Magnetic recording medium, magnetic tape cartridge, and magnetic recording and reproducing device
A nitrogen-containing polymer with a fluorine-containing group and polyester chain on the magnetic layer addresses spacing loss and abrasion issues, ensuring low friction and stability in magnetic recording media.
Patent Information
- Application Number
- JP2023070782
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Magnetic recording media experience spacing loss due to foreign matter adhering to the magnetic head, leading to output fluctuations, and the magnetic head is abraded when the magnetic layer surface abrasiveness is too high, while maintaining low friction and stability during repeated runs is desirable.
Incorporating a nitrogen-containing polymer with a fluorine-containing group and a polyester chain on the magnetic layer, forming a salt crosslinked structure, which enhances abrasion resistance and reduces friction, maintaining the surface shape and lubricity.
The magnetic layer exhibits appropriate abrasion resistance, low friction, and minimal shape change after repeated use, reducing spacing loss and protecting the magnetic head.
Smart Images

Figure 2024156375000001 
Figure 2024156375000002 
Figure 2024156375000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic recording medium, a magnetic tape cartridge, and a magnetic recording / reproducing device. [Background technology]
[0002] Magnetic recording media are generally produced by forming a magnetic layer containing ferromagnetic powder and optionally one or more additives on a non-magnetic support. For example, in the examples of Patent Document 1, a magnetic layer is formed using a magnetic layer-forming composition containing a polyalkyleneimine polymer together with ferromagnetic powder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-157252 A Summary of the Invention [Problem to be solved by the invention]
[0004] Recording data on a magnetic recording medium and reproducing the recorded data are usually performed by running the magnetic recording medium in a magnetic recording and reproducing device and contacting and sliding the magnetic head with the magnetic layer surface of the magnetic recording medium. If foreign matter adheres to the magnetic head due to sliding with the magnetic layer surface, the gap between the magnetic layer surface and the magnetic head will widen due to the presence of the foreign matter, and as a result, output fluctuations called spacing loss may occur. Therefore, if the magnetic layer surface exhibits abrasive properties and the foreign matter attached to the magnetic head can be removed by abrasion during sliding with the magnetic layer surface, it is desirable because the spacing loss can be reduced. On the other hand, if the abrasive properties of the magnetic layer surface are too high, the magnetic head itself will be worn away, so it is desirable for the magnetic layer surface to exhibit moderate abrasive properties.
[0005] From the viewpoint of running stability, it is also desirable that the coefficient of friction between the magnetic layer surface and the magnetic head is low even when the magnetic recording medium is repeatedly run.Furthermore, from the viewpoint of maintaining the wear resistance of the magnetic layer surface, it is also desirable that the change in the surface shape of the magnetic layer is small before and after repeated running.
[0006] One aspect of the present invention aims to provide a magnetic recording medium in which the magnetic layer surface can exhibit moderate wear resistance, can exhibit a low coefficient of friction even after repeated running, and in which the surface shape of the magnetic layer changes little before and after repeated running. [Means for solving the problem]
[0007] One aspect of the present invention is as follows. [1] A magnetic recording medium having a non-magnetic support and a magnetic layer containing a ferromagnetic powder, A nitrogen-containing polymer (hereinafter also referred to as a "fluorine-based nitrogen-containing polymer") is contained in the portion of the non-magnetic support on the magnetic layer side, The nitrogen-containing polymer comprises a fluorine-containing group and a polyester chain; the fluorine-containing group is bonded to a nitrogen atom of the nitrogen-containing polymer; The polyester chain is bonded to a nitrogen atom of the nitrogen-containing polymer or forms a salt bridge structure with a nitrogen atom of the nitrogen-containing polymer; and A magnetic recording medium, wherein the contact angle with water measured on the surface of the magnetic layer after washing with hexane is 90° or more. [2] The magnetic recording medium according to [1], wherein the nitrogen-containing polymer is a polyalkyleneimine-based polymer. [3] The magnetic recording medium according to [1] or [2], wherein the fluorine-containing group includes a group selected from the group consisting of a fluorinated alkyl group and a perfluoropolyether group. [4] The magnetic recording medium according to [3], wherein the fluoroalkyl group is a fluoroalkyl group having 1 to 6 carbon atoms. [5] The magnetic recording medium according to any one of [1] to [4], wherein the contact angle is 90° or more and 110° or less. [6] The magnetic recording medium according to any one of [1] to [5], further comprising at least one fatty acid compound selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides, on the magnetic layer side of the non-magnetic support. [7] The magnetic recording medium according to any one of [1] to [6], further comprising a nitrogen-containing polymer other than the nitrogen-containing polymer in a portion on the magnetic layer side of the non-magnetic support. [8] The magnetic recording medium according to any one of [1] to [7], further comprising a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer. [9] The magnetic recording medium according to any one of [1] to [8], further comprising a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.
[10] The magnetic recording medium according to any one of [1] to [9], which is a magnetic tape.
[11] The nitrogen-containing polymer is a polyalkyleneimine-based polymer, The fluorine-containing group includes a group selected from the group consisting of a fluorinated alkyl group and a perfluoropolyether group, The fluorinated alkyl group is a fluorinated alkyl group having 1 to 6 carbon atoms, The contact angle is equal to or greater than 90° and equal to or less than 110°, the non-magnetic support further comprises at least one fatty acid compound selected from the group consisting of fatty acids, fatty acid esters and fatty acid amides, and a nitrogen-containing polymer other than the nitrogen-containing polymer, on the magnetic layer side of the non-magnetic support; a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer, a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer; and The magnetic recording medium according to any one of [1] to
[10] , which is a magnetic tape.
[12] A magnetic tape cartridge comprising the magnetic tape described in
[10] or
[11] .
[13] A magnetic recording and reproducing device comprising the magnetic recording medium according to any one of [1] to
[11] . Effect of the Invention
[0008] According to one aspect of the present invention, it is possible to provide a magnetic recording medium in which the surface of the magnetic layer exhibits appropriate wear resistance, exhibits a low coefficient of friction even after repeated running, and exhibits little change in the surface shape of the magnetic layer before and after repeated running. Also, according to one aspect of the present invention, it is possible to provide a magnetic tape cartridge and a magnetic recording and reproducing device including the magnetic recording medium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Magnetic recording media] One aspect of the present invention relates to a magnetic recording medium having a non-magnetic support and a magnetic layer containing ferromagnetic powder. The magnetic recording medium includes a nitrogen-containing polymer on the magnetic layer side of the non-magnetic support, the nitrogen-containing polymer includes a fluorine-containing group and a polyester chain, the fluorine-containing group is bonded to a nitrogen atom of the nitrogen-containing polymer, the polyester chain is bonded to a nitrogen atom of the nitrogen-containing polymer, or forms a salt bridge structure with the nitrogen atom of the nitrogen-containing polymer, and the contact angle with water measured on the surface of the magnetic layer after hexane washing (hereinafter also referred to as "contact angle after hexane washing") is 90° or more.
[0010] In the present invention and this specification, the "portion on the non-magnetic support facing the magnetic layer" refers to the magnetic layer in the case of a magnetic recording medium having a magnetic layer directly on the non-magnetic support, and refers to the magnetic layer and / or the non-magnetic layer in the case of a magnetic recording medium having a non-magnetic layer described below between the non-magnetic support and the magnetic layer. The "portion on the non-magnetic support facing the magnetic layer" is also simply referred to as the "portion on the magnetic layer side." The presence of a certain component on the surface facing the magnetic layer of the magnetic recording medium is also included in the component being included in the portion on the magnetic layer side.
[0011] The magnetic recording medium includes the fluorine-based nitrogen-containing polymer in a portion on the magnetic layer side. The fluorine-based nitrogen-containing polymer includes a fluorine-containing group and a polyester chain. It is believed that the fluorine-based nitrogen-containing polymer can function as a lubricant for magnetic recording media. Lubricants can be broadly divided into boundary lubricants and fluid lubricants. The present inventor believes that the fluorine-based nitrogen-containing polymer can play a role in providing lubricity to the magnetic layer surface by being present on the magnetic layer surface and functioning as a boundary lubricant. For example, it is believed that at least a part of the fluorine-based nitrogen-containing polymer contained in the magnetic layer can be present on the magnetic layer surface. Furthermore, the present inventor presumes that the fluorine-based nitrogen-containing polymer contained inside the magnetic layer can be present on the magnetic layer surface by moving to the magnetic layer surface during sliding with the magnetic head, etc. In addition, the fluorine-based nitrogen-containing polymer may be contained in the non-magnetic layer described later, and it is believed that the fluorine-based nitrogen-containing polymer contained in the non-magnetic layer can move to the magnetic layer and further move to the magnetic layer surface to be present on the magnetic layer surface. The present inventor also believes that the contact angle after hexane washing can be an indicator of the amount of the fluorine-based nitrogen-containing polymer present in the magnetic layer side portion.The present inventor also speculates that the inclusion of the fluorine-based nitrogen-containing polymer in the magnetic layer side portion in an amount that makes the contact angle after hexane washing 90° or more leads to the magnetic layer surface of the magnetic recording medium being able to exhibit lubricity so as to realize the appropriate wear resistance of the magnetic layer surface, the low friction coefficient after repeated running, and the suppression of the change in the surface shape of the magnetic layer before and after repeated running.The fluorine-containing group and polyester chain of the fluorine-based nitrogen-containing polymer are hydrophobic parts, and the present inventor believes that the presence of these hydrophobic parts contributes to the provision of excellent lubricity to the magnetic layer surface. However, the above is merely speculation and does not limit the present invention, nor is the present invention limited to other speculations described in this specification.
[0012] The above magnetic recording medium will now be described in more detail.
[0013] <Contact angle after washing with hexane> In the present invention and this specification, the contact angle with water measured on the surface of the magnetic layer after washing with hexane (contact angle after washing with hexane) is determined by the following method. In the present invention and this specification, the "surface of the magnetic layer" is synonymous with the magnetic layer side surface of the magnetic recording medium.
[0014] "Room temperature" as used herein refers to a temperature in the range of 20 to 25° C. Unless otherwise specified, the following treatments are carried out at room temperature.
[0015] (Hexane wash) A sample piece for measuring the contact angle is cut out from the magnetic recording medium to be measured. For magnetic tape, the size of the sample piece is 30 cm in length. Magnetic tape is usually 1 / 2 inch wide. 1 inch = 0.0254 meters. For magnetic tape with a width other than 1 / 2 inch, a sample piece 30 cm in length is also cut out as the sample piece for measuring the contact angle. For magnetic disks, a sample piece of the same size as for magnetic tape can be cut out. The entire sample piece is immersed in 10 mL of fresh hexane for 1 hour. During the immersion, the container containing the sample and hexane is left to stand without stirring. n-hexane is used as the hexane. "Fresh" means unused. After 1 hour, the sample pieces are removed from the hexane and allowed to air dry at room temperature for at least 24 hours.
[0016] (Contact angle measurement) The contact angle is determined by the θ / 2 method, by dropping water onto the measurement points on the magnetic layer surface of the sample piece after washing with hexane in a measurement environment of an ambient temperature of 20°C and a relative humidity of 25%. An example of the measurement conditions will be described later in the Examples section. The measurement points are six randomly selected points on the magnetic layer surface, and the contact angle is measured at each of the six points. The arithmetic average of the six measured values thus obtained is regarded as the contact angle with water measured on the surface of the magnetic layer after washing with hexane of the magnetic recording medium to be measured.
[0017] The contact angle of the magnetic recording medium after washing with hexane may be 90° or more, or may be 95° or more or 100° or more, from the viewpoint of achieving appropriate wear resistance of the magnetic layer surface, a low coefficient of friction after repeated running, and suppression of changes in the surface shape of the magnetic layer before and after repeated running. The contact angle of the magnetic recording medium after washing with hexane is preferably 120° or less, more preferably 115° or less, and even more preferably 110° or less, from the viewpoint of maintaining the strength of the magnetic layer. The unit of angle "°" is also expressed as degree.
[0018] The contact angle of the magnetic recording medium after washing with hexane can be controlled by the amount of the fluorine-containing nitrogen-containing polymer used for manufacturing the magnetic recording medium. Also, the contact angle of the magnetic recording medium after washing with hexane can be controlled by the amount of the nitrogen-containing polymer and the fluorine-containing compound that can form the fluorine-containing nitrogen-containing polymer in the manufacturing process of the magnetic recording medium, as described below.
[0019] <Fluorine-based nitrogen-containing polymer> In the present invention and this specification, "polymer" includes homopolymers and copolymers. "Nitrogen-containing polymer" refers to a polymer having a nitrogen-containing repeating unit. The nitrogen-containing polymer may contain two or more types of nitrogen-containing repeating units with different structures.
