Processing method

A non-polymerized resin protective film on wafers, combined with a hardening liquid resin, prevents peeling during dicing and grinding, maintaining film integrity throughout the process.

JP2024157321APending Publication Date: 2024-11-07DISCO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023071618
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The protective film used during wafer dicing tends to peel off during processing due to cutting or laser beam irradiation, necessitating improvements to prevent this peeling.

Method used

A processing method involving the formation of a protective film made of non-polymerized resin on the workpiece surface, followed by a dicing step along planned lines, application of a hardening liquid resin, and subsequent curing, with the film and cured resin being removed together after processing.

Benefits of technology

The method effectively suppresses peeling of the protective film during processing by ensuring it remains intact throughout the cutting and grinding stages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157321000001_ABST
    Figure 2024157321000001_ABST
Patent Text Reader

Abstract

To provide a processing method capable of suppressing peeling of a protective film due to processing.SOLUTION: A processing method is a processing method for a workpiece having a set planned processing line, and includes a protective film forming step 101 of forming a protective film made of a non-polymerized resin on the surface of the workpiece, a dicing step 102 of dicing the workpiece together with the protective film along the planned processing line after the protective film is formed, a liquid resin supplying step 103 of supplying a liquid resin that hardens when subjected to an external stimulus onto the protective film, and then applying an external stimulus to the liquid resin to harden the liquid resin and fixing it to the protective film after the dicing step 102, and a removal step 105 of removing the protective film from the surface of the workpiece together with the hardened liquid resin after the liquid resin supplying step 103.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for machining a workpiece. [Background technology]

[0002] When dicing a wafer, the surface of the wafer is covered with a resin for protection (see, for example, Patent Document 1).

[0003] In addition, after forming a resin layer on the surface of a wafer, a laser beam is irradiated onto the resin layer to form openings along the intended processing lines, thereby forming a mask for plasma dicing (see, for example, Patent Documents 2 and 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-062958 A [Patent Document 2] JP 2021-100074 A [Patent Document 3] JP 2006-140311 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, processes such as dicing using a cutting blade or laser beam, or irradiation with a laser beam can cause the protective film to peel off significantly from the interface with the wafer surface, so improvements were desperately needed.

[0006] An object of the present invention is to provide a processing method capable of suppressing peeling of a protective film due to processing. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems and achieve the objective, the processing method of the present invention is a method for processing a workpiece having a planned processing line set, and is characterized by comprising a protective film forming step of forming a protective film made of a non-polymerized resin on the surface of the workpiece, and a dicing step of dicing the workpiece together with the protective film along the planned processing line after the protective film is formed.

[0008] The processing method may further include a liquid resin supplying step in which, after the dicing step, a liquid resin that hardens when subjected to an external stimulus is supplied onto the protective film, and then the external stimulus is applied to the liquid resin to harden the liquid resin and fix the liquid resin to the protective film, and a removal step in which, after the liquid resin supplying step, the protective film is removed from the surface of the workpiece together with the hardened liquid resin.

[0009] In the processing method, a plurality of intersecting processing lines are set on the workpiece, and in the dicing step, grooves are formed in the workpiece along the plurality of processing lines and uncut portions of the workpiece are formed below the grooves. After the liquid resin supplying step and before the removing step, the workpiece may be held on a holding table via the protective film to expose the back surface of the workpiece, and the exposed back surface is ground to thin the workpiece to a thickness reaching the grooves, thereby dividing the workpiece.

[0010] In the above processing method, in the liquid resin supplying step, a film may be disposed on the liquid resin, and the liquid resin may be fixed to the protective film and the film may be fixed to the liquid resin. Effect of the Invention

