Method for cutting wafer and method for processing laminated wafer

The described method addresses the issue of chipping and cracking in wafer cutting by using a combination of linear and circular cutting steps to minimize lateral loads, ensuring effective chamfer removal and preventing peeling in laminated wafers.

JP2024155667APending Publication Date: 2024-10-31DISCO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023133053
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-08-17
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing wafer cutting methods risk chipping or cracking at the outer peripheral edge, especially in laminated wafers, due to lateral loads applied during chamfer removal, and large chippings can peel off during grinding.

Method used

A method involving a holding step, linear cutting step, rotation step, and repeating step to remove chamfers while minimizing lateral loads, combined with a circular cutting step to form annular stepped portions, and a grinding step for laminated wafers to suppress chipping and cracking.

Benefits of technology

The method effectively removes chamfers while reducing chipping and cracking at the wafer's outer edge, and prevents peeling during grinding by minimizing lateral loads on the cutting blade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155667000001_ABST
    Figure 2024155667000001_ABST
Patent Text Reader

Abstract

To provide a method for cutting a wafer and a method for processing a laminated wafer, capable of removing a chamfered part while suppressing chipping and cracking of an outer peripheral end part of a wafer.SOLUTION: A method for cutting a wafer includes: a holding step 101 of holding a wafer on a holding surface of a chuck table; a positioning step 102 of locating an outer peripheral end part of a cutting blade at cutting depth of the wafer in a state that the cutting blade fitted at the end of a spindle having a rotary shaft in parallel to the holding surface is located at a position that does not overlap with the holding surface; a linearly cutting step 103 of cutting a part of a chamfered part of the wafer by linearly cutting the outer peripheral end part of the wafer; a rotation step 104 of rotating a chuck table at a prescribed rotation angle; and a repeating step 105 of repeatedly performing the linearly cutting step 103 and the rotation step 104 until all chamfered parts of the wafer are removed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wafer cutting method and a laminated wafer processing method. [Background technology]

[0002] In the manufacturing process of semiconductor devices, devices such as ICs (Integrated Circuits) and LSIs (Large Scale Integrations) are formed in areas partitioned by streets (planned division lines) formed in a grid pattern on the surface of a wafer. The backside of these wafers is ground to thin them to a specified thickness, and then they are divided along the streets by a cutting device or the like to be singulated into individual semiconductor device chips.

[0003] On the other hand, some wafers have a chamfer formed on the outer periphery from the front to the back. When such a plate-shaped workpiece is thinned to less than half its thickness, a so-called sharp edge is formed on the outer periphery, which may damage the wafer. To prevent this, a technique is known in which the outer periphery of the wafer is trimmed to remove the chamfer before thinning (Patent Document 1). One method for removing the chamfer is to rotate a chuck table that holds the wafer while a cutting blade is cut into the outer periphery of the wafer where the chamfer is formed, thereby removing all of the chamfer at the outer periphery. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-173961 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the above chamfer removal method, a lateral load is applied to the cutting blade by rotating the chuck table relative to the linearly formed processing point, which may cause chipping or cracking at the outer peripheral edge of the wafer from which the chamfer has been removed. Also, in stacked wafers, if the first wafer on the upper side has large or numerous chippings, there is a problem that the wafer is likely to peel off from the chipping during subsequent grinding.

[0006] The present invention has been made in consideration of these problems, and an object of the present invention is to provide a wafer cutting method and a laminated wafer processing method that can remove a chamfered portion while suppressing chipping and cracking of the outer peripheral edge of the wafer. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems and achieve the object, a wafer cutting method of the present invention is a wafer cutting method for cutting an outer peripheral edge of a disk-shaped wafer and removing a chamfered portion, the method comprising: a holding step of holding the wafer on a holding surface of a chuck table; a positioning step of bringing the spindle and the chuck table relatively close to each other in a direction perpendicular to the holding surface with a cutting blade attached to a tip of a spindle having a rotation axis parallel to the holding surface and positioned so as not to overlap the holding surface, thereby positioning the outer peripheral edge of the cutting blade at a cutting depth of the wafer; a linear cutting step of moving the spindle and the chuck table relatively in a direction parallel to the holding surface and perpendicular to the rotation axis of the spindle, thereby cutting the outer peripheral edge of the wafer in a linear manner, thereby cutting a part of the chamfered portion of the wafer; a rotation step of rotating the chuck table by a predetermined rotation angle after the linear cutting step; and a repeating step of repeatedly performing the linear cutting step and the rotation step until the entire chamfered portion of the wafer is removed.

[0008] The wafer cutting method of the present invention may further include, after the repeating step, a circular cutting step of cutting the outer peripheral edge of the wafer in a circular shape to form an annular step portion by rotating the chuck table while the cutting blade is cut into the outer peripheral edge of the wafer to the cutting depth.

