Dental workpiece and method for producing the same

A high-strength, translucent dental workpiece with enhanced machinability in the sintered state addresses the challenges of zirconia sintered bodies by allowing efficient machining with reduced tool wear and increased productivity, minimizing the number of hospital visits.

JP2024156857AInactive Publication Date: 2024-11-06KURARAY NORITAKE DENTAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024126485
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-01
Filing Date
2024-08-02
Publication Date
2024-11-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Zirconia sintered bodies used in dental prostheses have high strength and translucency but are difficult to machine due to high hardness, leading to long processing times and frequent tool wear, which limits productivity and increases the number of hospital visits required for treatment.

Method used

A dental workpiece with a biaxial bending strength of 300 MPa or more, featuring a micro-slurry jet erosion test with an erosion rate of 6.5 μm/g or more when using a spherical alumina slurry with an average particle diameter of 3.0 μm, allowing for excellent machinability in the sintered state.

Benefits of technology

The dental workpiece enables efficient machining in the sintered state with reduced tool wear, shortening processing time and increasing the number of prostheses that can be produced with a single tool, thus improving productivity and reducing the number of hospital visits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156857000001_ABST
    Figure 2024156857000001_ABST
Patent Text Reader

Abstract

To provide a dental workpiece that has suitable strength for dental use and has exceptional machinability in a sintered state.SOLUTION: The present invention relates to a dental workpiece for which the erosion rate is 8.0 μm / g or higher or the value of (erosion rate (μm / g))×(average crystal grain size (μm)) is 15 μm2 / g or greater when a spherical alumina slurry having an average particle size of 3.0 μm is projected in a micro slurry-jet erosion test, and for which the biaxial bending strength measured in conformance with ISO 6872: 2015 is 300 MPa or greater.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dental workpiece and a manufacturing method thereof, and more particularly to a dental workpiece excellent in strength and translucency and in machinability in a sintered state, and a manufacturing method thereof. [Background technology]

[0002] Ceramics made of metal oxides have been widely used industrially, and zirconia sintered bodies are particularly used as dental materials for dental prostheses due to their high strength and aesthetic properties.

[0003] Zirconia sintered bodies have excellent strength, so when they are used as dental materials such as prostheses, problems such as breakage rarely occur. In addition, zirconia sintered bodies have high translucency and are less likely to be discolored in the oral cavity, so they are also excellent in aesthetics. On the other hand, after being made into a completely sintered sintered body, they have high hardness and are almost impossible to process with dental processing machines. For example, if a zirconia sintered body having a cubic shape is machined to obtain a zirconia sintered body having a shape that matches the shape of a patient's teeth, the consumption of metal processing tools will be very large, and it will take a huge amount of time to manufacture even just one dental prosthesis.

[0004] For these reasons, when using a zirconia sintered body for dental material applications, it is usually not a completely sintered sintered body, but a calcined body in a semi-sintered state that is easy to process is processed into the shape of a desired dental prosthesis, and then further sintered to produce a sintered body processed into the shape of the intended dental prosthesis. After that, the sintered body is subjected to slight adjustment processing so that the sintered body having the shape of the dental prosthesis fits comfortably when it is worn in the oral cavity of a patient at a dental clinic. Moreover, in recent years, when the calcined body is processed into the desired shape of a dental prosthesis, machining using a CAD / CAM system is used to obtain a shape that matches the patient's tooth in the treatment area, and calcined bodies (mill blanks) for CAD / CAM systems are widely used.

[0005] As described above, when using zirconia sintered bodies for dental material applications, major machining is avoided after sintering due to the specific problems in sintering zirconia, and processing of the sintered body is limited to minor adjustments when it is fitted in the oral cavity of a patient at a dental clinic. In other words, measures are taken in dental material applications that correspond to the gradual changes in physical properties caused by sintering zirconia.

[0006] In addition, in dental treatment, taking into consideration the unique circumstances resulting from the physical properties of the above-mentioned zirconia sintered body, treatment is generally carried out through many steps, including a step of acquiring information on the shape of the patient's oral cavity, such as information on the dentition, a step of machining a calcined body (mill blank) into the shape of the desired dental prosthesis using a CAD / CAM system based on the acquired information, a step of sintering the calcined body having the shape of the desired dental prosthesis to obtain a sintered body, and a step of making slight adjustments to the sintered body so that it fits comfortably in the patient's oral cavity when worn at a dental clinic.

[0007] As described above, in dental treatment using a dental prosthesis made of zirconia sintered body, it is difficult to complete all the above steps in one visit to the dental clinic. Therefore, even for treatment of one tooth, multiple visits to the dental clinic are required, and the treatment period from start to finish often takes more than one month.

[0008] On the other hand, from the patient's perspective, it is desirable to minimize the number of visits to the hospital in order to reduce the time it takes for new artificial teeth to be fitted after treatment and to reduce the burden of having to go to the hospital, and the need to complete treatment in a short period of time is increasing every year.

[0009] If it were possible to perform significant machining on the zirconia sintered body, it would eliminate the need to machine the calcined body first and then produce a sintered body by sintering. After obtaining information on the shape of the patient's mouth, the unmachined sintered body could be machined into the shape of the desired dental prosthesis using a CAD / CAM system based on that information, and the prosthesis could then be fitted into the patient's mouth and fine-tuned, allowing dental treatment to be completed in one day.

[0010] In addition, when using dental prostheses, dental treatment that can be completed in one day is possible when materials other than zirconia, such as lithium disilicate glass ceramics and feldspar-based glass ceramics, are used. However, in the case of zirconia sintered bodies, there are unique circumstances resulting from the physical properties of the zirconia sintered bodies, making it very difficult to realize this.

[0011] As described above, zirconia is in high demand in terms of strength and aesthetics, and in response to the increasing need to shorten treatment periods, zirconia sintered bodies have been proposed that have excellent machinability in the sintered state and can be processed from a prismatic or disc-shaped mill blank into the shape of a desired dental prosthesis (e.g., Patent Documents 1 and 2).

[0012] For example, Patent Document 1 discloses a processable zirconia that is a sintered body formed so as to contain a tetragonal zirconia composite powder containing 79.8 to 92 mol% ZrO2, 4.5 to 10.2 mol% Y2O3, 3.5 to 7.5 mol% Nb2O5 or 5.5 to 10.0 mol% Ta2O5, and a TiO2 nanopowder whose mass ratio to the zirconia composite powder is more than 0 mass% and 2.5 mass% or less, and a method for producing the same.

[0013] Patent Document 2 discloses a machinable zirconia composition using a raw material containing 78 to 95 mol% ZrO2, 2.5 to 10 mol% Y2O3, 2 to 8 mol% Nb2O5, and / or 3 to 10 mol% Ta2O5, in which the main crystal phase of ZrO2 is monoclinic, and a method for producing the same. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2015-127294 A [Patent Document 2] International Publication No. 2021 / 132644 Summary of the Invention [Problem to be solved by the invention]

[0015] The zirconia sintered bodies disclosed in Patent Documents 1 and 2 can be machined even in a sintered state. However, the processing time required to cut out a dental prosthesis is long, and there is room for improvement in terms of shortening treatment time. In addition, although the zirconia sintered bodies disclosed in Patent Documents 1 and 2 can be machined, the number of dental prostheses that can be obtained by continuous machining using one machining tool is small, and the machining tool wears out quickly, so that the machining tool needs to be replaced more frequently, the tool replacement time increases, and productivity and cost efficiency decrease.

[0016] Furthermore, if the hardness of the material is reduced in order to improve machinability, there is a problem in that the strength of the material is reduced.

[0017] An object of the present invention is to provide a dental workpiece having strength suitable for dental use and excellent machinability in a sintered state. Another object of the present invention is to provide a dental workpiece that can be machined in a sintered state, requires a short machining time, suppresses wear on the machining tool, and allows a large number of dental prostheses to be machined by continuous machining using a single machining tool, thereby providing excellent productivity and cost-effectiveness. [Means for solving the problem]

[0018] The present inventors have conducted intensive research to solve the above problems, and as a result, have found that, in a dental workpiece having a biaxial bending strength of 300 MPa or more, the erosion rate is 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected in a microslurry jet erosion test, or the value of erosion rate (μm / g) × average crystal grain size (μm) is 15 μm or more. 2 / g or more, the present inventors carried out further research based on this finding and completed the present invention.

[0019] That is, the present invention includes the following inventions. [1] In a micro-slurry jet erosion test, when a spherical alumina slurry with an average particle size of 3.0 μm is projected, the erosion rate is 6.5 μm / g or more, or the value of erosion rate (μm / g) × average crystal grain size (μm) is 15 μm. 2 / g or more, A dental workpiece having a biaxial flexural strength of at least 300 MPa measured in accordance with ISO 6872:2015. [2] A dental workpiece according to [1], which has an erosion rate of 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected thereon in a microslurry jet erosion test. [3] The dental workpiece according to [1] or [2], wherein the dental workpiece is a ceramic sintered body. [4] The dental workpiece according to [3], wherein the ceramic sintered body is a sintered body containing zirconia. [5] The dental workpiece according to any one of [1] to [4], wherein the average crystal grain size of the dental workpiece is 0.05 to 15.0 μm. [6] In a micro-slurry jet erosion test, when spherical alumina slurry with an average particle size of 3.0 μm was projected, the value of erosion rate (μm / g) × average crystal grain size (μm) was 15 μm. 2 / g or more. [7] In a micro-slurry jet erosion test, when spherical alumina slurry with an average particle size of 3.0 μm was projected, the value of erosion rate (μm / g) × average crystal grain size (μm) was 15 μm. 2 / g or more, and the average crystal grain size of the dental workpiece is 3.0 μm to 15.0 μm. [8] A dental workpiece according to [5], in which in a microslurry jet erosion test, the erosion rate when a spherical alumina slurry having an average particle size of 3.0 μm is projected is 8.0 μm / g or more, and the average crystal grain size of the dental workpiece is 0.05 μm to 5.0 μm. Effect of the Invention

[0020] According to the present invention, it is possible to provide a dental workpiece having strength suitable for dental use and excellent machinability in a sintered state. Furthermore, according to the present invention, a dental workpiece having translucency suitable for dental use can be provided. Furthermore, according to the present invention, when the dental workpiece is a sintered body containing zirconia or a sintered body containing alumina, it can be machined in the sintered body state, the machining time is short, and wear of the machining tool can be suppressed. A large number of dental prostheses can be machined by continuous machining using a single machining tool (hereinafter also simply referred to as "continuous machining"), thereby providing a dental workpiece that is highly productive and economical. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic diagram showing the collision of spherical alumina particles in the MSE test of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of an MSE test apparatus used in the MSE test of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In a micro slurry-jet erosion (MSE) test (hereinafter also referred to as an "MSE test"), the dental workpiece of the present invention has an erosion rate of 6.5 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected thereon, or the value of erosion rate (μm / g)×average crystal grain size (μm) is 15 μm or more. 2 / g or more, The biaxial flexural strength measured in accordance with ISO 6872:2015 is 300 MPa or more.

