Efficient depolymerization method for polymer comprising ester functional group, and purification method therefor
A low-temperature depolymerization and purification method using polyhydric alcohols and specific catalysts effectively addresses the inefficiencies of existing methods, producing high-purity monomers with reduced energy consumption and catalyst residues, suitable for recycling polymers with ester functional groups.
Patent Information
- Application Number
- JP2024134820
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-02-26
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-06-24
AI Technical Summary
Existing depolymerization methods for polymers containing ester functional groups, such as hydrolysis, methanolysis, and glycolysis, face challenges including high energy consumption, low yield, and the presence of harmful catalyst residues, particularly in producing high-purity monomers for recycling, with difficulties in removing color-producing foreign substances like dyes and pigments.
A method involving the use of polyhydric alcohols, exchange esterification reaction catalysts, and a compound represented by a specific chemical formula to depolymerize polymers at lower temperatures, followed by a purification process using liquid-liquid extraction and recrystallization to achieve high-purity monomers, while minimizing energy consumption and catalyst residues.
The method enables high-yield, high-purity production of monomers suitable for recycling, reducing energy consumption and eliminating harmful catalyst residues, facilitating the production of environmentally friendly and economically viable recycled materials.
Smart Images

Figure 2024156985000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for low-temperature glycolysis of a polymer containing an ester functional group by adding an additive, Method for removing foreign matter that may be contained in monomer from depolymerized product of molecule and product using the same and an environmentally friendly method for depolymerizing said colored polymer.
[0002] More specifically, the present invention relates to a method for producing a colored polymer containing an ester functional group in a glycolysis reaction. By adding the additive, it is possible to maintain a high depolymerization yield even at low temperatures. A considerate depolymerization method, which adjusts the thermodynamic conditions of the obtained reaction product to pass through the liquid-liquid phase equilibrium A separation method that allows selective separation of color-producing foreign matter, high-performance liquid-liquid extraction A method for purifying addition monomers to a high degree of purity, and a method for low-value exchange esterification reaction free of harmful metals Using the reaction catalyst, harmful or quality-degrading organic or inorganic substances are present in the monomer product produced. The content of impurities can be significantly reduced by the use of colored polymers containing ester functional groups. The present invention relates to a method for depolymerization reaction and high-purity purification of monomer products. [Background technology]
[0003] Most discarded plastic ends up in designated landfills or in natural habitats where natural purification is difficult. The seriousness of the environmental pollution problem is increasing day by day. Degradable or biodegradable plastics can also be categorized according to the level of UV exposure, temperature, and the presence of decomposing microorganisms. They can persist for decades depending on local environmental factors.
[0004] In order to solve this problem, we have developed a new plastic material that has a short decomposition cycle in nature. In addition to developing new materials, we are also working to develop new methods for the physical regeneration of plastics, starting with the chemical decomposition of existing petroleum-based plastics. Minimize the accumulation of plastics and reduce their environmental impact from recycling to recycling and reprocessing. Various research projects are being conducted to achieve this.
[0005] Polymers containing ester functional groups undergo depolymerization. Monomerization is possible via decomposition, and various chemical reaction pathways have been developed. Theoretically, the synthesized monomer has the same properties as the raw material input into the initial polymer synthesis. The depolymerization process that is being applied industrially to recycle polyester can be The pathways are hydrolysis and glycolysis. ), Methanolysis, Ammonolysis These are combined to create a composite process that utilizes only the advantages of each process. Therefore, various chemical depolymerization methods are widely used.
[0006] The above-listed methods for producing polymers containing ester functional groups by depolymerization are described in more detail below. First, in the case of hydrolysis, various reaction pathways occur in the presence of acids, bases, and metal salt catalysts. It is known that decomposition can be carried out. In the case of acid-catalyzed reactions, in order to obtain high reaction yields, Very high concentration of sulfuric acid solution is required, which poses economic problems in process design, operation and post-treatment. When using bases and metal salt catalysts, the decomposition reaction rate is Very slow, low product purity, and difficult catalyst recovery issues make this process inefficient. This is true.
[0007] Methanolysis processes are currently used by not only global chemical companies but also small and medium-sized plastics companies. However, methanol is one of the processes that is widely used in commercial processes. Because it is used as a reaction solvent, it requires severe reaction conditions such as high temperature and high pressure. Not only is the design cost high, but additional unit processes for reactant recovery and product purification are required. For efficient methanolysis, the transesterification process is required. A catalyst is required and is a catalyst commonly used in the depolymerization reaction of polymers containing ester functional groups. Examples of catalysts include metals such as zinc acetate, magnesium acetate, cobalt acetate, and lead dioxide. However, the depolymerized product obtained may contain cations. The catalyst metals may remain, and depending on the use and purpose of the repolymerized material, it may be harmful to the human body. The type and amount of catalyst used is adjusted to minimize harmful effects and impact on product quality. There may be constraints that must be considered along with the efficiency and economics of the refining process.
[0008] Hydrolysis and methanolysis processes are used in many fields. The quality and yield of the products produced during the decomposition of terephthalic acid resins are limited, and the decomposition reaction time is long. As decomposition products, terephthalic acid (TPA) or dimethyl terephthalate (DMT) Only one of these is produced as the main product, and other forms of terephthalate compounds are produced as by-products. Since it is treated as a pure substance, in order to resynthesize the produced product into a high-quality polymer material, It may be necessary to configure the refining process in a way that is excessively energy intensive.
[0009] Glycolysis is a depolymerization reaction that adds glycol as a reactant. The most common example is the process in which ethylene glycol (EG), one of the monomer raw materials, is A process for producing bis(2-hydroxyethyl) terephthalate (BHET) by adding Since ethylene glycol, which is a part of the raw material for PET, is used as a reactant, the reaction It has high thermodynamic compatibility with the product, and requires only a small investment in equipment to change the existing polymerization process. The advantage is that the raw material can be directly applied to production without any additional chemical treatment. Glycolysis is generally carried out under reflux conditions of the glycol reactant. The rate of polymer decomposition is slow, and the product distribution is wide even at reaction equilibrium, so the reaction yield of the products is low. There may be limitations not only on the rate but also on the production yield, and the final product, the monomer, may be reacted. To separate it from the reactants in high yield and purity, costly purification steps may be necessary. The reaction catalysts used are those described in Korean Patent Publication No. 2012-01228480 and Korean As disclosed in Patent No. 1142328, zinc acetate or lithium acetate is generally used. Such metal salt catalysts may not be completely removed during the refining process and may remain in the product. There is a possibility that even small amounts of metals that are harmful to the human body may be contained in the recycled monomer. Products that are produced by reusing these substances, especially food materials, medical materials, and other products that require non-toxicity, In addition, Glico is not suitable as a raw material for reprocessing household goods. The lysis reaction is carried out at high temperatures, but the product recovery and purification process is carried out by low-temperature recrystallization. This is common, so energy consumption is high and the heat source supply method for the production process is also cost-effective. However, there are problems with this, such as reduced speed and efficiency.
[0010] In carrying out the above-mentioned glycolysis reaction, the depolymerization reaction rate at low temperatures can be increased, and If it were possible to apply a less harmful and environmentally friendly catalyst system, it would not only be possible to operate the plant efficiently and economically, but also The use of polymers containing ester functional groups, which are released in large quantities, limits product quality and applications. We expect that this can be efficiently used to manufacture environmentally friendly raw materials that do not require any chemicals.
[0011] On the other hand, the monomers generated by chemical decomposition such as depolymerization can theoretically be It can be produced with the same properties as the raw materials used in polymer synthesis, or with a purity that can be used in polymer polymerization. However, waste polymer materials discharged after use contain various forms of foreign matter, which This can provide the largest cause of poor quality of the final product.
[0012] In particular, color compounds such as dyes and pigments that induce direct penetration into polymeric substrates are decolorized. To prevent this, we have designed a series of physical and chemical pre- and post-treatment and coloring processes. Since products are manufactured through this process, it is difficult to remove it by simple washing processes alone, and the occurrence of depolymerization reactions In the case of low molecular weight compounds containing terephthalic acid structures, these compounds are chemically It is not easy to effectively separate or isolate them.
[0013] Pigments are used by dispersing them in a powdered particle state in a solvent, and have the property of not dissolving in water or oil. Dyes are pigments that dissolve uniformly in most solvents and have very small particle sizes. Most pigments are incorporated into polymer resins for painting or printing. The dyes are mainly used for dyeing textiles and leather, and are dyed by a dyeing process. Dyes are classified into two types: natural dyes obtained from plants, animals or minerals, and artificially synthesized dyes. Artificial dyes are classified into direct dyes, mordant dyes, reducing dyes, color-forming dyes, Examples of the dyes include disperse dyes and reactive dyes, and polymeric materials containing ester functional groups. Dyes that are mainly used in the field are classified into azo and anthraquinone types according to their chemical structure. The above disperse dyes are most commonly used.
[0014] When purifying the depolymerization reaction product of a polymer containing an ester functional group to obtain a high addition monomer, Prior art for obtaining high-purity monomers from which pigments have been removed includes activated carbon, etc. Adsorption methods using adsorbents, physical separation methods such as filtration and distillation, oxidation, reduction, hydrolysis, electrochemical separation, However, even if the amount of pigment compound is small, When it remains in the product, it develops color and has coloring properties that form complexes with polymer monomers. In addition, the costs of materials and energy applied in the separation process are excessive. There is a risk that the costs will be high, and in most cases it will be very difficult to ensure economic viability.
[0015] As a related prior art, Japanese Patent No. 4537288 describes the dye extraction process, solid-liquid separation process, A dye-colored polyester resin comprising a depolymerization reaction process, an ester exchange reaction process, and an active ingredient recovery process. The present invention discloses a method for producing dimethyl terephthalate and alkylene glycol from terephthalic acid fibers. This patent uses xylitol as an extractant to extract dye from dyed polyester fibers. The polyester is heated to a temperature above the glass transition temperature of 220°C. The dye is extracted and removed at temperatures below 100 ° C. before depolymerization. The polyester fibers are depolymerized with alkylene glycol in the presence of a depolymerization catalyst. By adding additional reaction mixture to cause the depolymerization reaction, bis-ω-hydroxyalkyl The present application discloses a process for obtaining a depolymerized solution containing BHAT. Extraction of the dye prior to depolymerization is not preferred as it is uneconomical and has low extraction efficiency.
[0016] In addition, Korean Patent No. 10-1142329 discloses a method for producing a polyester by depolymerization. The oligomer solution is contacted with an ion exchange resin to remove the catalyst in the oligomer solution, The oligomer solution from which the catalyst has been removed is passed through a decolorizing agent such as activated carbon, activated clay, or diatomaceous earth to remove the oligomers. The paper discloses a technique for removing colored substances in a sesame solution by adsorbing them onto a decolorizing agent. In this patent, the amount of decolorizing agent used may be excessive, and there is a limit to the regeneration of the adsorbent. It is not economical.
[0017] In order to solve this problem, a colored polymer containing an ester functional group is depolymerized to produce a colored polymer. Colored dyes or pigments made from terephthalate derivatives that occur during the refining process of products It is a substance that can effectively remove excess energy and prevent it from being consumed. Or process development is required. Summary of the Invention [Problem to be solved by the invention]
[0018] In the present invention, when decomposing a polymer containing an ester functional group, the monomer produced is Prepolymerization or initial feedstock produced in existing petrochemical processes with very low or no impurities The present invention can also be used to adjust the amount of waste generated after consumption. The polymer can be used as the raw material for depolymerization, and the monomer produced from it can also be subjected to an additional pretreatment process. It can be quickly reintroduced into the same process, contributing to the achievement of a circular economy for plastics. The present invention aims to provide a method for producing high-quality regenerated monomers based on glycolysis.
[0019] In addition, the present invention enables depolymerization under reaction conditions that are much lower than the conventional high-temperature reaction conditions. Therefore, an attempt was made to provide a depolymerization method that can significantly reduce energy consumption. do.
[0020] The present invention also provides reaction materials, reaction pathways and systems that are more environmentally friendly than existing processes. This allows for the construction of polymers containing ester functional groups, and also facilitates the purification process of the depolymerized products. The present invention aims to provide a method for producing monomers that is easy to use, economical and efficient compared to other reaction techniques. do.
[0021] On the other hand, the present invention is a method for adding a monomer of a polymer containing an ester functional group to the monomer. An extractant capable of selectively extracting and removing color-producing foreign matter present in a liquid, and a method for removing the extractant using the same The present invention provides a method for purifying monomers of polymers containing ester functional groups by using the above process.
[0022] The present invention also relates to a reaction product in which the monomer of the polymer is produced by a depolymerization reaction, or a purified The monomer mixture generated during the polymerization process can be used to produce monomers of the same quality as those before polymerization. The product is purified in situ using the same process used for the depolymerization reaction. Alternatively, the present invention aims to provide a method for purifying the product by adding one or more post-treatment steps.
[0023] The present invention also provides a method for extracting lactic acid bacteria by continuously applying the extraction process by adding a small amount of additives. The purity of the product can be adjusted by the addition of high purity monomers or derivative compounds of the polymer. A method of manufacture is provided. [Means for solving the problem]
[0024] In order to solve the above problems, the present invention provides a copolymer comprising: (1) one or more polyhydric alcohols; and (3) a mixture containing a compound represented by the following chemical formula 1: By contacting the polymer containing an ester functional group, The present invention relates to a method for depolymerizing a polymer containing an ester functional group, the method comprising the steps of: decomposing a polymer containing an ester functional group; provide.
[0025] [Chemical formula 1] TIFF2024156985000002.tif1750
[0026] In the formula, the substituent R 1 is hydrogen, hydroxyl group, aldehyde group, carboxyl group, C 1 ~C 6 Alkyl groups of C 4 ~C 6 Cycloalkyl groups of C 6 ~C 12 Among the aryl groups wherein n is an integer of 0 to 5; When n is 2 or more, R 1 may be the same or different, and the substituent R 2 is C 1 ~C 10 wherein m is an integer of 1 to 6; When m is 2 or more, -OR 2 may be the same or different.