[0011] The present invention has an effect of suppressing peeling of the protective film due to processing. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a perspective view showing an example of a workpiece to be processed by the processing method according to the first embodiment. [Diagram 2]FIG. 2 is a flowchart showing the flow of the processing method according to the first embodiment. [Diagram 3] FIG. 3 is a perspective view that typically shows a state in which a tape is attached to the back surface of a workpiece and a frame is attached to the outer edge of the tape in the protective film forming step of the processing method shown in FIG. [Figure 4] FIG. 4 is a side view, partially in section, that typically illustrates a state in which a protective film agent is applied to the entire surface of a workpiece in the protective film forming step of the processing method illustrated in FIG. [Diagram 5] FIG. 5 is a perspective view showing a workpiece having a protective film formed on its surface in the protective film forming step of the processing method shown in FIG. [Figure 6] FIG. 6 is a side view, partially in section, typically showing the dicing step of the processing method shown in FIG. [Figure 7] FIG. 7 is a cross-sectional view showing a schematic view of a main part of the workpiece after the dicing step of the processing method shown in FIG. [Figure 8] FIG. 8 is a cross-sectional view that typically illustrates a state in which liquid resin is supplied onto a protective film in the liquid resin supplying step of the processing method illustrated in FIG. [Figure 9] FIG. 9 is a cross-sectional view that typically shows a main part of the workpiece after liquid resin has been supplied onto the protective film in the liquid resin supplying step of the processing method shown in FIG. [Figure 10] FIG. 10 is a cross-sectional view that typically illustrates a state in which the liquid resin illustrated in FIG. 9 is cured. [Figure 11] FIG. 11 is a side view, partially in section, typically showing the dividing step of the processing method shown in FIG. [Figure 12] FIG. 12 is a cross-sectional view that typically shows the workpiece after the dividing step of the machining method shown in FIG. [Figure 13] FIG. 13 is a cross-sectional view that illustrates a removal step of the processing method illustrated in FIG. [Figure 14] FIG. 14 is a cross-sectional view partially illustrating a schematic view of a state in which an opening exposing a line to be processed is formed in a protective film in a dicing step of a processing method according to the second embodiment. [Figure 15] FIG. 15 is a cross-sectional view that illustrates a schematic configuration example of an etching apparatus that forms grooves in a workpiece in a dicing step of the processing method according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.

[0014] [Embodiment 1] A processing method according to a first embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view showing an example of a workpiece to be processed by the processing method according to the first embodiment. Fig. 2 is a flowchart showing the flow of the processing method according to the first embodiment.

[0015] (Work) The processing method according to the first embodiment is a method for processing a workpiece 1 shown in Fig. 1. In the first embodiment, the workpiece 1 is a wafer such as a disk-shaped semiconductor wafer or an optical device wafer, with a substrate 2 made of silicon, sapphire, gallium, or the like. As shown in Fig. 1, the workpiece 1 has a plurality of processing lines 5 that intersect with each other set on a surface 4, and devices 6 are formed in areas partitioned by the processing lines 5.

[0016] The device 6 is, for example, an integrated circuit such as an IC (Integrated Circuit) or an LSI (Large Scale Integration), an image sensor such as a CCD (Charge Coupled Device) or a CMOS (Complementary Metal Oxide Semiconductor), or a memory (semiconductor memory device).

[0017] In the present invention, the workpiece 1 may be something other than a disk-shaped wafer, and the device 6 may not be formed on the surface 4.

[0018] (Processing method) The processing method according to the first embodiment is a method for dividing the workpiece 1 into individual chips 10 along a planned processing line 5. The chips 10 include a part of the substrate 2 and a device 6 on the substrate 2. As shown in FIG. 2, the processing method according to the first embodiment includes a protective film forming step 101, a dicing step 102, a liquid resin supplying step 103, a dividing step 104, and a removing step 105.

[0019] (Protective film formation step) Fig. 3 is a perspective view showing a state where a tape is applied to the back surface of a workpiece and a frame is applied to the outer edge of the tape in the protective film forming step of the processing method shown in Fig. 2. Fig. 4 is a side view showing a state where a protective film agent is applied to the entire surface of a workpiece in the protective film forming step of the processing method shown in Fig. 2, partially in cross section. Fig. 5 is a perspective view showing a workpiece having a protective film formed on its surface in the protective film forming step of the processing method shown in Fig. 2.

[0020] The protective film forming step 101 is a step of covering the entire surface 4 of the workpiece 1 with a non-polymerized resin to form a protective film 12 made of a non-polymerized resin on the entire surface 4 of the workpiece 1. In the first embodiment, in the protective film forming step 101, first, as shown in Fig. 3, a central portion of a disk-shaped tape 8 having a larger diameter than the workpiece 1 is attached to the back surface 7 of the workpiece 1, and an annular frame 9 having an inner diameter larger than the outer diameter of the workpiece 1 is attached to the outer edge of the tape 8.

[0021] In addition, in embodiment 1, tape 8 is an adhesive tape having a base material made of a non-adhesive and flexible resin and an adhesive layer laminated on the base material and made of an adhesive and flexible resin, with the adhesive layer being attached to the workpiece 1 and frame 9, or a sheet consisting only of a base material without an adhesive layer, made of a thermoplastic resin, and heat-pressed to the workpiece 1 and frame 9.

