Wire or rod steel for semi-hard magnetic component, and method for producing semi-hard magnetic component using the same
A cost-effective wire rod or steel bar with controlled element composition and optimized pearlite structure achieves sufficient semi-hard magnetic properties through quenching and tempering, addressing high-cost issues in conventional materials.
Patent Information
- Application Number
- JP2023071024
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2043-04-24
AI Technical Summary
Conventional steel materials for semi-hard magnetic components contain high amounts of expensive elements like Ni, Cu, Co, and/or V, leading to high raw material costs and reduced semi-hard magnetic properties when quenching and tempering treatment is applied, and they are not available in wire rod or steel bar forms.
A wire rod or steel bar composition with controlled amounts of elements such as C, Si, Mn, Cr, and a specific pearlite structure with a spherical carbide phase, optimized for quenching and tempering treatment to achieve semi-hard magnetic properties, with a composition that minimizes expensive elements to reduce costs.
The solution provides a wire rod or steel bar with low raw material costs and sufficient semi-hard magnetic properties, exhibiting coercive force within 500 to 20,000 A/m, residual magnetic flux density of 1.40T or more, and a squareness ratio of 0.85 or more, suitable for manufacturing semi-hard magnetic components.
Smart Images

Figure 2024156506000001 
Figure 2024156506000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a wire or bar for a semi-hard magnetic component, and a method for manufacturing a semi-hard magnetic component using the same. [Background technology]
[0002] In recent years, the number of electromagnetic parts that require excellent magnetic properties both when excited and when not excited has been increasing. Semi-hard magnetic parts with a coercive force (500 to 20,000 A / m) intermediate between that of permanent magnets and soft magnetic materials are used as magnetic parts incorporated into such electromagnetic parts.
[0003] Semi-hard magnetic parts have a higher coercive force than soft magnetic parts, which are also known as magnetic materials, by controlling the metal structure and suppressing the movement of magnetic domain walls. Semi-hard magnetic parts are generally required to have a coercive force of 500 to 20,000 A / m as their semi-hard magnetic properties, as well as a high residual magnetic flux density that affects the electromagnetic force when not excited, and a high squareness ratio to increase the magnetic energy that can be stored.
[0004] The steel material for obtaining the above-mentioned semi-hard magnetic parts (hereinafter also referred to as "steel material for semi-hard magnetic parts") is also called quench-hardened steel or γ / α transformation alloy in connection with the structure control method for obtaining semi-hard magnetic properties, such as quenching treatment. Semi-hard magnetic parts can be obtained by subjecting the steel material for semi-hard magnetic parts to heat treatment such as quenching and tempering, and then subjecting it to part processing. Alternatively, semi-hard magnetic parts can be obtained by subjecting the steel material for semi-hard magnetic parts to part processing and then subjecting it to quenching and tempering.
[0005] Specific examples of steel materials for semi-hard magnetic parts include steel materials containing Ni, Mn, Co, Cr and / or V. Steel materials for semi-hard magnetic parts are often used in the form of wire rods and steel bars.
[0006] Patent Document 1 discloses a steel material for semi-hard magnetic parts containing 5.0 mass% or more of Ni. Patent Document 2 discloses a steel material for semi-hard magnetic parts containing 2.0 mass% or more of Cu. Non-Patent Document 1 discloses a steel material for Fe-Co-V-based semi-hard magnetic parts (Co content is, for example, 30 mass% or more, V content is, for example, 3 mass% or more). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2013 / 027665 [Patent Document 2] Patent Publication No. 2008-274399 [Non-patent literature]
[0008] [Non-Patent Document 1] Yasuo Kimura, "Current Status of Semi-Hard Magnetic Materials", Journal of the Japan Institute of Metals, Vol. 9, No. 11, 1970, pp. 703-707 Summary of the Invention [Problem to be solved by the invention]
[0009] In the conventional techniques disclosed in Patent Documents 1-2 and Non-Patent Document 1, the steel materials for semi-hard magnetic parts all contain a large amount (for example, 2.0 mass % or more in total) of expensive elements such as Ni, Cu, Co and / or V. In such a case, the raw material cost may become extremely high. Simply reducing the amount of the above elements can reduce costs, but the above elements are also useful elements for suppressing the movement of domain walls, and the semi-hard magnetic properties after quenching and tempering may be significantly reduced. In addition, Patent Documents 1-2 and Non-Patent Document 1 do not disclose that the steel materials for semi-hard magnetic parts have the form of wire or bar. Therefore, in the conventional techniques disclosed in Patent Documents 1-2 and Non-Patent Document 1, it was difficult to obtain wire or bar having sufficient semi-hard magnetic properties after quenching and tempering at low cost.
