follows: FA=t1 / t2 FA is an index showing the state of oxide-based inclusions in molten steel. When FA is small, the hard oxides containing Al and REM in the specific oxide-based inclusions are excessively reduced by Mg. As a result, the hardness of the oxides becomes excessively low. In this case, the aspect ratio of the specific oxide-based inclusions becomes excessively large.
[0095] If FA is 1.0 or more, the hardness of the oxide in the specific oxide-based inclusion is appropriate, and therefore, the aspect ratio and hardness of the specific oxide-based inclusion fall within appropriate ranges, provided that the other characteristics of the present invention are satisfied.
[0096] The upper limit of FA is not particularly limited, and may be, for example, 20.0. As long as FA is 1.0 or more, the retention time t1 and retention time t2 are not particularly limited. The retention time t1 is, for example, 50 to 1000 seconds. The retention time t2 is, for example, 30 to 200 seconds.
[0097] [(Step 12) Casting process] The molten steel produced by the above-mentioned refining process is used to produce a material (ingot or bloom). Specifically, the molten steel is used to produce a slab by a continuous casting method. The slab is, for example, a bloom or a billet. The molten steel may be used to produce an ingot by an ingot casting method. The slab or ingot may be further subjected to blooming or the like to produce a billet. The material (ingot, bloom, billet) is produced by the above-mentioned process.
[0098] [(Process 2) Hot processing process] In the hot working step, a prepared material is hot worked to produce a blank pipe. Specifically, a billet is heated in a heating furnace. Preferably, the billet is heated by being charged into a continuous heating furnace. Hereinafter, the case of heating by being charged into a continuous heating furnace will be described. In this case, the heating furnace may be a rotary hearth type heating furnace or a walking beam type heating furnace. The heating temperature is, for example, 1000 to 1300°C.
[0099] The billet extracted from the heating furnace is subjected to hot working to manufacture a mother pipe (seamless steel pipe). In this embodiment, the method of hot working is not particularly limited and may be a well-known method. For example, the Mannesmann process may be performed as hot working to manufacture a mother pipe. In this case, the round billet is pierced and rolled by a piercing machine. In the case of piercing and rolling, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The pierced and rolled round billet is further hot rolled by a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative reduction in area in the hot working process is, for example, 20 to 70%. Alternatively, a mother pipe may be manufactured from the billet by performing another hot working method. The mother pipe may be manufactured by forging such as the Erhardt process. The mother pipe is manufactured by the above steps.
[0100] The mother pipe produced by hot working may be air-cooled (as-rolled). The mother pipe produced by hot working may be directly quenched as the next quenching step after the hot working without being cooled to room temperature. Alternatively, the mother pipe may be supplemented with heat (reheated) after the hot working and then quenched. The quenching step will be described in detail below.
[0101] [(Step 3) Quenching process] In the quenching process, the mother tube prepared is quenched. The preferred quenching temperature is 800 to 1000°C. The holding time at the quenching temperature is not particularly limited, but is, for example, 5 to 100 minutes. For example, the quenching method is to continuously cool the mother tube from the quenching start temperature to continuously lower the surface temperature of the mother tube. The method of the continuous cooling treatment is not particularly limited, and may be a well-known method. For example, the method of the continuous cooling treatment is a method of immersing the mother tube in a water tank to cool it, or a method of accelerating cooling the mother tube by shower water cooling or mist cooling.
[0102] [(Process 4) Tempering process] In the tempering process, the mother pipe after the quenching process is tempered. The tempering temperature corresponds to the temperature of the furnace when the mother pipe after quenching is heated and held. The tempering time refers to the time from when the temperature of the mother pipe reaches a predetermined tempering temperature to when the mother pipe is removed from the heat treatment furnace.
[0103] The tempering temperature is adjusted appropriately depending on the chemical composition of the seamless steel pipe and the strength to be obtained (tensile strength of 531 to 758 MPa). In other words, the strength of the seamless steel pipe is adjusted by adjusting the tempering temperature for a mother pipe having the chemical composition of this embodiment. In the tempering process of this embodiment, the preferred tempering temperature is 500 to 700°C. In addition, the preferred tempering time in the tempering process of this embodiment is 5 to 240 minutes.
[0104] The seamless steel pipe according to the present embodiment can be manufactured by the above-mentioned manufacturing method. However, as described above, the above-mentioned manufacturing method is only an example, and the seamless steel pipe may be manufactured by other manufacturing methods. Hereinafter, the present invention will be described in more detail with reference to examples. EXAMPLES
[0105] Seamless steel pipes having the chemical compositions shown in Table 1 (Tables 1A and 1B) were manufactured.
[0106] [Table 1A]
[0107] [Table 1B]
[0108] Here, "-" in Table 1B means that the content of each element is at the impurity level. Also, "Fn" is shown in Table 1B.
[0109] Molten steel with each test number was produced as follows. The final composition of the molten steel in the ladle was adjusted by LT for secondary refining. The "Order of deoxidizing element addition" column in Table 2 shows the order of addition of Al, REM, and Mg during secondary refining. "Al → REM → Mg" means that Al, REM, and Mg were added in that order. "Al → Mg → REM" means that Al, Mg, and REM were added in that order.
