Packaging material and manufacturing method of packaging material

A packaging material with a white and light-shielding layer using a urethane resin derived from polyester polyol improves adhesion and lamination strength, addressing dispersion issues and design impairments in existing technologies.

JP2024157910AActive Publication Date: 2024-11-08TOYO INK MFG CO LTD +1

Patent Information

Application Number
JP2023072573
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

Existing packaging materials face challenges with substrate adhesion, appearance, and hot lamination strength, particularly when using light-shielding inks containing titanium oxide, carbon black, or aluminum particles, which are difficult to disperse uniformly and can impair design and reduce adhesion.

Method used

A packaging material comprising a base material with a white printed layer and a light-shielding printed layer, both containing a urethane resin derived from a polyester polyol condensation product of a dibasic acid and a diol, specifically using sebacic acid, succinic acid, or dimer acid, to improve adhesion and lamination strength.

Benefits of technology

The solution provides excellent substrate adhesion, appearance, and hot lamination strength, ensuring uniform dispersion and effective light shielding without impairing design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157910000001
    Figure 2024157910000001
  • Figure 2024157910000002
    Figure 2024157910000002
  • Figure 2024157910000003
    Figure 2024157910000003
Patent Text Reader

Abstract

To provide a packaging material that is excellent in adhesion to a base material, appearance, light-shielding properties, and hot lamination strength.SOLUTION: In a packaging material that has a base material, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant in this order. The white printed layer includes white pigment, the light-shielding printed layer contains at least one kind of pigment selected from a group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide, the white printed layer and the light-shielding printed layer include urethane resin, the urethane resin includes a structural unit derived from polyester polyol which is a condensation product of dibasic acid and diol, and the dibasic acid includes at least one kind of acid selected from the group consisting of sebacic acid, succinic acid, and dimer acid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging material and a method for making the packaging material. [Background technology]

[0002] Packaging materials may contain light-blocking materials such as aluminum foil, aluminum-deposited film, milky film, and black film in order to prevent the deterioration of the contents due to light. However, the use of aluminum foil and aluminum-deposited film has issues such as a large amount of CO2 emissions during production, which places a heavy burden on the environment, and the difficulty of recycling the packaging material, and the use of milky film and black film has issues such as the loss of the design of the packaging material. For this reason, in recent years, there have been an increasing number of cases where packaging materials are given light-blocking properties by using a printed layer that uses a light-blocking ink containing titanium oxide, carbon black, or aluminum particles.

[0003] For example, Patent Document 1 discloses a packaging material including a printed layer consisting of a white ink layer and a gray ink layer, which is said to have good light-shielding properties, whiteness, and lamination strength without the use of an aluminum compound, but has problems with adhesion to substrates without an isocyanate compound. Patent Document 2 discloses a packaging material including a concealing layer using silver ink made of aluminum paste and two solid white layers, which is said to have good light-shielding properties and concealing properties, but there is a concern that the adhesion to substrates and lamination strength may decrease with inks using conventional urethane resins in processes where heat is applied, such as extrusion lamination and retort processing. Furthermore, pigments that have light-blocking properties, such as carbon black, aluminum particles, and iron oxide, are generally difficult to disperse in ink, and it is difficult to form and maintain a uniformly dispersed state. This leads to poor printability, particularly ink transfer (trapping properties) during overprinting, and tends to result in a poor appearance of the packaging material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6864774 [Patent Document 2] Patent Publication No. 2022-082716 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a packaging material that is excellent in adhesion to a substrate, appearance, light-shielding properties, and hot lamination strength. [Means for solving the problem]

[0006] In view of the above problems, the inventors conducted intensive research and found that the above problems could be solved by using the packaging material described below, leading to the creation of the present invention.

[0007] That is, the present invention relates to the following [1] to [5].

[0008] [1] A packaging material having a substrate, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant in this order, The white printing layer contains a white pigment, the light-shielding printed layer contains at least one pigment selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide, the white printed layer and the light-shielding printed layer contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, The packaging material, wherein the dibasic acid comprises at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid.

[0009] [2] The packaging material according to [1], wherein the dibasic acid includes sebacic acid.

[0010] [3] The packaging material described in claim [1] or [2], wherein the white printed layer and / or the light-shielding printed layer contains a cured material derived from an isocyanate-based curing agent.

[0011] [4] A method for producing a packaging material having a substrate, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant in this order, comprising: A step of forming a white printing layer by gravure printing or flexographic printing with white ink; and forming a light-shielding printed layer by gravure printing or flexographic printing a light-shielding ink on the white printed layer, the light-shielding ink contains at least one selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide; the white ink and the light-shielding ink contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, The method for producing a packaging material, wherein the dibasic acid comprises at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid.

[0012] [5] The amount of light-blocking ink applied by printing is 0.5 g / m 2 More than 5g / m 2 The method for producing a packaging material described in [4], wherein the manufacturing cost is less than or equal to the manufacturing cost. Effect of the Invention

[0013] According to the present invention, it is possible to provide a packaging material that is excellent in adhesion to a substrate, appearance, light-shielding properties, and hot lamination strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.

[0015] The packaging material of the present invention will be described in detail below. The packaging material of the present invention is a packaging material having a base material, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant, in this order, wherein the white printed layer contains a white pigment, the light-shielding printed layer contains at least one selected from the group consisting of carbon black, aluminum particles, iron oxide and zinc oxide, the white printed layer and the light-shielding printed layer contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol, which is a condensation product of a dibasic acid and a diol, and the dibasic acid contains at least one selected from the group consisting of sebacic acid, succinic acid and dimer acid. It is believed that by providing the white printed layer and the light-shielding printed layer with the above-mentioned components, the affinity between the ink interfaces is improved, resulting in good trapping properties and good hot lamination strength.

[0016] In this specification, a printed layer that does not contain a light-shielding pigment is referred to as "other ink layers" in contrast to the "white printed layer" and "light-shielding printed layer" that have light-shielding properties. Furthermore, the white printed layer, the light-shielding printed layer, and the other ink layers are collectively referred to as "printed layers."

[0017] <Packaging material> The packaging material of the present invention is a packaging material having a structure in which a substrate, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant are laminated in this order from the outer layer side. Specific examples of the laminate structure can be exemplified below, in order from the outer layer side (left side). In the following structure notation, " / " means the boundary between each layer. (1) Base material / white printed layer / light-shielding printed layer / adhesive layer / sealant (2) Substrate / white printed layer / light-shielding printed layer / adhesive layer / intermediate substrate layer / adhesive layer / sealant (3) Substrate / other ink layer / white printing layer / light-shielding printing layer / adhesive layer / sealant (4) Substrate / white printed layer / other ink layers / light-shielding printed layer / adhesive layer / sealant (5) Substrate / white printed layer / light-shielding printed layer / other ink layers / adhesive layer / sealant (6) Substrate / other ink layer / white printing layer / light-shielding printing layer / adhesive layer / intermediate substrate layer / adhesive layer / sealant (7) Substrate / white printed layer / other ink layers / light-shielding printed layer / adhesive layer / intermediate substrate layer / adhesive layer / sealant (8) Substrate / white printing layer / light-shielding printing layer / other ink layers / adhesive layer / intermediate substrate layer / adhesive layer / sealant The layer structure can be selected arbitrarily, but it is preferable that the light-shielding printed layer be visible from the outside (substrate side).