[0022] In the first embodiment, in the protective film forming step 101, the protective film coating device 20 shown in FIG. 4 places the back surface 7 of the workpiece 1 on the holding surface 22 of the spinner table 21 via the tape 8, and holds the back surface 7 of the workpiece 1 on the holding surface 22 by suction via the tape 8, and clamps the frame 9 with the clamp unit 23 provided around the spinner table 21. In the first embodiment, in the protective film forming step 101, the protective film coating device 20 applies a liquid protective film agent 11 to the center of the front surface 4 of the workpiece 1 from the application nozzle 24 above the workpiece 1 while rotating the spinner table 21 around its axis, as shown in FIG. 4. Then, the protective film agent 11 applied to the front surface 4 of the workpiece 1 is spread to the outer edge side of the workpiece 1 by the centrifugal force generated by the rotation of the spinner table 21, and covers the entire front surface 4 of the workpiece 1.

[0023] Thus, in the first embodiment, in the protective film forming step 101, the protective film agent 11 is supplied to and applied to the workpiece 1 held on the spinner table 21 rotating about its axis, that is, applied by so-called spin coating. In the first embodiment, in the protective film forming step 101, the protective film agent 11 is dried to form a protective film 12 that covers the entire surface 4 of the workpiece 1, as shown in FIG.

[0024] In the first embodiment, the protective film agent 11 is composed of a non-polymerized resin and a solvent that dissolves the non-polymerized resin. The non-polymerized resin is composed of a single resin that is non-polymerized (i.e., molecules are not bonded to each other), such as a terpene resin or a rosin resin. The solvent is added to adjust the viscosity of the protective film agent 11 and to give the protective film agent 11 a viscosity that allows it to be applied.

[0025] In the first embodiment, the protective film agent 11 is made of a terpene resin as a non-polymerized resin and propylene glycol monomethyl ether acetate (PGMEA) as a solvent. The protective film 12 formed on the entire surface 4 of the workpiece 1 by drying the protective film agent 11 is formed to a uniform thickness.

[0026] In the present invention, in the protective film forming step 101, after the protective film 12 is formed on the front surface 4 of the workpiece 1, the center of the tape 8 may be adhered to the back surface 7 of the workpiece 1, and the frame 9 may be adhered to the outer edge of the tape 8.

[0027] (Dicing step) Fig. 6 is a side view, partially in cross section, showing a dicing step of the processing method shown in Fig. 2. Fig. 7 is a cross-sectional view showing a main part of the workpiece after the dicing step of the processing method shown in Fig. 2. The dicing step 102 is a step of dicing the workpiece 1 together with the protective film 12 along the intended processing line 5 after the protective film 12 is formed.

[0028] 6, in the dicing step 102, the cutting device 30 suction-holds the back surface 7 of the work 1 on the holding surface 32 of the holding table 31 via tape 8, and clamps the frame 9 with clamps 33 provided around the holding table 31. In the dicing step 102, in the embodiment 1, the cutting device 30 captures an image of the front surface 4 of the work 1 with an imaging unit (not shown) to detect the to-be-processed line 5, and performs alignment to align the work 1 with the cutting blade 35 of the cutting unit 34.

[0029] In the first embodiment, in the dicing step 102, the cutting device 30 cuts the cutting blade 35 into the planned processing line 5 up to the center in the thickness direction of the workpiece 1 while relatively moving the workpiece 1 and the cutting blade 35 rotated about the axis by the spindle along the planned processing line 5, thereby forming a groove 13 having a depth that does not reach the back surface 7 side of the workpiece 1. In the first embodiment, in the dicing step 102, the cutting blade 35 cuts into all the planned processing lines 5 of the workpiece 1 to form the grooves 13.

[0030] Thus, in the first embodiment, in the dicing step 102, grooves 13 are formed in the workpiece 1 along the multiple planned processing lines 5, and uncut portions 14 of the workpiece 1 are formed below the grooves 13, as shown in Fig. 7. Note that in the first embodiment, in the dicing step 102, a cutting blade 35 having a flat outer edge along the axis is cut into the planned processing lines 5 to form grooves 13 with flat bottoms in the planned processing lines 5.

[0031] (Liquid resin supply step) Fig. 8 is a cross-sectional view showing a state where liquid resin is supplied onto a protective film in a liquid resin supplying step of the processing method shown in Fig. 2. Fig. 9 is a cross-sectional view showing a main part of a workpiece after liquid resin is supplied onto a protective film in a liquid resin supplying step of the processing method shown in Fig. 2. Fig. 10 is a cross-sectional view showing a state where the liquid resin shown in Fig. 9 is hardened.

[0032] In the liquid resin supplying step 103, which is performed after the dicing step 102, liquid resin 15 that is hardened by an external stimulus is supplied onto the protective film 12, and then an external stimulus is applied to the liquid resin 15 to harden the liquid resin 15 and fix the liquid resin 15 to the protective film 12. In the liquid resin supplying step 103 in the first embodiment, as shown in FIG. 8, a resin supplying device 40 places a film 16 on an upper surface 42 of a support table 41 made of flat glass, and supplies liquid resin 15 onto the film 16.