[0110] In test numbers 1 to 34, Al was added, then REM was added, and then Mg was added. The holding time t0 (seconds) from the addition of Al to the addition of REM, the holding time t1 (seconds) from the addition of REM to the addition of Mg after the lapse of the uniform mixing time τ, and the holding time t2 (seconds) from the addition of Mg to the lapse of the uniform mixing time τ before tapping were as shown in Table 2.
[0111] On the other hand, in test number 35, Al was added, and then Mg was added. Then, REM was further added. In test number 35, the holding time from adding Al to adding Mg was t0 (seconds), the holding time from adding Mg and passing the uniform mixing time τ to adding REM was t1 (seconds), and the holding time from adding REM and passing the uniform mixing time τ to tapping was t2 (seconds) (see Table 2). Table 2 also shows FA (=t1 / t2). Molten steel of each test number was produced by the above process.
[0112] [Table 2]
[0113] A round billet was produced by continuous casting using the molten steel of each test number. After continuous casting, the round billet of each test number was subjected to the Mannesmann process as hot working to produce a blank pipe. The heating temperature in the hot working was 1250°C.
[0114] The obtained mother pipe of each test number was subjected to quenching and tempering. Specifically, the mother pipe of each test number was quenched by holding at 850-1000°C for 5-90 minutes and then water-cooling. The quenched mother pipe of each test number was further tempered by holding at 500-700°C for 5-240 minutes to adjust the tensile strength. Through the above manufacturing process, seamless steel pipes of each test number were obtained. The wall thickness (mm) of the seamless steel pipes of each test number is shown in Table 3. The outer diameter of the seamless steel pipe of each test number was 219.1 mm. Through the above manufacturing process, seamless steel pipes of each test number were manufactured.
[0115] [Table 3]
[0116] [Evaluation test] The seamless steel pipes with each test number were subjected to the following evaluation tests. (Test 1) Measurement test of the number density of specific oxide inclusions (Test 2) Measurement test of the aspect ratio of specific oxide inclusions (Test 3) Hardness measurement test for specific oxide inclusions (Test 4) Tensile test (Test 5) Fracture toughness evaluation test Tests 1 to 5 will be described below.
[0117] [(Test 1) Measurement test of the number density of specific oxide-based inclusions] Based on the method described in the above [Method for measuring the number density of specific oxide-based inclusions], the number density (pieces / mm 2 The number density of the specific oxide-based inclusions was measured using an automatic inclusion analyzer manufactured by FEI (ASPEX) under the product name of Metals Quality Analyzer. The number density of the specific oxide-based inclusions thus obtained is recorded as "Number density (pieces / mm 2 ) column.
[0118] [(Test 2) Measurement test of aspect ratio of specific oxide inclusions] The aspect ratio of the specific oxide-based inclusions of each test number was determined based on the method described in the above [Method for measuring the aspect ratio of specific oxide-based inclusions]. The aspect ratios of the specific oxide-based inclusions obtained are shown in the "Aspect ratio" column in Table 3.
[0119] [(Test 3) Hardness measurement test for specific oxide inclusions] The hardness (GPa) of the specific oxide-based inclusions was determined based on the method described in the above [Method for measuring hardness of specific oxide-based inclusions]. Note that a nanoindenter (product name: TI-950) manufactured by Bruker Japan was used as the nanoindenter. The hardness of the specific oxide-based inclusions obtained is shown in the "Hardness (GPa)" column in Table 3.
[0120] [(Test 4) Tensile test] Based on the method described in [Method of determining mechanical properties (tensile strength, yield ratio, etc.)] above, the yield strength, tensile strength, and yield ratio of the seamless steel pipes of each test number were determined. Note that No. 4 test pieces (round bar test pieces) specified in JIS Z 2241 (2011) were prepared as tensile test pieces. The obtained yield strength (MPa), tensile strength (MPa), and yield ratio are shown in the "Yield strength (MPa)", "Tensile strength (MPa)", and "Yield ratio" columns in Table 3.
[0121] [(Test 5) Fracture toughness evaluation test] Based on the method described above in [Method of measuring fracture toughness], the CTOD value (mm) at -20°C of the seamless steel pipe of each test number was obtained. The thickness B (mm) of the CTOD test piece of each test number was as shown in Table 3. The obtained CTOD value (mm) at -20°C of each test number is shown in the "CTOD value (-20°C) (mm)" column of Table 3.
[0122] [Test Results] With reference to Table 1 (Table 1A and Table 1B) to Table 3, the seamless steel pipes of test numbers 1 to 17 satisfied features 1 to 6. Therefore, in the fracture toughness evaluation test, the seamless steel pipes of these test numbers had a CTOD value of 0.25 mm or more at -20°C, and thus exhibited excellent fracture toughness. All of these seamless steel pipes had a microstructure mainly composed of tempered bainite. In other words, the volume fraction of tempered bainite was 90% or more.
