Copper alloy powder, additive manufactured product including the same, and copper alloy molded product composed of additive manufactured product

A copper alloy powder with specific elemental ratios addresses the limitations of copper in L-PBF by maintaining mechanical strength during heat treatment, achieving high electrical conductivity and mechanical strength in layered products.

JP2024156538APending Publication Date: 2024-11-06OSAKA RES INST OF IND SCI & TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071087
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

The challenge in using copper for additive manufacturing methods like L-PBF is its low energy absorption rate and rapid heat diffusion, limiting its application and resulting products.

Method used

A copper alloy powder with specific elemental ratios of chromium, vanadium, and/or lanthanum, which maintains mechanical strength during heat treatment at 500°C or higher, enabling high electrical conductivity.

Benefits of technology

The copper alloy powder produces layered products with improved electrical conductivity and mechanical strength, suitable for applications requiring both properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156538000001_ABST
    Figure 2024156538000001_ABST
Patent Text Reader

Abstract

To provide a copper alloy powder capable of forming an additive manufactured product having excellent conductivity while maintaining mechanical strength even when subjected to heat treatment.MEANS: A copper alloy powder for additive manufacturing contains chromium of 0.1 mass% or more and 20.0 mass% or less, vanadium and / or lanthanum of 0.1 mass% or more and 5.0 mass% or less, and copper of 75.0 mass% or more and 99.8 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper alloy powder, a layered product using the copper alloy powder and a manufacturing method thereof, and a copper alloy molded product consisting of a layered product and a manufacturing method thereof. [Background technology]

[0002] Three-dimensional additive manufacturing devices, so-called 3D printers, capable of rapidly forming components with three-dimensional complex shapes, are becoming increasingly popular. Among the methods of manufacturing additive objects using such three-dimensional printing devices, the powder bed fusion (PBF) method is known as a method of obtaining metal objects. In the PBF method, the surface of a layer of powder (powder bed) is irradiated with energy rays such as a high-energy laser or electron beam to sinter or melt and solidify the powder particles, and these are stacked into layers of several tens of microns and repeatedly bonded to obtain three-dimensional additive objects. The L-PBF method, which uses metal-based powder and a laser as a heat source, has also been put to practical use, and in the L-PBF method using metal-based powder such as Co-Cr alloy, titanium alloy, maraging steel, stainless steel, and nickel-based superalloy, the processing precision of the obtained additive objects and the degree of completion as a product are high, and additive objects that can be used for heat-resistant and high-heat applications are also beginning to be put to practical use. However, the metal-based powders that can be used with the current L-PBF method are limited, and the metal products that can be obtained are also limited to a certain range.

[0003] For example, copper is a metal with high thermal and electrical conductivity and excellent workability, but it is considered difficult to apply the L-PBF method to it. The main reasons for this are that the energy absorption rate of the laser light is extremely low, making it impossible to reach the melting point, and even if it does reach the melting point, its high thermal conductivity causes the heat to diffuse rapidly and prevents sufficient melting.

[0004] To address these problems, Patent Document 1 reports that by using copper alloy powder containing chromium, thermal conductivity can be reduced, making additive manufacturing easier, and that by subjecting the resulting additive manufactured product to heat treatment, it is possible to achieve excellent electrical conductivity, thermal conductivity, and mechanical strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-070169 A Summary of the Invention [Problem to be solved by the invention]

[0006] Since the copper alloy powder described above can be applied to the L-PBF method to obtain an additive manufacturing product having high electrical conductivity and mechanical strength, mechanical parts requiring high electrical conductivity and mechanical strength (e.g., induction heating coils, heat sinks, parts of power distribution equipment, etc.) are manufactured by the L-PBF method using copper alloy powder. When manufacturing these mechanical parts, the additive manufacturing product may be subjected to heat treatment in order to further improve the electrical conductivity of the resulting additive manufacturing product. That is, by heat treating an additive manufacturing product made of a copper alloy containing chromium at about 500°C or less, the chromium that was in a supersaturated solid solution in the parent phase precipitates finely as a chromium phase, which is thought to improve the electrical conductivity and mechanical strength (hardness) of the heat-treated additive manufacturing product.