[0020] In the above fluorine-based nitrogen-containing polymer, the fluorine-containing group is bonded to the nitrogen atom of the fluorine-based nitrogen-containing polymer. In the above fluorine-based nitrogen-containing polymer, the polyester chain is bonded to the nitrogen atom of the fluorine-based nitrogen-containing polymer or forms a salt bridge structure with the nitrogen atom of the fluorine-based nitrogen-containing polymer. The bond between the fluorine-containing group and the nitrogen atom and the bond between the polyester chain and the nitrogen atom can be a covalent bond. The above fluorine-based nitrogen-containing polymer can contain a plurality of fluorine-containing groups and polyester chains. All of the plurality of polyester chains may be bonded to the nitrogen atom of the fluorine-based nitrogen-containing polymer, all of them may form a salt bridge structure with the nitrogen atom of the fluorine-based nitrogen-containing polymer, or a part of them may be bonded to the nitrogen atom of the fluorine-based nitrogen-containing polymer, and the remaining part may form a salt bridge structure with the nitrogen atom of the fluorine-based nitrogen-containing polymer. The fluorine-based nitrogen-containing polymer can be synthesized by the reaction of a nitrogen-containing polymer with a fluorine-containing compound. The reaction can easily proceed by mixing the nitrogen-containing polymer with the fluorine-containing compound at room temperature. In one embodiment, a magnetic recording medium containing a fluorine-based nitrogen-containing polymer in the magnetic layer can be produced by forming a magnetic layer using a fluorine-based nitrogen-containing polymer synthesized by the reaction of a nitrogen-containing polymer with a fluorine-containing compound as a component of a magnetic layer forming composition. In another embodiment, a nitrogen-containing polymer and a fluorine-containing compound can be used as components of a magnetic layer forming composition, and these components can be mixed in the preparation process of the magnetic layer forming composition, thereby reacting the nitrogen-containing polymer with the fluorine-containing compound during the preparation process to form a fluorine-based nitrogen-containing polymer. The above points are also the same when forming a non-magnetic layer containing the fluorine-based nitrogen-containing polymer. Hereinafter, a nitrogen-containing polymer that can form a fluorine-based nitrogen-containing polymer by reacting with a fluorine-containing compound is called a "nitrogen-containing raw material polymer".
[0021] The fluorine-based nitrogen-containing polymer may contain a plurality of polyester chains having the same or different structures. For the polyester chains contained in the fluorine-based nitrogen-containing polymer, the description of the polyester chain described below can be referred to.
[0022] The fluorine-containing nitrogen-containing polymer can contain a plurality of fluorine-containing groups of the same or different structures. The fluorine-containing group of the fluorine-containing nitrogen-containing polymer can contain a group selected from the group consisting of fluorinated alkyl groups and perfluoropolyether groups. For details of fluorinated alkyl groups and perfluoropolyether groups, the description of the fluorine-containing compound described below can be referred to.
[0023] The fluorine-containing group can be a monovalent group represented by "*-L-Rf". Here, "Rf" represents a fluorinated alkyl group or a perfluoropolyether group, and details will be described later with respect to the fluorine-containing compound. * represents a bonding position where the monovalent group is bonded to a nitrogen atom of the fluorine-based nitrogen-containing polymer. L represents a divalent linking group. Examples of the divalent linking group represented by L include "-(C=O)-" (carbonyl group) and "-(C=O)-NH-" (amide bond). For example, the monovalent group can be a monovalent group represented by "*-(C=O)-Rf", "*-(C=O)-NH-Rf", etc.
[0024] In one embodiment, the fluorine-based nitrogen-containing polymer can be a polyalkyleneimine-based polymer. A "polyalkyleneimine-based polymer" is a polymer containing one or more polyalkyleneimine chains. A polyalkyleneimine chain is a polymer structure containing two or more identical or different alkyleneimine chains. The polyalkyleneimine chain is described further below. In one embodiment, it is believed that the polyalkyleneimine chain can function as an adsorption site for the ferromagnetic powder contained in the magnetic layer.
[0025] In the following, polyalkyleneimine-based polymers that can be used as nitrogen-containing raw polymers when the fluorine-based nitrogen-containing polymer is a polyalkyleneimine-based polymer will be described. The following description of polyalkyleneimine-based polymers also applies to the case where the fluorine-based nitrogen-containing polymer is a polyalkyleneimine-based polymer, unless otherwise specified.
[0026] (Nitrogen-containing raw polymer) Polyalkyleneimine Chain When the above-mentioned fluorine-containing nitrogen-containing polymer is a polyalkyleneimine-based polymer, examples of the nitrogen-containing raw material polymer that can be used to obtain such a fluorine-containing nitrogen-containing polymer include polyalkyleneimine-based polymers having polyester chains.
[0027] When the nitrogen-containing raw polymer is a polyalkyleneimine polymer, examples of the alkyleneimine chain contained in the polyalkyleneimine polymer include an alkyleneimine chain represented by the following formula A and an alkyleneimine chain represented by the following formula B. Among the alkyleneimine chains represented by the following formulas, the alkyleneimine chain represented by formula A includes a bonding position with a polyester chain described later. The alkyleneimine chain represented by formula B bonds to the polyester chain by forming a salt bridge structure (described in detail later). The polyalkyleneimine chain may be one that is composed of only a straight chain structure or one that has a branched tertiary amine structure. Examples of those that include a branched structure include the alkyleneimine chain represented by formula A below. 1 and * in the following formula B 2 and the like, which is bonded to an adjacent alkyleneimine chain in the following formula:
[0028] [ka]
[0029] In formula A, R 1 and R 2each independently represents a hydrogen atom or an alkyl group, a1 represents an integer of 2 or more, * 1 represents a bonding position to another adjacent polymer chain (for example, an adjacent alkyleneimine chain or a polyester chain described later), or to a hydrogen atom or a substituent.
[0030] [ka]
[0031] In formula B, R 3 and R 4 each independently represents a hydrogen atom or an alkyl group, and a2 represents an integer of 2 or more. The alkyleneimine chain represented by formula B is linked to another polymer chain having an anionic group by the N + and an anionic group contained in another polymer chain can form a salt bridge structure.
[0032] * in formula A and formula B, and * in formula B 2 each independently represents a position at which the group is bonded to an adjacent alkyleneimine chain, or a hydrogen atom or a substituent.
[0033] The above formula A and formula B will be described in more detail below. In the present invention and this specification, unless otherwise specified, the groups described may have a substituent or may be unsubstituted. When a group has a substituent, examples of the substituent include an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a hydroxyl group, an alkoxy group (e.g., an alkoxy group having 1 to 6 carbon atoms), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom), a cyano group, an amino group, a nitro group, an acyl group, and a carboxyl group. In addition, the "carbon number" of a group having a substituent means the carbon number of the portion not including the substituent.
[0034] R in formula A 1 and R 2 and R in formula B 3 and R 4Each of R independently represents a hydrogen atom or an alkyl group. Examples of the alkyl group include an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group or an ethyl group, and further preferably a methyl group. 1 and R 2 The combination of R in formula B includes a form in which one is a hydrogen atom and the other is an alkyl group, a form in which both are hydrogen atoms, and a form in which both are alkyl groups (the same or different alkyl groups), and preferably a form in which both are hydrogen atoms. 3 and R 4 The same applies to.
[0035] The structure with the smallest number of carbon atoms constituting the ring as an alkyleneimine is ethyleneimine, and the number of carbon atoms in the main chain of the alkyleneimine chain (ethyleneimine chain) obtained by ring-opening of ethyleneimine is 2. Therefore, the lower limit of a1 in formula A and a2 in formula B is 2. That is, a1 in formula A and a2 in formula B are each independently an integer of 2 or more. a1 in formula A and a2 in formula B can each independently be, for example, 10 or less, preferably 6 or less, more preferably 4 or less, even more preferably 2 or 3, and even more preferably 2.
[0036] The details of the bonds between the alkyleneimine chain represented by formula A and the alkyleneimine chain represented by formula B and the polyester chain, and the formation of the salt bridge structure will be described later.
[0037] Each of the alkyleneimine chains is bonded to an adjacent alkyleneimine chain, or a hydrogen atom or a substituent at the position represented by * in each formula. Examples of the substituent include monovalent substituents such as alkyl groups (e.g., alkyl groups having 1 to 6 carbon atoms), but are not limited thereto. In addition, other polymer chains (e.g., polyester chains described below) may be bonded as the substituent.
[0038] The number average molecular weight of the polyalkyleneimine chain contained in the polyalkyleneimine polymer is preferably 300 or more, more preferably 500 or more. The number average molecular weight of the polyalkyleneimine chain is preferably 3,000 or less, more preferably 2,000 or less. The number average molecular weight of the polyalkyleneimine chain contained in the polyalkyleneimine polymer is a value obtained as described in paragraph 0027 of JP 2015-28830 A. As described in the same paragraph, the number average molecular weight of the polyalkyleneimine used to synthesize the polyalkyleneimine polymer can be adopted as the number average molecular weight of the polyalkyleneimine chain contained in the polyalkyleneimine polymer.
[0039] In one embodiment, the proportion of polyalkyleneimine chains in the polyalkyleneimine polymer (hereinafter also referred to as "polyalkyleneimine chain ratio") is preferably less than 5.0% by mass, more preferably 4.9% by mass or less, even more preferably 4.8% by mass or less, even more preferably 4.5% by mass or less, even more preferably 4.0% by mass or less, and even more preferably 3.0% by mass or less. In one embodiment, the polyalkyleneimine chain ratio is preferably 0.2% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more. The proportion of the polyalkyleneimine chain described above can be controlled, for example, by the mixing ratio of the polyalkyleneimine and the polyester used during synthesis.
[0040] The proportion of polyalkyleneimine chains in a polyalkyleneimine-based polymer can be determined by nuclear magnetic resonance (NMR), more specifically, 1 H-NMR and 13It can be calculated from the analysis results obtained by C-NMR and elemental analysis using a known method. The value calculated in this way is the same as the theoretical value obtained from the blending ratio of the synthetic raw materials of the polyalkyleneimine polymer, so the theoretical value obtained from the blending ratio can be adopted as the proportion of the polyalkyleneimine chain in the polyalkyleneimine polymer (polyalkyleneimine chain ratio).
[0041] With respect to a fluorine-based nitrogen-containing polymer synthesized using a polyalkyleneimine-based polymer as a nitrogen-containing raw polymer, it can be said that the number average molecular weight of the polyalkyleneimine chains contained in this polymer and the proportion of the polyalkyleneimine chains are the same as the number average molecular weight of the polyalkyleneimine chains and the proportion of the polyalkyleneimine chains in the nitrogen-containing raw polymer.
[0042] Polyester Chain The polyalkyleneimine-based polymer that can be used as the nitrogen-containing raw material polymer can contain a polyester chain in addition to the polyalkyleneimine chain described above. In the present invention and this specification, the term "polyester chain" refers to a polymer chain having a plurality of ester bonds. In one embodiment, the polyester chain is an alkyleneimine chain represented by formula A and a * in formula A. 1 In another embodiment, the alkyleneimine chain and the polyester chain represented by formula B can be bonded to the nitrogen atom N contained in formula A via a carbonyl group -(C=O)- to form -N-(C=O)-. In another embodiment, the alkyleneimine chain and the polyester chain represented by formula B can be bonded to the nitrogen cation N + The polyester chain has an anionic group, and the polyester chain has an anionic group, which can form a salt bridge structure. - and N in formula B + Examples of the material include, but are not limited to, those formed by:
[0043] An example of a polyester chain formed by bonding an alkyleneimine chain represented by formula A and a nitrogen atom N contained in formula A via a carbonyl group -(C=O)- is a polyester chain represented by the following formula 1. The polyester chain represented by the following formula 1 is: 1 At the bonding position represented by the formula:, a nitrogen atom contained in the alkyleneimine chain and a carbonyl group -(C=O)- contained in the polyester chain form -N-(C=O)-, thereby bonding to the alkyleneimine chain represented by the formula A.
[0044] [ka]
[0045] In addition, the alkyleneimine chain represented by formula B and N in formula B + An example of a polyester chain in which an anionic group contained in the polyester chain forms a salt bridge structure and bonds with the polyester chain is the polyester chain represented by the following formula 2. The polyester chain represented by the following formula 2 is an oxygen anion O - Therefore, N in formula B + It is possible to form a salt bridge structure with
[0046] [ka]
[0047] L in Equation 1 1 and L in Eq. 2 each independently represents a divalent linking group. The divalent linking group is preferably an alkylene group having 3 to 30 carbon atoms. When the alkylene group has a substituent, the number of carbon atoms of the alkylene group refers to the number of carbon atoms in the portion excluding the substituent (main chain portion) as described above.
[0048] b11 in formula 1 and b21 in formula 2 each independently represent an integer of 2 or more, for example, an integer of 200 or less.
