Cement composition and method for producing the same

A cement composition with controlled calcium-containing waste powder additives addresses strength reduction issues in mixed cement, achieving equivalent strength to ordinary Portland cement with improved initial strength and reduced environmental impact.

JP2024155625AActive Publication Date: 2024-10-31MITSUBISHI UBE CEMENT CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023070498
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

Existing cement compositions that incorporate low-reactivity waste and by-products face challenges in maintaining strength development, particularly initial strength, while also contributing to environmental impact reduction.

Method used

A cement composition comprising calcium-containing waste powder with specific properties, including a limited insoluble residue, calcium carbonate content, and CaO balance, mixed in controlled amounts with cement, enhances strength development and initial strength while reducing environmental load.

Benefits of technology

The cement composition achieves strength development equivalent to ordinary Portland cement with excellent initial strength, effectively utilizing waste materials and reducing environmental burden.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155625000001
    Figure 2024155625000001
  • Figure 2024155625000002
    Figure 2024155625000002
  • Figure 2024155625000003
    Figure 2024155625000003
Patent Text Reader

Abstract

To provide a cement composition which has strength developability at a level equivalent to that of current ordinary Portland cement and especially excellent initial strength while reducing environmental load by the effective use of wastes and by-products.SOLUTION: There is provided a cement composition comprising cement and a calcium-containing waste powder. The calcium-containing waste powder has an insoluble residue of 70.0 mass% or less as measured in accordance with JIS R 5202:2010, contains 5.0 mass% or more of calcium carbonate and has a CaO residual amount of 18.0 mass% or less after subtracting the CaO amount derived from calcium carbonate and the cement composition contains 1.0 mass% or more and 7.5 mass% or less of the calcium-containing waste powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to cement compositions and methods for making same. [Background technology]

[0002] As an effort to reduce carbon dioxide emissions, attention has been focused on a technology for chemically producing precipitated calcium carbonate by dissolving carbon dioxide in a liquid phase and reacting it with calcium. Precipitated calcium carbonate fixes carbon dioxide in the form of stable calcium carbonate, which directly contributes to reducing carbon dioxide emissions.

[0003] When immobilizing a huge amount of carbon dioxide as calcium carbonate, it is possible to use waste and by-products that contain a lot of calcium and are discharged in large quantities, such as waste concrete and steelmaking slag, as a calcium source. After calcium is extracted from the waste and by-products, a large amount of extraction residue is left behind. Generally, such extraction residue is disposed of by landfill. However, if the extraction residue can be effectively utilized, it will contribute to extending the life of final disposal sites and reducing the environmental burden.

[0004] Possible uses for the extraction residue include substituting it as an admixture for part of Portland cement or using it as blended cement. This would allow for effective use of the extraction residue and reduce the amount of clinker used, making it possible to reduce carbon dioxide emissions.

[0005] In recent years, from the viewpoint of preventing global warming and achieving low carbon emissions, it has been desired to further increase the substitution ratio of admixtures in cement clinker in order to reduce the amount of cement clinker used. For example, Non-Patent Document 1 studies the blending of admixtures with ordinary Portland cement in amounts exceeding 5% by mass, which is the amount specified by the JIS standard. In this case, it is necessary to consider the effects on various physical properties caused by increasing the blending amount of admixtures. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] Abstract of the 72nd Cement Technology Conference 2018, "3315 Quality Evaluation of Cement with Increased Amounts of Minor Mixture Components" Summary of the Invention [Problem to be solved by the invention]

[0007] As mentioned above, when low-reactivity waste or by-products are mixed into cement clinker as admixtures, strength development may decrease. In particular, there is concern about a decrease in early strength in blended cement. Therefore, an object of the present disclosure is to provide a cement composition that reduces the environmental burden through the effective use of waste and by-products, while having strength development at a level equivalent to that of current Portland cement, and that is particularly excellent in early strength. [Means for solving the problem]

[0008] One aspect of the present disclosure is a cement composition comprising cement and a calcium-containing waste powder, The calcium-containing waste powder is The insoluble residue measured in accordance with JIS R 5202:2010 is 70.0% by mass or less, Contains 5.0% by mass or more of calcium carbonate, and The residual amount of CaO, after subtracting the amount of CaO derived from calcium carbonate, is 18.0% by mass or less, The object of the present invention is to provide a cement composition containing the calcium-containing waste powder in an amount of 1.0 mass % or more and 7.5 mass % or less.