[0007] In this study, the inventors subjected an additive manufacturing object made using a copper alloy powder containing chromium to a heat treatment at approximately 500°C or higher. They found that although the precipitation of the chromium phase progressed further and the electrical conductivity improved, the chromium phase coarsened and its number density decreased, resulting in a decrease in mechanical strength (hardness).

[0008] Therefore, an object of the present invention is to provide a copper alloy powder that can give a layered molded product having excellent electrical conductivity while maintaining mechanical strength even when subjected to heat treatment at 500°C or higher. [Means for solving the problem]

[0009] The inventors of the present invention have found that by using copper alloy powder containing a specific element in a specific ratio in addition to a specific amount of chromium, a layered object having excellent electrical conductivity while maintaining mechanical strength even when subjected to heat treatment at 500° C. or higher can be obtained. The present invention is based on this finding. That is, the gist of the present invention is as follows.

[0010] [1] A copper alloy powder for additive manufacturing, comprising: 0.1% by mass or more and 20.0% by mass or less of chromium; 0.1% by mass or more and 5.0% by mass or less of vanadium and / or lanthanum, 75.0% by mass or more and 99.8% by mass or less of copper; A copper alloy powder containing [2] The copper alloy powder according to [1], containing 0.5 mass% or more and 5.0 mass% or less of chromium. [3] The copper alloy powder according to [1] or [2], wherein the ratio of the chromium content to the total content of chromium, vanadium, and lanthanum is 5 mass% or more and 99 mass% or less. [4] A method for producing an additive manufacturing object using the copper alloy powder according to any one of [1] to [3], A first step of forming a powder layer containing the copper alloy powder; A second step of forming a modeling layer by solidifying the copper alloy powder at a predetermined position in the powder layer, A method for manufacturing a layered object, comprising sequentially repeating the first step and the second step to stack the modeling layers to manufacture a layered object. [5] The method according to [4], further comprising a heat treatment step of heat treating the layered object. [6] The method according to [5], wherein the heat treatment temperature in the heat treatment is 800°C or less. [7] The method according to [5], wherein the heat treatment temperature in the heat treatment is 700°C or less. [8] The method according to [5], wherein the heat treatment temperature is 500°C or higher and 600°C or lower. [9] An additive manufacturing object made of a copper alloy, 0.1% by mass or more and 20.0% by mass or less of chromium; 0.1% by mass or more and 5.0% by mass or less of vanadium and / or lanthanum, 75.0% by mass or more and 99.8% by mass or less of copper; An additive manufacturing object comprising:

[10] The additive manufacturing object according to [9], containing 0.5% by mass or more and 5.0% by mass or less of chromium.

[11] A method for producing a copper alloy molded product comprising the layered product according to [9] or

[10] , and heat treating the laminated structure.

[12] A copper alloy molded product comprising the additive manufacturing product according to [9] or

[10] , A copper alloy molded product having an electrical conductivity of 30% IACS or more and a Vickers hardness of 60 HV or more.

[13] A method for producing a copper alloy molded product comprising the layered product according to [9] or

[10] , A copper alloy molded product having an electrical conductivity of 40% IACS or more and a Vickers hardness of 60 HV or more.