[0018] <White printing layer, light-shielding printing layer> The packaging material of the present invention has a white printed layer and a light-shielding printed layer between the substrate and the sealant. The white printed layer and the light-shielding printed layer may be provided on the entire surface of the substrate, or on a part of the surface of the substrate. As described above, the packaging material may further have an ink layer. The white printed layer and the light-shielding printed layer of the packaging material of the present invention contain a urethane resin containing a structural unit derived from a polyester polyol, which is a condensate of a dibasic acid and a diol. Furthermore, the white printed layer of the packaging material of the present invention contains a white pigment, and the light-shielding printed layer contains a urethane resin and at least one pigment selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide.

[0019] (white ink) The white print layer can be formed by printing a white ink. The white ink can be produced by dissolving and / or dispersing a white pigment such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, or the like, and a urethane resin in an organic solvent. As the white pigment, titanium oxide is preferred from the viewpoints of coloring power, shielding properties, and light-shielding properties.

[0020] (Light-blocking ink) The light-shielding printed layer can be formed by printing a light-shielding ink. The light-shielding ink can be produced by dissolving and / or dispersing a light-shielding pigment and a urethane resin in an organic solvent. The amount of light-shielding ink applied by printing was set at 0.5 g / m immediately after application in order to achieve sufficient light-shielding properties and adhesion to the substrate. 2 More than 5g / m 2 It is preferably less than 0.6 g / m 2 More than 4.9g / m 2 Less than 0.7 g / m, more preferably 0.7 g / m 2 More than 4.5g / m 2 or less than 4g / m 2 The following is the result.

[0021] (Light-blocking pigment) The light-shielding printed layer contains at least one light-shielding pigment selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide. The light-shielding pigment may be used alone or in combination of two or more. The content of the light-shielding pigment in the light-shielding printed layer (i.e., the content of the light-shielding pigment in the total solid content of the light-shielding ink) is preferably 20 to 65 mass% of the total mass of the light-shielding printed layer (total solid content of the light-shielding ink), more preferably 35 to 63 mass%, and even more preferably 45 to 60 mass%. By making the content of the light-shielding pigment in the light-shielding printed layer 20% or more, the light-shielding properties are improved. By making the content 65% or less, the laminate properties are improved.

[0022] (Carbon Black) Specifically, the carbon black is preferably CI Pigment Black 7. The average particle size of the carbon black is preferably 20 to 120 nm, more preferably 23 to 100 nm, and even more preferably 25 to 100 nm. When the average particle size of the carbon black is within the above range, good pigment dispersibility and a vivid hue can be obtained. Here, the above average particle size is an arithmetic mean diameter determined by observing the carbon black particles under an electron microscope.

[0023] (aluminum particles) The aluminum particles are preferably aluminum flakes. The aluminum flakes may be either leafing or non-leafing metal flakes. The metal flakes have higher fatty acids adsorbed on the metal surface, and among these, fatty acids having carbon numbers of 12 to 18 are preferred, and fatty acids having carbon numbers of 16 to 18 are more preferred. Suitable examples of higher fatty acids include lauric acid, palmitic acid, stearic acid, oleic acid, vaccenic acid, elaidic acid, linoleic acid, and linolenic acid. Stearic acid and oleic acid are particularly preferred. Metal flakes that have been surface-treated with a resin may also be used.

[0024] (iron oxide, zinc oxide) As the light-shielding pigment, zinc oxide and / or iron oxide can be used. The average particle size (primary particle size) of zinc oxide is preferably 0.01 to 1 μm, more preferably 0.01 to 0.7 μm. The average particle size (primary particle size) of iron oxide is preferably 0.01 to 1 μm, more preferably 0.1 to 0.7 μm.

[0025] (Coloring agent) The light-shielding printed layer may contain a colorant. Examples of the colorant include dyes, pigments, and other colorants. Among them, it is preferable to contain a pigment, and the pigment may be either an inorganic pigment or an organic pigment. Examples of inorganic pigments include yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine, and cobalt blue, and examples of organic pigments include soluble azo, insoluble azo, azo, phthalocyanine, halogenated phthalocyanine, anthraquinone, anthanthrone, dianthraquinonyl, anthrapyrimidine, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, flavanthrone, diketopyrrolopyrrole, isoindoline, and indanthrone pigments. In addition, any pigment indicated by the CI pigment number in the Color Index may be used.

[0026] (urethane resin) The urethane resin contained in the white printed layer and the light-shielding printed layer contains a constituent unit derived from a polyester polyol which is a condensate of a dibasic acid and a diol, and the dibasic acid contains at least one selected from the group consisting of sebacic acid, succinic acid and dimer acid. The urethane resin contained in the white printed layer and the urethane resin contained in the light-shielding printed layer may be the same or different, but from the viewpoint of trapping properties, it is preferable that the urethane resin of each layer contains a constituent unit derived from the same dibasic acid. In addition, from the viewpoint of hot lamination strength, it is more preferable that the urethane resin of each layer contains a constituent unit derived from sebacic acid, and it is even more preferable that the ratio of the constituent unit derived from sebacic acid is the highest in the dibasic acid constituting the urethane resin of each layer.

[0027] The urethane resin is not limited to the following, but examples thereof include urethane resins obtained by reacting a urethane prepolymer obtained by reacting a polyisocyanate with a polyol, and then reacting a chain extender such as a polyamine and, if necessary, a reaction terminator, etc. The urethane resin may have urea bonds in addition to urethane bonds. In order to obtain a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, a polyester polyol which is a condensation product of a dibasic acid and a diol is used as the polyol.

[0028] The content of the urethane resin is preferably 5 to 50% by mass, and more preferably 10 to 40% by mass, in 100% by mass of the white ink. Also, the content is preferably 5 to 90% by mass, and more preferably 10 to 80% by mass, in 100% by mass of the white printed layer. When the content of the urethane resin is within this range, the adhesion to the substrate is good.

[0029] The content of the urethane resin is preferably 5 to 50% by mass, and more preferably 10 to 40% by mass, in 100% by mass of the light-shielding ink. Also, the content is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass, in 100% by mass of the light-shielding printed layer. When the content of the urethane resin is within this range, the adhesion to the substrate is good.

