Mixed body of after-firing tetrafluoroethylene resin powder derived from suspension polymerization method and virgin material tetrafluoroethylene resin powder derived from suspension polymerization method, recycled tetrafluoroethylene resin fired body derived from suspension polymerization method, and method of recycling after-firing tetrafluoroethylene resin powder derived from suspension polymerization method
By mixing virgin and recycled fluororesin powders and applying a pressing and firing process, the method enhances the mechanical strength and appearance of recycled molded products, addressing the limitations of existing fluororesin recycling methods.
Patent Information
- Application Number
- JP2023071406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Existing fluororesin recycling methods face challenges in achieving high weight ratios of recycled fluororesin powder without compromising the appearance and mechanical strength of recycled molded products, particularly due to the poor fusion properties of waste fluororesin powder after firing.
A mixture of polytetrafluoroethylene resin powder derived from suspension polymerization after firing and tetrafluoroethylene resin powder from virgin material suspension polymerization is used, with the virgin powder covering the outer surface of the recycled powder to enhance mechanical strength and appearance, followed by a pressing and firing process.
This approach allows for the production of recycled molded products with good appearance and sufficient mechanical strength, even at higher weight ratios of recycled powder, effectively utilizing waste fluororesin materials and reducing disposal.
Smart Images

Figure 2024157202000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after firing and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method, a fired tetrafluoroethylene resin derived from a recycled suspension polymerization method, and a method for recycling tetrafluoroethylene resin powder derived from a suspension polymerization method after firing. [Background technology]
[0002] Processing waste generated during molding of sintered fluororesin and pulverized powder of sintered fluororesin obtained by pulverizing used sintered fluororesin have poor fusibility when melted and are difficult to reuse by thermal melting, so they are often used as part of the material for other products, and the amount reused as fluororesin has not been sufficient. In recent years, a fluororesin recycling method has been proposed in Patent Document 1 (JP Patent Publication 2015-108126 A) etc., in which sintered fluororesin powder is mixed with virgin fluororesin in a required weight ratio and then pressure molded. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-108126 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the fluororesin recycling method disclosed in Patent Document 1, the weight ratio of sintered fluororesin powder, which is the so-called used material, is 30% or less. This is because, in the recycling technology in Patent Document 1, when the ratio of sintered fluororesin powder (used material) used in the recycled molded product material is increased, the appearance and mechanical strength, represented by tensile strength, of the recycled molded product are significantly reduced. In recent years, in order to protect mineral resources that are used as fluororesin materials, reduce the amount of fluororesin products discarded, and increase the amount reused as fluororesin products (horizontal recycling) rather than as part of the material for other products, further improvement in the weight ratio of fluororesin powder in recycled molded products that ensures necessary and sufficient mechanical strength is expected. [Means for solving the problem]
[0005] The present invention has been made to solve the above problems, and has the following objects. That is, the first object is to provide a mixture of sintered suspension polymerization method-derived tetrafluoroethylene resin powder and virgin suspension polymerization method-derived tetrafluoroethylene resin powder, which can be produced by a practical molding method to produce a recycled molded product having good appearance and necessary and sufficient mechanical strength (tensile strength) even if the weight ratio of sintered suspension polymerization method-derived tetrafluoroethylene resin powder in a recycled molded product of sintered suspension polymerization method-derived tetrafluoroethylene resin is increased. The second object is to provide a sintered recycled suspension polymerization method-derived tetrafluoroethylene resin having good appearance and necessary and sufficient mechanical strength (tensile strength). The third object is to provide a method for recycling sintered suspension polymerization method-derived tetrafluoroethylene resin powder, which enables the effective use of sintered suspension polymerization method-derived tetrafluoroethylene resin powder.
