Resin composition and molded body
A resin composition combining 4-methyl-1-pentene/α-olefin copolymer, inorganic filler, and thermoplastic elastomer addresses the challenge of flexibility and impact resistance in molded products, achieving a soft and heavy feel with high tanδ peak values and stress relaxation properties.
Patent Information
- Application Number
- JP2024120934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-01-25
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-01-20
AI Technical Summary
Existing resin compositions containing thermoplastic resins and inorganic fillers struggle to achieve a balance between flexibility, impact resistance, and moldability, often resulting in hard and inflexible molded products with poor viscoelastic properties.
A resin composition comprising 4-methyl-1-pentene/α-olefin copolymer, inorganic filler, and a thermoplastic elastomer, specifically formulated to have a tanδ peak value of 0.6 to 5.0 and a density of 1.0 to 5.0 g/cm³, ensuring a soft and heavy feel with high stress relaxation properties.
The composition allows for easy molding of products with a soft and heavy feel, exhibiting high tanδ peak values and excellent stress relaxation properties, suitable for daily goods and toys.
Smart Images

Figure 2024156761000001 
Figure 2024156761000002 
Figure 2024156761000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a molded article, more particularly to a resin composition containing a thermoplastic resin and an inorganic filler, and a molded article and uses thereof. [Background technology]
[0002] Among thermoplastic resins, polyolefins have been widely used in daily necessities. They can be mass-produced by injection molding, have a low specific gravity, and have excellent mechanical strength, gloss, colorability, chemical resistance, recyclability, and other various features. However, thin-walled molded bodies may be easily damaged by impact loads. For example, if a rib structure is provided as the shape of the molded body, it can exhibit an impact load buffering effect and prevent damage, but if the shape is such that it is difficult to provide a rib structure, a molding material filled with inorganic filler may be used to improve impact strength.
[0003] Polyolefins have been widely used in toys for a long time. Even for toys with thin walls, molding materials filled with inorganic fillers are used to improve impact resistance, just like everyday items. Such molding materials tend to be hard, and for example, young children who often have the opportunity to handle toys may get bored of playing with them because the hard feel means that the shape is not easily changed.
[0004] On the other hand, styrene-based thermoplastic elastomers are used in daily necessities and toys because of their elasticity similar to that of rubber materials. For example, styrene-ethylene-butylene-styrene copolymer (styrene-ethylene-butene-styrene block copolymer) (SEBS) has a structural unit in which a hard polystyrene part (hard segment) and a soft polybutylene part (soft segment) are copolymerized in a block shape. It is known that the terminal blocks of polystyrene form a structure (domain) in which they are aggregated with each other, and these polystyrene domains become pseudo-crosslinking points and exhibit elasticity similar to that of rubber materials. However, it is also a resin with strong self-adhesiveness (tackiness), and for example, during injection molding, the molded body sticks to the mold, making it difficult to mass-produce. To suppress the self-adhesiveness, molding materials containing crystalline polyolefins or inorganic fillers are used. However, these molding materials tend to be unable to maintain flexibility and tend to produce hard molded bodies.
[0005] Patent Document 1 discloses synthetic paper made of a resin composition containing inorganic mineral powder and polyethylene. Furthermore, Patent Document 2 and Patent Document 3 disclose sheet molded bodies made of resin compositions containing specific inorganic fillers and polyolefins. Of these, Patent Document 2 discloses a resin composition containing equal amounts of polypropylene resin and calcium carbonate, and a sheet made of the resin composition. Here, Patent Document 2 also discloses that polyethylene resin can be used instead of polypropylene resin. Furthermore, Patent Document 3 discloses a resin composition containing a crystalline polymer such as polypropylene resin or polyethylene resin and inorganic fine powder, and a sheet made of the resin composition. Here, Patent Document 3 specifically discloses a resin composition containing a propylene homopolymer, calcium carbonate, and a small amount of magnesium stearate as an example of such a resin composition. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-071378 A [Patent Document 2] JP 2003-026866 A [Patent Document 3] WO2018 / 092494 issue Summary of the Invention [Problem to be solved by the invention]
[0007] The loss factor is an index used to evaluate the viscoelasticity of materials such as elastomers when they deform. This loss factor is a numerical value expressed as the ratio (G" / G') of the loss modulus (G") to the storage modulus (G'), and is known as tan δ. Materials with a large tan δ tend to have a soft feel when molded into a product.
[0008] The resin composition of Patent Document 1 can be used as synthetic paper and has excellent foldability and tearability. However, it does not exhibit a high tan δ peak value and is a material with poor flexibility. It has been proposed that the resin compositions of Patent Documents 2 and 3 have good moldability even though they contain a large amount of inorganic filler. It is presumed that the stickiness of the molded body surface is eliminated. However, since they contain a large amount of inorganic filler, the molded body obtained is hard. Therefore, flexibility tends to be lost, and it is difficult to express a high tan δ peak value in the first place.
[0009] Therefore, an object of the present invention is to provide a resin composition which can be easily molded, and which is flexible and has a heavy feel, and which is made of a thermoplastic resin and an inorganic filler, and to provide a molded article. [Means for solving the problem]
[0010] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by using a resin composition containing a 4-methyl-1-pentene / α-olefin copolymer (A), an inorganic filler (B), and a specific thermoplastic elastomer (C) in a specific blending ratio, and have thus completed the present invention.
[0011] That is, the present invention relates to, for example, the following items [1] to [9]. [1] 15 to 50 parts by mass of a 4-methyl-1-pentene / α-olefin copolymer (A) satisfying at least one of the following requirements (d) and (e); 10 to 50 parts by mass of an inorganic filler (B); Thermoplastic elastomer (C) 5 to 49 parts by mass (the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C) is taken as 100 parts by mass); Including, The thermoplastic elastomer (C) is at least one selected from the group consisting of an olefin-based thermoplastic elastomer (C1) and a styrene-based thermoplastic elastomer (C2), and A resin composition characterized by satisfying the following requirements (a) to (c):
[0012] (a) In the temperature range of -40 to 150°C, the temperature at which the loss tangent tanδ value obtained by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) is maximized (hereinafter also referred to as tanδ peak temperature) is 0°C or higher and 60°C or lower.
[0013] (b) The maximum value of loss tangent tan δ (hereinafter also referred to as peak tan δ value) obtained by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C. is 0.6 or more and 5.0 or less.
[0014] (c) Density is 1.0 g / cm 3 More than 5.0g / cm 3 The following is the result. (d) Consists of 55 to 90 mol % of structural units derived from 4-methyl-1-pentene and 10 to 45 mol % of structural units derived from an α-olefin having 2 to 4 carbon atoms (the total of structural units derived from 4-methyl-1-pentene and structural units derived from an α-olefin having 2 to 4 carbon atoms is 100 mol %).
[0015] (e) The melting point as measured by differential scanning calorimetry (DSC) is 160°C or lower, or no melting point is observed. [2] The resin composition according to [1], wherein the 4-methyl-1-pentene·α-olefin copolymer (A) satisfies the following requirements (f) and (g):
[0016] (f) The tan δ peak temperature determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C is 15°C or more and 45°C or less. (g) The tan δ peak value determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C is 0.6 or more and 5.0 or less.
[0017] [3] The resin composition according to any one of [1] to [2], wherein the inorganic filler (B) is at least one selected from the group consisting of calcium carbonate, magnesium sulfate, barium sulfate, magnesium oxide, and talc.
[0018] [4] The inorganic filler (B) has an average particle size of 0.01 to 100 μm. The resin composition according to any one of [1] to [3].
[0019] [5] A molded article made of the resin composition according to any one of [1] to [4]. [6]
[0021] [1]-[4] are used as daily necessities comprising the resin composition according to any one of the above items.
[0020] [7] A toy made of the resin composition according to any one of [1] to [4]. [8] An ear insert made of the resin composition according to any one of [1] to [4].
[0021] [9] A sheet made of the resin composition according to any one of [1] to [4]. Effect of the Invention
[0022] According to the present invention, it is possible to provide a resin composition which can be easily molded, exhibits a high tan δ peak value, and has flexibility and a heavy feel, and a molded article. The molded article made of the resin composition of the present invention can provide, for example, daily necessities and toys that have high stress relaxation properties, shape retention in which the original shape is slowly restored after elastic deformation, and flexibility and a heavy feel, as well as components for wearable devices such as ear inserts. Therefore, the molded article obtained by the present invention is suitable as, for example, toys, daily necessities, and ear inserts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Specific embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be practiced with appropriate modifications within the scope of the object of the present invention. In this specification, the terms "polymer" and "(co)polymer" are used to include homopolymers and copolymers unless otherwise specified.
[0024] <Resin composition> The resin composition of the present invention contains a 4-methyl-1-pentene·α-olefin copolymer (A), an inorganic filler (B), and a thermoplastic elastomer (C).
[0025] Specifically, it contains 15 to 50 parts by mass of 4-methyl-1-pentene·α-olefin copolymer (A), 10 to 50 parts by mass of inorganic filler (B), and 5 to 49 parts by mass of thermoplastic elastomer (C). The total amount of 4-methyl-1-pentene·α-olefin copolymer (A), inorganic filler (B), and thermoplastic elastomer (C) is 100 parts by mass. In the present invention, the thermoplastic elastomer (C) is at least one selected from the group consisting of olefin-based thermoplastic elastomers (C1) and styrene-based thermoplastic elastomers (C2).