[0010] The present disclosure has been made in consideration of these circumstances, and one of its objectives is to provide a wire or steel bar for semi-hard magnetic parts that has low raw material costs and that can obtain sufficient semi-hard magnetic properties by undergoing quenching and tempering treatments, and a method for manufacturing semi-hard magnetic parts using the same. [Means for solving the problem]
[0011] Aspect 1 of the present invention is C: 0.30% by mass or more and 1.50% by mass or less, Si: 0.75 mass% or less (excluding 0 mass%) Mn: 2.00 mass% or less (excluding 0 mass%) P: 0.050% by mass or less (including 0% by mass), S: 0.050% by mass or less (including 0% by mass), Cu: 0.30 mass% or less (excluding 0 mass%) Ni: 0.30 mass% or less (excluding 0 mass%) Cr: 0.20 mass% or more and 2.30 mass% or less, Al: 0.100 mass% or less (excluding 0 mass%) Ti: 0.100 mass% or less (including 0 mass%) V: 1.00% by mass or less (including 0% by mass), Nb: 1.00 mass% or less (including 0 mass%) Mo: 1.00 mass% or less (including 0 mass%) Ta: 1.00 mass% or less (including 0 mass%) W: 1.00% by mass or less (including 0% by mass), B: 0.010% by mass or less (including 0% by mass), Ca: 0.100% by mass or less (including 0% by mass), Mg: 0.100% by mass or less (including 0% by mass), Zr: 0.100 mass% or less (including 0 mass%), and N: Contains 0.0200 mass% or less (including 0 mass%), The balance is iron and unavoidable impurities, Contains 65% or more of pearlite structure by area, The wire or bar steel for semi-hard magnetic parts contains 1% by area or more of a spherical carbide phase in the pearlite structure.
[0012] Aspect 2 of the present invention is A method for producing a semi-hard magnetic part, comprising subjecting the wire or steel bar for the semi-hard magnetic part according to aspect 1 to quenching and tempering treatment and part processing. Effect of the Invention
[0013] According to an embodiment of the present invention, it is possible to provide a wire or steel bar for semi-hard magnetic parts which has low raw material costs and which can obtain sufficient semi-hard magnetic properties by performing quenching and tempering treatment, and a method for manufacturing a semi-hard magnetic part using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The inventors have conducted research from various angles in order to realize a wire or steel bar for semi-hard magnetic parts that has low raw material costs and that can obtain sufficient semi-hard magnetic properties (high squareness ratio and high residual magnetic flux density) by performing quenching and tempering treatment. First, the inventors considered reducing the content of expensive elements such as Ni, Cu, Co and / or V to less than 2.0 mass% in total (preferably less than 1.0 mass%) in order to achieve low raw material costs.
[0015] Within the constraints of the above-mentioned composition, the inventors have investigated a metal structure capable of forming a tempered martensite phase by quenching and tempering. The tempered martensite phase has finer crystal grains than, for example, a ferrite phase, and the fine crystal grains pin the movement of the magnetic domain walls, thereby improving the squareness ratio. It is conceivable to increase the amount of solute C in order to refine the crystal grains of the tempered martensite phase and improve the squareness ratio, but increasing the amount of solute C reduces the magnetic moment of the tempered martensite phase, thereby reducing the residual magnetic flux density of the semi-hard magnetic component.
[0016] Therefore, the present inventors have studied a metal structure containing both a carbide phase that is easily dissolved in a quenching and tempering treatment and a carbide phase that is not easily dissolved in a quenching and tempering treatment, and have found a wire or steel bar for semi-hard magnetic parts that can obtain sufficient semi-hard magnetic properties after quenching and tempering by adjusting the composition to a predetermined composition, containing a pearlite structure containing an elongated carbide phase that is easily dissolved in a predetermined proportion, and containing a globular carbide phase that is not easily dissolved in the pearlite structure in a predetermined proportion.
[0017] The details of each requirement stipulated in the embodiment of the present invention are shown below. In this specification, "semi-hard magnetic" means that the coercive force is within the range of 500 to 20000 A / m. In addition, in this specification, "part" refers to a part that has been processed. For example, a part that has not been processed may have a simple shape, such as a cylindrical shape or a rectangular parallelepiped shape, in which the solid structure extends linearly in one direction as a result of rolling and / or wire drawing, while a part that has been processed may have a complex shape, such as a ground part, a bent part, and / or an opening part, in which the solid structure does not extend linearly in one direction as a result of further processing such as forging and cutting in addition to rolling and / or wire drawing.
[0018] <1. Ingredient composition> The wire or steel bar for a semi-hard magnetic part according to an embodiment of the present invention has a composition comprising C: 0.30% by mass or more and 1.50% by mass or less, Si: 0.75% by mass or less (excluding 0% by mass), Mn: 2.00% by mass or less (excluding 0% by mass), P: 0.050% by mass or less (including 0% by mass), S: 0.050% by mass or less (including 0% by mass), Cu: 0.30% by mass or less (excluding 0% by mass), Ni: 0.30% by mass or less (excluding 0% by mass), Cr: 0.20% by mass or more and 2.30% by mass or less, Al: 0.100% by mass or less (excluding 0% by mass), Ti: 0.100% by mass or less (including 0% by mass). %, V: 1.00 mass% or less (including 0 mass%), Nb: 1.00 mass% or less (including 0 mass%), Mo: 1.00 mass% or less (including 0 mass%), Ta: 1.00 mass% or less (including 0 mass%), W: 1.00 mass% or less (including 0 mass%), B: 0.010 mass% or less (including 0 mass%), Ca: 0.100 mass% or less (including 0 mass%), Mg: 0.100 mass% or less (including 0 mass%), Zr: 0.100 mass% or less (including 0 mass%), and N: 0.0200 mass% or less (including 0 mass%), with the balance being iron and inevitable impurities. Each element will be described in detail below.