[0049] b12 in formula 1 and b22 in formula 2 each independently represent 0 or 1.
[0050] X in formula 1 1 and X in Eq. 2 each independently represents a hydrogen atom or a monovalent substituent. Examples of the monovalent substituent include a monovalent substituent selected from the group consisting of an alkyl group, a haloalkyl group (such as a fluoroalkyl group), an alkoxy group, a polyalkyleneoxyalkyl group, and an aryl group.
[0051] The alkyl group may have a substituent or may be unsubstituted. As the alkyl group having a substituent, an alkyl group substituted with a hydroxy group (hydroxyalkyl group) or an alkyl group substituted with one or more halogen atoms is preferred. Also preferred is an alkyl group in which all hydrogen atoms bonded to carbon atoms are substituted with halogen atoms (haloalkyl group). Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom. As the alkyl group, an alkyl group having 1 to 30 carbon atoms is more preferred, and an alkyl group having 1 to 10 carbon atoms is even more preferred. The alkyl group may be linear, branched, or cyclic. The same applies to the haloalkyl group.
[0052] For specific examples of substituted or unsubstituted alkyl groups and haloalkyl groups, see paragraph 0052 of JP2015-28830A. For specific examples of alkoxy groups, see paragraph 0053 of JP2015-28830A.
[0053] Polyalkyleneoxyalkyl groups are R 10 (OR 11 R is a monovalent substituent represented by the formula: 10 represents an alkyl group, R 11 represents an alkylene group, n represents an integer of 2 or more, and m represents 0 or 1. R 10 For the alkyl group represented by X 1 , X 2 The alkyl group represented by R 11For details of the alkylene group represented by X 1 , X 2 The above description of the alkyl group represented by the following formula (1) can be applied to these alkylene groups by removing one hydrogen atom from them (for example, a methyl group can be replaced with a methylene group). n is an integer of 2 or more, for example, an integer of 10 or less, preferably an integer of 5 or less.
[0054] The aryl group may have a substituent or may be a condensed ring, and is more preferably an aryl group having 6 to 24 carbon atoms. Examples of the aryl group include a phenyl group, a 4-methylphenyl group, a 4-phenylbenzoic acid group, a 3-cyanophenyl group, a 2-chlorophenyl group, and a 2-naphthyl group.
[0055] The polyester chain represented by the formula 1 and the polyester chain represented by the formula 2 described above can each be a structure derived from a polyester obtained by a known polyester synthesis method. An example of the polyester synthesis method is ring-opening polymerization of lactone. Examples of the lactone include various lactones described in paragraph 0056 of JP-A-2015-28830. As the lactone, ε-caprolactone, lactide, or δ-valerolactone is preferred from the viewpoint of reactivity and / or availability. However, the lactone is not limited to these, and any lactone may be used as long as it can obtain a polyester by ring-opening polymerization.
[0056] For nucleophilic reagents for ring-opening polymerization of lactones, reference can be made to paragraph 0057 of JP2015-28830A.
[0057] However, the polyester chain is not limited to a structure derived from a polyester obtained by ring-opening polymerization of lactone, and may also be a structure derived from a polyester obtained by a known polyester synthesis method, for example, polycondensation of a polyvalent carboxylic acid and a polyhydric alcohol, or polycondensation of a hydroxycarboxylic acid.
[0058] In one embodiment, the number average molecular weight of the polyester chain is preferably 200 or more, more preferably 400 or more, and even more preferably 500 or more. In one embodiment, the number average molecular weight of the polyester chain is preferably 100,000 or less, and more preferably 50,000 or less. The number average molecular weight of the polyester chain is a value obtained as described in paragraph 0059 of JP2015-28830A.
[0059] Weight average molecular weight of polyalkyleneimine polymer The average molecular weight of the polyalkyleneimine-based polymer that can be used as the nitrogen-containing raw polymer can be, for example, 1,000 or more, and can be, for example, 80,000 or less, as a weight average molecular weight. The weight average molecular weight of the polyalkyleneimine-based polymer that can be used as the nitrogen-containing raw polymer is preferably 1,500 or more, more preferably 2,000 or more, and even more preferably 3,000 or more. In one embodiment, the weight average molecular weight of the polyalkyleneimine-based polymer that can be used as the nitrogen-containing raw polymer is preferably 60,000 or less, more preferably 40,000 or less, even more preferably 35,000 or less, even more preferably 34,000 or less, even more preferably 30,000 or less, even more preferably 20,000 or less, and even more preferably 10,000 or less. The above description is also applicable to the weight average molecular weight when the fluorine-based nitrogen-containing polymer is a polyalkyleneimine-based polymer.
[0060] In the present invention and this specification, the weight average molecular weight of a polyalkyleneimine polymer refers to a value calculated in terms of standard polystyrene by gel permeation chromatography (GPC). For the measurement conditions, see the Examples section of JP2015-28830A.
[0061] Synthesis method The synthesis method of the polyalkyleneimine polymer is not particularly limited. For one embodiment of the synthesis method, reference can be made to paragraphs 0061 to 0069 of JP2015-28830A and the section of Examples therein.
[0062] (Fluorine-containing compounds) Examples of fluorine-containing compounds capable of forming a fluorine-based nitrogen-containing polymer include compounds having one or more groups selected from the group consisting of fluorinated alkyl groups and perfluoropolyether groups in one molecule.
[0063] The fluorinated alkyl group has a structure in which some or all of the hydrogen atoms constituting the alkyl group are substituted with fluorine atoms, and preferably has a structure in which all are substituted with fluorine atoms, i.e., is a perfluoroalkyl group. The fluorinated alkyl group may have a straight chain structure, may have a branched structure, or may be a cyclic fluorinated alkyl group, and is preferably a straight chain structure. The fluorinated alkyl group may have a substituent or may be unsubstituted, and is preferably unsubstituted. The fluorinated alkyl group may be, for example, C n H 2n+1 The fluorinated alkyl group may have a structure in which some or all of the hydrogen atoms constituting the alkyl group represented by - are substituted with fluorine atoms. The number of carbon atoms in the fluorinated alkyl group may be, for example, 1 or more, 2 or more, or 3 or more. The number of carbon atoms in the fluorinated alkyl group may be, for example, 20 or less, 15 or less, 10 or less, 7 or less, 6 or less, 5 or less, or 4 or less.
[0064] The perfluoropolyether group refers to a perfluoroalkyl group having one or more ether bonds, and may be a monovalent group or a divalent or higher group. Examples of the perfluoropolyether group include CF3-(CF2O) p -(CF2CF2O) q -, CF3-[CF(CF3)CF2O] p -[CF2(CF3)]-, CF3-(CF2CF2CF2O) p -, CF3-(CF2CF2O) p -, CF3-(CF2)p -O-[CF(CF3)CF2OCF(CF3)] q The sum of p and q is preferably 1 to 83, more preferably 1 to 43, and further preferably 5 to 23.
[0065] In one embodiment, the fluorine-containing compound can be a fluorinated alkyl group-containing carboxylate or a perfluoropolyether group-containing carboxylate represented by "RfCOOX". Here, "Rf" represents a fluorinated alkyl group or a perfluoropolyether group, and the details are as described above. "X" represents an alkyl group. The alkyl group can be, for example, an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group or an ethyl group, and even more preferably a methyl group. Specific examples of the carboxylate represented by "RfCOOX" include the following fluorine-containing compounds.
[0066] C 11 F 23 COOCH3 C9F 19 COOCH3 C6F 13 COOCH3 C5F 11 COOCH3 C4F9COOCH3 C3F7COOCH3 (CF3)2CFCOOCH3
[0067] [ka]
[0068] In another embodiment, the fluorine-containing compound may be a fluorinated alkyl group-containing isocyanate or a perfluoropolyether group-containing isocyanate represented by "RfNCO". Here, "Rf" represents a fluorinated alkyl group or a perfluoropolyether group, and the details are as described above. A specific example of the isocyanate represented by "RfNCO" may be C4F9NCO (nonafluorobutyl isocyanate).
[0069] The above fluorine-containing compound may be obtained as a commercially available product or may be synthesized by a known method.
[0070] For example, the magnetic layer or the composition for forming the magnetic layer may contain 0.1 parts by mass or more of the fluorine-based nitrogen-containing polymer per 100 parts by mass of the ferromagnetic powder, and preferably 0.5 parts by mass or more. The content of the fluorine-based nitrogen-containing polymer in the magnetic layer or the composition for forming the magnetic layer may be, for example, 20.0 parts by mass or less, 15.0 parts by mass or less, or 10.0 parts by mass or less per 100 parts by mass of the ferromagnetic powder. The fluorine-based nitrogen-containing polymer contained in the magnetic layer or the composition for forming the magnetic layer may be only one type or two or more types. When two or more types are contained, the above content is the total content of the two or more types of fluorine-based nitrogen-containing polymers. Furthermore, when a nitrogen-containing raw material polymer and a fluorine-containing compound are used as components of the magnetic layer forming composition, the contents of the nitrogen-containing raw material polymer and the fluorine-containing compound in the magnetic layer forming composition are as follows. The content of the nitrogen-containing raw polymer in the magnetic layer forming composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, per 100 parts by mass of the ferromagnetic powder. The content of the nitrogen-containing raw polymer in the magnetic layer forming composition can be, for example, 20.0 parts by mass or less, 15.0 parts by mass or less, or 10.0 parts by mass or less, per 100 parts by mass of the ferromagnetic powder. The content of the fluorine-containing compound in the magnetic layer forming composition is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more per 100 parts by mass of the ferromagnetic powder. The content of the fluorine-containing compound in the magnetic layer forming composition can be, for example, 20.0 parts by mass or less, 15.0 parts by mass or less, or 10.0 parts by mass or less per 100 parts by mass of the ferromagnetic powder. For the non-magnetic layer and the composition for forming the non-magnetic layer, the above description can be applied by replacing the ferromagnetic powder with a non-magnetic powder. Regarding the mixing ratio of the nitrogen-containing raw polymer and the fluorine-containing compound, the ratio of the fluorine-containing compound can be 10 mass% or more, 15 mass% or more, 20 mass% or more, 25 mass% or more, or 30 mass% or more, and can be 90 mass% or less, 80 mass% or less, 70 mass% or less, 60 mass% or less, or 50 mass% or less, where the total amount (mass basis) of the fluorine-containing raw polymer and the fluorine-containing compound is 100 mass%.
[0071] The magnetic recording medium may or may not contain a nitrogen-containing polymer other than the fluorine-based nitrogen-containing polymer (hereinafter also referred to as "other nitrogen-containing polymer") in the magnetic layer side portion on the non-magnetic support together with the fluorine-based nitrogen-containing polymer. In one embodiment, the other nitrogen-containing polymer may be the polyalkyleneimine-based polymer described above as an example of the nitrogen-containing raw material polymer. The polyalkyleneimine-based polymer described above can function as a dispersant for improving the dispersibility of ferromagnetic powder. The fluorine-based nitrogen-containing polymer can also function as a dispersant for improving the dispersibility of ferromagnetic powder. When another nitrogen-containing polymer is included, the content of the other nitrogen-containing polymer in the magnetic layer or magnetic layer-forming composition can be, for example, 0.1 to 20.0 parts by mass, or 1.0 to 15.0 parts by mass, per 100 parts by mass of the ferromagnetic powder. For the nonmagnetic layer and the nonmagnetic layer-forming composition, the above description can be applied by replacing the ferromagnetic powder with the nonmagnetic powder.
[0072] The magnetic layer of the magnetic recording medium will now be described in more detail. <Magnetic layer> (Ferromagnetic powder) The magnetic layer contains ferromagnetic powder. As the ferromagnetic powder contained in the magnetic layer, one or more of known ferromagnetic powders used in the magnetic layers of various magnetic recording media can be used in combination. It is preferable to use ferromagnetic powders with a small average particle size from the viewpoint of improving recording density. From this viewpoint, the average particle size of the ferromagnetic powder is preferably 50 nm or less, more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, and even more preferably 20 nm or less. On the other hand, from the viewpoint of magnetization stability, the average particle size of the ferromagnetic powder is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.
[0073] Hexagonal Ferrite Powder A preferred specific example of the ferromagnetic powder is hexagonal ferrite powder. For details of the hexagonal ferrite powder, see, for example, JP2011-225417A, paragraphs 0012-0030, JP2011-216149A, paragraphs 0134-0136, JP2012-204726A, paragraphs 0013-0030, and JP2015-127985A, paragraphs 0029-0084.