[0033] In the first embodiment, the film 16 is made of a resin such as PET (Polyethylene terephthalate) resin, and is formed into a disk shape having a larger diameter than the workpiece 1. The liquid resin 15 is made of a resin that is liquid before an external stimulus is applied and hardens when the external stimulus is applied. In the first embodiment, the liquid resin 15 hardens when irradiated with ultraviolet light 17 (shown in FIG. 10), which is an external stimulus, but in the present invention, the liquid resin 15 may harden when heated, which is an external stimulus.

[0034] In the first embodiment, in the liquid resin supply step 103, as shown in FIG. 8, the tape 8 is peeled off from the back surface 7 of the workpiece 1, and the back surface 7 of the workpiece 1 is suction-held on the holding surface 46 of the suction table 45, which is sucked by the suction source 44 via the opening and closing valve 43. In the first embodiment, in the liquid resin supply step 103, the front surface 4 of the workpiece 1 suction-held on the holding surface 46 of the suction table 45 is made to face the upper surface 42 of the support table 41, and then the suction table 45 is brought close to the upper surface 42 of the support table 41, and the liquid resin 15 on the film 16 is spread on the front surface 4 side of the workpiece 1, and the liquid resin 15 is applied between the protective films 12 and the grooves 13 are filled with the liquid resin 15, as shown in FIG. 9. Since the protective film 12 is made of a non-polymerized resin and the molecules are not bonded to each other, the liquid resin 15 permeates the protective film 12 as shown by the arrow in FIG. 9.

[0035] 10, in the liquid resin supplying step 103, ultraviolet rays 17 are irradiated from an ultraviolet irradiating means 18 from below the support table 41 through the support table 41 onto the liquid resin 15 to harden the liquid resin 15 applied to the front surface 4 side of the workpiece 1, fixing the liquid resin 15 to the protective film 12, and bonding the hardened liquid resin 15 to the film 16. Thus, in the liquid resin supplying step 103 in the first embodiment, the film 16 is disposed on the liquid resin 15, and the liquid resin 15 is fixed to the protective film 12 and the film 16 is fixed to the liquid resin 15.

[0036] (split step) Fig. 11 is a side view, partially in cross section, that typically shows the division step of the processing method shown in Fig. 2. Fig. 12 is a cross-sectional view that typically shows the workpiece after the division step of the processing method shown in Fig. 2. The division step 104 is a step in which, after the liquid resin supply step 103 and before the removal step 105, the workpiece 1 is held by the holding table 61 via the protective film 12, the back surface 7 of the workpiece 1 is exposed, and the exposed back surface 7 is ground to thin the workpiece 1 to a thickness that reaches the grooves 13, thereby dividing the workpiece 1 into individual chips 10.

[0037] In the first embodiment, in the division step 104, the grinding device 60 places the front surface 4 side of the workpiece 1 on the holding surface 62 of the holding table 61 through the film 16, the cured liquid resin 15, and the protective film 12, as shown in Fig. 11, opens the on-off valve 63, sucks the holding surface 62 with the suction source 64, and holds the workpiece 1 on the holding surface 62 by suction, thereby exposing the back surface 7 of the workpiece 1. In the first embodiment, in the division step 104, as shown in Fig. 11, the grinding device 60 rotates the grinding wheel 66 around its axis by the spindle 65 and rotates the holding table 61 around its axis, so that the grinding stone 67 of the grinding wheel 66 abuts against the back surface 7 of the workpiece 1 and approaches the holding table 61 at a predetermined feed rate, and grinds the back surface 7 of the workpiece 1 with the grinding stone 67.

[0038] In the first embodiment, in the dividing step 104, the grinding device 60 grinds the back surface 7 of the workpiece 1 until the thickness of the workpiece 1 reaches a predetermined thickness (a thickness at which the grooves 13 are exposed on the back surface 7). In the first embodiment, in the dividing step 104, when the thickness of the workpiece 1 reaches the predetermined thickness, the grinding device 60 moves the grinding wheel 94 away from the back surface 7 of the workpiece 1 and stops the rotation around the axis of the holding table 61, as shown in FIG. 12. Then, the grooves 13 are exposed on the back surface 7 of the workpiece 1, and the workpiece 1 is divided into individual chips 10.