[0026] In a typical and preferred embodiment of the present invention, the resin composition of the present invention contains only one of the olefin-based thermoplastic elastomer (C1) and the styrene-based thermoplastic elastomer (C2) as the thermoplastic elastomer (C). In this embodiment, the amount of either the olefin-based thermoplastic elastomer (C1) or the styrene-based thermoplastic elastomer (C2) is 0 parts by mass.
[0027] In the case of a resin composition that does not contain a styrene-based thermoplastic elastomer (C2), the standard of 100 parts by mass is the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the olefin-based thermoplastic elastomer (C1). In other words, in such a resin composition, the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the olefin-based thermoplastic elastomer (C1) is taken as 100 parts by mass, 4-methyl-1-pentene / α-olefin copolymer (A): 15 to 50 parts by mass, Inorganic filler (B): 10 to 50 parts by mass; Olefin-based thermoplastic elastomer (C1): 5 to 49 parts by mass but does not include styrene-based thermoplastic elastomer (C2).
[0028] In the case of a resin composition that does not contain an olefin-based thermoplastic elastomer (C1), the standard of 100 parts by mass is the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the styrene-based thermoplastic elastomer (C2). In other words, in such a resin composition, the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the styrene-based thermoplastic elastomer (C2) is taken as 100 parts by mass, 4-methyl-1-pentene / α-olefin copolymer (A): 15 to 50 parts by mass, Inorganic filler (B): 10 to 50 parts by mass; Styrene-based thermoplastic elastomer (C2): 5 to 49 parts by mass but does not include olefin-based thermoplastic elastomer (C1).
[0029] The resin composition of the present invention satisfies all of the following requirements (a) to (c). Requirement(a) The resin composition of the present invention has a temperature (hereinafter also referred to as "tan δ peak temperature") at which the loss tangent tan δ value obtained by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) is maximum in a temperature range of -40 to 150°C. Here, the lower limit of the tan δ peak temperature is preferably 2°C or more, more preferably 4°C or more. In addition, the upper limit of the tan δ peak temperature is preferably 55°C or less, more preferably 50°C or less, and particularly preferably 45°C or less. By adjusting the tan δ peak temperature to the above temperature range, the molded product can exhibit high stress relaxation properties in a wide range of environmental temperatures.
[0030] Requirement (b) The resin composition of the present invention has a maximum value of loss tangent tan δ (hereinafter also referred to as "tan δ peak value") of 0.6 or more and 5.0 or less, as determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C. This tan δ peak value is preferably 0.6 or more and 4.5 or less, more preferably 0.6 or more and 4.0 or less, and particularly preferably 0.6 or more and 3.5 or less. By adjusting the tan δ peak value within the above range, the obtained molded article has excellent stress relaxation properties and can slowly recover to its original shape after elastic deformation.
[0031] The loss tangent tan δ can be calculated as the ratio (G″ / G′) of the storage modulus (G′) to the loss modulus (G”) measured by dynamic viscoelasticity. In the present invention, the loss tangent tanδ is determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C, and the temperature at which the loss tangent tanδ is maximum in this temperature range is defined as the above-mentioned tanδ peak temperature, and the value of the loss tangent tanδ at that time is defined as the tanδ peak value. The above-mentioned tanδ peak temperature is considered to be due to the glass transition temperature of the resin composition. Details of the measurement method are as described in the examples below.
[0032] Requirement(c) The resin composition of the present invention has a density of 1.0 g / cm 3 More than 5.0g / cm 3 Regarding the lower limit of the density of the resin composition, the density is 1.05 g / cm 3 It is preferable that the content is 1.1 g / cm or more. 3 The upper limit of the density of the resin composition is preferably 4.0 g / cm or more. 3 It is preferable that the density is 3.5 g / cm or less. 3It is more preferable that the density of the resin composition is within the above range, since a weighty feeling can be obtained when the resin composition is molded into a molded product. For example, when the resin composition is used for daily necessities, stability can be expected when the resin composition is placed on a desk or table. Details of the method for measuring the density are as described in the Examples below.
[0033] Furthermore, when the resin composition of the present invention is formed into a sheet-like molded article, the lower limit of the Shore A hardness 15 seconds after the start of indenter contact (measured in accordance with ASTM D2244, with three molded articles each having a thickness of 2 mm stacked on top of each other) is preferably 10, more preferably 20, and even more preferably 30. On the other hand, the upper limit of the Shore A hardness 15 seconds after the start of indenter contact is preferably 95, more preferably 92, and even more preferably 88. The method for producing the molded article is as shown in the Examples.
[0034] When the resin composition of the present invention is molded into a sheet-like article, the lower limit of the change in Shore A hardness (measured in accordance with ASTM D2244, with three 2 mm-thick molded articles stacked together) ΔHS defined by the following formula is preferably 5, more preferably 10, and even more preferably 15. On the other hand, the upper limit of ΔHS is preferably 60, more preferably 50, and even more preferably 40.
[0035] ΔHS = (Shore A hardness value immediately after the indenter starts contacting the material - Shore A hardness value 15 seconds after the indenter starts contacting the material) The ΔHS can be changed arbitrarily by the 4-methyl-1-pentene·α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C) that constitute the resin composition, and when the ΔHS is within the above range, the flexibility is excellent.
[0036] If it is difficult to measure the Shore A hardness, the same evaluation can be performed using the Shore D hardness instead. In this case, instead of the above ΔHS, the evaluation can be performed using the value of the change ΔHS' in the Shore D hardness (measured in accordance with ASTM D2244, with three 2 mm thick molded bodies stacked together) defined by the following formula:
[0037] ΔHS' = (Shore D hardness value immediately after the indenter starts contacting the specimen - Shore D hardness value 15 seconds after the indenter starts contacting the specimen) In this case, the lower limit of ΔHS' is preferably 5, more preferably 8, and even more preferably 11. On the other hand, the upper limit of ΔHS' is preferably 60, more preferably 50, and even more preferably 40. Like the above ΔHS, this ΔHS' can also be changed arbitrarily by the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C), and when ΔHS' is within the above range, excellent flexibility is achieved.
[0038] <4-Methyl-1-pentene / α-olefin copolymer (A)> The 4-methyl-1-pentene·α-olefin copolymer (A) contained in the resin composition of the present invention is not limited, but preferably satisfies one or more of the following requirements (d) to (g), more preferably two or more, even more preferably three or more, and particularly preferably all of them. In a typical embodiment of the present invention, the 4-methyl-1-pentene·α-olefin copolymer (A) satisfies at least one of the requirements (d) and (e). That is, the 4-methyl-1-pentene·α-olefin copolymer (A) may satisfy only the requirement (d), may satisfy only the requirement (e), or may satisfy both the requirements (d) and (e). In this embodiment, the 4-methyl-1-pentene·α-olefin copolymer (A) further satisfies, in addition to the requirements (d) and / or (e), preferably either one of the requirements (f) and (g), particularly preferably both the requirements (f) and (g).
[0039] Requirement(d) It is composed of 55 to 90 mol % of structural units derived from 4-methyl-1-pentene (hereinafter sometimes referred to as "structural units (i)") and 10 to 45 mol % of structural units derived from an α-olefin having 2 to 4 carbon atoms (hereinafter sometimes referred to as "structural units (ii)") (the total of structural units (i) and structural units (ii) being 100 mol %).
[0040] Requirement(e) The melting point as measured by differential scanning calorimetry (DSC) is 160° C. or less, or no melting point is observed.
[0041] Requirement(f) The tan δ peak temperature determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C is 15°C or higher and 45°C or lower.
[0042] Requirements(g) The tan δ peak value determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C is 0.6 or more and 5.0 or less.
[0043] The above requirement (d) specifies that the 4-methyl-1-pentene / α-olefin copolymer (A) contains a specific ratio of structural units (i) derived from 4-methyl-1-pentene and structural units (ii) derived from an α-olefin having 2 to 4 carbon atoms.
[0044] In this specification, a structural unit derived from an α-olefin refers to a structural unit corresponding to an α-olefin, i.e., a structural unit represented by -CH2-CHR- (wherein R is a hydrogen atom or an alkyl group). The structural unit (i) derived from 4-methyl-1-pentene can be interpreted in the same way, and refers to a structural unit corresponding to 4-methyl-1-pentene (i.e., a structural unit represented by -CH2-CH(-CH2CH(CH3)2)-).
[0045] In the 4-methyl-1-pentene-α-olefin copolymer (A), the lower limit of the amount of structural units derived from 4-methyl-1-pentene is 55 mol%, preferably 60 mol%, more preferably 68 mol%, while the upper limit of the amount of structural units derived from 4-methyl-1-pentene is 90 mol%, preferably 86 mol%, more preferably 85 mol%, and even more preferably 84 mol%.
[0046] In the 4-methyl-1-pentene-α-olefin copolymer (A), if the amount of the structural unit (i) derived from 4-methyl-1-pentene is equal to or greater than the lower limit above, the tan δ peak temperature measured by dynamic viscoelasticity is near room temperature, making it easy to adjust the tan δ peak temperature of the resin composition to within the aforementioned range. On the other hand, if the amount of the structural unit (i) derived from 4-methyl-1-pentene is equal to or less than the upper limit above, the relaxation property at room temperature increases, improving the fit of the molded article.