[0074] In the present invention and this specification, the term "hexagonal ferrite powder" refers to a ferromagnetic powder in which the crystal structure of hexagonal ferrite is detected as the main phase by X-ray diffraction analysis. The main phase refers to the structure to which the diffraction peak with the highest intensity is assigned in the X-ray diffraction spectrum obtained by X-ray diffraction analysis. For example, when the diffraction peak with the highest intensity in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to the crystal structure of hexagonal ferrite, it is determined that the crystal structure of hexagonal ferrite is detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is regarded as the main phase. The crystal structure of hexagonal ferrite contains at least an iron atom, a divalent metal atom, and an oxygen atom as constituent atoms. The divalent metal atom is a metal atom that can become a divalent cation as an ion, and examples of the divalent metal atom include an alkaline earth metal atom such as a strontium atom, a barium atom, and a calcium atom, and a lead atom. In the present invention and this specification, the hexagonal strontium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a strontium atom, and the hexagonal barium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a barium atom. The main divalent metal atom refers to the divalent metal atom that is the most abundant of the divalent metal atoms contained in the powder on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms. In the present invention and this specification, the "rare earth atom" is selected from the group consisting of scandium atoms (Sc), yttrium atoms (Y), and lanthanoid atoms. The lanthanide atom is selected from the group consisting of a lanthanum atom (La), a cerium atom (Ce), a praseodymium atom (Pr), a neodymium atom (Nd), a promethium atom (Pm), a samarium atom (Sm), a europium atom (Eu), a gadolinium atom (Gd), a terbium atom (Tb), a dysprosium atom (Dy), a holmium atom (Ho), an erbium atom (Er), a thulium atom (Tm), a ytterbium atom (Yb), and a lutetium atom (Lu).
[0075] Hereinafter, hexagonal strontium ferrite powder, which is one form of hexagonal ferrite powder, will be described in more detail.
[0076] The activation volume of the hexagonal strontium ferrite powder is preferably 800 to 1500 nm 3 The finely divided hexagonal strontium ferrite powder exhibiting an activation volume in the above range is suitable for producing a magnetic recording medium exhibiting excellent electromagnetic conversion characteristics. The activation volume of the hexagonal strontium ferrite powder is preferably 800 nm 3 For example, 850 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the hexagonal strontium ferrite powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:
[0077] "Activation volume" is a unit of magnetization reversal and is an index showing the magnetic size of a particle. The activation volume and the anisotropy constant Ku described in the present invention and this specification are values obtained by measuring the coercive force Hc measurement section at magnetic field sweep speeds of 3 minutes and 30 minutes (measurement temperature: 23°C ± 1°C) using a vibrating sample magnetometer, and calculating from the following relationship between Hc and activation volume V. The unit of the anisotropy constant Ku is 1 erg / cc = 1.0 x 10 -1 J / m 3 It is. Hc=2Ku / Ms{1-[(kT / KuV)ln(At / 0.693)] 1 / 2} [In the above formula, Ku: anisotropy constant (unit: J / m 3 ), Ms: saturation magnetization (unit: kA / m), k: Boltzmann constant, T: absolute temperature (unit: K), V: activation volume (unit: cm 3 ), A: spin precession frequency (unit: s -1 ), t: magnetic field reversal time (unit: s)]
[0078] The anisotropy constant Ku can be used as an index of reduction in thermal fluctuation, in other words, improvement in thermal stability. The hexagonal strontium ferrite powder is preferably 1.8×10 5 J / m 3 More preferably, the Ku is 2.0×10 or more. 5 J / m 3 The Ku of the hexagonal strontium ferrite powder can be, for example, 2.5×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is therefore preferable, the Ku value is not limited to the above-mentioned values.
[0079] The hexagonal strontium ferrite powder may or may not contain rare earth atoms. When the hexagonal strontium ferrite powder contains rare earth atoms, it is preferable that the rare earth atoms are contained at a content (bulk content) of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the hexagonal strontium ferrite powder containing rare earth atoms can have uneven distribution of rare earth atoms in the surface layer portion. In the present invention and this specification, the term "surface distribution of rare earth atoms" refers to the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by partially dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "surface content of rare earth atoms" or simply "surface content" for rare earth atoms), which is greater than the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by completely dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "bulk content of rare earth atoms" or simply "bulk content" for rare earth atoms), Rare earth atom surface content / rare earth atom bulk content>1.0 The rare earth atom content of the hexagonal strontium ferrite powder described later is synonymous with the rare earth atom bulk content. In contrast, partial dissolution using an acid dissolves the surface layer of the particles constituting the hexagonal strontium ferrite powder, so the rare earth atom content in the solution obtained by partial dissolution is the rare earth atom content in the surface layer of the particles constituting the hexagonal strontium ferrite powder. The rare earth atom surface layer content satisfying the ratio of "rare earth atom surface layer content / rare earth atom bulk content>1.0" means that the rare earth atoms are unevenly distributed (i.e., more present in the surface layer) in the particles constituting the hexagonal strontium ferrite powder. In the present invention and this specification, the surface layer refers to a portion of the region extending from the surface of the particles constituting the hexagonal strontium ferrite powder toward the inside.
[0080] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atom content (bulk content) is preferably in the range of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. It is considered that the rare earth atoms contained in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder contribute to suppressing the decrease in the reproduction output during repeated reproduction. This is presumed to be because the hexagonal strontium ferrite powder contains rare earth atoms in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder can increase the anisotropy constant Ku. The higher the value of the anisotropy constant Ku, the more the occurrence of a phenomenon called thermal fluctuation can be suppressed (in other words, the thermal stability can be improved). By suppressing the occurrence of thermal fluctuation, the decrease in the reproduction output during repeated reproduction can be suppressed. It is speculated that the uneven distribution of rare earth atoms in the surface layer of hexagonal strontium ferrite powder particles contributes to stabilizing the spin of the iron (Fe) sites in the crystal lattice of the surface layer, thereby increasing the anisotropy constant Ku. In addition, it is presumed that using the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface as the ferromagnetic powder of the magnetic layer also contributes to suppressing the wear of the magnetic layer surface due to sliding with the magnetic head. That is, it is presumed that the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface can also contribute to improving the running durability of the magnetic recording medium. This is presumed to be because the uneven distribution of rare earth atoms on the surface of the particles constituting the hexagonal strontium ferrite powder contributes to improving the interaction between the particle surface and the organic substance (e.g., binder and / or additive) contained in the magnetic layer, and as a result, the strength of the magnetic layer is improved. From the viewpoint of further suppressing the decrease in regeneration output during repeated regeneration and / or further improving running durability, the rare earth atom content (bulk content) is more preferably in the range of 0.5 to 4.5 atomic %, even more preferably in the range of 1.0 to 4.5 atomic %, and even more preferably in the range of 1.5 to 4.5 atomic %.
[0081] The bulk content is the content obtained by completely dissolving the hexagonal strontium ferrite powder. In the present invention and this specification, unless otherwise specified, the content of an atom refers to the bulk content obtained by completely dissolving the hexagonal strontium ferrite powder. The hexagonal strontium ferrite powder containing rare earth atoms may contain only one rare earth atom as a rare earth atom, or may contain two or more rare earth atoms. The bulk content when containing two or more rare earth atoms is obtained for the total of two or more rare earth atoms. This point is the same for other components in the present invention and this specification. That is, unless otherwise specified, a certain component may be used only one type, or two or more types may be used. When two or more types are used, the content or content refers to the total of two or more types.
[0082] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atoms contained therein may be any one or more of rare earth atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, preferred rare earth atoms include neodymium atoms, samarium atoms, yttrium atoms and dysprosium atoms, more preferred are neodymium atoms, samarium atoms and yttrium atoms, and even more preferred are neodymium atoms.
[0083] In the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the rare earth atoms may be unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the degree of uneven distribution is not limited. For example, for the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the ratio of the surface content of rare earth atoms obtained by partial dissolution under the dissolution conditions described below to the bulk content of rare earth atoms obtained by complete dissolution under the dissolution conditions described below, "surface content / bulk content", is more than 1.0 and can be 1.5 or more. The "surface content / bulk content" being greater than 1.0 means that the rare earth atoms are unevenly distributed in the surface layer (i.e., more than in the interior) in the particles constituting the hexagonal strontium ferrite powder. In addition, the ratio of the surface layer content of rare earth atoms obtained by partial dissolution under the dissolution conditions described later to the bulk content of rare earth atoms obtained by total dissolution under the dissolution conditions described later, "surface layer content / bulk content", can be, for example, 10.0 or less, 9.0 or less, 8.0 or less, 7.0 or less, 6.0 or less, 5.0 or less, or 4.0 or less. However, in a hexagonal strontium ferrite powder having rare earth atom surface layer uneven distribution, it is sufficient that the rare earth atoms are unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the above "surface layer content / bulk content" is not limited to the upper or lower limit exemplified.
[0084] The partial and total dissolution of hexagonal strontium ferrite powder will be described below. For hexagonal strontium ferrite powder present as powder, the sample powders to be partially and completely dissolved are taken from the same lot of powder. On the other hand, for hexagonal strontium ferrite powder contained in the magnetic layer of a magnetic recording medium, a part of the hexagonal strontium ferrite powder taken out of the magnetic layer is subjected to partial dissolution, and the other part is subjected to total dissolution. The hexagonal strontium ferrite powder can be taken out of the magnetic layer by, for example, the method described in paragraph 0032 of JP 2015-91747 A. The above-mentioned partial dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder can be visually confirmed in the liquid at the end of dissolution. For example, the partial dissolution can dissolve a region of 10 to 20 mass% of the particles constituting the hexagonal strontium ferrite powder, with the whole particles being 100 mass%. On the other hand, the above-mentioned complete dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder cannot be visually confirmed in the liquid at the end of dissolution. The partial dissolution and the surface layer content are measured, for example, by the following method. Note that the dissolution conditions such as the amount of sample powder are merely examples, and any dissolution conditions that allow partial or complete dissolution can be used. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 1 mol / L hydrochloric acid is placed on a hot plate set at 70°C for 1 hour. The resulting solution is filtered through a 0.1 μm membrane filter. Elemental analysis of the filtrate thus obtained is performed using an inductively coupled plasma (ICP) analyzer. In this way, the surface layer content of rare earth atoms relative to 100 atomic % of iron atoms can be determined. When multiple types of rare earth atoms are detected by elemental analysis, the total content of all rare earth atoms is taken as the surface layer content. This is also true for the measurement of bulk content. On the other hand, the total dissolved and bulk contents are measured, for example, by the following method. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 4 mol / L hydrochloric acid is placed on a hot plate set at 80° C. for 3 hours. After that, the bulk content relative to 100 atomic % of iron atoms can be calculated by carrying out the same procedure as the partial dissolution and surface layer content measurement described above.
[0085] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic recording medium, it is desirable for the mass magnetization σs of the ferromagnetic powder contained in the magnetic recording medium to be high. In this regard, hexagonal strontium ferrite powder containing rare earth atoms but not having uneven distribution of rare earth atoms in the surface layer has a tendency to have a significantly lower σs than hexagonal strontium ferrite powder not containing rare earth atoms. In contrast, hexagonal strontium ferrite powder having uneven distribution of rare earth atoms in the surface layer is considered to be preferable in terms of suppressing such a large decrease in σs. In one embodiment, the σs of the hexagonal strontium ferrite powder is 45 A·m 2 / kg or more, and 47A·m 2 / kg or more. On the other hand, from the viewpoint of noise reduction, σs is 80A·m 2 / kg or less, and 60A·m 2 / kg or less is more preferable. σs can be measured using a known measuring device capable of measuring magnetic properties, such as a vibrating sample magnetometer. In the present invention and this specification, unless otherwise specified, the mass magnetization σs is a value measured at a magnetic field strength of 1194 kA / m (15 kOe).
[0086] Regarding the content (bulk content) of the constituent atoms of the hexagonal strontium ferrite powder, the strontium atom content can be, for example, in the range of 2.0 to 15.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the divalent metal atoms contained in the hexagonal strontium ferrite powder can be only strontium atoms. In another embodiment, the hexagonal strontium ferrite powder can also contain one or more other divalent metal atoms in addition to strontium atoms. For example, it can contain barium atoms and / or calcium atoms. When divalent metal atoms other than strontium atoms are contained, the barium atom content and calcium atom content in the hexagonal strontium ferrite powder can each be, for example, in the range of 0.05 to 5.0 atomic % relative to 100 atomic % of iron atoms.