[0006] As a result of intensive research by the inventors to solve the above problems, the inventors have come up with the following configuration: That is, the present invention is a mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after firing and tetrafluoroethylene resin powder derived from a virgin material suspension polymerization method, characterized in that the average particle size of the tetrafluoroethylene resin powder derived from the virgin material suspension polymerization method is larger than the average particle size of the tetrafluoroethylene resin powder derived from the suspension polymerization method after firing, and the tetrafluoroethylene resin powder derived from the virgin material suspension polymerization method is attached to an outer surface of the tetrafluoroethylene resin powder derived from the suspension polymerization method after firing.
[0007] This makes it possible to provide a mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after calcination and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method, which can produce a tetrafluoroethylene resin powder derived from a recycled suspension polymerization method that has a good appearance and necessary and sufficient mechanical strength (tensile strength) even if the weight ratio of tetrafluoroethylene resin powder derived from a suspension polymerization method after calcination is increased in the recycled suspension polymerization method-derived tetrafluoroethylene resin calcined body using tetrafluoroethylene resin derived from a suspension polymerization method after calcination.
[0008] There is also an invention relating to a sintered recycled suspension polymerization-derived tetrafluoroethylene resin product, which is obtained by sintering a press-molded product made from a mixture of the above-described sintered suspension polymerization-derived tetrafluoroethylene resin powder and virgin suspension polymerization-derived tetrafluoroethylene resin powder.
[0009] This makes it possible to provide a fired recycled suspension polymerization-derived tetrafluoroethylene resin product having a good appearance and necessary and sufficient mechanical strength (tensile strength).
[0010] Also, there is provided a method for recycling tetrafluoroethylene resin powder derived from a suspension polymerization method after sintering, the method comprising the steps of: a mixture production step of producing a mixture in which tetrafluoroethylene resin powder derived from a virgin suspension polymerization method is adhered to an outer surface of the tetrafluoroethylene resin powder derived from a suspension polymerization method after sintering, the tetrafluoroethylene resin powder being adjusted to a first predetermined average particle size and a virgin suspension polymerization method-derived tetrafluoroethylene resin powder being adjusted to a second predetermined average particle size that is equal to or larger than the first predetermined average particle size; a mixture injection step of pouring the mixture produced in the mixture production step into a molding die; a press step of clamping the molding die with a required clamping force to form a press-molded product; and a firing step of firing the press-molded product produced in the press step.
[0011] This makes it possible to provide a method for recycling tetrafluoroethylene resin powder derived from the suspension polymerization method after firing, which enables effective utilization of the tetrafluoroethylene resin powder derived from the suspension polymerization method after firing. Effect of the Invention
[0012] By adopting the configuration of the present invention, which comprises a mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after calcination and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method, a sintered tetrafluoroethylene resin body derived from a recycled suspension polymerization method, and a method for recycling tetrafluoroethylene resin powder derived from a suspension polymerization method after calcination, it becomes possible to produce a sintered tetrafluoroethylene resin body derived from a recycled suspension polymerization method that has a good appearance and necessary and sufficient mechanical strength (tensile strength), even if the weight ratio of tetrafluoroethylene resin powder derived from a suspension polymerization method after calcination in the sintered tetrafluoroethylene resin body derived from a recycled suspension polymerization method is increased. [Brief description of the drawings]