[0027] In one embodiment of the present invention, the transesterification catalyst is selected from Group 1A, Group 2A, and It may contain one or more selected from metal salts of Group 2B metals.
[0028] In one embodiment of the invention, the counter-ion of the metal salt is Consists of an organic anion selected from carbonate, bicarbonate, alkoxide, or acetate. Ugh.
[0029] In one embodiment of the present invention, the polyhydric alcohol is ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentane Diol, 1,6-Hexanediol, 1,7-Octanediol, 1,9-Nonanedio ethanol, neopentyl glycol, 1,4-cyclohexanediol, isosorbide, and 1,4-cyclohexanedimethanol may be one or more selected from the group consisting of cyclohexanedimethanol and cyclohexanedimethanol.
[0030] In one embodiment of the present invention, the polymer containing ester functional groups is polyethylene terephthalate. Poly(ethylene terephthalate) (PET), polypropylene terephthalate (PPT), polyglycolide or Polyglycolic acid (PGA), polylactic acid (PLA), polycaprolactone (PCL), Trihydroxyalkanoate (PHA), polyhydroxybutyric acid (PHB), polyethylene Adipate (PEA), Polybutylene succinate (PBS), Poly(3-hydroxybutyrate) Poly(butylene terephthalate) (PBT) ), Polytrimethylene terephthalate (PTT), Polyethylene naphthalate (PEN) and Vectran.
[0031] In one embodiment of the present invention, the compound represented by Formula 1 is methoxybenzene, 1,2-Dimethoxybenzene, 1,3-Dimethoxybenzene, 1,4-Dimethoxybenzene benzene, 1,2,3-trimethoxybenzene, 1,2,4-trimethoxybenzene, 1,3, 5-Trimethoxybenzene, 1,2,3,4-Tetramethoxybenzene, 1,2,3,5 -Tetramethoxybenzene, 1,2,4,5-tetramethoxybenzene, 2-methoxybenzene phenol, 1,3-dimethoxy-2-hydroxybenzene, 4-hydroxy-3,5-di Methoxybenzoic acid, 3-(4-hydroxy-3,5-dimethoxyphenyl)prop-2- Enal, 4-hydroxy-3,5-dimethoxybenzaldehyde, 4-hydroxy-3, 5-Dimethoxyacetophenone, 3-(4-hydroxy-3,5-dimethoxyphenyl Prop-2-enoic acid, 4-enyl-2,6-dimethoxyphenol, 4-hydroxy-3- Methoxybenzaldehyde, 3-hydroxy-4-methoxybenzaldehyde, 2-hydroxy 2-Hydroxy-3-methoxybenzaldehyde, 2-Hydroxy-5-methoxybenzaldehyde 2-Hydroxy-4-methoxybenzaldehyde, 3,4-dihydroxybenzaldehyde aldehyde, 1-methoxy-4-[(E)-prop-1-enyl]benzene, 1-bromo-4 -Methoxybenzene, 2-tert-butyl-4-methoxyphenol, ethoxybenzene 1,3,5-trichloro-2-methoxybenzene, 1,3,5-tribromo-2-methoxybenzene Toxobenzene, 4-(prop-2-en-1-yl)phenol, 1-methoxy-4( prop-2-en-1-yl)benzene, 5-(prop-2-en-1-yl)-2H- 1,3-Benzodioxole, 4-Methoxy-2-[(E)-prop-1-yl]pheno and 2-methoxy-4-(prop-1-en-yl)phenol There may be one or more of the above.
[0032] The present invention also provides a composition for polymer depolymerization containing an ester functional group, comprising: (A)1 (B) a transesterification reaction catalyst; and (C) a compound represented by the above formula 1. The present invention provides a composition comprising the compound.
[0033] The catalyst for the transesterification reaction is a metal-free organic compound catalyst or a Group 1A or 2A group and Group 2B metal salts.
[0034] The amount of polyhydric alcohol contained in the composition is equal to the molar equivalent of the repeating unit of the polymer to be depolymerized. The ratio of moles per unit time is 1 to 50, and the amount of the exchange esterification catalyst is determined by the repeat rate of the polymer to be depolymerized. The ratio of moles per mole of the return unit is 0.001 to 1, and the amount of the compound represented by chemical formula 1 is The ratio of moles per mole of the repeating unit of the polymer to be depolymerized is 0.001 to 50. It may also be a mixture of
[0035] The present invention also relates to a method for purifying a glycol addition monomer obtained by the depolymerization method of the present invention. A method is provided.
[0036] The purification method includes: (1) isolating the compound represented by Chemical Formula 1 from the depolymerization reaction product into a gas-liquid mixture; (2) separating the unreacted esters from the mixture after step (1) using solvent extraction or liquid-liquid extraction; (3) a solids separation step of separating solids containing a polymer having a carboxylic functional group; a recovery step of recovering the glycol addition monomer by recrystallization after separation of the solids of the step; include.
[0037] In one embodiment of the invention, the purification method comprises the step of: The product can be separated using physical filtration, and the glycol addition in the above step (3) can be carried out. The recrystallization of the monomer may be preceded by a step of isolating the oligomers.
[0038] On the other hand, the present invention removes color-producing foreign matter from monomers of polymer resins containing ester functional groups. The extractant for removing fluorine-containing compounds is characterized in that it contains a compound represented by the chemical formula 1. Extractant for removing color-producing contaminants from monomers of polymeric resins containing ester functional groups to provide.
[0039] In one embodiment of the present invention, the monomer of the polymeric resin containing an ester functional group is , characterized in that it is obtained by the depolymerization reaction of a polymer resin containing an ester functional group. It can be said that:
[0040] The present invention also provides a method for removing foreign matter from a monomer of a polymer resin containing an ester functional group. A purification method for producing a high purity monomer, comprising the steps of: 1) removing an ester containing color-producing foreign matter; The compound represented by the formula 1 is added to and mixed with a polymer monomer containing a cyclic functional group. 2) allowing the mixture from step 1 to stand to induce liquid-liquid phase separation; and 3) Separating and discharging the phase-separated liquid-liquid layer into an upper organic solution layer and a lower aqueous solution layer; A high-purity monomer containing an ester functional group is subjected to removal of color-producing foreign matter to obtain a monomer having a high purity. A purification method for producing the monomer is provided.
[0041] In another embodiment of the purification method of the present invention, in step 1), a compound represented by Chemical Formula 1 is In addition to the compound represented by formula 1, a hydrophilic liquid or water that is not mixed with the compound represented by formula 1 is added to the color generating agent. It can be characterized by adding the compound to a monomer containing the compound.
[0042] In another embodiment of the purification method of the present invention, the monomer contains an ester functional group. or a mixture obtained after said depolymerization reaction. The present invention can be characterized as being a partially purified form of the above-mentioned.
[0043] In the purification method according to the present invention, the separated aqueous solution layer is added with a compound represented by chemical formula 1. and repeating the steps one or more times to add more of the compound that produces the color and to extract more of the color-producing foreign matter. The separated organic solution layer contains a hydrophilic liquid that is not miscible with the compound represented by formula 1. Alternatively, the method may further include the step of adding more water and mixing, followed by another phase separation.
[0044] In the purification method according to the present invention, esophageal ulcers are isolated from the separated aqueous phase via recrystallization. recovering the monomer of the polymeric resin containing tert-functional groups. .
[0045] The present invention also provides a method for producing a colored polymer having an ester functional group, comprising: (a) administering to the polymer a compound represented by the formula 1; (b) depolymerizing the polymer containing ester functional groups. (c) adding a compound represented by Chemical Formula 1 to the depolymerization reaction product obtained from the depolymerization reaction, (d) adding an immiscible hydrophilic solution or water and mixing the mixture of the above (c) step. (e) separating the phase-separated liquid-liquid layer into an upper phase. and separating and discharging the resulting mixture into an organic solvent layer and a lower aqueous solution layer. High purity monomers are obtained by removing color-producing foreign matter from the monomers obtained by depolymerization of color polymers. A purification process for producing
[0046] In another embodiment of the present invention, the organic solution layer separated and discharged in step (e) is It can be characterized by recovering the organic solvent via distillation and recycling it. Effect of the Invention
[0047] According to the method for depolymerizing a polymer containing an ester functional group of the present invention, Glycol addition monomers, which are raw materials for pre-production or polymer resynthesis, are prepared from polymers having the above structure. - (e.g., bis(2-hydroxyethyl) terephthalate)) in high yield and purity It is possible to use polyethylene terephthalate ( Poly(ethyleneterephthalate, PET) and waste polyester Using fibers as raw materials, high-purity bis(2-hydroxyethyl) terephthalate (bi Regeneration of s(2-hydroxyethyl)terephthalte (BHET) etc. This can be useful for large-scale production of monomers.
[0048] According to the present invention, the reaction conditions are milder than those of the existing reaction conditions, and the reaction conditions are environmentally friendly. A reaction system composed of these materials is applied to the production of depolymerized monomers based on glycolysis. By this, the reactivity of the polymer containing the ester functional group to degradation and the target moiety can be improved. At the same time, selectivity for the nomer can be ensured, and many of the materials containing the catalyst after the reaction are Recovery is easy because all thermodynamic phase separation methods such as liquid-liquid extraction and gas-liquid separation can be effectively applied. and the impurity content in the decomposition products can be significantly reduced.
[0049] In addition, the present invention uses a lower temperature and a larger amount of glycerol than the glycolysis processes reported in the existing prior art. It is possible to obtain a glycol addition monomer with high purity in high yield even under atmospheric pressure.
[0050] In addition, the selection of catalysts that can be applied to the technology according to the present invention is very diverse and is not limited to those that have been used in the past. This allows the use of inexpensive catalysts that are less toxic than commercially available catalysts (e.g., zinc acetate), It is possible to produce products that are harmless to the human body, and also to produce eco-friendly and economical products. be.
[0051] The monomers depolymerized by the technology of this invention can be used to polymerize plastics and resin products. It is a complete chemical recycling technology, as there are no quality or application restrictions for reuse as raw materials. It is possible to realize this technique.
[0052] On the other hand, according to the extraction agent and purification method of the present invention, it is possible to obtain a monolayer of a polymer containing an ester functional group. It is possible to purify the mer to a high degree of purity.
[0053] The monomers of the polymer are also produced by depolymerization of colored polymers containing ester functional groups. The depolymerized monomer obtained by the above-mentioned process is of the same quality as that obtained before the production of the polymer, or is capable of producing addition monomers (eg, BHET) in high yield and purity.
[0054] In addition, the extractant does not participate in the depolymerization reaction, so the monomer purification process after the depolymerization reaction It can be used directly without separation, and can be added before or after the depolymerization reaction, making it easy to use in the process. It has high operational efficiency and ease of operation.
[0055] In addition, the extractant reduces the hydrogen bonding strength between foreign substances and additives, and the π- The affinity of depolymerized small molecules is increased by adjusting non-covalent mutual attraction such as overlap. The force can be reduced, and the free dye compound is in the organic phase, and the product terephthalate compound is in the Since the substances are distributed in high concentration in the hydrophilic lower phase, the products can be purified to a high purity by physical phase separation. The depolymerization reaction process itself can be converted into a purification process, or a continuous purification process can be performed. It is possible to realize a series process by flow, simplifying the process configuration. This has the advantage of reducing energy consumption.
[0056] The present invention can apply less stringent operating conditions compared to existing separation processes, and can save energy. Each compound is made of environmentally friendly materials, which can minimize gy loss. The extraction agent and some or all of the compounds used in the reaction are separated in a separate process. This allows for recovery and reuse of the product, making it an environmentally friendly and economical refining process. It is possible.
[0057] In addition, the extraction agent and purification method of the present invention do not require complicated process steps, but are simple and repetitive. The use of separation methods can increase the purity of the depolymerization products, making them suitable for use in a variety of forms and methods. This can be applied to high-purity, high-yield purification technology. [Brief description of the drawings]
[0058] [Figure 1] FIG. 1 is a H-NMR spectrum of BHET obtained from PET depolymerization according to a comparative example of the present invention. [Diagram 2] 1H-NMR spectrum of a sample obtained by repeatedly washing BHET obtained from PET depolymerization according to a comparative example of the present invention with water several times. [Diagram 3] 1 is a H-NMR spectrum of BHET obtained from PET depolymerization according to one embodiment of the present invention. [Figure 4]1 shows a liquid-liquid phase equilibrium diagram (Tx) of a binary compound consisting of anisole, which is one of the extractants according to the present invention, and a hydrophilic solvent (water or ethylene glycol). [Diagram 5] 1H-NMR spectra of organic pigments extracted and purified depolymerized monomer products during the depolymerization and product purification of colored waste PET polymers in some comparative examples and examples of the present invention. [Figure 6] 1H-NMR spectra of the organic dye extracted and the purified depolymerized monomer product during the depolymerization and product purification of colored polyester fibers according to some embodiments of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0059] Unless otherwise defined, all technical and scientific terms used herein are within the meaning of the present invention. It has the same meaning as commonly understood by a skilled artisan in the relevant technical field. Generally, the nomenclature used herein is consistent with that well known and commonly used in the art. This is what we have in mind.
[0060] Throughout this specification, when a part "comprises" a certain component, this is particularly Unless stated to the contrary, the term includes, but does not exclude, other elements. This means that it is possible.
[0061] The present invention relates to a process for producing a polymerizable composition comprising: (A) one or more polyhydric alcohols; (B) an ester exchange reaction catalyst; and (C) a polymerizable composition for producing a polymerizable composition comprising: C) A mixture containing a compound represented by the following formula 1 is treated with the polymer having an ester functional group: The polymer containing the ester functional group is depolymerized by contacting the polymer with an ester functional group. The present invention provides a method for depolymerizing a polymer containing an ester functional group.
[0062] The present invention also provides a composition for polymer depolymerization containing an ester functional group, comprising: (A)1 (B) a transesterification reaction catalyst; and (C) a compound represented by the following chemical formula 1: A composition for depolymerizing a polymer containing an ester functional group, comprising a compound to provide.