[14] A method for producing a copper alloy molded product comprising the layered product according to [9] or

[10] , A copper alloy molded product having an electrical conductivity of 50% IACS or more and a Vickers hardness of 60HV or more. Effect of the Invention

[0011] According to the present invention, by producing a copper alloy powder containing a specified amount of chromium as well as specific elements in specified ratios, it is possible to realize a copper alloy powder that can produce an additive manufacturing product having excellent electrical conductivity while maintaining its mechanical strength even when subjected to heat treatment at 500°C or higher. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is an example of three-dimensional shape data. [Diagram 2] FIG. 2 is an example of slice data. [Diagram 3]FIG. 3 is a first schematic diagram showing a manufacturing process of a layered object. [Figure 4] FIG. 4 is a second schematic diagram showing the manufacturing process of the additive manufacturing object. [Diagram 5] FIG. 5 is a third schematic diagram showing the manufacturing process of the additive manufacturing object. [Figure 6] FIG. 6 is a fourth schematic diagram showing the manufacturing process of the additive manufacturing object. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Copper alloy powder] The copper alloy powder according to the present invention is used as a raw material powder in an additive manufacturing method. In the additive manufacturing method, the raw material powder is irradiated with an energy beam, whereby the raw material powder melts and is rapidly cooled and solidified. That is, the raw material powder is solidified by irradiation with the energy beam. Details of the additive manufacturing method will be described later in the section "Method for manufacturing an additive manufactured product."

[0014] The copper alloy powder according to one embodiment of the present invention includes 0.1% to 20.0% by mass of chromium, 0.1% to 5.0% by mass of vanadium and / or lanthanum, and 75.0% to 99.8% by mass of copper. The copper alloy powder according to one embodiment of the present invention includes 0.1% to 20.0% by mass of chromium, 0.1% to 5.0% by mass of vanadium and / or lanthanum, 75.0% to 99.8% by mass of copper, and inevitable impurities. The copper alloy powder according to one embodiment of the present invention may include elements other than copper, chromium, vanadium, and lanthanum that are intentionally added during production.

[0015] According to the present invention, by making a copper alloy powder by adding a predetermined amount of chromium and a predetermined amount of vanadium and / or lanthanum to copper, it is possible to obtain a layered object having excellent electrical conductivity while maintaining mechanical strength even when subjected to a heat treatment at 500° C. or higher. The reason for this is believed to be as follows. That is, chromium is an element that is difficult to dissolve in copper, and when a copper alloy containing chromium is heat-treated at a temperature below the eutectic temperature of copper and chromium (about 1070 ° C), the supersaturated solid solution chromium precipitates from the parent phase as a chromium phase. Therefore, it is considered that the electrical conductivity of the copper alloy is improved. However, when a copper alloy containing chromium is heat-treated at about 500 ° C or higher, the chromium phase precipitates coarsely, and the number density decreases, which is presumed to reduce the mechanical strength (hardness) of the copper alloy. In the present invention, among elements that are difficult to dissolve in copper like chromium, vanadium and lanthanum, which precipitate more finely than chromium, are focused on, and by including these elements in the copper alloy in a predetermined ratio in addition to chromium, it is considered that even when subjected to heat treatment at 500 ° C or higher, a fine vanadium phase and an intermetallic compound phase of lanthanum and copper are precipitated in addition to the chromium phase, thereby suppressing the decrease in strength. Therefore, it is expected that the layered object obtained by the manufacturing method of the present invention will maintain its mechanical strength even after heat treatment and have excellent heat resistance.

[0016] The content of chromium contained in the copper alloy powder is preferably 0.5% by mass or more and 5.0% by mass or less, more preferably 0.5% by mass or more and 3.1% by mass or less, and even more preferably 0.5% by mass or more and 2.5% by mass or less. The content of chromium contained in the copper alloy powder can be measured by ICP emission spectrometry (inductively coupled plasma emission spectrometry) in accordance with JIS H 1071 (method for determining chromium in copper and copper alloys). Specifically, a melt is first prepared by alkali melting treatment of the copper alloy, and a solution is prepared by acid dissolution treatment of the melt. The solution is diluted to prepare a measurement sample. Alternatively, a solution may be directly prepared by acid dissolution treatment of the copper alloy. The solution is diluted to prepare a measurement sample.

[0017] The vanadium and / or lanthanum content in the copper alloy powder is preferably 0.1 mass% or more and 5.0 mass% or less, and more preferably 0.2 mass% or more and 4.0 mass% or less. The vanadium and / or lanthanum content in the copper alloy powder can be measured by ICP emission spectrometry in the same manner as in accordance with JIS H 1071.