[0023] The dental workpiece of the present invention is preferably a ceramic sintered body. Examples of the ceramic sintered body include a sintered body containing zirconia and a sintered body containing alumina. Hereinafter, a sintered body containing zirconia that has excellent machinability in a sintered body state is also referred to as a "machinable zirconia composite sintered body."

[0024] In one preferred embodiment, a dental workpiece is a ceramic sintered body containing zirconia. The sintered body containing zirconia means a body in which ZrO2 particles (powder) are completely sintered (sintered state). In this specification, the upper and lower limits of numerical ranges (contents of each component, ratios calculated from each component, values, and properties) can be combined as appropriate. In this specification, the mechanical processing includes cutting and grinding, and may be either wet processing or dry processing, and is not particularly limited.

[0025] The dental workpiece of the present invention has both excellent strength for dental use and machinability in a sintered state, and therefore, in an MSE test, (i) an erosion rate when a spherical alumina slurry having an average particle size of 3.0 μm is projected thereon is 6.5 μm / g or more, or (ii) the value of erosion rate (μm / g) × average crystal grain size (μm) is 15 μm or more. 2 / g or more. The dental workpiece of the present invention may satisfy both (i) and (ii).

[0026] In a preferred embodiment (hereinafter also referred to as embodiment (A)), the dental workpiece of the present invention has both excellent strength for dental use and machinability in a sintered state, and therefore has an erosion rate of 6.5 μm / g or more, preferably 8.0 μm / g or more, and more preferably 8.5 μm / g or more, when a spherical alumina slurry having an average particle size of 3.0 μm is projected in an MSE test, and from the viewpoint of excellent machinability in a sintered state, it is even more preferable that the erosion rate is 9.0 μm / g or more, particularly preferably 10.0 μm / g or more, and most preferably 12.0 μm / g or more. In embodiment (A), the upper limit of the erosion rate is not particularly limited as long as the effects of the present invention are achieved, but it is preferably 100.0 μm / g or less, more preferably 60.0 μm / g or less, even more preferably 40.0 μm / g or less, and particularly preferably 30.0 μm / g or less.

[0027] In embodiment (A), the dental workpiece of the present invention has an erosion rate within the above range. Therefore, when the dental workpiece is, for example, a ceramic sintered body (preferably a sintered body containing zirconia), it is presumed that the strength of the interface between particles (hereinafter also referred to as "grain boundary") constituting the sintered body can be weakened within a range suitable for dental use, and the machinability in the sintered body state can be improved, the machining time can be shortened, wear of the machining tools can be suppressed, and the number of dental prostheses that can be machined by continuous machining can be increased. Furthermore, by having the erosion rate be within the above range, the grain boundary strength is weakened, resulting in excellent machinability in the sintered state, while not impairing the strength suitable for dental use, making it possible to achieve both strength and machinability in the sintered state.

[0028] The MSE test method (hereinafter also referred to as the "slurry localized jet abrasion method") is one of the test methods for evaluating the mechanical properties of materials on an energy scale using fine particle projection processing technology. In the MSE test method, the amount of microparticle collisions under conditions of a constant impact speed corresponds to the applied energy, and the amount of wear at that time represents the strength of the material.

[0029] In the MSE test method, an apparatus is used that combines a part for measuring the shape of the abrasion damage caused by the collision of particles and the projection mark (erosion mark). A schematic diagram showing the collision of spherical alumina in the MSE test method is shown in Figure 1. In Figure 1, spherical alumina 1 projected from a projection nozzle collides with a sintered compact 2, and the sintered compact 2 is scraped. The projection mark (erosion mark) obtained by projecting the spherical alumina 1 is measured by the shape measurement part. Figure 1 is a partially enlarged view of the case where spherical alumina 1 projected from a projection gun 42 having a projection nozzle 50 in Figure 2 is projected onto the sintered compact 2, which is the sample W.

[0030] The MSE test device may be, for example, a device equipped with a projection unit having a projection gun and a projection nozzle, a shape measurement unit (a unit for acquiring the profile of the projection mark), and a data processing unit. An example of the MSE test device is shown in Figure 2.

[0031] In the localized slurry injection abrasion device 10 of FIG. 2, the above-mentioned slurry 34 is stored in a slurry tank 35 and stirred by an agitator 36. A slurry pressure is applied from a compressed air source 38 through a slurry pressure regulating valve 40 into the slurry tank 35 , and the slurry 34 from the slurry tank 35 is supplied to the projection gun 42 through a slurry flow meter 44 . Moreover, air pressure is supplied from the compressed air source 38 to the projection gun 42 via an air pressure regulating valve 46 and an air flow meter 48 . The projection nozzle 50 provided at the bottom of the projection gun 42 has a projection cross-sectional area of ​​1.0 mm 2 It has a nozzle of (1 mm length x 1 mm width) and is covered by the projection booth 54. The projection gun 42 mixes the supplied slurry 34 with air and sprays it locally from the projection nozzle 50 at a projection distance of 4 mm toward the dental workpiece specimen W fixed to the jig 52, forming a recess by locally wearing away the surface of the dental workpiece specimen W. The jig 52 on which the dental workpiece sample W is fixed is moved in and out of the blast booth 54 by a table drive device 56. The slurry 34 stored in the blast booth 54 is returned to the slurry tank 35 by a recovery pump 58.

[0032] As the MSE test device, a known device (for example, a slurry localized injection abrasion device (MSR-A type, manufactured by Palmeso Co., Ltd.)) can be used.

[0033] In the MSE test in this specification, a slurry in which spherical alumina with an average particle size of 3.0 μm is dispersed is projected onto a dental workpiece, which is a sintered body, to destroy the grain boundaries, and the erosion rate is calculated using the depth of the sintered body shaved off by the destruction, as calculated by the following formula. Erosion rate [μm / g] = Erosion depth [μm] ÷ Projected slurry mass [g] The measurement conditions for the MSE test in this specification are as described in the Examples section below. As the spherical alumina, a commercially available product (for example, product number: MSE-BA-3-3, manufactured by Palmeso Co., Ltd.) can be used.

[0034] The average particle size of the spherical alumina slurry used in the MSE test can be measured on a volume basis using, for example, a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation) and a 0.2% aqueous solution of sodium hexametaphosphate as a dispersion medium.

[0035] Hereinafter, the embodiment will be described taking as an example a case where the dental workpiece in the embodiment (A) is a sintered body containing zirconia. Since the dental workpiece of the present invention is not limited to a sintered body containing zirconia, the sintered body containing zirconia may be read as a sintered body containing alumina, unless otherwise stated.

[0036] The zirconia-containing sintered body preferably contains ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, Nb2O5 and / or Ta2O5, and further contains a Group I element as required. Hereinafter, as a preferred embodiment, a sintered body containing zirconia containing ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia (hereinafter, also simply referred to as a "stabilizer"), Nb2O5, and / or Ta2O5, and further containing a Group I element as necessary, will be taken as an example to explain the embodiment.

[0037] In the sintered body containing zirconia, the total content of ZrO2 and HfO2 is preferably 78 to 97.5 mol% in a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. From the viewpoint of superior translucency and strength, the total content is more preferably 79 mol% or more and 96 mol% or less, even more preferably 80 mol% or more and 94 mol% or less, and particularly preferably 81 mol% or more and 93 mol% or less. In the sintered body containing alumina, the content of Al2O3 may be interpreted as the total content of ZrO2 and HfO2 in the sintered body containing zirconia, in the total of 100 mol% of Al2O3, Nb2O5, and Ta2O5. In a preferred embodiment, the content of Al2O3 in the total of 100 mol% is preferably 78 to 99 mol%, and from the viewpoint of superior translucency and strength, the content is more preferably 80 mol% or more and 98.8 mol% or less, even more preferably 82 mol% or more and 98.5 mol% or less, and particularly preferably 83 mol% or more and 98.4 mol% or less. In addition, in the sintered body containing alumina, it is not necessary to contain a stabilizer.

[0038] Examples of stabilizers capable of suppressing the phase transition of zirconia include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide (Y2O3), cerium oxide (CeO2), scandium oxide (Sc2O3), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr2O3, Pr6O11 Examples of the oxide include samarium oxide (Sm2O3), europium oxide (Eu2O3), thulium oxide (Tm2O3), gallium oxide (Ga2O3), indium oxide (In2O3) and ytterbium oxide (Yb2O3), and Y2O3 (yttria) and / or CeO2 are preferred because they provide a better effect of the present invention and are particularly aesthetically pleasing. The stabilizers may be used alone or in combination of two or more.

[0039] In the sintered body containing zirconia, the content of the stabilizer capable of suppressing the phase transition of zirconia is preferably 1 to 12 mol%, more preferably 2 mol% or more and 10 mol% or less, in a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. From the viewpoint of superior translucency and strength, the content is further preferably 3 mol% or more and 8 mol% or less, and particularly preferably 3.5 mol% or more and 7.5 mol% or less. As a preferred embodiment, there is mentioned a sintered body containing zirconia, in which a stabilizer capable of suppressing a phase transition of zirconia contains Y2O3 and / or CeO2, and the total content of Y2O3 and CeO2 is 2 mol% or more and 10 mol% or less. Another preferred embodiment is a sintered body containing zirconia, in which a stabilizer capable of suppressing a phase transition of zirconia contains Y2O3 and the content of Y2O3 is 2 mol% or more and 10 mol% or less. In any of the above-described embodiments, the content of Y2O3 and CeO2 can be appropriately changed within the range described in this specification. For example, in order to obtain better translucency and strength, the total content of Y2O3 and CeO2 may be 2.5 mol% or more and 10 mol% or less, or 3 mol% or more and 9 mol% or less.