[0087] Known crystal structures of hexagonal ferrite include magnetoplumbite type (also called "M type"), W type, Y type, and Z type. The hexagonal strontium ferrite powder may have any of the crystal structures. The crystal structure can be confirmed by X-ray diffraction analysis. The hexagonal strontium ferrite powder may be one in which a single crystal structure or two or more types of crystal structures are detected by X-ray diffraction analysis. For example, in one embodiment, the hexagonal strontium ferrite powder may be one in which only the M-type crystal structure is detected by X-ray diffraction analysis. For example, M-type hexagonal ferrite is AFe 12 O 19Here, A represents a divalent metal atom, and when the hexagonal strontium ferrite powder is of the M type, A is only a strontium atom (Sr), or when A contains a plurality of divalent metal atoms, the strontium atom (Sr) accounts for the largest proportion on an atomic % basis as described above. The divalent metal atom content of the hexagonal strontium ferrite powder is usually determined by the type of crystal structure of the hexagonal ferrite, and is not particularly limited. The same applies to the iron atom content and the oxygen atom content. The hexagonal strontium ferrite powder contains at least an iron atom, a strontium atom, and an oxygen atom, and may further contain a rare earth atom. Furthermore, the hexagonal strontium ferrite powder may or may not contain atoms other than these atoms. As an example, the hexagonal strontium ferrite powder may contain an aluminum atom (Al). The content of aluminum atoms can be, for example, 0.5 to 10.0 atomic % relative to 100 atomic % of iron atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, the hexagonal strontium ferrite powder contains iron atoms, strontium atoms, oxygen atoms, and rare earth atoms, and the content of atoms other than these atoms is preferably 10.0 atomic % or less, more preferably in the range of 0 to 5.0 atomic %, relative to 100 atomic % of iron atoms, and may be 0 atomic %. That is, in one embodiment, the hexagonal strontium ferrite powder may not contain atoms other than iron atoms, strontium atoms, oxygen atoms, and rare earth atoms. The content expressed in atomic % above is obtained by converting the content (unit: mass %) of each atom obtained by completely dissolving the hexagonal strontium ferrite powder into a value expressed in atomic % using the atomic weight of each atom. In addition, in the present invention and this specification, "not containing" a certain atom means that the content measured by an ICP analyzer after completely dissolving is 0 mass %. The detection limit of an ICP analyzer is usually 0.01 ppm (parts per million) or less on a mass basis. The above term "free" is used to mean that the content is below the detection limit of the ICP analyzer.In one form, the hexagonal strontium ferrite powder can be one that does not contain bismuth atoms (Bi).
[0088] metal powder A specific preferred example of the ferromagnetic powder is a ferromagnetic metal powder. For details of the ferromagnetic metal powder, reference can be made to, for example, paragraphs 0137 to 0141 of JP 2011-216149 A and paragraphs 0009 to 0023 of JP 2005-251351 A.
[0089] ε-iron oxide powder A preferred specific example of the ferromagnetic powder is ε-iron oxide powder. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which the ε-iron oxide crystal structure is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to the ε-iron oxide crystal structure, it is determined that the ε-iron oxide crystal structure is detected as the main phase. Known methods for producing ε-iron oxide powder include a method of producing it from goethite and a reverse micelle method. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a part of Fe is replaced by a substitution atom such as Ga, Co, Ti, Al, or Rh, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp.5200-5206, etc. However, the method for producing the ε-iron oxide powder that can be used as the ferromagnetic powder in the magnetic layer of the magnetic recording medium is not limited to the method given here.
[0090] The activation volume of the ε-iron oxide powder is preferably 300 to 1500 nm 3 The finely divided ε-iron oxide powder exhibiting an activation volume in the above range is suitable for producing a magnetic recording medium exhibiting excellent electromagnetic conversion characteristics. The activation volume of the ε-iron oxide powder is preferably 300 nm 3For example, 500 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the ε-iron oxide powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:
[0091] The anisotropy constant Ku can be used as an index of the reduction in thermal fluctuation, in other words, the improvement in thermal stability. The ε-iron oxide powder is preferably 3.0×10 4 J / m 3 More preferably, the Ku is 8.0×10 or more. 4 J / m 3 The Ku of the ε-iron oxide powder can be, for example, 3.0×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.
[0092] From the viewpoint of increasing the reproduction output when reproducing data recorded on the magnetic recording medium, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic recording medium is high. In this regard, in one embodiment, the σs of the ε-iron oxide powder is 8 A m 2 / kg or more, and 12 A m 2 On the other hand, the σs of ε-iron oxide powder is 40 A m 2 / kg or less, and 35A·m 2 It is more preferable that the amount is not more than 1 / kg.
[0093] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as ferromagnetic powders is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and a photograph of the particles that make up the powder is obtained by printing it on photographic paper or displaying it on a display so that the total magnification is 500,000 times. From the obtained particle photograph, the target particle is selected, and the particle outline is traced with a digitizer to measure the particle (primary particle) size. Primary particles are independent particles that are not aggregated. The above measurements are carried out for 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software, unless otherwise specified. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact with each other, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.
[0094] As a method for collecting a sample powder from a magnetic recording medium for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.
[0095] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or unspecified shape, and the major axis of the particle cannot be specified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.
[0096] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).
[0097] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass % relative to the total mass of the magnetic layer, and more preferably in the range of 60 to 90 mass %. The magnetic layer contains ferromagnetic powder, may contain a binder, and may optionally contain one or more further additives. A high filling rate of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.
[0098] (Binding agent, hardener) The magnetic recording medium may be a coating type magnetic recording medium, and the magnetic layer may contain a binder. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coating type magnetic recording media may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination of a plurality of resins. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the non-magnetic layer and / or backcoat layer described later. For the above binders, refer to paragraphs 0028 to 0031 of JP-A-2010-24113. The content of the binder in the magnetic layer can be, for example, 1.0 to 30.0 parts by mass relative to 100.0 parts by mass of the ferromagnetic powder. The average molecular weight of the resin used as the binder can be, for example, 10,000 or more and 200,000 or less in weight average molecular weight. Unless otherwise specified, the weight average molecular weight in the present invention and this specification is a value obtained by converting a value measured by gel permeation chromatography (GPC) under the following measurement conditions into a standard polystyrene equivalent. The binder can be used in an amount of, for example, 1.0 to 30.0 parts by mass relative to 100.0 parts by mass of the ferromagnetic powder. GPC equipment: HLC-8120 (Tosoh Corporation) Column: TSK gel Multipore HXL-M (Tosoh Corporation, 7.8 mm ID (inner diameter) × 30.0 cm) Eluent: tetrahydrofuran (THF)
[0099] A curing agent can also be used together with the resin usable as a binder. In one embodiment, the curing agent can be a thermosetting compound that undergoes a curing reaction (crosslinking reaction) by heating, and in another embodiment, a photocuring compound that undergoes a curing reaction (crosslinking reaction) by irradiation with light. The curing agent can be included in the magnetic layer in a state where at least a part of the curing agent reacts (crosslinks) with other components such as the binder as the curing reaction proceeds during the magnetic layer forming process. This point is also true for layers formed using a composition used to form other layers that contains a curing agent. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details about polyisocyanate, refer to paragraphs 0124 to 0125 of JP 2011-216149 A. The content of the curing agent in the magnetic layer forming composition can be, for example, 0 to 80.0 parts by mass relative to 100.0 parts by mass of the binder, and can be 50.0 to 80.0 parts by mass from the viewpoint of improving the strength of the magnetic layer.
[0100] (Additives) The magnetic layer may contain one or more additives as necessary. An example of the additive is the curing agent. Examples of the additives contained in the magnetic layer include non-magnetic powder, lubricant, dispersant, dispersion aid, antifungal agent, antistatic agent, antioxidant, and the like. For the dispersant, refer to paragraphs 0061 and 0071 of JP-A-2012-133837. The dispersant may be added to the non-magnetic layer forming composition. For the dispersant that can be added to the non-magnetic layer forming composition, refer to paragraph 0061 of JP-A-2012-133837. Examples of the non-magnetic powder that can be contained in the magnetic layer include non-magnetic powder that can function as an abrasive, non-magnetic powder that can function as a protrusion forming agent that forms protrusions that protrude appropriately on the magnetic layer surface, and the like. Examples of the abrasive include powders of alumina (Al2O3), silicon carbide, boron carbide (B4C), TiC, chromium oxide (Cr2O3), cerium oxide, zirconium oxide (ZrO2), iron oxide, diamond, etc., which are materials usually used as abrasives for magnetic layers, and among these, powders of alumina such as α-alumina, silicon carbide, and diamond are preferred. The content of the abrasive in the magnetic layer is preferably 1.0 to 20.0 parts by mass, more preferably 3.0 to 15.0 parts by mass, and even more preferably 4.0 to 10.0 parts by mass, relative to 100.0 parts by mass of ferromagnetic powder. The average particle size of the abrasive is, for example, in the range of 30 to 300 nm, and preferably in the range of 50 to 200 nm. Examples of the protrusion-forming agent include carbon black and colloidal particles. The content of the protrusion-forming agent in the magnetic layer is preferably 0.1 to 10.0 parts by mass, more preferably 0.1 to 5.0 parts by mass, and even more preferably 0.5 to 5.0 parts by mass, relative to 100.0 parts by mass of the ferromagnetic powder. The average particle size of the colloidal particles is preferably in the range of, for example, 90 to 200 nm, and more preferably in the range of 100 to 150 nm. The average particle size of the carbon black is preferably in the range of 5 to 200 nm, and more preferably in the range of 10 to 150 nm.
[0101] The magnetic recording medium may contain at least one fatty acid compound selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides in the magnetic layer on the non-magnetic support. The fatty acid compound may function as a lubricant. The magnetic layer may contain only one, two, or three fatty acid compounds selected from fatty acids, fatty acid esters, and fatty acid amides. The fatty acid may contain only one or two or more fatty acids. This also applies to fatty acid esters and fatty acid amides. Examples of fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc., with stearic acid, myristic acid, palmitic acid, etc. being preferred, and stearic acid being more preferred. The fatty acid may be contained in the magnetic layer in the form of a salt such as a metal salt. Examples of fatty acid esters include esters of the various fatty acids exemplified above, etc. Specific examples include butyl myristate, butyl palmitate, butyl stearate (butyl stearate), neopentyl glycol dioleate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, oleyl oleate, isocetyl stearate, isotridecyl stearate, octyl stearate, isooctyl stearate, amyl stearate, butoxyethyl stearate, etc. Examples of the fatty acid amide include amides of the various fatty acids exemplified above, such as lauric acid amide, myristic acid amide, palmitic acid amide, and stearic acid amide. As for fatty acids and fatty acid derivatives (amides, esters, etc.), it is preferable that the fatty acid-derived portion of the fatty acid derivative has the same or similar structure as the fatty acid used in combination. For example, when stearic acid is used as the fatty acid, it is preferable to use stearic acid amide and / or stearic acid ester in combination. In one embodiment, a magnetic recording medium containing one or more fatty acid compounds selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides in the magnetic layer side can be manufactured by forming a magnetic layer using a magnetic layer forming composition containing one or more of the fatty acid compounds. In another embodiment, a magnetic recording medium containing one or more of the fatty acid compounds in the magnetic layer side can be manufactured by forming a nonmagnetic layer using a nonmagnetic layer forming composition containing one or more of the fatty acid compounds. In another embodiment, a magnetic recording medium containing one or more of the fatty acid compounds in the magnetic layer side can be manufactured by forming a nonmagnetic layer using a nonmagnetic layer forming composition containing one or more of the fatty acid compounds and forming a magnetic layer using a magnetic layer forming composition containing one or more of the fatty acid compounds. The nonmagnetic layer can play a role of retaining components that can function as lubricants such as fatty acids, fatty acid esters, and fatty acid amides and supplying them to the magnetic layer. Lubricants such as fatty acids, fatty acid esters, and fatty acid amides contained in the nonmagnetic layer can migrate to the magnetic layer and exist in the magnetic layer. The content of fatty acid in the magnetic layer or in the composition for forming the magnetic layer is preferably 0.5 to 3.0 parts by mass per 100.0 parts by mass of ferromagnetic powder. The content of the fatty acid ester in the magnetic layer or in the composition for forming the magnetic layer is, for example, 0 to 10.0 parts by mass, and preferably 0.5 to 7.0 parts by mass, per 100.0 parts by mass of the ferromagnetic powder. The content of the fatty acid amide in the magnetic layer or in the composition for forming the magnetic layer is, for example, 0 to 1.0 part by mass, and preferably 0.1 to 1.0 part by mass, per 100.0 parts by mass of the ferromagnetic powder. Regarding the contents of fatty acids, fatty acid esters and fatty acid amides in the nonmagnetic layer or the composition for forming the nonmagnetic layer, the above description can be applied by replacing the ferromagnetic powder with the nonmagnetic powder. Regarding the mixing ratio of the fluorine-based nitrogen-containing polymer and the fatty acid compound in the magnetic layer or the composition for forming the magnetic layer, the ratio of the fatty acid compound can be 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more, and can be 90% by mass or less, 80% by mass or less, 70% by mass or less, 60% by mass or less, or 50% by mass or less, where the total amount (mass basis) of the fluorine-containing raw material polymer and the fatty acid compound is taken as 100% by mass. The above points also apply to the mixing ratio of the fluorine-based nitrogen-containing polymer and the fatty acid compound in the nonmagnetic layer or the composition for forming the nonmagnetic layer.