[0030] (Polyisocyanate) The polyisocyanate preferably contains a diisocyanate. Examples of the diisocyanate include aliphatic diisocyanates such as tetramethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate; cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimers in which the carboxyl groups of dimer acids are converted to isocyanate groups. Alicyclic diisocyanates such as diisocyanates; and aromatic diisocyanates such as α,α,α',α'-tetramethylxylylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dimethyldiphenylmethane diisocyanate, tetramethyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, o-xylylene diisocyanate, and 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate. Among these, from the viewpoints of easy reaction control and good balance of the performance of the resulting urethane resin, alicyclic or araliphatic diisocyanates are preferred, and isophorone diisocyanate and α,α,α',α'-tetramethylxylylene diisocyanate are particularly preferred. At least one diisocyanate may be used, and two or more diisocyanates may be used in combination.

[0031] (Polyol) The polyol is essentially a polyester polyol, which is a condensate of a diol and a dibasic acid including at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid. In addition, polyester polyols not including the dibasic acid, polyether polyols, polycarbonate polyols, and polyolefin polyols can be used in combination. The content of the polyester polyol-derived structural unit in the total mass of the urethane resin is preferably 50% by mass or more (main component), more preferably 60% by mass or more, and even more preferably 70% by mass or more. In addition, it is particularly preferable that the dibasic acid is sebacic acid.

[0032] The number average molecular weight of the polyol is preferably 500 to 10,000. Here, the number average molecular weight of the polyol is calculated from the hydroxyl value, which is a value calculated by esterifying or acetylating the hydroxyl groups in the resin, back titrating the remaining acid with an alkali, converting the amount of hydroxyl groups in 1 g of the resin into mg of potassium hydroxide, and is a value measured according to JIS K0070. When the number average molecular weight of the polyol is 10,000 or less, the ink has excellent blocking resistance to the plastic substrate. Also, when the number average molecular weight of the polyol is 500 or more, the flexibility of the urethane resin film is excellent, and the ink has excellent adhesion to the plastic film. For the above reasons, the number average molecular weight of the polyol is more preferably 1,000 to 5,000.

[0033] The polyol is preferably a diol. The diol refers to a compound having two hydroxyl groups in one molecule. Examples of the diol include polyester polyol, polyether diol, polycarbonate, polybutadiene glycol, and other polyols. At least one diol may be used, and two or more diols may be used in combination.

[0034] (Polyester polyol) The polyester polyol has as its essential component a polyester polyol which is a condensation product of a dibasic acid including at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid with a diol, but it is also possible to use other polyester polyols in combination.

[0035] Suitable examples of diols used in the polyester polyol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol. As for the diol, it is preferable to use a combination of a linear diol such as ethylene glycol, 1,4-butanediol, 1,3-propanediol, etc. and a branched diol such as propylene glycol, neopentyl glycol, 3-methyl-1,5-pentanediol, etc. The linear diol imparts crystallinity, while the branched diol imparts flexibility, and depending on the balance between them, the adhesion between the ink and the plastic substrate and the solubility of the ink composition in the solvent are improved.

[0036] The dibasic acid used in the polyester polyol must contain at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid, but other suitable examples include adipic acid, phthalic anhydride, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, oxalic acid, malonic acid, pimelic acid, azelaic acid, suberic acid, glutaric acid, 1,4-cyclohexyl dibasic acid, and hydrogenated dimer acid. Of the total mass of the dibasic acid, it is preferable that at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid is contained in an amount of 5 mass% or more, more preferably 10 mass%, and even more preferably 20 mass%. Among these, it is preferable that the dibasic acid contains at least sebacic acid.

[0037] Furthermore, a polyol having three or more hydroxyl groups and / or a polyvalent carboxylic acid having three or more carboxyl groups can be used in combination as a raw material for the polyester polyol.

[0038] When used in a light-shielding printed layer, the amount of constituent units of sebacic acid in the total mass of the dibasic acid is preferably 20 mass % or more, more preferably 30 mass % or more, and even more preferably 40 mass % or more. When used in a white print layer, the amount of constituent units of sebacic acid in the total mass of the dibasic acid is preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more.

[0039] (Chain extender) The chain extender is preferably a polyamine. Suitable examples of the polyamine include, but are not limited to, ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and diamines obtained by converting the carboxyl groups of dimer acid to amino groups. These may be used alone or in combination of two or more.

[0040] Amino acids can also be used as chain extenders. The term "amino acid" refers to a compound having both an amino group and an acidic functional group in one molecule, and preferred examples include glutamine, asparagine, lysine, diaminopropionic acid, ornithine, diaminobenzoic acid, and diaminobenzenesulfonic acid. In addition, in the synthesis process of the urethane resin, the acidic group is highly likely to remain unreacted with the isocyanate group, so that the acidic group remains in the urethane resin and the acid value can be maintained.

[0041] (Reaction stopper) In the case of a urethane resin that can be produced only by the urethanization step, it is preferable to use a monoalcohol or a monoamine as the reaction terminator, and in the case of a urethane resin that is produced by carrying out a urethanization reaction step in addition to the urethanization step, it is preferable to use a monoamine. The monoalcohol is preferably a substituted or unsubstituted alcohol, and suitable examples thereof include methanol, ethanol, n-propanol, isopropyl alcohol, and 1-butanol. The monoamine is preferably a substituted or unsubstituted monoamine, and suitable examples thereof include n-butylamine, n-dibutylamine, octylamine, diethylamine, monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, etc. As the reaction terminator, the compounds exemplified as the chain extender can also be used, and at least one of them may be used, or two or more of them may be used in combination.

[0042] In producing a urethane prepolymer having an isocyanate group at its end obtained by reacting a polyisocyanate with a polyol, the molar equivalent ratio of NCO of the polyisocyanate to OH of the polyol (molar equivalent of NCO of the polyisocyanate / molar equivalent of OH of the polyol compound) is preferably 1.3 to 3, more preferably 1.5 to 2.

[0043] The urethane resin preferably has an active hydrogen group such as a hydroxyl group and / or an amino group. This is to obtain a reaction site with the isocyanate-based curing agent described later. When the urethane resin has a hydroxyl group, the hydroxyl value is preferably 0.5 to 30 mgKOH / g, more preferably 1 to 20 mgKOH / g, and even more preferably 2 to 15 mgKOH / g. When the urethane resin has an amino group, the amine value is preferably 0.1 to 15 mgKOH / g, and even more preferably 1 to 12 mgKOH / g. On the other hand, the acid value of the urethane resin is preferably 5 mgKOH / g or less, and even more preferably 3 mgKOH / g or less. This is because the acid group is difficult to react with the isocyanate-based curing agent described later.

