Base paper for vapor-deposited paper, vapor-deposited paper, and packaging bag
The base paper for vapor-deposited paper, with a resin layer and pigment coating layer, addresses the need for improved printability and processability in metallized paper, ensuring excellent performance in automatic packaging.
Patent Information
- Application Number
- JP2023128435
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-08-07
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Metallized paper used for packaging materials requires excellent printability and processability, particularly in automatic packaging, which existing technologies do not adequately address.
A base paper for vapor-deposited paper is designed with a resin layer on one side and a pigment coating layer on the other, featuring specific pigment content and smoothness, along with controlled friction coefficients, to enhance printability and processability.
The solution provides vapor-deposited paper with excellent printability and processability, suitable for automatic packaging applications, maintaining these properties even after forming a vapor-deposited layer.
Smart Images

Figure 2024155665000001 
Figure 2024155665000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a base paper for metallized paper, metallized paper using the same, and a packaging bag using the metallized paper. [Background technology]
[0002] Conventionally, packaging materials having a paper base material imparted with water vapor barrier properties that provide a barrier against water vapor, gas barrier properties that provide a barrier against gases other than water vapor, and in particular, oxygen barrier properties that provide a barrier against oxygen, have been used in packaging foods, medical products, electronic components, and the like to prevent deterioration of the contents.
[0003] Metal-deposited paper is a paper base material on which a metal-deposited layer is provided in order to improve the barrier properties of the paper base material against oxygen and water vapor.
[0004] Patent Document 1 discloses a base paper for metallized paper for forming a metallized layer by deposition, which has a coating layer having a clay coat layer and a resin layer containing a water-dispersible polyurethane resin in this order from the paper substrate side on at least one side of the paper substrate, the Cobb water absorbency of the surface having the coating layer is in a specific range, and the contact angle of the coating layer surface with water is a specific value or less. Patent Document 2 discloses a base paper for metallized paper for forming a metallized layer by deposition, which has a clay coat layer and a resin layer in this order on at least one side of the paper substrate, the wetting tension of the resin layer surface is a specific value or more, and the surface roughness is a specific value or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6958756 [Patent Document 2] Patent No. 6958757 Summary of the Invention [Problem to be solved by the invention]
[0006] Metallized paper used as a packaging material for food and the like is required to have excellent printability on the printing surface and, particularly when used as a packaging bag, excellent processability in automatic packaging.
[0007] Therefore, an object of the present invention is to provide a base paper for metallized paper that provides metallized paper having excellent printability and processability in automatic packaging, and to provide metallized paper made using the base paper. Another object of the present invention is to provide a packaging bag made using the metallized paper. [Means for solving the problem]
[0008] The inventors have discovered that the above problem can be solved by providing a base paper for metallized paper having a pigment coating layer containing a specific amount of pigment on the other side of the paper substrate, and the side having the pigment coating layer has an Oken smoothness of a specific value or more and a dynamic friction coefficient against stainless steel of a specific value or less.
[0009] That is, the present invention has the following configuration. <1> A base paper for metallized paper having a resin layer on one side of a paper substrate, for forming a metallized layer on the resin layer, and having a pigment coating layer on the other side of the paper substrate, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, the side having the pigment coating layer having an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <2> A clay coating layer is provided between the paper base material and the resin layer. <1> 2. A base paper for metallized paper according to claim 1. <3> The resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin. <1> or <2> 2. A base paper for metallized paper according to claim 1. <4> A base paper for metallized paper has a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate, the metallized paper having a metallized layer on the resin layer, wherein the pigment content in the pigment coating layer is 50% by mass or more and 85% by mass or less, and the surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <5> A heat seal layer is provided on the deposition layer. <4> The metallized paper described in <6> An overcoat layer is provided between the deposition layer and the heat seal layer. <5> The metallized paper described in <7> A clay coating layer is provided between the paper base material and the resin layer. <4> ~ <6> 13. The metallized paper according to claim 12, <8> The resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin. <4> ~ <7> 13. The metallized paper according to claim 12, <9> <4> ~ <8> A packaging bag made using the metallized paper described in any one of the above. Effect of the Invention
[0010] According to the present invention, there is provided a base paper for metallized paper that provides metallized paper having excellent printability and processability in automatic packaging, and a metallized paper made using the base paper. Furthermore, according to the present invention, there is provided a packaging bag made using the metallized paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Base paper for metallized paper] The base paper for metallized paper of this embodiment (hereinafter also simply referred to as base paper for metallized paper) has a resin layer on one side of a paper substrate, is a base paper for metallized paper for forming a metallized layer on the resin layer, has a pigment coating layer on the other side of the paper substrate, the pigment coating layer has a pigment content of 50% by mass or more and 85% by mass or less, and the surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The base paper for metallized paper of this embodiment provides a metallized paper with excellent printability and processability in automatic packaging.
[0012] The configuration and physical properties of the base paper for metallized paper of this embodiment will be described in more detail below. In this specification, the numerical range represented by "X to Y" means a numerical range including X as the lower limit and Y as the upper limit. When the numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. In addition, "(meth)acrylic" is a generic term including both acrylic and methacrylic.
[0013] The base paper for metallized paper of this embodiment has a resin layer on one side of a paper substrate, on which a metallized layer can be formed, and has a pigment coating layer on the other side of the paper substrate. From the viewpoint of smoothing the surface of the paper substrate, the base paper for metallized paper of this embodiment preferably has a clay coat layer between one side of the paper substrate and the resin layer. That is, the base paper for metallized paper of this embodiment preferably has a clay coat layer on one side of the paper substrate, and a resin layer on the clay coat layer.
[0014] <Paper base material> The pulp constituting the paper base material in this embodiment is preferably mainly composed of plant-derived pulp, and more preferably mainly composed of wood pulp. Examples of wood pulp include hardwood pulp and softwood pulp. Examples of non-wood pulp include cotton pulp, hemp pulp, kenaf pulp, bamboo pulp, etc. Materials other than pulp fibers, such as synthetic fibers such as rayon fibers and nylon fibers, may also be blended as secondary paper materials as long as they do not impair the effects of the present invention.
[0015] From the viewpoints of the texture, physical properties and recyclability of the metallized paper, the proportion of hardwood pulp in the pulp constituting the paper base material is preferably 65% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, and may be 100% by mass.
[0016] Examples of the internal sizing agent include rosin-based, alkyl ketene dimer-based, alkenyl succinic anhydride-based, styrene-unsaturated carboxylic acid-based, higher fatty acid-based, petroleum resin-based, etc. The content of the internal sizing agent is not particularly limited, but is preferably 0 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the pulp (bone dry mass) of the paper base material.
[0017] In addition to the internal sizing agent, other known internal additives may be added to the paper base material, such as fillers, paper strength agents, retention aids, pH adjusters, drainage improvers, water resistance agents, softeners, antistatic agents, defoamers, slime control agents, dyes, and pigments.
[0018] Examples of fillers include titanium dioxide, kaolin, talc, calcium carbonate (heavy calcium carbonate, light calcium carbonate), calcium sulfite, gypsum, calcined kaolin, white carbon, amorphous silica, delaminated kaolin, diatomaceous earth, magnesium carbonate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, and the like.
[0019] The paper base material is obtained by making a papermaking raw material mainly composed of a pulp slurry. The pulp slurry can be obtained from wood or non-wood raw material chips through processes such as cooking, washing, and bleaching. There are no particular limitations on the methods used in the cooking, washing, and bleaching processes. The pulp slurry obtained through these processes is preferably further beaten in the presence of water.