[0009] The method for processing laminated wafers of the present invention is a method for processing laminated wafers in which a first wafer and a second wafer having chamfered portions at their outer circumferential edges are bonded together, and includes a first holding step of exposing the surface of the laminated wafers facing the second wafer by holding the surface of the laminated wafer facing the second wafer on a first holding surface of a first chuck table; a positioning step of moving the first spindle and the first chuck table relatively close to each other in a direction perpendicular to the first holding surface with a cutting blade attached to a tip of a first spindle having a rotation axis parallel to the first holding surface and positioned so as not to overlap the first holding surface, thereby positioning the outer circumferential edge of the cutting blade at a cutting depth of the first wafer; and a positioning step of moving the first spindle and the first chuck table relatively close to each other in a direction perpendicular to the first holding surface with the cutting blade positioned so as not to overlap the first holding surface with the cutting blade. a linear cutting step of relatively moving the first chuck table in a direction to linearly cut the outer circumferential edge of the first wafer, thereby cutting a part of the chamfered portion of the first wafer; a rotating step of rotating the first chuck table by a predetermined rotation angle after the linear cutting step; a repeating step of repeatedly performing the linear cutting step and the rotating step until the entire chamfered portion of the first wafer is removed; a second holding step of exposing the surface of the stacked wafers facing the second wafer by holding the surface of the stacked wafers facing the second wafer on a second holding surface of the second chuck table; and a grinding step of bringing a grinding wheel attached to a tip of a second spindle having a rotation axis perpendicular to the second holding surface and the second chuck table relatively close to each other to grind the first wafer.

[0010] The processing method for laminated wafers of the present invention may further include a circular cutting step, after the repeating step and before the second holding step, of cutting the outer peripheral edge of the first wafer in a circular shape to form an annular step portion by rotating the first chuck table while the cutting blade is cutting into the outer peripheral edge of the first wafer to the cutting depth. Effect of the Invention

[0011] The present invention can remove the chamfered portion while suppressing chipping and cracking of the outer peripheral edge of the wafer. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a flowchart showing the flow of the wafer cutting method according to the first embodiment. [Diagram 2] FIG. 2 is a side view, partly in section, showing a state after the holding step shown in FIG. [Diagram 3] FIG. 3 is a side view, partly in section, showing a state after the positioning step shown in FIG. [Figure 4] FIG. 4 is a plan view of FIG. [Diagram 5] FIG. 5 is a side view, partially in section, showing one state of the linear cutting step shown in FIG. [Figure 6] FIG. 6 is a plan view of FIG. [Figure 7] FIG. 7 is a side view, partially in section, showing a state after the rotation step shown in FIG. [Figure 8] FIG. 8 is a plan view of FIG. [Figure 9] FIG. 9 is a plan view of the wafer after the repeating steps shown in FIG. [Figure 10] FIG. 10 is a flowchart showing the flow of the laminated wafer processing method according to the second embodiment. [Figure 11] FIG. 11 is a side view, partially in section, showing a state after the first holding step shown in FIG. [Figure 12]FIG. 12 is a side view, partially in cross section, showing a state after the second holding step shown in FIG. [Figure 13] FIG. 13 is a side view, partly in section, showing one state of the grinding step shown in FIG. [Figure 14] FIG. 14 is a flowchart showing the flow of the wafer cutting method according to the third embodiment. [Figure 15] FIG. 15 is a side view showing one state of the circular cutting step shown in FIG. [Figure 16] FIG. 16 is a top view of the wafer after the circular cutting step shown in FIG. [Figure 17] FIG. 17 is a flowchart showing the flow of the laminated wafer processing method according to the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in each of the following embodiments. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.

[0014] [First embodiment] First, a method for cutting a wafer 1 according to a first embodiment of the present invention will be described with reference to the drawings. The method for cutting a wafer 1 is a method for cutting an outer peripheral edge 7 of a disk-shaped wafer 1 and removing a chamfered portion 3. FIG. 1 is a flowchart showing the flow of the method for cutting a wafer 1 according to the first embodiment. As shown in FIG. 1, the method for cutting a wafer 1 according to the first embodiment includes a holding step 101, a positioning step 102, a linear cutting step 103, a rotating step 104, and a repeating step 105.

[0015] (Retention step 101) Fig. 2 is a side view, partially in section, showing a state after the holding step 101 shown in Fig. 1. The holding step 101 is a step of holding the wafer 1 on the holding surface 21 of the chuck table 20.

[0016] The wafer 1 is, for example, a disk-shaped semiconductor wafer, an optical device wafer, or the like, having a substrate 2 made of silicon (Si), silicon carbide (SiC), gallium nitride (GaN), gallium arsenide (GaAs), or other semiconductor material. Alternatively, the wafer 1 is a disk-shaped wafer having a substrate 2 made of a material such as sapphire (Al2O3), glass, or quartz. Examples of glass include alkali glass, non-alkali glass, soda-lime glass, lead glass, borosilicate glass, and quartz glass. The wafer 1 is not limited to a disk shape, and may be a plate-shaped wafer such as a resin package substrate or a metal substrate.

[0017] 2, the wafer 1 has a chamfered portion 3 along its outer periphery. The chamfered portion 3 in the first embodiment is formed to have an arc-shaped cross section from the front surface 4 to the back surface 5 of the substrate 2. The wafer 1 has, for example, a plurality of planned division lines set in a grid pattern on the front surface 4 of the substrate 2, and devices formed in each area partitioned by the planned division lines.