[0044] The mass average molecular weight of the urethane resin is preferably 5,000 to 100,000, more preferably 7,000 to 90,000, and even more preferably 10,000 to 80,000. When the urethane resin has the above mass average molecular weight, the printed layer becomes a strong film by crosslinking with the curing agent described below, and sufficient hot lamination strength is obtained. The mass average molecular weight of the present invention and the molecular weight distribution (Mw / Mn) described later can be measured by gel permeation chromatography (GPC). As an example, Water2690 (manufactured by Waters Corporation) or HLC-8220 (manufactured by Tosoh Corporation) can be used as a GPC device, and PLgel, 5 μm, MIXED-D (manufactured by Polymer Laboratories) or TSKgel Super AW series (manufactured by Tosoh Corporation) can be used as a column. Tetrahydrofuran, 1,2,4-trichlorobenzene, N,N-dimethylformamide (with 0.01N lithium bromide added), etc. can be used as a developing solvent, and the flow rate is preferably 0.5 to 1.5 milliliters / minute. An RI detector or the like can be used for detection, and the measurement can be performed under conditions such as a sample injection concentration of 0.5 to 1.5 milligrams / milliliter and an injection amount of 0.1 to 1.0 microliter. The mass average molecular weight can be determined as a polystyrene equivalent value.

[0045] (Molecular weight distribution of urethane resin (Mw / Mn)) The molecular weight distribution (Mw / Mn) of the urethane resin is preferably 4 to 12, more preferably 4.5 to 10, and further preferably 5 to 8. Mw represents the mass average molecular weight, and Mn represents the number average molecular weight. When the molecular weight distribution of the urethane resin is within the above range, the cohesive force and adhesive force are strengthened, and the substrate adhesion and hot lamination strength become good. Note that Mw, Mn, and Mw / Mn can be determined by gel permeation chromatography (GPC) as described above.

[0046] In order to set the molecular weight distribution (Mw / Mn) of the urethane resin within the above range, there are methods for appropriately selecting the urethane synthesis raw materials and the solid content mass ratio in the urethane resin synthesis, the dropping speed of reactive raw materials such as polyisocyanate in the synthesis reaction, the stirring speed and shape of the stirring blade, and the reaction temperature.

[0047] Furthermore, when carrying out a chain extension reaction, it is effective to control the dropping speed and temperature range to a certain range, particularly when reacting polyamine with urethane prepolymer. Reaction temperature control is important, and it is preferable to control it to a range of 50 to 130°C in the synthesis of urethane prepolymer, and it is preferable to control it to a range of 10 to 50°C when reacting polyamine with urethane prepolymer. In addition, setting the charging ratio of the reaction raw materials to an appropriate ratio is also effective in keeping the molecular weight distribution within a predetermined range. Examples of the charging ratio include the NCO / OH ratio, which is the ratio of the hydroxyl groups of the polyol and hydroxy acid, and the isocyanate groups of the polyisocyanate, and the amino group / NCO ratio, which is the ratio of the amino groups of the polyamine and the isocyanate groups of the urethane prepolymer. In order to control the molecular weight distribution, it is preferable to use the above-mentioned reaction terminator for the purpose of preventing excessive polymerization reaction.

[0048] (Isocyanate-based hardener) In the packaging material of the present invention, in order to further improve the hot lamination strength and the adhesion to the substrate, the white printed layer and / or the light-shielding printed layer preferably contain a cured product derived from an isocyanate-based curing agent. That is, the white ink forming the white printed layer and / or the light-shielding ink forming the light-shielding printed layer preferably contain an isocyanate-based curing agent. When the urethane resin in the ink has a hydroxyl group, an amino group or other active hydrogen group, the ink crosslinks with the active hydrogen group, and when the urethane resin does not have the active hydrogen group, the ink crosslinks with itself only with the isocyanate-based curing agent, thereby improving the laminate strength.

[0049] The mass average molecular weight of the isocyanate-based curing agents used in conventional packaging materials is small, less than 500, and they are mostly low molecular weight compounds. However, although this is not a problem if it is simply used in packaging materials, when pearl pigments, metal flakes, etc. are included as pigment components, the cohesive force is insufficient and the characteristics are not satisfactory. In addition, there are concerns that low molecular weight compounds may migrate into the substrate, ink layer, or adhesive layer.

[0050] Therefore, in the present invention, the mass average molecular weight of the isocyanate curing agent is preferably 500 to 8000, more preferably 600 to 6000, and even more preferably 700 to 4000. The molecular weight distribution (Mw / Mn) of the isocyanate curing agent is preferably 2 to 5, more preferably 2.2 to 4.5, and even more preferably 2.5 to 4. When the mass average molecular weight and Mw / Mn are within the above ranges, it is believed that the cohesive force and adhesive force are strengthened by the action with the urethane resin, improving the adhesion to the substrate and the hot lamination strength.

[0051] As the isocyanate-based curing agent, polyisocyanates including adduct type polyisocyanates (adduct bodies), biuret type polyisocyanates (biuret bodies), isocyanurate type polyisocyanates (isocyanurate bodies) and the like are suitable, and examples of the adduct bodies, biuret bodies and isocyanurate bodies include adduct bodies obtained by reacting trimethylolpropane or other polyols with diisocyanates, biuret bodies in which diisocyanates are dimerized and linked by biuret bonds, and isocyanurates obtained by cyclic trimerization reaction of diisocyanates. The diisocyanate may be selected from the above diisocyanates and used, and among them, preferred examples include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hydrogenated diphenylmethane diisocyanate (hydrogenated MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate, xylylene diisocyanate (XDI), hydrogenated xylylene diisocyanate (hydrogenated XDI), etc. Adduct type polyisocyanates, biuret type polyisocyanates, and isocyanurate type polyisocyanates may be used in combination, and may also be used in combination with other polyisocyanates.

[0052] In order to set the mass average molecular weight and molecular weight distribution (Mw / Mn) of the isocyanate-based curing agent in the above range, it is effective to appropriately set the selection of diisocyanate, polyol, etc., the solid content mass ratio, the dripping speed of reactive raw materials such as polyisocyanate in the synthesis reaction, the stirring speed, the shape of the stirring blade, and the reaction temperature in the isocyanate-based curing agent synthesis. In addition, it is effective to set the dripping speed and temperature range control in a constant range when reacting polyamine and polyisocyanate to set the molecular weight distribution in a predetermined range. In addition, it is also effective to set the charging ratio of the reactive raw materials to an appropriate ratio. The charging ratio includes, for example, the NCO / OH ratio, which is the ratio of the isocyanate groups of polyol and polyisocyanate, and the amino group / NCO ratio, which is the ratio of the amino group of polyamine and the isocyanate group of polyisocyanate. Control of the reaction temperature is important, and in synthesis using polyol and polyisocyanate, it is preferable to control it between 50 and 130°C, and in the reaction of polyamine and polyisocyanate, it is preferable to control it in the range of 10 to 50°C. In addition, it is preferable to set the solid content during the reaction to 40 to 80 mass%. As the reaction solvent, it is preferable to use ethyl acetate, normal propyl acetate, and other ester-based organic solvents.

[0053] The mass ratio of the urethane resin to the isocyanate-based curing agent (urethane resin:isocyanate-based curing agent) is preferably 99:1 to 60:40, more preferably 98:2 to 65:35, and even more preferably 95:5 to 70:30. When a combined resin described below is used in addition to the urethane resin, the mass ratio of the total amount of the urethane resin and combined resin to the isocyanate-based curing agent (total amount of resin:isocyanate-based curing agent) is preferably 99:1 to 60:40, and even more preferably 95:5 to 70:30. Within this range, the effects of crosslinking of the ink and adhesion to the substrate are particularly good, and the substrate adhesion and laminate strength are improved.