[0020] In the papermaking of the paper base material, a known wet papermaking machine can be appropriately selected and used. Examples of the papermaking machine include a fourdrinier papermaking machine, a gap former type papermaking machine, a cylinder papermaking machine, and a short wire papermaking machine. The paper layer formed by the papermaking machine is preferably conveyed, for example, by a felt and dried by a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying by the dryer.
[0021] The paper base material obtained as described above may be subjected to a surface treatment using a calendar to uniformize the paper thickness and gloss profile. For the calendar treatment, a known calendaring machine can be appropriately selected and used.
[0022] Specific examples of the paper substrate used for the base paper for metallized paper of this embodiment include bleached kraft paper, unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-sided glossy paper, glassine paper, graphene paper, etc. Among these, bleached kraft paper, unbleached kraft paper, fine paper, and one-sided glossy paper are preferred.
[0023] (Stockigt size) The paper substrate is not particularly limited, but from the viewpoint of improving the barrier property, the Stockigt sizing degree of at least the surface on which the resin layer described later is provided is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 5 seconds or more, and the upper limit is not particularly limited, but is preferably 100 seconds or less, more preferably 30 seconds or less. The Stockigt sizing degree of the paper substrate is measured in accordance with JIS P 8122:2004. The Stockigt sizing degree of the paper substrate can be controlled by the type and content of the internal sizing agent, the type of pulp, smoothing treatment, etc.
[0024] (Basic weight) The basis weight of the paper base material is not particularly limited, but is preferably 20 g / m from the viewpoint of strength when used as a packaging bag. 2 More preferably, 30 g / m 2 More preferably, 40 g / m 2 From the viewpoints of economy and ease of production, it is preferably 500 g / m 2 Less than 400 g / m 2 More preferably, 200 g / m 2 More preferably, 100 g / m 2 The basis weight of the paper base material is measured in accordance with JIS P 8124:2011.
[0025] (Thickness) The thickness of the paper substrate is not particularly limited, but from the viewpoint of strength when used as a packaging bag, it is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 30 μm or more, and even more preferably 50 μm or more, and from the viewpoint of economy and ease of production, it is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 75 μm or less. The thickness of the paper substrate is measured in accordance with JIS P 8118:2014.
[0026] (density) The density of the paper base material is preferably 0.5 g / cm from the viewpoint of moldability. 3 More preferably, 0.6 g / cm 3 More preferably, 0.7 g / cm 3 and preferably 1.2 g / cm 3 Less than 1.0 g / cm, more preferably 1.0 g / cm 3 The density of the paper substrate is calculated from the basis weight and thickness of the paper substrate measured by the above-mentioned methods.
[0027] (Oken type smoothness) From the viewpoint of obtaining a uniform deposition layer, the paper substrate has an Oken smoothness of at least the surface on which the deposition layer is to be formed (i.e., the resin layer surface) of preferably 5 seconds or more, more preferably 10 seconds or more, and the upper limit is not particularly limited, but is preferably 1000 seconds or less, for example. The Oken smoothness of the paper substrate is measured in accordance with JIS P 8155:2010.
[0028] <Resin layer> The base paper for metallized paper of this embodiment has a resin layer on one side of the paper substrate, and preferably has a resin layer on the clay coat layer described later. By providing the resin layer, the adhesion between the metallized layer of the metallized paper and the paper substrate of the base paper for metallized paper is improved, and the barrier properties are improved. In addition, the resin layer has oxygen barrier properties and water vapor barrier properties, and therefore has the function of improving the barrier properties when made into metallized paper.
[0029] The resin layer preferably contains a water-suspendable polymer, and more preferably contains mainly a water-suspendable polymer. The phrase "the resin layer mainly contains a water-suspendable polymer" means that the content of the water-suspendable polymer in the resin layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The resin layer may further contain any component other than the water-suspendable polymer.
[0030] (Water-suspended polymer) The water-dispersible polymer contained in the resin layer is not particularly limited, but may be an alkyd resin; (meth)acrylic (co)polymer, styrene-(meth)acrylic resin; olefin-unsaturated carboxylic acid copolymer such as ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer; polyvinyl alcohol resin such as ethylene-vinyl alcohol copolymer (ethylene-modified polyvinyl alcohol); cellulose resin; polyurethane resin; polyester resin, etc. These may be used alone or in combination of two or more. Among these, the water-dispersible polymer is preferably one or more selected from the group consisting of water-dispersible polyvinyl alcohol resin, water-dispersible polyurethane resin, and water-dispersible polyester resin, and more preferably one or more selected from the group consisting of water-dispersible polyurethane resin and water-dispersible polyester resin.
[0031] <Water-suspendable polyurethane resin> The water-suspendable polyurethane-based resin contained in the resin layer is not particularly limited, and is preferably, for example, one or more selected from the group consisting of polyurethane-based resin dispersions and emulsions, more preferably one that can be prepared into a polyurethane-based resin dispersion or emulsion, and even more preferably one that can be prepared into a polyurethane-based resin dispersion.
[0032] The water-suspendable polyurethane resin contained in the resin layer preferably contains at least one selected from the group consisting of a constituent unit derived from meta-xylylene diisocyanate and a constituent unit derived from hydrogenated meta-xylylene diisocyanate. When the polyurethane resin contains at least one of a constituent unit derived from meta-xylylene diisocyanate and a constituent unit derived from hydrogenated meta-xylylene diisocyanate, the total content of the constituent units derived from meta-xylylene diisocyanate and the constituent units derived from hydrogenated meta-xylylene diisocyanate relative to the total amount of the constituent units derived from polyisocyanate is preferably 50 mol% or more. Such a polyurethane resin exhibits high cohesive strength due to hydrogen bonds and the stacking effect between xylylene groups, and therefore has excellent gas barrier properties. The above content is 1 The identification can be performed using known analytical techniques such as H-NMR.
[0033] -Oxygen permeability- The water-dispersible polyurethane resin contained in the resin layer preferably has an oxygen permeability of 100 mL / (m2) at 23° C. and 50% RH when converted into a 25 μm thick sheet. 2 ·day·atm) or less, preferably 50mL / (m 2 ·day·atm) or less, and more preferably 25mL / (m 2 ·day·atm) or less, and even more preferably 10 mL / (m 2 ·day·atm) or less, and even more preferably 5 mL / (m 2 ·day·atm) or less. A low oxygen permeability of the resin layer is preferable because it imparts better gas barrier properties to the base paper for metallized paper. In this specification, oxygen permeability is measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) under conditions of 23°C and 50% RH.
[0034] -Glass transition temperature- The glass transition temperature of the water-dispersible polyurethane resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of increasing film-formability in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyurethane resin is measured in accordance with JIS K 7122:2012.
[0035] As the water-dispersible polyurethane-based resin, a synthetic product may be used, and examples thereof include the polyurethane-based resins described in WO 2015 / 016069.
[0036] As the water-dispersible polyurethane resin, commercially available products may be used, such as "Takelac W series (product name)", "Takelac WPB series (product name)", and "Takelac WS series (product name)" manufactured by Mitsui Chemicals, Inc., and specifically, "Takelac WPB-341 (product name)" is exemplified. Other commercially available products include "HPU W-003 (product name)" (hydroxyl value 235 mg KOH / g) manufactured by Dainichiseika Chemicals Mfg. Co., Ltd.