[0013] [Figure 1] 1 is a micrograph of recycled powder (polytetrafluoroethylene resin powder derived from a suspension polymerization method after firing) in the first embodiment. [Diagram 2]1 is a micrograph of virgin powder (virgin material suspension polymerization-derived tetrafluoroethylene resin powder) in the first embodiment. [Diagram 3] 1 is a micrograph of a mixture in the first embodiment (a mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after firing and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method). [Figure 4] 3 is a micrograph of the surface state of a sintered polytetrafluoroethylene resin produced by a recycled suspension polymerization method in the first embodiment. [Diagram 5] 1 is a micrograph of the surface state of a new sintered polytetrafluoroethylene resin produced by a suspension polymerization method and consisting only of virgin powder. [Figure 6] 13 is a micrograph of a mixture according to a second embodiment. [Figure 7] 11 is a micrograph of the surface state of a sintered polytetrafluoroethylene resin produced by a recycled suspension polymerization method in a second embodiment. [Figure 8] 1 is a table showing average tensile strengths of sintered polytetrafluoroethylene resins derived from a recycled suspension polymerization method in the first to fourth embodiments. [Figure 9] 13 is a micrograph of a mixture in the fifth embodiment. [Figure 10] 13 is a micrograph of a sintered polytetrafluoroethylene resin produced by a recycled suspension polymerization method according to the fifth embodiment. [Figure 11] 1 is a table showing average tensile strengths of sintered polytetrafluoroethylene resins derived from a recycled suspension polymerization method in the fifth to eighth embodiments. [Figure 12] 13 is a micrograph of a mixture in the sixth embodiment. [Figure 13] 13 is a micrograph of a sintered polytetrafluoroethylene resin produced by a recycled suspension polymerization method according to the sixth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the fired suspension polymerization-derived tetrafluoroethylene resin powder in this embodiment is a concept that includes all finely ground fired suspension polymerization-derived tetrafluoroethylene resin, such as processing chips generated when firing suspension polymerization-derived tetrafluoroethylene resin is subjected to cutting processing or the like, and ground powder obtained by cooling and grinding fired suspension polymerization-derived tetrafluoroethylene resin.
[0015] (First embodiment) In this embodiment, a method for recycling tetrafluoroethylene resin powder derived from a suspension polymerization method after firing using tetrafluoroethylene resin powder derived from a suspension polymerization method after firing, the first predetermined average particle size of which is adjusted to 40 μm, and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method, the second predetermined average particle size of which is larger than the first predetermined average particle size, adjusted to 50 μm, will be described. Hereinafter, in this specification, the tetrafluoroethylene resin powder derived from a suspension polymerization method after firing is referred to as "recycled powder", and the tetrafluoroethylene resin powder derived from a virgin suspension polymerization method is referred to as "virgin powder". Note that the raw materials of the recycled powder 10 and the virgin powder 20 in this embodiment are both Polyflon PTFE M-18 (manufactured by Daikin Industries, Ltd.), but the raw materials of the tetrafluoroethylene resin powder derived from a suspension polymerization method after firing and the tetrafluoroethylene resin powder derived from a virgin suspension polymerization method in the present invention are not limited to Polyflon PTFE M-18.
[0016] FIG. 1 is a micrograph of the recycled powder in this embodiment. FIG. 1A is a micrograph at a magnification of 100 times, and FIG. 1B is a micrograph at a magnification of 500 times. As is clear from FIG. 1, the grain size of the recycled powder 10 varies little, and the surface is dominated by smooth surfaces. FIG. 2 is a micrograph of the virgin powder in this embodiment. FIG. 2A is a micrograph at a magnification of 100 times, and FIG. 2B is a micrograph at a magnification of 500 times. As is clear from FIG. 2, the grain size of the virgin powder 20 varies more than the grain size of the recycled powder 10, and the surface is dominated by fluffy portions.
[0017] By mechanically mixing the recycled powder 10 shown in FIG. 1 and the virgin powder 20 shown in FIG. 2 with a stirring device not shown, a mixture 30 of the recycled powder 10 and the virgin powder 20 (a mixture of tetrafluoroethylene resin powder derived from suspension polymerization after firing and tetrafluoroethylene resin powder derived from virgin suspension polymerization) is obtained (mixture generation process). In this embodiment, the mixture 30 was obtained by mechanically mixing the recycled powder:virgin powder in a mass ratio of 10:90. FIG. 3 is a micrograph of the mixture in this embodiment. FIG. 3A is a micrograph at a magnification of 100 times, and FIG. 3B is a micrograph at a magnification of 500 times.