[0019] (C: 0.30 mass% or more and 1.50 mass% or less) C promotes the formation of tempered martensite phase, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the domain wall movement of the tempered martensite phase. It is also necessary to form a pearlite structure before quenching and tempering. In order to effectively exert the above effects, the C content is set to 0.30 mass% or more. The C content is preferably 0.4 mass% or more, and more preferably 0.50 mass% or more. If the C content is excessive, the formation of metal structures other than pearlite structures, such as bainite structures, is promoted in the metal structure before quenching and tempering, and the proportion of pearlite structures is reduced. The reduction in pearlite structures reduces the magnetic moment of the tempered martensite phase and reduces the residual magnetic flux density. Therefore, the C content is set to 1.50 mass% or less. The C content is preferably 1.40 mass% or less, more preferably 1.30 mass% or less, and even more preferably 1.20 mass% or less.
[0020] (Si: 0.75 mass% or less (excluding 0 mass%)) Silicon effectively acts as a deoxidizer and also contributes to improving the semi-hard magnetic properties after quenching and tempering. To effectively exert these effects, the silicon content is set to more than 0 mass%. The silicon content is preferably 0.010 mass% or more, more preferably 0.050 mass% or more, and even more preferably 0.10 mass% or more. If the Si content is excessive, the magnetic moment decreases, and the semi-hard magnetic properties decrease. Furthermore, if the Si content is excessive, the hardness after quenching and tempering increases due to solid solution strengthening, and the workability decreases. Therefore, the Si content is set to 0.75 mass% or less. The Si content is preferably 0.65 mass% or less, more preferably 0.55 mass% or less, and even more preferably 0.35 mass% or less.
[0021] (Mn: 2.00 mass% or less (excluding 0 mass%)) Mn effectively acts as a deoxidizer, promotes the formation of tempered martensite phase, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the domain wall movement of the tempered martensite phase. It also promotes the formation of a globular carbide phase in the pearlite structure. In order to fully exert the above effects, the lower limit of the Mn content is more than 0 mass%. The Mn content is preferably 0.05 mass% or more, and more preferably 0.10 mass% or more. If the Mn content is excessive, the magnetic moment decreases, and the semi-hard magnetic properties decrease. In addition, the hardness increases after quenching and tempering, and the workability decreases. Therefore, the Mn content is set to 2.00 mass% or less. The Mn content is preferably 1.80 mass% or less, more preferably 1.70 mass% or less, and further preferably 1.50 mass% or less.
[0022] (P: 0.050% by mass or less (including 0% by mass)) P (phosphorus) is an inevitable impurity and a harmful element that causes grain boundary segregation in steel and adversely affects toughness. Therefore, the P content is set to 0.050 mass% or less. The P content is preferably 0.030 mass% or less, and more preferably 0.020 mass% or less. The lower limit of the P content may be more than 0 mass%, or may be 0.001 mass% or more. In this specification, "including 0 mass%" means that it includes embodiments in which it is not added intentionally, i.e., the content is below the unavoidable impurity level (it does not exclude the case where it is added intentionally).
[0023] (S: 0.050% by mass or less (including 0% by mass)) S (sulfur) is an inevitable impurity, and forms MnS in steel, which deteriorates ductility and is therefore a harmful element to workability. Therefore, the S content is set to 0.050 mass% or less. The S content is preferably 0.030 mass% or less, more preferably 0.020 mass% or less, and further preferably 0.010 mass% or less. The lower limit of the S content may be more than 0 mass%, or may be 0.001 mass% or more.
[0024] (Cu: 0.30 mass% or less (excluding 0 mass%), Ni: 0.30 mass% or less (excluding 0 mass%)) Both Cu and Ni promote the formation of a tempered martensite phase and contribute to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the tempered martensite phase on the magnetic domain wall motion. Therefore, the contents of Cu and Ni are each set to more than 0 mass%. If the contents of Cu and Ni are excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the contents of Cu and Ni are each set to 0.30 mass% or less. Preferably, each is set to 0.25 mass% or less, more preferably, each is set to 0.20 mass% or less, and even more preferably, each is set to 0.10 mass% or less. In addition, from the viewpoint of further reducing the raw material cost, it is even more preferable that Cu is less than 0.05 mass%. Similarly, from the viewpoint of further reducing the raw material cost, it is even more preferable that Ni is less than 0.05 mass%.
[0025] (Cr: 0.20 mass% or more and 2.30 mass% or less) Cr promotes the formation of tempered martensite phase, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the tempered martensite phase against magnetic domain wall movement. It also promotes the formation of globular carbides in the pearlite structure. To effectively exert these effects, the Cr content is 0.20 mass% or more, preferably 0.25 mass% or more, more preferably 0.30 mass% or more, and even more preferably 0.35 mass% or more. If the Cr content is excessive, the formation of metal structures other than pearlite structures, such as martensite and / or bainite structures, is promoted in the metal structure before quenching and tempering, and the proportion of pearlite structures is reduced. Since the ferrite phase in the martensite and bainite structures has a larger amount of dissolved C than the ferrite phase in the pearlite structure, the amount of dissolved C contained in the tempered martensite phase after quenching and tempering is excessive, and the residual magnetic flux density is reduced. Therefore, the Cr content is set to 2.30 mass% or less. The Cr content is preferably 2.00 mass% or less, and more preferably 1.80 mass% or less.