[0037] <Water-dispersible polyester resin> The water-suspendable polyester-based resin contained in the resin layer is not particularly limited, and is preferably, for example, one or more selected from the group consisting of polyester-based resin dispersions and emulsions, more preferably one that can be prepared into a polyester-based resin dispersion or emulsion, and even more preferably one that can be prepared into a polyester-based resin dispersion.
[0038] -Acid value- From the viewpoint of obtaining superior adhesion to a vapor deposition layer described later, the acid value of the water-suspendable polyester resin is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, even more preferably 5 mgKOH / g or more, and even more preferably 6 mgKOH / g or more, and the upper limit is not particularly limited, but is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and even more preferably 15 mgKOH / g or less. The acid value of the water-suspendable polyester resin is measured in accordance with JIS K 0700:1992.
[0039] -Hydroxyl value- From the viewpoint of obtaining superior adhesion to a vapor deposition layer described later, the hydroxyl value of the water-dispersible polyester resin is preferably 0.5 mgKOH / g or more, more preferably 1 mgKOH / g or more, even more preferably 1.5 mgKOH / g or more, and even more preferably 2 mgKOH / g or more, and the upper limit is not particularly limited, but is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and even more preferably 10 mgKOH / g or less. The hydroxyl value of the water-dispersible polyester resin is measured in accordance with JIS K 0700:1992.
[0040] -Glass transition temperature- The glass transition temperature of the water-dispersible polyester resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of increasing film-formability in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyester resin is measured in accordance with JIS K 7122:2012.
[0041] As the water-dispersible polyester resin, commercially available products may be used, such as the "ELITEL KT Series (product name)" manufactured by Unitika Ltd. and the "LANDY PL Series (product name)" manufactured by Miyoshi Oil & Fats Co., Ltd., and specific examples thereof include "ELITEL KT-8803 (product name)" and "LANDY PL-3000 (product name)."
[0042] (Silane coupling agent) From the viewpoint of improving the flex resistance of the resin layer, the resin layer may contain a silane coupling agent in addition to the water-dispersible polymer.
[0043] Silane coupling agent is a compound having at least one alkoxysilyl group and at least one reactive functional group other than the alkoxysilyl group in the molecule. The alkoxysilyl group may be any of monoalkoxysilyl group, dialkoxysilyl group, and trialkoxysilyl group, but from the viewpoint of reactivity, trialkoxysilyl group is preferred.
[0044] Examples of reactive functional groups other than the alkoxysilyl group include a vinyl group, an epoxy group, a styryl group, a (meth)acryloyloxy group, an amino group, an isocyanato group, a ureido group, and an acid anhydride group. Among these, the amino group, the epoxy group, and the acid anhydride group are preferred, and the amino group is more preferred.
[0045] Examples of epoxy group-containing silane coupling agents include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0046] Examples of amino group-containing silane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane. Of these, 3-aminopropyltriethoxysilane is preferred.
[0047] An example of an acid anhydride group-containing silane coupling agent is 3-trimethoxysilylpropylsuccinic anhydride.
[0048] As the silane coupling agent, commercially available products may be used, and examples thereof include KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, and X-12-967C manufactured by Shin-Etsu Chemical Co., Ltd.
[0049] The amount of the silane coupling agent is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, particularly preferably 0.3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less, and particularly preferably 5 parts by mass or less, relative to 100 parts by mass of the water-suspendable polymer.
[0050] (optional ingredient) Optional components that may be contained in the resin layer include other resins and additives, such as defoamers, surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and mold release agents.
[0051] The coating amount of the resin layer is not particularly limited, but is preferably 0.1 g / m2 in terms of solid content. 2 More preferably, 0.5 g / m 2 More preferably, 0.7 g / m2 and preferably 10 g / m 2 Less than 5g / m, more preferably 2 Less than 3 g / m, more preferably 2 The method for forming the resin layer is not particularly limited, but it is preferable to form the resin layer by applying an aqueous coating liquid containing a water-dispersible polymer and drying it.
[0052] <Clay court layer> As described above, the base paper for metallized paper of this embodiment preferably has a clay coat layer between the paper substrate and the resin layer, which seals the paper substrate and smoothes the surface on which the resin layer is to be formed, forming a flatter resin layer. As a result, when the metallized paper described below is formed, a uniform metallized layer can be formed, improving the barrier properties.
[0053] The clay coat layer preferably contains an inorganic pigment and a binder, and more preferably is mainly composed of an inorganic pigment and a binder. The phrase "the clay coat layer is mainly composed of an inorganic pigment and a binder" means that the total content of the inorganic pigment and the binder in the clay coat layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The clay coat layer may further contain any other components in addition to the inorganic pigment and the binder.
[0054] (Inorganic pigments) The inorganic pigment contained in the clay coat layer is not particularly limited, but may be kaolin, talc, mica, etc., and is preferably kaolin. The content of the inorganic pigment in the clay coat layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and is preferably 98% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less.
[0055] Aspect ratio From the viewpoint of forming a uniform and smooth resin layer, the aspect ratio of the inorganic pigment is preferably 50 or less, more preferably 45 or less, and the lower limit is not particularly limited, but is preferably 1 or more, more preferably 5 or more. The aspect ratio of the inorganic pigment can be measured by observation with an electron microscope or X-ray diffraction measurement.
[0056] ≪Average particle size≫ From the viewpoint of forming a uniform and smooth resin layer, the average particle size of the inorganic pigment is preferably 5 μm or less, more preferably 3 μm or less, even more preferably 1 μm or less, and even more preferably 0.50 μm or less, and the lower limit is not particularly limited, but is preferably 0.05 μm or more, more preferably 0.10 μm or more. The average particle size of the inorganic pigment means the median size (d50) measured by a laser diffraction scattering type particle size distribution measurement.
[0057] (binder) The binder contained in the clay coat layer is not particularly limited, and examples thereof include styrene-butadiene resins; (meth)acrylic (co)polymers; styrene-(meth)acrylic resins; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; and polylactic acid. These may be used alone or in combination of two or more. Among these, it is preferable to use one or more selected from the group consisting of styrene-butadiene resins, styrene-(meth)acrylic resins, olefin-unsaturated carboxylic acid copolymers, and polylactic acid, more preferably one or more selected from the group consisting of styrene-(meth)acrylic resins, ethylene-(meth)acrylic acid copolymers, and polylactic acid, and even more preferably one or more selected from the group consisting of styrene-acrylic resins, ethylene-acrylic resins, and polylactic acid.
[0058] The (meth)acrylic (co)polymer is a (co)polymer of one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters. The (meth)acrylic acid ester is not particularly limited, but is preferably an alkyl ester of (meth)acrylic acid having 1 to 12 carbon atoms.
[0059] The styrene-(meth)acrylic resin is a copolymer of styrene and one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters, and is preferably a styrene-acrylic resin or a styrene-methacrylic resin, and more preferably a styrene-acrylic acid copolymer or a styrene-acrylic acid ester copolymer.
[0060] The content of the binder in the clay coat layer is preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less.
[0061] (optional ingredient) Optional components that may be contained in the clay coat layer include adhesives, dispersants, thickeners, water retention agents, defoamers, water resistance agents, colorants, surfactants, etc. Adhesives include proteins such as casein, soy protein, synthetic protein, etc. Starches such as oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, dextrin, etc. Cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, hydroxymethyl cellulose, etc.
[0062] The coating amount of the clay coating layer is not particularly limited, but is preferably 5 g / m2 in terms of solid content. 2 More preferably, 8 g / m 2 More preferably, 10 g / m 2 and preferably 30 g / m 2 Less than 20 g / m 2 Less than 15 g / m, more preferably 2 The following is the result.