[0047] Therefore, in the 4-methyl-1-pentene·α-olefin copolymer (A), the upper limit of the amount of the structural unit (ii) derived from an α-olefin having 2 to 4 carbon atoms is 45 mol %, preferably 40 mol %, more preferably 32 mol %.
[0048] On the other hand, the lower limit of the amount of the structural unit (ii) derived from an α-olefin having 2 to 4 carbon atoms is 10 mol%, preferably 14 mol%, more preferably 15 mol%, and even more preferably 16 mol%.
[0049] The content (mol %) of each of the structural units constituting the 4-methyl-1-pentene / α-olefin copolymer (A) is 13 The measurement is performed by C-NMR. Details of the measurement method are as described in the Examples below.
[0050] Thus, the 4-methyl-1-pentene-α-olefin copolymer (A) used in the present invention contains an α-olefin having 2 to 4 carbon atoms as the α-olefin. In the resin composition of the present invention containing such a 4-methyl-1-pentene-α-olefin copolymer (A), the crystallinity is lower and a softer composition is obtained compared to a resin composition containing a 4-methyl-1-pentene-α-olefin copolymer consisting of 4-methyl-1-pentene and an α-olefin having a larger number of carbon atoms. Specific examples of the α-olefin having 2 to 4 carbon atoms include ethylene, propylene, and 1-butene, and among these, propylene is particularly preferred. The structural unit (ii) may be derived from one of these compounds or from two or more compounds.
[0051] By selecting propylene as the α-olefin having 2 to 4 carbon atoms, uniform and good kneadability of the inorganic filler (B) and the thermoplastic elastomer (C) can be obtained, and a molded article made of the resin composition is likely to have flexibility. The inorganic filler (B) and the thermoplastic elastomer (C) used in the present invention will be described in detail later in the sections "Inorganic filler (B)" and "Thermoplastic elastomer (C)", respectively.
[0052] In a typical embodiment of the present invention, the 4-methyl-1-pentene·α-olefin copolymer (A) constituting the resin composition of the present invention is composed only of the structural units (i) and (ii). That is, in this embodiment, the 4-methyl-1-pentene·α-olefin copolymer (A) is a copolymer of 4-methyl-1-pentene and an α-olefin having 2 to 4 carbon atoms.
[0053] Regarding the above requirement (e), the 4-methyl-1-pentene·α-olefin copolymer (A) has a melting point of 160° C. or less or no melting point is observed, preferably a melting point of 140° C. or less or no melting point is observed, and more preferably no melting point is observed, as measured by a differential scanning calorimeter (DSC).
[0054] By satisfying these requirements, in the resin composition of the present invention, good kneadability between the inorganic filler (B) and the thermoplastic elastomer (C) can be obtained, and the stress relaxation property can be improved.
[0055] Regarding the above requirement (f), the 4-methyl-1-pentene / α-olefin copolymer (A) has a tan δ peak temperature determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C. of 15° C. or more and 45° C. or less, preferably 20° C. or more and 45° C. or less, and more preferably 25° C. or more and 45° C. or less.
[0056] By setting the tan δ peak temperature within the above range, the stress relaxation properties can be more effectively exhibited at around room temperature. Regarding the above requirement (g), the 4-methyl-1-pentene / α-olefin copolymer (A) has a tan δ peak value determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C. of 0.6 to 5.0, preferably 1.0 to 5.0, more preferably 1.5 to 5.0, and even more preferably 2.0 to 4.0.
[0057] By setting the tan δ peak value within the above range, the material has excellent restoring property in which it gradually returns to its original shape in response to the tensile stress and the rate of deformation. The 4-methyl-1-pentene-α-olefin copolymer (A) preferably has an intrinsic viscosity [η] measured in decalin at 135° C. in the range of 0.1 to 5.0 dl / g. More preferably, it is 0.5 to 4.0 dl / g, and even more preferably, it is 1.0 to 3.5 dl / g. As described later, by using hydrogen in combination during polymerization, the molecular weight can be controlled, and low molecular weight to high molecular weight substances can be freely obtained, and the intrinsic viscosity [η] can be adjusted to the above range. Details of the measurement method are as described in the examples below.
[0058] The 4-methyl-1-pentene·α-olefin copolymer (A) has a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) in terms of polystyrene of preferably 1,000 to 1,000,000 or less, more preferably 5,000 to 800,000 or less, and even more preferably 10,000 to 500,000 or less. Details of the measurement method are as described in the examples below.
[0059] The 4-methyl-1-pentene·α-olefin copolymer (A) preferably has a molecular weight distribution (Mw / Mn), which is the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) measured by gel permeation chromatography (GPC), in the range of 1.0 to 3.5, more preferably 1.2 to 3.0, and even more preferably 1.5 to 2.8 or less. When the molecular weight distribution (Mw / Mn) is 3.5 or less, the influence of low molecular weight and low stereoregular polymers derived from the composition distribution is small, and the mechanical strength of the obtained molded article is less likely to decrease, which is preferable.
[0060] The melt mass flow rate (MFR; based on ASTM D1238, temperature 230°C, load 2.16 kg) of the 4-methyl-1-pentene / α-olefin copolymer (A) is preferably 0.1 to 100 g / 10 min, more preferably 0.5 to 50 g / 10 min, and further preferably within the range of 1.0 to 30 g / 10 min.
[0061] When the melt mass flow rate (MFR) of the 4-methyl-1-pentene·α-olefin copolymer (A) is equal to or higher than the lower limit of the above range, good dispersibility of the inorganic filler (B) and the thermoplastic elastomer (C) can be obtained.
[0062] When it is equal to or less than the upper limit of the aforementioned range, the molecular weight of the resin is not too low, and a molded article having sufficient mechanical strength can be obtained, which is preferable. The density of the 4-methyl-1-pentene / α-olefin copolymer (A) is preferably 830 to 870 kg / m 3, more preferably 830 to 860 kg / m 3 , more preferably 830 to 850 kg / m 3 The density of the 4-methyl-1-pentene-α-olefin copolymer (A) can be appropriately changed by changing the comonomer composition ratio of the 4-methyl-1-pentene-α-olefin copolymer. The 4-methyl-1-pentene-α-olefin copolymer (A) having a density within the above range is advantageous because it has good kneadability with the inorganic filler (B) and can be uniformly and favorably dispersed in the thermoplastic elastomer (C), i.e., in both the olefin-based thermoplastic elastomer (C1) and the styrene-based thermoplastic elastomer (C2).
[0063] The amount of 4-methyl-1-pentene·α-olefin copolymer (A) added in the resin composition of the present invention is 15 to 50 parts by mass per 100 parts by mass of the total amount of 4-methyl-1-pentene·α-olefin copolymer (A), inorganic filler (B), and thermoplastic elastomer (C). The amount added is preferably a certain amount or more, more preferably 20 parts by mass or more, in order that a molded article made of the resin composition can exhibit a high tan δ peak value. On the other hand, the amount added is preferably a certain amount or less, more preferably 50 parts by mass or less, in order that a molded article made of the resin composition can have a heavy feel.
[0064] <Production method of 4-methyl-1-pentene / α-olefin copolymer (A)> The method for producing the 4-methyl-1-pentene / α-olefin copolymer (A) is not particularly limited. For example, the copolymer can be produced by polymerizing 4-methyl-1-pentene and the above-mentioned α-olefin having 2 to 4 carbon atoms in the presence of an appropriate polymerization catalyst such as a magnesium-supported titanium catalyst or a metallocene catalyst.
[0065] Suitable polymerization catalysts that can be used herein include conventionally known catalysts, such as magnesium-supported titanium catalysts, and metallocene catalysts described in WO 01 / 53369, WO 01 / 27124, JP 3-193796, or JP 2-41303, WO 2011 / 055803, WO 2014 / 050817, etc. Polymerization can be carried out by an appropriate method selected from liquid phase polymerization methods including solution polymerization and suspension polymerization, and gas phase polymerization methods.
[0066] In the liquid phase polymerization method, an inert hydrocarbon solvent can be used as the solvent that constitutes the liquid phase.Examples of the inert hydrocarbon include aliphatic hydrocarbons including propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, alicyclic hydrocarbons including cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane, aromatic hydrocarbons including benzene, toluene, and xylene, and halogenated hydrocarbons including ethylene chloride, chlorobenzene, dichloromethane, trichloromethane, and tetrachloromethane, and mixtures thereof.
[0067] In addition, in the liquid phase polymerization method, bulk polymerization can also be performed using the monomer corresponding to the structural unit (i) derived from the above-mentioned 4-methyl-1-pentene (i.e., 4-methyl-1-pentene) and the monomer corresponding to the structural unit (ii) derived from the above-mentioned α-olefin having 2 to 4 carbon atoms (i.e., the above-mentioned α-olefin having 2 to 4 carbon atoms) themselves as a solvent.
[0068] By stepwise copolymerizing the 4-methyl-1-pentene with the α-olefin having 2 to 4 carbon atoms, the composition distribution of the 4-methyl-1-pentene structural unit (i) and the α-olefin structural unit (ii) having 2 to 4 carbon atoms constituting the 4-methyl-1-pentene-α-olefin copolymer (A) can be appropriately controlled.
[0069] The polymerization temperature is preferably −50 to 200° C., more preferably 0 to 100° C., and further preferably 20 to 100° C. The polymerization pressure is preferably normal pressure to 10 MPa gauge pressure (i.e., normal pressure or higher (normal pressure + 10 MPa) or lower), and more preferably normal pressure to 5 MPa gauge pressure (i.e., normal pressure or higher (normal pressure + 5 MPa) or lower).