[0026] (Al: 0.100% by mass or less (excluding 0% by mass)) Al is an element that effectively acts as a deoxidizer, and has the effect of reducing impurities as a result of deoxidization. In order to effectively exert this effect, the Al content is made to be more than 0 mass%. The Al content is preferably 0.005 mass% or more, and more preferably 0.010 mass% or more. If the Al content is excessive, the magnetic moment decreases and the residual magnetic flux density decreases. Therefore, the Al content is set to 0.100 mass% or less. The Al content is preferably 0.080 mass% or less, more preferably 0.050 mass% or less, and further preferably 0.040 mass% or less.
[0027] (N: 0.0200% by mass or less (including 0% by mass)) N is an impurity that is inevitably contained in steel, but if the steel contains a large amount of solute N, it causes an increase in hardness and a decrease in ductility due to strain aging, and therefore decreases workability. Therefore, the N content is set to 0.0200 mass% or less, preferably 0.0180 mass% or less, more preferably 0.0160 mass% or less, and further preferably 0.0140 mass% or less.
[0028] (Ti: 0.100 mass% or less (including 0 mass%)) Ti is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Ti content is equal to or lower than the level of unavoidable impurities, i.e., 0 mass %. Ti forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement (i.e., the pinning effect of the domain wall movement). In order to effectively exert this effect, the Ti content may be more than 0 mass %. The Ti content is preferably 0.005 mass % or more, and more preferably 0.010 mass % or more. If the Ti content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the Ti content is set to 0.100 mass% or less. The Ti content is preferably 0.080 mass% or less, more preferably 0.050 mass% or less, and further preferably 0.040 mass% or less.
[0029] (V: 1.00% by mass or less (including 0% by mass)) V is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the V content is equal to or lower than the level of unavoidable impurities, i.e., 0 mass %. V forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing domain wall movement (i.e., the pinning effect of domain wall movement). In order to effectively exert this effect, the V content may be more than 0 mass %. The V content is preferably 0.01 mass % or more, and more preferably 0.02 mass % or more. If the V content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the V content is set to 1.00 mass% or less. The V content is preferably 0.80 mass% or less, more preferably 0.50 mass% or less, and further preferably 0.40 mass% or less.
[0030] (Nb: 1.00 mass% or less (including 0 mass%)) Nb is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Nb content is equal to or lower than the level of unavoidable impurities, i.e., 0 mass%. Nb forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement (i.e., the pinning effect of the domain wall movement). In order to effectively exert this effect, the Nb content may be more than 0 mass%. The Nb content is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more. If the Nb content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the Nb content is set to 1.00 mass% or less. The Nb content is preferably 0.80 mass% or less, more preferably 0.50 mass% or less, and further preferably 0.40 mass% or less.
[0031] (Mo: 1.00 mass% or less (including 0 mass%)) Mo is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Mo content is equal to or less than the level of unavoidable impurities, i.e., 0 mass%. Mo forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement (i.e., the pinning effect of the domain wall movement). Furthermore, Mo promotes the formation of a tempered martensite phase, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the tempered martensite phase on the domain wall movement. To effectively exert this effect, the Mo content may be more than 0 mass%. The Mo content is preferably 0.01 mass% or more, and more preferably 0.02 mass% or more. If the Mo content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the Mo content is set to 1.00 mass% or less. The Mo content is preferably 0.80 mass% or less, more preferably 0.50 mass% or less, and further preferably 0.40 mass% or less.
[0032] (Ta: 1.00 mass% or less (including 0 mass%)) Ta is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Ta content is equal to or lower than the level of unavoidable impurities, i.e., 0 mass %. Ta forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement (i.e., the pinning effect of the domain wall movement). To effectively exert this effect, the Ta content may be more than 0 mass %. The Ta content is preferably 0.01 mass % or more, and more preferably 0.02 mass % or more. If the Ta content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the Ta content is set to 1.00 mass% or less. The Ta content is preferably 0.80 mass% or less, more preferably 0.50 mass% or less, and further preferably 0.40 mass% or less.
[0033] (W: 1.00% by mass or less (including 0% by mass)) W is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the W content is equal to or less than the level of unavoidable impurities, i.e., 0% by mass. W forms fine carbides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement of the carbides (i.e., the pinning effect of the domain wall movement). Furthermore, W promotes the formation of a tempered martensite phase, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the domain wall movement of the tempered martensite phase. In order to effectively exert this effect, the W content may be more than 0% by mass. The W content is preferably 0.01% by mass or more, and more preferably 0.02% by mass or more. If the W content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the W content is set to 1.00 mass% or less. The W content is preferably 0.80 mass% or less, more preferably 0.50 mass% or less, and further preferably 0.40 mass% or less.
[0034] (B: 0.010% by mass or less (including 0% by mass)) B is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the B content is equal to or less than the level of unavoidable impurities, i.e., 0 mass%. B forms fine carbides and / or nitrides in the metal structure, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the effect of suppressing the domain wall movement (i.e., the pinning effect of the domain wall movement). Furthermore, B promotes the formation of a tempered martensite phase by adding a small amount, and contributes to improving the semi-hard magnetic properties after quenching and tempering due to the pinning effect of the domain wall movement of the tempered martensite phase. To effectively exert this effect, the B content may be more than 0 mass%. The B content is preferably 0.001 mass% or more, and more preferably 0.002 mass% or more. If the B content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the B content is set to 0.010 mass% or less. The B content is preferably 0.005 mass% or less, and more preferably 0.003 mass% or less.