[0040] The reason why the sintered body containing zirconia has an erosion rate within the above-mentioned range, has strength and translucency suitable for dental use, and has high machinability, and can be machined in the sintered state is not clear, but is presumed to be as follows. In a sintered body containing zirconia, which contains ZrO2, HfO2, a stabilizer capable of suppressing a phase transition of zirconia, Nb2O5 and / or Ta2O5, and further a Group I element, the presence of the Group I element at the grain boundaries of the zirconia particles reduces the grain boundary strength, acting in a direction that makes it easier for the particles to peel off from each other, making it easier to cut, and the erosion rate falls within the above-mentioned range, so it is presumed that the machinability in the sintered body state (particularly the machinability in continuous processing) is improved while suppressing a decrease in strength.

[0041] In addition, in a sintered body containing Nb2O5 and / or Ta2O5 and zirconia, Nb2O5 and / or Ta2O5 act in the direction of coarsening the microstructure and decreasing the hardness, so that the group I element and Nb2O5 and / or Ta2O5 act together to improve the machinability. Therefore, the group I element and Nb2O5 and / or Ta2O5 act together to provide the strength required for an artificial tooth while providing excellent machinability, so that an erosion rate within the above range is obtained, and with an erosion rate within the above range, in addition to being able to shorten the machining time in the state of the sintered body by machining, it is possible to suppress the wear of the machining tool, and it is possible to increase the number of dental prostheses obtained by continuous machining using one machining tool, and it is presumed that the problems specific to continuous machining of sintered bodies can also be solved. On the other hand, even in a sintered body that does not contain Nb2O5 and / or Ta2O5 but does contain zirconia, it is presumed that by adjusting the content of the Group I element, for example by increasing it, the presence of the Group I element at the grain boundaries of the zirconia particles reduces the grain boundary strength, so that the particles are easily peeled off from each other, making them easier to cut, and the erosion rate falls within the above-mentioned range, thereby suppressing a decrease in strength and improving the machinability (particularly the machinability in continuous processing) in the sintered body state.

[0042] In the zirconia-containing sintered body of the present invention, the Group I element acts as an agent for imparting machinability as described above, and an erosion rate within the above-mentioned range is obtained without significantly impairing strength and translucency.

[0043] The content of Group I elements contained in the zirconia-containing sintered body of the present invention (particularly the sintered body containing Nb2O5 and / or Ta2O5) is preferably more than 0 mol% and 3 mol% or less, and is more preferably 0.05 mol% or more and 3 mol% or less in terms of excellent machinability in the sintered body state and the number of dental prostheses that can be continuously machined with one machining tool being increased, and is even more preferably 0.06 mol% or more and 2.5 mol% or less in terms of particularly excellent machinability in the sintered body state and the machining time being shortened, and is particularly preferably 0.07 mol% or more and 1.0 mol% or less, and is most preferably 0.08 mol% or more and 0.34 mol% or less. In the sintered body containing alumina, the content of Group I elements can also be set within the above range. In another preferred embodiment, the content of Group I elements contained in the sintered body containing zirconia but not containing Nb2O5 and / or Ta2O5 is preferably 0.5 mol% or more and 6 mol% or less, and from the viewpoint of providing superior machinability in the sintered body state and enabling a further increase in the number of dental prostheses that can be continuously machined with one machining tool, the content is more preferably 0.8 mol% or more and 5 mol% or less, even more preferably 1.0 mol% or more and 4.0 mol% or less, particularly preferably 1.2 mol% or more and 3.5 mol% or less, and most preferably 1.5 mol% or more and 3.0 mol% or less.

[0044] Examples of Group I elements include Li, Na, K, Rb, Cs, and Fr, and Li, Na, and K are preferred because they can further improve the machinability of the sintered body. The Group I elements may be used alone or in combination of two or more.

[0045] As described above, the Group I element and Nb2O5 and / or Ta2O5 act together, and therefore the effect of the stabilizer is not impaired. Therefore, the stabilizer is not particularly limited, and the effects of the present invention are achieved.

[0046] In the zirconia-containing sintered body of the present invention, the total content of Nb2O5 and Ta2O5 is preferably 1 to 9 mol%, more preferably 1.5 mol% or more and 8.5 mol% or less, based on a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. From the viewpoint of acting integrally with the Group I elements and achieving superior machinability in the sintered body state, it is even more preferably 2.5 mol% or more and 8 mol% or less, and particularly preferably 3 mol% or more and 7 mol% or less. When the total content of Nb2O5 and Ta2O5 is 1 mol% or more, sufficient machinability is easily obtained in the sintered state. When the total content of Nb2O5 and Ta2O5 is 9 mol% or less, the occurrence of chipping and the like in the obtained dental workpiece is suppressed, and sufficient physical properties are easily obtained. In the alumina-containing sintered body of the present invention, the total content of Nb2O5 and Ta2O5, relative to a total of 100 mol% of Al2O3, Nb2O5, and Ta2O5, is preferably 0.5 mol% or more and 9 mol% or less, more preferably 0.8 mol% or more and 8.5 mol% or less, and from the viewpoint of acting integrally with the Group I elements and achieving superior machinability in the sintered body state, is further preferably 1.0 mol% or more and 8 mol% or less, and particularly preferably 1.5 mol% or more and 7 mol% or less. When the total content of Nb2O5 and Ta2O5 is 0.5 mol% or more, sufficient machinability is easily obtained in the sintered state. When the total content of Nb2O5 and Ta2O5 is 9 mol% or less, the occurrence of chipping and the like in the obtained dental workpiece is suppressed, and sufficient physical properties are easily obtained.

[0047] As described above, Nb2O5 and Ta2O5 act to coarsen the microstructure and reduce hardness, and act together with Group I elements to impart excellent machinability. In addition, by interacting with other components (e.g., TiO2, Al2O3) added to the zirconia-containing sintered body and by applying HIP, the sintered density can be maximized, ensuring the aesthetics of natural teeth.

[0048] In this specification, the content of each component in the dental workpiece can be calculated from the charged amount of the raw material. In addition, the content of each of the components ZrO2, HfO2, stabilizer, Nb2O5, and Ta2O5 in the dental workpiece can also be measured by, for example, inductively coupled plasma (ICP) emission spectrometry, fluorescent X-ray analysis, or the like. The content (mol%) of Group I elements is the external addition rate relative to the total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. Therefore, the content of Group I elements in the dental workpiece can be calculated by converting the amount (mass) of the raw material added at the time of addition into mol%. The content (mass%) of the zirconia reinforcement is the external addition rate relative to the total of 100 mass% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. Therefore, the content of the zirconia reinforcement in the dental workpiece can be calculated from the amount (mass) of the raw material added when added.

[0049] The content of each of the above-mentioned ZrO2, HfO2, stabilizer, Nb2O5, and Ta2O5 components is the percentage relative to the total of 100 mol% of ZrO2, HfO2, stabilizer, Nb2O5, and Ta2O5, and the total of ZrO2, HfO2, stabilizer, Nb2O5, and Ta2O5 does not exceed 100 mol%. For example, when the raw material composition contains Nb2O5 but does not contain Ta2O5, the content of each of the ZrO2, HfO2, stabilizer, and Nb2O5 components means the content percentage relative to the total of 100 mol% of ZrO2, HfO2, stabilizer, and Nb2O5.

[0050] Furthermore, when the content of the stabilizer is A mol % and the total content of Nb2O5 and Ta2O5 is B mol %, the ratio A / B is preferably 0.9 to 3 inclusive from the viewpoint of machinability, and more preferably 0.95 to 2 inclusive, and even more preferably 1 to 1.6 inclusive, since this enhances the effect of the Group I element and Nb2O5 and / or Ta2O5 acting together, thereby imparting better machinability, suppressing wear of the machining tool, and enabling a further increase in the number of dental prostheses obtained by continuous machining using one machining tool.

[0051] In one preferred embodiment (A-1), in a microslurry jet erosion test, the erosion rate is 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected, The biaxial bending strength measured in accordance with ISO 6872:2015 is 300 MPa or more. Contains ZrO2, HfO2, a stabilizer capable of suppressing a phase transition of zirconia, and Nb2O5 and / or Ta2O5; In the case where the total amount of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5 is 100 mol%, The total content of ZrO2 and HfO2 is 78 to 97.5 mol%, The content of the stabilizer is 1 to 12 mol %, The total content of Nb2O5 and Ta2O5 is 1 to 9 mol%, Further containing a Group I element, the stabilizer comprises Y2O3 and / or CeO2; The content of the Group I element is more than 0 mol% and 3 mol% or less with respect to a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5, When the content of the stabilizer is A mol % and the total content of Nb2O5 and Ta2O5 is B mol %, the dental workpiece has an A / B ratio of 0.9 or more and 3 or less.

[0052] One embodiment (A-2) of the present invention is a dental workpiece comprising, in addition to ZrO2, HfO2, a stabilizer capable of inhibiting the phase transformation of zirconia, Nb2O5 and / or Ta2O5, and a Group I element, a zirconia reinforcement agent. The zirconia strengthening agent means a strength improving agent that acts together with Group I elements in a dental workpiece containing ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, and Nb2O5 and / or Ta2O5, and can improve the strength of the sintered body.

[0053] As described above, even in dental workpieces containing zirconia reinforcement, the total content of ZrO2 and HfO2, the type and content of stabilizer, the total content of Nb2O5 and Ta2O5, the type and content of Group I elements, and the A / B ratio can be changed as appropriate.

[0054] In dental workpieces containing a zirconia reinforcing agent, the content of the zirconia reinforcing agent is preferably more than 0 mass% and not more than 5.0 mass%, relative to a total of 100 mass% of ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, Nb2O5, and Ta2O5. Because the zirconia reinforcing agent acts together with a Group I element when combined with the Group I element to provide superior strength, the content of the zirconia reinforcing agent is more preferably 0.01 mass% to 4.5 mass%, and even more preferably 0.5 mass% to 4.0 mass%.

[0055] Examples of the zirconia reinforcing agent include TiO2, Al2O3, etc. The zirconia reinforcing agent may be used alone or in combination of two or more kinds.

[0056] Another preferred embodiment is a dental workpiece in which the zirconia reinforcing agent contains TiO2 and the TiO2 content is 0.6 to 3.7 mass % in any of the above-mentioned embodiments.