[0070] During polymerization, hydrogen may be added for the purpose of controlling the molecular weight and polymerization activity of the polymer produced. The amount of hydrogen added is appropriately about 0.001 to 100 NL per 1 kg of the total amount of the above-mentioned 4-methyl-1-pentene and the above-mentioned α-olefin having 2 to 4 carbon atoms.
[0071] <Inorganic filler (B)> The resin composition of the present invention contains, in addition to the 4-methyl-1-pentene / α-olefin copolymer (A), an inorganic filler (B). This inorganic filler (B) plays a role in imparting sufficient impact strength to the resin composition of the present invention and also imparting sufficient weight to the resin composition.
[0072] The inorganic filler (B) is not particularly limited as long as it is an inorganic compound, and known fillers can be used. For example, carbon black or carbon black surface-treated with graphite or a silane coupling agent, finely powdered silicic acid, silica (including fumed silica, precipitated silica, diatomaceous earth and quartz), oxide fillers including alumina, iron oxide, ferrite, magnesium oxide, titanium oxide, antimony trioxide, zirconium oxide, barium oxide and calcium oxide, hydroxide fillers including aluminum hydroxide and magnesium hydroxide, silicate fillers including aluminum silicate (clay), magnesium silicate (talc), mica, kaolin, calcium silicate, glass fiber, glass flakes, glass beads, sedimentary rock fillers including diatomaceous earth and limestone, montmorillonite (montmorillonite), magnesian montmorillonite, tetsumo Examples of suitable fillers include clay mineral-based fillers including montmorillonite, ferromagnesian montmorillonite, beidellite, aluminian beidellite, nontronite, aluminian nontronite, saponite, aluminian saponite, hectorite, sauconite, stevensite, and bentonite; magnetic fillers including ferrite, iron, and cobalt; conductive fillers including silver, gold, copper, and alloys thereof; thermally conductive fillers including aluminum nitride, boron nitride, and silicone carbide; sulfate-based fillers including aluminum sulfate, magnesium sulfate, barium sulfate, and calcium sulfate; sulfite-based fillers including calcium sulfite; calcium carbonate, basic magnesium carbonate, dolomite, barium titanate, and potassium titanate.
[0073] Among the above, as the inorganic filler (B) used in the present invention, silica, magnesium sulfate, barium sulfate, calcium carbonate, magnesium hydroxide, magnesium oxide, and talc are preferred, magnesium sulfate, barium sulfate, calcium carbonate, magnesium oxide, and talc are more preferred, magnesium sulfate, barium sulfate, calcium carbonate, and talc are even more preferred, and from the viewpoints of performance, ease of handling, supply stability, price, and the like, barium sulfate, calcium carbonate, and talc are most preferred.
[0074] These inorganic fillers (B) may be used alone or in combination of two or more kinds within the scope of the present invention that does not impair the characteristics of the present invention. The particle size of the inorganic filler (B) is preferably 0.01 μm to 100 μm, more preferably 0.01 μm to 80 μm, and even more preferably 0.01 μm to 50 μm, from the viewpoint of molding processability with the 4-methyl-1-pentene / α-olefin copolymer (A) and the thermoplastic elastomer (C).
[0075] The particle size of the inorganic filler (B) can be determined by a known method using a laser diffraction particle size distribution analyzer, and specifically, it is the 50% average particle size (d50) obtained from the cumulative % distribution curve measured with the laser diffraction particle size distribution analyzer.
[0076] The amount of inorganic filler (B) added in the resin composition of the present invention is 10 to 50 parts by mass relative to 100 parts by mass of the total amount of the 4-methyl-1-pentene·α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C). The amount added is preferably a certain amount or more, more preferably 20 parts by mass or more, from the viewpoint of obtaining a heavy feel and sufficient impact strength of a molded article made of the resin composition. On the other hand, the amount added is preferably a certain amount or less, more preferably 50 parts by mass or less, from the viewpoint of obtaining high stress relaxation property of a molded article made of the resin composition, i.e., shape retention in which the original shape is slowly restored after elastic deformation.
[0077] When two or more types of inorganic filler (B) are used, the above-mentioned numerical ranges are applied to the total amount of inorganic filler (B) added. <Thermoplastic elastomer (C)> The resin composition of the present invention contains a thermoplastic elastomer (C) in addition to the 4-methyl-1-pentene-α-olefin copolymer (A) and the inorganic filler (B). Here, the "thermoplastic elastomer (C)" used in the present invention is at least one selected from the group consisting of an olefin-based thermoplastic elastomer (C1) and a styrene-based thermoplastic elastomer (C2). In the present invention, both the olefin-based thermoplastic elastomer (C1) and the styrene-based thermoplastic elastomer (C2) described below play a role in adjusting the tan δ peak temperature required for the resin composition of the present invention to a range of 0°C or more and 60°C or less. In a typical and preferred embodiment of the present invention, the resin composition of the present invention contains only one of the olefin-based thermoplastic elastomer (C1) and the styrene-based thermoplastic elastomer (C2).
[0078] In a first aspect of the present invention, the resin composition of the present invention contains the 4-methyl-1-pentene·α-olefin copolymer (A), the inorganic filler (B), and an olefin-based thermoplastic elastomer (C1), but does not contain a styrene-based thermoplastic elastomer (C2).
[0079] In a second embodiment of the present invention, the resin composition of the present invention contains the 4-methyl-1-pentene·α-olefin copolymer (A), the inorganic filler (B), and a styrene-based thermoplastic elastomer (C2), but does not contain an olefin-based thermoplastic elastomer (C1).
[0080] Olefin-based thermoplastic elastomer (C1) The olefin-based thermoplastic elastomer (C1) is not particularly limited, and any conventionally known resin can be used. Specific examples include ethylene-based polymers, propylene-based polymers, and butene-based polymers. More specifically, ethylene-based elastomers consisting of propylene-based copolymers such as copolymers of ethylene and an α-olefin having 3 to 20 carbon atoms, copolymers of ethylene and an α-olefin having 3 to 20 carbon atoms and a cyclic olefin, and ethylene-based copolymers having various vinyl compounds as comonomers such as styrene, vinyl acetate, (meth)acrylic acid, (meth)acrylic acid esters, etc., and various ethylene-based elastomers having an island-sea structure containing polyethylene as a hard segment; Propylene-based elastomers made of propylene-based copolymers such as copolymers of propylene and an α-olefin having 4 to 20 carbon atoms, copolymers of propylene, ethylene and an α-olefin having 4 to 20 carbon atoms, and copolymers of propylene, an α-olefin having 4 to 20 carbon atoms and a cyclic olefin, as well as various propylene-based elastomers having an island-sea structure containing polypropylene as a hard segment; and butene-based elastomers consisting of 1-butene copolymers such as copolymers of 1-butene and an α-olefin having 5 to 20 carbon atoms, and copolymers of 1-butene and an α-olefin having 5 to 20 carbon atoms and a cyclic olefin, as well as butene-based elastomers having an island-sea structure containing polybutene as a hard segment; etc.
[0081] Here, the term "ethylene-based copolymer" refers to a copolymer having ethylene as the main component (specifically, containing 50% by mass or more, preferably 70% by mass or more of ethylene), the term "propylene-based copolymer" refers to a copolymer having propylene as the main component (specifically, containing 50% by mass or more, preferably 70% by mass or more of propylene), and the term "butene-based copolymer" refers to a copolymer having butene as the main component (specifically, containing 50% by mass or more, preferably 70% by mass or more of butene).
[0082] In one preferred embodiment of the present invention, the olefin-based thermoplastic elastomer (C1) is a copolymer of propylene, ethylene, and an α-olefin having 4 to 20 carbon atoms, and a preferred example of such a copolymer is a copolymer of propylene, ethylene, and butene.
[0083] The olefin-based thermoplastic elastomer (C1) that can be used in the present invention may be one type alone or a combination of two or more types. In the present invention, the olefinic thermoplastic elastomer (C1) may be an unmodified olefinic thermoplastic elastomer, or may be a modified olefinic thermoplastic elastomer obtained by modifying an olefinic thermoplastic elastomer with at least one functional group selected from the group consisting of an acid anhydride group, a carboxyl group, an amino group, an imino group, an alkoxysilyl group, a silanol group, a silyl ether group, a hydroxyl group, and an epoxy group. In one preferred embodiment of the present invention, the olefinic thermoplastic elastomer (C1) is an unmodified olefinic thermoplastic elastomer.
[0084] Among the above, as the olefin-based thermoplastic elastomer (C1), a propylene-based copolymer is preferred because of its kneadability with the 4-methyl-1-pentene / α-olefin copolymer (A) and the inorganic filler (B) and because it can be easily molded into the resin composition of the present invention to give a molded product having flexibility.
[0085] Styrene-based thermoplastic elastomer (C2) The styrene-based thermoplastic elastomer (C2) is, for example, a block copolymer of a polystyrene block that is the hard part (or crystalline part) and a diene monomer block that is the soft part (or amorphous part), and the hard part may be at both ends of the soft part. Examples of the styrene-based thermoplastic elastomer (C2) include styrene-butadiene-styrene copolymer (SBS), hydrogenated styrene-butadiene-styrene copolymer (hydrogenated styrene-butadiene rubber) (HSBR), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-ethylene-butene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), styrene-isobutylene-styrene copolymer (SIBS), styrene-isobutylene copolymer (SIB), and styrene-ethylene-butene-styrene-styrene copolymer (SEBSS).