[0063] The method for forming the clay coat layer is not particularly limited, but is preferably a method of forming the clay coat layer by applying a dispersion containing an inorganic pigment and a binder onto a paper substrate and drying it. The dispersion containing an inorganic pigment and a binder is preferably one that uses an aqueous medium containing water as a main component as a solvent.
[0064] <Pigment coating layer> The base paper for metallized paper of this embodiment has a pigment coating layer on the other side of the paper substrate, i.e., the side opposite to the side having the resin layer. By providing the pigment coating layer and further performing a calendaring process under predetermined conditions, the smoothness of the surface can be increased and the dynamic friction coefficient against stainless steel can be reduced, resulting in a metallized paper with excellent printability and processability. The pigment coating layer is preferably composed mainly of a pigment and a binder. Note that "the pigment coating layer is mainly composed of a pigment and a binder" means that the total content of the pigment and the binder in the pigment coating layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. Note that the pigment coating layer may further contain any component other than the pigment and the binder.
[0065] (Pigments) The pigment contained in the pigment coating layer is not particularly limited, and examples thereof include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, calcined clay, heavy calcium carbonate, light calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white; and organic pigments such as solid, hollow, or core-shell types. These may be used alone or in combination of two or more. Among these, at least one selected from the group consisting of kaolin and calcium carbonate is preferred, and it is more preferred to use kaolin and calcium carbonate in combination, and it is even more preferred to use kaolin, heavy calcium carbonate, and light calcium carbonate in combination. From the viewpoint of further improving printability, the mass ratio of kaolin to calcium carbonate in the pigment (kaolin / calcium carbonate) is preferably 10 / 90 to 50 / 50, and more preferably 20 / 80 to 40 / 60.
[0066] The pigment content in the pigment coating layer is 50% by mass or more, preferably 60% by mass or more, and 85% by mass or less, preferably 83% by mass or less, from the viewpoint of preventing the ink from peeling off and achieving excellent printability when forming a vapor-deposited paper and printing on the vapor-deposited paper.
[0067] (binder) The binder contained in the pigment coating layer is not particularly limited, and examples thereof include styrene-butadiene resins; acrylic resins such as methyl (meth)acrylate copolymers and styrene-(meth)acrylic copolymers; olefin-unsaturated carboxylic acid copolymers such as ethylene-(meth)acrylic acid copolymers; natural polysaccharides such as dextrin, mannan, chitosan, arabinogalactan, glycogen, inulin, pectin, hyaluronic acid, hydroxyethylated starch, oxidized starch, etherified starch, phosphated starch, enzyme-modified starch, and modified starch obtained by flash drying thereof, as well as oligomers and modified products thereof. Among these, it is preferable to use one or more selected from the group consisting of acrylic resins, styrene-butadiene resins, and modified starches, more preferably one or more selected from the group consisting of styrene-(meth)acrylic copolymers, styrene-butadiene resins, and oxidized starches, even more preferably one or more selected from the group consisting of styrene-butadiene resins and oxidized starches, and even more preferably to use both in combination.
[0068] The content of the binder in the pigment coating layer is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 50% by mass or less, more preferably 45% by mass or less. When oxidized starch is used as the binder, the content of the oxidized starch in the pigment coating layer is preferably 1% by mass or more, more preferably 2% by mass or more, and preferably 12% by mass or less, more preferably 8% by mass or less.
[0069] (optional ingredient) Optional components that may be contained in the pigment coating layer include adhesives, dispersants, thickeners, water retention agents, defoamers, water resistance agents, colorants, surfactants, etc. Adhesives include proteins such as casein, soy protein, synthetic protein, etc. Starches such as oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, dextrin, etc. cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, hydroxymethyl cellulose, etc.
[0070] The coating amount of the pigment coating layer is not particularly limited, but is preferably 3 g / m2 in terms of solid content. 2 More preferably, 5 g / m 2 More preferably, 7 g / m 2 and preferably 30 g / m 2 Less than 20 g / m, more preferably 20 g / m 2 More preferably, 15 g / m or less 2 The following is the result.
[0071] The method for forming the pigment coating layer is not particularly limited, but a method of forming the pigment coating layer by coating a dispersion containing a pigment and a binder on a paper substrate and drying the same is preferred. The dispersion containing a pigment and a binder is preferably one that uses an aqueous medium containing water as a main component as a solvent.
[0072] <Physical properties of base paper for metallized paper> (Oken type smoothness) From the viewpoint of obtaining a base paper for metallized paper having excellent printability, the Oken smoothness of the surface having the pigment coating layer of the base paper for metallized paper is 300 seconds or more, preferably 350 seconds or more, more preferably 450 seconds or more, even more preferably 650 seconds or more, and even more preferably 850 seconds or more, and the upper limit is not particularly limited, but is preferably 5000 seconds or less, more preferably 3000 seconds or less. Note that the Oken smoothness of the surface having the pigment coating layer of the base paper for metallized paper does not change even after a process of providing a metallized layer to obtain metallized paper, so that if it is in the above range, metallized paper having excellent printability can be obtained. The Oken smoothness of the surface having the pigment coating layer is measured in accordance with JIS P 8155:2010. The Oken smoothness of the surface having the pigment coating layer can be adjusted to the above range by adjusting the Oken smoothness of the paper base material used, or by carrying out a calendar treatment under the following conditions after forming the pigment coating layer. As for the calendering conditions, the linear pressure is preferably 10 kg / cm or more, more preferably 30 kg / cm or more, even more preferably 50 kg / cm or more, and is preferably 1000 kg / cm or less, more preferably 500 kg / cm or less, even more preferably 200 kg / cm or less. Furthermore, when heating is performed in the calendaring process, the heating temperature is not particularly limited, but from the viewpoint of enhancing the effect of the treatment while preventing thermal deterioration of the paper base material or the pigment coating layer and sticking of the pigment coating layer, the heating temperature is preferably 20°C or higher, more preferably 30°C or higher, even more preferably 35°C or higher, and is preferably 80°C or lower, more preferably 70°C or lower, even more preferably 60°C or lower. The calendaring may be performed in one or more stages. From the viewpoint of further improving printability and / or automatic packaging suitability, however, it is preferable to perform the calendaring in multiple stages (two or more stages), more preferably five or more stages, and even more preferably ten or more stages. Although there is no particular upper limit, it is preferably 15 stages or less.
[0073] (Kinematic friction coefficient against stainless steel) The dynamic friction coefficient of the pigment-coated surface of the base paper for metallized paper against stainless steel is 0.35 or less, more preferably 0.32 or less, from the viewpoint of obtaining a base paper for metallized paper with excellent processing suitability, and is more preferably 0.22 or less, even more preferably 0.20 or less, from the viewpoint of further improving processing suitability (transportability in an automatic packaging machine), and the lower limit is not particularly limited, but is preferably 0.10 or more. The dynamic friction coefficient of the pigment-coated surface of the base paper for metallized paper against stainless steel does not change even after a process of providing a deposition layer, so that the dynamic friction coefficient in the above range is excellent in processing suitability. The dynamic friction coefficient of the pigment-coated surface against stainless steel is measured in accordance with JIS P 8147:2010, and specifically, can be measured by the method described in the examples. The dynamic friction coefficient of the surface having the pigment coating layer against stainless steel can be adjusted to within the above range by adjusting the Oken smoothness of the paper base material used, or by performing a calendar treatment under the above conditions after forming the pigment coating layer.