[0018] The device is formed on a flat surface radially inward from a region where the chamfered portion 3 is formed on the surface 4. The device is, for example, an integrated circuit such as an IC or an LSI, an image sensor such as a CCD (Charge Coupled Device) or a CMOS (Complementary Metal Oxide Semiconductor), or a MEMS (Micro Electro Mechanical Systems).

[0019] In the holding step 101 of the first embodiment, the front surface 4 side of the wafer 1 is held by the holding surface 21 of the chuck table 20. The chuck table 20 is mounted on a cutting device that performs a cutting method for the wafer 1.

[0020] The chuck table 20 is configured to be rotatable about a vertical axis and movable between a processing area facing a cutting unit 30 described below and a load / unload area for loading and unloading the wafer 1. The holding surface 21 of the chuck table 20 is disk-shaped and made of, for example, porous ceramics, and is connected to a vacuum suction source via a vacuum suction path, so that the wafer 1 placed on the holding surface 21 can be suction-held.

[0021] (Positioning step 102) Fig. 3 is a side view, partially in section, showing the state after the positioning step 102 shown in Fig. 1. Fig. 4 is a plan view of Fig. 3. The positioning step 102 is a step of positioning the outer peripheral end 33 of the cutting blade 32 at the cutting depth 6 of the wafer 1 in a state where the cutting blade 32 attached to the tip of the spindle 31 is positioned at a position where it does not overlap the holding surface 21.

[0022] The spindle 31 and the cutting blade 32 are included in a cutting unit 30 of a cutting device that performs a cutting method for the wafer 1. The cutting unit 30 includes the spindle 31, the cutting blade 32, and a cutting fluid supplying means (not shown) that supplies cutting fluid to the wafer 1 and the cutting blade 32 during cutting processing by the cutting unit 30.

[0023] The spindle 31 shown in FIG. 3 etc. is a shaft member having a rotation axis parallel to the holding surface 21 of the chuck table 20. The cutting blade 32 is attached to the tip of the spindle 31. The cutting blade 32 includes abrasive grains such as diamond or CBN (Cubic Boron Nitride) and a bond material such as metal or resin, and has a cutting edge formed to a predetermined thickness. Depending on the type of the density, hardness, etc. of the wafer 1, a cutting blade 32 having an appropriate cutting edge with chipping and cracking within appropriate values ​​is selected. The cutting edge is, for example, a resin bond, a metal bond, a porous bond, or the like.

[0024] The cutting device for carrying out the cutting method of the wafer 1 further includes an imaging unit (not shown) and a moving unit (not shown). The imaging unit (not shown) is provided to move integrally with the cutting unit 30, and captures an image of the upper surface of the wafer 1 held on the chuck table 20. The moving unit (not shown) moves the chuck table 20 and the cutting unit 30 relative to each other.

[0025] The moving units include, for example, a processing feed unit, an indexing feed unit, and a cutting feed unit. The processing feed unit relatively feeds the chuck table 20 and the cutting unit 30 for processing in a direction parallel to the holding surface 21 of the chuck table 20 and perpendicular to the rotation axis of the spindle 31. The indexing feed unit relatively indexes and feeds the chuck table 20 and the cutting unit 30 in a direction parallel to the rotation axis of the spindle 31. The cutting feed unit relatively cuts and feeds the chuck table 20 and the cutting unit 30 in a direction perpendicular to the holding surface 21.

[0026] In the positioning step 102, first, an imaging unit (not shown) images the wafer 1 held on the holding surface 21 of the chuck table 20 to detect the outer circumferential edge 7 including the chamfered portion 3. Next, a moving unit (not shown) moves the chuck table 20 and the cutting unit 30 relatively in the indexing feed direction (direction parallel to the rotation axis of the spindle 31) to align the cutting blade 32 in a plan view on an extension of the processing feed direction (direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31) of the boundary between the outer circumferential edge 7 and the central portion side of the wafer 1. The outer circumferential edge 7 is an area to be cut to a cutting depth of 6 in a linear cutting step 103 described later.

[0027] Next, the chuck table 20 and the cutting unit 30 are moved relatively in the processing feed direction by a moving unit (not shown) to a position where the cutting blade 32 does not overlap the holding surface 21 in a plan view (the position shown in FIG. 4). Next, the chuck table 20 and the cutting unit 30 are moved relatively closer to each other in the cutting feed direction (the direction perpendicular to the holding surface 21) by a moving unit (not shown) to position the lower end of the outer circumferential end 33 of the cutting blade 32 at the cutting depth 6 of the wafer 1. In the following description, the position of the cutting unit 30 positioned in the positioning step 102 is referred to as the standby position.

[0028] (Straight line cutting step 103) Fig. 5 is a side view, partially in cross section, showing one state of the linear cutting step 103 shown in Fig. 1. Fig. 6 is a plan view of Fig. 5. The linear cutting step 103 is a step in which the spindle 31 and the chuck table 20 are relatively moved in a direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31 to linearly cut the outer circumferential edge 7 of the wafer 1, thereby cutting a part of the chamfered portion 3 of the wafer 1.