[0035] (Ca: 0.100% by mass or less (including 0% by mass)) Ca is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Ca content is equal to or less than the level of unavoidable impurities, i.e., 0% by mass. Ca can finely disperse inclusions generated by a deoxidizer in the metal structure, and has the effect of suppressing the adverse effects of the inclusions. Furthermore, the finely dispersed inclusions can refine the crystal grains, and the effect of suppressing domain wall movement (i.e., the pinning effect of domain wall movement) contributes to improving the semi-hard magnetic properties after quenching and tempering. In order to effectively exert this effect, the Ca content may be more than 0% by mass. The Ca content is preferably 0.005% by mass or more, and more preferably 0.010% by mass or more. If the Ca content is excessive, the magnetic moment decreases and the residual magnetic flux density decreases. Therefore, the Ca content is set to 0.100 mass% or less. The Ca content is preferably 0.080 mass% or less, more preferably 0.050 mass% or less, and even more preferably 0.040 mass% or less.
[0036] (Mg: 0.100% by mass or less (including 0% by mass)) Mg is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Mg content is equal to or less than the level of unavoidable impurities, i.e., 0% by mass. Mg can finely disperse inclusions generated by a deoxidizer in the metal structure, and has the effect of suppressing the adverse effects of the inclusions. Mg can further refine the crystal grains by the finely dispersed inclusions, and contributes to improving the semi-hard magnetic properties after quenching and tempering treatments due to the effect of suppressing domain wall movement (i.e., the pinning effect of domain wall movement). In order to effectively exert this effect, the Mg content may be more than 0% by mass. The Mg content is preferably 0.005% by mass or more, and more preferably 0.010% by mass or more. If the Mg content is excessive, the magnetic moment decreases and the residual magnetic flux density decreases. Therefore, the Mg content is set to 0.100 mass% or less. The Mg content is preferably 0.080 mass% or less, more preferably 0.050 mass% or less, and further preferably 0.040 mass% or less.
[0037] (Zr: 0.100 mass% or less (including 0 mass%)) Zr is an element that may be optionally contained. The embodiment of the present invention also includes an embodiment in which the Zr content is equal to or less than the unavoidable impurity level, i.e., 0 mass%. Zr can finely disperse inclusions generated by a deoxidizer in the metal structure, and has the effect of suppressing the adverse effects of the inclusions. Zr can further refine the crystal grains by the finely dispersed inclusions, and contributes to improving the semi-hard magnetic properties after quenching and tempering treatment by the effect of suppressing domain wall movement (i.e., the pinning effect of domain wall movement). In order to effectively exert this effect, the Zr content may be more than 0 mass%. The Zr content is preferably 0.005 mass% or more, and more preferably 0.010 mass% or more. If the Zr content is excessive, the magnetic moment decreases, the residual magnetic flux density decreases, and the raw material cost increases. Therefore, the Zr content is set to 0.100 mass% or less. The Zr content is preferably 0.080 mass% or less, more preferably 0.050 mass% or less, and further preferably 0.040 mass% or less.
[0038] The wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention preferably contains the above-mentioned composition, and in one embodiment of the present invention, the balance is preferably iron and inevitable impurities. As inevitable impurities, the inclusion of trace elements (e.g., As, Sb, Sn, etc.) brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. Note that, for example, there are elements such as P, S, and N, which are usually preferable to have a smaller content and are therefore inevitable impurities, but whose composition ranges are separately specified as above. For this reason, in this specification, when the term "unavoidable impurities" is used, it is a concept excluding elements whose composition ranges are separately specified.
[0039] <2.Metal structure> The wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention contains 65% by area or more of pearlite structure, and the pearlite structure contains 1% by area or more of spheroidal carbide phase. Each requirement will be described in detail below.
[0040] (Pearlite structure of 65% or more area) The wire or steel bar for the semi-hard magnetic part according to the embodiment of the present invention contains 65% or more of a pearlite structure. The pearlite structure is a structure in which ferrite phases and elongated carbide phases are densely and uniformly distributed alternately. By making this pearlite structure exist in an amount of 65% or more of the metal structure before the quenching and tempering treatment, the elongated carbide phase is dissolved in large amounts by the quenching and tempering treatment, and the tempered martensite phase becomes fine, so that the squareness ratio of the semi-hard magnetic part after the quenching and tempering treatment can be improved, and as a result, a sufficient squareness ratio and a sufficient residual magnetic flux density can be achieved at the same time. The upper limit of the area ratio of the pearlite structure is not particularly limited, but is approximately 99 area % in consideration of the component composition and production conditions according to the embodiment of the present invention.