[0018] In the present embodiment, the mixture 30 is in a state where the virgin powder 20 is attached so as to cover the outer surface of the recycled powder 10. The recycled powder 10 is a fine powder obtained by sintering the virgin powder 20. Therefore, the recycled powder 10 is harder than the virgin powder 20, and by mixing the recycled powder 10 and the virgin powder 20 with a stirring device, the recycled powder 10 penetrates the soft virgin powder 20 before sintering. It is presumed that the recycled powder 10 that penetrates the virgin powder 20 maintains the adhesion state between the two due to the adhesiveness of the virgin powder 20. In the present embodiment, the mixture 30 has a high ratio of virgin powder 20, so most of the outer surface of the mixture 30 is exposed to the virgin powder 20.
[0019] As shown in FIG. 3, the mixture 30 in which the outer surface of the recycled powder 10 is covered with the virgin powder 20 is put into a molding die (not shown) (mixture putting step). Next, the molding die is clamped with the same clamping force (30 MPa) as when molding only the virgin powder to generate a press-molded product (not shown) (pressing step). The press-molded product in this embodiment is a cylindrical body with a diameter of 100 mm and a height of 100 mm. This press-molded product is fired at a temperature equal to or higher than the melting temperature of the virgin powder 20 (here, 370 degrees Celsius) (firing step), thereby obtaining a fired tetrafluoroethylene resin 40 derived from the recycling suspension polymerization method. FIG. 4 is a micrograph of the surface state of the fired tetrafluoroethylene resin 40 derived from the recycling suspension polymerization method in this embodiment. FIG. 4A is a micrograph at a magnification of 100 times, and FIG. 4B is a micrograph at a magnification of 500 times. Fig. 5 is a micrograph of the surface state of new suspension polymerization-derived tetrafluoroethylene resin sintered body 42 consisting only of virgin powder 20. The manufacturing method of new suspension polymerization-derived tetrafluoroethylene resin sintered body 42 is the same as the manufacturing method of recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40. Fig. 5A is a micrograph at a magnification of 100 times, and Fig. 5B is a micrograph at a magnification of 500 times.
[0020] Comparing FIG. 4 and FIG. 5, the surface state of the new suspension polymerization-derived tetrafluoroethylene resin sintered body 42 shown in FIG. 5 is more uniform than the surface state of the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 shown in FIG. 4. The recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 is slightly darker in color than the new suspension polymerization-derived tetrafluoroethylene resin sintered body 42. Furthermore, the surface state of the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 has more irregularities than the surface state of the new suspension polymerization-derived tetrafluoroethylene resin sintered body 42. When the tactile feel of the surfaces of both was confirmed by a sensory test, almost no difference in feel was felt between the two. The following are considered to be the causes of the above-mentioned difference in appearance. That is, it is considered that the virgin powder 20 adheres to the mixture 30 before sintering of the sintered polytetrafluoroethylene resin 40 derived from the recycled suspension polymerization method so as to cover the outer surface of the recycled powder 10, and adjacent virgin powders 20 are melted and integrated with each other while the recycled powder 10 is trapped inside.
[0021] Three test pieces (not shown) were cut out from the recycled suspension polymerization-derived sintered tetrafluoroethylene resin 40 obtained in this embodiment, and a tensile test (test method: JIS K 7137-2) was conducted, revealing that the average tensile strength of the three test pieces was 36.4 MPa. This tensile strength corresponds to 91.0% of the average tensile strength of 40 MPa of the new suspension polymerization-derived sintered tetrafluoroethylene resin 42 produced under the same conditions, and it was confirmed that the test pieces have a tensile strength (mechanical strength) sufficient for practical use.