[0029] The linear cutting step 103 is performed after the positioning step 102. That is, at the start of the linear cutting step 103, the cutting blade 32 is positioned at the standby position. In the linear cutting step 103, first, a cutting fluid supplying means (not shown) starts to supply cutting fluid toward the processing point of the cutting blade 32, and the spindle 31 starts to rotate.

[0030] Next, the chuck table 20 and the cutting unit 30 are moved relatively in the processing feed direction (a direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31) by a moving unit (not shown). This causes the cutting blade 32 to cut from the outer periphery of the wafer 1 along the boundary line between the outer periphery end 7 and the central side to a cutting depth of 6. Then, the processing feed of the cutting unit 30 is continued, and the outer periphery end 7 of the wafer 1 is cut in a straight line to a cutting depth of 6, thereby cutting a part of the chamfered portion 3.

[0031] The outer peripheral end 7 cut by the cutting blade 32 is formed into a step having a cutting surface 8-1 (see FIGS. 7 and 8) located 6 minutes below the rear surface 5 as the upper surface. After the linear cutting step 103 is completed, the chuck table 20 and the cutting unit 30 are moved relatively by a moving unit (not shown) to move the cutting unit 30 to a standby position.

[0032] (Rotation step 104) Fig. 7 is a side view, partially in cross section, showing the state after the rotating step 104 shown in Fig. 1. Fig. 8 is a plan view of Fig. 7. The rotating step 104 is performed after the linear cutting step 103. The rotating step 104 is a step in which the chuck table 20 is rotated by a predetermined rotation angle.

[0033] In the rotating step 104 of the first embodiment, the chuck table 20 is rotated 45 degrees counterclockwise in a plan view. During the rotating step 104, the supply of cutting fluid and the rotation of the spindle 31 are continued.

[0034] The rotation angle by which the chuck table 20 is rotated in the rotating step 104 is determined in advance based on the width of the chamfered portion 3 and the width of the outer circumferential end portion 7 to be cut in the linear cutting step 103. That is, in the subsequent repeating step 105, the rotation angle of the chuck table 20 in the rotating step 104 is determined so that the chamfered portion 3 does not remain between adjacent cutting surfaces 8.

[0035] (Repeat step 105) Fig. 9 is a plan view showing the wafer 1 after the repeating step 105 shown in Fig. 1. The repeating step 105 is a step in which the linear cutting step 103 and the rotating step 104 are repeatedly performed until the entire chamfered portion 3 of the wafer 1 is removed.

[0036] The second and subsequent linear cutting steps 103 are performed after the rotation step 104. That is, at the start of the linear cutting step 103, the cutting blade 32 is positioned at a standby position where the cutting blade 32 does not overlap the holding surface 21 and the outer peripheral end 33 of the cutting blade 32 is at the cutting depth 6 of the wafer 1 (see FIGS. 7 and 8).

[0037] In the second linear cutting step 103, similarly to the first linear cutting step 103, the chuck table 20 and the cutting unit 30 are moved relatively in the processing feed direction (a direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31) to linearly cut the outer circumferential edge 7 of the wafer 1 at a cutting depth of 6, thereby cutting away a part of the chamfered portion 3. The outer circumferential edge 7 cut by the cutting blade 32 is formed into a step whose upper surface is the cutting surface 8-2 located below the back surface 5 by the cutting depth of 6.

[0038] In the repeat step 105, the linear cutting step 103 and the rotation step 104 are repeated in order, and the outer peripheral edge 7 of the wafer 1 rotated by a predetermined rotation angle in the rotation step 104 is cut one after another to form steps with the cut surfaces 8-2, 8-3, 8-4, 8-5, 8-6, 8-7, and 8-8 as upper surfaces. As a result, the outer peripheral edge 7 on the back surface 5 side of the wafer 1 is trimmed into a polygonal shape (a regular octagonal shape in the first embodiment). Note that, when the outer peripheral edge 7 is cut in the n-th linear cutting step 103 (the eighth in the first embodiment) and all of the chamfered portion 3 is removed, the n-th rotation step 104 may be omitted.

[0039] As described above, in the wafer 1 of the first embodiment, the cutting blade 32 is moved only in a direction perpendicular to the rotation axis of the spindle 31 for the wafer 1 held on the chuck table 20, and the outer peripheral end 7 is cut in a straight line to cut a part of the chamfered portion 3, and this is repeated to cut all of the chamfered portion 3. As a result, the chamfered portion 3 can be removed while suppressing the lateral load on the cutting blade 32 compared to cutting the chamfered portion 3 in an annular shape, and therefore chipping and cracking can be suppressed.

[0040] Second Embodiment Next, a method for processing a laminated wafer 10 according to a second embodiment of the present invention will be described with reference to the drawings. In the following description, elements similar to those in the first embodiment are given the same reference numerals and description thereof will be omitted.