[0063] The present invention uses one or more polyhydric alcohols as raw materials for the glycolysis reaction, As the reaction catalyst, an existing catalyst such as zinc acetate may be used, but it is also possible to use a catalyst selected from the group consisting of Group 1A, Group 2A, and Group 2C. Group B metal cations with carbonate, bicarbonate, or arsenic as counterions Salts of organic anions such as alkoxides or acetates can also be used as catalysts. Non-metallic organic catalysts composed of rare organic materials can also be used.
[0064] In addition, the present invention relates to a compound represented by the following formula 1, which is added as an additive to form an ester functional group. Activity of depolymerization reactions for converting functionalized polymeric feedstocks into glycol addition monomers. The conversion energy can be significantly reduced, and as mentioned above, it is possible to reduce the conversion energy not only to Group 2B, but also to Group 1A and 2 The reaction is carried out using low-value catalysts containing various forms of metals such as group A metals, or organic catalysts that undergo decomposition at high temperatures. Since it can be selected as a material, it is possible to ensure economic efficiency by reusing and recovering materials and to control impurities. Therefore, the present invention can maintain high depolymerization reactivity at low temperatures. In addition, it is characterized by improving the purity, yield and reaction selectivity of the depolymerized monomer. .
[0065] [Chemical formula 1] TIFF2024156985000003.tif1750
[0066] In the formula, the substituent R 1 is hydrogen, hydroxyl group, aldehyde group, carboxyl group, C1 ~C 6 Alkyl groups of C 4 ~C 6 Cycloalkyl groups of C 6 ~C 12 Among the aryl groups wherein n is an integer of 0 to 5; When n is 2 or more, R 1 may be the same or different, and the substituent R 2 is C 1 ~C 10 wherein m is an integer of 1 to 6; When m is 2 or more, -OR 2 may be the same or different.
[0067] The depolymerization method of the present invention is useful for depolymerizing polymers containing ester functional groups, The polymer containing ester functional groups is used in the form of single or mixed waste plastics, e.g. For example, polyethylene, high density polyethylene, low density polyethylene, polypropylene or a combination thereof. The combination may be in the form of a mixture with the polymer containing the ester functional group. Other polymers that may be mixed with the polymers containing ester functional groups listed as examples include: These are merely examples and are not limiting.
[0068] In addition, polymers containing ester functional groups are formed by condensation polymerization of dicarboxylic acids and dialcohols. The dicarboxylic acid may be terephthalic acid, naphthalene, diphenyl dicarboxylic acid, diphenyl ether dicarboxylic acid, diphenyl sulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, succinic acid, adipic acid, Bacic acid, Azelaic acid, Decanedicarboxylic acid, Cyclohexanedicarboxylic acid, Trimellitic acid , pyromellitic acid, and combinations thereof; and the dialcohol is selected from the group consisting of ethyl alcohol, ethyl alcohol, ethyl ester ... Trimethylene glycol, 1,2-propanediol, tetramethylene Glycol, neopentyl glycol, hexamethylene glycol, decane methylene glycol Recall, dodecamethylene glycol, 1,4-cyclohexanedimethanol, diethylene Glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol Coal, dipropylene glycol, tripropylene glycol, tetrapropylene glycol Polypropylene glycol, di(tetramethylene) glycol, tri(tetramethylene) glycol (ethylene) glycol, polytetramethylene glycol, pentaerythritol, 2,2-bis(2,2-dimethylphenyl) (4-β-hydroxyethoxyphenyl)propane, and combinations thereof is selected from the group.
[0069] As an example, the polymer containing the ester functional group is polyethylene terephthalate (P ET), polypropylene terephthalate (PPT), polyglycolide or polyglycol Poly(GA), Polylactic acid (PLA), Polycaprolactone (PCL), Polyhydroxya Polyhydroxybutyrate (PHA), Polyhydroxybutyrate (PHB), Polyethylene adipate (P EA), polybutylene succinate (PBS), poly(3-hydroxybutyrate-co-3- Hydroxyvaleric acid (PHBV), polybutylene terephthalate (PBT), polytrimethylsilane (PTA) Polyethylene terephthalate (PTT), polyethylene naphthalate (PEN), Vectran ( Vectran), and combinations thereof.
[0070] One of the most common examples of polymers containing ester functional groups is polyethylene terephthalate. terephthalate, wherein the starting material for the preparation of the polymer is terephthalic acid or The derived monomer and ethylene glycol.
[0071] The polymers containing ester functional groups used in the present invention are not in a pure state but are available in various forms. Impurities may be present. For example, in addition to polymers containing ester functional groups, This may include, but is not limited to, bottle caps, glue, paper, liquid residue, dust, or any combination thereof. Any mixture of debris can be used as the feedstock for depolymerization, without limitation.
[0072] According to the present invention, the method for depolymerizing a polymer containing an ester functional group comprises the steps of: The polymer containing functional groups can be contained in an amount of about 0.1% by mass to about 70% by mass of the reaction raw materials. If less than 0.1% by mass is added at the beginning, it becomes difficult to ensure economic viability. If the amount is more than 0 mass%, the mass transfer is restricted and the reaction rate is significantly reduced. There is a risk of problems occurring.
[0073] The polyhydric alcohol for the glycolysis depolymerization of the polymer containing the ester functional group is , a compound having at least two alcohol functional groups, more specifically a compound having a second linear This includes, but is not limited to, compounds having two or more hydroxyl groups, such as chain alcohols. do not have.
[0074] The polyhydric alcohol has a mole ratio of 1 to 50 per mole of the repeating unit of the polymer. Can be used in range.
[0075] Examples of polyhydric alcohols having at least two alcohol functional groups according to the present invention are ethyl alcohols. Ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3- Methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-octanediol 1,9-nonanediol, neopentyl glycol, 1,4-cyclohexanediol isosorbide, 1,4-cyclohexanedimethanol, and the like. There may be one or more of the above.
[0076] The catalyst for the transesterification reaction according to the present invention is an organic catalyst that does not contain metal. Non-limiting examples of the organic catalyst include linear amines (e.g., ethylenediamine, Diamine, diethylenetriamine, tris(2-aminoethyl)amine, tetraethylene pentamine), amides (e.g., acetamide), guanidines (e.g., triazabi Cyclodecene), imidazoles (e.g., 2-ethyl-4-methylimidazole), urine Amines (e.g., urea, 1,1-dimethylurea, 1,3-dimethylurea), aromatic amines (e.g., benzene dimethanamine) and cycloalkylamines (e.g., cyclohexylamine). dimethyl amine, dimethyl cyclohexyl amine) However, it is preferred that the compound constituting the catalyst does not itself directly participate in the reaction.
[0077] Other examples of catalysts according to the present invention include those comprising a group 1A, 2A or 2B metal cation and a corresponding isothiocyanate. Carbonate, bicarbonate, alkoxide, acetate, etc. as counter ion and an anion selected from the group consisting of:
[0078] The Group 1A ions used in the catalyst were lithium (Li + ), sodium (N a + ), potassium (K + ), Group 2A metal magnesium (Mg 2+ ), Calcium (Ca 2 + ) and zinc (Zn 2+ ) are possible, but are not limited to these. stomach.
[0079] The amount of the catalyst is in a ratio of 0.001 to 1 moles per mole of the repeating unit of the polymer. Preferably, the molar ratio per mole of repeating unit is in the range of 0.01 to 0.1. .
[0080] The compound represented by the formula 1 has a depolymerization reactivity for a polymer containing an ester functional group. It is used as an additive in the depolymerization reaction to increase the catalytic activity and to increase the selectivity of useful products. As an example, the substituent R 2 is C 1 ~C 10 Alkyl groups of the formula C 1 ~C 6 No.A alkyl groups, more preferably C 1 ~C 3 The alkyl group may be:
[0081] In one embodiment of the present invention, the compound represented by Formula 1 contained in the additive is Methoxybenzene, 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4 -Dimethoxybenzene, 1,2,3-trimethoxybenzene, 1,2,4-trimethoxy Benzene, 1,3,5-trimethoxybenzene, 1,2,3,4-tetramethoxybenzene 1,2,3,5-tetramethoxybenzene, 1,2,4,5-tetramethoxybenzene phenol, 2-methoxyphenol, 1,3-dimethoxy-2-hydroxybenzene, 4-hydroxyphenyl 3-(4-hydroxy-3,5-dimethoxyphenyl) Nyl)prop-2-enal, 4-hydroxy-3,5-dimethoxybenzaldehyde, 4 -Hydroxy-3,5-dimethoxyacetophenone, 3-(4-hydroxy-3,5-di Methoxyphenylprop-2-enoic acid, 4-enyl-2,6-dimethoxyphenol, 4 -Hydroxy-3-methoxybenzaldehyde, 3-hydroxy-4-methoxybenzaldehyde aldehyde, 2-hydroxy-3-methoxybenzaldehyde, 2-hydroxy-5-meth 2-Hydroxy-4-methoxybenzaldehyde, 3,4-dihydroxybenzaldehyde 1-Methoxy-4-[(E)-prop-1-enyl]benzene 1-Methoxy-4-[(E)-prop-1-enyl]benzene 1-Bromo-4-methoxybenzene, 2-tert-butyl-4-methoxyphenyl Nol, ethoxybenzene, 1,3,5-trichloro-2-methoxybenzene, 1,3, 5-Tribromo-2-methoxybenzene, 4-(prop-2-en-1-yl)phenol 4-[prop-2-enyl]phenol; 1-methoxy-4(prop 1-metoxy-4-[prop-2-en-1-yl]benzene; 1-Methoxy 4-[prop-1-en-1-yl]benzene), 5-(prop-2-en-1-yl)-2H -1,3-benzodioxole (5-[prop-2-en-1-yl]-2H-1,3-benzodioxole), 4-Methoxy 4-metoxy-2-[(E)-prop-1-yl]phenol 4-Methoxy[prop-1-yl]phenol), and 2-Methoxy-4-(prop-1-yl)phenol 2-metoxy-4-[prop-1-en-yl]phenol; 4-Methoxy[prop-1-en-yl]phenol The compound is selected from the group consisting of naturally occurring or synthetic compounds such as phenol, There may be one or more of the above.
[0082] The amount of the additive is 0.001 to 50 moles per mole of the repeating unit of the polymer. The molar ratio may be, preferably, 0.1 to 10 per mole of the repeating unit.
[0083] The method for depolymerizing a polymer according to the present invention is carried out at a temperature in the range of 100°C to 200°C, preferably 130°C. We present a rapid method for depolymerizing polymers containing ester functional groups at temperatures in the range of ~160 °C. As a result, the method for depolymerizing a polymer containing an ester functional group provided herein is This method can realize energy savings because the reaction can be carried out at lower temperatures than conventional methods. The catalyst and additives used can be recovered and reused through a separate recovery process. Therefore, it is economical.
[0084] In addition, the depolymerization method of the present invention can be carried out at atmospheric pressure. Depending on the vapor pressure of the agents and reactants, the reaction may be carried out in a pressurized form.
[0085] In the methods described herein, the depolymerization reaction time varies depending on the amount of polymer used. The depolymerization can be carried out for a reaction time of 0.5 to 12 hours. To minimize the yield of by-products, a reaction time of 0.5 to 4 hours is preferred.
[0086] After the reaction, a further step is carried out in which unreacted polymeric substances are separated and removed from the reaction mixture by filtration. It is possible.
[0087] The depolymerization of the polymer containing ester functional groups according to the present invention can be carried out by using a polyhydric alcohol. It is a type of polymerization reaction, which can be considered as a glycolysis depolymerization reaction.
[0088] The method for purifying the glycol addition monomer obtained by the depolymerization method according to the present invention includes the steps of: ) The compound represented by the formula 1, which is an additive, is separated from the depolymerization reaction product by gas-liquid separation or liquid separation. (2) separating the unreacted ester functional groups after step (1) using liquid extraction; (3) a solids separation step of separating solids containing the polymer; and a recovery step of recrystallizing and recovering the glycol addition monomer after separation of the product. Cut.
[0089] The gas-liquid separation of the additive may be carried out separately from the reaction, but is preferably carried out continuously after the reaction is completed. For example, a condenser that is maintained at a low temperature may be used to condense the vaporized additive. The reaction is then condensed and refluxed in the reactor, and the temperature is then increased or decreased after the reaction is completed. The flow path of the condensed additives that were being refluxed was changed from inside the reactor to outside. It can be separated.
[0090] Liquid-liquid extraction is a method of adding water to separate the desired product for recovery and purification. When water was added, a clear phase separation boundary was generated, and when only the organic layer was separated at low temperature, The additives that can remain in the aqueous solution after separation are determined by the content of water. If the temperature is increased or decreased, the solubility of the amine is very limited, so it is difficult to separate and recover the amine. By crystallization, the majority of the product can be recovered, resulting in a purified product of interest. Trace amounts of additives that may remain in the product should be dried by heating at 50 to 150°C, preferably in a vacuum. It can be easily and completely removed by drying under heat.
[0091] Gas-liquid phase separation for additive recovery by the methods described herein allows for the recovery of a portion or portions of the additive. The temperature of the reactor after the reaction is raised above the reaction temperature so that all of the reactants are vaporized or volatilized. The method includes a method of separating the additives by distillation to the outside. Although using water may be the most economical option, it can also induce thermodynamically unstable phases with additives. Any hydrophilic material that can be used can be used, which is similar to the glycol or diglyceride used as a reactant. It may be an oar.
[0092] The solid matter containing the polymer containing the unreacted ester functional group is precipitated after the depolymerization reaction, Removal before or after the end of the reaction by various physical methods such as filtration, flocculation, flotation, compression, etc. In the case of the removal method using filtration, the unreacted high molecular weight compounds can be removed by filtration and then reintroduced into the depolymerization. A filter having fine pores smaller than the particle size of a molecule can be used, and the filtrate flow rate can be Pressure or pressure can be applied in parallel to increase the speed.