[0057] In one preferred embodiment, in a microslurry jet erosion test, the erosion rate is 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected; The biaxial bending strength measured in accordance with ISO 6872:2015 is 300 MPa or more. Contains ZrO2, HfO2, a stabilizer capable of suppressing a phase transition of zirconia, and Nb2O5 and / or Ta2O5; In the case where the total amount of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5 is 100 mol%, The total content of ZrO2 and HfO2 is 78 to 97.5 mol%, The content of the stabilizer is 1 to 12 mol %, The total content of Nb2O5 and Ta2O5 is 1 to 9 mol%, Further containing a Group I element, the stabilizer comprises Y2O3 and / or CeO2; The zirconia reinforcement agent contains TiO2, and the TiO2 content is 0.6 to 3.7 mass%; The content of the Group I element is more than 0 mol% and 3 mol% or less with respect to a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5, When the content of the stabilizer is A mol % and the total content of Nb2O5 and Ta2O5 is B mol %, the dental workpiece has an A / B ratio of 0.9 or more and 3 or less. As described above, by setting the erosion rate within the above range, the material has a strength suitable for dental use, even in various compositions, and has excellent machinability (particularly machinability in continuous processing) in the sintered state.

[0058] The average crystal grain size of the dental workpiece of the present invention is preferably 0.05 to 15.0 μm, and from the viewpoint of superior machinability, strength and translucency in the sintered state, is more preferably 0.1 to 10.0 μm, further preferably 0.3 to 7.0 μm, and particularly preferably 0.5 to 5.0 μm. The method for measuring the average crystal grain size is as described in the Examples below. The average crystal grain size can be measured by adjusting the number of particles so that the number of particles contained in one field of view of an SEM photograph is about 50 or 100, in the method described in the Examples.

[0059] In embodiment (A), the average crystal grain size of the dental workpiece is preferably 0.05 μm to 5.0 μm, from the viewpoints of efficient use of energy from the projection of the alumina particles in grain boundary fracture and excellent machinability in the sintered state, and more preferably 0.08 to 4.0 μm, even more preferably 0.1 to 3.5 μm, and particularly preferably 0.3 to 3.0 μm, from the viewpoints of excellent machinability, strength, and translucency in the sintered state.

[0060] In a preferred embodiment (hereinafter also referred to as embodiment (B)), the dental workpiece of the present invention has both excellent strength for dental use and machinability in a sintered state, and therefore has an erosion rate (μm / g)×average crystal grain size (μm) value of 15 μm when a spherical alumina slurry having an average grain size of 3.0 μm is projected in an MSE test. 2 / g or more, and has excellent machinability in the sintered state. 2 / g or more, and 23 μm 2 / g or more is more preferable, and 25 μm 2 / g or more is more preferable, and 30 μm 2 / g or more is particularly preferred. In embodiment (B), the upper limit of the erosion rate (μm / g)×average crystal grain size (μm) is not particularly limited as long as the effects of the present invention are achieved. 2 / g or less, and2 / g or less is more preferable, and 65 μm 2 / g or less is more preferable, and 50 μm 2 / g or less is particularly preferred.

[0061] The MSE test method, MSE test device, and measurement method and conditions for the erosion rate (μm / g) and average crystal grain size (μm) in embodiment (B) are the same as those in embodiment (A).

[0062] In embodiment (B), the average crystal grain size of the dental workpiece may be 0.05 to 15.0 μm. From the viewpoint of excellent machinability in the sintered body state, however, it is preferably 3.0 μm to 15.0 μm, more preferably 4.0 to 15.0 μm, even more preferably 5.0 to 15.0 μm, and particularly preferably 5.5 to 15.0 μm.

[0063] In embodiment (B), although the dental workpiece of the present invention does not contain a Group I element, by adjusting the firing time during preparation of the primary sintered body, for example, to be significantly longer, the erosion rate (μm / g) x average crystal grain size (μm) is within the above-mentioned range. Therefore, when the dental workpiece is, for example, a ceramic sintered body (preferably a sintered body containing zirconia), it is presumed that the strength of the interface (hereinafter also referred to as "grain boundary") of the particles constituting the sintered body can be weakened within a suitable range for dental use, and the machinability in the sintered body state is excellent, the machining time can be shortened, wear of the machining tool can be suppressed, and the number of dental prostheses that can be machined by continuous machining can be increased. Regarding this erosion rate (μm / g) x average crystal grain size (μm), the denominator (g) in the unit of erosion rate (μm / g) indicates the mass of alumina slurry injected per unit time, and can be considered as the work done on the sample since the alumina slurry is injected onto the sample at a constant speed on average. The numerator (μm) is the actual measurement of the depth of the sample scraped off by the injection of the alumina slurry. In other words, the average crystal grain size x erosion rate is the average grain size per unit area (μm 2 ) can be scraped off (μm 2 / W). Therefore, it can be said that there is a correlation between this value and machinability, and further, in the dental workpiece of the present invention, when the erosion rate (μm / g) × average crystal grain size (μm) is within the above range, the machinability is significantly improved. Furthermore, in the dental workpiece of the present invention, by having the erosion rate (μm / g)×average crystal grain size (μm) within the above-mentioned range, the grain boundary strength is weakened, resulting in excellent machinability in the sintered state, while not impairing the strength suitable for dental use, making it possible to achieve both strength and machinability in the sintered state.

[0064] Furthermore, in embodiment (B), although not particularly limited, the erosion rate may be 8.0 μm / g or more, or may be less than 8.0 μm / g, or may be 6.5 μm / g or more, less than 6.5 μm / g, or 6.0 μm / g or less. In embodiment (B), the erosion rate may overlap with that of embodiment (A) or may be excluded, so long as the effects of the present invention are obtained. In the embodiment (B), when the erosion rate is 6.5 μm / g or more, a suitable erosion rate for the embodiment (A) can be appropriately set.

[0065] Hereinafter, the embodiment will be described taking as an example a case in which the dental workpiece in embodiment (B) is a sintered body containing zirconia. The dental workpiece of the present invention is not limited to a sintered body containing zirconia, and therefore a sintered body containing zirconia may be read as, for example, a sintered body containing alumina.

[0066] As a preferred embodiment (B-1), the zirconia-containing sintered body in embodiment (B) is a zirconia-containing sintered body containing ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, Nb2O5 and / or Ta2O5, and further containing a Group I element as necessary.

[0067] Another preferred embodiment (B-2) is a sintered body containing zirconia that does not contain a Group I element and contains ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, and Nb2O5 and / or Ta2O5.

[0068] In embodiment (B), including embodiments (B-1) and (B-2), the total content of ZrO2 and HfO2, the type and content of the stabilizer capable of suppressing a phase transition of zirconia, the total content of Nb2O5 and Ta2O5, the type and content of Group I elements, and the content of the stabilizer are A mol %, and the total content of Nb2O5 and Ta2O5 is B mol %, respectively, and the ratio A / B and the type and content of the zirconia reinforcement agent are the same as those in embodiment (A).

[0069] In both the embodiment (A) and the embodiment (B), the density of the processable zirconia composite sintered body is set to 5.5 g / cm because the higher the density, the fewer the internal voids, the less likely the light is to be scattered, the better the translucency, and the better the strength. 3 It is preferable that the content is 5.7 g / cm or more. 3 More preferably, it is 5.9 g / cm or more. 3 More preferably, it is equal to or greater than this. It is particularly preferable that the workable zirconia composite sintered body contains substantially no voids. The density of the compound sintered body can be calculated by (mass of the compound sintered body) / (volume of the compound sintered body).

[0070] In an embodiment of the sintered body containing zirconia, the method for producing a dental workpiece of the present invention includes, for example, a sintered body containing ZrO2, HfO2, a stabilizer capable of suppressing a phase transition of zirconia, and Nb2O5 and / or Ta2O5, In the case where the total amount of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5 is 100 mol%, The total content of ZrO2 and HfO2 is 78 to 97.5 mol%, The content of the stabilizer is 1 to 12 mol %, The total content of Nb2O5 and Ta2O5 is 1 to 9 mol%, a step of producing a molded body using a raw material composition, which may further contain a raw material compound of a Group I element as necessary; and sintering the green body.

[0071] In the following, unless otherwise stated, each condition can be applied to any embodiment of the manufacturing method. For example, in the embodiment of the sintered body containing alumina, in the manufacturing method of the dental workpiece in which the dental workpiece is a sintered body containing zirconia, ZrO2 and HfO2 can be replaced with Al2O3, the components can be changed such that the stabilizer is not included, and the content of each component can be adjusted within the range described in this specification.

[0072] The raw material composition used in the manufacture of a dental workpiece contains ZrO2, HfO2, a stabilizer capable of suppressing the phase transition of zirconia, Nb2O5 and / or Ta2O5, and, if necessary, a raw material compound of a group I element. The raw material composition used in the manufacture of a dental workpiece may be in a dry state, or may be in a state containing a liquid or in a state contained in a liquid. The raw material composition may be in the form of, for example, a powder, granules or granulated material, a paste, a slurry, or the like.

[0073] In a preferred embodiment, the raw material composition contains a raw material compound of a Group I element so that the resulting dental workpiece contains an element of Group I. Examples of the raw material compound of a Group I element include hydroxides and / or salts of the Group I element. In certain other preferred embodiments, the source composition does not include source compounds of Group I elements. When the raw material composition does not contain a raw material compound of a Group I element, the value of erosion rate (μm / g) × average crystal grain size (μm) can be adjusted to fall within a predetermined range by significantly increasing the sintering temperature (maximum sintering temperature) at which the molded body described below is sintered.

[0074] Examples of hydroxides of Group I elements include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, and francium hydroxide. Examples of salts of Group I elements include carbonates and hydrogen carbonates. Examples of carbonates of Group I elements include lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, francium carbonate, and cesium carbonate. Group I hydrogen carbonates include lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, rubidium hydrogen carbonate, francium hydrogen carbonate, and cesium hydrogen carbonate. The hydroxides and salts of Group I elements may each be used alone or in combination of two or more.