[0086] The styrene-based thermoplastic elastomer (C2) that can be used in the present invention may be one type alone or a combination of two or more types. As the styrene-based thermoplastic elastomer (C2), a commercially available product can also be used.
[0087] An example of HSBR is Dynaron (registered trademark) manufactured by JSR Corporation. SEPS is a product obtained by hydrogenating a styrene-isoprene-styrene block copolymer (SIS). Examples of SIS include JSR SIS (registered trademark) manufactured by JSR Corporation, Hybler (registered trademark) manufactured by Kuraray Co., Ltd., and Kraton D (registered trademark) manufactured by Kraton Polymer Japan Co., Ltd. Examples of SEPS include Septon (registered trademark) manufactured by Kuraray Co., Ltd., and Kraton (registered trademark) manufactured by Kraton Polymer Japan Co., Ltd. Examples of SEBS include Tuftec H Series (registered trademark) manufactured by Asahi Kasei Corporation, and Kraton (registered trademark) manufactured by Kraton Japan Polymer Co., Ltd. Examples of SEBSS include SOE (registered trademark) manufactured by Asahi Kasei Corporation, which has a structure containing styrene even in the soft part. Examples of SIB and SIBS include Shibstar (registered trademark) manufactured by Kaneka Corporation. Examples of commercially available compounds obtained by combining the above-mentioned styrene-based copolymer with other resins such as polyolefins include TEFABLOC (registered trademark) manufactured by Mitsubishi Chemical Corporation, ARNESTON (registered trademark) manufactured by Kuraray Plastics Co., Ltd., and ELASTOMER AR Series (registered trademark) manufactured by Aronkasei Co., Ltd.
[0088] Amount of thermoplastic elastomer (C) added The amount of the thermoplastic elastomer (C) added in the resin composition of the present invention is 5 to 49 parts by mass relative to 100 parts by mass of the total amount of the 4-methyl-1-pentene-α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C). The amount added is preferably a certain amount or more from the viewpoint of adjusting the tan δ peak temperature of the resin composition to a range of 0° C. to 60° C., and more preferably 10 parts by mass or more. On the other hand, from the viewpoint of shape retention that an article made of the resin composition slowly recovers to its original shape after elastic deformation, the amount added is preferably a certain amount or less, and more preferably 40 parts by mass or less.
[0089] Here, when the thermoplastic elastomer (C) is of two or more types (i.e., when two or more types of olefin-based thermoplastic elastomers are used as the olefin-based thermoplastic elastomer (C1), and when two or more types of styrene-based thermoplastic elastomers are used as the styrene-based thermoplastic elastomer (C2)), the above-mentioned numerical range is applied to the total amount of thermoplastic elastomer (C) that can be contained in the resin composition of the present invention.
[0090] <Other ingredients> The resin composition of the present invention contains the 4-methyl-1-pentene-α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C). Here, the resin composition of the present invention may be composed of the 4-methyl-1-pentene-α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C). However, the resin composition of the present invention may further contain other components (hereinafter, "other components") that do not fall under the 4-methyl-1-pentene-α-olefin copolymer (A), the inorganic filler (B), or the thermoplastic elastomer (C) as necessary, within a range that does not impair the characteristics of the present invention. Examples of such "other components" include known additives.
[0091] Examples of additives include, but are not limited to, softeners, release agents, antioxidants, flame retardants, ultraviolet absorbers, surfactants, antistatic agents, pigments, dyes, slip agents, weather stabilizers, heat stabilizers, infrared absorbers, antiblocking agents, antifogging agents, lubricants, plasticizers, antioxidants, hydrochloric acid absorbers, crystal nucleating agents, antifungal agents, antibacterial agents, and organic fillers. These additives may be used alone or in combination of two or more.
[0092] Examples of the softener include known softeners including process oil, lubricating oil, paraffin, liquid paraffin, polyethylene wax, polypropylene wax, petroleum-based substances including petroleum asphalt and Vaseline, coal tars including coal tar and coal tar pitch, fatty oils including castor oil, linseed oil, rapeseed oil, soybean oil and coconut oil, tall oil, beeswax, carnauba wax and lanolin, fatty acids or metal salts thereof including ricinoleic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, montanic acid, oleic acid and erucic acid, synthetic polymers including petroleum resin, coumarone-indene resin and atactic polypropylene, ester-based plasticizers including dioctyl phthalate, dioctyl adipate and dioctyl sebacate, microcrystalline wax, liquid polybutadiene or modified or hydrogenated products thereof, and liquid thiokol.
[0093] Further, examples of the softening agent include aromatic carboxylates (dibutyl phthalate, etc.), aliphatic carboxylates (methyl acetylricinoleate, etc.), aliphatic dialkoxylates (adipic acid-propylene glycol polyesters, etc.), aliphatic tricarboxylates (triethyl citrate, etc.), phosphate triesters (triphenyl phosphate, etc.), epoxy fatty acid esters (epoxybutyl stearate, etc.), and petroleum resins.
[0094] Examples of release agents include lower alcohol esters (having 1 to 4 carbon atoms) of higher fatty acids (such as butyl stearate), polyhydric alcohol esters (having 4 to 30 carbon atoms) of fatty acids (such as hydrogenated castor oil), glycol esters of fatty acids, and liquid paraffin.
[0095] Examples of antioxidants include phenol-based (2,6-di-t-butyl-4-methylphenol, etc.), polycyclic phenol-based (2,2'-methylenebis(4-methyl-6-t-butylphenol) and other methylene-bridged polycyclic phenols, etc.), phosphorus-based (tetrakis(2,4-di-t-butylphenyl)-4,4-biphenylene diphosphonate, etc.), and amine-based (N,N-diisopropyl-p-phenylenediamine, etc.).
[0096] Examples of the flame retardant include phosphate esters and other phosphorus compounds such as ammonium polyphosphate, ethylene bis tris (2-cyanoethyl) phosphonium chloride, tris (tribromophenyl) phosphate, tris (tribromophenyl) phosphate, and tris (3-hydroxypropyl) phosphine oxide; chlorine-based flame retardants such as chlorinated paraffin, chlorinated polyolefin, and perchlorocyclopentadecane; bromine-based flame retardants such as hexabromobenzene, ethylene bis dibromonorbornane dicarboximide, ethylene bis tetrabromophthalimide, tetrabromobisphenol A derivatives, tetrabromobisphenol S, and tetrabromodipentaerythritol; and mixtures thereof.
[0097] Examples of the ultraviolet absorbing agent include benzotriazole-based, benzophenone-based, salicylic acid-based, and acrylate-based agents. Antibacterial agents include quaternary ammonium salts, pyridine compounds, organic acids, organic acid esters, halogenated phenols, and organic iodines.
[0098] Examples of the surfactant include nonionic, anionic, cationic, or amphoteric surfactants. Examples of the nonionic surfactant include polyethylene glycol-type nonionic surfactants such as higher alcohol ethylene oxide adducts, fatty acid ethylene oxide adducts, higher alkylamine ethylene oxide adducts, and polypropylene glycol ethylene oxide adducts; polyhydric alcohol-type nonionic surfactants such as fatty acid esters of polyethylene oxide or glycerin, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol or sorbitan, alkyl ethers of polyhydric alcohols, and fatty amides of alkanolamines. Examples of the anionic surfactant include sulfate ester salts such as alkali metal salts of higher fatty acids; sulfonates such as alkylbenzene sulfonates, alkyl sulfonates, and paraffin sulfonates; and phosphate ester salts such as higher alcohol phosphate ester salts. Examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium salts. Examples of the amphoteric surfactant include amino acid-type amphoteric surfactants such as higher alkylaminopropionates; and betaine-type amphoteric surfactants such as higher alkyldimethyl betaines and higher alkyldihydroxyethyl betaines.
[0099] Examples of the antistatic agent include the above-mentioned surfactants, fatty acid esters, and polymeric antistatic agents. Examples of the fatty acid esters include esters of stearic acid and oleic acid, and examples of the polymeric antistatic agents include polyether ester amides.
[0100] Examples of pigments include inorganic pigments (titanium oxide, iron oxide, chromium oxide, cadmium sulfide, etc.) and organic pigments (azo lake type, thioindigo type, phthalocyanine type, anthraquinone type). Examples of dyes include azo type, anthraquinone type, triphenylmethane type, etc.
[0101] The amount of these pigments and dyes added is not particularly limited, but is usually 5 parts by mass or less, and preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the resin composition of the present invention. Examples of slip agents include waxes (such as carnauba wax), higher fatty acids (such as stearic acid), higher fatty acid salts (such as calcium stearate), higher alcohols (such as stearyl alcohol), and higher fatty acid amides (such as stearamide and erucic acid amide).
[0102] The amount of each of the above-mentioned additives to be added is not particularly limited depending on the application as long as the object of the present invention is not impaired. However, it is preferable that the total amount of each of the additives is 0.01 to 30 parts by mass per 100 parts by mass of the resin composition of the present invention.