[0102] The magnetic layer described above can be provided directly on the surface of the non-magnetic support, or indirectly via a non-magnetic layer.
[0103] <Nonmagnetic layer> Next, the non-magnetic layer will be described. The magnetic recording medium may have a magnetic layer directly on the surface of the non-magnetic support, or may have a magnetic layer on the surface of the non-magnetic support via a non-magnetic layer containing non-magnetic powder. The non-magnetic powder used in the non-magnetic layer may be an inorganic powder or an organic powder. Carbon black or the like can also be used. Examples of inorganic powders include powders of metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, metal sulfides, and the like. These non-magnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black usable in the non-magnetic layer, refer to paragraphs 0040 to 0041 of JP-A-2010-24113. The content (filling rate) of the non-magnetic powder in the non-magnetic layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass.
[0104] The non-magnetic layer may be a layer containing a non-magnetic powder and a binder, and may further contain one or more additives. For other details of the binder, additives, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additives, known techniques related to magnetic layers can also be applied.
[0105] In the present invention and this specification, the nonmagnetic layer also includes a substantially nonmagnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, along with a nonmagnetic powder. A substantially nonmagnetic layer here refers to a layer whose residual magnetic flux density is 10 mT or less, whose coercive force is 100 Oe or less, or whose residual magnetic flux density is 10 mT or less and whose coercive force is 100 Oe or less. 1 [kOe] = 10 6 / 4π[A / m]. It is preferable that the nonmagnetic layer has no residual magnetic flux density and no coercive force.
[0106] <Nonmagnetic support> Next, the non-magnetic support (hereinafter, simply referred to as "support") will be described. Examples of the non-magnetic support include known biaxially stretched polyethylene terephthalate, polyethylene naphthalate, polyamide, polyamideimide, aromatic polyamide, and the like. Among these, polyethylene terephthalate, polyethylene naphthalate, and polyamide are preferred. These supports may be previously subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, and the like.
[0107] <Backcoat layer> The magnetic recording medium may also have a backcoat layer containing a nonmagnetic powder on the surface side opposite to the surface side having the magnetic layer of the nonmagnetic support. The backcoat layer preferably contains either or both of carbon black and inorganic powder. The backcoat layer may be a layer containing a nonmagnetic powder and a binder, and may further contain one or more additives. For the binder of the backcoat layer and various additives that may be optionally contained therein, known techniques related to the backcoat layer may be applied, and known techniques related to the formulation of the magnetic layer and / or the nonmagnetic layer may also be applied. For example, the descriptions in paragraphs 0018-0020 of JP 2006-331625 A and in column 4, line 65 to column 5, line 38 of the specification of U.S. Pat. No. 7,029,774 may be referred to for the backcoat layer.
[0108] <Various thicknesses> The thickness of the nonmagnetic support is, for example, 3.0 to 80.0 μm, preferably 3.0 to 20.0 μm, more preferably 3.0 to 10.0 μm, and even more preferably 3.0 to 6.0 μm.
[0109] The thickness of the magnetic layer can be optimized according to the saturation magnetization amount of the magnetic head used, the head gap length, the band of the recording signal, etc. From the viewpoint of high density recording, the thickness of the magnetic layer is preferably 10 nm to 150 nm, more preferably 20 nm to 120 nm, and even more preferably 30 nm to 100 nm. There should be at least one magnetic layer, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers.
[0110] The thickness of the nonmagnetic layer is, for example, 0.1 to 3.0 μm, preferably 0.1 to 2.0 μm, and more preferably 0.1 to 1.5 μm.
[0111] The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably in the range of 0.1 to 0.7 μm.
[0112] The thickness of each layer of the magnetic recording medium and the non-magnetic support can be determined by a known film thickness measurement method. For example, the cross section of the magnetic recording medium in the thickness direction is exposed by a known method such as ion beam or microtome, and then the exposed cross section is observed by a scanning electron microscope. Various thicknesses can be determined as the thickness determined at any one point in the cross section observation, or the arithmetic average of the thicknesses determined at two or more randomly selected points, for example, two points. Alternatively, the thickness of each layer may be determined as a design thickness calculated from the manufacturing conditions.
[0113] <Method of manufacturing magnetic recording medium> The process of preparing the composition for forming the magnetic layer, and the optional non-magnetic layer and backcoat layer can usually include at least a kneading process, a dispersion process, and a mixing process provided before or after these processes as necessary. Each of the individual processes may be divided into two or more stages. The components used in the preparation of each layer-forming composition may be added at the beginning or during any process. Also, each raw material may be added in two or more steps in a divided manner. As described above, a fluorine-containing nitrogen-containing polymer can be formed by using one or more nitrogen-containing raw material polymers and one or more fluorine-containing compounds as components of the magnetic layer-forming composition and mixing them in the preparation process of the magnetic layer-forming composition. In one embodiment, before the preparation of the magnetic layer-forming composition, one or more nitrogen-containing raw material polymers and one or more fluorine-containing compounds are mixed to form a fluorine-containing nitrogen-containing polymer, and then the polymer can be used as a component of the magnetic layer-forming composition to prepare the magnetic layer-forming composition. This point also applies to the preparation process of the non-magnetic layer-forming composition. In order to prepare each layer-forming composition, a known technique can be used. In the kneading step, it is preferable to use a kneader having a strong kneading force, such as an open kneader, a continuous kneader, a pressure kneader, or an extruder. Details of these kneading processes are described in JP-A-1-106338 and JP-A-1-79274. In addition, in order to disperse each layer-forming composition, one or more types of dispersion beads selected from the group consisting of glass beads and other dispersion beads can be used as a dispersion medium. As such dispersion beads, zirconia beads, titania beads, and steel beads, which are dispersion beads with high specific gravity, are suitable. The particle size (bead diameter) and packing rate of these dispersion beads can be optimized for use. A known dispersing machine can be used. Each layer-forming composition may be filtered by a known method before being subjected to the coating step. Filtration can be performed, for example, by filter filtration. As the filter used for filtration, for example, a filter with a pore size of 0.01 to 3 μm (for example, a glass fiber filter, a polypropylene filter, etc.) can be used.
[0114] The magnetic layer can be formed by applying the magnetic layer-forming composition directly onto the surface of the non-magnetic support, or by applying the magnetic layer-forming composition successively or simultaneously in a multilayer manner with the non-magnetic layer-forming composition. The backcoat layer can be formed by applying the backcoat layer-forming composition onto the surface of the non-magnetic support opposite to the surface on which the magnetic layer is provided (or will be provided later).
[0115] After the coating step, various treatments such as drying, orientation of the magnetic layer, and surface smoothing (calendering) can be performed. For the coating step and various treatments, known techniques can be applied, and for example, refer to paragraphs 0051 to 0057 of JP-A-2010-24113. For example, vertical orientation can be performed as the orientation. The vertical orientation can be performed by known methods such as a method using magnets with opposite poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the transport speed of the magnetic recording medium in the orientation zone. In addition, the coating layer may be pre-dried before being transported to the orientation zone.
[0116] In the magnetic recording medium manufactured as described above, a servo pattern can be formed by a known method in order to enable tracking control of a magnetic head in a magnetic recording and reproducing device, control of the running speed of the magnetic recording medium, and the like. "Formation of a servo pattern" can also be called "recording of a servo signal." The magnetic recording medium may be a tape-shaped magnetic recording medium (magnetic tape) or a disk-shaped magnetic recording medium (magnetic disk). The formation of a servo pattern will be described below using a magnetic tape as an example.
[0117] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Control methods that use servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.
[0118] As shown in ECMA (European Computer Manufacturers Association)-319, magnetic tapes (generally called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard employ a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. As described above, the reason why the servo pattern is formed by a pair of non-parallel magnetic stripes is to inform the servo signal reading element passing over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this purpose, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.
[0119] A servo band is made up of a series of servo signals along the length of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is called a data band. A data band is made up of multiple data tracks, and each data track corresponds to one servo track.
[0120] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.
[0121] As a method for uniquely identifying servo bands, there is also a method using the staggered method as specified in ECMA-319. In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. Since the combination of the shift between adjacent servo bands is unique across the entire magnetic tape, it is possible to uniquely identify the servo bands when reading the servo pattern with two servo signal reading elements.
[0122] Also, as specified in ECMA-319, information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.
[0123] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.
[0124] The head for forming a servo pattern is called a servo write head. The servo write head has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.
[0125] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.
[0126] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This makes it possible to increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.
[0127] [Magnetic tape cartridge] One aspect of the present invention relates to a magnetic tape cartridge including the above-mentioned magnetic recording medium in tape form (that is, a magnetic tape).
[0128] The details of the magnetic tape contained in the magnetic tape cartridge are as described above.
[0129] In a magnetic tape cartridge, the magnetic tape is generally accommodated inside the cartridge body in a state where it is wound around a reel. The reel is provided rotatably inside the cartridge body. As the magnetic tape cartridge, a single-reel type magnetic tape cartridge having one reel inside the cartridge body and a twin-reel type magnetic tape cartridge having two reels inside the cartridge body are widely used. When a single-reel type magnetic tape cartridge is loaded into a magnetic recording and reproducing device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound around the reel on the magnetic recording and reproducing device side. A magnetic head is disposed on the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape is fed and wound between the reel (supply reel) on the magnetic tape cartridge side and the reel (take-up reel) on the magnetic recording and reproducing device side. During this time, the magnetic head comes into contact with and slides on the surface of the magnetic layer side of the magnetic tape, thereby recording and / or reproducing data. In contrast, a dual-reel magnetic tape cartridge has both a supply reel and a take-up reel inside the magnetic tape cartridge. The magnetic tape cartridge may be either a single-reel or dual-reel magnetic tape cartridge. The magnetic tape cartridge may include the magnetic tape according to one aspect of the present invention, and other aspects may be based on known techniques.
[0130] [Magnetic recording and playback device] One aspect of the present invention relates to a magnetic recording and reproducing device including the above magnetic recording medium.
[0131] In the present invention and this specification, the term "magnetic recording and reproducing device" refers to a device capable of at least one of recording data to a magnetic recording medium and reproducing data recorded on the magnetic recording medium. Such a device is generally called a drive. The magnetic recording and reproducing device may be, for example, a sliding type magnetic recording and reproducing device. The sliding type magnetic recording and reproducing device refers to a device in which the surface of the magnetic layer and a magnetic head come into contact and slide when recording data on the magnetic recording medium and / or reproducing the recorded data. For example, the magnetic recording and reproducing device may include the magnetic tape cartridge in a removable manner.
[0132] The magnetic recording and reproducing device may include a magnetic head. The magnetic head may be a recording head capable of recording data on a magnetic recording medium, or may be a reproducing head capable of reproducing data recorded on the magnetic recording medium. In one embodiment, the magnetic recording and reproducing device may include both a recording head and a reproducing head as separate magnetic heads. In another embodiment, the magnetic head included in the magnetic recording and reproducing device may have a configuration in which both an element for recording data (recording element) and an element for reproducing data (reproducing element) are provided in one magnetic head. Hereinafter, the element for recording data and the element for reproducing data are collectively referred to as "data element". As the reproducing head, a magnetic head (MR head) including a magnetoresistive (MR) element capable of reading data recorded on a magnetic recording medium with good sensitivity as a reproducing element is preferable. As the MR head, various known MR heads such as an anisotropic magnetoresistive (AMR) head, a giant magnetoresistive (GMR) head, and a tunnel magnetoresistive (TMR) head may be used. Also, the magnetic head that records and / or reproduces data may include a servo signal read element. Alternatively, the magnetic recording and reproducing device may include a magnetic head (servo head) equipped with a servo signal read element as a head separate from the magnetic head that records and / or reproduces data. For example, a magnetic head that records and / or reproduces recorded data (hereinafter also referred to as a "recording and reproducing head") may include two servo signal read elements, and each of the two servo signal read elements can simultaneously read two adjacent servo bands. One or more data elements may be disposed between the two servo signal read elements.
[0133] In the magnetic recording and reproducing device, the recording of data on the magnetic recording medium and / or the reproduction of data recorded on the magnetic recording medium can be performed, for example, by contacting and sliding the magnetic head against the surface of the magnetic recording medium on the magnetic layer side. The magnetic recording and reproducing device may include the magnetic recording medium according to one embodiment of the present invention, and other known techniques may be applied.
[0134] For example, when recording data and / or reproducing recorded data, tracking using servo signals is first performed. That is, the servo signal reading element is made to follow a specific servo track, so that the data element passes over the target data track. The data track is moved by changing the servo track read by the servo signal reading element in the tape width direction. The recording / reproducing head can also record and / or reproduce data on other data bands by using the UDIM information described above to move the servo signal reading element to a specific servo band and start tracking on that servo band. EXAMPLES
[0135] An embodiment of the present invention will be described below based on an example. However, the present invention is not limited to the embodiment shown in the example. The indications of "parts" and "%" below mean "parts by mass" and "% by mass" unless otherwise specified. "eq" is an equivalent, and is a unit that cannot be converted to SI units. In addition, the following various steps and operations were carried out in an environment with a temperature of 20 to 25° C. and a relative humidity of 40 to 60%, unless otherwise specified.