[0075] For ZrO2 and HfO2, commercially available zirconia powder can be used. Examples of commercially available products include zirconia powder (trade name "Zpex (registered trademark)" (Y2O3 content: 3 mol%), "Zpex (registered trademark) 4" (Y2O3 content: 4 mol%), "Zpex (registered trademark) 4" (Y2O3 content: 4 mol%), Smile (registered trademark) (Y2O3 content: 5.5 mol%), TZ-3Y (Y2O3 content: 3 mol%), TZ-3YS (Y2O3 content: 3 mol%), TZ-4YS (Y2O3 content: 4 mol%), TZ-6Y (Y2O3 content: 6 mol%), TZ-6YS (Y2O3 content: 6 mol%), TZ-8YS (Y2O3 content: 8 mol%), TZ-10YS (Y2O3 content: 10 mol%), TZ-3Y-E (Y2O3 content: 3 mol%) "TZ-3YS-E" (Y2O3 content: 3 mol%), "TZ-3YB-E" (Y2O3 content: 3 mol%), "TZ-3YSB-E" (Y2O3 content: 3 mol%), "TZ-3YB" (Y2O3 content: 3 mol%), "TZ-3YSB" (Y2O3 content: 3 mol%), "TZ-3Y20AB" (Y2O3 content: 3 mol%), "TZ-8YSB" (Y2O3 content: 8 mol%), "TZ-0" (Y2O3 content: 0 mol%); all manufactured by Tosoh Corporation. The commercially available zirconia powder also contains HfO2. Commercially available products that also contain Y2O3 can also be used. As the zirconia powder, the raw material composition of the present invention can also use zirconia powder in which Y2O3 is uniformly dispersed and solid-solved, such as the commercially available TZ series (part of the product name includes "TZ").

[0076] There are no particular limitations on the method for producing the zirconia powder, and any known method can be used, such as a breakdown process in which coarse particles are pulverized into fine powder, or a building-up process in which zirconia powder is synthesized from atoms or ions through a nucleation and growth process.

[0077] The type of zirconia powder in the raw material composition is not particularly limited, and when the zirconia powder contains ZrO2 and HfO2 and does not contain a stabilizer, or when the content of the stabilizer is increased as necessary, stabilizer particles can be added separately. The stabilizer particles are not particularly limited as long as the content of the stabilizer contained in the dental workpiece can be adjusted to the above-mentioned predetermined range. The particles of the stabilizer may be, for example, a commercially available product, or a powder of the commercially available product may be ground in a known grinding and mixing device (such as a ball mill) before use.

[0078] In a preferred embodiment, the method for producing a dental workpiece includes a stabilizer (preferably, Y2O3) that is not solid-dissolved in ZrO2 and HfO2, because this is one of the factors that makes it easy to obtain a target dental workpiece from the raw material composition. The fact that the stabilizer includes one that is not solid-dissolved in zirconia can be confirmed, for example, by an X-ray diffraction (XRD) pattern.

[0079] When a peak attributable to the stabilizer is confirmed in the XRD pattern of the raw material composition or the molded body, it means that the stabilizer is present in the raw material composition or the molded body without being dissolved in ZrO2 and HfO2. When the entire amount of the stabilizer is dissolved in ZrO2 and HfO2, basically, no peaks derived from the stabilizer are observed in the XRD pattern. However, depending on the conditions such as the crystal state of the stabilizer, even if there is no stabilizer peak in the XRD pattern, the stabilizer may not be dissolved in ZrO2 and HfO2.

[0080] The case where the stabilizer includes a stabilizer that is not solid-dissolved in ZrO2 and HfO2 will be described below by taking an example in which the stabilizer is yttria.

[0081] In the raw material composition or molded body of the present invention, the abundance rate f of yttria that is not dissolved in ZrO2 and HfO2 (hereinafter sometimes referred to as "undissolved yttria") isy can be calculated based on the following formula (1). f y =I 29 / (I 28 +I 29 +I 30 ) x 100 (In the formula, f y represents the percentage of undissolved yttria (%). In the XRD measurement, I 28 represents the integrated intensity of the peak at 2θ = 28° where the main monoclinic peak appears, and I 29 represents the intensity of the peak at 2θ = 29° where the main peak of yttria appears, and I 30 represents the integrated intensity of the peak near 2θ=30° where the main peak of the tetragonal or cubic crystal system appears.)

[0082] In addition, when a stabilizer other than yttria is used, I 29 By substituting the peak of another stabilizer instead of yttria, the above formula can also be applied to calculate the undissolved fraction of stabilizers other than yttria.

[0083] Undissolved yttria abundance f y From the viewpoint of facilitating the production of the intended dental workpiece, the content of undissolved yttria f is preferably greater than 0%, more preferably 1% or more, even more preferably 2% or more, and particularly preferably 3% or more. y The upper limit may be, for example, 25% or less, but preferably depends on the content of yttria in the raw material composition or the molded body.

[0084] For example, when the content of yttria in the raw material composition or the molded body of the present invention is 3 mol% or more and 8 mol% or less, when the content of yttria is 3 mol% or more and less than 4.5 mol%, f y When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f y When the yttria content is 5.8 mol% or more and 8 mol% or less, f ymay be no more than 25%.

[0085] For example, when the yttria content is 3 mol% or more and less than 4.5 mol%, f y is preferably 2% or more, more preferably 3% or more, even more preferably 4% or more, and particularly preferably 5% or more. When the yttria content is 4.5 mol% or more and less than 5.8 mol%, f y is preferably 3% or more, more preferably 4% or more, even more preferably 5% or more, even more preferably 6% or more, and particularly preferably 7% or more. When the yttria content is 5.8 mol% or more and 8 mol% or less, f y is preferably 4% or more, more preferably 5% or more, even more preferably 6% or more, even more preferably 7% or more, and particularly preferably 8% or more.

[0086] In the raw material composition or molded body of the present invention, the entire stabilizer does not have to be solid-dissolved in ZrO2 and HfO2. In the present invention, the stabilizer being solid-dissolved means, for example, that an element (atom) contained in the stabilizer is solid-dissolved in ZrO2 and HfO2.

[0087] The Nb2O5 and / or Ta2O5 added to the raw material composition of the present invention is not particularly limited as long as the content of Nb2O5 and / or Ta2O5 contained in the dental workpiece can be adjusted to the above-mentioned predetermined range. Nb2O5 and / or Ta2O5 are not particularly limited, and for example, commercially available products may be used, or the commercially available powder may be ground with a known grinding and mixing device (such as a ball mill) before use.

[0088] The process for preparing the raw material composition may, for example, be a method in which the raw materials of the raw material composition (ZrO2, HfO2, a stabilizer, Nb2O5 and / or Ta2O5, a raw material compound of a Group I element (e.g., a hydroxide and / or a salt of a Group I element), and further a zirconia reinforcement agent as necessary) are wet-mixed in a solvent containing water to obtain the raw material composition.

[0089] The method for wet-mixing the raw materials in a solvent containing water is not particularly limited. For example, the raw materials may be wet-pulverized and mixed in a known pulverizing and mixing device (such as a ball mill) to form a slurry, and then the slurry may be dried and granulated to produce a granular raw material composition.

[0090] In the wet mixing step, additives such as a binder, a plasticizer, a dispersant, an emulsifier, an antifoaming agent, a pH adjuster, a lubricant, etc. may be further included. Each of the additives may be used alone or in combination of two or more kinds.

[0091] The binder may be added after milling a primary powder of a mixture of ZrO2, HfO2, Y2O3, Nb2O5 and / or Ta2O5, and hydroxides and / or salts of Group I elements in water to form a slurry.

[0092] The binder is not particularly limited, and known binders can be used. Examples of binders include polyvinyl alcohol binders, acrylic binders, wax binders (paraffin wax, etc.), methyl cellulose, carboxymethyl cellulose, polyvinyl butyral, polymethyl methacrylate, ethyl cellulose, polyethylene, polypropylene, ethylene-vinyl acetate copolymers, polystyrene, atactic polypropylene, and methacrylic resins.

[0093] Examples of the plasticizer include polyethylene glycol, glycerin, propylene glycol, and dibutyl phthalate.

[0094] Examples of dispersants include ammonium polycarboxylate (e.g., triammonium citrate), ammonium polyacrylate, acrylic copolymer resin, acrylic acid ester copolymer, polyacrylic acid, bentonite, carboxymethyl cellulose, anionic surfactants (e.g., polyoxyethylene alkyl ether phosphates such as polyoxyethylene lauryl ether phosphate), nonionic surfactants, olein glyceride, amine salt surfactants, oligosaccharide alcohols, and stearic acid.

[0095] Examples of the emulsifier include alkyl ethers, phenyl ethers, sorbitan derivatives, and ammonium salts.

[0096] Examples of the defoaming agent include alcohol, polyether, silicone, wax, and the like.

[0097] Examples of pH adjusters include ammonia, ammonium salts (including ammonium hydroxides such as tetramethylammonium hydroxide), and the like.

[0098] Examples of the lubricant include polyoxyethylene alkylate ether and wax.

[0099] The solvent used in the wet mixing is not particularly limited as long as it contains water, and an organic solvent may be used, a mixed solvent of water and an organic solvent may be used, or only water may be used. Examples of the organic solvent include ketone solvents such as acetone and ethyl methyl ketone; alcohol solvents such as ethanol, 1-propanol, 2-propanol, 2-methyl-2-propanol, glycerin, diglycerin, polyglycerin, propylene glycol, dipropylene glycol, polypropylene glycol, ethylene glycol, diethylene glycol, polyethylene glycol, polyethylene glycol monomethyl ether, 1,2-pentanediol, 1,2-hexanediol, and 1,2-octanediol.

[0100] The raw material composition of the dental workpiece used in the present invention may contain ZrO2, Y2O3, Nb2O5, Ta2O5, hydroxides and / or salts of Group I elements, and other components other than the zirconia reinforcement agent as necessary, as long as the effects of the present invention are achieved. Examples of such other components include colorants (pigments and composite pigments), fluorescent agents, SiO2, etc. Each of the other components may be used alone, or two or more may be mixed.

[0101] Examples of the pigment include oxides of at least one element selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb, and Er (specifically, NiO, Cr2O3, etc.), and oxides of at least one element selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, and Tb are preferred, and oxides of at least one element selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd, and Tb are more preferred. However, Y2O3 and CeO2 may be excluded from the pigment.

[0102] Examples of the composite pigment include (Zr,V)O2, Fe(Fe,Cr)2O4, (Ni,Co,Fe)(Fe,Cr)2O4·ZrSiO4, and (Co,Zn)Al2O4.