[0074] (Thickness) The thickness of the base paper for metallized paper is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less. The thickness of the base paper for metallized paper is measured in accordance with JIS P 8118:2014.
[0075] There is no limitation on the method for producing the base paper for metallized paper of this embodiment, but for example, it is preferable to coat and dry a clay coating layer coating liquid containing an inorganic pigment and a binder as necessary on one side of the paper substrate, then coat and dry a resin layer coating liquid containing a water-dispersible polymer, and coat and dry a pigment coating layer coating liquid containing a pigment and a binder on the other side of the paper substrate, and then perform a calendar treatment under the above conditions. Note that, if the base paper for metallized paper of this embodiment can be obtained, after forming a pigment coating layer on one side of the paper substrate, a clay coating layer and a resin layer may be provided on the other side of the paper substrate as necessary. Each layer can be formed by coating as described above.
[0076] [Metal-deposited paper] The metallized paper of this embodiment is a metallized paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the base paper for metallized paper, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, and the surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The metallized paper of this embodiment is excellent in printability and processability in automatic packaging. The Oken smoothness and dynamic friction coefficient against stainless steel of the surface having the pigment coating layer of the metallized paper do not change even if a metallized layer or the like is provided on the resin layer of the base paper for metallized paper.
[0077] The paper substrate used in the metallized paper of this embodiment may be one of the paper substrates exemplified for the base paper for metallized paper described above. The resin layer provided on one side of the paper substrate may also be one of the resin layers exemplified for the base paper for metallized paper described above. The pigment coating layer provided on the other side of the paper substrate may also be one of the pigment coating layers exemplified for the base paper for metallized paper described above.
[0078] <Vapour-deposited layer> The metal-deposited paper of this embodiment has a metal-deposited layer on the resin layer of the base paper for metal-deposited paper. The metal-deposited layer is at least one of a layer made of metal and a layer made of ceramic. That is, the metal-deposited layer may be any of a layer made of metal, a layer made of ceramic, and a laminate of a metal layer and a ceramic layer. When the metal-deposited layer is a laminate of a metal layer and a ceramic layer, the metal layer may be on the resin layer side of the base paper for metal-deposited paper, and the ceramic layer may be on the resin layer side of the base paper for metal-deposited paper, and there is no particular limitation.
[0079] The vapor-deposited layer may be a layer made of a metal, a layer made of a ceramic, or a laminate of these, but is preferably a layer made of a metal. When the vapor-deposited layer is a layer made of a metal, specific examples of the metal include aluminum and titanium. When the vapor-deposited layer is a layer made of ceramic, specific examples of the ceramic include silicon oxide, titanium oxide, aluminum oxide, diamond-like carbon, and the like. These may be used alone or in combination of two or more.
[0080] Among these, the vapor deposition layer is preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, silicon oxide, and diamond-like carbon, and from the viewpoint of ease of production, is more preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, and diamond-like carbon, and is even more preferably a layer made of one or more materials selected from the group consisting of aluminum and aluminum oxide.
[0081] (Thickness) The thickness of the deposition layer is preferably 1 nm or more, more preferably 2 nm or more, and even more preferably 3 nm or more, and is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 100 nm or less. From the viewpoint of barrier properties, the thickness of the deposition layer is preferably 10 nm or more, more preferably 15 nm or more, and is preferably 80 nm or less, and more preferably 70 nm. From the viewpoints of adhesion to other layers and cost, the thickness of the deposition layer is preferably 4 nm or more, more preferably 5 nm or more, and is preferably 100 nm or less, more preferably 70 nm or less, and even more preferably 60 nm or less.
[0082] <Heat seal layer> The metallized paper of the present embodiment preferably has a heat seal layer on the metallized layer. The heat seal layer is a layer that is melted and bonded by heating, ultrasonic waves, or the like. Methods for forming the heat seal layer include coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it, and extrusion lamination. Among these, it is preferable to coat a thermoplastic resin solution or a thermoplastic resin dispersion and dry it. The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves a thermoplastic resin, a dispersion using an organic solvent that disperses a thermoplastic resin, or a dispersion using an aqueous medium, and from the viewpoint of coatability and environmental load, a dispersion using an aqueous medium is preferred.
[0083] (thermoplastic resin) Thermoplastic resins suitable for dispersions using aqueous media may be either natural resins or synthetic resins, and examples thereof include starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, acrylic resins, ionomer resins, maleic acid resins, urethane resins, polyester resins, styrene-butadiene resins, vinyl chloride resins, and polyolefin resins. More specifically, examples of the acrylic resin include an acrylic resin copolymerized with (meth)acrylic acid and its alkyl ester or styrene as a monomer component, a styrene-maleic acid resin, a styrene-acrylic acid-maleic acid resin, a water-soluble polyurethane resin, and a water-soluble polyester resin. As the ionomer resin, for example, an ethylene-acrylic acid copolymer ionomer and an ethylene-methacrylic acid ionomer are preferable. Here, an ionomer is a polymer neutralized with a cation, and the cation may be a metal ion or an ammonium ion (NH4 + ), and organic ammonium ions. Metal ions include lithium ions (Li + ), sodium ion (Na + ), potassium ion (K + ), magnesium ions (Mg 2+ ), calcium ion (Ca 2+ ), alkaline earth metal ions such as zinc ions (Zn 2+ ), copper ions (Cu 2+ Among these, sodium ions are preferred as the metal ions from the viewpoint of availability and the like. Among these, from the viewpoints of the stability of the coating liquid and the solvent resistance of the coating layer, the thermoplastic resin is preferably one or more selected from the group consisting of starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, ionomer-based resins, acrylic resins, polyolefin-based resins, and maleic acid-based resins, more preferably one or more selected from the group consisting of starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, acrylic resins, polyolefin-based resins, and maleic acid-based resins, even more preferably at least one selected from starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, acrylic resins, and polyolefin-based resins, even more preferably one or more selected from the group consisting of polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, and polyolefin-based resins, and even more preferably one or more selected from the group consisting of ionomer-based resins and polyolefin-based resins.
[0084] Methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include a bar coating method, a blade coating method, a squeeze coating method, an air knife coating method, a roll coating method, a gravure coating method, and a transfer coating method, and a coating machine such as a fountain coater or a slit die coater may be used.
[0085] The coating amount of the heat seal layer is not particularly limited, but from the viewpoint of ensuring sufficient heat sealability, it is preferably 0.5 g / m 2 More preferably, 1 g / m 2 More preferably, 1.5 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 15 g / m 2 Less than 10 g / m 2 Less than 7 g / m, more preferably 2 Less than 5 g / m 2 The following is the result.
[0086] <Overcoat layer> The vapor-deposited paper of this embodiment may have an overcoat layer between the vapor-deposited layer and the heat seal layer. The overcoat layer is a layer for protecting the vapor-deposited layer. The vapor-deposited paper of this embodiment has a certain barrier property by having the vapor-deposited layer, but the oxygen barrier property can be further improved by having an overcoat layer on the vapor-deposited layer. In addition, the vapor-deposited layer is unlikely to be damaged by processing such as bending, and even if it is damaged, the oxygen barrier property can be guaranteed by the overcoat layer, and excellent oxygen barrier property can be maintained.
[0087] The overcoat layer is not particularly limited and may contain an organic compound, an inorganic compound, or both. That is, the overcoat layer may be any of an organic layer, an inorganic layer, and an organic-inorganic hybrid layer. Examples of the organic compound include vinyl alcohol resins such as polyvinyl alcohol, polyurethane resins, (meth)acryloyl compounds, and reaction products of (meth)acryloyl compounds. Examples of the inorganic compound include oxides of silicon, aluminum, and the like.