[0103] Typical and exemplary embodiments of the resin composition of the present invention include the following (X1) to (X4): (X1) a resin composition comprising the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the olefin-based thermoplastic elastomer (C1); (X2) a resin composition comprising the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the styrene-based thermoplastic elastomer (C2); (X3) a resin composition consisting only of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), the olefin-based thermoplastic elastomer (C1), and the various additives; (X4) a resin composition consisting only of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), the styrene-based thermoplastic elastomer (C2), and the various additives; When the resin composition of the present invention contains "other components", the total amount of the "other components" in the resin composition of the present invention is preferably 0.01 to 30 parts by mass, and more preferably, for example, 0.1 to 3 parts by mass, relative to 100 parts by mass of the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C).
[0104] <Method of producing resin composition> The method for producing the resin composition of the present invention is not particularly limited, and for example, a conventionally known production method can be used. An example of the method is to dry blend the 4-methyl-1-pentene-α-olefin copolymer (A), the inorganic filler (B), the thermoplastic elastomer (C), and the optional "other components" that constitute the resin composition of the present invention using a known mixer. Here, examples of the mixer include a Henschel mixer, a tumbler blender, and a V-blender.
[0105] After dry blending with the above mixer, for example, at a temperature setting of 180 to 250°C, a method of melt kneading with a single screw extruder, a twin screw extruder, a Banbury mixer, a kneader, a roll mill, etc., followed by granulation or pulverization can be adopted. Among these, melt kneading with a twin screw extruder or a Banbury mixer is preferred from the viewpoint of the mixability of each component and productivity. By these methods, high-quality pellets in which each component is uniformly mixed and dispersed can be obtained.
[0106] The inorganic filler (B) may be used in the form of a mixture with a resin component such as the 4-methyl-1-pentene / α-olefin copolymer (A), for example, a master batch obtained by previously mixing the inorganic filler (B) with a resin component such as the 4-methyl-1-pentene / α-olefin copolymer (A).
[0107] <Method of manufacturing molded body> The molded article of the present invention is made of the resin composition of the present invention described above. Examples of the molded article of the present invention include toys, daily necessities, ear inserts, and sheet-like molded articles.
[0108] The method for producing the molded article of the present invention is not particularly limited, and for example, a conventionally known manufacturing method can be used, such as injection molding, extrusion molding, compression molding, 3D modeling, microwave heating molding, etc. Among such molding methods, injection molding using a required mold is preferred, and such injection molding can suitably produce a molded article.
[0109] Furthermore, when a sheet-shaped molded product is to be obtained, extrusion sheet molding equipped with a general T-die is preferred. A single-screw extruder or twin-screw extruder equipped with a T-die can be used to produce a film at a cylinder temperature of 180 to 250°C and a casting roll temperature of 20 to 80°C to produce a sheet. The thickness of the sheet varies depending on the application, but is usually 10 to 1000 μm, preferably 20 to 500 μm, so that no pinholes are generated during sheet molding, sufficient mechanical strength is obtained, and it is also advantageous for mass production of sheets.
[0110] The surface of the sheet may be embossed, and the sheet may be stretched during or after molding. Furthermore, in order to remove residual stress in the sheet, annealing may be performed at a temperature below the melting point of the resin.
[0111] <Applications of molded products> The molded article made of the resin composition of the present invention has a feature that it improves the fit due to its high stress relaxation property in the room temperature range, and also slowly recovers to its original shape after elastic deformation.
[0112] The molded article made of the resin composition of the present invention is useful not only for daily necessities, toys, ear inserts, and seats, but also for conventionally known automotive materials, clothing materials, sanitary materials, construction materials, sports materials, living materials, leisure materials, industrial materials, electronic materials, and the like.
[0113] They can also be used in the field of household goods. Specific examples include containers for food, forks and spoons (especially the handles and grips of forks and spoons), dishes, etc. These can be easily molded by injection molding, and are useful as containers and dishes to replace ceramics because they have a sense of weight.
[0114] It is also possible to expand into other applications where ceramics are used, such as everyday items such as lampshades and vases, structural components for certain audio speakers, and water-related products such as washbasins and toilets. In addition to ceramics, its characteristic of being able to impart a sense of weight can be utilized to expand its use to models such as plastic models, components for musical instruments, tiles, substitutes for artificial marble, building components, and the like. It is also useful as a container for containers with lids (including airless containers, etc.) and cosmetic compacts. In addition, it is also useful as a filament material for 3D printers, taking advantage of its moldability and shape retention.
[0115] Furthermore, by taking advantage of the characteristics such as weight, texture and design, the material is also useful as an ear insert, for example. The hearing aid can be properly fitted in the ear, and can be used stably and comfortably. In particular, wearable devices that allow devices to be carried around have been developed recently. Among them, it is also useful for earphone components that connect to audio equipment using a connector or listen to music using wireless communication such as Bluetooth, Wi-Fi, and infrared. It reduces pressure on the ear and prevents excessive movement of the earphone, providing a good fit and comfort. It can also be suitably used as a band component for a smart watch.
[0116] Furthermore, by taking advantage of the inorganic material's filling property and conformability, it is also useful as a heat dissipation material for electronic information materials, for example. In particular, the amount of heat emitted from electronic devices has increased due to the recent trend toward high-definition semiconductor circuits, making it necessary to improve the efficiency of heat dissipation materials. By taking advantage of the adhesiveness and conformability, it is possible to efficiently improve the heat dissipation effect. EXAMPLES
[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the physical properties of resins, the resins used, the methods for preparing test pieces, and the evaluation methods in the following examples and comparative examples are as follows.
[0118] [Method of measuring resin physical properties] <Content of structural units> The 4-methyl-1-pentene and α-olefin contents in the polymer were quantified using the following equipment and conditions: 13 The α-olefin content was based on the results measured by C-NMR, but the content of 4-methyl-1-pentene was not included in the α-olefin content measured by this method.
[0119] The ECP500 nuclear magnetic resonance spectrometer manufactured by JEOL Ltd. was used, and the mixture solvent of orthodichlorobenzene / deuterated benzene (80 / 20% by volume) was used. The sample concentration was 55 mg / 0.6 mL. The measurement temperature was 120°C. The observed nuclei were 13 The measurements were performed using C (125 MHz), a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 s, and an accumulation count of 10,000 or more, with 27.50 ppm as the reference value for the chemical shift. 13 The composition of 4-methyl-1-pentene·α-olefin (A) was quantified by C-NMR spectroscopy.
[0120] <Intrinsic viscosity> This value was measured in decalin at 135°C using an Ubbelohde viscometer. Approximately 20 mg of the polymerized powder, pellets, or resin mass was collected and dissolved in 15 mL of decalin, and the specific viscosity ηsp of the resulting decalin solution was measured in an oil bath heated to 135°C. After diluting this decalin solution by adding 5 mL of decalin solvent, the specific viscosity ηsp was measured in the same manner. This dilution procedure was repeated two more times, and the value of ηsp / C when the concentration (C) was extrapolated to zero was calculated as the limiting viscosity [η] (see the formula below).
[0121] [η]=lim(ηsp / C) (C→0) <Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn value)> The molecular weight was measured by gel permeation chromatography (GPC).
[0122] Specifically, a Waters ALC / GPC150-Cplus type (integrated with differential refractometer detector) was used as a liquid chromatograph, two Tosoh GMH6-HT columns and two GMH6-HTL columns connected in series were used as separation columns, o-dichlorobenzene was used as a mobile phase medium, and 0.025% by mass dibutylhydroxytoluene (Takeda Pharmaceutical Co., Ltd.) was used as an antioxidant, the mobile phase medium was moved at 1.0 mL / min, the sample concentration was 15 mg / 10 mL, the sample injection amount was 500 μL, and a differential refractometer was used as a detector. Standard polystyrenes with weight average molecular weights (Mw) of 1,000 or more and 4,000,000 or less, manufactured by Tosoh Corporation, were used.
[0123] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn value) were calculated by preparing a calibration curve using a standard polystyrene sample and analyzing the obtained chromatogram by a known method. The measurement time per sample was 60 minutes.
[0124] <Melt Mass Flow Rate (MFR)> The measurements were performed at a temperature of 230°C and a load of 2.16 kg in accordance with ASTM D1238. <Melting point> The melting point was determined as the highest temperature at the apex of the melting peak measured at a heating rate of 10° C. / min using a differential scanning calorimeter DSC220C manufactured by Seiko Instruments Inc. in accordance with JIS K7121.
[0125] <Density of 4-methyl-1-pentene / α-olefin copolymer (A)> Density of 4-methyl-1-pentene / α-olefin copolymer (A) (kg / m 3 ) was measured using a density gradient tube in accordance with JIS K7112.
[0126] <Synthesis of 4-methyl-1-pentene-α-olefin copolymer (A)> A 1.5 L stainless steel autoclave equipped with an agitator and thoroughly purged with nitrogen was charged with 300 ml of n-hexane (dried over activated alumina under a dry nitrogen atmosphere) and 450 ml of 4-methyl-1-pentene at 23° C. 0.75 ml of a 1.0 mmol / ml toluene solution of triisobutylaluminum (TIBAL) was charged into the autoclave and stirred.
[0127] Next, the autoclave was heated to an internal temperature of 60° C., and pressurized with propylene to a total pressure (gauge pressure) of 0.40 MPa. Next, 0.34 ml of a toluene solution containing 1 mmol of methylaluminoxane (calculated as aluminum) and 0.01 mmol of diphenylmethylene(1-ethyl-3-t-butyl-cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, which had been previously prepared, was injected into the autoclave with nitrogen pressure to initiate the polymerization reaction.