[0018] The mixing ratio of chromium and vanadium and / or lanthanum added to copper is preferably such that the ratio of the chromium content to the total content of chromium, vanadium, and lanthanum is 5 mass% or more and 99 mass% or less, and more preferably 5 mass% or more and 95 mass% or less.

[0019] The copper content in the copper alloy powder is preferably 85% by mass or more and 99.5% by mass or less, and more preferably 90% by mass or more and 99% by mass or less. The copper content in the copper alloy powder can be measured by ICP emission spectrometry in accordance with JIS H 1051 (Method for determining copper in copper and copper alloys).

[0020] The copper alloy powder of the present invention may contain inevitable impurity elements other than the above-mentioned components, or may contain elements intentionally added during the production of the copper alloy powder. For example, inevitable impurity elements such as oxygen, phosphorus, and iron, and elements such as nickel, zinc, tin, silver, beryllium, zirconium, aluminum, silicon, cobalt, titanium, magnesium, and tellurium may be contained. Even when these elements are contained, the contents of each element of copper, chromium, vanadium, and / or lanthanum must be within the above-mentioned range.

[0021] The shape of each particle constituting the copper alloy powder is not particularly limited, but when used in a metal additive manufacturing method such as the L-PBF method, from the viewpoint of forming a powder bed with a high packing density of the copper alloy powder by squeegeeing, it is preferable that each particle has a shape close to a sphere. Therefore, it is preferable to use a copper alloy powder obtained by an atomization method. The atomization method includes a gas atomization method and a water atomization method, and from the viewpoint of making each particle closer to a sphere, the gas atomization method is preferable. According to the high-pressure gas atomization method, it is possible to obtain a copper alloy powder having a particle shape that is more uniform and closer to a sphere. Specifically, first, a molten copper alloy prepared to have the above-mentioned composition is dropped from a tundish, and the molten copper being dropped is brought into contact with a high-pressure gas. As a result, the molten copper is rapidly cooled and solidified, and the copper alloy powder can be produced.

[0022] The copper alloy powder obtained as described above can be classified as necessary to make the particle size uniform. This classification can be easily carried out by separating coarse powder and fine powder from the obtained copper alloy powder using an appropriate classification device so as to obtain a powder with a target average particle size.

[0023] From the viewpoint of obtaining a fine and dense additive manufacturing product and from the viewpoint of the fluidity of the copper alloy powder, the average particle size of the copper alloy powder used is preferably 1 μm or more and 500 μm or less, more preferably 5 μm or more and 200 μm or less, and particularly preferably 10 μm or more and 100 μm or less. By using a copper alloy powder having an average particle size within the above range, a powder bed with high packing density can be formed in a metal additive manufacturing method such as the L-PBF method, and the relative density of the molded product obtained by sintering or melting and solidifying the copper alloy powder can also be increased. In this specification, the average particle size refers to the particle size (D 50 ) is shown.

[0024] [Manufacturing method for laminated objects] Next, a method for manufacturing an additive manufacturing object using the copper alloy powder will be described. The additive manufacturing object can be manufactured by forming a powder layer containing copper alloy powder (first step), solidifying the copper alloy powder at a predetermined position in the powder layer to form a modeling layer (second step), and sequentially repeating the first step and the second step to stack the modeling layers. Hereinafter, a specific embodiment will be described with reference to the drawings. Note that, as a means for solidifying the metal powder, an embodiment using a laser in the powder bed fusion method will be described. However, the means is not limited to a laser as long as the metal powder can be solidified. The means may be, for example, an electron beam, plasma, or the like. In this embodiment, an additive manufacturing method (AM) other than the powder bed fusion method may be used. In this embodiment, for example, a directed energy deposition method, a binder jet method, a fused deposition modeling method, a cold spray method, or the like may be used. Furthermore, in this embodiment, cutting may be performed during modeling.