[0009] Another aspect of the present disclosure is a method for producing a cement composition including cement and a calcium-containing waste powder, the method comprising: The calcium-containing waste powder is The insoluble residue measured in accordance with JIS R 5202:2010 is 70.0% by mass or less, Contains 5.0% by mass or more of calcium carbonate, and The residual amount of CaO, after subtracting the amount of CaO derived from calcium carbonate, is 18.0% by mass or less, The object of the present invention is to provide a method for producing a cement composition, which comprises mixing the cement composition with the calcium-containing waste powder so that the calcium-containing waste powder is contained in the cement composition in an amount of 0.5 mass % to 7.5 mass %. [Effects of the Invention]

[0010] According to the present disclosure, a cement composition and a method for producing the same are provided that, by effectively utilizing waste and by-products, reduces the environmental impact while exhibiting strength development at a level equivalent to that of current Portland cement, and that is particularly excellent in early strength. DETAILED DESCRIPTION OF THE INVENTION

[0011] Unless otherwise specified, the materials exemplified in this disclosure can be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the cement composition according to the present disclosure, the content of each component in the cement composition means the total amount of the multiple substances present in the cement composition, unless otherwise specified.

[0012] One embodiment of a cement composition according to the present disclosure includes cement and calcium-containing waste powder.

[0013] As the cement, any cement known in the relevant technical field can be used without particular limitation. For example, ordinary Portland cement, early-strength Portland cement, medium-heat cement, low-heat cement, oil well cement, etc. can be used. From the viewpoints of easy availability and further improvement of initial strength, the cement preferably contains at least one of ordinary Portland cement and early-strength Portland cement, more preferably contains at least early-strength Portland cement, and it is also possible to use only early-strength Portland cement.

[0014] The cement clinker in the cement contains C3S, C2S, C3A, and C4AF. The respective contents of C3S, C2S, C3A, and C4AF can be calculated by the Bogue formula. The Bogue formula is a widely used formula for calculating the content ratio of the main minerals in cement clinker from the content ratio of chemical compositions. By using the Bogue formula shown below, the contents of tricalcium silicate (3CaO·SiO2, denoted as C3S), dicalcium silicate (2CaO·SiO2, denoted as C2S), tricalcium aluminate (3CaO·Al2O3, denoted as C3A), and tetracalcium aluminoferrite (4CaO·Al2O3·Fe2O3, denoted as C4AF) in the cement clinker can be calculated. The chemical formula represents the content ratio (mass %) of each compound shown by the chemical analysis values according to JIS R 5204:2019 "Fluorescent X-ray Analysis Method for Cement".

[0015] <Bogue formula> C3S [mass %] = (4.07 × CaO [mass %]) - (7.60 × SiO2 [mass %]) - (6.72 × Al2O3 [mass %]) - (1.43 × Fe2O3 [mass %]) - (2.85 × SO3 [mass %]) C2S [mass %] = (2.87 × SiO2 [mass %]) - (0.754 × C3S [mass %]) C3A [mass %] = (2.65 × Al2O3 [mass %]) - (1.69 × Fe2O3 [mass %]) C4AF [mass %] = 3.04 × Fe2O3 [mass %]

[0016] The amount of C3S in the cement clinker in the cement is preferably 50.0 mass% or more, more preferably 55.0 mass% or more, even more preferably 60.0 mass% or more, and even more preferably 65.0 mass% or more. By making the amount of C3S equal to or more than the above value, the early strength of the cement composition upon hardening can be further improved. The amount of C3S in the cement clinker is preferably 80.0 mass% or less, more preferably 75.0 mass% or less, and even more preferably 70.0 mass% or less. By keeping the amount of C3S at the above value or less, heat generation during hardening of the cement composition can be suppressed.

[0017] The amount of C2S in the cement clinker is preferably 2.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 8.0 mass% or more. By making the amount of C2S equal to or more than the above value, the long-term strength of the cement composition upon hardening can be further improved. The amount of C2S in the cement clinker is preferably 40.0 mass% or less, more preferably 30.0 mass% or less, even more preferably 15.0 mass% or less, and even more preferably 10.0 mass% or less. By making the amount of C2S less than the above value, the early strength of the cement composition upon hardening can be further improved.