[0103] Examples of the fluorescent agent include Y2SiO5:Ce, Y2SiO5:Tb, (Y,Gd,Eu)BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, and BaMgAl 10 O 17 :Eu, etc.

[0104] Next, the obtained raw material composition is molded to produce a molded body. The molding method is not particularly limited, and a known method (for example, press molding, etc.) can be used.

[0105] In the case of producing a zirconia molded body by a method having a step of press-molding a raw material composition, the specific method of press molding is not particularly limited, and can be performed using a known press molding machine. Specific examples of the press molding method include uniaxial pressing.

[0106] The pressing pressure is set to an appropriate optimum value depending on the size, open porosity, biaxial bending strength, and particle size of the raw material powder of the target molded body, and is usually 5 MPa to 1000 MPa. By increasing the pressing pressure during molding in the above-mentioned manufacturing method, the pores of the obtained molded body are filled more, the open porosity can be set low, and the density of the molded body can be increased. In addition, in order to increase the density of the obtained zirconia molded body, a cold isostatic pressing (CIP) treatment may be further performed after uniaxial pressing.

[0107] Next, the resulting green body is sintered. The term "molded body" refers to a body that has not yet reached a semi-sintered state (calcined state) or a sintered state. In other words, the molded body is distinguished from the calcined body and the sintered body in that the molded body is a body that has been molded and then not sintered. The sintering temperature (maximum sintering temperature) for obtaining a dental workpiece is, for example, preferably 1300°C or higher, more preferably 1350°C or higher, even more preferably 1400°C or higher, even more preferably 1450°C or higher, and particularly preferably 1500°C or higher. The sintering temperature is, for example, preferably 1680°C or lower, more preferably 1650°C or lower, and even more preferably 1600°C or lower. In the method for producing the dental workpiece of the present invention, it is preferable to sinter a molded body at a maximum sintering temperature of 1300 to 1680°C. The maximum sintering temperature is preferably a temperature in the atmosphere.

[0108] From the viewpoint of keeping the erosion rate (μm / g) within the range according to embodiment (A), when the molded body is obtained from a raw material composition containing a raw material compound of a Group I element and contains a raw material compound of a Group I element, the holding time (holding time) at the maximum sintering temperature is preferably 30 hours or less, more preferably 20 hours or less, even more preferably 10 hours or less, even more preferably 5 hours or less, particularly preferably 3 hours or less, and most preferably 2 hours or less, depending on the temperature. Furthermore, the holding time can be 25 minutes or less, 20 minutes or less, or 15 minutes or less. Moreover, the holding time is preferably 1 minute or more, more preferably 5 minutes or more, and even more preferably 10 minutes or more. According to the manufacturing method of the present invention, a dental workpiece excellent in bending strength, translucency, and machinability can be produced according to the content of the stabilizer. Moreover, the sintering time may be shortened as long as the effect of the present invention can be obtained. By shortening the sintering time, it is possible to increase production efficiency and reduce energy costs. Regarding embodiment (B), when the molded body does not contain a raw material compound of a Group I element, the holding time (retention time) at the maximum sintering temperature can be set to 41 hours or more, 45 hours or more, or even 50 hours or more, since the value of erosion rate (μm / g)×average crystal grain size (μm) can be adjusted to fall within a predetermined range. Furthermore, the holding time can be set to 200 hours or less, 150 hours or less, or 120 hours or less.

[0109] In the method for producing a dental workpiece of the present invention, when the molded body is sintered, the heating rate is not particularly limited, and is preferably 0.1°C / min or more, more preferably 0.2°C / min or more, and even more preferably 0.5°C / min or more. The heating rate is preferably 50°C / min or less, more preferably 30°C / min or less, and even more preferably 20°C / min or less. By setting the heating rate at or above the lower limit, productivity is improved.

[0110] A general dental zirconia firing furnace can be used in the step of sintering the molded body. Commercially available dental zirconia firing furnaces may be used. Examples of commercially available products include Noritake Katana (registered trademark) F-1, F-1N, and F-2 (all manufactured by SK Medical Electronics Co., Ltd.).

[0111] Furthermore, the step of sintering the molded body preferably includes a step of hot isostatic pressing (HIP) treatment in addition to sintering at the maximum sintering temperature described above. The HIP treatment can further improve the translucency and strength of the dental workpiece.

[0112] Hereinafter, the sintered body obtained by sintering at the above-mentioned maximum sintering temperature is referred to as a "primary sintered body", and the sintered body after the HIP treatment is referred to as a "HIP-treated sintered body".

[0113] The HIP treatment can be carried out using a known hot isostatic press (HIP) device.

[0114] The temperature of the HIP treatment is not particularly limited, but since a dense dental workpiece with high strength can be obtained, the HIP temperature is preferably 1200° C. or higher, more preferably 1300° C. or higher, and even more preferably 1400° C. or higher. The HIP temperature is preferably 1700° C. or lower, more preferably 1650° C. or lower, and even more preferably 1600° C. or lower.

[0115] In the manufacturing method of the dental workpiece of the present invention, when the primary sintered body is subjected to HIP treatment, the HIP pressure is not particularly limited, and since a dense sintered body with high strength can be obtained, the HIP pressure is preferably 100 MPa or more, more preferably 125 MPa or more, and even more preferably 130 MPa or more. The upper limit of the HIP pressure is not particularly limited, but can be, for example, 400 MPa or less, 300 MPa or less, or even 200 MPa or less.

[0116] In the method for producing a dental workpiece of the present invention, when the primary sintered body is subjected to HIP treatment, the heating rate is not particularly limited, and is preferably 0.1°C / min or more, more preferably 0.2°C / min or more, and even more preferably 0.5°C / min or more. The heating rate is preferably 50°C / min or less, more preferably 30°C / min or less, and even more preferably 20°C / min or less. By setting the heating rate at or above the lower limit, productivity is improved.

[0117] In the manufacturing method of the dental workpiece of the present invention, when the primary sintered body is subjected to HIP treatment, the HIP time is not particularly limited, and since a dense dental workpiece with high strength can be obtained, the HIP treatment time is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. Also, the HIP treatment time is preferably 10 hours or less, more preferably 6 hours or less, and even more preferably 3 hours or less.

[0118] In the manufacturing method of the dental workpiece of the present invention, when the primary sintered body is HIP-treated, the pressure medium is not particularly limited, and from the viewpoint of having little effect on zirconia, the pressure medium can be at least one selected from the group consisting of oxygen, oxygen containing 3% hydrogen, air, and inert gases (e.g., nitrogen, argon, etc.). When the primary sintered body is subjected to the HIP treatment in an oxygen mixed gas atmosphere, the oxygen concentration is not particularly limited, but can be, for example, more than 0% and 20% or less. When an oxygen mixed gas is used, at least one inert gas (eg, nitrogen, argon, etc.) can be selected as the gas other than oxygen.

[0119] In the manufacturing method of the dental workpiece of the present invention, if the HIP treatment is performed in a reducing atmosphere, such as by using an inert gas, blackening may occur due to oxygen defects. In that case, in order to remove the blackening, it is preferable to include a step of heat treatment in air or in an oxygen-rich atmosphere at 1650°C or less (hereinafter also referred to as "tempering treatment") after the HIP treatment step, and from the viewpoint of efficient heat treatment, it is more preferable to perform the heat treatment in an oxygen-rich atmosphere. An oxygen-rich atmosphere means that the oxygen concentration is higher than that of air. The oxygen-rich atmosphere is not particularly limited as long as the oxygen concentration is more than 21% and 100% or less, and can be appropriately selected from this range. For example, the oxygen concentration may be 100%.

[0120] The dental workpiece of the present invention is not particularly limited as long as it exhibits the effects of the present invention, and may be a primary sintered body, a HIP-treated sintered body, or a sintered body after tempering treatment. One preferred embodiment is a dental workpiece that is a sintered body after tempering.

[0121] Depending on the aesthetics of the dental workpiece (eg, the shade of a dental prosthesis), the temperature of the heat treatment in air or in an oxygen-rich atmosphere can be appropriately changed. In a preferred embodiment, the temperature of the heat treatment in air or in an oxygen-rich atmosphere is preferably 1650°C or less, more preferably 1600°C or less, and even more preferably 1550°C or less, from the standpoint of the aesthetics of the dental workpiece. In another preferred embodiment, the temperature of the heat treatment in air or in an oxygen-rich atmosphere is preferably 1400°C or less, more preferably 1300°C or less, and even more preferably 1200°C or less, from the standpoint of the aesthetics of the dental workpiece. Furthermore, in any embodiment, the temperature of the heat treatment is preferably 500° C. or higher, more preferably 600° C. or higher, and even more preferably 700° C. or higher.

[0122] A general dental zirconia firing furnace can be used for the tempering treatment. Commercially available dental zirconia firing furnaces may be used. Examples of commercially available products include Noritake Katana (registered trademark) F-1, F-1N, and F-2 (all manufactured by SK Medical Electronics Co., Ltd.).

[0123] Although the dental workpiece of the present invention is a sintered body, it has excellent machinability, so there is no need to machine the semi-sintered calcined body in the form of a mill blank and then sinter it to form a sintered body. On the other hand, a method for producing a dental workpiece may also be a method in which a molded body obtained using the raw material composition is calcined to produce a calcined body in a semi-sintered state, and the unprocessed calcined body is machined to produce a sintered body.

[0124] In the case where the dental workpiece is a sintered body containing zirconia, another embodiment includes a method for producing a dental workpiece, the method including a step of producing a molded body using the raw material composition, a step of calcining the obtained molded body to obtain a zirconia calcined body (calcining step), and a step of sintering the zirconia calcined body.

[0125] In order to ensure blocking, the firing temperature (calcination temperature) in the calcination step is, for example, preferably 800° C. or higher, more preferably 900° C. or higher, and even more preferably 950° C. or higher. The calcination temperature is, for example, preferably 1200° C. or lower, more preferably 1150° C. or lower, and even more preferably 1100° C. or lower. The calcination temperature is, for example, preferably 800° C. to 1200° C. At such a calcination temperature, it is considered that the dissolution of the stabilizer does not progress significantly in the calcination step.

[0126] The zirconia calcined body of the present invention means a body in which ZrO2 particles are necked (adhered) to each other and the ZrO2 particles (powder) are in a state where they are not completely sintered (semi-sintered state).