[0123] Furthermore, the Al content was 0.072% or more in test numbers 1, 5 to 7, and 15 to 17. Therefore, in the fracture toughness evaluation test, the CTOD value at -20°C was 0.70 mm or more, and remarkably excellent fracture toughness was obtained.
[0124] On the other hand, the seamless steel pipes of test numbers 18 and 19 had too high an Al content. As a result, the density of specific oxide-based inclusions was 40 pieces / mm 2 As a result, in the fracture toughness evaluation test, the seamless steel pipes with these test numbers had a CTOD value of less than 0.25 mm at -20°C, and did not exhibit excellent fracture toughness.
[0125] The seamless steel pipe of test number 20 had an excessively high Si content, and as a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0126] In the seamless steel pipe of test number 21, the Mg content was too low and the Fn value was too high. Therefore, the hardness of the specific oxide inclusions exceeded 18 GPa. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0127] In the seamless steel pipe of test number 22, the Mg content was too high. As a result, the density of specific oxide inclusions was 40 pieces / mm 2 As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0128] In the seamless steel pipe of test number 23, the REM content was too low. Therefore, the aspect ratio of the specific oxide inclusions exceeded 2.0. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0129] In the seamless steel pipes of test numbers 24 and 25, the REM content was too low and the Fn value was too low. Therefore, the aspect ratio of the specific oxide inclusions exceeded 2.0. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0130] In the seamless steel pipe of test number 26, the REM content was too high and the Fn value was too high. As a result, the density of specific oxide inclusions was 40 pieces / mm 2 In addition, the hardness of the specific oxide inclusions exceeded 18 GPa. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0131] The seamless steel pipe of test number 27 had an excessively high Mo content, and as a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0132] In the seamless steel pipe of test number 28, the Ca content was too high. Therefore, the hardness of the specific oxide inclusions exceeded 18 GPa. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0133] In the seamless steel pipe of test number 29, the B content was too high. Therefore, the tensile strength exceeded 758 MPa. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0134] In the seamless steel pipe of test number 30, the Fn value was too high. As a result, the hardness of the specific oxide inclusions exceeded 18 GPa. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0135] In the seamless steel pipes of test numbers 31 and 32, the FA value was less than 1.0 in the refining process. Therefore, the aspect ratio of the specific oxide-based inclusions exceeded 2.0. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0136] In the seamless steel pipe of test number 33, the holding time t0 after adding Al in the refining process was too short. As a result, the density of specific oxide-based inclusions was 40 pieces / mm 2 As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0137] In the seamless steel pipe of test number 34, Fn was below the lower limit. Therefore, the aspect ratio of the specific oxide inclusions exceeded 2.0. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0138] In the seamless steel pipe of test number 35, the order of adding deoxidizing elements in the refining process was inappropriate. Specifically, Mg was added after adding Al, and then REM was added. As a result, the aspect ratio of the specific oxide inclusions exceeded 2.0. As a result, in the fracture toughness evaluation test, the CTOD value at -20°C was less than 0.25 mm, and excellent fracture toughness was not obtained.
[0139] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. A seamless steel pipe, In mass percent, C: 0.03-0.08%, Si: 0.05-0.25%, Mn: 1.0 to 2.5%, P: 0.05% or less, S: 0.005% or less, Al: 0.030-0.100%, Ti: 0.001 to 0.050%, Mg: 0.0005-0.0050%, Rare earth elements: 0.0005 to 0.0050%, N: 0.0150% or less, O: 0.0050% or less, Mo: 0-0.3%, Nb: 0 to 0.020%, Ca: 0-0.0002%, B: 0 to 0.0002%, Cu: 0 to 0.50%, Ni: 0 to 0.50%, Cr: 0 to 0.50%, V: 0 to 0.08%, and the balance being Fe and impurities, satisfying formula (1); The tensile strength is 531 to 758 MPa, The density of specific oxide-based inclusions, which are oxide-based inclusions with an equivalent circle diameter of 2.0 μm or more, is 40 pieces / mm 2 is as follows: the aspect ratio of the specific oxide inclusions is 2.0 or less, The hardness of the specific oxide inclusions is 18 GPa or less. Seamless steel pipe. 0.3≦REM / Mg≦2.0 (1) Here, in formula (1), the content of the rare earth element in mass % is substituted for "REM", and the content of Mg in mass % is substituted for "Mg".
2. The seamless steel pipe according to claim 1, Al: 0.072-0.100%, Contains Seamless steel pipe.
3. The seamless steel pipe according to claim 1, Cu: 0.01 to 0.50%, Ni: 0.01-0.50%, Cr: 0.01 to 0.50%, and V: 0.01 to 0.08%; Seamless steel pipe.
4. The seamless steel pipe according to any one of claims 1 to 3, The seamless steel pipe is a seamless steel pipe for line pipe. Seamless steel pipe.
Citation Information
Patent Citations
Seamless steel pipe and manufacturing method therefor
JP2004124158A
Thick-walled seamless steel pipe for line pipe
JP2010242222A
Cited By
Seamless steel pipe and method for manufacturing seamless steel pipe
WO2026116398A1