[0054] <Concomitant Resin> The white printing layer and / or the light-shielding printing layer preferably contain a co-used resin together with the urethane resin. Examples of the co-used resin include polyolefin resins such as polyethylene resins and chlorinated polypropylene resins, poly(meth)acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, polystyrene resins, styrene-butadiene copolymers, vinylidene fluoride resins, polyvinyl alcohol resins, polyvinyl acetal resins, polyvinyl butyral resins, polybutadiene resins, polyester resins, polyamide resins, alkyd resins, epoxy resins, unsaturated polyester resins, thermosetting poly(meth)acrylic resins, melamine resins, urea resins, phenolic resins, xylene resins, maleic acid resins, cellulose resins such as nitrocellulose, ethyl cellulose, acetyl butyl cellulose, and ethyloxyethyl cellulose, rubber resins such as chlorinated rubber and cyclized rubber, petroleum resins, and natural resins such as rosin and casein. Among them, at least one resin selected from vinyl chloride copolymer resin, cellulose-based resin and rosin-based resin is preferred, and vinyl chloride copolymer resin is even more preferred.

[0055] The vinyl chloride copolymer resin is preferably a vinyl chloride-vinyl acetate copolymer resin, a vinyl chloride-acrylic copolymer resin, a vinyl chloride-vinyl acetate-acrylic copolymer resin, or the like. The mass average molecular weight of the vinyl chloride copolymer resin is preferably 5,000 to 100,000, more preferably 5,000 to 50,000. The content of the constituent unit derived from the vinyl acetate monomer in 100 mass% of the solid content of the vinyl chloride copolymer resin is preferably 70 to 95 mass%. The glass transition temperature of the vinyl chloride copolymer resin is preferably 50°C to 90°C. The vinyl chloride copolymer resin preferably has a hydroxyl group, and the hydroxyl value is preferably 10 to 200 mgKOH / g. This is because the reactivity with the isocyanate-based curing agent is improved, and the hydroxyl group is preferably derived from a hydroxyl group derived from a vinyl alcohol unit or an acrylic monomer having a hydroxyl group.

[0056] In each of the white printed layer and the light-shielding printed layer, the mass ratio of the urethane resin to the combined resin (urethane resin: combined resin) is preferably 95:5 to 30:70, and more preferably 90:10 to 40:60, because this improves the adhesion of the ink to the substrate, the coating properties, the laminate strength, etc.

[0057] (Liquid medium) The white ink forming the white printed layer and the light-shielding ink forming the light-shielding printed layer may contain an organic solvent, water, or other liquid medium. Although not limited thereto, suitable organic solvents include toluene and other aromatic organic solvents, methyl ethyl ketone and other ketone-based organic solvents, ethyl acetate, normal propyl acetate, and other ester-based organic solvents, ethanol, isopropanol, normal propanol, and other alcohol-based organic solvents. Water may be contained, and when an organic solvent is used as the main liquid medium, the water content in the ink is preferably 10% by mass or less.

[0058] (Additives) The white ink forming the white printed layer and the light-shielding ink forming the light-shielding printed layer may further contain any additives as necessary, such as fillers, stabilizers, plasticizers, antioxidants, light stabilizers such as ultraviolet absorbers, dispersants, thickeners, drying agents, lubricants, antistatic agents, crosslinking agents, etc.

[0059] (Other ink layers) In the present invention, the other ink layer refers to a printed layer formed from a printing ink that does not contain the above-mentioned light-shielding pigment. The other ink layer may be located between the substrate and the white printed layer, between the white printed layer and the light-shielding printed layer, or between the light-shielding printed layer and the adhesive layer. From the viewpoint of enhancing the design of the packaging material, it is also preferable that the other ink layer is a colored ink layer formed from a colored ink.

[0060] Suitable printing inks include conventional screen inks, gravure inks, flexographic inks, inkjet inks, offset inks, and others. For example, printing inks described in JP-A-2005-298618, JP-A-2006-299136, JP-A-2009-249388, JP-A-2013-127038, JP-A-2017-19991, JP-A-2006-131844, JP-A-2013-40248, JP-A-2007-231148, JP-A-2006-257302, etc. can be used. However, the present invention is not limited to these. Among them, the use of gravure inks, flexographic inks, and inkjet inks is preferred, and the use of gravure inks and / or flexographic inks is even more preferred.

[0061] <Base material> The substrate serves as the substrate on the outer layer side of the packaging material, and is preferably made of a light-transmitting material so that the printed layer can be visually recognized from the outside. The substrate is preferably a plastic film, and specifically includes polyolefin resins such as polyethylene (PE) and polypropylene (PP), cyclic polyolefin resins, polystyrene resins, acrylonitrile-styrene copolymer (AS) resins, acrylonitrile-butadiene-styrene copolymer (ABS) resins, poly(meth)acrylic resins, polycarbonate resins, polyvinyl alcohol resins, ethylene-vinyl alcohol copolymer (EVOH), saponified ethylene-vinyl ester copolymers, polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN), polyamide resins such as various nylons (Ny), polyurethane resins, acetal resins, cellulose resins, and polyvinylidene chloride resins (PVDC). The substrate may be uniaxially or biaxially stretched. It may also be a composite film in which two or more of the above resin films are laminated. It may also be in a form in which a metal oxide such as silica or alumina is vapor-deposited.

[0062] The thickness of the substrate is not particularly limited and can be appropriately set depending on the application of the packaging material, but is usually preferably about 5 to 50 μm, more preferably 10 to 30 μm.

[0063] The substrate preferably has a total light transmittance of 85% or more, more preferably 90% or more, as measured in accordance with JIS K7361-1: 1997. The substrate also preferably has a haze of 1.5% or less, more preferably 1.0% or less, and even more preferably 0.5% or less, as measured in accordance with JIS K7136: 2000.

[0064] <Formation of white printed layer and light-shielding printed layer> The white printed layer and the light-shielding printed layer can be suitably formed on the substrate using the white ink and the light-shielding ink by a printing method such as screen printing, offset printing, flexographic printing, dry offset printing, gravure printing, inkjet printing, etc. Among these, gravure printing or flexographic printing is more preferable.

[0065] <Gravure printing> (Photogravure version) The gravure plate is a cylindrical metal plate, and recesses for each color are made by engraving, etching, or laser. There are no restrictions on the use of engraving and laser, and they can be set arbitrarily according to the pattern. The number of lines used is appropriately 100 to 300 lines, and the higher the number of lines, the finer the printing. The thickness of the printing layer is preferably 0.1 μm to 100 μm. (gravure printing machine) One printing unit in the gravure printing press is equipped with the gravure plate and doctor blade. There are many printing units, and printing units corresponding to organic solvent-based printing inks and picture inks can be set, and each unit has an oven drying unit. Printing is performed by rotary printing, and a roll-to-roll printing method is used. The type of plate and the type of doctor blade are appropriately selected according to the specifications.