[0041] The method for processing the laminated wafer 10 is a method for cutting the outer peripheral edge 7 of the first wafer 1-1 to remove the chamfered portion 3 and grinding the surface 11 on the first wafer 1-1 side in the laminated wafer 10 in which the first wafer 1-1 and the second wafer 1-2 are laminated. FIG. 10 is a flowchart showing the flow of the method for processing the laminated wafer 10 according to the second embodiment. As shown in FIG. 10, the method for processing the laminated wafer 10 according to the second embodiment includes a first holding step 201, a positioning step 202, a linear cutting step 203, a rotation step 204, a repeating step 205, a second holding step 206, and a grinding step 207.

[0042] (First holding step 201) Fig. 11 is a side view, partially in cross section, showing a state after the first holding step 201 shown in Fig. 10. The first holding step 201 is a step in which the surface 12 of the laminated wafer 10 facing the second wafer 1-2 is held by the holding surface 21 of the chuck table 20, thereby exposing the surface 11 facing the first wafer 1-1.

[0043] The laminated wafer 10 is a laminated wafer in which a first wafer 1-1 and a second wafer 1-2 are bonded together. The first wafer 1-1 is the same wafer as the wafer 1 in the first embodiment. In the second embodiment, the second wafer 1-2 is described as being the same wafer as the first wafer 1-1, but in the present invention, the second wafer 1-2 may be a simple substrate wafer without a pattern.

[0044] The first wafer 1-1 and the second wafer 1-2 are bonded to each other at their front surfaces 4 having devices. That is, the surface 11 of the laminated wafer 10 on the first wafer 1-1 side is the back surface 5 of the first wafer 1-1, and the surface 12 of the laminated wafer 10 on the second wafer 1-2 side is the back surface 5 of the second wafer 1-2. The first wafer 1-1 and the second wafer 1-2 may be bonded to each other via a bonding layer or directly. The bonding layer may be formed by applying a double-sided tape with an adhesive layer laminated on the front and back surfaces of a base layer, an oxide film, or an adhesive containing a resin or the like.

[0045] In the first holding step 201 of the second embodiment, the surface 12 of the laminated wafer 10 facing the second wafer 1-2, i.e., the back surface 5 of the second wafer 1-2, is held by the holding surface 21 of the chuck table 20. This exposes the surface 11 facing the first wafer 1-1, i.e., the back surface 5 of the first wafer 1-1. The chuck table 20 is the chuck table 20 mounted on the cutting device used in the first embodiment.

[0046] (Positioning step 202) In the positioning step 202, the cutting blade 32 attached to the tip of the spindle 31 is positioned so as not to overlap the holding surface 21, and the spindle 31 and the chuck table 20 are moved relatively close to each other in a direction perpendicular to the holding surface 21, thereby positioning the outer circumferential end 33 of the cutting blade 32 at the cutting depth 6 of the first wafer 1-1. The positioning step 202 in the second embodiment is the same as the positioning step 102 in the first embodiment, except that "wafer 1" is replaced with "first wafer 1-1", and therefore a description thereof will be omitted.

[0047] (Straight line cutting step 203) The linear cutting step 203 is a step of cutting a part of the chamfered portion 3 of the first wafer 1-1 by relatively moving the spindle 31 and the chuck table 20 in a direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31 to linearly cut the outer peripheral edge 7 of the first wafer 1-1. The linear cutting step 203 of the second embodiment is the same as the linear cutting step 103 of the first embodiment except that "wafer 1" and "cut depth 6" are replaced with "first wafer 1-1" and "cut depth 6-2" (see FIG. 12), and therefore a description of the procedure will be omitted.

[0048] In the linear cutting step 203 of the second embodiment, the cutting depth 6-2 is set to the thickness of the first wafer 1-1, and the entire thickness direction of the outer circumferential edge 7, including the chamfered portion 3, is removed. That is, no step is formed with the cut surface 8 as the upper surface as in the first embodiment, and the first wafer 1-1 is formed into a columnar shape with the outer circumferential edge 7 cut in a linear manner as a segmented circle as the bottom surface.

[0049] (Rotation step 204) The rotation step 204 is performed after the linear cutting step 203. The rotation step 204 is a step for rotating the chuck table 20 by a predetermined rotation angle. The rotation step 204 in the second embodiment is the same as the rotation step 104 in the first embodiment except that "wafer 1" is replaced with "first wafer 1-1", and therefore a description thereof will be omitted.

[0050] (Repeat step 205) In the repeat step 205, the linear cutting step 203 and the rotation step 204 are repeatedly performed until the entire chamfered portion 3 of the first wafer 1-1 is removed. The repeat step 205 in the second embodiment is the same as the repeat step 105 in the first embodiment except that "wafer 1" and "cut depth 6" are replaced with "first wafer 1-1" and "cut depth 6-2", and therefore a description of the procedure will be omitted.