[0018] The amount of C3A in the cement clinker is preferably 7.0% by mass or more, more preferably 8.0% by mass or more, even more preferably 9.0% by mass or more, even more preferably 9.5% by mass or more, and particularly preferably 10.0% by mass or more. By making the amount of C3A equal to or more than this value, it is possible to produce a cement composition that uses an increased amount of waste and by-products such as coal ash, which are used as raw materials for cement clinker. The C3A content in cement clinker is preferably 13.0 mass% or less, more preferably 12.0 mass% or less, even more preferably 11.0 mass% or less, even more preferably 10.5 mass% or less, and particularly preferably 10.0 mass% or less. By keeping the C3A content at or below this value, it is possible to suppress the regeneration of ettringite (a compound represented by 3CaO·Al2O3·3CaSO4·32H2O), and also to further reduce the increase in heat generation when the cement composition hardens.

[0019] The C4AF content in cement clinker is preferably 5.0% by mass or more, more preferably 6.0% by mass or more, even more preferably 7.0% by mass or more, even more preferably 8.0% by mass or more, and particularly preferably 8.5% by mass or more. By making the C4AF content equal to or greater than the above value, it is possible to produce a cement composition that uses an increased amount of waste and by-products such as coal ash, which are used as raw materials for cement clinker. The C4AF content in the cement clinker is preferably 14.0 mass% or less, more preferably 12.0 mass% or less, even more preferably 11.0 mass% or less, still more preferably 10.0 mass% or less, and particularly preferably 9.0 mass% or less. By keeping the C4AF content at or below the above value, the increase in the calorific value when the cement composition hardens can be further reduced.

[0020] The content of cement clinker is preferably 70% by mass or more and 95% by mass or less, more preferably 75% by mass or more and 93% by mass or less, and even more preferably 85% by mass or more and 90% by mass or less, when the total amount of cement is 100% by mass.

[0021] The cement may contain gypsum. Examples of gypsum that can be used include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. One type of gypsum may be used alone, or a combination of two or more types may be used. The gypsum content in the cement may be the same as the gypsum content in general Portland cement. Specifically, the gypsum content in the cement, calculated as SO3, is preferably 0.5% by mass or more and 3.5% by mass or less, more preferably 0.7% by mass or more and 3.0% by mass or less, and even more preferably 1.0% by mass or more and 2.5% by mass or less, based on 100% by mass of the total amount of cement.

[0022] The cement may be commercially available Portland cement or a mixture of cement clinker, gypsum, limestone and / or calcium carbonate, which have been separately ground and mixed together. Alternatively, two or more materials may be ground simultaneously to produce a cement mixture.

[0023] The cement content in the cement composition according to the present disclosure is preferably 92.0% by mass or more, more preferably 93.5% by mass or more, and even more preferably 94.5% by mass or more, based on the cement composition. By making the cement content equal to or greater than this value, the cement composition according to the present disclosure has strength development at the same level as ordinary Portland cement, and is particularly excellent in early strength. Furthermore, the cement content in the cement composition according to the present disclosure is preferably 99.5% by mass or less, more preferably 98.5% by mass or less, even more preferably 97.0% by mass or less, and even more preferably 95.5% by mass or less, based on the cement composition. By setting the cement content to the above value or less, waste materials such as waste concrete and waste mortar that have been discarded in the past can be effectively utilized, thereby reducing the environmental burden.

[0024] The cement composition according to the present disclosure contains calcium-containing waste powder in addition to cement. In the present disclosure, the term "calcium-containing waste powder" refers to powder of various waste materials that have no specific use and are normally disposed of, and that contain calcium.

[0025] The calcium-containing waste powder is derived from waste materials such as waste concrete, waste mortar, waste cement paste, concrete sludge, paper sludge, blast furnace slag, converter slag, electric furnace slag, slowly cooled slag, chlorine bypass dust, coal ash, biomass ash, or incineration ash. The calcium-containing waste powder is not the waste material itself, but the residue remaining after calcium is extracted from the waste material. In other words, the calcium-containing waste powder in the present disclosure refers to the calcium-containing waste powder after calcium extraction. The waste material preferably contains calcium in an amount calculated as CaO of 5.0 mass % or more, more preferably 10.0 mass % or more, and even more preferably 20.0 mass % or more, from the viewpoint of enabling efficient recovery of calcium from the waste material and contributing to resource recycling.