[0066] <Flexographic printing> (Flexographic plate) Plates used in flexographic printing include photosensitive resin plates that utilize ultraviolet curing with a UV light source, and elastomer material plates that use a direct laser engraving method. Regardless of the method for forming the image part of the flexographic plate, the screening line count of the plate is 75 lpi or more. Any sleeve or cushion tape can be used to attach the plate. (Flexographic printing machine) Flexographic printing machines include CI type multi-color flexographic printing machines and unit type multi-color flexographic printing machines, and ink supply methods include chamber methods and two-roll methods, and an appropriate printing machine can be used.

[0067] <Lamination processing> The packaging material of the present invention can be obtained, for example, by providing an adhesive layer on the printed layer of a printed matter obtained by printing ink on a substrate, and laminating it with a sealant or an intermediate substrate layer (laminating). Representative examples of lamination include extrusion lamination, dry lamination, non-solvent lamination, and the like. Extrusion lamination is a method in which an anchor coating agent is applied as an adhesive assistant on the printed layer of a printed matter, and molten polyethylene resin, molten polypropylene resin, or the like is extruded thereon and simultaneously laminated with a sealant. The dry lamination method and non-solvent lamination method are methods in which an adhesive is applied and dried on the printed layer of a printed matter, and laminated with a sealant by thermocompression. The difference between the dry lamination method and the non-solvent lamination method is whether or not an organic solvent or other volatile medium is contained.

[0068] <Adhesive layer> The adhesive layer is preferably an anchor coating agent layer made of an anchor coating agent in extrusion lamination, and is preferably a reactive urethane adhesive layer in dry lamination or non-sol lamination.

[0069] (Anchor coating layer) The anchor coating agent used as an adhesive in extrusion lamination is selected from, for example, solvent-soluble or water-soluble polyester resins, isocyanate resins, urethane resins, acrylic resins, polyvinyl alcohol resins, ethylene vinyl alcohol resins, vinyl modified resins, epoxy resins, imine resins, oxazoline group-containing resins, modified styrene resins, modified silicone resins, alkyl titanates, etc., which can be used alone or in combination of two or more. In addition, various additives such as curing agents, catalysts, stabilizers, initiators, etc. may be added to the anchor coating agent layer depending on the resin used.

[0070] The anchor coating agent layer can usually be made to have a thickness of about 5 nm to 5 μm. The anchor coating agent layer having such a thickness can be formed on the surface of the printing layer with a uniform thickness that suppresses internal stress. The more preferred thickness of the anchor coating agent layer is 10 nm to 1 μm. In order to improve the coatability and adhesiveness of the anchor coating agent layer, the surface of the printed layer may be subjected to a corona treatment or the like prior to the formation of the anchor coating agent layer.

[0071] (Reactive urethane adhesive layer) The adhesive layer used during dry lamination or non-solvent lamination processing is preferably a reactive urethane-based adhesive layer consisting of a reactive urethane-based adhesive with a polyol base and a curing agent that is an isocyanate compound, and in particular, it is preferably a solvent-free (non-solvent) urethane-based adhesive layer or a dry laminate-type urethane-based adhesive layer containing an organic solvent.

[0072] (Polyol base) Suitable examples of the polyol used in the polyol base include polyester polyol, polyether polyol, polylactone polyol, polycarbonate polyol, polyolefin polyol, castor oil polyol, hydrogenated castor oil polyol, dimer diol, and hydrogenated dimer diol. Among these, polyester polyol, polyether polyol, castor oil polyol, and hydrogenated castor oil polyol are more preferred, and polyester polyol and castor oil polyol are even more preferred.

[0073] The polyol used in the polyol base resin means a resin containing two or more terminal hydroxyl groups, and those having a urethane bond derived from a reaction with an isocyanate compound are also suitable.

[0074] The mass average molecular weight of the polyol base is preferably 2000 to 100000, more preferably 10000 to 80000, and even more preferably 20000 to 50000. The molecular weight distribution (Mw / Mn) of the polyol base is preferably 1.5 to 20.0, and more preferably 2.0 to 15.0, because this improves the leveling property during adhesive coating and the adhesion between each layer.

[0075] In the adhesive layer, the content of the polyol base agent is preferably 70 to 95% by mass, and more preferably 80 to 90% by mass.

[0076] (Polyester polyol) The polyester polyol is preferably a polyester polyol which is a condensation product of a diol and a dibasic acid.

[0077] (Diol) Suitable examples of the diol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol. The polyester polyol can be used alone or in combination of two or more kinds. Also usable are diols obtained by ring-opening reaction of cyclic esters (lactones, etc.).

[0078] The diol preferably includes both a branched diol and a linear diol. The linear diol is a diol having two or more atoms, such as alkylene glycol, dialkylene glycol, trialkylene glycol, and other diols. The branched diol is a diol in which at least one hydrogen atom of the hydrocarbon group of an alkylene glycol is substituted with a non-hydrogen atom.

[0079] The linear diol imparts crystallinity, while the branched diol imparts flexibility; the right balance between these two properties ensures that the urethane adhesive coating after the two-component curing process is tough, resulting in high lamination strength and heat resistance.

[0080] Examples of the branched diol include 2-butyl-2-ethyl-1,3-propanediol (hereinafter also referred to as BEPG), 2-methyl-1,3-propanediol (hereinafter also referred to as MPO), 3-methyl-1,5-pentanediol (hereinafter also referred to as MPD), neopentyl glycol (hereinafter also referred to as NPG), 1,2-propylene glycol (hereinafter also referred to as PG), 2,4-diethyl-1,5-pentanediol, 1,3-butanediol, dipropylene glycol, and the like. At least one branched diol selected from NPG and PG is particularly preferred.

[0081] The linear diol is preferably an alkylene glycol, and examples of such compounds include ethylene glycol (also written as EG), diethylene glycol, 1,3-propanediol (also written as 1,3-PD), 1,4-butanediol (also written as 1,4-BD), 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,4-butynediol, 1,4-butylenediol, diethylene glycol, and triethylene glycol. Among these, linear diols having 8 or less carbon atoms, preferably 6 or less carbon atoms, are preferred, such as EG, 1,3-PD, 1,4-BD, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, etc. From the viewpoint of physical properties, EG is particularly preferred.

[0082] In addition, the branched diol units and the linear diol units may each be present in one polyester polyol, or a polyester polyol containing only branched diol units and a polyester polyol containing only linear diol units may be used as a mixture raw material. Approximately the same effect can be obtained.

[0083] (Dibasic acid) Suitable dibasic acids include adipic acid, phthalic anhydride, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, pimelic acid, azelaic acid, sebacic acid, suberic acid, glutaric acid, 1,4-cyclohexyl dibasic acid, dimer acid, hydrogenated dimer acid, etc. Among these, adipic acid, succinic acid, and sebacic acid are more preferred, and sebacic acid is even more preferred.