[0136] [Ferromagnetic powder] In the examples and comparative examples, the following hexagonal strontium ferrite was used as the ferromagnetic powder.
[0137] 1707 g of SrCO3, 687 g of H3BO3, 1120 g of Fe2O3, 45 g of Al(OH)3, 24 g of BaCO3, 13 g of CaCO3, and 235 g of Nd2O3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1390°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roller to produce an amorphous body. 280 g of the produced amorphous body was placed in an electric furnace, heated to 635°C (crystallization temperature) at a heating rate of 3.5°C / min, and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000g of zirconia beads with a particle size of 1mm and 800mL of 1% aqueous acetic acid solution were added to the glass bottle containing the crushed material, and the mixture was dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the hexagonal strontium ferrite powder obtained above is 18 nm, and the activation volume is 902 nm. 3 , the anisotropy constant Ku is 2.2×10 5 J / m 3 , mass magnetization σs is 49A m 2 / kg. A 12 mg sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was partially dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the surface layer content of neodymium atoms. Separately, 12 mg of sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was completely dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the bulk content of neodymium atoms. The neodymium atom content (bulk content) relative to 100 atomic % of iron atoms in the hexagonal strontium ferrite powder obtained above was 2.9 atomic %. The surface layer content of neodymium atoms was 8.0 atomic %. The ratio of the surface layer content to the bulk content, "surface layer content / bulk content," was 2.8, confirming that neodymium atoms were unevenly distributed in the surface layers of the particles.
[0138] It was confirmed that the powder obtained above exhibited a hexagonal ferrite crystal structure by scanning with CuKα radiation at a voltage of 45 kV and an intensity of 40 mA and measuring the X-ray diffraction pattern under the following conditions (X-ray diffraction analysis). The powder obtained above exhibited a magnetoplumbite-type (M-type) hexagonal ferrite crystal structure. The crystal phase detected by the X-ray diffraction analysis was a single phase of magnetoplumbite type. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees
[0139] [Synthesis example of polyalkyleneimine polymer] <Synthesis of polyester (i-1)> In a 500mL three-neck flask, 16.8g of n-octanoic acid (manufactured by Wako Pure Chemical Industries, Ltd.) as a carboxylic acid, 100g of ε-caprolactone (Daicel Industrial Chemical Industries, Ltd., Plaxel M) as a lactone, and 2.2g of monobutyltin oxide (manufactured by Wako Pure Chemical Industries, Ltd.) (C4H9Sn(O)OH) as a catalyst were mixed and heated at a temperature of 160°C for 1 hour. 100g of ε-caprolactone was added dropwise over 5 hours and stirred for another 2 hours. After that, the mixture was cooled to room temperature to obtain polyester (i-1). The number average molecular weight of the obtained polyester was 5,800. The number of units of the lactone repeating unit calculated from the raw material charging ratio was 15. The number of units of the lactone repeating unit corresponds to b11 in formula 1 or b21 in formula 2.
[0140] <Synthesis of polyalkyleneimine polymer A> 2.4 g of polyethyleneimine (SP-006, manufactured by Nippon Shokubai Co., Ltd., number average molecular weight 600) and 100 g of polyester (i-1) were mixed and heated at a temperature of 110° C. for 3 hours to obtain a polyalkyleneimine-based polymer. The weight average molecular weight of the obtained polyalkyleneimine-based polymer was 7,000. The obtained polyalkyleneimine-based polymer was as follows: 1 H-NMR and 13 From the results of both C-NMR analysis and elemental analysis using a combustion method, the proportion of polyalkyleneimine chains in the polyalkyleneimine polymer (polyalkyleneimine chain ratio) was calculated to be 2.3 mass%. The calculated polyalkyleneimine chain ratio was the same as the value calculated from the amounts of polyalkyleneimine and polyester charged. 1 H-NMR and 13 From the results of both C-NMR and C-NMR, it was confirmed that a polymer having the following repeating unit structure was obtained.
[0141] [ka]
[0142] The above number average molecular weight and weight average molecular weight are values measured by GPC and calculated in terms of standard polystyrene.
[0143] The conditions for measuring the average molecular weight of polyester, polyalkyleneimine (polyethyleneimine), and polyalkyleneimine-based polymer were as follows.
[0144] (Measurement conditions for number average molecular weight of polyester) Measuring instrument: HLC-8220GPC (Tosoh Corporation) Column: TSKgel Super HZ 2000 / TSKgel Super HZ 4000 / TSKgel Super HZ-H (Tosoh Corporation) Eluent: tetrahydrofuran (THF) Flow rate: 0.35mL / min Column temperature: 40℃ Detector: Refractive Index (RI) detector
[0145] (Measurement conditions for number average molecular weight of polyalkyleneimine and weight average molecular weight of polyalkyleneimine polymer) Measuring instrument: HLC-8320GPC (Tosoh Corporation) Column: 3 TSKgel Super AWM-H (Tosoh Corporation) Eluent: N-methyl-2-pyrrolidone (with 10 mM lithium bromide as an additive) Flow rate: 0.35mL / min Column temperature: 40℃ Detector: RI
[0146] [Synthesis example of fluorine-based nitrogen-containing polymer] <Synthesis of polymer 1> In a 100mL three-neck flask, 6g of the polyalkyleneimine polymer synthesized above and 20g of methyl ethyl ketone (MEK) were added and dissolved at a liquid temperature of 40°C. After cooling to room temperature, 7.94g of methyl trifluorodecaheptanoate was added and stirred at room temperature for 1 hour. The reaction liquid was dropped into 200mL of hexane and reprecipitated to obtain 5.4g of polymer 1.1 H-NMR and 19 Using F-NMR and 2,2-bis(4-hydroxyphenyl)hexafluoropropane as an internal standard, it was confirmed that a polymer having the following repeating unit structure was obtained.
[0147] [ka]
[0148] <Synthesis method of polymer 2> Polymer 2 (5.2 g) was obtained by the same procedure except that methyl trifluorodecaheptanoate was replaced with 5.85 g of methyl nonafluoropentanoate in the synthesis of polymer 1. 19 Using F-NMR and 2,2-bis(4-hydroxyphenyl)hexafluoropropane as an internal standard, it was confirmed that a polymer having the following repeating unit structure was obtained.
[0149] [ka]
[0150] <Synthesis method of polymer 3> The methyl trifluorodecaheptanoate used in the synthesis of polymer 1 was replaced with 5.48 g of nonafluorobutyl isocyanate, and 4.8 g of polymer 3 was obtained by the same procedure. 19 Using F-NMR and 2,2-bis(4-hydroxyphenyl)hexafluoropropane as an internal standard, it was confirmed that a polymer having the following repeating unit structure was obtained.
[0151] [ka]
[0152] [Example 1] <Preparation of Magnetic Layer-Forming Composition> The following ingredients were mixed in an open kneader and then dispersed in a sand mill. Ferromagnetic powder: 100.0 parts Polyalkyleneimine polymer A: See Table 1 Polyurethane resin: (Vylon (registered trademark) UR4800 manufactured by Toyobo Co., Ltd., functional group: SO3Na, functional group concentration: 70eq / ton): 4.0 parts Polyvinyl chloride resin (Kaneka MR104): 10.0 parts Methyl ethyl ketone: 150.0 parts Cyclohexanone: 150.0 parts α-Al2O3 (average particle size 0.1μm): 6.0 parts Carbon black (average particle size: 20 nm): 0.7 parts
[0153] The following components were added to the dispersion obtained above, and the mixture was stirred, then ultrasonically treated and filtered using a filter having a pore size of 1 μm to prepare a composition for forming a magnetic layer. Fluorine-based nitrogen-containing polymer (see Table 1 for types and amounts added) Stearic acid: 1.5 parts Butyl stearate: 0.5 parts Stearic acid amide: 0.3 parts Methyl ethyl ketone: 110.0 parts Cyclohexanone: 110.0 parts Polyisocyanate compound (Tosoh Coronate 3041): 3.0 parts
[0154] <Preparation of composition for forming nonmagnetic layer> The following components were kneaded in an open kneader and then dispersed using a sand mill. The resulting dispersion was filtered using a filter with a pore size of 1 μm to prepare a composition for forming a nonmagnetic layer. Carbon black: 100.0 parts DBP (Dibutyl phthalate) oil absorption: 100mL / 100g pH:8 BET (Brunauer-Emmett-Teller) specific surface area: 250m 2 / g Volatile content: 1.5% Polyurethane resin (Vylon UR4800 manufactured by Toyobo Co., Ltd., functional group: SO3Na, functional group concentration: 70eq / ton): 20.0 parts Vinyl chloride resin (functional group: OSO3K, functional group concentration: 70eq / ton): 30.0 parts Trioctylamine: 4.0 parts Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Stearic acid amide: 0.3 parts Toluene: 3.0 parts Polyisocyanate compound (Tosoh Coronate 3041): 5.0 parts
[0155] <Preparation of Composition for Forming Backcoat Layer> The following components were pre-mixed in a roll mill and then dispersed in a sand mill. To the resulting dispersion, 4.0 parts of polyester resin (Vylon 500 manufactured by Toyobo Co., Ltd.), 14.0 parts of polyisocyanate compound (Coronate 3041 manufactured by Tosoh Corporation) and 5.0 parts of α-Al2O3 (manufactured by Sumitomo Chemical Co., Ltd.) were added, stirred and then filtered to prepare a composition for forming a backcoat layer. Carbon black (average particle size 40 nm): 85.0 parts Carbon black (average particle size 100 nm): 3.0 parts Nitrocellulose: 28.0 parts Polyurethane resin: 58.0 parts Copper phthalocyanine dispersant: 2.5 parts Nipolan 2301 (Tosoh Corporation): 0.5 parts Methyl isobutyl ketone: 0.3 parts Methyl ethyl ketone: 860.0 parts Toluene: 240.0 parts
[0156] <Magnetic recording medium production> Both surfaces of a biaxially oriented polyethylene naphthalate support having a thickness of 5.0 μm were subjected to a corona discharge treatment. The non-magnetic layer forming composition was applied onto one surface of the polyethylene naphthalate support so that the non-magnetic layer had a dry thickness of 1.0 μm, and immediately thereafter, the magnetic layer forming composition was simultaneously applied thereon in a multi-layer manner so that the magnetic layer had a dry thickness of 100 nm. While both layers were in a wet state, a vertical orientation treatment was performed using a cobalt magnet having a magnetic force of 0.5 T (tesla) and a solenoid having a magnetic force of 0.4 T, and then a drying treatment was performed. Then, the backcoat layer forming composition was applied onto the other surface of the polyethylene naphthalate support so that the backcoat layer had a dry thickness of 0.5 μm, and then calendering was performed at a speed of 80 m / min with a calender roll surface temperature of 100° C. using a seven-stage calender consisting of metal rolls. Then, the sheet was slit into a width of 1 / 2 inch (1 inch is 0.0254 meters) to prepare a magnetic tape.
[0157] [Examples 2 to 4, Comparative Example 1] A magnetic tape was produced by the method described in Example 1, except that various items were changed as shown in Table 1.
[0158] [Examples 5 to 11] A magnetic tape was produced by the method described for Example 1, except that the magnetic layer forming composition was prepared by the method described below.
[0159] <Preparation of Magnetic Layer-Forming Composition> The following ingredients were mixed in an open kneader and then dispersed in a sand mill. Ferromagnetic powder: 100.0 parts Polyalkyleneimine polymer A: See Table 1 Fluorine-based nitrogen-containing polymer (see Table 1 for types and amounts added) Polyurethane resin: (Vylon (registered trademark) UR4800 manufactured by Toyobo Co., Ltd., functional group: SO3Na, functional group concentration: 70eq / ton): 4.0 parts Polyvinyl chloride resin (Kaneka MR104): 10.0 parts Methyl ethyl ketone: 150.0 parts Cyclohexanone: 150.0 parts α-Al2O3 (average particle size 0.1μm): 6.0 parts Carbon black (average particle size: 20 nm): 0.7 parts
[0160] The following components were added to the dispersion obtained above, and the mixture was stirred, then ultrasonically treated and filtered using a filter having a pore size of 1 μm to prepare a composition for forming a magnetic layer. Stearic acid: 1.5 parts Butyl stearate: 0.5 parts Stearic acid amide: 0.3 parts Methyl ethyl ketone: 110.0 parts Cyclohexanone: 110.0 parts Polyisocyanate compound (Tosoh Coronate 3041): 3.0 parts
[0161] [Examples 12 and 13, Comparative Example 2] A magnetic tape was produced by the method described for Example 1, except that the magnetic layer forming composition was prepared by the method described below.