[0039] In the present invention, in the dicing step 102, a laser beam having a wavelength absorbed by the work 1 is irradiated to form grooves 13, and then in the dividing step 104, the back surface 7 of the work 1 may be ground. Alternatively, in the dicing step 102, a cutting blade 35 or a laser beam may be used to form dividing grooves that divide the work 1, thereby dividing the work 1 in the dicing step 102, and then in the dividing step 104, the back surface 7 of the work 1 may be ground.

[0040] In the present invention, in the dicing step 102, a stealth dicing process may be performed in which a laser beam having a wavelength that is transparent to the workpiece 1 is irradiated to form a modified layer on the workpiece 1. In this case, it is preferable to form a modified layer along the planned processing line 5 and a crack that extends from the modified layer to the protective film 12 and divides the protective film 12. The modified layer means a region in which the density, refractive index, mechanical strength, and other physical properties are different from those of the surrounding area, and examples of the modified layer include a melting process region, a crack region, an insulation breakdown region, a refractive index change region, and a region in which these regions are mixed.

[0041] (Removal step) Fig. 13 is a cross-sectional view showing a schematic diagram of the removing step of the processing method shown in Fig. 2. The removing step 105 is a step of removing the protective film 12 together with the hardened liquid resin 15 from the front surface 4 of the workpiece 1 after the liquid resin supplying step 103. In the first embodiment, in the removing step 105, the peeling device 70 places the back surface 7 side of the workpiece 1 on the holding surface 72 of the holding table 71, opens the on-off valve 73, and sucks the holding surface 72 with the suction source 74, thereby suction-holding the workpiece 1 on the holding surface 72.

[0042] 13, in the removing step 105, a peeling device 70 holds one end of the film 16 with a chuck 75 and moves the chuck 75 along a holding surface 72 toward the other end, thereby peeling off the liquid resin 15 and protective film 12 fixed to the film 16 from the surface 4 of the workpiece 1. After the opening / closing valve 73 is closed, the chip 10 is picked up from the holding surface 72 of the holding table 71.

[0043] The processing method according to the first embodiment described above forms the protective film 12 with a non-polymerized resin. Since the non-polymerized resin constituting the protective film 12 is in a state in which the molecules are not bonded to each other, the entire protective film 12 does not peel off even when subjected to an impact from the cutting process in the dicing step 102, but rather the area subjected to the load from the cutting process peels off locally. Therefore, the processing method according to the first embodiment has the effect of suppressing peeling of the protective film 12 caused by the cutting process.

[0044] Furthermore, even if a non-polymerized resin is laminated on the protective film 12 when peeling off the protective film 12, the protective film 12 will peel off locally where a load is applied, making it difficult to peel off the protective film 12. However, in the processing method according to the first embodiment, before peeling off the protective film 12, liquid resin 15 is supplied onto the protective film 12 and the liquid resin 15 is allowed to permeate the protective film 12 made of a non-polymerized resin. For this reason, in the processing method according to the first embodiment, the protective film 12 and the liquid resin 15 can be firmly fixed together by curing the liquid resin 15.

[0045] As a result, in the processing method according to the first embodiment, the protective film 12 can be peeled off from the workpiece 1 by peeling off the protective film 12 together with the hardened liquid resin 15.

[0046] [Embodiment 2] A processing method according to the second embodiment will be described with reference to the drawings. Fig. 14 is a cross-sectional view that shows a state in which an opening that exposes a line to be processed is formed in a protective film in a dicing step of the processing method according to the second embodiment. Fig. 15 is a cross-sectional view that shows a schematic configuration example of an etching device that forms a groove in a workpiece in a dicing step of the processing method according to the second embodiment. In Fig. 14, the same parts as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted.

[0047] The processing method according to the second embodiment includes a protective film forming step 101, a dicing step 102, a liquid resin supplying step 103, a dividing step 104, and a removing step 105, similar to the first embodiment, except for the dicing step 102. In the processing method according to the second embodiment, the protective film agent 11 is made of a non-polymerized resin, a solvent that dissolves the non-polymerized resin, and a light-absorbing material that is absorbent to the wavelength of the laser beam 86 shown in FIG.

[0048] The non-polymerized resin constituting the protective film agent 11 is a resin that is resistant to the plasmatized etching gas used in the dicing step 102. The light absorbing material is a material that is absorptive to the laser beam 86 having a wavelength of, for example, 355 nm, and for example, carbon black or phthalocyanine is used. In addition, the protective film 12 formed on the entire surface 4 of the workpiece 1 by drying the protective film agent 11 contains the above-mentioned resin, and is therefore made of a material that is resistant to the plasmatized etching gas used in the dicing step 102, and is formed to a uniform thickness that is resistant to the etching gas, and is absorptive to the laser beam 86 having a wavelength of, for example, 355 nm.