[0026] In particular, the calcium-containing waste powder is preferably the residue obtained after calcium extraction from at least one waste material selected from waste concrete, waste mortar, and waste cement paste. By using the residues of these waste materials as components of a cement composition, materials that have previously been discarded can be effectively utilized, thereby reducing the environmental impact. Furthermore, the cement composition of the present disclosure containing the calcium-containing waste powder has strength development equivalent to that of ordinary Portland cement, and is particularly excellent in early strength.

[0027] The calcium-containing waste powder has a Blaine specific surface area of ​​2500 cm 2 / g or more 20000cm 2 / g or less, and 2 / g or more 15000cm 2 / g or less, and more preferably 6000 cm 2 / g or more 10000cm 2 / g or less is even more preferable. The Blaine specific surface area is measured in accordance with the description of JIS R 5201:2015 "Physical Measurement Methods of Cement." A calcium-containing waste powder having a Blaine specific surface area value in this range can be obtained by subjecting the residue after calcium extraction from waste materials such as waste concrete to processing such as crushing, sieving, and classification. By having the calcium-containing waste powder have a Blaine specific surface area value in this range, the cement composition according to the present disclosure can reduce production costs and have strength development at a level equivalent to that of ordinary Portland cement, and is particularly excellent in early strength.

[0028] In relation to the Blaine specific surface area value of the calcium-containing waste powder, the Blaine specific surface area value of the cement composition is 2500 cm from the same viewpoint as above. 2 / g or more 6000cm 2 / g or less, and 2 / g or more 5000cm 2 / g, and more preferably 3500 cm 2 / g or more 4500cm 2 The Blaine specific surface area is measured in accordance with the description of JIS R 5201:2015 "Physical measurement methods for cement."

[0029] The calcium-containing waste powder preferably has an insoluble residue of 70.0% or less, more preferably 60.0% or less, and even more preferably 55.0% or less, as measured in accordance with JIS R 5202:2010 "Methods for Chemical Analysis of Cement." By setting the insoluble residue of the calcium-containing waste powder to the above value or less, the amount of highly crystalline, low-reactivity components such as sand can be reduced, which has the advantage of increasing the strength development of the cement composition when added as an admixture. Furthermore, there is no particular lower limit for the insoluble residue of the calcium-containing waste powder, but it is preferably 1.0% or more, more preferably 5.0% or more, even more preferably 10.0% or more, even more preferably 25.0% or more, and even more preferably 50.0% or more. Setting the insoluble residue of the calcium-containing waste powder to the above value or more has the advantage of reducing the cost of separating highly crystalline, low-reactivity components such as sand from the waste. The insoluble residue of the calcium-containing waste powder can be adjusted to the above value by separating the relatively low-strength, soft components such as cement paste from the highly crystalline, hard components such as sand, for example, by processes such as crushing, grinding, sieving, and classification.

[0030] The calcium-containing waste powder preferably contains 5.0% by mass or more of calcium carbonate, more preferably 10.0% by mass or more, more preferably 12.0% by mass or more, even more preferably 15.0% by mass or more, and even more preferably 20.0% by mass or more. By setting the calcium carbonate content in the calcium-containing waste powder to the above value or more, the cement composition according to the present disclosure will have strength development equivalent to that of ordinary Portland cement, and will have particularly excellent early strength. Furthermore, since a sufficient amount of calcium carbonate produced by carbon dioxide fixation is contained in the calcium-containing waste, it can contribute to reducing carbon dioxide emissions. The higher the proportion of calcium carbonate contained in the calcium-containing waste powder, the more desirable it is from the viewpoint of improving the strength development of the cement composition according to the present disclosure. However, if the proportion of calcium carbonate is as high as about 40.0 mass%, the strength development is sufficiently improved.

[0031] The amount of calcium carbonate contained in the calcium-containing waste powder is measured, for example, by TG-DTA. In this measurement, the mass loss in the temperature range of 500°C to 800°C is assumed to be due to decarbonation of CO2 from calcium carbonate, and the amount of calcium carbonate can be calculated from the mass loss value.