[0084] The content of sebacic acid is preferably 10 to 70 mass %, and more preferably 20 to 60 mass %, of the total amount of dibasic acids.

[0085] The dibasic acid preferably further contains an aromatic dibasic acid such as isophthalic acid. The content of the aromatic dibasic acid in the total amount of the dibasic acids is preferably 25 to 90 mass%, more preferably 40 to 80 mass%.

[0086] Furthermore, a polyol having three or more hydroxyl groups and a polycarboxylic acid having three or more carboxyl groups can be used in combination as raw materials for the polyester polyol.

[0087] In addition, a part of the hydroxyl groups of the polyester polyol may contain a structural unit derived from trimellitic anhydride and / or trimellitic ester anhydride. Partially acid-modified polyols that have been esterified with trimellitic anhydride and / or trimellitic ester anhydride are preferred. Partial acid modification provides excellent adhesive strength, hot water resistance, acid resistance, and oil resistance, and does not cause deterioration in appearance due to unintentional folding during stacking after retort. Furthermore, even when highly acidic or oily foods are filled as the contents of the packaging bag, the adhesive strength is prevented from decreasing, which contributes to maintaining strength over time.

[0088] The polyester polyol may be a reaction product with a polyisocyanate, in which case the polyester polyol has a hydroxyl group at the end. As the polyisocyanate, the polyisocyanate described in the explanation of "urethane resin" is preferably used.

[0089] (Castor oil polyol) The castor oil polyol is not particularly limited, and known castor oil, castor oil derivatives, ricinoleic acid, and ricinoleic acid polyols, etc., can be used. One type may be used alone, or two or more types may be used in combination.

[0090] Examples of castor oil derivatives include dehydrated castor oil, hydrogenated castor oil which is a hydrogenated product of castor oil, castor oil fatty acid, dehydrated castor oil fatty acid, castor oil fatty acid condensate, 5 to 50 moles of ethylene oxide adduct of castor oil, ricinoleic acid polyol, and castor oil-based polyol.

[0091] Among them, from the viewpoint of the stability of the production quality of the polyol, the acid value of the castor oil polyol is preferably in the range of 0.1 to 5.0 mgKOH / g, more preferably in the range of 0.1 to 2.0 mgKOH / g, and further preferably in the range of 0.1 to 1.0 mgKOH / g. From the viewpoint of various resistances, the content of the castor oil polyol is preferably 3 to 80 mass% based on the total mass of the polyol.

[0092] (Polyether polyol) Suitable examples of polyether polyols include polyalkylene glycols such as polyethylene glycol, polytrimethylene glycol, polypropylene glycol, polytetramethylene glycol, and polybutylene glycol; polyethylene glycol / polypropylene glycol block copolymers; and propylene oxide / ethylene oxide random polyethers. From the viewpoint of coatability due to the viscosity effect during adhesive coating, polyether polyols containing structural units derived from polypropylene glycol are preferred. The number average molecular weight of the polyether glycol is preferably 400 to 10,000, and more preferably 400 to 5,000.

[0093] In addition, an addition polymer obtained by addition polymerization of an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran to a low molecular weight polyol initiator such as water, ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, or sucrose may be used as the polyether polyol. Examples of the addition polymer include propylene glycol propylene oxide adducts, glycerin propylene oxide adducts, sorbitol-based propylene oxide adducts, and sucrose-based propylene oxide adducts.

[0094] (Isocyanate compounds) In the reactive urethane adhesive, the isocyanate compound used as a curing agent is preferably a diisocyanate or a urethane prepolymer which is a reaction product of a diisocyanate and a polyol, and various known aromatic, aliphatic or alicyclic diisocyanates can be used as the diisocyanate. For example, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylsilyl diisocyanate, tetra ... Representative examples include methylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group. These can be used alone or in combination of two or more kinds.

[0095] The content of the isocyanate compound in the adhesive layer is preferably from 5 to 30% by mass, and more preferably from 10 to 20% by mass.

[0096] The isocyanate compound can be used without any limitation so long as it functions as a curing agent and contains a group reactive with the hydroxyl group of the polyol.

[0097] As the isocyanate compound, a urethane prepolymer having an isocyanate group at the end can be suitably used.Furthermore, from the viewpoint of preventing yellowing and imparting flexibility for improving adhesion, it is preferable to use aliphatic diisocyanates such as hexamethylene diisocyanate and xylene diisocyanate, and alicyclic diisocyanates such as isophorone diisocyanate, and from the viewpoint of compatibility with retort resistance, it is preferable to use an adduct such as trimethylolpropane, an isocyanurate, a biuret, or another polyisocyanate compound having three or more functional groups.

[0098] In the polyol base material and the isocyanate compound, the ratio NCO / OH of the isocyanate group derived from the isocyanate compound to the hydroxyl group derived from the polyol used as the polyol base material is preferably 1.0 to 8.0, and more preferably 1.5 to 5.0.

[0099] <Sealant> The inner layer of the sealant comes into direct contact with the packaged goods and serves to protect the packaged goods. In order to make the packaging material into a bag shape, it is preferable that the innermost layer of the sealant has heat sealability. Examples of materials constituting the sealant include polyolefin resins such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), ethylene-vinyl acetate copolymer, propylene homopolymer, and ethylene-propylene copolymer, and one or more of these resins can be used. The sealant may be composed of a single layer or may be composed of two or more layers. Note that the sealant is preferably a non-stretched film made of the above resin in order to suppress shrinkage during heat sealing.

[0100] The thickness of the sealant is not particularly limited and is appropriately set depending on the application of the packaging material and the type and properties of the packaged item, but is usually preferably 10 to 200 μm. In the case of a pouch (particularly a retort pouch), the thickness of the sealant is preferably 20 to 150 μm, more preferably 30 to 100 μm.

[0101] <Intermediate base material layer> The packaging material of the present invention may have an intermediate substrate layer between the light-shielding printed layer and the sealant. The intermediate substrate layer is a layer that is provided as necessary for the purpose of improving the strength and processing suitability of the packaging material. Examples of the constituent material of the intermediate substrate layer include a plastic film-like substrate. The substrate can be the same as the substrate used for the substrate layer described above.

[0102] <Manufacturing method of packaging materials> The method for producing a packaging material of the present invention is a method for producing a packaging material having a substrate, a white printed layer, a light-blocking printed layer, an adhesive layer, and a sealant in this order, and includes a step of forming a white printed layer by gravure printing or flexographic printing a white ink, and a step of forming a light-blocking printed layer by gravure printing or flexographic printing the light-blocking ink on the white printed layer, wherein the light-blocking ink contains at least one selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide, the white ink and the light-blocking ink contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, and the dibasic acid contains at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid.