[0088] Among these, the overcoat layer is preferably one of the resins exemplified as being contained in the resin layer of the base paper for metallized paper, more preferably contains at least one resin selected from the group consisting of water-suspendable polyurethane resins and water-suspendable polyester resins, even more preferably is capable of being prepared into one or more resins selected from the group consisting of polyurethane resin dispersions and emulsions, even more preferably is capable of being prepared into a polyurethane resin dispersion or emulsion, and even more preferably is capable of being prepared into a polyurethane resin dispersion.
[0089] The water-dispersible polyurethane resin or water-dispersible polyester resin that the overcoat layer may contain may be the same type as the resin contained in the resin layer of the base paper for metallized paper described above, or may be a different type, but it is preferable that they are the same type. In addition, the synthetic products or commercially available products listed as usable for the resin layer of the base paper for metallized paper may be used.
[0090] The content of the water-dispersible polyurethane resin or water-dispersible polyester resin in the overcoat layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 99% by mass or more, and the upper limit is not particularly limited, but is 100% by mass.
[0091] The overcoat layer may contain other resins and additives within the range that does not impair the effects of the present invention. Examples of additives include surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and release agents. When the polyurethane resin is used as an aqueous dispersion, it is preferable to use a dispersant to disperse the polyurethane resin in an aqueous medium and obtain a uniform overcoat layer film.
[0092] The coating amount of the overcoat layer is preferably 0.1 g / m2 in terms of solid content from the viewpoint of protecting the deposition layer. 2 More preferably, 0.2 g / m 2 More preferably, 0.3 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 10 g / m 2 Less than 7g / m 2 Less than 5 g / m, more preferably 2 The following is the result.
[0093] From the viewpoint of protecting the vapor-deposited layer, the thickness of the overcoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more, and from the viewpoint of recyclability of the vapor-deposited paper, the thickness is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 4 μm or less.
[0094] The method for forming the overcoat layer is not particularly limited, but it is preferable to form the overcoat layer by coating an aqueous medium of an organic compound or an inorganic compound that constitutes the overcoat layer and drying it.
[0095] In the metallized paper of this embodiment, the overcoat layer may be the outermost layer. Even if the overcoat layer is the outermost layer, it does not impair the design of the glossy metallized layer.
[0096] [Method of manufacturing metallized paper] The method for producing the metal-deposited paper of this embodiment is not limited, but preferably includes the steps of forming a metal-deposited layer by depositing at least one of metal and ceramic on the resin layer of the base paper for metal-deposited paper, which has a clay coat layer and a resin layer in this order as necessary, on one side of the paper substrate, and applying a coating liquid for the heat-sealing layer onto the deposition layer and drying to form a heat-sealing layer. In this case, an overcoat layer may be formed by coating on the deposition layer before forming the heat-sealing layer.
[0097] The method for depositing the metal or ceramic is preferably a method in which the metal or ceramic is directly deposited in vacuum on the surface of the resin layer of the base paper for the metallized paper.
[0098] From the viewpoint of efficiently protecting the deposition layer and enhancing the barrier property, the overcoat layer is preferably formed directly on the deposition layer. The overcoat layer is preferably formed by applying a liquid for the overcoat layer and drying it. By using the method of applying a coating liquid for the overcoat layer to form the overcoat layer, a relatively thin overcoat layer of 10 μm or less can be formed.
[0099] The coating liquid for the overcoat layer used here may be an aqueous medium for an organic compound or an inorganic compound constituting the overcoat layer. Among these, a solution using an organic solvent that dissolves a polyurethane resin, a dispersion using an organic solvent that disperses a polyurethane resin, or a dispersion using an aqueous medium is preferred, and from the viewpoints of coatability and environmental load, a dispersion using an aqueous medium is more preferred.
[0100] Examples of methods for applying the coating liquid for the overcoat layer include a bar coating method, a blade coating method, a squeeze coating method, an air knife coating method, a roll coating method, a gravure coating method, and a transfer coating method, and a coater such as a fountain coater or a slit die coater may be used. The coated metal-deposited paper coated with the coating liquid for the overcoat layer is dried to remove the organic solvent or the aqueous medium, thereby obtaining a metal-deposited paper having an overcoat layer on the metal-deposited layer.
[0101] A heat seal layer containing a thermoplastic resin can be formed on the deposition layer or the overcoat layer. Methods for forming the heat seal layer include coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it, and extrusion lamination. Among these, coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it is preferred.
[0102] The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves the thermoplastic resin, a dispersion using an organic solvent that disperses the thermoplastic resin, or a dispersion using an aqueous medium, and from the standpoint of coatability and environmental load, a dispersion using an aqueous medium is preferred.
[0103] Methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include a bar coating method, a blade coating method, a squeeze coating method, an air knife coating method, a roll coating method, a gravure coating method, and a transfer coating method, and a coating machine such as a fountain coater or a slit die coater may be used.
[0104] The coated metal-deposited paper coated with a thermoplastic resin solution or thermoplastic resin dispersion can be dried to remove the organic solvent or aqueous medium, yielding a metal-deposited paper having a heat seal layer on the metal-deposited layer or overcoat layer.
[0105] <Physical properties of metallized paper> (Thickness) The thickness of the metallized paper is preferably 20 μm or more, more preferably 50 μm or more, and preferably 200 μm or less, more preferably 150 μm or less. The thickness of the metallized paper is measured in accordance with JIS P 8118:2014.
[0106] (Oxygen permeability) The oxygen permeability of the metallized paper at 23°C and 50% RH is preferably 1.5 mL / (m 2 ·day·atm) or less, more preferably 1.0mL / (m 2 ·day·atm), and its lower limit is 0 mL / (m 2 The oxygen permeability of the metallized paper is measured in accordance with JIS K 7126-2:2006, specifically, by the method described in the examples.
[0107] (Water vapor permeability) The water vapor permeability of the metallized paper at 40°C and 90% RH is preferably 1.0 g / (m 2 ·day) or less, more preferably 0.7g / (m 2 ·day), and the lower limit is 0g / (m 2 The water vapor permeability of the metallized paper is measured in accordance with JIS K 7129-2:2019, specifically, by the method described in the examples.
[0108] Taking advantage of the excellent printability, processability, and gas barrier properties described above, the metallized paper of this embodiment can be suitably used as a packaging material, particularly as a packaging bag, for foods such as coffee, confectionery, and milk, medicines, medical supplies, and electronic components.
[0109] [Packaging bag] A packaging bag according to another embodiment of the present disclosure is a packaging bag made using the above-mentioned vapor-deposited paper. Examples of the packaging bag include a standing pouch type, a side seal type, a two-sided seal type, a three-sided seal type, a four-sided seal type, an envelope seal type, a joint seal type (pillow seal type), a pleated seal type, a flat bottom seal type, a square bottom seal type, and a gusset type. The packaging bag of the present embodiment may be formed by folding one of the above-mentioned vapor-deposited papers having a heat seal layer or by overlapping two sheets of the paper together so that the heat seal layers face each other and heat-sealing the peripheral edges of the paper to form the above-mentioned shape, or by folding the above-mentioned vapor-deposited paper or by overlapping two sheets of the paper together and bonding the peripheral edges of the paper together with an adhesive to form the above-mentioned shape.