[0051] In the second and subsequent linear cutting steps 203, the cutting depth 6-2 is also set to the thickness of the first wafer 1-1, and the entire thickness direction of the outer circumferential edge 7, including the chamfered portion 3, is removed. In the repeating step 205, the linear cutting step 203 and the rotating step 204 are repeated in sequence, and the outer circumferential edge 7 of the wafer 1 rotated a predetermined rotation angle in the rotating step 204 is cut one after another, so that the outer circumferential edge 7 is formed into a linearly cut polygonal prism (a regular octagonal prism in the second embodiment) (see FIG. 12).

[0052] (Second holding step 206) Fig. 12 is a side view, partially in cross section, showing a state after the second holding step 206 shown in Fig. 10. The second holding step 206 is a step in which the surface 12 of the laminated wafer 10 facing the second wafer 1-2 is held by the second holding surface 41 of the second chuck table 40, thereby exposing the surface 11 facing the first wafer 1-1.

[0053] The second chuck table 40 is mounted on a grinding device that performs a grinding step 207 described later. The second chuck table 40 is configured to be rotatable about a vertical axis and movable between a processing area facing a grinding unit 50 described later and a load / unload area for loading and unloading the laminated wafers 10. The second holding surface 41 of the second chuck table 40 has a disk shape made of, for example, porous ceramics, and is connected to a vacuum suction source via a vacuum suction path, and is capable of suction-holding the laminated wafers 10 placed on the second holding surface 41.

[0054] (Grinding step 207) 13 is a side view partially in cross section showing one state of the grinding step 207 shown in FIG. The grinding step 207 is a step of grinding the first wafer 1-1. In the grinding step 207, the back surface 5 side of the first wafer 1-1 is thinned to a predetermined thickness by a grinding device. The grinding device includes the second chuck table 40, the grinding unit 50, a lifting unit (not shown) that brings the grinding wheel 52 and the second chuck table 40 relatively close to each other, and a grinding fluid supplying means (not shown) that supplies a grinding fluid to the processing points of the first wafer 1-1 and the grinding unit 50.

[0055] The grinding unit 50 includes a second spindle 51, a grinding wheel 52, and a grinding stone 53. The second spindle 51 is a shaft member having a rotation axis perpendicular to the second holding surface 41 of the second chuck table 40. The grinding wheel 52 is attached to the tip of the second spindle 51 and rotates with the rotation of the second spindle 51. The grinding stone 53 is attached to the lower surface of the grinding wheel 52 and faces the second holding surface 41 of the second chuck table 40 in the processing area.

[0056] In the grinding step 207, first, the second chuck table 40 starts to rotate about its axis and the second spindle 51 starts to rotate. Next, a grinding fluid supplying means (not shown) starts to supply grinding fluid toward the processing point of the grinding wheel 53, and a lifting unit (not shown) moves the grinding wheel 52 and the second chuck table 40 relatively closer to each other. By moving the grinding wheel 53 closer to the first wafer 1-1 at a predetermined feed speed, the back surface 5 of the first wafer 1-1 is ground by the grinding wheel 53, thereby thinning the wafer to a predetermined thickness.

[0057] As described above, in the processing method for laminated wafers 10 of the second embodiment, the cutting blade 32 is moved only in a direction perpendicular to the rotation axis of the spindle 31 with respect to the first wafer 1-1 held on the chuck table 20 in the same procedure as in the first embodiment, and the outer peripheral end portion 7 is cut in a linear manner to cut a part of the chamfered portion 3, and this is repeated to cut all of the chamfered portion 3. As a result, compared to cutting the chamfered portion 3 in an annular shape, the chamfered portion 3 can be removed while suppressing the lateral load on the cutting blade 32, thereby suppressing chipping and cracking.

[0058] Furthermore, in the grinding step 207, when grinding the wafer (first wafer 1-1), grinding is performed from the outer periphery of the wafer toward the center, so that the grinding wheel 53 comes into contact with the wafer edge and activates the self-sharpening edge. Therefore, in the laminated wafer 10, if the first wafer 1-1 has a large or frequent chipping, grinding from the outer periphery during grinding may cause the wafer to peel off starting from the chipping. In the processing method for laminated wafers 10 of the second embodiment, chipping can be suppressed, and therefore peeling during grinding can be suppressed.

[0059] Third Embodiment Next, a method for cutting the wafer 1 according to a third embodiment of the present invention will be described with reference to the drawings. In the following description, elements similar to those in the first embodiment will be given the same reference numerals and description thereof will be omitted.

[0060] Fig. 14 is a flow chart showing the flow of the wafer cutting method according to the third embodiment. As shown in Fig. 14, the wafer cutting method according to the third embodiment includes a holding step 301, a positioning step 302, a linear cutting step 303, a rotating step 304, a repeating step 305, and a circular cutting step 306.

[0061] The holding step 301, positioning step 302, straight cutting step 303, rotating step 304, and repeating step 305 in the third embodiment are similar to the holding step 101, positioning step 102, straight cutting step 103, rotating step 104, and repeating step 105 in the first embodiment, and therefore their explanations are omitted.