[0049] 14 sucks and holds the back surface 7 of the work 1 on a holding surface 82 of a chuck table 81 via a tape 8, and clamps the frame 9 with a clamp portion 87 provided around the chuck table 81. In the dicing step 102 of the second embodiment, the laser processing device 80 captures an image of the front surface 4 of the work 1 with an imaging camera, and performs alignment to align the work 1 with a condenser lens 84 of a laser beam application unit 83.

[0050] In the first embodiment, in the dicing step 102, the laser processing device 80 irradiates the protective film 12 on each of the to-be-processed lines 5 with a laser beam 86 having a wavelength (e.g., 355 nm) absorbed by the protective film 12 oscillated by an oscillator 85 while relatively moving the chuck table 81 and the laser beam application unit 83 along the to-be-processed line 5 as shown in Fig. 14, thereby removing the protective film 12 on each of the to-be-processed lines 5 by ablation processing. In the second embodiment, in the dicing step 102, the laser processing device 80 forms an opening along the to-be-processed line 5 over the entire length of each of the to-be-processed lines 5. The opening exposes the to-be-processed line 5 at its bottom.

[0051] (Etching equipment) Next, an etching apparatus 50 for performing the dicing step 102 of the processing method according to embodiment 2 will be described with reference to the drawings. As shown in FIG. 15, the etching apparatus 50 includes a rectangular parallelepiped chamber 51, a holding unit 52, an upper electrode 53, and a control unit 55.

[0052] The chamber 51 has a processing space 511 formed therein where plasma etching is performed. The chamber 51 has an opening 513 for loading and unloading the workpiece 1, and an opening / closing door 514 for opening and closing the opening 513, provided on one side wall 512. The opening / closing door 514 opens and closes the opening 513 by being raised and lowered by an opening / closing mechanism 515 constituted by an air cylinder or the like.

[0053] Further, an exhaust port 517 that connects the inside and outside of the chamber 51 is formed in the bottom wall 516 of the chamber 51. An exhaust mechanism 510 such as a vacuum pump is connected to the exhaust port 517.

[0054] The holding unit 52 and the upper electrode 53 are disposed opposite to each other in the processing space 511 of the chamber 51. The upper surface of the holding unit 52 is a holding surface 524 that holds the workpiece 1 via the tape 8. The holding unit 52 is also made of a conductive material and functions as a lower electrode.

[0055] The holding unit 52 includes a disk-shaped holding portion 521 and a columnar support portion 520 protruding downward from the center of the lower surface of the holding portion 521. The support portion 520 is inserted into an opening 522 formed in a bottom wall 516 of the chamber 51. In the opening 522, an annular insulating member 523 is disposed between the bottom wall 516 and the support portion 520, and the chamber 51 and the holding unit 52 are electrically insulated from each other. In addition, the holding unit 52 is connected to a high-frequency power source 56 outside the chamber 51.

[0056] An electrode 526 connected to a high-frequency power source (not shown) is provided on the holding portion 521 of the holding unit 52. When power is applied from the high-frequency power source to the electrode 526, the holding unit 52 generates a dielectric polarization phenomenon between the holding surface 524 and the workpiece 1, and the workpiece 1 is attracted and held on the holding surface 524 by electrostatic attraction force due to the polarization of the charge.

[0057] Moreover, inside the holding part 521 and inside the support part 520 of the holding unit 52, a cooling flow path 527 through which a cooling fluid flows for cooling the holding unit 52 is formed. Both ends of the cooling flow path 527 are connected to a refrigerant circulation mechanism 528. When the refrigerant circulation mechanism 528 is operated, the cooling fluid such as water circulates through the cooling flow path 527, and the holding unit 52 is cooled.

[0058] The upper electrode 53 is made of a conductive material and includes a disk-shaped gas ejection part 531 and a cylindrical support part 530 protruding upward from the center of the upper surface of the gas ejection part 531. The support part 530 is inserted into an opening 532 formed in an upper wall 518 of the chamber 51. In the opening 532, an annular insulating member 533 is disposed between the upper wall 518 and the support part 530, and the chamber 51 and the upper electrode 53 are electrically insulated from each other.

[0059] The upper electrode 53 is connected to a high-frequency power source 57 outside the chamber 51. In addition, a support arm of a lifting mechanism 534 is attached to the upper end of the support part 530. The upper electrode 53 is raised and lowered by the lifting mechanism 534.