[0041] (Spherical carbide phase of 1% or more by area in pearlite structure) In the wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention, the spherical carbide phase contained in the pearlite structure is 1% by area or more. Compared to the elongated carbide phase that constitutes a lamellar structure in the pearlite structure, the spherical carbide phase in the pearlite structure is stable, and the solid solution of the carbide phase during quenching and tempering is suppressed. Therefore, by having the spherical carbide phase be 1% by area or more, the amount of C that is solid-dissolved in the martensite phase during quenching and tempering is reduced, the magnetic moment in the tempered martensite phase after quenching and tempering is increased, and a semi-hard magnetic part having sufficient residual magnetic flux density can be obtained. The upper limit of the area ratio of the globular carbide phase is not particularly limited, but is approximately 10% by area, taking into consideration the component composition and manufacturing conditions according to the embodiment of the present invention. In this specification, the "globular carbide phase" refers to a carbide phase that exists in a pearlite structure, has an aspect ratio of 3 or less, and has a major axis of 0.04 μm or more. In this specification, the maximum length of the globular carbide phase is the "major axis", the longest line segment perpendicular to the major axis of the globular carbide phase is the "minor axis", and the "major axis / minor axis" is the "aspect ratio".
[0042] The above-mentioned area ratios can be determined from a cross section at any position except the surface layer of the wire rod or steel bar by the method described in the Examples below. The surface layer of the wire rod or steel bar may be a position at a depth of less than 1 mm from the surface toward the center.
[0043] The diameter of the wire or steel bar for the semi-hard magnetic component according to the embodiment of the present invention is not particularly limited, but in the case of wire, it may be, for example, 5.5 mm to 55 mm, and in the case of steel bar, it may be, for example, 18 mm to 105 mm.
[0044] The wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention exhibits sufficient semi-hard magnetic properties by undergoing quenching and tempering treatment, specifically, the coercive force is within the range of 500 to 20,000 A / m, the residual magnetic flux density (Br) is 1.40 T or more, and the squareness ratio (Br / B10k) is 0.85 or more. Note that "B10k" is the magnetic flux density (unit: T) when the magnetic field is 10 kA / m. Preferably, the residual magnetic flux density (Br) is 1.45 T or more.
[0045] <3. Manufacturing method of wire or steel bar for semi-hard magnetic parts> A method for producing a wire or steel bar for a semi-hard magnetic component according to an embodiment of the present invention includes the steps of: preparing a steel billet having the above-mentioned composition; heating the steel slab to 800 to 1000°C; After the heating step, the method includes a step of cooling to 600° C. at an average cooling rate of 1.0° C. / sec or more and less than 20° C. / sec. After the cooling step, the wire or bar for semi-hard magnetic components according to the embodiment of the present invention is obtained. Each step will be described in detail below.
[0046] (The process of preparing steel pieces) A steel slab satisfying the above-mentioned composition is prepared. For example, the steel slab may be prepared by melting and casting the steel slab according to a normal melting method.
[0047] After casting, soaking may be performed as necessary. By performing soaking, component segregation and texture segregation in the steel slab can be eliminated, and a homogeneous metal structure can be obtained. In order to sufficiently diffuse the components in the steel slab, it is preferable to perform soaking at a high temperature for a long time. Specifically, the soaking temperature is preferably 1150°C or higher, and the soaking time is preferably 1 hour or longer. On the other hand, if the temperature is too high, there is a risk that part of the steel slab will melt and a homogeneous metal structure cannot be obtained, so the soaking temperature is preferably 1350°C or lower, and more preferably 1300°C or lower.
[0048] (Heating process) The steel slab is heated to 800 to 1000°C. At this time, if necessary, processing such as rolling or forging (i.e., hot processing) may be performed to form a wire rod or a steel bar, or the wire rod or steel bar may be formed by processing at a different timing. If the heating temperature exceeds 1000°C, there is a risk that the globular carbides will be excessively dissolved. The heating temperature is preferably 950°C or less. On the other hand, if the heating temperature is less than 800°C, there is a risk that the desired metal structure will not be obtained. In addition, when hot processing is performed, problems such as increased hardness and increased load on equipment such as a rolling mill may occur.
[0049] (Cooling process) After the heating step, the material is cooled to 600°C at an average cooling rate of 1.0°C / sec or more. By increasing the average cooling rate, atomic diffusion in the metal structure at high temperatures is less likely to proceed, nucleation of a reticulated carbide phase other than the globular carbide phase is suppressed, and carbide growth with the undissolved globular carbide phase as a nucleus is promoted, making it easier to increase the area ratio of the globular carbide phase. Therefore, the average cooling rate is 1.0°C / sec or more, preferably 1.3°C / sec or more. In addition, such structure formation progresses particularly at high temperatures up to about 600°C. Therefore, the average cooling rate in the temperature range below 600°C may be any rate. If the average cooling rate to 600°C is too fast, the formation of bainite and / or martensite phases is promoted, and the pearlite structure is not sufficiently obtained, resulting in a deterioration of the semi-hard magnetic properties after quenching and tempering. Therefore, the average cooling rate is set to less than 20°C / sec. The average cooling rate is preferably less than 15°C / sec, and more preferably less than 10°C / sec.
[0050] Regarding the method of controlling the average cooling rate up to 600°C, since the average cooling rate when simply cooling naturally is usually slower than 1.0°C / sec, it is effective to control the cooling rate using cooling water or oil. The cooling method below 600°C is not particularly limited, and cooling may be performed under any conditions, such as natural cooling.
[0051] The method for producing a wire or steel bar for a semi-hard magnetic component according to the embodiment of the present invention may include other steps, such as a processing step, without departing from the scope of the present invention.