[0110] The vapor-deposited paper of the present embodiment may be used for purposes other than packaging bags, for example, soft packaging materials such as lids and labels, liquid containers such as milk cartons (hereinafter also referred to as liquid paper containers), packaging containers such as cups, trays, plates, lids, laminated tubes, etc. In this case, the contents to be packaged may be liquids, solids (granular materials, powdery materials, etc.), or gels. EXAMPLES
[0111] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Furthermore, unless otherwise specified, "%" and "parts" represent "% by mass" and "parts by mass", respectively. Furthermore, the operations of the examples and comparative examples were carried out under conditions of room temperature (20 to 25°C) and normal humidity (40 to 50% RH) unless otherwise specified.
[0112] [Measurement and Evaluation] The metallized paper base paper, metallized paper (packaging material), and packaging bags according to the examples and comparative examples were analyzed and evaluated as follows.
[0113] <Base paper for metallized paper> (Oken type smoothness) The Oken smoothness of the surface having the pigment coating layer was measured in accordance with JIS P 8155:2010.
[0114] (Kinematic friction coefficient against stainless steel) The dynamic friction coefficient of the pigment-coated surface against stainless steel was measured in accordance with JIS P 8147:2010 by fixing a stainless steel plate to the sled side and placing the test piece on the table side so that the pigment-coated surface was in contact with the stainless steel.
[0115] <Metal-deposited paper> (Oxygen permeability) The oxygen permeability of the metallized paper was measured using an oxygen permeability measuring device ("OX-TRAN2 / 22" manufactured by MOCON) under conditions of a temperature of 23°C and a relative humidity of 50%. Specifically, an isocyanate-based adhesive (manufactured by DIC Corporation, a mixture of 10 parts by mass of DIC Dry LX-500 and 1 part by mass of DIC Dry KW-75) was applied at 5 g / m2 to the surface of the heat seal layer of the metallized paper obtained in the examples and comparative examples. 2 After coating, a 20 μm thick CPP film (GP-32, manufactured by Hokuetsu Chemical Industry Co., Ltd.) was attached to form a laminate sheet. The oxygen permeability of the laminate sheet was measured at a temperature of 23° C. and a relative humidity of 50% in accordance with JIS K7126-2:2006. The lower the oxygen permeability value, the better the oxygen barrier property.
[0116] (Water vapor permeability) The water vapor permeability of metallized paper was measured in accordance with JIS Z 7129-2:2019 (temperature 40°C ± 0.5°C, relative humidity 90% ± 2%) by positioning the overcoat layer or metallized layer of the metallized paper on the inside (low humidity side). The lower the water vapor permeability value, the better the water vapor barrier property.
[0117] (Printability) Test printing was carried out in four colors using a gravure printing machine, and the print density was evaluated using a Gretag Macbeth portable reflection densitometer RD-19A. A: Print density of all four colors is 1.0 or higher B: Print density is less than 1.0 for one or more colors, but blank spaces are not noticeable. C: Print density is less than 1.0 for one or more colors, and white spots are noticeable
[0118] (Processability) <Cracks or chipping of pigment coating layer> Using a horizontal pillow packaging machine (manufactured by Fujikikai Co., Ltd., product name "α8 Series FW3410"), empty bags measuring 150 mm wide and 250 mm long were continuously produced without any contents at a speed of 60 bags / min, and the condition of the pigment coating layer of the resulting empty bags was evaluated according to the following criteria. A: There are no cracks or chips. B: There are cracks and chips, but they are barely noticeable. C: Cracks or chipping are present and noticeable.
[0119] <Easy transport with automatic packaging machines> Using a horizontal pillow packaging machine (manufactured by Fujikikai Co., Ltd., product name "α8 Series FW3410"), empty bags measuring 150 mm wide and 250 mm long were continuously produced at a speed of 60 bags per minute without any contents inside. The transportability of the packaging material unwound from the reel before being made into packaging bags was evaluated according to the following criteria. A: The packaging material is pulled smoothly and does not twist or wobble. B: The packaging material gets caught slightly, but does not meander. C: The packaging material cannot be pulled continuously or meandering occurs.
[0120] <Packaging bag> (exterior) The appearance of the empty packaging bags produced in the above-mentioned evaluation of processability was evaluated according to the following criteria. A: The bag is not warped and there are no seal defects. B: The bag is slightly warped, but the seal is not defective. C: The bag is significantly distorted or a seal defect has occurred.
[0121] (Gas barrier properties) The empty packaging bags produced in the above-mentioned evaluation of processability were measured using an oxygen transmission rate measuring device ("OX-TRAN2 / 22" manufactured by MOCON) at a temperature of 23°C and a relative humidity of 50%, and were evaluated according to the following criteria. "pkg" stands for "package". A: Oxygen permeability is less than 0.1mL / (day·pkg·0.2atm) B: Oxygen permeability is 0.1mL / (day·pkg·0.2atm) or more and less than 1mL / (day·pkg·0.2atm) C: Oxygen permeability is 1mL / (day·pkg·0.2atm) or more
[0122] Example 1 <Preparation of base paper for metallized paper> A coating solution for the clay coat layer was prepared by mixing 70 parts of kaolin (Imerys' product name "Contour Xtreme", aspect ratio 33, average particle size d50: 0.26 μm) and 30 parts (solid content) of a styrene-acrylic copolymer aqueous dispersion (BASF's product name "ACRONAL S504"). 2 , thickness 60μm, density 0.83g / cm 3 The above clay coating layer coating solution was applied to the glossy surface of a 100 mm thick glass substrate (12 g / m2, Stockigt sizing degree (glossy surface) 9 seconds, Oken smoothness (glossy surface) 430 seconds) with a Mayer bar, and dried at 120°C for 1 minute to form a clay coating layer (12 g / m2). 2 Next, a 25 μm-thick PET film with an oxygen permeability (23° C., 50% RH) of 2.0 mL / (m 2 The resin layer coating liquid, which contains 100 parts of an aqueous dispersion of a polyurethane resin binder (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content concentration 30%), is diluted with water to a solid content concentration of 10%, and then coated with a Mayer bar and dried at 120°C for 1 minute to form a resin layer (1 g / m 2 A thin film (1 μm thick) was formed. Next, 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") was added as a dispersant per 100 parts of kaolin to be dispersed in an aqueous solution, to which 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 25 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as binders per 70 parts (solids) of pigment to prepare coating solution A for the pigment coating layer with a final solids concentration of 60%. This was applied to the side opposite the resin layer in a thickness of 10 g / m2 in terms of solids. 2 After coating with a Mayer bar so that the thickness was 100 mm, the coated surface was dried in a 120°C air dryer for 1 minute, and finally, the resin layer coated surface was contacted with a chilled roll and the pigment layer coated surface was contacted with a cotton roll at a linear pressure of 90 kg / cm. The rolls were heated to 40°C and a 12-stage supercalendering process was carried out to obtain a base paper for metallized paper (thickness 65 μm, smoothness of the resin layer side: 7000 sec, smoothness of the pigment coating layer side on the opposite side: 2400 sec, dynamic friction coefficient of the pigment coating layer side against stainless steel: 0.188). The obtained base paper for metallized paper was subjected to the above-mentioned analysis and evaluation. The results are shown in Table 1. <Preparation of metallized paper> An aluminum vapor deposition layer (50 nm thick) was formed on the resin layer of the base paper for the above-mentioned metallized paper using a batch-type vacuum deposition device. Next, an aqueous dispersion of ethylene-methacrylic acid copolymer sodium salt (active content 35% by mass, trade name "Chemipearl S-300" manufactured by Mitsui Chemicals, Inc.) was diluted with water so that the active content was 20% by mass to prepare a coating liquid for the heat seal layer. This was applied with a Mayer bar and dried at 120°C for 1 minute to form a heat seal layer (3 g / m 2 ) was formed to obtain metallized paper. The obtained metallized paper was subjected to the above-mentioned analysis and evaluation. The results are shown in Table 1.