[0127] The density of the calcined zirconia body is 2.7 g / cm 3The density of the calcined zirconia body is preferably 4.0 g / cm 3 Less than 3.8 g / cm is preferred. 3 Less than 3.6 g / cm is more preferable. 3 The following is even more preferable. When the density is within this range, processing can be easily performed. The density of the calcined body can be calculated, for example, by dividing the mass of the calcined body by the volume of the calcined body.

[0128] The three-point bending strength of the zirconia calcined body is preferably from 15 to 70 MPa, more preferably from 18 to 60 MPa, and even more preferably from 20 to 50 MPa. The bending strength can be measured using a test piece having a thickness of 5 mm, a width of 10 mm, and a length of 50 mm, in accordance with ISO 6872:2015, except for the size of the test piece. The face of the test piece and the C face (the face of the test piece with the corners chamfered at an angle of 45°) are surface-finished in the longitudinal direction with 600-grit sandpaper. The test piece is arranged so that the widest face faces vertically (load direction). In the bending test measurement, the span is 30 mm, and the crosshead speed is 1.0 mm / min.

[0129] The step of sintering the zirconia calcined body can be carried out by the same method and under the same conditions (temperature, pressure, etc.) as the step of sintering the molded body described above. Therefore, in the embodiment of the production method using the zirconia calcined body, the "molded body" can be read as the "calcined body".

[0130] The dental workpiece of the present invention has excellent strength. The biaxial bending strength of the dental workpiece of the present invention is preferably 300 MPa or more, more preferably 350 MPa or more, even more preferably 400 MPa or more, even more preferably 450 MPa or more, and particularly preferably 500 MPa or more. By having such a biaxial bending strength, the dental workpiece of the present invention can suppress fracture in the oral cavity when used as a dental prosthesis, for example. There is no particular limit to the upper limit of the biaxial bending strength, but the biaxial bending strength can be, for example, 1200 MPa or less, or even 1000 MPa or less. The biaxial bending strength of dental workpieces can be measured in accordance with ISO 6872:2015.

[0131] The dental workpiece of the present invention preferably has high translucency. The translucency can be evaluated by ΔL*. Specifically, regarding the translucency, the dental workpiece of the present invention preferably has ΔL* of 10 or more at a diameter of 15 mm and a thickness of 1.2 mm, more preferably 12 or more, even more preferably 13 or more, and particularly preferably 14 or more. When the ΔL* is within the above range, a dental workpiece with high translucency can be obtained.

[0132] ΔL* means the difference between the lightness (first L* value) on a white background and the lightness (second L* value) on a black background for the same sample. Specifically, it means the difference between the L* value on a white background (JIS Z 8781-4:2013 Colorimetry-Part 4: CIE 1976 L*a*b* color space) and the L* value on a black background. The white background means the white part of the hiding ratio test paper described in JIS K 5600-4-1:1999 Part 4 Section 1, and the black background means the black part of the hiding ratio test paper.

[0133] There is no particular upper limit to ΔL*, but it can be, for example, 25 or less, and from the standpoint of aesthetics, even 20 or less.

[0134] In addition, ΔL* for a dental workpiece having a diameter of 15 mm and a thickness of 1.2 mm can be measured using a spectrophotometer, for example, a dental color measuring device ("Crystal Eye CE100-CE / JP", 7-band LED light source, analysis software "Crystal Eye" (manufactured by Olympus Corporation)).

[0135] Examples of dental prostheses manufactured from the dental workpiece of the present invention include crown restorations such as inlays, onlays, veneers, crowns, core-integrated crowns, and bridges, as well as abutments, dental posts, dentures, denture bases, and implant members (fixtures, abutments). The machining is preferably performed using a commercially available dental CAD / CAM system. Examples of such CAD / CAM systems include the CEREC system manufactured by Dentsply Sirona Dental Systems Inc. and the Katana (registered trademark) system manufactured by Kuraray Noritake Dental Co., Ltd.

[0136] Furthermore, the dental workpiece of the present invention can be used for purposes other than dental purposes, and is particularly suitable for use as a zirconia member having an irregular or complicated shape and requiring strength. The dental workpiece of the present invention can be processed as a sintered body without using existing manufacturing methods (injection molding, CIP, slip casting, 3D printing, etc.). Therefore, for example, it is economical when a desired zirconia member can be obtained in a short time, and in the case of a part with a complex shape that is difficult to manufacture by the conventional manufacturing method, it is possible to obtain a zirconia member that maintains high strength because there is no need to obtain multiple members by mechanical fitting. Furthermore, since the sintered body can be processed as it is, a sintering step is not necessary when dimensional accuracy is required, and since uneven firing shrinkage does not occur, zirconia components can be obtained with high accuracy. Specifically, the method can be used for manufacturing jewelry, engine and interior components for mobility such as aircraft and automobiles, display panel frames, building components, electrical appliance components, household goods components, and toy parts. The zirconia member may also be fitted with a different material to be used as a composite member.

[0137] The present invention includes embodiments in which all or part of the above configurations are combined in various ways within the scope of the technical idea of ​​the present invention, as long as the effects of the present invention are achieved. EXAMPLES

[0138] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples, and many modifications within the scope of the technical concept of the present invention are possible by those having ordinary skill in the art. In the following examples and comparative examples, the average particle size refers to the average primary particle size, which can be determined by a laser diffraction scattering method. Specifically, it can be measured on a volume basis using a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation) with a 0.2% aqueous solution of sodium hexametaphosphate as a dispersion medium.

[0139] [Examples 1 to 8 and Comparative Example 1] The measurement samples of each of the Examples and Comparative Examples were prepared through the steps of preparing a granular raw material composition, preparing a compact, and preparing a sintered body (preparation of a primary sintered body, HIP treatment, and tempering treatment).

[0140] [Preparation of granular raw material composition] In order to prepare the granular raw material composition of each Example and Comparative Example, commercially available ZrO2 powder, Al2O3 powder, Y2O3 powder, Nb2O5 powder, TiO2 powder, hydroxide or carbonate of Group I elements were mixed to the composition shown in Tables 1 and 2, water was added to prepare a slurry, and the mixture was wet-pulverized and mixed in a ball mill until the average particle diameter was 0.13 μm or less. After adding a binder to the pulverized slurry, the mixture was dried with a spray dryer to prepare a granular raw material composition (hereinafter, also simply referred to as "raw material composition"), which was used in the manufacture of a molded body described below. The average particle diameter was measured on a volume basis using a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation) using a 0.2% sodium hexametaphosphate aqueous solution as a dispersion medium.

[0141] [Preparation of molded body] For each of the Examples and Comparative Examples, pellet-shaped compacts and block-shaped compacts were prepared as follows so as to obtain sintered body samples for evaluating translucency and strength and for evaluating processability. For pellet-shaped compacts, a cylindrical mold having a diameter of 19 mm was used, and the raw material composition was placed in the mold so that the thickness of the dental workpiece after sintering would be 1.2 mm. Next, the raw material composition was press-molded at a surface pressure of 200 MPa using a uniaxial press molding machine to produce a pellet-shaped compact.

[0142] For the block-shaped molded body, the raw material composition was placed in a mold having an inner dimension of 19 mm×18 mm so that the height of the dental workpiece after sintering would be 14.5 mm. Next, the raw material composition was press-molded at a surface pressure of 200 MPa using a uniaxial press molding machine to produce a block-shaped compact.

[0143] [Preparation of primary sintered body] The pellet-shaped and block-shaped compacts obtained were subjected to a sintering furnace "Noritake Katana (registered trademark) F-1" manufactured by SK Medical Electronics Co., Ltd., and were subjected to sintering in the atmosphere at the maximum sintering temperature shown in Tables 1 and 2 for 2 hours to obtain pellet-shaped and block-shaped samples of sintered bodies containing zirconia or sintered bodies containing alumina (primary sintered bodies). In the following, in Example 6, the HIP treatment and tempering treatment were not performed, and the primary sintered body was used as a dental workpiece to evaluate each characteristic.

[0144] [Preparation of HIP-treated sintered body] The pellet-shaped and block-shaped sintered bodies containing zirconia or sintered bodies containing alumina (primary sintered bodies) obtained were subjected to a HIP apparatus "O2-Dr.HIP" manufactured by Kobe Steel, Ltd., at 150 MPa and the HIP temperatures shown in Tables 1 and 2 for 2 hours to obtain samples of pellet-shaped and block-shaped sintered bodies containing zirconia or sintered bodies containing alumina (HIP-treated sintered bodies).

[0145] [Preparation of dental workpieces (sintered bodies after tempering)] The obtained pellet-shaped and block-shaped zirconia-containing sintered body or alumina-containing sintered body (HIP-treated sintered body) was heated at 700°C for 60 hours in a sintering furnace "Noritake Katana (registered trademark) F-1" manufactured by SK Medical Electronics Co., Ltd., to obtain pellet-shaped and block-shaped dental workpiece samples (tempered sintered body). The size of the obtained samples was 15 mm in diameter x 1.2 mm in thickness for the pellet shape and 15.7 mm in width x 16.5 mm in length x 14.5 mm in height for the block shape.

[0146] The content of each component of the sintered body in Tables 1 and 2 is a value calculated from the amount of raw material charged. The content (mol %) of the Group I elements in Tables 1 and 2 is the external addition rate relative to a total of 100 mol % of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. The content (mol%) of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5 in Tables 1 and 2 is the content of each component in a total of 100 mol% of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. Only ZrO2 and HfO2 are shown as the total content of ZrO2 and HfO2. The content (mass %) of TiO2 in Tables 1 and 2 is the external addition rate relative to the total of 100 mass % of ZrO2, HfO2, the stabilizer, Nb2O5, and Ta2O5. In Tables 1 and 2, A / B represents the ratio of A to B when the content of Y2O3 is A mol % and the total content of Nb2O5 and Ta2O5 is B mol %.

[0147] The properties of each of the dental workpieces obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Tables 1 and 2 below.