[0062] (Circular cutting step 306) Fig. 15 is a side view showing one state of the circular cutting step 306 shown in Fig. 14. Fig. 16 is a plan view showing the wafer 1 after the circular cutting step 306 shown in Fig. 14. The circular cutting step 306 is a step in which the outer peripheral edge 7 of the wafer 1 is cut into an annular shape by rotating the chuck table 20 while the cutting blade 32 is cutting into the outer peripheral edge 7 of the wafer 1 to a cutting depth of 6, thereby forming an annular step portion 9.

[0063] The circular cutting step 306 is performed after the repeating step 305. That is, at the start of the circular cutting step 306, the front surface 4 side of the wafer 1 is held on the holding surface 21 of the chuck table 20. Also, the outer peripheral end 7 on the back surface 5 side of the wafer 1 is trimmed into a polygonal shape (for example, a regular octagonal shape in the first embodiment). The cutting unit 30 is positioned such that the lower end of the outer peripheral end 33 of the cutting blade 32 is positioned at the cutting depth 6, and the cutting blade 32 does not overlap the holding surface 21 in a plan view.

[0064] In the circular cutting step 306, first, the chuck table 20 and the cutting unit 30 are moved relatively by a moving unit (not shown) in a direction parallel to the holding surface 21 and perpendicular to the rotation axis of the spindle 31, so that the cutting blade 32 is positioned at a position where it overlaps with the cutting surface 8 of the wafer 1 in a plan view. Next, cutting fluid is supplied toward the processing point of the cutting blade 32 and the chuck table 20 is rotated around its axis at a predetermined speed while rotating the spindle 31. As a result, the corners of the polygonal columnar portion of the wafer 1 cut to a depth of 6 are removed and cut into a cylindrical shape, and the outer peripheral end portion 7 of the cut to a depth of 6 is removed in an annular shape.

[0065] As described above, in the method for cutting the wafer 1 according to the third embodiment, the linear cutting step 303 for removing the outer peripheral end 7 in a linear manner is repeatedly performed prior to normal annular trimming (circular cutting step 306) to trim the outer peripheral end 7 into a polygonal shape. This makes it possible to reduce the area to be removed in the circular cutting step 306, thereby suppressing the occurrence of chipping, cracking, and the like caused by a lateral load applied to the cutting blade 32. In addition, by performing annular trimming to make the rear surface 5 on the trimmed side into a circular shape, it is possible to suppress vacuum leakage when the rear surface 5 is suction-held by a chuck table in the subsequent process.

[0066] [Fourth embodiment] Next, a method for processing a laminated wafer 10 according to a fourth embodiment of the present invention will be described with reference to the drawings. In the following description, elements similar to those in the second embodiment will be given the same reference numerals and description thereof will be omitted.

[0067] Fig. 17 is a flowchart showing the flow of a processing method for laminated wafers 10 according to the fourth embodiment. As shown in Fig. 17, the processing method for laminated wafers 10 according to the fourth embodiment includes a first holding step 401, a positioning step 402, a linear cutting step 403, a rotating step 404, a repeating step 405, a circular cutting step 406, a second holding step 407, and a grinding step 408.

[0068] The first holding step 401, positioning step 402, straight cutting step 403, rotating step 404, repeating step 405, second holding step 407, and grinding step 408 in the fourth embodiment are similar to the first holding step 201, positioning step 202, straight cutting step 203, rotating step 204, repeating step 205, second holding step 206, and grinding step 207 in the second embodiment, and therefore their explanations are omitted.

[0069] (Circular cutting step 406) The circular cutting step 406 is performed after the repeating step 405 and before the second holding step 407. The circular cutting step 406 is a step of cutting the outer peripheral end 7 of the first wafer 1-1 into an annular shape by rotating the chuck table 20 while the cutting blade 32 is cutting the outer peripheral end 7 of the first wafer 1-1 to a cutting depth 6-2, thereby forming an annular step portion 9. The circular cutting step 406 of the fourth embodiment has the same procedure as the circular cutting step 306 of the third embodiment, except that "wafer 1" and "cut depth 6" are replaced with "first wafer 1-1" and "cut depth 6-2" (see FIG. 12), and therefore a description of the procedure will be omitted.

[0070] As described above, in the processing method for laminated wafers 10 of the fourth embodiment, the linear cutting step 403 for removing the outer peripheral end 7 in a linear manner is repeatedly performed to trim the outer peripheral end 7 into a polygonal shape before normal annular trimming (circular cutting step 406) in the same procedure as in the third embodiment. This makes it possible to reduce the area to be removed in the circular cutting step 406, thereby suppressing the occurrence of chipping, cracking, and the like caused by a lateral load applied to the cutting blade 32. In addition, by performing annular trimming to make the rear surface 5 of the first wafer 1-1 on the trimmed side into a circular shape, it is possible to suppress vacuum leakage when the rear surface 5 is suction-held by a chuck table in the subsequent process.

[0071] It should be noted that the present invention is not limited to the above-described embodiment, and can be practiced in various modified forms without departing from the gist of the present invention.