[0052] <4. Manufacturing method of semi-hard magnetic parts> The method for manufacturing the semi-hard magnetic component according to the embodiment of the present invention includes subjecting the wire or steel bar for the semi-hard magnetic component according to the embodiment of the present invention to quenching and tempering treatment and component processing.
[0053] (Hardening and tempering treatment) In the wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention, a metal structure including a magnetic martensite phase can be formed by performing a quenching treatment. The martensite phase has finer crystal grains than the ferrite phase, which inhibits the movement of domain walls and allows a high coercive force and squareness ratio to be obtained. However, immediately after the quenching treatment, the hardness is very high and the workability is poor due to thermal strain and / or transformation strain. Therefore, it is recommended to perform a tempering treatment to reduce the strain. The conditions for the quenching and tempering treatment are not particularly limited, and the treatment may be performed by a known method. In order to effectively exhibit the effects of the pearlite structure and the spheroidal carbide phase in the pearlite structure of the wire or steel bar for the semi-hard magnetic component according to the embodiment of the present invention, the following conditions may be mentioned, for example: Holding temperature during quenching: 800℃ to 900℃; Holding time during quenching: 10 minutes or more and 60 minutes or less; Cooling method during quenching: oil quenching; Holding temperature during tempering: 500℃ to 650℃; Holding time during tempering: 30 minutes or more and 180 minutes or less; and Cooling method during tempering process: air cooling. The atmosphere during the quenching and tempering treatment does not significantly change the structure, so quenching and tempering may be performed in any atmosphere.
[0054] The wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention can be subjected to part processing such as cutting and / or surface treatment in addition to the above-mentioned quenching and tempering treatment to obtain a semi-hard magnetic part. Note that even if the part is processed at a temperature below the tempering treatment temperature, it does not have a significant adverse effect on the semi-hard magnetic properties. Therefore, when obtaining a semi-hard magnetic part from the wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention, the order of part processing at a temperature below the tempering treatment temperature and quenching and tempering is not limited. For example, a semi-hard magnetic part having sufficient semi-hard magnetic properties can be manufactured in either case of processing the part before quenching and tempering and then quenching and tempering, or processing the part after quenching and tempering.
[0055] The semi-hard magnetic parts obtained from the wire or steel bar for semi-hard magnetic parts according to the embodiment of the present invention can be suitably used as composite magnetic parts (parts consisting of multiple members, at least some of which are magnetic) such as relays (latching relays, ferrites), reed switches, memories, motors (external rotor, internal rotor), electromagnetic clutches (moving member, stator), electromagnetic brakes, etc. The composite magnetic parts including the semi-hard magnetic parts are industrially useful because they include steel parts having sufficient semi-hard magnetic properties. EXAMPLES
[0056] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.
[0057] Test materials A to I having the composition shown in Table 1 were melted by button melting and then cast. The obtained steel pieces were heated at 900 to 1000 ° C, and then air-cooled to 600 ° C at the average cooling rate shown in Table 1 to obtain steel materials of test Nos. 1 to 9. These steel materials were cast into a cylindrical shape with a diameter of 40 mm and a thickness of 20 mm to simulate a wire rod or steel bar with a diameter of 40 mm and have the same material properties and characteristics as the wire rod or steel bar. Test material J having the composition shown in Table 1 was melted in a converter, and the cast steel pieces were heated to 900 to 1000 ° C, hot-rolled, and formed into a rod shape with a diameter of 65 mm, and then air-cooled to 600 ° C at the average cooling rate shown in Table 1 to obtain a steel bar of test No. 10. Regarding the average cooling rate during air cooling, the steel products (simulated wire rod or steel bar) of Test Nos. 1 to 9 had smaller sizes before air cooling than the steel bar of Test No. 10, and therefore had faster average cooling rates from the heating temperature to 600°C, as shown in Table 2.
[0058] [Table 1]
[0059] The steel materials (simulations of wire rod or steel bar) of Test Nos. 1 to 9 were processed into rings with an outer diameter of 18 mm, an inner diameter of 10 mm, and a thickness of 4 mm. At this time, the center of the cylinder before processing and the center of the ring after processing were made to coincide. The steel bar of Test No. 10 was processed into a ring with an outer diameter of 38 mm, an inner diameter of 30 mm, and a thickness of 4 mm. At this time, the center of the rod (cylinder) before processing and the center of the ring after processing were made to coincide. For Test Nos. 1 to 10 (ring-shaped parts) machined into ring shapes, the area ratio of the pearlite structure and the area ratio of spherical carbides in the pearlite structure were measured by the following method.
[0060] <Area ratio of pearlite structure> The ring-shaped part was cut so that a cross section perpendicular to the circumferential direction of the part could be measured, then embedded in resin, emery-polished, diamond-buff-polished, and then etched with nital. An optical microscope image was obtained at a magnification of 400 times near the center of the cross section (usually the symmetric center of a 4×4 mm square cross section, and in the case where the metal structure is nonuniform due to segregation, the center of the range excluding that part was taken). In the image, 150 meshes (10 vertical points × 15 horizontal points) with equal intervals of 15 μm were set, the structure of each lattice point was identified, and the area ratio of the pearlite structure shown in Table 2 was calculated from the ratio of the number of lattice points that are pearlite structures to the total number of lattice points. As described above, the pearlite structure in this specification refers to a structure (lamella structure) in which an elongated carbide phase is mixed in a striped pattern in a ferrite phase. The elongated carbide phase in the pearlite structure can be divided by a globular carbide phase, but even when it is divided, it is considered to be a pearlite structure.