[0032] In the calcium-containing waste powder, the residual CaO content, after subtracting the amount of CaO derived from calcium carbonate, is preferably 18.0% by mass or less, more preferably 15.0% by mass or less, even more preferably 12.0% by mass or less, and even more preferably 10.0% by mass or less. The residual CaO content refers to the degree of calcium extraction when obtaining calcium-containing waste powder from waste materials such as waste concrete and waste mortar. Setting the residual CaO content to the above value or less means that calcium is sufficiently extracted when obtaining calcium-containing waste powder from the waste materials, which is advantageous from the perspective of effective calcium utilization and the ability to effectively obtain calcium carbonate by reacting calcium with carbon dioxide. From this perspective, there is no particular lower limit for the residual CaO content, but it may be 0% by mass or more, 3.0% by mass or more, 6.0% by mass or more, or 9.0% by mass or more. The amount of residual CaO is measured as follows. First, the total CaO content is calculated from chemical composition analysis using fluorescent X-rays. Next, from TG-DTA measurement, the mass loss at 500 to 800°C is considered to be decarbonation from calcium carbonate, and the amount of calcium carbonate is calculated using the following formula. Amount of calcium carbonate (mass%) = (mass loss from 500°C to 800°C) (mass%) × 100 / 44 The remaining amount of CaO, after subtracting the amount of CaO derived from calcium carbonate, can be calculated using the following formula. Residual amount of CaO (mass%) = Total CaO content (mass%) - (amount of calcium carbonate) (mass%) × 56 / 100

[0033] The calcium-containing waste powder preferably has an R2O content defined by the following formula (1) of 2.5 mass% or less, more preferably 2.0 mass% or less, and even more preferably 1.5 mass% or less. From the viewpoint of inhibiting the alkali-silica reaction, it is desirable to reduce the total amount of alkali in cement and concrete, and from that viewpoint, it is desirable to reduce the R2O content of the calcium-containing waste powder. The R2O content of the calcium-containing waste powder can be determined by chemical composition analysis using fluorescent X-rays. R2O amount [mass%]=Na2O+K2O×0.658[mass%] (1) Na2O and K2O represent the contents [mass %] of Na2O and K2O, respectively.

[0034] The calcium-containing waste powder preferably has a basicity of 0.50 or more, more preferably 0.70 or more, and even more preferably 0.90 or more. Generally, basicity is an index that indicates the reactivity of ground granulated blast furnace slag; the higher the basicity, the higher the reactivity and the better the strength development. Similarly, the higher the basicity, the better the strength development when calcium-containing waste powder is added. From this perspective, there is no particular upper limit on the basicity, but it may be 3.0 or less, 2.0 or less, 1.5 or less, or 1.0 or less. The basicity of the calcium-containing waste powder can be calculated from the component values ​​obtained by chemical component analysis using fluorescent X-rays using the following formula (2): Basicity = (CaO + Al2O3 + MgO) / SiO2(2) CaO, Al2O3, MgO, and SiO2 represent the contents [mass %] of CaO, Al2O3, MgO, and SiO2, respectively.

[0035] The calcium-containing waste powder is the residue left after calcium is extracted from calcium-containing waste materials, and there are no particular limitations on the method for extracting calcium from the waste materials. To efficiently and sufficiently extract calcium from the waste materials, it is desirable to employ a method in which the carbon dioxide partial pressure is increased above atmospheric pressure. Specifically, it is preferable to employ a method comprising the following steps (a) to (c): (a) A step of preparing a powder of calcium-containing waste material. (b) A step of setting the partial pressure of carbon dioxide to more than 0.1 MPa and not more than 5.0 MPa, and dispersing or dissolving the powder in water under said partial pressure to prepare a liquid to be extracted. (c) A step of separating the liquid component and the solid residue from the liquid to be extracted.

[0036] The powdering of the waste material in step (a) can be carried out using various conventionally known techniques. The average particle size of the powdered waste material may be set to a specific surface area large enough to efficiently extract calcium from the waste material, for example, 10 μm to 5 mm. This step not only includes the actual pulverization of the waste material, but also includes cases where finely powdered waste containing calcium is obtained in advance, such as incineration ash discharged from a thermal power plant.

[0037] In step (b), by setting the partial pressure of carbon dioxide in the gas phase in contact with the liquid to be extracted within the above range, the concentration of calcium ions extracted into the liquid phase can be increased, thereby improving the efficiency of recycling calcium from calcium-containing waste materials. From this perspective, it is more preferable that the partial pressure of carbon dioxide is 0.1 MPa or more and 3 MPa or less.

[0038] The components other than carbon dioxide in the gas phase can be components generally contained in the atmosphere. That is, examples of the components other than carbon dioxide in the gas phase include nitrogen and oxygen. The gas phase is conveniently a gas obtained by supplying carbon dioxide to the atmosphere and increasing the partial pressure of carbon dioxide.