[0148] [MSE Exam] For each of the examples and comparative examples, one sample (width 15.7 mm x length 16.5 mm x height 3.0 mm) of the processable zirconia composite sintered body is prepared and evaluated using a localized slurry injection wear device (MSR-A type, manufactured by Palmeso Co., Ltd.). For the evaluation, a spherical alumina slurry was prepared by mixing 3% by volume of spherical alumina (product number: MSE-BA-3-3, manufactured by Palmeso Co., Ltd.) with an average particle size of 3.0 μm in water, and used in the localized slurry injection abrasion method. The spherical alumina slurry was used immediately after production. The projection pressure was adjusted by projecting the obtained spherical alumina slurry onto a standard test piece (product number: HRC45, manufactured by Palmeso Co., Ltd.) so that the standard value (erosion rate: 1.00 μm / g ± 5%) was obtained. The projection conditions selected for the evaluation were an impact mode in which the air pressure supplied to the projection nozzle was 0.335 MPa, the slurry pressure was 0.317 MPa, the air flow rate supplied to the projection nozzle was 10.8 L / min, and the slurry flow rate was 125 L / min. The projection force of this impact mode was confirmed by the erosion rate formed on a standard test piece made of acrylic resin being 24.0±5%μm / g.

[0149] [Measurement of wear depth formed by wear and calculation of erosion rate] The wear depth (erosion depth) of the sample was measured by using a localized slurry injection abrasion method using a spherical alumina slurry containing spherical alumina particles by injecting the slurry under the following measurement conditions. Three measurement points were randomly selected for each sample, and each measurement point was measured. Next, the maximum value D (μm) of the wear depth was measured from each of the obtained profiles. Next, the amount of projected particles (g) projected onto the sample was calculated based on the slurry flow rate supplied to the projection nozzle 50 from a preset relationship for the spherical alumina slurry containing spherical alumina particles. Then, the average value of the maximum value D (μm) for the sample was divided by the amount of projected particles (g) to calculate the spherical particle wear rate (spherical particle erosion rate) (μm / g) when using the slurry local injection abrasion method using the spherical alumina slurry containing spherical alumina particles. The average values ​​of the erosion rates at the three measurement points described above are shown in Tables 1 and 2.

[0150] (Measurement conditions) Model used: Stylus-type measuring instrument (PU-EU1) manufactured by Kosaka Laboratory Co., Ltd. Stylus load: 100μN Measurement magnification: 10000 Side length: 4mm Measurement speed: 0.2 mm / sec

[0151] [Translucency evaluation of dental workpieces] The translucency was evaluated by the following method (n=3) using the pellet-shaped dental workpiece (sintered body after tempering) samples (diameter about 15 mm × thickness 1.2 mm) of each Example and Comparative Example as they are. As a measuring device, Olympus Corporation's dental color measuring device "Crystal Eye" (7 band LED light source) was used, and first, the background (underlay) of the sample was made white (the opposite side of the measuring device with respect to the sample was made white) and the L* value of the L*a*b* color system (JIS Z 8781-4:2013 Colorimetry-Part 4: CIE 1976 L*a*b* color space) was measured and defined as the first L* value. Next, for the same sample for which the first L* value was measured, the background (underlay) of the sample was made black (the opposite side of the measuring device with respect to the sample was made black) and the L* value of the L*a*b* color system was measured and defined as the second L* value. In the present invention, the difference between the first L* value and the second L* value (the value obtained by subtracting the second L* value from the first L* value) is regarded as the light transmittance, and is expressed as ΔL*. A high ΔL* value indicates high light transmittance, and a low ΔL* value indicates low light transmittance. For the black and white background (underlay) in the chromaticity measurement, the hiding power test paper used in the measurement of paints described in JIS K 5600-4-1:1999 can be used. The average ΔL* values ​​of each sample are shown as results in Tables 1 and 2. In an embodiment requiring light transmittance, a ΔL* of 10 or more was considered acceptable.

[0152] [Strength evaluation of dental workpieces] The biaxial bending strength of the pellet-shaped dental workpiece (sintered body after tempering) samples of each Example and Comparative Example was measured as is using a universal testing machine "AGS-X" (manufactured by Shimadzu Corporation) at a crosshead speed of 1.0 mm / min in accordance with ISO6872:2015 (n=5). The average values ​​are shown as the measurement results in Tables 1 and 2. A strength of 300 MPa or more was considered acceptable.

[0153] [Method for measuring average crystal grain size in sintered body] For each of the pellet-shaped dental workpieces (sintered bodies after tempering) in each of the Examples and Comparative Examples, images of the surface were taken with a scanning electron microscope (product name "VE-9800", manufactured by Keyence Corporation). After the grain boundaries of each crystal grain were noted on the obtained images, the average crystal grain size was calculated by image analysis. The average crystal grain size was measured using image analysis software (product name "Image-Pro Plus", manufactured by Hakuto Co., Ltd.), the captured SEM image was binarized, the brightness range was adjusted so that the grain boundaries were clear, and the particles were recognized from the field of view (area). The crystal grain size obtained with Image-Pro Plus was the average of the lengths of the line segments connecting the outlines passing through the center of gravity determined from the outlines of the crystal grains, measured at intervals of two degrees from the center of gravity, and the average value of the crystal grain size of all the particles not overlapping the edge of the image in the SEM photograph images (three fields of view) of each Example and Comparative Example was taken as the average crystal grain size (number basis) in the sintered body. "Particles not on the image edge" refers to particles excluding those whose outlines do not fit within the screen of the SEM photograph (particles whose outlines end at the top, bottom, left, and right boundaries). The crystal grain size of all particles not on the image edge was determined by selecting the option to exclude all particles on the boundary lines in Image-Pro Plus.

[0154] [Evaluation of machinability of dental workpieces] Thirty block-shaped dental workpieces (sintered bodies after tempering) samples of each Example and Comparative Example were prepared with metal jigs attached to the surface of approximately 15.7 mm wide x 14.5 mm high, and processed into a general anterior tooth crown shape using the CEREC system "MC-XL" (manufactured by Dentsply Sirona). The processing program used the software "inLab (registered trademark) CAM version 20.0.1.203841", and the following settings were selected: Manufacturer: IVOCLAR VIVADENT, Material name: IPS e.max CAD, Production Method: Grinding, Block size: C16, and the processing tools used were Step Bur 12 and Cylinder Pointed Bur 12S.

[0155] [Processing time] The processing times shown in Tables 1 and 2 are the times required to complete processing of the first sample using new processing tools under the conditions described in [Evaluation of machinability of dental workpieces] above. In addition, if an error occurred due to the load during processing, etc., and the CEREC system "MC-XL" stopped midway through processing, a new processing tool was attached and processing was restarted. This operation was repeated until processing of one sample was completed, and the time required was recorded as the processing time.

[0156] [Number of pieces] The number of processed pieces shown in Tables 1 and 2 is the number of samples that could be processed into the shape of a front tooth crown using a brand new set of processing tools under the conditions described in the above [Evaluation of the machinability of dental workpieces] without ever changing the processing tools. A maximum of 30 samples were used for the test, and if processing of up to 30 samples could be completed with one processing tool, additional processing tests were not conducted and the number was uniformly stated as "30 or more." Furthermore, if an error occurs due to the load during processing before the first sample is completed, and the MC-XL stops midway through processing, a new processing tool is attached and processing is resumed. This operation is repeated until one sample is processed, and the reciprocal of the number of processing tools used is taken as the number of processed samples. For example, "0.2 pieces" in Comparative Example 1 in Table 2 means that five processing tools were used to obtain a sample processed into the crown shape of one front tooth.

[0157] [Table 1]

[0158] [Table 2]

[0159] From the above results, it was confirmed that the dental workpiece of the present invention has strength and translucency suitable for dental use, and also has excellent machinability in the sintered state. Moreover, in Examples 1 to 3, wear of the processing tool could be suppressed, and the number of dental prostheses that could be continuously processed with one processing tool could be increased compared to the conventional technology. Furthermore, it has been confirmed that the dental workpiece of the present invention has strength and translucency suitable for dental use, even in embodiments where high translucency is required, and has excellent machinability in the sintered state. On the other hand, in Comparative Example 1, which corresponds to Patent Document 1 and in which the erosion rate was not within the predetermined range, the reduction in processing time was not sufficient. [Industrial Applicability]

[0160] The dental workpiece of the present invention has suitable strength and translucency, and is excellent in machinability, and is particularly useful as a dental material for dental prostheses and the like for dental treatment applications. [Explanation of symbols]

[0161] 10: Localized slurry injection abrasion device 34: Slurry 35: Slurry tank 36: Mixer 38: Compressed air source 40: Slurry pressure regulating valve 42: Projection gun 44: Slurry flow meter 46: Air pressure regulator 48: Air flow meter 50: Projection nozzle 52: Jig 54: Projection Booth 56: Table drive device 58: Recovery pump

Claims

1. In a micro-slurry jet erosion test, when a spherical alumina slurry with an average particle size of 3.0 μm is projected, the erosion rate is 6.5 μm / g or more, or the value of erosion rate (μm / g) × average crystal grain size (μm) is 15 μm. 2 / g or more, A dental workpiece having a biaxial bending strength of 300 MPa or more measured in accordance with ISO 6872:2015.

2. 2. The dental workpiece according to claim 1, which has an erosion rate of 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected thereon in a microslurry jet erosion test.

3. 3. The dental workpiece according to claim 1, wherein the dental workpiece is a ceramic sintered body.

4. The dental workpiece according to claim 3 , wherein the ceramic sintered body is a sintered body containing zirconia.

5. 5. The dental workpiece according to claim 1, wherein the average crystal grain size of the dental workpiece is 0.05 to 15.0 μm.

6. In a micro-slurry jet erosion test, when spherical alumina slurry with an average particle size of 3.0 μm was projected, the value of erosion rate (μm / g) × average crystal grain size (μm) was 15 μm. 2 The dental workpiece according to any one of claims 1 to 5, wherein the surface roughness is 1 / g or more.

7. In a micro-slurry jet erosion test, when spherical alumina slurry with an average particle size of 3.0 μm was projected, the value of erosion rate (μm / g) × average crystal grain size (μm) was 15 μm. 2 6. The dental workpiece according to claim 5, wherein the average crystal grain size of the dental workpiece is 3.0 μm to 15.0 μm.

8. 6. The dental workpiece according to claim 5, wherein the erosion rate is 8.0 μm / g or more when a spherical alumina slurry having an average particle size of 3.0 μm is projected in a microslurry jet erosion test, and the average crystal grain size of the dental workpiece is 0.05 μm to 5.0 μm.

Citation Information

Patent Citations

  • Machinable zirconia and method for producing the same

    JP2015127294A

  • Production method for workable zirconia composite sintered body, raw material composition for workable zirconia composite sintered body, and workable zirconia composite calcined body

    WO2021132644A1