[0093] The method for recovering the glycol addition monomer by the recrystallization process includes removing unreacted substances from the reaction. It is more preferable to carry out the treatment after removing the solvent, and the treatment is carried out at a temperature higher than room temperature, for example, in the range of 60°C to 120°C. Preferably, the temperature is in the range of 90°C to 110°C, and the water or the solvent required for crystallization of the target product is used. A solvent is used, but this can be followed by an additional step of separating the oligomers by filtration. The filtrate can be kept at a low temperature and recovered as a product through a recrystallization process. Repeated physical separation and recrystallization processes are used to adjust the concentration of impurities in the It is also possible to separate oligomers before the recrystallization of the glycol addition monomer in the above step (3). The step of:
[0094] In forming a reaction system by the depolymerization method of the present invention, a non-metallic catalyst is used, Or a group 1A or 2A metal cation and carbon as a counter-ion. The catalyst is a metal salt of an organic anion such as an acid, bicarbonate, alkoxide, or acetate. When used in this way, the metal components that may remain in the refined monomer product are less harmful and can be easily purified. Since the removal rate during the process is high, it is easy to control the concentration of impurities.
[0095] On the other hand, the present invention relates to a process for producing colorants such as pigments and dyes from polymeric monomers containing ester functional groups. An extractant for removing foreign substances, comprising the compound represented by the above formula 1. The present invention provides an extractant characterized in that the compound represented by formula 1 has one or more aryl groups in an aromatic ring. The alkyl group is linked via a linker, the linker having at least one oxygen atom. do.
[0096] An example of the compound represented by the formula 1 which is an extractant is an additive for removing the foreign matter. The compounds represented by the formula 1 in the above are the same as those listed as examples. In order to avoid duplication, duplicate entries will be omitted.
[0097] In one embodiment of the present invention, a monomer of the polymer containing an ester functional group is is obtained by depolymerization of a polymer containing an ester functional group, and in particular The polymer containing an ester functional group may be a colored polymer, and may be a colored polymer represented by the formula 1. The compound, when added to a depolymerization reaction, reacts with the polymer containing ester functional groups. Although it does not participate directly as a catalyst, the performance in terms of depolymerization reactivity and product selectivity was evaluated in a low-temperature reaction. It has the property of being able to maintain its properties even after depolymerization, and is mixed with the polymer before the depolymerization reaction. It can also be used in a form that combines the two.
[0098] The extractant according to the invention is capable of extracting pigments and dyes from polymeric monomers containing ester functional groups. and the like. The molecules are in the form of single or mixed waste plastics, e.g., polyethylene, high density polyethylene Polyethylene, low density polyethylene, polypropylene or a combination thereof is The above-listed esters may be mixed with a polymer containing a hydroxyl group. Other polymers that may be mixed with the polymer containing tertiary functional groups are merely exemplary and are not intended to be limiting. Not limited to those listed.
[0099] The present invention also provides a method for removing foreign matter from a monomer of a polymer containing an ester functional group, thereby producing a highly pure product. The present invention provides a purification method for producing a high degree of monomer.
[0100] The purification method includes the steps of: 1) purifying a polymer monomer containing an ester functional group containing color-producing foreign matter; 2) adding the compound represented by formula 1 to the mixture of step 1 and mixing the mixture; 3) inducing liquid-liquid phase separation by allowing the mixture to stand; and and separating the organic solution layer and the lower aqueous solution layer.
[0101] The step 1) is for extracting foreign substances from monomers of polymers containing ester functional groups. Add the extractant and mix it to distribute the foreign matter more evenly into the extractant. be.
[0102] The extraction and distribution temperature in step 1) is generally used for depolymerization of polymers containing ester functional groups. Phase separation was induced at or below the reaction temperature without the addition of a hydrophilic solvent, and then extraction was performed. However, the material represented by Formula 1 has very limited solubility. If excess water having a high viscosity is added, the phase separation boundary becomes clearer and the depolymerization products and foreign matter are separated. It is possible to induce an extremely asymmetric distribution of the monomers to recover them in high purity.
[0103] The compound represented by the formula 1 has a relatively high color-producing organic property, such as dyes and pigments. Since it is a substance that has a high affinity for dyes, pigments, etc. in the above step 1), The foreign matter moves to the organic phase, which is mostly composed of the compound represented by Chemical Formula 1, and other hydrophobic compounds are removed. Most of the compounds and monomer products can transfer to the hydrophilic phase.
[0104] The temperature range during extraction and distribution in step 1) may be in the range of 25 to 150°C.
[0105] The removal of foreign matter from dyes and pigments and the purification of monomers by liquid-liquid extraction according to the present invention The process may be most economical using water, but it may induce thermodynamically unstable phases with the additives. Any hydrophilic substance that can be introduced into the reaction mixture without the addition of a separate solvent can be used. It can also be carried out in the presence of polyhydric alcohols used in the present invention.
[0106] In the step 2), the mixture is mixed in a liquid-liquid phase after asymmetric distribution of foreign matter, etc. This is the step that allows separation to occur.
[0107] The liquid-liquid phase separation can be induced continuously or batchwise using known means such as a decanter. and have sufficiently low thermodynamic miscibility with each other that phase separation occurs. The composition and temperature at which the phase separation occurs can be determined by one of ordinary skill in the art. Since this can be easily selected, a detailed description will be omitted.
[0108] As an example, FIG. 4 shows a comparison of anisole, which is one of the extractants according to the present invention, and a hydrophilic solvent (water To distinguish the thermodynamic state of a binary compound composed of ethylene glycol and According to one embodiment of the present invention, on a temperature-dependent liquid-liquid phase equilibrium curve determined by a titration method for The reaction conditions under which the depolymerization was carried out and the purification conditions under which the extraction was carried out are shown diagrammatically. The x-axis represents the composition of the organic extractant, anisole, in mole fractions, and the y-axis represents the reaction mass. The reaction or purification temperatures are shown in Fig. 1. The temperature and temperature can be selected.
[0109] The step 3) is to separate the organic phase (organic solution layer) and the aqueous phase (aqueous solution layer) from the mixture in which phase separation has occurred. This is the stage where the two layers are separated and discharged. The separation is carried out by conventional means. The organic and aqueous phases can be separately post-treated to further increase the recovery of the desired product. do.
[0110] In another embodiment of the purification method of the present invention, In the organic solution layer (or organic phase) in which the compound represented by the above-mentioned Chemical Formula 1 is the majority, water or the like is added to the organic solution layer (or organic phase). Back-extraction by adding additional hydrophilic solvent to redistribute the small amount of monomer remaining in the organic phase and recovering additional monomer product therefrom.
[0111] The organic phase separated and discharged by the liquid-liquid extraction according to the present invention is further treated with a compound represented by the formula In order to recover the additives represented by 1 and separate the dyes and pigments, a gas-liquid separation is used. This may include methods such as distillation, which involves
[0112] The monomer product concentrated in the separated aqueous solution layer is crystallized to remove most of the product. The amount of additives that can be recovered and remain in the purified product is 50-150%. It can be easily and completely removed by heating and drying at 0°C, preferably under vacuum. It is also possible.
[0113] The monomer purification process for the polymer containing ester functional groups according to the present invention is carried out without removing some foreign matter. A process of separating and removing the organic solvent by physical filtration can be additionally or simultaneously carried out.
[0114] In one embodiment of the present invention, the monomer of the polymer containing an ester functional group in step 1) is The monomer is a depolymerization reaction mixture obtained by depolymerizing a polymer containing the ester functional group. or a compound derived therefrom, and the depolymerization reaction mixture may be The product may be in a state where it has not been subjected to purification or has been partially purified after the reaction.
[0115] Thus, in the present invention, the monomer of the polymer containing the ester functional group in step 1) a depolymerization reaction mixture obtained by depolymerizing a polymer containing an ester functional group, or or a derivative compound obtained therefrom, the extractant is added during the depolymerization reaction. This can be done before or after the process.
[0116] Polymers containing ester functional groups undergo depolymerization reactions to produce monomers, dimers, and oligomers. It can be decomposed into low molecular weight compounds such as cellulose, cellulose acetate, and cellulose acetate. Hydrolysis, glycolysis, methanolysis These include methanolysis and ammonolysis. A combined process can be utilized.
[0117] Specifically, the extractant is added to the depolymerization reaction mixture prior to the depolymerization reaction. The color-producing foreign matter was removed, and the model obtained from the depolymerization of colored polymers containing ester functional groups was The method for purifying the colored polymer to a high purity comprises: (a) adding the above-mentioned (b) adding a compound of Formula 1 to the polymer containing the ester functional group; (c) adding water or a compound of formula I to the depolymerization reaction mixture obtained from the depolymerization reaction. (d) adding and mixing a hydrophilic solution which is immiscible with the compound represented by the formula (c); (e) allowing the mixture at step 1 to stand to induce liquid-liquid phase separation; and and separating and draining the layers into an upper organic solution layer and a lower aqueous solution layer.
[0118] The purification process of the depolymerized monomer of the colored polymer containing ester functional groups according to the present invention is carried out by decomposing the monomer. A process in which unreacted polymeric substances and some foreign matter are physically filtered out from a polymerization reaction mixture to separate and remove them. Additional steps or parallel steps may be performed.
[0119] The depolymerization of polymers containing ester functional groups according to the present invention can be carried out in the presence or absence of a catalyst. According to the reaction pathway of addition of alcohol, water or hydroxide, and the transesterification reaction It may be depolymerized by the polymerization of the carboxylic acid.
[0120] The process of the present invention will be described in detail below through examples, comparative examples and experimental examples. These are representative examples related to the invention and cannot limit the scope of the invention. stomach.
[0121] 1. Method for depolymerizing polymers containing ester functional groups [Ingredients 1~4] A polymeric substance containing an ester functional group is cut into PET bottles that are discarded after use. Cut it, 1cm 2 Single-layer plastic flakes with an area of less than or equal to 0.3 mm and a thickness of less than or equal to 0. (Ingredient 1) and 1cm 2 Area below 0.8 to 1.2 mm thick (10 or more layers) The plastic flakes (raw material 2) having the composition (composition) were prepared as raw materials. The colored labels of the PET bottles discharged into the water were cut into 1cm pieces. 2 Area less than 0.1mm The plastic pieces (raw material 3) are made to have the thickness shown below, and the polyester discharged after use is Cut the tel cloth into 1cm pieces 2 The waste fiber pieces ( Raw material 4) was prepared as the raw material.
[0122] [Experimental Example 1: Depolymerization reaction stage (when no additives are added before the reaction)] Approximately 10 g of the polymer raw material prepared by "Raw Material 1" was measured as the raw material for the reaction. Approximately 38.75 g of ethylene glycol, a polar solvent for dihydric alcohol (polymer repeating units) (12 moles per mole of unit) was placed in a three-neck flask and heated at atmospheric pressure with a reflux condenser attached. After the mixture was attached, it was heated and stirred using a heating magnetic stirrer. When the temperature reached 177°C, Then, 10 g of polymer raw material was added, and the temperature was increased while stirring was continued. When the mixture reaches 197°C or the reflux temperature, the catalyst is added at 0. The catalytic reaction was started by adding 0.4 moles of ethanol. The reaction was continued for 2 hours with constant stirring. The temperature is kept constant within ±0.5℃ while the condenser is exposed to atmospheric pressure at one end. The reaction was carried out using the following. The unreacted material in the product after the reaction was separated by filtration and quantified. The decomposition product, monomer, dimer, and by-product, mono(hydroxyethyl)terephthalate, Mono(hydroxyethyl)terephthalate, MHET and oligomers, etc., were measured using high performance liquid chromatography (HPLC) PLC, reversed-phase C18 column (250 mm, 5 micron), and UV detector (λ = 25 The concentration was quantified using a HPLC analysis solution containing methanol: A mixture of 70:30 volumetric ratio of water was used, with the flow rate kept constant at 0.7mL / min. did.
[0123] [Experimental Example 2: Depolymerization reaction stage (additives added before reaction)] Before the depolymerization reaction begins, the additive is added in an amount of 4 moles per mole of repeat unit of the polymer raw material. The additive was weighed in about 38.7 ml of ethylene glycol, a dihydric alcohol polar solvent. 5g (12 moles per mole of polymer repeating unit) into a three-neck flask and A pressure reflux condenser was attached, and the mixture was heated and stirred using a heating magnetic stirrer. When the temperature reaches 20°C lower than the final reaction temperature, 10 g of polymer raw material is added and the temperature continues to rise. When the reaction mixture reached the reaction temperature, the catalyst was added to the monomers of the polymer repeat units. The catalytic reaction was started by adding 0.04 moles of additive per unit. The same method as in Experimental Example 1 was applied, except that the reaction temperature was kept low at 153°C or less. The reaction and analysis were carried out.
[0124] [Experimental Example 3: Product Refining Stage] Add the reaction mixture and 400 mL of distilled water to a 500 mL round-bottom flask and then add 90-9 The mixture was stirred continuously for about 1 hour at a temperature in the range of 5°C. The oligomers in the mixture after the reaction were removed by vacuum pump. The filter paper (Whatman, pore diameter The filtrate obtained in the first step was filtered again using the same filter. The recrystallized oligomers and solids were separated and removed by this. The crystallization is carried out by storing the crystals in a cryostat maintained at 0.4 °C or less for 16 hours or more, and then vacuum filtering. After collecting the precipitate through a filter, it was dried in an oven maintained at about 80°C for 6 hours. The resulting white powder was then quantified as the glycol addition product.
[0125] To confirm the residual metal content in the refined product, approximately 0.1 g of the refined product was HNO 3 After pretreatment by dissolving in ethanol and treating with acid, analysis; inductively coupled plasma-atomic emi ssion spectrometry) (Model name: Thermo Fisher S scientific iCAP 6500Duo) and ICP-MS (ICP mass spectrometry; inductively coupled plasma-mass spectro metry) (Model name: Thermo Fisher Scientific XS The measurements were performed using a 3D sigma-based ...
[0126] To characterize the purified product, approximately 0.1 g of the product was diluted in DMSO-d 6 To the solvent The sample was prepared by diluting the monomer to a concentration of 6.25% by weight. 1 H-NMR ( 1 H nuclear magnetic resonance (Model name: Bruk AVANCE II + NMR spectra were obtained via a 500 MHz NMR spectrometer.