[0025] 1 shows an example of three-dimensional shape data. For example, the three-dimensional shape data can be created by a 3D scanner, etc. The three-dimensional shape data is, so to speak, a design drawing of a layered object.

[0026] 2 is an example of slice data. The slice data is created by slicing the three-dimensional shape data at a predetermined interval (t). The slice interval may also be referred to as a slice thickness. The slice data is, so to speak, a design drawing of a modeling layer.

[0027] 3 is a first schematic diagram showing a manufacturing process of an additive manufacturing object. An additive manufacturing apparatus 100 is prepared. The additive manufacturing apparatus 100 may also be called a "3D printer" or the like. The additive manufacturing apparatus 100 includes a piston 101, a table 102, and an output unit 103. The piston 101 supports the table 102. The piston 101 can move up and down.

[0028] The piston 101 lowers the table 102. The amount of descent corresponds to one layer of slice data. Copper alloy powder is laid on the table 102. This forms a powder bed 1. The surface of the powder bed 1 may be smoothed, for example, by a squeegee (not shown). The powder bed 1 contains copper alloy powder. For example, the powder bed 1 may consist essentially of copper alloy powder.

[0029] FIG. 4 is a second schematic diagram showing the manufacturing process of an additive manufacturing object. The output unit 103 irradiates the powder bed 1 (copper alloy powder) with an energy beam. The energy beam is scanned in a predetermined pattern within the powder bed 1. The scanning pattern follows the slice data. The copper alloy powder irradiated with the energy beam melts and then rapidly cools and solidifies or sinters. That is, the copper alloy powder irradiated with the energy beam solidifies. A modeling layer 2 is formed according to the scanning pattern of the energy beam. The modeling layer 2 may also be called a solidified layer, solidified layer, sintered layer, unit layer, etc. Note that "solidification" refers to the loss of fluidity of the metal particle group as a result of the metal particle group fusing and becoming one.

[0030] The energy beam may include, for example, at least one selected from the group consisting of a laser, an electron beam, and plasma. The energy beam may include, for example, at least one selected from the group consisting of a Yb fiber laser, a YAG laser, a CO2 laser, a semiconductor laser, a blue laser, and a green laser. The output of the energy beam may be, for example, 20 to 10,000 W. The scanning speed of the energy beam may be, for example, 50 to 10,000 mm / s. The energy density of the energy beam may be, for example, 10 to 2,000 J / mm 3 may be also possible.

[0031] 5 is a third schematic diagram showing the manufacturing process of a layered object. After the formation of the modeling layer 2 (first layer), the piston 101 again lowers the table 102. The amount of descent corresponds to one layer of the slice data. Similarly to the above, the modeling layer 2 (second layer) is further formed.

[0032] 6 is a fourth schematic diagram showing the manufacturing process of a layered object. The layered object 10 can be constructed by repeatedly forming the modeling layer 2. That is, the layered object 10 can be manufactured by stacking a plurality of modeling layers 2.

[0033] For example, the layered object may be manufactured in an inert gas atmosphere. By manufacturing the layered object in an inert gas atmosphere, it is expected that oxidation of the layered object is suppressed. The inert gas may contain at least one gas selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He). For example, the layered object may be manufactured in a reducing gas atmosphere. The reducing gas may contain hydrogen (H2), etc. For example, the layered object may be manufactured in a reduced pressure atmosphere.

[0034] The additive manufacturing product produced as described above contains the same composition as the copper alloy powder, i.e., 0.1% by mass or more and 20.0% by mass or less of chromium, 0.1% by mass or more and 5.0% by mass or less of vanadium and / or lanthanum, and 75.0% by mass or more and 99.8% by mass or less of copper.

[0035] The electrical conductivity of the layered product obtained as described above is improved by subjecting it to heat treatment. In the present invention, the layered product is made of copper alloy powder containing a specific element in a specific ratio in addition to a specific amount of chromium, and the copper alloy molded product obtained by subjecting it to heat treatment at 500°C or higher has excellent electrical conductivity while maintaining mechanical strength. The heat treatment can be performed using a heat treatment furnace or the like. The heat treatment temperature can be measured by a temperature sensor or the like attached to the heat treatment furnace. For example, if the set temperature of the heat treatment furnace is 300°C, the heat treatment temperature can be considered to be 300°C.