[0022] Second embodiment In this embodiment, the mixture ratio of the recycled powder 10 and the virgin powder 20 used in the first embodiment is 40:60, and a sintered polytetrafluoroethylene resin 40 derived from the recycled suspension polymerization method is obtained in the same manner as in the first embodiment. In this embodiment, the mass ratio of the recycled powder:virgin powder is 40:60, and the mixture 30 is obtained by mechanically mixing them with a stirring device to obtain a mixture 30. FIG. 6 is a micrograph of the mixture 30 in this embodiment. FIG. 6A is a micrograph at a magnification of 100 times, and FIG. 6B is a micrograph at a magnification of 500 times. In the mixture 30 in this embodiment, the amount of virgin powder 20 attached to the recycled powder 10 per grain is reduced compared to the mixture 30 in the first embodiment, but a plurality of virgin powders 20 are attached to the outer surface of the recycled powder 10.
[0023] Fig. 7 is a micrograph showing the surface state of a sintered tetrafluoroethylene resin derived from a recycled suspension polymerization method, obtained by carrying out a method for recycling a suspension polymerization-derived tetrafluoroethylene resin powder after sintering the mixture in this embodiment shown in Fig. 6 under the same procedure and conditions as in the first embodiment. Fig. 7A is a micrograph at a magnification of 100 times, and Fig. 7B is a micrograph at a magnification of 500 times. Comparing Fig. 7 with Fig. 4, it can be said that the surface state of the sintered tetrafluoroethylene resin derived from a recycled suspension polymerization method 40 in this embodiment is comparable to the surface state of the sintered tetrafluoroethylene resin derived from a recycled suspension polymerization method 40 in the first embodiment.
[0024] As with the first embodiment, three test pieces were cut out from the recycled suspension polymerization-derived sintered tetrafluoroethylene resin 40 obtained in the second embodiment, and a tensile test was performed under the same conditions as in the first embodiment, resulting in an average tensile strength of 27.8 MPa for the three test pieces (see FIG. 8). This was 76.4% of the average tensile strength of the test pieces in the first embodiment, and 69.5% of the average tensile strength of the new suspension polymerization-derived sintered tetrafluoroethylene resin 42 produced under the same conditions.
[0025] Third embodiment In this embodiment, the mass ratio of recycled powder to virgin powder is set to 20:80, and a mixture 30 obtained under the same procedure and under the same conditions as in the first and second embodiments is used. The mixture 30 in this embodiment is sintered to obtain a sintered product 40 of tetrafluoroethylene resin derived from a recycled suspension polymerization method. A tensile test was performed under the same conditions as in the first and second embodiments using the sintered product 40 of tetrafluoroethylene resin derived from a recycled suspension polymerization method obtained in this embodiment, and the average tensile strength was 34.3 MPa (see FIG. 8). This was 94.2% of the average tensile strength of the test piece in the first embodiment, and 85.8% of the average tensile strength of a new sintered product 42 of tetrafluoroethylene resin derived from a suspension polymerization method produced under the same conditions.
[0026] (Fourth embodiment) In this embodiment, the mass ratio of recycled powder to virgin powder is set to 30:70, and a mixture 30 obtained under the same procedure and under the same conditions as in the first to third embodiments is used. The mixture 30 in this embodiment is sintered to obtain a sintered product 40 of tetrafluoroethylene resin derived from a recycled suspension polymerization method. A tensile test was performed under the same conditions as in the first to third embodiments using the sintered product 40 of tetrafluoroethylene resin derived from a recycled suspension polymerization method obtained in this embodiment, and the average tensile strength was 31.5 MPa (see FIG. 8). This was 86.5% of the average tensile strength of the test piece in the first embodiment, and 78.8% of the average tensile strength of a new sintered product 42 of tetrafluoroethylene resin derived from a suspension polymerization method produced under the same conditions.