[0127] [Experimental Example 4: Further Refining Step] The white powder obtained from Experiment 3 was placed in a 250 mL round-bottom flask containing 100 mL of distilled water. The mixture was stirred while maintaining the temperature at 90-95°C. After stirring for about 1 hour, the mixture was cooled to 4°C or lower. The mixture was then transferred to a low-temperature bath maintained at 40°C and left for 16 hours or more to allow recrystallization. The precipitate was collected using the same filter as in Example 3, after which additional washing was performed. The resulting precipitate was dried in an oven maintained at about 80° C. for 6 hours to obtain glycol A white powder was obtained, which corresponds to the addition monomer. The same method as in 3 was used for ICP-AES, ICP-MS, and 1H-NMR analysis was carried out.
[0128] [Calculation formula] Among the products obtained from the depolymerization carried out according to the comparative examples and examples of the present invention, The unreacted material obtained was quantified by gravimetry, and the product obtained in the form dissolved in the liquid phase was diluted. The conversion rate and product yield were then calculated by the following formula: The calculation was made as follows.
[0129] Polymer depolymerization conversion rate by depolymerization (%) = (Initial input polymer molecular weight - Unreacted polymer molecular weight) / (Initial input polymer molecular weight) x 100
[0130] Yield of monomer obtained by depolymerization (%) = (number of moles of BHET obtained) / (number of moles of terephthalate units in the input polymer structure) ) x 100
[0131] Yield of dimer obtained by depolymerization (%) = (number of moles of dimer obtained) / (number of moles of terephthalate units in the input polymer structure)× 100
[0132] Yield (%) of by-product (MHET) obtained by depolymerization = (number of moles of MHET obtained) / (number of moles of terephthalate units in the input polymer structure) ×100
[0133] 1.1 Comparison of reaction characteristics of depolymerization using metal salts as catalysts [Table 1]
[0134] Table 1 shows the most commonly used reactions to compare and explain the effects of the embodiments of the present invention. The performance of the glycolysis reaction of polymer raw materials containing ester functional groups was evaluated under the following conditions: For this reason, excess ethylene glycol (per mole of polymer repeat unit) 12 moles) was used, and the glycol was heated at atmospheric pressure under ethylene glycol reflux conditions (197°C). The most commonly used catalyst for the reaction, zinc acetate, was added to the reaction mixture to form the copolymer. In order to investigate the depolymerization performance of ethylene terephthalate, the depolymerization was carried out according to the method described above in Experimental Example 1. A polymerization reaction was carried out, which is shown as Comparative Example 1. In addition, a modified combination according to an embodiment of the present invention was also carried out. As a catalyst that can be combined, an alkali acetate salt having the same mole number was selected instead of zinc acetate, and the comparative example was The depolymerization reactions carried out by adding the same number of moles of catalyst as in 1 are shown in Comparative Example 2 and Comparative Example 3. Ta.
[0135] As already reported in numerous patent and non-patent publications, zinc acetate was used as a catalyst. When the reaction was applied (Comparative Example 1), the polymer was completely decomposed after only 2 hours of reaction, and BHET was 90 In contrast, the same reaction conditions were carried out with potassium as a catalyst, and the product was obtained in a high yield of up to 100%. The experiment was carried out using acetates with alkali metal cations such as sodium or tungsten. High reactivity was also observed in the depolymerization of polyethylene terephthalate. The selectivity of the monomer BHET was observed to be low. Yield can affect productivity and the need to separate less valuable and cheaper by-products. This could cause various economic and environmental problems, such as the burden of the refining process and the disposal of by-products. do.
[0136] 1.2 PET glycolysis under low temperature conditions Choosing the Glycolysis Reaction Pathway for Depolymerization of Polymers Containing Ester Functional Groups In this case, as shown in the depolymerization reaction conditions of Comparative Examples 1 to 3, The boiling point of ethylene glycol (197°C) or higher, which is added as an addition reactant It is common to carry out the reaction at a temperature of 100° C. Even if an excess of catalyst is used, or at a very dilute concentration, Even if the polymer raw material is applied to the reaction, lowering the reaction temperature may result in insufficient depolymerization reaction. Since it has no activation energy, the reactivity is very low or the side reactions are relatively low. The reaction rate increases and the desired product cannot be obtained. On the other hand, high reaction temperatures are required. In the case of a manufacturing process in which the fuel or utility is applied to provide a heat source for the reaction, may be limited, and excessive costs are required for investment in equipment and operation of the process. Therefore, it is possible to provide a low-temperature glycol catalysis that can provide high reactivity and high yields. The design of the Coriosis depolymerization reaction is an effective and decisive measure to ensure the economic viability of the process. A step can be provided.
[0137] We have carried out the depolymerization of polymers containing ester functional groups along the glycolysis reaction pathway. Many prior art documents indicate that the temperature is equal to or higher than the boiling point of ethylene glycol (197°C). The present paper presents reaction conditions for a catalyst composed of a single or specific component, and does not merely Even if a composite material is added by mixing it, it is very difficult to lower the reaction activation energy. It is known to be difficult to achieve this, especially when it is difficult to significantly lower the reaction temperature while maintaining the same performance. No substantial examples of reaction systems capable of this have been reported.
[0138] In the present invention, as a means for overcoming this problem, the linking group between the aromatic ring and the alkyl group is Adding a compound containing at least one oxygen atom in the functional group as an additive activates the catalytic reaction. This significantly reduces the energy required for the reaction, which is 40°C lower than that required for a typical glycolysis reaction. In the low temperature region lower than that, depolymerization of polymers containing ester functional groups occurs. This will allow us to propose a new reaction pathway that will allow us to maintain performance at high temperatures where decomposition may occur. Or organic compounds that may be difficult to recover, or Group 1A or 2A compounds that are less harmful to humans. We have investigated the low-temperature glycolysis reaction in which metal salts consisting of cations of group metals can be used as catalysts. This paper aims to present a way to achieve this.
[0139] In order to specifically explain the effect of the present invention on the low-temperature glycolysis reaction, a comparative example and The results of the glycolysis reaction when the same composition was used but carried out at a low temperature (153°C) The results are shown in Table 2. In order to explain the characteristics of the low-temperature glycolysis reaction according to the present invention, The reaction results for each catalyst system were compared under the same conditions, with or without additives. The results are shown separately for Comparative Examples and Examples.
[0140] In Comparative Examples 4 to 6, the polymer raw material, the reaction catalyst, and ethylene glycol were added, and the reaction temperature was Glycolysis depolymerization was carried out in the same manner as in the comparative example, except that the temperature was kept at 153°C. In Comparative Example 4, the depolymerization reaction was carried out using zinc acetate as a catalyst. In Comparative Examples 5 and 6, potassium acetate and sodium acetate were used as catalysts in the depolymerization reactions. In Example 1, a zinc acetate catalyst was used, which corresponds to the above-mentioned Chemical Formula 1. The compound anisole was added as an additive and the depolymerization reaction was carried out according to the method of Experimental Example 2. In Examples 2 and 3, potassium acetate and sodium acetate were used as catalysts, respectively. The rest of the experiment was carried out in the same manner as in Example 1.
[0141] The anisole used as the additive is extracted from natural sources, but is not commercially available. It can also be synthesized in large quantities and is used as a raw material or precursor for the production of fragrances and perfumes. Its toxicity is much lower than that of other aromatic compounds.
[0142] The raw materials derived from PET bottles used in the comparative examples and examples have an amorphous structure. Since the raw material with a large unit area of less than 0.3 mm is fed into the reaction, the initial depolymerization A high effective contact area with additives, catalysts, reactants, etc. can be maintained from the early stage. Depolymerization raw materials with different geometric forms, such as molecular polymerization degree, properties, and material thickness, have different mass transfer and This can affect the reaction rate and ultimately the desired product of depolymerization. Examples 4 to 6 show a significant effect on the yield and performance of the waste plastics that may be generated in daily life. Among plastics, multi-layered PET bottles, colored PET labels, polyester The terephthalate fiber was crushed and cut into 1 cm pieces. 2 The waste resin prepared in the following areas was quantified as polymer raw material. After that, the depolymerization reaction was carried out for each of them. Depolymerization was carried out.
[0143] [Table 2]
[0144] As shown in Table 1, Comparative Example 1 in which zinc acetate was used as a catalyst and a high temperature of 197° C. was applied In the case of the same reaction mixture composition, most of the PET was decomposed, but at a lower temperature (153 According to the results shown as Comparative Example 4 in Table 2, the conversion rate was less than 10%. The reactivity of the product was extremely low. In addition, the ratio of by-products was relatively high compared to the target product. Obtained.
[0145] Comparative Examples 5 and 6 were prepared in a similar manner, but using alkali metal cations instead of zinc acetate. The reaction is carried out using metal salts, specifically potassium acetate and sodium acetate, as catalysts. Compared to Comparative Example 4, the conversion rate increased slightly, but the reactivity was greatly improved. At the same time, the amount of by-products produced increased significantly. (Comparative Example 1 and Comparative Example 4) showed higher BHET selectivity.
[0146] The reaction results of Example 1 were the same as those of Comparative Example 4 except that only anisole was added to the reactant composition. The glycolysis was carried out at a low temperature (153°C) using the following. When comparing the depolymerization results of the two, the addition of the additive of the present invention dramatically changed the depolymerization performance. It can be seen that this has a beneficial effect. The reaction in Example 1 was carried out at low temperatures, 40°C or higher. Despite the low yield, a BHET yield of 82.5% was obtained within 2 hours. When the reaction time was maintained for more than 3 hours, a BHET yield of 85% to 90% was obtained. .
[0147] When the catalyst was changed to an alkali metal acetate catalyst, a more dramatic effect was observed. For example, potassium acetate and sodium acetate are used as catalysts, and the reaction is carried out at low temperature (15 The results of the glycolysis reaction carried out at a temperature of 3°C (Examples 2 and 3) are compared with those of the reaction at a high temperature (Comparative Example 2 and Comparative Example 3) and the low-temperature glycolysis reaction without additives (Comparative Examples 5 and The reaction product composition of Comparative Example 5 (or Comparative Example 6) can be compared with that of Comparative Example 6. In the case of Example 2 (or Example 3) where low-temperature glycolysis was carried out with the addition of alcohol, the presence of the additive As in Example 1, in which depolymerization was carried out using zinc acetate as a catalyst under the presence of The depolymerization was observed by adding anisole to the reaction system using alkali metal as a catalyst. Even though the reaction temperature was kept low at 153°C, all the raw PET was In addition, the selectivity of BHET was also significantly improved. It is effective for the high temperature glycolysis reaction at 197℃. Catalysts in modified form, such as catalysts in the form of other salts containing alkali metals, and catalysts based on guanidine The addition of anisole to catalyst systems containing nonmetallic organic catalysts such as As a result, the reactivity was dramatically increased in the low-temperature glycolysis reaction below 153°C. For the catalytic systems, selectivity was also observed to improve. Performance is explained in more detail in Section 1.7.
[0148] On the other hand, the depolymerization of Examples 4 to 6, in which polymer raw materials with different properties were used under the same conditions, Comparing the synthesis reaction results, the intrinsic viscosity (IV~ 0.65), it is expected that the mass transfer restriction during the depolymerization process is low. In the case of Example 6, polyester fiber was used as the raw material, but the PET flakes were used as the raw material (IV= It was found that a higher yield of BHET was obtained compared to other cases where the catalyst was used as a catalyst (0.74). In the case of Example 4, in which multi-layered PET flakes were used as the raw material, the The yield of BHET from the reaction alone was observed to be somewhat low at 82.5%.
[0149] On the other hand, thin colored PET films are expected to be less affected by mass transfer. In the case of Example 5, in which the starting material was used, the initial reactivity was observed to be high, but the yield was 8. In this case, the yield did not improve even if the reaction was left in the reaction conditions for a long time. The BHET yield is low and not improved, but impurities such as pigments have a negative effect on the depolymerization performance. It can be inferred that this is the result of the influence.
[0150] 1.3 Temperature range of low-temperature depolymerization reaction In the following embodiment, the composition of reactants is maintained effective for the low temperature glycolysis reaction, thereby This is to explain the range in which the reaction or depolymerization performance is effective at low temperatures. In the following example, we will consider other factors besides temperature to determine the qualitative and quantitative reaction characteristics of the depolymerization reaction. The conditions are kept the same and the temperature is changed to observe the depolymerization performance. Includes specific examples.
[0151] [Table 3]
[0152] Table 3 shows the results of the reaction carried out in the same manner as in Example 3, except that the reaction temperature was kept at 130 to 150°C. The results are shown in Table 1. Sodium acetate (NaOAc) was used as a catalyst at 0.04 moles, and anisole and ethyl acetate were The ethylene glycol was used at 4 and 12 moles, respectively. The reaction time was 3 or 6 hours in total. The experiment was repeated so that the reaction could proceed in the same way. Samples were prepared and quantitatively analyzed by HPLC, and the conversion rates and yields were compared. did.
[0153] According to an example of the reactant composition according to the present invention, anisole was added to the PET feedstock. As a result of low-temperature glycolysis, clear and effective reaction characteristics were observed at temperatures above 130°C. At 145°C or higher, the conversion rate approaches 100% when exposed to a long reaction time (6 hours). A very dramatic effect was observed.
[0154] On the other hand, in the case of Example 11 where depolymerization was carried out at 150°C, the depolymerization was completed within 3 hours due to the high reactivity. However, when exposed to reaction conditions for a long time, it decomposed into the monomer product (BHET). The selectivity of the target product to the catalyzed reaction was observed to be somewhat low. This is because the target product already produced was converted to the catalyzed reaction at high temperatures. With sustained exposure, the side reaction pathway of hydrolysis of BHET ) the MHET yield increases gradually. In order to ensure complete decomposition and prevent side reactions from proceeding, it is necessary to control not only the temperature but also the reaction rate. The reaction time is also preferably optimized to improve the final yield of the desired product.
[0155] 1.4 Evaluation of depolymerization reaction performance depending on the amount of additive The following specific examples are examples of reactant compositions and reaction conditions that are effective for low-temperature glycolysis reactions. Both of these are intended to explain the effective range in which the additive's effects are expressed. In the example, to characterize the depolymerization reaction, the reaction conditions were kept the same but the additive was added. Specific examples are included that were carried out to observe the depolymerization performance at different dosages.