[0036] The heat treatment needs to be performed at a temperature below the melting point of the copper alloy, but may be, for example, 800°C or lower. By setting the heat treatment temperature at 800°C or lower, improvement of mechanical strength is expected. The heat treatment temperature is more preferably 700°C or lower, and more preferably 600°C or lower. On the other hand, from the viewpoint of improving electrical conductivity and mechanical strength, the lower limit of the heat treatment temperature is preferably 500°C or higher. The heat treatment temperature may be changed during the heat treatment process. For example, the temperature may be raised from room temperature to 700°C, held at 700°C for 1 hour, lowered from 700°C to 500°C, held at 500°C for 5 hours, and lowered from 500°C to room temperature.

[0037] The heat treatment time may be, for example, 0.1 to 100 hours, 0.5 to 50 hours, or 1 to 40 hours. The atmosphere in the heat treatment furnace may be, for example, an air atmosphere, a nitrogen atmosphere, an argon atmosphere, a hydrogen atmosphere, a reduced pressure atmosphere, or the like.

[0038] The copper alloy molded product obtained by heat-treating the additive manufacturing product may have, for example, a conductivity of 30% IACS or more. It preferably has a conductivity of 40% IACS or more, and more preferably has a conductivity of 50% IACS or more. On the other hand, the additive manufacturing product before heat treatment may have a conductivity of, for example, 8 to 25% IACS. Note that the "conductivity" is the IACS conductivity. In other words, the conductivity of annealed standard soft copper (International Annealed Copper Standard, IACS) is defined as 100% IACS. The conductivity is measured by an eddy current conductivity meter. The measurement temperature is room temperature (15 to 25°C).

[0039] The copper alloy molded product obtained by heat-treating the layered product may have a Vickers hardness of 60 HV or more, preferably 80 HV or more, more preferably 89 HV or more, and even more preferably 100 HV or more. The Vickers hardness (HV) is a value measured in accordance with JIS Z 2244.

[0040] The copper alloy molded product obtained by heat-treating the additive manufacturing product may have any shape. For example, it may have a seamless and complex internal structure. For example, it is considered difficult to form a seamless and complex internal structure by cutting processing.

[0041] The additively manufactured object and the copper alloy molded object are made of a copper alloy. The copper alloy may have high electrical conductivity and high thermal conductivity. The additively manufactured object may be applied to an application in which the properties of the copper alloy are utilized. The additively manufactured object may be applied to, for example, an induction heating coil, a heat sink, a rocket engine, etc. In the additively manufactured object, a complex water cooling path (internal structure) or the like may be realized without any joints.

[0042] The above-mentioned layered product and copper alloy molded product may have a relative density of, for example, 97 to 100%. The layered product and copper alloy molded product according to an embodiment of the present invention may have a relative density of, for example, 99% or more. The relative density of the copper alloy molded product may be substantially the same as the relative density of the layered product before the heat treatment. The relative density is expressed as a percentage of the measured density with respect to the theoretical density. Here, the "theoretical density" is defined as the density of an ingot material having substantially the same alloy composition as the alloy composition of the measurement target (layered product). The measured density may be measured in accordance with "JIS Z 2501 Sintered metal material-Density, oil content and open porosity test method". When measuring the measured density, water is used as a replacement liquid. EXAMPLES

[0043] Next, the embodiments of the present invention will be described in detail with reference to the following examples, but the present invention is not limited to these examples.