[0027] The applicant confirmed that there was no significant difference in the surface state or color of the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method obtained in the first to fourth embodiments. However, as shown in FIG. 8, as the mixing ratio of the recycled powder 10 increases, the decrease rate of the average tensile strength of the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method gradually increases. However, the average tensile strength of the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method with a mixing ratio of the recycled powder 10 of 40% is significantly greater than half (69.5%) of the tensile strength of the new sintered tetrafluoroethylene resin 42 derived from the suspension polymerization method, and it can be said that the sintered fluororesin has sufficient strength in the practical range of the sintered fluororesin. In this way, it was found that the mixture 30 in which the recycled powder 10 and the virgin powder 20 adjusted to an average particle size larger than the average particle size of the recycled powder 10 are mixed and the virgin powder 20 is attached to the outer surface of the recycled powder 10 can effectively utilize the recycled powder 10. The fired polytetrafluoroethylene resin body 40 produced by the recycling suspension polymerization method and molded using the mixture 30 in the first to fourth embodiments can contribute to the effective use of the recycled powder 10.
[0028] Fifth embodiment In this embodiment, the average particle size of the recycled powder 10 in the first embodiment is 25 μm, and the conditions other than the average particle size of the recycled powder 10 are the same as those in the first embodiment. FIG. 9 shows a micrograph of the mixture 30 in this embodiment. FIG. 9A is a micrograph at a magnification of 100 times, and FIG. 9B is a micrograph at a magnification of 500 times. As is clear from FIG. 9, the outer surface of the recycled powder 10 is covered with the virgin powder 20. Since the ratio of the virgin powder 20 is high, the virgin powder 20 is adjacent to each other. FIG. 10 shows a micrograph of a sintered polytetrafluoroethylene resin 40 derived from a recycled suspension polymerization method produced by the same procedure and conditions as the first embodiment using the mixture 30 in this embodiment. FIG. 10A is a micrograph at a magnification of 100 times, and FIG. 10B is a micrograph at a magnification of 500 times.
[0029] As is clear from FIG. 10, the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 in this embodiment has a better surface condition and color than the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 in the first embodiment, and is close to the surface condition and color of the new suspension polymerization-derived tetrafluoroethylene resin sintered body 42 manufactured only from the virgin powder 20. Three test pieces were cut out from the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 in this embodiment in the same manner as in the first embodiment, and a tensile test was performed in the same manner as in the first embodiment. As a result, the average tensile strength of the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 in this embodiment was 32.2 MPa (see FIG. 11), which was 80.5% of the tensile strength of the new suspension polymerization-derived tetrafluoroethylene resin sintered body 42. From this result, it can be said that the recycled suspension polymerization-derived tetrafluoroethylene resin sintered body 40 in the embodiment has a tensile strength sufficient for practical use, and is suitable for use in places where both strength and appearance are highly required.
[0030] Sixth embodiment In this embodiment, the average particle size of the recycled powder 10 in the second embodiment is 25 μm, and the conditions other than the average particle size of the recycled powder 10 are the same as those in the second embodiment. FIG. 12 shows a micrograph of the mixture 30 in this embodiment. FIG. 12A is a micrograph at a magnification of 100 times, and FIG. 12B is a micrograph at a magnification of 500 times. In the mixture 30 in this embodiment, the amount of virgin powder 20 attached to the recycled powder 10 per grain is reduced compared to the mixture 30 in the fifth embodiment, but multiple virgin powders 20 are attached to the outer surface of the recycled powder 10.
[0031] Fig. 13 shows a micrograph of a sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method, which was produced using the mixture 30 of this embodiment under the same procedure and conditions as those of the fifth embodiment. Fig. 13A is a micrograph at a magnification of 100 times, and Fig. 13B is a micrograph at a magnification of 500 times. It can be said that the surface state of the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method of this embodiment has a more uniform texture and is more homogeneous than the surface state of the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method of the second embodiment. Three test pieces were cut out from the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method of this embodiment, and a tensile test was performed under the same conditions as those of the fifth embodiment. As a result, the average tensile strength was 23.0 MPa (see Figure 11), which was 71.4% of the tensile strength of the recycled suspension polymerization method-derived tetrafluoroethylene resin sintered body 40 in the fifth embodiment and 57.5% of the tensile strength of the new suspension polymerization method-derived tetrafluoroethylene resin sintered body 42.