[0156] Table 4 shows the results of depolymerization of PET without adding any additives (Comparative Example 5 and Comparative Example 6). The amount of additive added to the reaction was varied (Examples 12 and 13). ) and depolymerized at low temperature (153℃) for 2 hours. The results show the change in the amount of anisole added from 0g to 39.4g. g (7 moles per mole of polymer repeating unit) and repeated experiments were performed. The glycolysis depolymerization was carried out in the same manner as in Example 2 or Example 3, except for the amount of additives. This corresponds to the case where the implementation and evaluation of the project was carried out.
[0157] [Table 4]
[0158] Although a metal salt containing an alkali metal cation is used as a catalyst, the chemical formula according to the present invention In Comparative Examples 5 and 6, in which no additive corresponding to 1 was added, the glycolysis reaction was very poor. Although the stress response was observed, even a small amount of additive (anisole) was added. The results of Example 13 show that not only was the reactivity increased, but the glycolysis reaction of PET also In particular, the selectivity of the BHET produced by the applied polymer precursor is greatly improved. When the molar ratio of additive to feedstock is increased to 3 or more, the polymer is formed in only 2 hours of reaction. It can be seen that most of the product is decomposed, and the selectivity to the target product is maintained at a high value.
[0159] On the other hand, the additives used are used as reactants when the temperature drops below 100°C. Phase separation occurs from the excess ethylene glycol, and excess ethylene glycol is removed for purification of the desired product. When water is added, only a very limited concentration of additives remains in the aqueous solution of the desired product. Therefore, the additive can be easily recovered by liquid-liquid extraction. It is easy to separate them, but rather, at the end of the reaction, the reaction temperature is raised to the boiling point of the additive. After the addition, some or all of the additive condensed in the condenser is separated into the external stream. The liquid separation method is more advantageous in terms of efficiency. The additive according to the present invention does not directly participate in the reaction. However, it is considered to be a catalyst because it clearly has the effect of lowering the activation energy of the reaction. It has similar properties, but does not show direct reactivity in the absence of metal salts or other catalysts. It can be seen that the catalyst exhibits promoter-like properties because it does not result in any increase in the catalyst load.
[0160] 1.5 Performance evaluation of depolymerization reaction depending on catalyst amount The following examples are examples of reactant compositions and reaction conditions that are effective for low-temperature glycolysis reactions. The following example is intended to explain the effect of adjusting the amount of catalyst added. In order to distinguish the characteristics of the polymerization reaction, the reaction conditions were kept the same (reaction temperature: 153°C, reaction time: The depolymerization performance was observed by changing the amount of catalyst added. This document includes specific examples of how to achieve this.
[0161] [Table 5]
[0162] Table 5 shows the amount of catalyst (metal salt containing alkali metal cation) added, from 0 g to 1.0 g (high The experiment was repeated with the concentration of The glycolysis depolymerization was carried out in the same manner as in Examples 2 and 3, respectively. The results are shown in Examples 14 and 15.
[0163] The catalyst is added in a minute amount of less than 0.01 moles relative to the repeating unit of the polymer raw material. It was observed that the reactivity decreased significantly, but the selectivity of the target product, BHET, was This is because the side reaction rate increases with increasing catalyst loading. It can be expected that this is because the catalyst has a greater effect on the repeated synthesis of polymer raw materials. When added in excess of 0.01 mole ratio to the unit, the high reactivity of the added units Most of the added PET was degraded, and when added at >0.03, complete degradation occurred. To ensure complete decomposition, the amount of catalyst should be greater than 0.03 but less than 0.10 molar ratio. Within the range of the catalyst ratio, the selectivity and yield of the target product (BHET) are very small depending on the amount of catalyst. A significant change was observed, but when the catalyst was used in excess of 0.10 molar, the amount of by-products produced increased. This confirmed that the BHET yield was somewhat lower. As a result of observing the characteristics of the depolymerization reaction depending on the amount of catalyst input, it was found that the depolymerization reaction was stable over a relatively wide range. This allows the reaction performance to be maintained and adjusted by reusing some of the catalyst after the reaction is completed. Even if the catalyst concentration is not precisely adjusted when the catalyst is added, the amount of catalyst that is considered to have disappeared may be large. Since only the production department needs to be replenished, it is expected that flexibility will be ensured in the operation of the process. This can be done.
[0164] 1.6 Evaluation of depolymerization reaction performance by type of additive The following examples are examples of reactant compositions and reaction conditions that are effective for low-temperature glycolysis reactions. Also, the effect of the reaction when the additive according to the present invention is partially or completely modified is explained. In order to characterize the depolymerization reaction, the reaction conditions were kept the same (reaction temperature, Temperature: 153°C, reaction time: 2 hours, catalyst: KOAc) but the reaction When using compounds that contain oxygen in the bonded functional group, do you change the number of bonded functional groups? A specific example of observing the depolymerization performance by adding an additive having a modified form is shown below. include.
[0165] [Table 6]
[0166] Table 6 shows that instead of the anisole used as the additive in the examples, other forms of additive were used. The purpose of this study is to investigate the effect of using this product on low-temperature depolymerization reactions. Other forms of additives were used in place of anisole at 4 moles per mole of polymer repeat unit. Glycolysis depolymerization was carried out and evaluated in the same manner as in Example 2, except that the mixture was added to the Ta.
[0167] Comparative Example 5, in which PET glycolysis was performed without the addition of any additive, and Comparative Example 6, in which PET glycolysis was performed without the addition of any additive and The method was carried out by adding a compound containing at least one oxygen atom in the bond functional group between the Comparing the results of Example 2 and Examples 16 to 20, there are some differences in performance, but It can be seen that the effect of adding the additive of the present invention is remarkable. According to the results of the depolymerization performance in Examples 16 to 18, which show examples of the agent, When m in the cyclohexane dimer is increased to 2 or more, the reactivity and selectivity of the target product are somewhat decreased. In Examples 19 and 20, the number of carbon atoms in the alkyl group bonded by oxygen is 1. Modification additives that may be further bonded to other types of functional groups that are not alkyl functional groups or may not have alkyl functional groups. This is an example of depolymerization performed by adding the above. Although some deviations in reactivity and BHET yield were observed, the effect of the present invention was It was found that the above phenomenon was clearly observed. Comparative Example 7 was a compound having the same structure as the additive of the present invention. However, the central functional group of the compound is different from that of methoxycyclohexane (at least one The alkyl groups are linked via a linker, the linker having at least one oxygen atom. (The central functional group is not an aromatic ring but a saturated cycloalkane compound with the same number of carbon atoms.) The depolymerization performance was evaluated by replacing the additive with the additive. Even lower reactivity and BHET selectivity were observed than in the case of 5.
[0168] In a specific embodiment of the present invention, the additives added are evaluated on the basis of the same mole number. However, different forms of the binding functional groups may result in different interactions with raw materials and additives. By adjusting the form and amount of additives added to the reactants, the performance deficiencies can be compensated for. It is also possible.
[0169] 1.7 Performance evaluation of low-temperature depolymerization reaction using various catalysts The following specific examples are examples of reactant compositions and reaction conditions that are effective for low-temperature glycolysis reactions. The reaction temperature was 153°C and the reaction time was 2 hours, and the type of the catalyst according to the present invention was partially or completely The purpose of this study is to explain the effect of different parts of the reaction on the depolymerization reaction. In order to distinguish between the two, the reaction conditions were kept the same, and alkali metal or alkaline earth metal cations were added. Metal salts containing cations are used as catalysts, and counter ions are carbonate, bicarbonate, or alkoxy. Either transform it into another form such as silane, or apply a metal-free organic compound catalyst. This includes a specific example in which the change in depolymerization performance is observed by changing the temperature.
[0170] [Table 7]
[0171] Table 7 compares the low-temperature (153°C) depolymerization performance by applying the various catalyst forms described. The additive according to the present invention is added, but all the additives added to the polymer are By limiting the amount of compound, the reaction rate limit region (kinet The catalyst was evaluated in the ic limited regime. Add 0.02 moles of ethylene glycol per mole, and add about 32.30 g (polymer 10 moles per mole of repeating unit), and about 16.88 g of anisole (polymer repeating unit The glycolysis depolymerization was carried out in the same manner as in Example 1, except that a 100% glycerol was used (3 moles per mole). The results were not included, but the counter ions listed in Table 7 were used in different forms. The catalyst used was one of the various modified catalysts or organic compounds listed in the above, but the additives according to the present invention were not used. The catalyst's standalone performance was first observed by carrying out depolymerization at low temperature (153°C) without the addition of additives. As can be expected from the results of the specific comparison explained above, even if the catalyst is changed, the additives are added. When the reaction was carried out without using the catalyst, the reactivity was low and the reaction was extremely slow, similar to the performance results of Comparative Examples 4 to 6. Only limited BHET yields were observed.
[0172] Example 21 using a metal salt catalyst with a cation of Group 1A metal and an anion of carbonate ion In the case of Example 22, similar to the case where a catalyst in which the anion is an acetate ion is used, high High reactivity and high monomer yields were observed. In contrast, the same number of moles of bicarbonate were added to the anion. In the cases of Examples 23 and 24 having the same as the cation exchange resin as the cation exchange resin, relatively low reaction performance was observed. Glycolysis carried out under the same conditions using metal carbonate catalysts composed of group 2A metal cations In the case of the reaction (Example 25), the catalyst was an alkali metal salt having bicarbonate as the anion. High reactivity and high monomer yield were observed even when the same conditions were applied and the metal-containing Triazabicyclodecene, an organic compound catalyst that does not have the same molar amount, was used as the catalyst. In the case of Example 27, the conversion rate of the reaction was 99.0% or more, and the yield of BHET was 81. A highly effective glycolysis reaction was observed, with a conversion of more than 0.8%.
[0173] As can be seen from the results of the depolymerization reaction using various modified forms of the transesterification catalyst, By adding the additive of the present invention (a compound represented by chemical formula 1), the esophagus can be heated at a low temperature (153°C). The glycolysis reactivity of polymers containing tert-functional groups can be significantly improved. It is clear that a high yield of BHET can be obtained below the boiling point of ethylene glycol.
[0174] 1.8 Purification and analysis of glycol addition monomer produced after depolymerization reaction In the following specific example, a polymer containing an ester functional group is depolymerized by the method of the present invention. After that, the physical and chemical properties, including purity, of the BHET product obtained from the refining process are identified. Such a process may include a separation method to recover the additive. As explained in the specific example above, the addition of additives increases the temperature range below 153°C. It is possible to carry out high-performance glycolysis reactions in the high-temperature range of 197°C or higher. It is possible to introduce catalytic systems that are difficult to dissolve, which can bring various benefits to the refining process. For example, the range of catalytic reactions that perform optimally at low temperatures is dominated by alkali metal salts. It can be expanded and used as a catalyst for organic compounds that may decompose at high temperatures without loss. This allows for easy purification and material recovery. , eliminating the need for catalysts containing harmful metals such as zinc, lead, and other heavy metals. Manufacturing raw materials for environmentally friendly high-quality materials, or creating a perfect waste plastic circular economy It is expected that this technology will prove useful as a recycling technology for this purpose.
[0175] In the following examples, the mass ratios of the compounds presented in this invention are kept the same and the The depolymerization reaction using zinc acetate as a catalyst without additives at 197°C and anisotropy were The solution was carried out at low temperature (153°C) using acetates of group 1A metals as catalysts with the addition of ethanol. The glycoconjugates obtained after the purification process of the products from each of the reaction products obtained from the polymerization reaction and Specific examples are included that were carried out to assess the yield and purity of the diol addition monomer.
[0176] Table 8 shows the quality of the polymer raw material, reaction catalyst, and ethylene glycol used in the depolymerization reaction. The ratio is 1:0.1:4 (when additives are added, the amount of additives is twice as much as the polymer raw material. A certain amount of the mixture was added so that the depolymerization was carried out according to the method of Experimental Example 1 or Experimental Example 2. In the case of Comparative Example 8, in which a zinc acetate catalyst was used without adding any additive, at a high temperature (197°C), Examples 28 and 29 in which anisole was added and potassium acetate and sodium acetate were used as catalysts In the case of 29, depolymerization was performed at a low temperature (153 °C), and the same purification process as in Experimental Example 3 was performed. The depolymerized product was obtained through ICP and 1 H-NMR For Comparative Example 8, the product was washed in the same manner as in Experimental Example 4. Comparative Example 9) It was confirmed whether the quality was improved.
[0177] [Table 8]
[0178] The residual metal amounts of Comparative Example 8 and Examples 28 to 29 shown in Table 8 were determined by the glycolysis reaction of PET. After obtaining the product according to the route, the BHET obtained by the first recrystallization was The residual metal content was measured by ICP-MS and ICP-AES with a detection limit of 1 ppm or more. These are the results of analysis using analytical methods.
[0179] In the case of BHET, which was purified after reacting with zinc acetate, some residual metals were detected. The zinc used as a catalyst is classified as an important mineral for the human body. High doses or sustained exposure to the human body through the use of products such as beverage containers can lead to digestive disorders. It is classified as a hazardous metal that can cause chemical disorders. It remains in plastics. Indirect absorption occurs when zinc is naturally excreted as waste and accumulated in plants and animals, and then reabsorbed by the human body. Depending on the route, various side effects may occur. Therefore, it is important to use an alternative route. The potential of low-temperature depolymerization reaction technology based on non-toxic metal catalysts will improve not only the commercial viability of the product but also the environment. This may be advantageous in terms of reducing pollution.
[0180] Therefore, an alkali metal salt is used as a catalyst, but the same zinc acetate as used in Comparative Example 8 is used. The same mass was added as a catalyst (the number of moles of metal was greater than in Comparative Example 8). ) and the reaction and purification were carried out. No residual metals were detected in the final product produced using the potash metal salt catalyst. The metal ions that make up the metal are themselves essential electrolytes in the human body and are less harmful than zinc. The advantage of this is that the residual metal content in the products produced by Examples 28 and 29 is low. The reason for the low distillate is that the components that make up the catalyst are much more stable in the aqueous solution than zinc acetate during the refining process. Since it has a very high degree of ionization, dissociation occurs easily and recrystallization and physical filtration are not possible. The solid phase remains in the recovered BHET product, or does not dissolve into the aqueous phase. This is because the amount of metal is very dilute.