[0039] From the viewpoint of efficient extraction of calcium, it is preferable to carry out step (b) by adding the finely powdered waste to water under the above-mentioned carbon dioxide partial pressure and stirring for a predetermined time, for example, from 1 minute to 90 minutes. From the same viewpoint, the liquid to be extracted is preferably kept at 20°C or higher and 80°C or lower, more preferably 20°C or higher and 50°C or lower, and even more preferably 20°C or higher and 30°C or lower.

[0040] In step (c), it is preferable to perform solid-liquid separation while maintaining the partial pressure of carbon dioxide in the gas phase within the above-mentioned range and the temperature of the liquid to be extracted within the above-mentioned range. Solid-liquid separation can be performed using a conventionally known filtration technique. Seed crystals may also be added to the liquid phase.

[0041] The calcium-containing waste obtained in this manner before pulverization preferably has an average particle size of 10 μm or more and 1000 μm or less, from the viewpoint of improving the strength development and pulverization efficiency of the cement composition according to the present disclosure. To further enhance this advantage, the average particle size of the calcium-containing waste is more preferably 300 μm or more and 600 μm or less, and even more preferably 400 μm or more and 500 μm or less. The average particle size of calcium-containing waste can be determined by particle size measurement using sieving, etc. Specific methods include, for example, using the sieving test method for aggregates in JIS A 1102:2014, and measuring in the same manner as in the sieving test for fine aggregates.

[0042] The calcium-containing waste obtained by the above-mentioned method may be used as is, or may be subjected to crushing, sieving, and classification to obtain a desired average particle size. In the latter case, the average particle size is preferably 2 μm or more and 50 μm or less from the viewpoint of strength development and fluidity retention. To further enhance this advantage, the average particle size of the calcium-containing waste is more preferably 5 μm or more and 30 μm or less, and even more preferably 10 μm or more and 20 μm or less.

[0043] The content of calcium-containing waste powder in the cement composition according to the present disclosure is preferably 7.5% by mass or less, more preferably 6.5% by mass or less, and even more preferably 5.5% by mass or less, based on the cement composition. By setting the content of calcium-containing waste powder to the above value or less, the cement composition according to the present disclosure has strength development at the same level as ordinary Portland cement, and is particularly excellent in early strength. Furthermore, the content of calcium-containing waste powder in the cement composition according to the present disclosure is preferably 0.5% by mass or more, more preferably 1.5% by mass or more, even more preferably 3.0% by mass or more, and even more preferably 4.5% by mass or more, relative to the cement composition. By making the content of calcium-containing waste powder equal to or more than the above value, waste materials such as waste concrete and waste mortar that have been discarded until now can be effectively utilized, thereby reducing the environmental burden.

[0044] The cement composition according to the present disclosure may contain limestone in addition to cement and calcium-containing waste powder. Examples of limestone that can be used include commonly available powders containing calcium carbonate as a main component, such as limestone, limestone powder, and kansui stone powder. The limestone preferably includes limestone that complies with the minor mixing components specified in JIS R 5210:2019 "Portland Cement."

[0045] The limestone content in the cement composition according to the present disclosure is preferably 15.0 mass% or less, more preferably 10.0 mass% or less, and even more preferably 5.0 mass% or less, based on the cement composition. By setting the limestone content to the above value or less, the cement composition will have excellent strength development. The limestone content in the cement composition according to the present disclosure is preferably 1.5% by mass or more, more preferably 3.0% by mass or more, and even more preferably 4.6% by mass or more, based on the cement composition. By making the limestone content equal to or greater than this value, strength development is improved compared to when limestone is not added, while contributing to a reduction in carbon dioxide emissions.

[0046] In addition to cement and calcium-containing waste powder, the cement composition according to the present disclosure may contain other components within the scope of the present disclosure, such as calcium hydroxide, silica powder, other calcium-containing powders (excluding gypsum and limestone), concrete water-reducing agents, accelerators, and retarders.

[0047] The cement composition according to the present disclosure is preferably obtained by a manufacturing method in which cement and calcium-containing waste powder are mixed so that the calcium-containing waste powder is contained in the cement composition in an amount of preferably 1.0 mass % or more and 7.5 mass % or less.

[0048] The cement composition according to the present disclosure may be mixed with ground granulated blast furnace slag, fly ash, silica fume, or the like and used as a mixed cement. 3 It may also be used with cements outside of JIS standards, such as Lime Calcined Clay Cement. [Example]

[0049] The present disclosure will be described in more detail below with reference to examples, comparative examples, and reference examples, although the present disclosure is not limited to the following examples.