[0162] <Preparation of Magnetic Layer-Forming Composition> The following ingredients were mixed in an open kneader and then dispersed in a sand mill. Ferromagnetic powder: 100.0 parts Polyalkyleneimine polymer A: See Table 1 Polyurethane resin: (Vylon (registered trademark) UR4800 manufactured by Toyobo Co., Ltd., functional group: SO3Na, functional group concentration: 70eq / ton): 4.0 parts Polyvinyl chloride resin (Kaneka MR104): 10.0 parts Methyl ethyl ketone: 150.0 parts Cyclohexanone: 150.0 parts α-Al2O3 (average particle size 0.1μm): 6.0 parts Carbon black (average particle size: 20 nm): 0.7 parts
[0163] The following components were added to the dispersion obtained above, and the mixture was stirred, then ultrasonically treated and filtered using a filter having a pore size of 1 μm to prepare a composition for forming a magnetic layer. Fluorine-containing compounds (see Table 1 for types and amounts added) Stearic acid: 1.5 parts Butyl stearate: 0.5 parts Stearic acid amide: 0.3 parts Methyl ethyl ketone: 110.0 parts Cyclohexanone: 110.0 parts Polyisocyanate compound (Tosoh Coronate 3041): 3.0 parts
[0164] A sample piece having a length of 30 cm was cut out from each of the magnetic tapes of Example 12, Example 13, and Comparative Example 2. The cut out sample piece was placed on a petri dish and the entire sample piece was immersed in 10 mL of tetrahydrofuran (THF) for 1 hour for extraction treatment. The THF after extraction treatment was transferred to a 50 mL one-necked eggplant flask, distilled off with an evaporator, and dried under reduced pressure. 1 H-NMR and 19 Using F-NMR and 2,2-bis(4-hydroxyphenyl)hexafluoropropane as an internal standard, the presence of a polymer in which the fluorine-containing group of the fluorine-containing compound is bonded to the fluorine atom of polyalkyleneimine-based polymer A was confirmed.
[0165] [Evaluation method] <Contact angle after washing with hexane> For each of the magnetic tapes of the Examples and Comparative Examples, the contact angle was determined after washing with hexane by the method described above. Specifically, the contact angle after washing with hexane was determined as follows. A sample piece having a length of 30 cm was cut out from each of the magnetic tapes of the Examples and Comparative Examples. The cut out sample piece was placed on a petri dish and the entire sample piece was immersed in 10 mL of fresh hexane. After one hour, the sample piece was removed from the hexane and allowed to dry naturally at room temperature for 24 hours or more. After the above hexane washing, the contact angle with water on the magnetic layer surface of the sample piece was measured by the following method using a contact angle measuring device (Contact angle measuring device DropMaster 700 manufactured by Kyowa Interface Science Co., Ltd.) The contact angle measurement was performed in a measurement environment with an atmospheric temperature of 20°C and a relative humidity of 25%. The above sample piece was placed on a glass slide so that the backcoat layer surface was in contact with the glass slide surface. 2.0 μL of the liquid for measurement (water) was dropped onto the surface of the sample piece (magnetic layer surface), and after visually confirming that the dropped liquid formed a stable droplet, the droplet image was analyzed using the contact angle analysis software FAMAS attached to the contact angle measuring device, and the contact angle between the sample piece and the droplet was measured. The contact angle was calculated using the θ / 2 method. The measurement points were six randomly selected points on the magnetic layer surface, and the contact angle was measured at each of the six points. The arithmetic average of the six measured values thus obtained was taken as the contact angle of the magnetic tape to be measured after washing with hexane. Method: Droplet method (θ / 2 method) Droplet recognition: automatic Droplet detection line (distance from needle tip): 50dots Algorithm: Automatic Image Mode: Frame Threshold Level: Automatic
[0166] <Friction> In an environment controlled at an atmospheric temperature of 13°C and a relative humidity of 80%, a magnetic head removed from an IBM LTO (registered trademark) G7 (Linear Tape-Open Generation 7) drive was attached to the tape running system, and a 20 m long magnetic tape was run at 4.0 m / s for 10,000 cycles while being unwound from the unwound roll and wound onto the take-up roll with a tension of 0.6 N. The frictional force acting on the magnetic head during each of the first and 10,000 cycles was measured using a strain gauge, and the friction coefficient μ value was calculated from the measured frictional force. The friction coefficient after repeated runs was evaluated from the measured μ value according to the following evaluation criteria. Evaluation results of A or B are preferable, with A being the most preferable. (Evaluation Criteria) A: μ value is less than 0.08 B: μ value is 0.08 or more and 0.12 or less C: μ value is greater than 0.12
[0167] <Wear resistance> In an environment controlled at an atmospheric temperature of 23°C and a relative humidity of 50%, the magnetic layer surface of an unrunning magnetic tape was brought into contact with one edge (edge) of an AlFeSil rectangular pillar (a pillar defined in ECMA (European Computer Manufacturers Association)-288 / Annex H / H2) at a wrap angle of 12 degrees so as to be perpendicular to the longitudinal direction of the pillar, and in this state, the 580 m long magnetic tape was made to reciprocate 50 times at a speed of 3 m / sec under a tension of 1.0 N. The AlFeSil rectangular pillar is a rectangular pillar made of AlFeSil, a sendust-based alloy. The edge of the above-mentioned rectangular pillar was observed from above using an optical microscope, and the wear width (AlFeSil wear width) explained in paragraph 0015 of JP 2007-026564 A based on FIG. 1 of the same publication was obtained. From the wear width obtained, the wear of the magnetic layer surface was evaluated according to the following evaluation criteria. The wear width is measured in μm. Evaluation results of A or B are preferable, with A being most preferable. A: Wear width is 15 or more and less than 25 B: Wear width is 25 to 40 C: Wear width less than 15 or more than 40
[0168] <5 nm protrusion reduction rate (evaluation of changes in the surface shape of the magnetic layer before and after repeated running)> For each of the magnetic tapes in the Examples and Comparative Examples, the number of protrusions having a height of 5 nm or more on the magnetic layer surface was determined by the following method for the magnetic tape before running and for the magnetic tape after repeated running in the above environment. The number of protrusions with a height of 5 nm or more is determined by measurement using an atomic force microscope (AFM). More specifically, in a planar image of the magnetic layer surface obtained by AFM, the surface where the volume of the convex and concave components in the measurement area is equal is defined as the reference plane, and the number of protrusions with a height of 5 nm or more from this reference plane is determined. Note that among the protrusions with a height of 5 nm or more that exist in the measurement area, there may be some that are partly within the measurement area and other parts that are outside the measurement area. When determining the number of protrusions, the number of protrusions including such protrusions is measured. The measurement area for AFM measurements is a 5 μm square (5 μm x 5 μm) area on the magnetic layer surface. Measurements are performed in three different measurement areas on the magnetic layer surface (n=3). The number of protrusions with a height of 5 nm or more is calculated as the arithmetic mean of the three values obtained by such measurements. The following measurement conditions are used for AFM measurements. An AFM (Veeco's Nanoscope 4) is used in tapping mode to measure a 5 μm square (5 μm × 5 μm) area on the surface of the magnetic layer of the magnetic tape. A BRUKER's RTESP-300 is used as the probe, with a resolution of 512 pixels × 512 pixels and a scan speed of 341 seconds per screen (512 pixels × 512 pixels). The change in the surface shape of the magnetic layer before and after repeated running was evaluated according to the following evaluation criteria using the protrusion reduction rate calculated by the following formula: The smaller the protrusion reduction rate, the more suppressed the change in the surface shape of the magnetic layer before and after repeated running can be judged to be. Protrusion reduction rate (%)=[(protrusion number found on unrun magnetic tape)−(protrusion number found on magnetic tape after the above repeated running) / (protrusion number found on unrun magnetic tape)]×100 (Evaluation Criteria) A: Protrusion reduction rate is 40% or less B: Protrusion reduction rate is more than 40% and less than 70% C: Protrusion reduction rate is 70% or more
[0169] <Dispersibility> For each of the examples and comparative examples, a sample solution was prepared by taking a portion of the magnetic layer-forming composition prepared above and diluting it to 1 / 50 by mass with the organic solvent used in the preparation of the composition. The arithmetic mean particle diameter of the prepared sample solution was measured using a light scattering particle size distribution meter (HORIBA LB500) and taken as the dispersed particle diameter. Dispersibility was evaluated according to the following evaluation criteria. It can be determined that the smaller the dispersed particle diameter value, the better the dispersibility of the ferromagnetic powder in the magnetic layer-forming composition. (Evaluation Criteria) A: Dispersed particle size is 25 nm or less B: Dispersed particle size is more than 25 nm and less than 40 nm C: Dispersed particle size is 40 nm or more
[0170] The evaluation results are shown in Table 1.
[0171] [Table 1]
[0172] The results shown in Table 1 confirm that the magnetic tapes of Examples 1 to 13 have a magnetic layer surface with moderate wear resistance, a low coefficient of friction even after repeated running, and little change in the surface shape of the magnetic layer before and after repeated running. In addition, when comparing, for example, Example 1 with Examples 5 to 11 in terms of the evaluation results of dispersibility shown in Table 1, the evaluation results of dispersibility in Examples 5 to 11, in which the amount of polyalkyleneimine-based polymer A added was smaller than that in Example 1, were also A, similar to Example 1. From this result, it can be confirmed that the fluorine-based nitrogen-containing polymers 1 to 3 contributed to the improvement of dispersibility, similar to the polyalkyleneimine-based polymer A. [Industrial Applicability]
[0173] One aspect of the present invention is useful in the technical field of magnetic recording media for high density recording.
Claims
1. A non-magnetic support and a magnetic layer containing ferromagnetic powder, a nitrogen-containing polymer is contained in a portion of the non-magnetic support on the magnetic layer side, the nitrogen-containing polymer comprises a fluorine-containing group and a polyester chain; the fluorine-containing group is bonded to a nitrogen atom of the nitrogen-containing polymer; The polyester chain is bonded to a nitrogen atom of the nitrogen-containing polymer or forms a salt bridge structure with a nitrogen atom of the nitrogen-containing polymer; and A magnetic recording medium, wherein the contact angle with water measured on the surface of said magnetic layer after washing with hexane is 90° or more.
2. 2. The magnetic recording medium according to claim 1, wherein the nitrogen-containing polymer is a polyalkyleneimine-based polymer.
3. 2. The magnetic recording medium according to claim 1, wherein the fluorine-containing group includes a group selected from the group consisting of a fluorinated alkyl group and a perfluoropolyether group.
4. 4. The magnetic recording medium according to claim 3, wherein the fluoroalkyl group has 1 to 6 carbon atoms.
5. 2. The magnetic recording medium according to claim 1, wherein the contact angle is equal to or greater than 90[deg.] and equal to or less than 110[deg.].
6. 2. The magnetic recording medium according to claim 1, further comprising at least one fatty acid compound selected from the group consisting of fatty acids, fatty acid esters and fatty acid amides, on the portion of the non-magnetic support on the side of the magnetic layer.
7. 2. The magnetic recording medium according to claim 1, further comprising a nitrogen-containing polymer other than the nitrogen-containing polymer in a portion on the magnetic layer side of the non-magnetic support.
8. 2. The magnetic recording medium according to claim 1, further comprising a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer.
9. 2. The magnetic recording medium according to claim 1, further comprising a backcoat layer containing a nonmagnetic powder on the surface of said nonmagnetic support opposite to the surface having said magnetic layer.
10. 2. The magnetic recording medium according to claim 1, which is a magnetic tape.
11. the nitrogen-containing polymer is a polyalkyleneimine-based polymer, the fluorine-containing group includes a group selected from the group consisting of a fluorinated alkyl group and a perfluoropolyether group, The fluorinated alkyl group is a fluorinated alkyl group having 1 to 6 carbon atoms, The contact angle is equal to or greater than 90° and equal to or less than 110°, the magnetic layer side portion of the non-magnetic support further comprises at least one fatty acid compound selected from the group consisting of fatty acids, fatty acid esters and fatty acid amides, and a nitrogen-containing polymer other than the nitrogen-containing polymer; a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer, a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer; and 2. The magnetic recording medium according to claim 1, which is a magnetic tape.
12. A magnetic tape cartridge comprising the magnetic tape according to claim 10 or 11.
13. A magnetic recording and reproducing device comprising the magnetic recording medium according to any one of claims 1 to 11.
Citation Information
Patent Citations
Magnetic recording medium and its production
JP1993307746A
Magnetic recording medium, and magnetic recording / reproducing device
JP2020161203A
Magnetic tape cartridge group and magnetic recording and reproducing device
US20220415350A1
Magnetic tape
JP2017157252A