[0181] The qualitative characteristics of the purified glycol addition monomer were 1 H-NMR was used to observe the Specific spectra are shown in FIG. 1 to FIG.
[0182] For the high-temperature glycolysis-based monomer obtained by purification according to the method of Comparative Example 8 1 H-NM R is as follows:
[0183] 1 H-NMR (500 MHz, DMSO-d 6 ) δ(ppm): 8.12(s, 4H) , 4.99(br s, 2H), 4.33(t, 4H), 3.73(t, 4H)
[0184] Ethylene glycol was used as a monomer for BHET obtained from the glycolysis of PET. According to many previous publications on NMR spectra, the most important peaks are observed around 4.95 ppm. The characteristic peak due to the hydrogen of the terminal hydroxyl group is dominated by the hydrogen of the adjacent ethylene group. At around 3.73 ppm, the triplet is split into three peaks, one for the hydroxyl group and one for the 1.25 group. A quartet characterized by hydrogens attached to adjacent carbons (c in Figures 2 and 3). The peaks observed are generally reported in the literature as being in the form of quartet. However, the BHET monomer obtained after simple purification according to the method of Comparative Example 8 1 H-NM In the R spectrum, a broad single peak is observed at around 4.99 ppm and 3.27 ppm. A triplet was observed near m. This is due to impurities remaining in BHET, as shown in Table 8. It can be assumed that this is due to interference from the zinc acetate catalyst.
[0185] In Comparative Example 9, the amount of residual metal in the glycol addition monomer obtained in Comparative Example 8 was In order to reduce the amount of EDTA, an additional purification method was carried out. The final white powder product from Comparative Example 8 was added with distilled water maintained at a constant temperature. After the addition, the mixture was stirred for about 1 hour. After the completion of the above, the mixture was filtered using the same filter as that used in Comparative Example 8. The washed precipitate was collected and dried. The process is repeated until the BHET monomer is no longer detectable within the ICP detection limit. After obtaining it, it was remeasured 1H The characteristic peaks in the NMR spectrum are as follows:
[0186] 1 H-NMR (500 MHz, DMSO-d 6 ) δ(ppm): 8.12(s, 4H) , 4.97(t, 2H), 4.33(t, 4H), 3.73(q, 4H)
[0187] The high-temperature glycolysis-based monomer obtained by purification according to the method of Comparative Example 8 had a 4.9 A broad single peak was observed at around 9 ppm, which split into a triplet at around 4.97 ppm. At around 3.73 ppm, a quartet rather than a triplet peak was observed.
[0188] The following is a description of how glycolysis was carried out using the method of Example 28 (using potassium acetate) and how the product was purified. The analytical method of Comparative Example 8 was used for the BHET monomer recovered without any additional purification process after preparation. As well as the law 1 Structural analysis was performed using H-NMR, and the characteristic peaks observed were as follows: there were.
[0189] 1 H-NMR (500 MHz, DMSO-d 6 ) δ(ppm): 8.12(s, 4H) , 4.95(t, 2H), 4.33(t, 4H), 3.73(q, 4H) BHET (act.) recovered by reaction and purification using the method of Example 29 (using sodium acetate) The same process and method as in Example 28 are applied. 1 H-NMR spectrum I was able to get it.
[0190] These comparative examples and examples show that the monomer containing residual zinc metal and the monomer with high purity are As well as the distinct structural characteristics, the catalytic systems prepared according to the present invention provide The BHET obtained can be obtained in high purity through a simple purification process. This is advantageous in terms of productivity and economy.
[0191] 2. Extractant for removing color-producing foreign substances from monomers of polymers containing ester functional groups and a method for purifying a monomer using the same
[0192] [Raw materials 5 and 6] Colored label paper made from waste plastic containers discarded after consumption, the polymer component of which is PET Chisels were collected and separated by main color, and cut into pieces with each side measuring 0.5 cm or less. The polyester fabric dyed with disperse dyes is cut into 1 cm 2 Raw material 6 was prepared as a fiber raw material so as to have the following area.
[0193] Example 5: Liquid-liquid extraction step After the reaction was completed, about 200 g of distilled water at 95 to 100°C was added to the filtrate. The mixture was transferred to a vessel kept at 75°C and stirred. After one hour, stirring was stopped and phase separation was observed. When this occurred, the aqueous solution layer below was removed and left at room temperature to lower the temperature.
[0194] Example 6: Liquid-liquid stripping step The organic solution layer separated in the liquid-liquid extraction step similar to that in Experiment 5 was diluted with distilled water at 95-100°C. After adding 200g, transfer to a container maintained at 75°C and stir. Stop stirring after 1 hour. When the reaction was stopped and phase separation occurred, the lower aqueous solution layer was removed and left at room temperature to lower the temperature.
[0195] Experimental Example 7: Depolymerization product stage The reaction mixture solution containing the monomer or the reaction mixture solution of Experimental Example 5 or The aqueous phase extracted in Experiment 6 was left for 12 hours, and the crystallized solid phase was separated by physical filtration. After removing a large amount of water using the method, the solid was taken out. The depolymerized product was obtained after transferring to a vacuum dryer maintained at room temperature and vacuum drying for 12 hours or more.
[0196] Experimental Example 8: Organic Solvent and Dye Recovery Step The upper phase (organic layer) remaining after separation of the aqueous solution layer in Experimental Example 5 or Experimental Example 6 was distilled in a simple distillation apparatus. The anisole was separated into the vapor phase and condensed into the liquid phase. Each of the resulting products was measured with an accuracy of ±0.05. Quantification was performed using a 0.1 mg high precision balance.
[0197] 2.1 Production of high-purity monomers from waste PET films containing pigments Comparative Examples 10 and 11 are colored PET films containing pigments (classified into yellow and green). The raw material 5 thus obtained is used as the polymer raw material, and the reaction conditions and Depolymerization was performed using the above compound composition, and each of the products was filtered using the filtration method of Experimental Example 3. After removing the oligomers from the reaction mixture, the monomer product was obtained according to the procedure of Experimental Example 7. .
[0198] In Example 30, the raw material 5 was used, and the same reactant composition and reaction conditions as in Example 2 were used to depolymerize the raw material 5. The mixture was mixed and subjected to liquid-liquid extraction according to the method of Experimental Example 5, after which the aqueous phase was taken and the same was extracted as in Experimental Example 7. The monomer product was obtained through the process, and Example 31 is the water-soluble monomer product obtained in Example 30. The liquid-liquid extraction step of Example 5 was repeated one more time with additional anisole (22.5 g) added to the liquid layer. After repeating the cycle, the monomer product was obtained according to the process of Experimental Example 7.
[0199] In Example 32, the depolymerized product obtained from Comparative Example 10 was mixed with about 22.5 g of anisole and 95 to 100 g of ethanol. After adding about 200 g of distilled water at 100° C., the liquid-liquid extraction of Experimental Example 5 was carried out, and then the aqueous solution The phase was separated and the monomer product was obtained according to the method of Example 7.
[0200] Example 33 is a liquid-liquid extraction method for the liquid-liquid extraction of Example 6 using the organic layer separated in the liquid-liquid extraction process of Example 31. After the liquid stripping step, the aqueous phase was taken and the monomer product was obtained according to the method of Example 7. That's what I wanted.
[0201] Nuclear magnetic resonance spectrometer (model Name: Bruker Avance II 500MHz) The structural characteristics were confirmed. The mass values of the samples and the relative area ratios of the characteristic peaks were used to determine the depolymerization products. The amount of color-producing organic foreign matter remaining in the product was estimated. For foreign substances, add 10 mg of DMSO-d 6 The samples were diluted with 0.7 ml of solvent and measured. was used.
[0202] Glycolysis using polymers containing ester functional groups as starting materials. The reaction product BHET (bis(2-hydroxyethyl)terephthalate) alate) monomer and concentrated pigment recovered from colored PET film (according to Example 8) (manufactured by 1 The H-NMR spectrum is shown in Figure 5. Processes of Examples 31 to 33 The depolymerized product produced by the method is BHET monomer purified to a high purity of 99.9% or more. This was diluted and measured. 1 The H NMR spectrum has been reported in many publications. The observed peak values were very similar to the reported characteristic peak values.
[0203] 1 H-NMR (500 MHz, DMSO-d 6 ) δ(ppm): 8.13(s, 4H) , 4.96(t, 2H), 4.32(t, 4H), 3.72(q, 4H)
[0204] As reported, the hydroxyl group at the most terminal group at around 4.96 ppm The characteristic peaks due to the hydrogen atoms in the adjacent ethylene groups are triplet peaks due to the interaction with the hydrogen atoms in the adjacent ethylene groups. It was observed as a triplet, and at around 3.72 ppm, A hydrogen bonded directly to the ethylene functional group adjacent to the silyl group (BHET chemistry shown in Figure 5) A quartet-like peak characterized by the following formulas (corresponding to formulas 3 and 4): No distortion was observed.
[0205] NMR spectrum of pigment-containing organic foreign matter extracted from colored PET film (Figure 5 The upper spectrum of the 100 nm NMR spectrum is very complex and requires the usual physical properties to purify the polymer depolymerization products. If only selective filtration is applied, some of the organic matter can be removed, but the color-producing organic mixture cannot be removed. It is not easy to do this. In particular, the chemical shift value is Organic compounds characterized as 0.94 and 4.69 ppm were present in only trace amounts. The color-developing properties of the film are similar to those of the starting colored PET film. By using this extraction method, it is possible to highly purify the polymer depolymerized monomer product (BHET). It was Noh.
[0206] The mass values of the samples (organic foreign matter and purified BHET) used in the NMR spectra were identified. The amount of foreign matter was calculated by comparing the integral value of the functional peak with the chemical shift value. The estimated foreign matter content is presented in Table 9.
[0207] [Table 9]
[0208] The yield of the depolymerization product is the total number of moles of repeating units in the polymer that was added as the initial raw material. The amount of depolymerized product obtained in each step was determined by HPLC. The ratio of the number of films per 1000 was calculated as a percentage. The depolymerized cellulose was recovered in Comparative Example 10, Comparative Example 11, and Examples 30 to 33. The amount of monomer product is listed as the molar yield (%) of BHET in Table 9. By repeating the above process, it was observed that the content of foreign matter was very low. As the mass of monomer lost during the purification process increased, the yield of the final product decreased. .
[0209] 2.2 Production of high-purity monomer from dye-containing polyester fiber Unlike pigments, which are colored in the form of particles or powder after being dispersed in a solvent, Dyes used in this field are mainly used to dye textile materials, leather, etc. In particular, polymeric fibers containing ester functional groups, such as polyester, are used as textile materials. Dyes, a form of organic compound containing one or more aromatic rings, are commonly used for coloring. will be done.
[0210] The dye is selected from terephthalic acid, which is a component of the polymer fiber, in order to prevent discoloration from the polymer fiber. Substances that have a very high affinity for the carboxylate functional group are used as dyes and have physical and chemical properties. It must have the properties to be chemically uniformly distributed in the fibers, which allows the solution to be High interaction with monomers or low molecular weight compounds produced by depolymerization even if polymerization is performed Therefore, it is not easy to separate and purify the product into high purity. Or, a solvent that has some miscibility with low molecular weight compounds but has a strong affinity with organic dyes. When a large amount of hydrophilic solvent is added to the mixture, the asymmetric distribution of the solute (dye) is achieved. This allows for the recovery of high purity products.
[0211] Comparative Example 12 was the same as Comparative Example 1 except that Raw Material 6 (dark blue waste polyester fiber) was used. The monomer product was obtained by the same method as in Example 1, and Example 34 used raw material 6. Except for this, the monomer product was obtained in the same manner as in Example 31.
[0212] Example 35 uses the organic layer separated during the repeated liquid-liquid extraction of Example 34 as a raw material. After carrying out the liquid-liquid stripping step of Example 6, the aqueous phase was taken and subjected to the method of Example 7. The monomer product was obtained by
[0213] In Example 36, the liquid-liquid extraction process in Example 34 was repeated a total of four times, and then the aqueous solution was The liquid phase was taken and the monomer product was obtained according to the method of Example 7.
[0214] Figure 6 shows the depolymerization of colored polyester fiber as raw material and the BH obtained from the reaction. The NMR spectra for the ET monomer and the dyestuff recovered and concentrated by Experiment 8 are shown. .
[0215] A portion of the product produced according to the methods of Examples 34 to 36 was obtained as a sample. 1 H-NMR The spectra are similar to those obtained from Examples 30 to 33, which apply raw materials containing pigments. The main peak was clearly observed from the characteristic chemical shift value, which indicates the structural characteristics of the BHET monomer. However, limiting extraction recovery or recovering additional product by back-extraction The overall yield of depolymerized products can be increased, whereas the purity of BHET monomer is 99%. %, and the dye-specific color is contained, and the removal of foreign matter is effective It can be seen that this is not the case. As a result, even if only a trace amount of organic dyes (1% or less by weight) remains, it is considered that the product contains color impurities. It was easily possible to visually determine that the material was present.
[0216] As an example, a high-performance pigment was obtained by purifying the reaction product obtained from the depolymerization of waste PET raw materials containing pigments. In order to recover BHET of the same quality as the monomer product (Examples 31 to 33) with the same purity, It can be seen that multiple repeated extraction steps are required, as in the purification step of Example 36.
[0217] Table 10 shows the results of the depolymerization reaction mixture obtained using a colored polyester raw material to obtain high-purity monolayers. This is a specific example showing the process of obtaining mer. Extraction and purification by adding a compound represented by chemical formula 1 By applying the process (Example 5), it is possible to efficiently remove organic disperse dyes that make up the color. It was found that when the extraction and purification process was repeated two or more times (Example 34), When back-extraction was performed using the organic phase generated during the extraction process (Example 35), the product obtained was: Although the product had a purity of 99.5% or more, a slight amount of residual dye caused a pale red powder to appear in the product. When the extraction and purification process was repeated four or more times, the yield of the final product was about 51%. The residual amount of dye was detected at a level of less than 0.1%. A white BHET product was obtained.