[0123] Example 2 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 1, except that Coating Solution B for the pigment coating layer was used in which the blending amounts of the pigment, oxidized starch, and styrene-butadiene copolymer latex in the Coating Solution A for the pigment coating layer in Example 1 were changed to 80 parts by mass, 5 parts by mass, and 15 parts by mass of the styrene-butadiene copolymer latex in the Coating Solution B for the pigment coating layer.
[0124] Example 3 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 1, except that Coating Solution C for a pigment coating layer was used in which the blending amounts of pigment, oxidized starch, and styrene-butadiene copolymer latex were 35 parts by mass, as compared to Coating Solution A for a pigment coating layer in Example 1.
[0125] Example 4 To an aqueous solution containing 0.1 parts of sodium polyacrylate (Aron T-50, manufactured by Toagosei Co., Ltd.) as a dispersant per 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (Milagros J, manufactured by BASF), 40 parts of light calcium carbonate (TP-123CS, manufactured by Okutama Kogyo Co., Ltd.), and 30 parts of heavy calcium carbonate (Hydrocarb 90, manufactured by Bihoku Funka Kogyo Co., Ltd.) were added and dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (manufactured by Oji Cornstarch Co., Ltd. under the trade name "Oji Ace A") and 15 parts (solids) of styrene-butadiene copolymer latex (manufactured by JSR Corporation under the trade name "OJ1000H") were added as binders per 80 parts (solids) of pigment, to prepare a coating solution D for the pigment coating layer with a final solids concentration of 60%. The coating amount of the clay coating layer was set to 12 g / m. 2 From 10g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that the thickness was changed to 3.8 μm.
[0126] Example 5 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the deposition source was changed from aluminum to a mixture of aluminum and oxygen, which was vacuum-deposited, and the deposition layer was made of alumina (AlOx) and had a thickness of 20 nm.
[0127] Example 6 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the deposition source was changed from aluminum to a deposition layer of silica (SiOx) using electron beam deposition to a thickness of 20 nm.
[0128] Example 7 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that chemical vapor deposition was performed using acetylene instead of aluminum as the deposition source, the deposition layer was made of diamond-like carbon (DLC), and the thickness was 20 nm.
[0129] Example 8 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the coating liquid for the heat seal layer was changed to a polyolefin dispersion (active content 43 mass%, product name "Rhobarr 320" manufactured by Dow Chemical Japan, Ltd.).
[0130] Example 9 After aluminum deposition, the oxygen permeability (23°C, 50% RH) of a 25 μm thick film was 2.0 mL / (m 2 The overcoat layer coating solution containing 100 parts by mass of an aqueous dispersion of a polyurethane resin binder (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content concentration 30%) was applied using a Mayer bar and dried at 120°C for 1 minute to form an overcoat layer (0.5 g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that a 0.5 μm thick film (0.01 μm thick) was formed.
[0131] Example 10 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 stages to 6 stages.
[0132] Example 11 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 stages to 2 stages.
[0133] Example 12 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the coating liquid for the resin layer was a coating liquid for the resin layer containing 100 parts of a polyester resin (product name "Elitter KT-8803" manufactured by Unitika Ltd., acid value 8 mg KOH / g, hydroxyl value 3 mg KOH / g, glass transition temperature 65°C). The results of Examples 1 to 12 are shown in Table 1 below.
[0134] [Table 1]
[0135] Comparative Example 1 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 1, except that a pigment coating layer was not formed.
[0136] Comparative Example 2 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Comparative Example 1, except that the 12-stage supercalendering was not performed.
[0137] Comparative Example 3 A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 1, except that a resin coating coating solution containing 100 parts by mass (solid content) of a styrene-(meth)acrylic resin (BASF's product name "ACRONAL S504") was used instead of coating solution A for the pigment coating layer.
[0138] Comparative Example 4 A pigment slurry was prepared by adding 30 parts of fine kaolin (BASF's product name "Milagros J"), 40 parts of light calcium carbonate (Okutama Kogyo Co., Ltd.'s product name "TP-123CS"), and 30 parts of heavy calcium carbonate (Bihoku Funka Kogyo Co., Ltd.'s product name "Hydrocarb 90") to an aqueous solution containing 0.1 parts of sodium polyacrylate (Toagosei Co., Ltd.'s product name "Aron T-50") as a dispersant relative to 100 parts of kaolin to be dispersed, and dispersing the mixture with a Coles disperser. A base paper for metallized paper and a metallized paper were obtained in the same manner as in Example 1, except that 5 parts (solid content) of oxidized starch (Oji Cornstarch Co., Ltd.'s product name "Oji Ace A") and 75 parts (solid content) of styrene-butadiene copolymer latex (JSR Corporation's product name "OJ1000H") were added as binders relative to 20 parts (solid content) of pigment to the pigment slurry, and the resulting mixture was used as coating solution E for the pigment coating layer.
[0139] Comparative Example 5 To an aqueous solution containing 0.1 parts of sodium polyacrylate (Aron T-50, manufactured by Toagosei Co., Ltd.) as a dispersant per 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (Milagros J, manufactured by BASF), 40 parts of light calcium carbonate (TP-123CS, manufactured by Okutama Kogyo Co., Ltd.), and 30 parts of heavy calcium carbonate (Hydrocarb 90, manufactured by Bihoku Funka Kogyo Co., Ltd.) were added and dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (Oji Ace A, product name, manufactured by Oji Cornstarch Co., Ltd.) and 5 parts (solids) of styrene-butadiene copolymer latex (OJ1000H, product name, manufactured by JSR Corporation) were added as binders per 90 parts (solids) of pigment to prepare coating solution F for the pigment coating layer with a final solids concentration of 60%. Except for this, a base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4. The results of Comparative Examples 1 to 5 are shown in Table 2.
[0140] [Table 2]
[0141] The metallized paper produced using the base paper for metallized paper of the examples was excellent in printability and processability. In addition, the metallized paper produced using the base paper for metallized paper of the examples also had a good appearance when made into a packaging bag.
Claims
1. A metal-deposited paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate, the metal-deposited paper having a metal-deposited layer on the resin layer, The content of the pigment in the pigment coating layer is 50% by mass or more and 85% by mass or less, The surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less, A heat seal layer is provided on the deposition layer, The coating amount of the heat seal layer is 0.5 g / m 2 15g / m or more 2 Below is the metallized paper.
2. The metallized paper according to claim 1 , further comprising an overcoat layer between the metallized layer and the heat seal layer.
3. The metallized paper according to claim 1 or 2, further comprising a clay coating layer between the paper substrate and the resin layer.
4. 3. The metallized paper according to claim 1, wherein the resin layer comprises at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.
5. A packaging bag made using the metallized paper according to claim 1 or 2.
Citation Information
Patent Citations
Paper for metal vacuum deposited label and production thereof
JP1989221593A
Biodegradable paper sheet and paper container
JP2003013391A
Antenna paper sheet, sheet-like antenna using the same, and RFID tag
JP2009239817A
Support for inkjet recording material and its manufacturing method
JP2010030231A
Base paper for container and production method thereof
JP2015030955A