[0044] <Preparation of copper alloy powder> Twelve types of copper alloy powder samples with different compositions were prepared by atomization. The alloy composition of each sample is shown in Table 1 below. In each sample, the remainder after removing alloying elements and unavoidable impurities was Cu. The copper alloy powder of each sample had an average particle size (D 50 )

[0045] <Manufacturing of additively manufactured objects> An "EOSINT M280 (manufactured by EOS)" was used as the additive manufacturing device, and additive manufacturing objects were manufactured under the following conditions. Manufacturing conditions: Energy beam: Fiber laser, maximum output 400W Spot diameter: 0.05~0.20mm Scanning speed: 50~2000mm / s Layer pitch: 0.02~0.1mm Model size: 250mm x 250mm x 280mm

[0046] A cylindrical test piece (diameter 14 mm x height 15 mm) was manufactured as an additive manufacturing object.

[0047] <Heat treatment of additive manufacturing products> Each test piece obtained as described above was placed in a heat treatment furnace and heat-treated at a temperature of 600° C. for 1 hour. In addition, each test piece was placed in a heat treatment furnace and heat-treated at a temperature of 700° C. for 1 hour.

[0048] For the test pieces heat-treated at each temperature, the Vickers hardness was measured in accordance with JIS Z 2244, and the electrical conductivity was measured using an eddy current type electrical conductivity meter.

[0049] [Table 1] [Explanation of symbols]

[0050] 1 powder bed 2 Build layer 10 Additive manufacturing 100 Additive manufacturing equipment 101 Piston 102 Table 103 Output section

Claims

1. A copper alloy powder for additive manufacturing, comprising: 0.1% by mass or more and 20.0% by mass or less of chromium; 0.1% by mass or more and 5.0% by mass or less of vanadium and / or lanthanum, 75.0% by mass or more and 99.8% by mass or less of copper; A copper alloy powder containing

2. The copper alloy powder according to claim 1, containing 0.5% by mass or more and 5.0% by mass or less of chromium.

3. 2. The copper alloy powder according to claim 1, wherein the ratio of the content of chromium to the total content of chromium, vanadium, and lanthanum is 5 mass% or more and 99 mass% or less.

4. A method for manufacturing an additive manufacturing object using the copper alloy powder according to claim 1, A first step of forming a powder layer containing the copper alloy powder; A second step of forming a modeling layer by solidifying the copper alloy powder at a predetermined position in the powder layer, A method for manufacturing a layered object, comprising sequentially repeating the first step and the second step to stack the modeling layers to manufacture a layered object.

5. The method according to claim 4 , further comprising a heat treatment step of heat treating the additively shaped object.

6. The method according to claim 5 , wherein the heat treatment temperature in the heat treatment is 800° C. or less.

7. The method according to claim 5 , wherein the heat treatment temperature in the heat treatment is 700° C. or less.

8. The method according to claim 5 , wherein the heat treatment temperature is 500° C. or more and 600° C. or less.

9. An additive manufacturing object made of a copper alloy, 0.1% by mass or more and 20.0% by mass or less of chromium; 0.1% by mass or more and 5.0% by mass or less of vanadium and / or lanthanum, 75.0% by mass or more and 99.8% by mass or less of copper; An additive manufacturing object comprising:

10. The layered object according to claim 9 , containing 0.5% by mass or more and 5.0% by mass or less of chromium.

11. A method for producing a copper alloy molded product comprising the layered product according to claim 9 or 10, and heat treating the laminated structure.

12. A copper alloy molded product comprising the layered product according to claim 9 or 10, A copper alloy molding having an electrical conductivity of 30% IACS or more and a Vickers hardness of 60 HV or more.

13. A copper alloy molded product comprising the layered product according to claim 9 or 10, A copper alloy molding having an electrical conductivity of 40% IACS or more and a Vickers hardness of 60 HV or more.

14. A copper alloy molded product comprising the layered product according to claim 9 or 10, A copper alloy molding having an electrical conductivity of 50% IACS or more and a Vickers hardness of 60 HV or more.

Citation Information

Patent Citations

  • Copper alloy powder, heat treatment method for multilayer shaped structure, method for producing copper alloy shaped structure, and copper alloy shaped structure

    JP2019070169A