[0050] [Raw materials for cement compositions] The following materials were used as raw materials for the cement composition.

[0051] (1) Preparation of cement clinker The cement clinkers used were ordinary Portland cement clinker (cement clinker A) and high-early-strength Portland cement clinker (cement clinker B), whose mineral compositions according to the Bogue formula are listed in Table 1. The chemical composition of the cement used in the Bogue formula calculation was measured in accordance with the method specified in JIS R 5204:2019 "Method for X-ray fluorescence analysis of cement."

[0052] [Table 1]

[0053] (2) Plaster preparation The gypsum used met the requirements set forth in JIS R 9151:2009 "Natural gypsum for cement."

[0054] (3) Preparation of limestone powder The limestone (LS) used was a fine powder of crushed limestone that had a calcium carbonate content of 90.0% by mass or more and an aluminum oxide content of 1.0% by mass or less, and that met the requirements for minor mixed components described in JIS R 5210:2019 "Portland cement" (Blaine specific surface area: 7470 cm). 2 / g).

[0055] (4) Calcium-containing waste powder Waste concrete was crushed and sieved to obtain powder with sieving openings of 2 mm or less. The powder was then added to pure water to obtain a dispersion. This dispersion was airtightly packed into a pressure-resistant stirring tank type extraction device, and while stirring, carbon dioxide was supplied into the device and the partial pressure was increased to 1.0 MPa to extract calcium into the liquid phase. During this time, the pressure of the gas phase was monitored and the partial pressure of carbon dioxide was maintained. The reactor was then separated into a liquid phase and an extraction residue, and the liquid phase to which the seed crystals had been added was depressurized to obtain calcium carbonate. The solid fraction obtained by the solid-liquid separation was recovered to obtain an extraction residue. The extraction residue was dried at 105°C to remove moisture, and the target calcium-containing waste was obtained. Table 2 shows the particle size of calcium-containing waste before crushing. For reference, the particle sizes of the Cement Association's standard sand and a typical silica sand (product name: Toyoura Silica Sand, manufacturer: Toyoura Silica Industry Co., Ltd.) are also shown. It can be seen that calcium-containing waste has a particle size distribution relatively close to that of standard sand. It can also be seen that calcium-containing waste contains approximately 5.0 mass% of fine powder of 0.063 mm or less.

[0056] [Table 2]

[0057] Calcium-containing waste was milled in 50 g portions for 60 seconds using a stainless steel disc mill to obtain calcium-containing waste powder. The Blaine specific surface area of ​​the calcium-containing waste powder was 8090 cm 2 / g. The Blaine specific surface area was measured in accordance with JIS R 5201:2015 "Physical Measurement Methods for Cement." The average particle size of the calcium-containing waste powder was 17.0 μm. The average particle size was measured using a laser diffraction scattering particle size distribution analyzer (Malvern Instruments, Mastersizer 3000E).

[0058] The physical properties of the calcium-containing waste powder are shown in Tables 3 and 4. The densities shown in these tables were measured using an automatic density meter (instrument: MAT-7000, Seishin Enterprise Co., Ltd.).

[0059] The chemical composition of the calcium-containing waste powder was determined by chemical analysis using the fundamental parameter method using fluorescent X-rays (equipment used: Rigaku ZSX-100e). Loss on ignition (Ignition loss) and insoluble residue were measured according to JIS R 5202:2010 "Methods for Chemical Analysis of Cement." The calcium carbonate content of the calcium-containing waste was calculated by assuming the loss from 500°C to 800°C in TG-DTA measurement (equipment name: Hitachi High-Tech STA-7300, nitrogen gas flow environment, heating rate: 10°C / min) to be the loss of carbon dioxide due to the decarbonation of calcium carbonate. [Table 3]

[0060] [Table 4]

[0061] [Production of cement composition] Base cement was obtained by adding 1.0% gypsum, calculated as SO3, to Portland cement clinker having the chemical composition shown in Table 1, and mixing and grinding the mixture. Cement compositions were obtained by mixing the base cement, the calcium-containing waste powder, and limestone powder in the proportions shown in Table 5. The Blaine specific surface area values ​​of the obtained cement compositions are shown in Table 5.