[0061] <Area ratio of spherical carbides in pearlite structure> The ring-shaped part was cut so that a cross section perpendicular to the circumferential direction of the part could be measured, then embedded in resin, emery-polished, diamond-buff-polished, and picral-etched. The center of the cross section was observed using a SEM (Scanning Electron Microscope), and a secondary electron image was obtained at a magnification of 10,000 times so that the pearlite structure or the boundary between the pearlite structure and the pearlite structure was included in the center of the field of view. 560 points (20 points vertically × 28 points horizontally) of a 0.43 μm square mesh were set at equal intervals in each field of view, the structure of each lattice point was identified, and the area ratio of the spheroidal carbide phase was calculated from the ratio of the number of lattice points that were spheroidal carbide phase to the number of lattice points that were pearlite structure.
[0062] For the ring-shaped test pieces No. 1 to 10 (ring-shaped parts), a laboratory furnace was used to carry out quenching and tempering treatment at a holding temperature of 840°C, a holding time of 30 minutes, a cooling method of quenching, oil quenching, a holding temperature of 600°C, a holding time of 120 minutes, and a cooling method of quenching, air cooling. After quenching and tempering treatment, the semi-hard magnetic properties were evaluated by the following method.
[0063] <Semi-hard magnetic property evaluation> After the quenching and tempering process, an insulating conductor was wound uniformly around the circumference of the ring as a magnetic field application coil and a magnetic flux detection coil, and the ring was demagnetized by applying an AC magnetic field. The BH curve was then measured at room temperature using a DC current under a maximum magnetic field of 10 kA / m to determine the coercive force Hc, residual magnetic flux density Br, and squareness ratio Br / B10k.
[0064] The above results are summarized in Table 2.
[0065] [Table 2]
[0066] The results in Table 2 can be considered as follows: Test Nos. 1 to 5 in Table 2 all satisfied the requirements stipulated in the embodiment of the present invention, were low in raw material cost, and exhibited sufficient semi-hard magnetic properties (coercive force: 500 to 20,000 A / m, residual magnetic flux density (Br): 1.40 T or more, squareness ratio (Br / B10k): 0.85 or more) by applying quenching and tempering treatment. On the other hand, Test Nos. 6 to 10 in Table 2 did not satisfy the requirements stipulated in the embodiment of the present invention, and the semi-hard magnetic properties after quenching and tempering were insufficient.
[0067] In Test Nos. 6 and 7, the C content was less than 0.30 mass %, the pearlite structure was less than 65 area %, and the squareness ratio (Br / B10k) after quenching and tempering was less than 0.85.
[0068] In Test No. 8, the C content exceeded 1.50 mass %, the pearlite structure was less than 65 area %, and the residual magnetic flux density (Br) after quenching and tempering was less than 1.40 T.
[0069] In Test No. 9, the Cr content exceeded 2.30 mass %, the pearlite structure was less than 65 area %, and the residual magnetic flux density (Br) after quenching and tempering was less than 1.40 T.
[0070] In Test No. 10, the average cooling rate to 600° C. was less than 1.0° C. / sec, the spheroidal carbide phase in the pearlite structure was less than 1 area %, and the residual magnetic flux density (Br) after quenching and tempering was less than 1.40 T.
Claims
1. C: 0.30% by mass or more and 1.50% by mass or less, Si: 0.75 mass% or less (excluding 0 mass%) Mn: 2.00% by mass or less (excluding 0% by mass), P: 0.050% by mass or less (including 0% by mass), S: 0.050% by mass or less (including 0% by mass), Cu: 0.30% by mass or less (excluding 0% by mass), Ni: 0.30 mass% or less (excluding 0 mass%) Cr: 0.20% by mass or more and 2.30% by mass or less, Al: 0.100% by mass or less (excluding 0% by mass), Ti: 0.100 mass% or less (including 0 mass%), V: 1.00% by mass or less (including 0% by mass), Nb: 1.00 mass% or less (including 0 mass%), Mo: 1.00 mass% or less (including 0 mass%), Ta: 1.00 mass% or less (including 0 mass%), W: 1.00% by mass or less (including 0% by mass), B: 0.010% by mass or less (including 0% by mass), Ca: 0.100% by mass or less (including 0% by mass), Mg: 0.100% by mass or less (including 0% by mass), Zr: 0.100% by mass or less (including 0% by mass), and N: Contains 0.0200 mass% or less (including 0 mass%), The balance is iron and unavoidable impurities, Contains 65% or more of pearlite structure, The wire or bar steel for semi-hard magnetic parts contains 1 area % or more of a spheroidal carbide phase in the pearlite structure.
2. A method for producing a semi-hard magnetic part, comprising subjecting the wire or steel bar for a semi-hard magnetic part according to claim 1 to quenching and tempering treatment and part processing.
Citation Information
Patent Citations
JP1971040853B1
Wire rod having excellent wire drawability and its production method
JP2007327084A
Hot rolled wire
JP2019112703A
Non-heat-treated forged component and non-heat-treated forging steel
JP2019143236A
Semi-hard magnetic steel and semi-hard magnetic steel component
JP2023065295A