[0128] During the polymerization reaction, the internal temperature of the autoclave was adjusted to 60°C. Sixty minutes after the start of polymerization, 5 ml of methanol was injected into the autoclave with nitrogen to terminate the polymerization reaction, and the autoclave was then depressurized to atmospheric pressure. After depressurization, acetone was added to the reaction solution while stirring.
[0129] The resulting powdery copolymer containing the solvent was dried at 100°C under reduced pressure for 12 hours. The product, 4-methyl-1-pentene·α-olefin copolymer (A), weighed 36.9 g, and the 4-methyl-1-pentene content in the copolymer was 72.3 mol%, and the propylene content was 27.7 mol%. No melting point was observed when DSC was performed. The measurement results of each physical property are shown in Table 1.
[0130] <Dynamic viscoelasticity measurement of 4-methyl-1-pentene / α-olefin copolymer (A)> A predetermined amount of 4-methyl-1-pentene·α-olefin copolymer (A) obtained by the method described above was filled into a SUS mold, and the mixture was preheated for 7 minutes using a hydraulic hot press machine (PEWR-30 manufactured by Kansai Roll Co., Ltd.) with the heating plate set at 200°C, and then pressed at a gauge pressure of 10 MPa for 2 minutes. The mixture was then transferred to a cooling plate set at 20°C, compressed at a gauge pressure of 10 MPa, and cooled for 3 minutes to prepare a press sheet for measurement with a thickness of 2.0 mm.
[0131] Next, test pieces with dimensions of 35 mm length x 10 mm width were punched out from the 2.0 mm thick measurement press sheet obtained by the above-mentioned method, and the temperature dispersion of the dynamic viscoelasticity was observed from -40 to 150°C using a rheometer (Anton Paar MCR301) under conditions of torsion mode, frequency of 10 rad / s (1.6 Hz), strain setting of 0.1%, and heating rate of 2°C / min. The tan δ peak value was 2.70 and the tan δ peak temperature was 30°C.
[0132] The measurement results of each physical property are shown in Table 1.
[0133] [Table 1]
[0134] <Inorganic filler (B)> As the inorganic filler (B-1), heavy calcium carbonate (KS-1000: 50% average particle size 4.2 μm, manufactured by Calfine Co., Ltd.) was used.
[0135] <Inorganic filler (B-2)> As the inorganic filler (B-2), barium sulfate (Sakai Chemical Industry Co., Ltd., average particle size 10.0 μm) was used.
[0136] <Olefin-based thermoplastic elastomer (C1)> As the olefin-based thermoplastic elastomer (C1), the following three types were used. (C1-1): Toughmer PN-2060 manufactured by Mitsui Chemicals, Inc. (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 230°C, load 2.16 kg) 6 g / 10 min, density 868 kg / m 3 , melting point 160℃, surface hardness (ASTM D2244 compliant) Shore A84) (C1-2): Mitsui EPT3072EPM manufactured by Mitsui Chemicals, Inc. (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 190°C, load 2.16 kg) 1.0 g / 10 min, density 880 kg / m 3 (No melting point observed) (C1-3): Mitsui EPT K-9720M manufactured by Mitsui Chemicals, Inc. (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 190°C, load 2.16 kg) 0.5 g / 10 min, density 870 kg / m 3 (No melting point observed) <Styrene-based thermoplastic elastomer (C2)> The following four types of styrene-based thermoplastic elastomers (C2) were used.
[0137] (C2-1): Asahi Kasei Corporation Tuftec H1052 (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 230°C, load 2.16 kgf) 13 g / 10 min, density 0.89 g / cm 3 , surface hardness (ASTM D2244 compliant) Shore A67), (C2-2): Asahi Kasei Corporation Tuftec H1272 (density 0.90 g / cm 3 , surface hardness (ASTM D2244 compliant) Shore A35, oil-extended composition), (C2-3): Kuraray Plastics Co., Ltd., Arneston CJ001N (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 230°C, load 2.16 kgf) 2g / 10min, density 0.90g / cm 3 , surface hardness (ASTM D2244 compliant) Shore A40), (C2-4): Kuraray Plastics Co., Ltd., Arneston JS20N (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 190°C, load 2.16 kgf) 15 g / 10 min, density 0.89 g / cm3 , surface hardness (JIS K6253-3 compliant) Shore E20) (C2-5): SOE S1613 manufactured by Asahi Kasei Corporation (Melt mass flow rate (MFR; compliant with ASTM D1238, temperature 230°C, load 2.16 kgf) g / 14 min, density 0.93 g / cm 3 , surface hardness (ASTM D2244 compliant) Shore A46), For the olefin-based thermoplastic elastomer (C1) and the styrene-based thermoplastic elastomer (C2), the numerical values immediately following the expressions "Shore A" and "Shore E" are the values in Shore A hardness and Shore E hardness, respectively.
[0138] <Propylene-based resin (E)> As the propylene-based resin (E), J105G (melt mass-flow rate (MFR; compliant with ASTM D1238, temperature 230° C., load 2.16 kg) 9 g / 10 min, melting point 162° C.), a propylene homopolymer manufactured by Prime Polymer Co., Ltd., was used.
[0139] <Preparation of Resin Composition> The resin composition of the present invention was prepared using a Banbury mixer (Kobe Steel, Ltd. BB-L1800: tangential 4-blade rotor, kneading tank volume 1.63 L) equipped with a single-screw extruder for pelletization. A predetermined amount of various resin components that had been dry-blended in advance was added to the hopper of the Banbury mixer, and the resin components were pushed into the mixing chamber by a floating weight, and a predetermined amount of the inorganic filler (B) was added from the hopper side plate. The mixture was melt-kneaded under conditions of a temperature setting of 220°C and a rotor rotation speed of 80 rpm, and the kneaded product that maintained the molten state was sent to the single-screw extruder and granulated using a die (pelletizing head) with circular holes, a cooling water tank, and a pelletizer, to obtain pellets of the resin composition. The pellets of the obtained resin composition were uniformly mixed and dispersed, and the pellet diameter was 2.5 to 3.0 mm.
[0140] <Preparation of Molded Body> To evaluate the physical properties of molded products based on the material composition of the resin composition, a square plate with a length of 120 mm, a width of 130 mm, and a thickness of 2 mm and a dumbbell with a thickness of 3 mm (dumbbell-shaped molded product test piece) conforming to ASTM D638 for measuring mechanical properties were produced using an injection molding machine (ES75SXIII manufactured by Toshiba Machine Co., Ltd.; clamping force 735 kN, screw diameter Φ32 mm). The main molding conditions were as follows.
[0141] Cylinder temperature setting: 220~240℃ Screw speed: 100 rpm Injection pressure: 30~40MPa ·Injection speed: 25~30mm / sec Mold temperature: 30~60℃ (40℃ for square plates) Cooling time: 30 to 60 seconds (40 seconds for square plates) Physical property evaluation of molded products <Measurement of dynamic viscoelasticity> Test pieces with dimensions of 35 mm in length and 10 mm in width were punched out from the 2.0 mm thick molded body obtained by the above-mentioned method, and the tan δ peak temperature and tan δ peak value were observed over a temperature distribution of -40 to 150°C using a rheometer (Anton Paar MCR301) under conditions of torsion mode, frequency of 10 rad / s (1.6 Hz), strain setting of 0.1%, and heating rate of 2°C / min.
[0142] <Density of molded body> From the 2 mm (2.0 mm) thick molded body (square plate) obtained by the above-mentioned method, a test piece with dimensions of 62 mm length × 13 mm width was punched out and the density of the molded body (g / cm3) was measured by the underwater displacement method according to JIS K7112. 3 ) was measured.
[0143] <Surface hardness> Three 2 mm (2.0 mm) thick molded bodies (square plates) obtained by the above method were stacked to form test pieces, and the Shore A hardness was measured immediately after and 15 seconds after the indenter of a hardness tester was pressed against the surface of the test piece at 23°C in accordance with ASTM D2244. Normally, for Shore A90 or higher, measurements are made using a Shore D hardness tester, but for the purpose of understanding the displacement over time caused by the pressure of the indenter, measurements were made without changing the hardness tester even for Shore A90 or higher.
[0144] Based on the obtained Shore A hardness values, the ΔHS value was calculated according to the following formula. ΔHS = (Shore A hardness value immediately after the indenter starts contacting the material - Shore A hardness value 15 seconds after the indenter starts contacting the material) <Mechanical properties> The tensile strength and tensile modulus of the molded body were measured by a tensile test using the dumbbell-shaped molded body test piece. The tensile test was performed at 23° C. and a test speed of 50 mm / min using a five-strand tensile tester 2005X-5 manufactured by Intesco Co., Ltd. in accordance with ASTM D638.
[0145] <Mold shrinkage rate> The shrinkage rate was calculated by measuring the difference in length between the injection mold and the 2.0 mm thick molded body (square plate) along its four sides and calculating the dimensional change relative to the length of the mold.
[0146] Example 1 A resin composition containing 32 parts by mass of 4-methyl-1-pentene / α-olefin copolymer (A), 48 parts by mass of inorganic filler (B-1), and 20 parts by mass of olefin-based thermoplastic elastomer (C1) was melt-kneaded according to the method described above to obtain pellets.