[0062] [Evaluation of cement composition] The compressive strength of the resulting cement composition was evaluated at a predetermined age. Compressive strength was measured using a 10 x 10 x 60 mm rectangular column specimen. The water-cement ratio was 0.50, the sand-cement ratio was 1.0, and silica sand (product name: Toyoura Silica Sand, manufacturer: Toyoura Silica Industry Co., Ltd.) with the particle size shown in Table 2 was used as sand. To form the mortar, 50 g of water, 100 g of cement, and 100 g of sand were mixed in a chemical mixer at 500 rpm for 3 minutes and then poured into a 10 x 10 x 60 mm formwork. The mixture was sealed and cured for 24 hours, then demolded and underwater cured until the desired age was reached. The compressive strengths of Example 1 and Comparative Example 1 were evaluated as a compressive strength ratio when the compressive strength of the specimen of Reference Example 1 was set to 100. The compressive strengths of Example 2 and Comparative Example 2 were evaluated as a compressive strength ratio when the compressive strength of the specimen of Reference Example 2 was set to 100.

[0063] [Table 5]

[0064] As is clear from the results shown in Table 5, the hardened bodies obtained in the examples exhibited compressive strengths as high as those of the hardened bodies of the reference examples. In particular, the hardened bodies obtained in each example have high compressive strength at 7 days. Furthermore, in the case of Example 2, which used high-early-strength Portland cement as the base cement, the compressive strength at 28 days is higher than in Example 1, which used ordinary Portland cement.

Claims

1. A cement composition comprising cement and a calcium-containing waste powder, The calcium-containing waste powder is The insoluble residue measured in accordance with JIS R 5202:2010 is 70.0% by mass or less, Contains 5.0% by mass or more of calcium carbonate, and The residual amount of CaO, which is obtained by subtracting the amount of CaO derived from calcium carbonate, is 18.0% by mass or less, The calcium-containing waste powder is contained in an amount of 0.5% by mass or more and 7.5% by mass or less.

2. The calcium-containing waste powder has a Blaine specific surface area of ​​2500 cm 2 / g or more 20000cm 2 The cement composition of claim 1, wherein the Cementitious Agent is Cr, Mn, MnO, MnO+, MnO2, MnO+ ...

3. The calcium-containing waste powder represented by the following formula (1) R 2 The cement composition according to claim 1, wherein the O content is 2.5 mass% or less. R 2 O amount [mass %] = Na 2 O+K 2 O×0.658[% by mass] (1)

4. 2. The cement composition of claim 1, wherein the calcium-containing waste powder is derived from a waste material selected from waste concrete, waste mortar, and waste cement paste.

5. C of the cement clinker in the cement 3 The cement composition according to claim 1, wherein the S content is 50.0 mass% or more and 80.0 mass% or less.

6. Blaine specific surface area is 2500 cm 2 / g or more 6000cm 2 The cement composition of claim 1, wherein the Cementitious Agent is Cr, Mn, MnO, MnO+, MnO2, MnO+ ...

7. A method for producing a cement composition comprising cement and a calcium-containing waste powder, comprising the steps of: The calcium-containing waste powder is The insoluble residue measured in accordance with JIS R 5202:2010 is 70.0% by mass or less, Contains 5.0% by mass or more of calcium carbonate, and The residual amount of CaO, which is obtained by subtracting the amount of CaO derived from calcium carbonate, is 18.0% by mass or less, A method for producing a cement composition, comprising mixing the cement and the calcium-containing waste powder so that the calcium-containing waste powder is contained in the cement composition in an amount of 0.5 mass % or more and 7.5 mass % or less.

8. The method according to claim 7, wherein the calcium-containing waste powder is derived from a waste material selected from waste concrete, waste mortar and waste cement paste.

9. Prepare a powder of waste material containing calcium; The partial pressure of carbon dioxide is set to more than 0.1 MPa and not more than 5.0 MPa, and the powder is dispersed or dissolved in water under the partial pressure to prepare a liquid to be extracted; The method according to claim 7, wherein the calcium-containing waste powder is obtained by separating a liquid component and a solid residue from the liquid to be extracted.

Citation Information

Patent Citations

  • Process for the production of aggregates for making road foundations and the like

    EP2272598A1

  • Production of building material

    JP1991295839A

  • Treatment of concrete waste

    JP1999319765A

  • Method and system for producing calcium carbonate

    JP2013129543A

  • Concrete binder for blast furnace cement concrete