[0060] A plurality of ejection ports 535 are provided on the lower surface side of the gas ejection part 531. The ejection port 535 is connected to a first etching gas supply source 58 and a second etching gas supply source 59 through a flow path 536 formed in the gas ejection part 531 and the support part 530. The first etching gas supply source 58 supplies the first etching gas from the ejection port 535 through the flow path 536 into the chamber 51. In the first embodiment, when the substrate 2 of the work 1 is made of silicon, the first etching gas supply source 58 supplies a fluorine-based gas as the first etching gas into the chamber 51. The second etching gas supply source 59 supplies a second etching gas from the ejection port 535 through the flow path 536 into the chamber 51. In the first embodiment, the second etching gas supply source 59 supplies an oxygen-based gas as the second etching gas into the chamber 51.

[0061] The control unit 55 controls each component of the etching apparatus 50 to cause the etching apparatus 50 to perform plasma etching on the workpiece 1. The control unit 55 is a computer having an arithmetic processing device having a microprocessor such as a CPU (central processing unit), a storage device having a memory such as a ROM (read only memory) or a RAM (random access memory), and an input / output interface device. The arithmetic processing device of the control unit 55 performs arithmetic processing according to a computer program stored in the storage device, and outputs control signals for controlling the etching apparatus 50 to each component of the etching apparatus 50 via the input / output interface device.

[0062] The control unit 55 is connected to a display unit configured with a liquid crystal display device or the like that displays various information and images, and an input unit that an operator uses to register processing content information, etc. The input unit is configured with at least one of a touch panel provided on the display unit and an external input device such as a keyboard.

[0063] In the second embodiment, in the dicing step 102 , the etching device 50 raises the upper electrode 53 by the lifting mechanism 534 , and then lowers the opening / closing door 514 by the opening / closing mechanism 515 to open the opening 513 .

[0064] In the second embodiment, in the dicing step 102, the workpiece 1 having an opening formed in the protective film 12 is carried into the processing space 511 by a transport unit (not shown) in the etching device 50, and the workpiece 1 is placed on the holding surface 524 of the holding unit 52 via the tape 8. In the second embodiment, in the dicing step 102, the etching device 50 applies power from a high-frequency power source to the electrode 526, and adsorbs and holds the back surface 7 of the workpiece 1 on the holding surface 524 via the tape 8.

[0065] In the second embodiment, in the dicing step 102, the etching apparatus 50 raises the opening / closing door 514 by the opening / closing mechanism 515 to close the opening 513, operates the exhaust mechanism 510 to reduce the pressure inside the chamber 51, places the processing space 511 in a vacuum state (low pressure state), and operates the coolant circulation mechanism 528 to circulate a cooling fluid such as water inside the cooling passage 527 to suppress an abnormal temperature rise in the holding unit 52. In the second embodiment, in the dicing step 102, the etching apparatus 50 lowers the upper electrode 53 by the lifting mechanism 534, and positions the distance between the lower surface of the upper electrode 53 and the workpiece 1 held by the holding unit 52 constituting the lower electrode at a predetermined inter-electrode distance suitable for plasma etching.

[0066] In the second embodiment, in the dicing step 102, the etching device 50 supplies a first etching gas from the first etching gas supply source 58 at a predetermined flow rate and ejects the first etching gas from the multiple ejection ports 535 of the gas ejection part 531 toward the workpiece 1 held on the holding unit 52. In the second embodiment, in the dicing step 102, while the first etching gas is being supplied from the first etching gas supply source 58, the etching device 50 applies high-frequency power from the high-frequency power source 57 to the upper electrode 53 to create and maintain plasma, and applies high-frequency power from the high-frequency power source 56 to the holding unit 52, which is the lower electrode, to attract ions.

[0067] In the second embodiment, in the dicing step 102, the etching device 50 converts the first etching gas in the space between the holding unit 52 and the upper electrode 53 into plasma, and this plasmatized first etching gas is drawn into the workpiece 1 side to etch (so-called plasma etching) the front surface 4 of the line to be processed 5 exposed from the opening in the protective film 12 of the workpiece 1, forming grooves 13 on the front surface 4 of the line to be processed 5, and the grooves 13 proceed toward the back surface 7 of the workpiece 1. Thus, in the second embodiment, in the dicing step 102, plasma etching is performed on the workpiece 1 through the protective film 12, and the grooves 13 proceed toward the back surface 7 of the workpiece 1 by so-called plasma dicing.

[0068] In the second embodiment, when the substrate 2 is made of silicon, a fluorine-based gas such as SF6, C4F8 or CF4 is used as the first etching gas, but the first etching gas is not limited to these. In the second embodiment, in the dicing step 102, the etching device 50 performs plasma etching on the work 1 by the Bosch method, which alternately repeats plasma etching by supplying SF6 and deposition of a protective film on the inner side surface of the groove 13 by supplying C4F8, but in the present invention, plasma etching may be performed by supplying a single etching gas.