[0218] [Table 10]
[0219] As described above, certain parts of the present invention have been described in detail. To those skilled in the art, these specific techniques are merely preferred embodiments and should not be construed as limiting the scope of the invention. It is clear that the scope of the present invention is not limited by the above. The true scope of the invention is defined by the appended claims and their equivalents. It should be. [Industrial Applicability]
[0220] A method for depolymerizing polymers containing ester functional groups, with or without pigments or dyes; Compositions for the depolymerization and purification of the polymer by selectively separating contaminants from monomers of the polymer. The present invention relates to a method for the preparation, recovery, reuse, etc. of polymers containing ester functional groups. The present invention can be usefully used in the above technical fields, and thus has industrial applicability.
Claims
1. 1. A method for depolymerizing a polymer containing an ester functional group, comprising the steps of: (A) one or more polyhydric alcohols, (B) a transesterification catalyst, and (C) A compound represented by the following chemical formula 1: contacting the polymer containing ester functional groups with a mixture comprising A method for producing a polymer containing an ester functional group, comprising the steps of: depolymerizing a polymer containing an ester functional group; A method for depolymerizing a polymer. [Chemical formula 1] (Wherein, the substituent R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 Alkyl groups of C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 of aryl groups One of the following is selected: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, The substituent R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.)
2. The catalyst for the transesterification reaction is a metal-free organic catalyst or a Group 1A, 2A 2. The metal salt of claim 1, wherein the metal salt is one or more selected from the group consisting of metal salts of group 2A and 2B metals.
2. A method for depolymerizing a polymer containing an ester functional group according to claim 1.
3. The metal salt has a counter ion of carbonate, bicarbonate, alkoxide or is composed of an organic anion selected from the group consisting of acetate and ethyl acetate.
2. A method for depolymerizing a polymer containing an ester functional group according to claim 1.
4. The polyhydric alcohol is ethylene glycol, diethylene glycol, triethylene glycol, Licor, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol ol, 1,7-octanediol, 1,9-nonanediol, neopentyl glycol , 1,4-cyclohexanediol, isosorbide, and 1,4-cyclohexane The compound according to claim 1, characterized in that the compound is at least one selected from the group consisting of xane dimethanol. The present invention relates to a method for depolymerizing a polymer containing an ester functional group.
5. Polymers containing ester functional groups include polyethylene terephthalate (PET), polypropylene propylene terephthalate (PPT), polyglycolide or polyglycolic acid (PGA), Polylactic acid (PLA), polycaprolactone (PCL), polyhydroxyalkanoate ( PHA), polyhydroxybutyric acid (PHB), polyethylene adipate (PEA), polyb Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) Acid) (PHBV), Polybutylene terephthalate (PBT), Polytrimethylene terephthalate Poly(ethylene terephthalate), polyethylene naphthalate (PEN), and Vectran The ester functional group-containing polymer according to claim 1, characterized in that it is one or more selected from the group consisting of A method for depolymerizing polymers.
6. The compound represented by the formula 1 is methoxybenzene, 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, 1,2,3-trimethoxy Benzene, 1,2,4-trimethoxybenzene, 1,3,5-trimethoxybenzene, 1 , 2,3,4-tetramethoxybenzene, 1,2,3,5-tetramethoxybenzene, 1 , 2,4,5-tetramethoxybenzene, 2-methoxyphenol, 1,3-dimethoxy -2-hydroxybenzene, 4-hydroxy-3,5-dimethoxybenzoic acid, 3-(4- Hydroxy-3,5-dimethoxyphenyl)prop-2-enal, 4-hydroxy-3, 5-Dimethoxybenzaldehyde, 4-hydroxy-3,5-dimethoxyacetophenone , 3-(4-hydroxy-3,5-dimethoxyphenylprop-2-enoic acid, 4-enyl -2,6-dimethoxyphenol, 4-hydroxy-3-methoxybenzaldehyde, 3 -Hydroxy-4-methoxybenzaldehyde, 2-hydroxy-3-methoxybenzaldehyde aldehyde, 2-hydroxy-5-methoxybenzaldehyde, 2-hydroxy-4-meth xybenzaldehyde, 3,4-dihydroxybenzaldehyde, 1-methoxy-4-[ (E)-prop-1-enyl]benzene, 1-bromo-4-methoxybenzene, 2-te rt-Butyl-4-methoxyphenol, ethoxybenzene, 1,3,5-trichloro- 2-Methoxybenzene, 1,3,5-tribromo-2-methoxybenzene, 4-(propanol -2-en-1-yl)phenol, 1-methoxy-4(prop-2-en-1-yl) Benzene, 5-(prop-2-en-1-yl)-2H-1,3-benzodioxole, 4-Methoxy-2-[(E)-prop-1-yl]phenol and 2-methoxy-4-( It is particularly preferred that the compound is at least one selected from the group consisting of (prop-1-en-yl)phenol.
2. The method for depolymerizing a polymer containing an ester functional group according to claim 1 .
7. A composition for polymer depolymerization containing an ester functional group, comprising: (A) one or more polyhydric alcohols, (B) a transesterification catalyst, and (C) An ester functional group-containing compound represented by the following chemical formula 1: A composition for depolymerizing polymers. [Chemical formula 1] (Wherein, the substituent R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 Alkyl groups of C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 of aryl groups One of the following is selected: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, The substituent R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.)
8. The catalyst for the transesterification reaction is a metal-free organic catalyst or a Group 1A, 2A The present invention relates to a method for producing a metal salt of the present invention, and more particularly to a method for producing a metal salt of the present invention. The composition for depolymerization of polymers containing ester functional groups as described above.
9. The amount of polyhydric alcohol contained in the composition is determined based on the mole ratio of the repeating unit of the polymer to be depolymerized. The ratio of moles per unit time is 1 to 50, and the amount of the exchange esterification catalyst is determined based on the repeat rate of the polymer to be depolymerized. The ratio of moles of the repeating unit to the number of moles of the compound represented by the formula 1 is 0.001 to 1. The amount is a ratio of 0.001 to 50 moles per mole of the repeating unit of the polymer to be depolymerized. The ester functional group according to claim 7, characterized in that A composition for depolymerization of polymers comprising:
10. The depolymerization method according to any one of claims 1 to 6, A method for purifying a glycol addition monomer obtained by a depolymerization reaction of a monomer, comprising the steps of: (1) The compound represented by Chemical Formula 1 below is separated by gas-liquid separation or liquid-liquid extraction from the depolymerization reaction product. and separating the mixture using [Chemical formula 1] (Wherein, the substituent R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 Alkyl groups of C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 of aryl groups One of the following is selected: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, The substituent R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.) (2) After step (1), a solid material containing a polymer containing unreacted ester functional groups is a solids separation stage for separating (3) After the solid separation in the above (2) step, the glycol addition monomer is recrystallized and recovered. and a recovery step of said depolymerization reaction of a polymer containing an ester functional group. A method for purifying a glycol addition monomer obtained by the above process.
11. The solids containing unreacted ester functional groups are preferably separated using physical filtration. The present invention relates to a polymer having an ester functional group, and the polymer is obtained by depolymerization of the polymer having an ester functional group according to claim 10. A method for purifying the glycol addition monomer.
12. A step of separating oligomers before the recrystallization of the glycol addition monomer in the step (3). The polymer containing ester functional groups according to claim 10, characterized in that the step of A method for purifying glycol addition monomers obtained by the depolymerization reaction of the monomers.
13. Extractant for removing color-producing foreign substances from monomers of polymers containing ester functional groups And, The extractant is characterized in that it contains a compound represented by the following formula 1: Extractants for removing color-producing contaminants from monomers of polymers containing groups. [Chemical formula 1] (In the formula, R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 of Alkyl group, C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 The aryl group is selected from the group consisting of One of the following: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.)
14. The compound represented by the formula 1 is methoxybenzene, 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, 1,2,3-trimethoxy Benzene, 1,2,4-trimethoxybenzene, 1,3,5-trimethoxybenzene, 1 , 2,3,4-tetramethoxybenzene, 1,2,3,5-tetramethoxybenzene, 1 , 2,4,5-tetramethoxybenzene, 2-methoxyphenol, 1,3-dimethoxy -2-hydroxybenzene, 4-hydroxy-3,5-dimethoxybenzoic acid, 3-(4- Hydroxy-3,5-dimethoxyphenyl)prop-2-enal, 4-hydroxy-3, 5-Dimethoxybenzaldehyde, 4-hydroxy-3,5-dimethoxyacetophenone , 3-(4-hydroxy-3,5-dimethoxyphenylprop-2-enoic acid, 4-enyl -2,6-dimethoxyphenol, 4-hydroxy-3-methoxybenzaldehyde, 3 -Hydroxy-4-methoxybenzaldehyde, 2-hydroxy-3-methoxybenzaldehyde aldehyde, 2-hydroxy-5-methoxybenzaldehyde, 2-hydroxy-4-meth xybenzaldehyde, 3,4-dihydroxybenzaldehyde, 1-methoxy-4-[ (E)-prop-1-enyl]benzene, 1-bromo-4-methoxybenzene, 2-te rt-Butyl-4-methoxyphenol, ethoxybenzene, 1,3,5-trichloro- 2-Methoxybenzene, 1,3,5-tribromo-2-methoxybenzene, 4-(propanol -2-en-1-yl)phenol, 1-methoxy-4(prop-2-en-1-yl) Benzene, 5-(prop-2-en-1-yl)-2H-1,3-benzodioxole, 4-Methoxy-2-[(E)-prop-1-yl]phenol and 2-methoxy-4-( It is particularly preferred that the compound is at least one selected from the group consisting of (prop-1-en-yl)phenol. The color expression characteristic of the monomer of the polymer containing the ester functional group according to claim 13 is different. An extractant for removing material.
15. The monomer of the polymer containing an ester functional group is a polymer containing an ester functional group. The estradiol according to claim 13, which is obtained by depolymerization of a resin. Extractant for removing color-producing contaminants from monomers of polymeric resins containing aryl functional groups.
16. High purity monomers are obtained by removing color-producing foreign matter from polymer monomers containing ester functional groups.
1. A purification method for producing 1) A polymer monomer containing an ester functional group containing color-producing foreign matter is treated with the following chemical formula: adding and mixing a compound represented by formula 1; 2) allowing the mixture from step 1) to stand to induce liquid-liquid phase separation; 3) Separating and discharging the phase-separated liquid-liquid layer into an upper organic solution layer and a lower aqueous solution layer. and removing color-producing foreign matter from a monomer of a polymer containing an ester functional group to obtain a high-quality product. Purification methods to produce high purity monomers. [Chemical formula 1] (In the formula, R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 of Alkyl group, C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 The aryl group is selected from the group consisting of One of the following: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.)
17. In the step 1), in addition to the compound represented by Chemical Formula 1, The present invention is characterized in that a hydrophilic liquid or water that cannot be used for color development is added to the monomer containing the color-developing foreign matter. The present invention relates to a method for removing color-producing foreign substances from a monomer of a polymer containing an ester functional group according to claim 16. and a purification method to remove the dimethylformamide to produce a high purity monomer.
18. The monomer is a depolymerized polymer containing an ester functional group. or a partially purified mixture of the above after the depolymerization reaction. A color developing method for a polymer containing an ester functional group according to claim 16, A purification method to remove contaminants and produce high purity monomer.
19. The compound represented by formula 1 is further added to the separated aqueous solution layer to remove color-producing impurities.
17. The method according to claim 16, further comprising repeating the steps of: Color-producing foreign matter is removed from the monomer of a polymer containing a steric functional group to obtain a high-purity monomer. Purification methods for producing.
20. The separated organic solution layer is then treated with a hydrophilic liquid or Further comprising the step of adding more water and mixing, and then performing phase separation again. The method for removing color-producing foreign matter from the monomer of the polymer containing the ester functional group according to claim 16 and a purification method to produce high purity monomer.
21. From the separated aqueous phase, the monomers of polymers containing ester functional groups were obtained via recrystallization.
17. The method of claim 16, further comprising the step of recovering the ester functional group. To remove color-producing foreign matter from a polymer monomer containing A method for refining.
22. (a) adding a compound of formula 1 to a colored polymer containing an ester functional group: Floor and (b) depolymerizing the polymer containing ester functional groups; (c) adding a compound represented by Chemical Formula 1 to the depolymerization reaction product obtained from the depolymerization reaction. adding and mixing an immiscible hydrophilic solution or water; (d) allowing the mixture from step (c) to stand to induce liquid-liquid phase separation; (e) The phase-separated liquid-liquid layer is separated and discharged into an upper organic solution layer and a lower aqueous solution layer. and a monomer obtained by depolymerization of a colored polymer containing an ester functional group. A purification method for removing color-producing contaminants from cellulose acetate to produce high purity monomer. [Chemical formula 1] (In the formula, R 1 is a hydrogen atom, a hydroxyl group, an aldehyde group, a carboxyl group, C 1 ~C 6 of Alkyl group, C 4 ~C 6 and the cycloalkyl group of C 6 ~C 12 The aryl group is selected from the group consisting of One of the following: The n is an integer of 0 to 5, and when the n is 2 or more, R 1 may be the same or different, R 2 is C 1 ~C 10 is an alkyl group of the formula The m is an integer of 1 to 6, and when the m is 2 or more, -O -R 2 may be the same or different.)
23. The organic solvent is recovered from the organic solution layer separated and discharged in the step (e) through distillation, 23. The method of claim 22, further comprising recycling the colored pigment containing ester functional groups. High-purity monomers are obtained by removing color-producing foreign matter from the monomers obtained by depolymerization of polymers. Purification methods for producing.
Citation Information
Patent Citations
Polyester resin for electrostatic charge image developing toner and method of manufacturing the same, electrostatic charge image developing toner and method of manufacturing the same, electrostatic charge image developer, image forming method, and image forming device
JP2009192856A
hair dyeing composition
JP2009523733A
recycling process
JP2017522444A
Depolymerization of polyethylene terephthalate
JP2018522107A
Recycling process
JP2020100842A