[0032] Seventh embodiment In this embodiment, the average particle size of the recycled powder 10 in the third embodiment is 25 μm, and the conditions other than the average particle size of the recycled powder 10 are the same as those in the third embodiment. A sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method was manufactured using the mixture 30 in this embodiment under the same procedure and conditions as those in the third embodiment. Three test pieces were cut out from the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method in this embodiment, and a tensile test was performed under the same conditions as those in the fifth and sixth embodiments. As a result, the average tensile strength was 29.3 MPa (see FIG. 11), which was 91.0% of the tensile strength of the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method in the fifth embodiment, and 73.3% of the tensile strength of the sintered tetrafluoroethylene resin 42 derived from a new suspension polymerization method.
[0033] Eighth embodiment In this embodiment, the average particle size of the recycled powder 10 in the fourth embodiment is 25 μm, and the conditions other than the average particle size of the recycled powder 10 are the same as those in the fourth embodiment. A sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method was manufactured using the mixture 30 in this embodiment under the same procedure and conditions as those in the fourth embodiment. Three test pieces were cut out from the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method in this embodiment, and a tensile test was performed under the same conditions as those in the fifth to seventh embodiments. As a result, the average tensile strength was 26.3 MPa (see FIG. 11), which was 81.7% of the tensile strength of the sintered tetrafluoroethylene resin 40 derived from a recycled suspension polymerization method in the fifth embodiment, and 65.8% of the tensile strength of the sintered tetrafluoroethylene resin 42 derived from a new suspension polymerization method.
[0034] The applicant confirmed that there is no significant difference in surface condition and color between the sintered tetrafluoroethylene resin bodies 40 derived from the recycled suspension polymerization method obtained in the fifth to eighth embodiments, but all of them have better surface condition and color than the sintered tetrafluoroethylene resin bodies 40 derived from the recycled suspension polymerization method obtained in the first to fourth embodiments (closer to the condition of the new sintered tetrafluoroethylene resin body 42 derived from the suspension polymerization method sintered only with the virgin powder 20). Also, as shown in Fig. 11, it can be said that the decrease rate of the average tensile strength of the sintered tetrafluoroethylene resin bodies 40 derived from the recycled suspension polymerization method gradually increases as the mixing ratio of the recycled powder 10 increases.
[0035] The tensile strength of the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method obtained in the above-mentioned first to eighth embodiments is higher in the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method using the recycled powder 10 having a larger average particle size when the mixing ratio of the recycled powder 10 is the same. This is presumed to be because, when the recycled powder 10 acts as a filler (aggregate) for the virgin powder 20, the particle size of the recycled powder 10 as a filler (aggregate) is preferably to a certain extent larger than the average particle size of the virgin powder 20. In addition, the appearance state of the sintered tetrafluoroethylene resin 40 derived from the recycled suspension polymerization method obtained in the above-mentioned first to eighth embodiments is better when the average particle size of the recycled powder 10 is smaller than the average particle size of the virgin powder 20 when the mixing ratio of the recycled powder 10 is the same. This is presumed to be because the finer the recycled powder 10, the more reliably it can be sintered in a state of being covered by the virgin powder 20. From these findings, it was found that in places where tensile strength (mechanical strength) is important, it is preferable to increase the average particle size of the recycled powder 10, and in places where appearance is important, it is preferable to decrease the average particle size of the recycled powder 10.
[0036] As described above, by adopting the mixture 30 of the tetrafluoroethylene resin powder (recycled powder 10) derived from the suspension polymerization method after firing and the tetrafluoroethylene resin powder (virgin powder 20) derived from the virgin suspension polymerization method according to the present invention, the tetrafluoroethylene resin powder derived from the suspension polymerization method after firing, which was difficult to recycle in the past, can be reused, the amount of tetrafluoroethylene resin powder derived from the suspension polymerization method after firing discarded can be significantly reduced, and it is possible to protect mineral resources and reduce disposal costs. In addition, the weight ratio of the recycled powder 10 in the mixture 30 and the tetrafluoroethylene resin powder derived from the suspension polymerization method after firing can be increased to 40%, and the usage rate (recycle rate) of the recycled powder 10 can be increased.