[0147] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-1. Example 2 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-1, molded bodies and various test pieces were prepared in the same manner as in Example 1, and physical property evaluations were performed. The results are shown in Table 2-1.
[0148] Example 3 Among the resins used, except that the olefin-based thermoplastic elastomer (C1) was changed to a styrene-based thermoplastic elastomer (C2-1), molded bodies and various test pieces were prepared in the same manner as in Example 1, and physical property evaluations were performed. The results are shown in Table 2-1.
[0149] Example 4 Among the resins used, except that the olefin-based thermoplastic elastomer (C1) was changed to a styrene-based thermoplastic elastomer (C2-2), molded bodies and various test pieces were prepared in the same manner as in Example 1, and physical property evaluations were performed. The results are shown in Table 2-1.
[0150] Example 5 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-1, molded bodies and various test pieces were prepared in the same manner as in Example 4, and physical property evaluations were performed. The results are shown in Table 2-1.
[0151] Example 6 A resin composition containing 30 parts by mass of 4-methyl-1-pentene / α-olefin copolymer (A), 40 parts by mass of inorganic filler (B-1), and 30 parts by mass of styrene-based thermoplastic elastomer (C2-3) was melt-kneaded according to the method described above to obtain pellets.
[0152] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-1. Example 7 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-1, molded bodies and various test pieces were prepared in the same manner as in Example 6, and the physical properties were evaluated. The results are shown in Table 2-1.
[0153] Example 8 Among the resins used, except that the styrene-based thermoplastic elastomer (C2-3) was changed to the styrene-based thermoplastic elastomer (C2-4), molded bodies and various test pieces were prepared in the same manner as in Example 6, and physical property evaluations were performed. The results are shown in Table 2-2.
[0154] Example 9 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-2, molded bodies and various test pieces were prepared in the same manner as in Example 8, and the physical properties were evaluated. The results are shown in Table 2-2.
[0155] Example 10 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-2, molded bodies and various test pieces were prepared in the same manner as in Example 8, and the physical properties were evaluated. The results are shown in Table 2-2.
[0156] Example 11 A resin composition containing 40 parts by mass of 4-methyl-1-pentene / α-olefin copolymer (A), 30 parts by mass of inorganic filler (B-1), and 30 parts by mass of styrene-based thermoplastic elastomer (C2-5) was melt-kneaded according to the method described above to obtain pellets.
[0157] Next, the pellets were used to prepare molded bodies and various test pieces according to the above-mentioned methods, and the physical properties were evaluated as described above. The results are shown in Table 2-2. Example 12 A resin composition containing 40 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A), 30 parts by mass of inorganic filler (B-2), and 30 parts by mass of styrene-based thermoplastic elastomer (C2-5) was melt-kneaded according to the method described above to obtain pellets.
[0158] Next, the pellets were used to prepare molded bodies and various test pieces according to the above-mentioned methods, and the physical properties were evaluated as described above. The results are shown in Table 2-2. Example 13 A resin composition containing 50 parts by mass of 4-methyl-1-pentene / α-olefin copolymer (A), 40 parts by mass of inorganic filler (B-1), and 10 parts by mass of olefin-based thermoplastic elastomer (C1-2) was melt-kneaded according to the method described above to obtain pellets.
[0159] Next, the pellets were used to prepare molded bodies and various test pieces according to the above-mentioned methods, and the physical properties were evaluated as described above. The results are shown in Table 2-2. Example 14 Except for changing the blending amounts of the resin and inorganic filler (B-1) used as shown in Table 2-2, molded bodies and various test pieces were prepared in the same manner as in Example 13, and physical property evaluations were performed. The results are shown in Table 2-2.
[0160] Example 15 A resin composition containing 50 parts by mass of 4-methyl-1-pentene / α-olefin copolymer (A), 40 parts by mass of inorganic filler (B-1), and 10 parts by mass of olefin-based thermoplastic elastomer (C1-3) was melt-kneaded according to the method described above to obtain pellets.
[0161] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-3. Example 16 Except for changing the blending amount of the resin and inorganic filler (B-1) used as shown in Table 2-3, molded bodies and various test pieces were prepared in the same manner as in Example 15, and the physical properties were evaluated. The results are shown in Table 2-3.
[0162] Comparative Example 1 Except for changing the material composition of the resin composition to 4-methyl-1-pentene·α-olefin copolymer (A) alone, molded bodies and various test pieces were prepared in the same manner as in Example 1, and the physical properties were evaluated. The results are shown in Table 2-3.
[0163] Comparative Example 2 A resin composition containing 30 parts by mass of the 4-methyl-1-pentene·α-olefin copolymer (A) and 70 parts by mass of the inorganic filler (B-1) was melt-kneaded in the same manner as described above to obtain pellets.
[0164] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-3. Comparative Example 3 A resin composition containing 40 parts by mass of the 4-methyl-1-pentene·α-olefin copolymer (A) and 60 parts by mass of the propylene-based resin (E) was melt-kneaded in the same manner as described above to obtain pellets.
[0165] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-3. Comparative Example 4 A resin composition containing 30 parts by mass of the 4-methyl-1-pentene·α-olefin copolymer (A) and 70 parts by mass of the inorganic filler (B-2) was melt-kneaded in the same manner as described above to obtain pellets.
[0166] Next, the pellets were used to prepare molded bodies and various test pieces in the manner described above, and the physical properties were evaluated as described above. The results are shown in Table 2-3.
[0167] [Table 2-1]
[0168] [Table 2-2]
[0169] [Table 2-3]
[0170] As shown in Tables 2-1 to 2-3, the molded articles made of the resin compositions obtained in Examples 1 to 16 have a tan δ peak temperature of 0°C to 60°C and a tan δ peak value of 0.6 to 5.0, as measured by dynamic viscoelasticity (temperature range of -40 to 150°C) at a frequency of 10 rad / s (1.6 Hz), and therefore have excellent stress relaxation properties in the room temperature range and slowly recover to their original shape after elastic deformation. 3 More than 5.0g / cm 3 The results showed that the molded product had a soft feel, because the surface hardness measurement showed a large change in hardness immediately after and 15 seconds later. [Industrial Applicability]
[0171] The resin composition and molded article of the present invention can be suitably used as daily necessities, toys, and ear inserts. Daily necessities made of the resin composition of the present invention include, for example, containers for holding food, forks and spoons (especially handles and grips of forks and spoons), tableware such as plates, containers with lids, cosmetic compacts, and other containers. Toys include, for example, models such as plastic models. Ear inserts include, for example, hearing aid components and earphone components. Other examples include heat dissipation materials, etc.
Claims
1. 15 to 50 parts by mass of a 4-methyl-1-pentene / α-olefin copolymer (A) satisfying at least one of the following requirements (d) and (e); 10 to 50 parts by mass of an inorganic filler (B); Thermoplastic elastomer (C) 5 to 49 parts by mass (the total amount of the 4-methyl-1-pentene / α-olefin copolymer (A), the inorganic filler (B), and the thermoplastic elastomer (C) is taken as 100 parts by mass); Including, The thermoplastic elastomer (C) is at least one selected from the group consisting of an olefin-based thermoplastic elastomer (C1) and a styrene-based thermoplastic elastomer (C2), and A resin composition characterized by satisfying the following requirements (a) to (c): (a) In the temperature range of −40 to 150° C., the temperature at which the loss tangent tan δ value obtained by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) is maximized (hereinafter also referred to as tan δ peak temperature) is 0° C. or higher and 60° C. or lower. (b) The maximum value of loss tangent tan δ (hereinafter also referred to as tan δ peak value) determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of −40 to 150° C. is 0.6 or more and 5.0 or less. (c) density is 1.0 g / cm 3 5.0g / cm or more 3 The following is the result. (d) Consists of 55 to 90 mol % of structural units derived from 4-methyl-1-pentene and 10 to 45 mol % of structural units derived from an α-olefin having 2 to 4 carbon atoms (the total of structural units derived from 4-methyl-1-pentene and structural units derived from an α-olefin having 2 to 4 carbon atoms is 100 mol %). (e) The melting point measured by differential scanning calorimetry (DSC) is 160° C. or less, or no melting point is observed.
2. 2. The resin composition according to claim 1, wherein the 4-methyl-1-pentene·α-olefin copolymer (A) satisfies the following requirements (f) and (g): (f) The tan δ peak temperature determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of −40 to 150° C. is 15° C. or more and 45° C. or less. (g) The tan δ peak value determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of −40 to 150° C. is 0.6 or more and 5.0 or less.
3. The resin composition according to any one of claims 1 to 2, characterized in that the inorganic filler (B) is at least one selected from the group consisting of calcium carbonate, magnesium sulfate, barium sulfate, magnesium oxide and talc.
4. 4. The resin composition according to claim 1, wherein the inorganic filler (B) has an average particle size of 0.01 to 100 μm.
5. A molded article made of the resin composition according to any one of claims 1 to 4.
6. A daily necessities comprising the resin composition according to any one of claims 1 to 4.
7. A toy comprising the resin composition according to any one of claims 1 to 4.
8. An ear insert member comprising the resin composition according to any one of claims 1 to 4.
9. A sheet comprising the resin composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Thermoplastic elastomer composition
JP2002327098A
Flame-retardant resin composition and molded article using the same
JP2011116868A
Shoe insole and shoe
JP2018042908A
Menstruation cup