[0069] In the second embodiment, in the dicing step 102, the etching device 50 has a predetermined time set in advance for plasma etching the substrate 2 of the work 1 according to the thickness of the substrate 2 of the work 1. In the second embodiment, in the dicing step 102, the etching device 50 applies high-frequency power to the holding unit 52 and the upper electrode 53 while supplying the first etching gas for a predetermined time, thereby completely removing the processing lines 5 exposed from the openings in the protective film 12, and may divide the work 1 into individual chips 10, or may form grooves 13 in the work 1 as in the first embodiment.

[0070] In the processing method according to the second embodiment, the protective film 12 is formed of a non-polymerized resin, and the molecules of the non-polymerized resin constituting the protective film 12 are not bonded to each other, so that the entire protective film 12 does not peel off even when subjected to an impact due to the ablation process in the dicing step 102, but the area subjected to the load due to the ablation process peels off locally. Therefore, the processing method according to the second embodiment has an effect of suppressing peeling of the protective film 12 due to the ablation process.

[0071] Next, the inventor of the present invention confirmed the effects of the present invention. In the confirmation, the inventor confirmed the peeling state of the protective film 12 from the surface 4 of the workpiece 1 after cutting the workpiece 1 on which the protective film 12 of the present invention and the comparative example was formed to form the groove 13. The results are shown in Table 1 below.

[0072] [Table 1]

[0073] In the present invention, the groove 13 was formed in the workpiece 1 by cutting the workpiece 1 on which the protective film 12 made of a non-polymerized resin was formed. In Comparative Example 1, the groove 13 was formed in the workpiece 1 by cutting the workpiece 1 on which the protective film was formed by coating with an ultraviolet-curable resin made of acrylate, a photopolymerization agent, and a solvent and curing (polymerizing) it by irradiating it with ultraviolet light. In Comparative Example 2, the groove 13 was formed in the workpiece 1 by cutting the workpiece 1 on which the protective film was formed by coating with a water-soluble liquid resin made of polyvinyl alcohol (PVA), which is a polymerized resin, by spin coating and drying it to harden it.

[0074] According to Table 1, in Comparative Examples 1 and 2, the protective film peeled off from the surface 4 of the workpiece 1 at the edge of the groove 13, whereas in the product of the present invention, the protective film 12 did not peel off from the surface 4 of the workpiece 1 at the edge of the groove 13. Therefore, according to Table 1, it is clear that by forming the protective film 12 from a non-polymerized resin, peeling of the protective film 12 due to processing such as cutting can be suppressed more than when the protective film is formed from a polymerized resin.

[0075] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]

[0076] 1 Work 4 surface 5 Processing lines 6 Devices 7 Back side 11 Protective Film Agent 12 Protective film 13 Groove 14 Remaining cut 15 Liquid resin 16 Film 17 Ultraviolet rays (external stimulation) 61 Holding Table 101 Protective film formation step 102 Dicing Step 103 Liquid resin supply step 104 division steps 105 Removal Steps

Claims

1. A method for processing a workpiece in which a planned processing line is set, a protective film forming step of forming a protective film made of a non-polymerized resin on the surface of the workpiece; a dicing step of dicing the workpiece together with the protective film along the planned processing line after the protective film is formed.

2. a liquid resin supplying step of supplying a liquid resin that is hardened by an external stimulus onto the protective film after the dicing step, and then hardening the liquid resin and fixing the liquid resin to the protective film by applying the external stimulus to the liquid resin; 2. The processing method according to claim 1, further comprising a removing step of removing the protective film together with the hardened liquid resin from the surface of the workpiece after the liquid resin supplying step.

3. The workpiece is set up with multiple intersecting processing lines, In the dicing step, grooves are formed in the workpiece along the plurality of planned processing lines, and uncut portions of the workpiece are formed below the grooves; 3. The processing method according to claim 2, further comprising a dividing step in which, after the liquid resin supplying step and before the removing step, the workpiece is held on a holding table via the protective film to expose the back surface of the workpiece, and the exposed back surface is ground to thin the workpiece to a thickness that reaches the groove, thereby dividing the workpiece.

4. 4. The processing method according to claim 2, wherein in the liquid resin supplying step, a film is disposed on the liquid resin, and the liquid resin is fixed to the protective film and the film is fixed to the liquid resin.

Citation Information

Patent Citations

  • Protective film agent used for laser dicing and method of processing wafer using the same

    JP2006140311A

  • Dividing method for lithium tantalate wafer

    JP2015062958A

  • Processing method for work-piece

    JP2021100074A