[0037] In the above embodiment, the average particle size (second predetermined average particle size) of the virgin suspension polymerization-derived tetrafluoroethylene resin powder (virgin powder 20) is larger than the average particle size (first predetermined average particle size) of the sintered suspension polymerization-derived tetrafluoroethylene resin powder (recycled powder 10), but the present invention is not limited to this embodiment. As a result of simple experiments conducted by the applicant, it has been confirmed that even if the average particle size (second predetermined average particle size) of the virgin suspension polymerization-derived tetrafluoroethylene resin powder is the same as the average particle size (first predetermined average particle size) of the sintered suspension polymerization-derived tetrafluoroethylene resin powder, there is a tendency similar to that of the first to fourth embodiments and the fifth to eighth embodiments.
[0038] It is also possible to adopt a configuration in which various modified examples of the embodiment described above are appropriately combined. [Explanation of symbols]
[0039] 10: Recycled powder (polytetrafluoroethylene resin powder derived from suspension polymerization method after firing) 20: Virgin powder (virgin polytetrafluoroethylene resin powder derived from suspension polymerization method) 30: Mixture (mixture of tetrafluoroethylene resin powder derived from suspension polymerization method after baking and virgin tetrafluoroethylene resin powder derived from suspension polymerization method) 40: Recycled polytetrafluoroethylene resin fired body derived from suspension polymerization method 42: New tetrafluoroethylene resin fired body derived from suspension polymerization method
Claims
1. The present invention includes a tetrafluoroethylene resin powder derived from a suspension polymerization method after baking and a virgin suspension polymerization method-derived tetrafluoroethylene resin powder, The average particle size of the virgin suspension polymerization-derived tetrafluoroethylene resin powder is equal to or larger than the average particle size of the fired suspension polymerization-derived tetrafluoroethylene resin powder, A mixture of tetrafluoroethylene resin powder derived from a suspension polymerization method after baking and tetrafluoroethylene resin powder derived from a virgin suspension polymerization method, characterized in that the tetrafluoroethylene resin powder derived from a suspension polymerization method after baking is adhered to the outer surface of the tetrafluoroethylene resin powder derived from a suspension polymerization method after baking.
2. A sintered recycled suspension polymerization-derived tetrafluoroethylene resin product, characterized in that it is obtained by sintering a press-molded product made from a mixture of the sintered suspension polymerization-derived tetrafluoroethylene resin powder according to claim 1 and virgin suspension polymerization-derived tetrafluoroethylene resin powder.
3. a mixture producing step of producing a mixture by using a sintered suspension polymerization method-derived tetrafluoroethylene resin powder adjusted to a first predetermined average particle size and a virgin material suspension polymerization method-derived tetrafluoroethylene resin powder adjusted to a second predetermined average particle size, the second predetermined average particle size being equal to or larger than the first predetermined average particle size, and by adhering the virgin material suspension polymerization method-derived tetrafluoroethylene resin powder to an outer surface of the sintered suspension polymerization method-derived tetrafluoroethylene resin powder; a mixture injection step of injecting the mixture produced in the mixture production step into a molding die; a pressing process in which the molding die is clamped with a required clamping force to form a press-molded product; a calcination step of calcining the press-molded product formed by the pressing step.
Citation Information
Patent Citations
Method for recycling fluororesin
JP2015108126A
Method for producing fluororesin composition, fluororesin composition, and molded body
JP2022159204A
Method for manufacturing fired body of fluororesin, fired body of fluororesin, method for manufacturing fluororesin dispersion, method for manufacturing fired body, fluororesin dispersion, and fired body