[0072] For example, in each embodiment, the linear cutting steps 103, 203, 303, and 403 are performed eight times, but the number of cuttings is not particularly limited and may be determined based on the width of the chamfered portion 3 and the width of the outer circumferential end portion 7 to be cut, together with the rotation angle of the chuck table 20 in the rotation steps 104, 204, 304, and 404. Furthermore, the order of cutting is not limited to counterclockwise in plan view, but may be clockwise, and adjacent outer circumferential end portions 7 do not need to be cut consecutively.

[0073] Furthermore, in the linear cutting step 103 of the first embodiment and the linear cutting step 303 of the third embodiment, the cutting depth 6 is set to be smaller than half the thickness of the wafer 1 to form a step with the cutting surface 8 as the upper surface, but as in the linear cutting step 203 of the second embodiment and the linear cutting step 403 of the fourth embodiment, the entire thickness direction of the wafer 1 may be cut with a cutting depth 6-2, which is the entire thickness direction of the wafer 1, up to the surface 4 side.

[0074] Furthermore, in the linear cutting step 203 of the second embodiment and the linear cutting step 403 of the fourth embodiment, the cutting depth 6-2 is set to the entire thickness direction of the wafer 1, and the entire thickness direction of the wafer 1 is cut up to the surface 4 side. However, as in the linear cutting step 103 of the first embodiment and the linear cutting step 303 of the third embodiment, a step may be formed with a cutting depth 6 that is less than half the thickness of the wafer 1, with the cutting surface 8 as the upper surface. [Explanation of symbols]

[0075] 1 wafer 1-1 First wafer 1-2 Second wafer 3 Chamfered part 4 surface 5 Back side 6, 6-2 Cutting depth 7 Outer edge 8 Cutting surface 9 Step 10 Stacked wafers 11, 12 sides 20 Chuck table (first chuck table) 21 Holding surface (1st holding surface) 30 Cutting unit 31 Spindle (1st Spindle) 32 Cutting blade 33 Outer edge 40 Second chuck table 41 Second holding surface 50 Grinding Unit 51 Second Spindle 52 Grinding Wheel 53 Grinding Wheel

Claims

1. A method for cutting a wafer, comprising the steps of: cutting an outer peripheral edge of a disk-shaped wafer and removing a chamfered portion, the method comprising the steps of: a holding step of holding the wafer on a holding surface of a chuck table; a positioning step in which a cutting blade attached to a tip of a spindle having a rotation axis parallel to the holding surface is positioned so as not to overlap the holding surface, the spindle and the chuck table are moved relatively close to each other in a direction perpendicular to the holding surface, and an outer peripheral end of the cutting blade is positioned at a cutting depth of the wafer; a linear cutting step of cutting a part of the chamfered portion of the wafer by relatively moving the spindle and the chuck table in a direction parallel to the holding surface and perpendicular to the rotation axis of the spindle to linearly cut the outer peripheral edge of the wafer; a rotating step of rotating the chuck table by a predetermined rotation angle after the linear cutting step; a repeating step of repeatedly performing the linear cutting step and the rotating step until all of the chamfer of the wafer is removed; A method for cutting a wafer comprising the steps of:

2. After the repeating step, the method further includes a circular cutting step of cutting the outer peripheral edge of the wafer in an annular shape by rotating the chuck table while the cutting blade is cutting the outer peripheral edge of the wafer to the cutting depth, thereby forming an annular step portion.

2. The method for cutting a wafer according to claim 1.

3. A method for processing a laminated wafer in which a first wafer and a second wafer having a chamfered portion at an outer peripheral end portion are bonded together, comprising the steps of: a first holding step of holding a surface of the laminated wafer facing the second wafer on a first holding surface of a first chuck table to expose the surface facing the first wafer; a positioning step of moving the first spindle and the first chuck table relatively close to each other in a direction perpendicular to the first holding surface while a cutting blade attached to a tip of the first spindle having a rotation axis parallel to the first holding surface is positioned so as not to overlap the first holding surface, and positioning the outer circumferential end of the cutting blade at a cutting depth of the first wafer; a linear cutting step of relatively moving the first spindle and the first chuck table in a direction parallel to the first holding surface and perpendicular to a rotation axis of the first spindle to linearly cut the outer circumferential edge of the first wafer, thereby cutting a part of the chamfered portion of the first wafer; a rotating step of rotating the first chuck table by a predetermined rotation angle after the linear cutting step; a repeating step of repeatedly performing the linear cutting step and the rotating step until all of the chamfer of the first wafer is removed; a second holding step of holding the surface of the laminated wafer facing the second wafer on a second holding surface of a second chuck table to expose the surface facing the first wafer; a grinding step of grinding the first wafer by bringing a grinding wheel attached to a tip of a second spindle having a rotation axis perpendicular to the second holding surface and the second chuck table relatively close to each other; The method for processing a laminated wafer includes the steps of:

4. The method further includes a circular cutting step of cutting the outer peripheral edge of the first wafer annularly to form an annular step portion by rotating the first chuck table while the cutting blade is cutting the outer peripheral edge of the first wafer to the cutting depth after the repeating step and before the second holding step. The method for processing laminated wafers according to claim 3 .

Citation Information

Patent Citations

  • Method and apparatus for manufacturing semiconductor device

    JP2000173961A