[0103] In order to achieve sufficient light-shielding properties and adhesion to the substrate, the amount of light-shielding ink applied by printing is set to 0.5 g / m in the above-mentioned manufacturing method. 2 More than 5g / m 2 It is preferably less than 0.6 g / m 2 More than 4.9g / m 2 Less than 0.7 g / m, more preferably 0.7 g / m2 More than 4.5g / m 2 Less than or equal to 4g / m 2 The following is the result.

[0104] Furthermore, if necessary, other ink layers may be formed on the substrate, the white printed layer, or the light-shielding printed layer to improve the design. The adhesive layer may be formed by coating on the printed layer, or may be formed by coating on the sealant.

[0105] A preferred embodiment of the method for producing a packaging material of the present invention is, for example, a method in which an adhesive is applied onto the printed layer, and then a sealant is laminated. When the packaging material further has an intermediate substrate layer, a preferred embodiment includes a step of laminating the printed layer and the intermediate substrate layer with an adhesive, and then laminating the intermediate substrate layer and the sealant. The configuration is arbitrary and is not particularly limited.

[0106] The packaging material thus obtained can be cut to a predetermined size, and the edges of the sealants are heat-sealed together to form a bag, to produce a packaging bag. The heat-sealing temperature is preferably 50 to 250°C, and more preferably 80 to 180°C. The heat-sealing pressure is 1 to 5 kg / cm. 2 The above conditions are preferable. One sheet of packaging material may be folded and the edges may be heat sealed, or two or more sheets of packaging material may be heat sealed. Furthermore, the packaging bag made of the packaging material may be one in which all openings are heat sealed after the contents are packaged. EXAMPLES

[0107] The present invention will be described in detail below with reference to examples, but the following embodiments are merely examples of the present invention and the present invention is not limited to these examples. Note that parts and % in the present invention represent parts by mass and % by mass unless otherwise noted.

[0108] <Method for measuring amine value> The amine value is the number of milligrams of potassium hydroxide equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of resin, and was determined according to the following method in accordance with JIS K0070. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg). 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added to the obtained solution as an indicator, and the obtained solution was titrated with 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the endpoint, and the titration amount (A mL) at this point was used to calculate the amine value according to the following (Equation 1). (Equation 1) Amine value = (A x f x 0.2 x 56.108) / S [mg KOH / g]

[0109] (Mass average molecular weight Mw, number average molecular weight Mn and molecular weight distribution Mw / Mn) The weight average molecular weight Mw, number average molecular weight Mn and molecular weight distribution Mw / Mn were determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min

[0110] <Method for measuring hydroxyl value> It was determined according to the method described in JIS K0070.

[0111] <Acid value measurement method> It was determined according to the method described in JIS K0070.

[0112] [Synthesis Example 1-1] (Synthesis of polyester polyol A1) In a round-bottom flask equipped with a stirrer, a thermometer, a water divider and a nitrogen gas inlet tube, 26 parts of 1,3-propanediol (hereinafter also abbreviated as 1,3-PD), 26 parts of neopentyl glycol (hereinafter also abbreviated as NPG), 48 parts of sebacic acid and 0.002 parts of tetrabutyl titanate were charged, and esterification was carried out for 8 hours at 230°C under a nitrogen stream while removing water generated by condensation. After confirming that the acid value of the polyester was 15 or less, the degree of vacuum was gradually increased using a vacuum pump to terminate the reaction. As a result, a polyester polyol (A1) with a number average molecular weight of 2000, a hydroxyl value of 56.1 mgKOH / g and an acid value of 0.3 mgKOH / g was obtained.

[0113] [Synthesis Examples 1-2 to 1-7] (Synthesis of Polyester Polyols A2 to A7) Except for changing the raw materials and charging ratios as shown in Table 1, the same method as in Synthesis Example 1-1 was used to obtain polyester polyols A2 to A7.

[0114] [Comparative Synthesis Example 1-8] (Synthesis of Polyester Polyol A8) A polyester polyol A8 was obtained in the same manner as in Synthesis Example 1-1, except that the raw materials and the charging ratios were changed to those shown in Table 1.

[0115] [Table 1]

[0116] [Synthesis Example 2-1] (Synthesis of polyester-based urethane resin B1) A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with 23.6 parts of polyester polyol A1, 4.68 parts of isophorone diisocyanate (hereinafter also abbreviated as IPDI), 7.5 parts of ethyl acetate, and 0.003 parts of tin 2-ethylhexanoate, and reacted for 6 hours at 120°C under a nitrogen stream. 7.5 parts of propyl acetate was added, and the mixture was cooled to obtain a solution of a terminal isocyanate prepolymer. Next, the obtained solution of isocyanate-terminated prepolymer was gradually added at room temperature to a mixture of 1.60 parts of isophorone diamine (hereinafter also abbreviated as IPDA), 0.12 parts of dibutylamine (hereinafter also abbreviated as DBA), 34 parts of ethyl acetate and 21 parts of isopropyl alcohol (hereinafter also abbreviated as IPA), and then the mixture was reacted at 50°C for 1 hour to obtain a polyester-based urethane resin B1 solution with a solid content of 30%, a mass average molecular weight of 70,000, an amine value of 4 mgKOH / g and a molecular weight distribution (Mw / Mn) of 5.5.

[0117] [Synthesis Examples 2-2 to 2-7] (Synthesis of polyester-based urethane resins B2 to B7) Except for changing the raw materials and charging ratios as shown in Table 2, the same procedure as in Synthesis Example 2-1 was carried out to obtain polyester-based urethane resins B2 to B7.

[0118] [Comparative Synthesis Example 2-8] (Synthesis of polyester-based urethane resin B8) A polyester-based urethane resin B8 was obtained in the same manner as in Synthesis Example 2-1, except that the raw materials and charging ratios were changed to those shown in Table 2.

[0119] [Table 2]

[0120] [White Ink Preparation Example 3-1] (Preparation of Ink C1) 35 parts of titanium oxide, 10 parts of urethane resin B1 solution, and 20 parts of a mixed solvent (n-propyl acetate / IPA = 70 / 30 (mass ratio)) were stirred and mixed and dispersed in a sand mill, and then 20 parts of urethane resin B1 solution and 15 parts of a mixed solvent (propyl acetate / isopropyl alcohol = 70 / 30 (mass ratio)) were stirred and mixed to obtain white ink C1.

[0121] [White Ink Preparation Examples 3-2 to 3-8] (Preparation of Inks C2 to C8) Except for changing the raw materials and charging ratios as shown in Table 3, the same method as in White Ink Preparation Example 3-1 was used to obtain White Inks C2 to C8. Vinyl chloride-vinyl acetate resin solution (vinyl chloride-vinyl acetate copolymer resin with a hydroxyl value of 140 mgKOH / g and a mass average molecular weight of 50,000, a 30% solids solution)

[0122] [Comparative Preparation Examples 3-9 to 3-10] (Preparation of Inks C9 to C10) Except for changing the raw materials and charging ratios as shown in Table 3, the same method as in White Ink Preparation Example 3-1 was used to obtain White Inks C9 to C10. Polyether urethane resin (mass average molecular weight 70,000, solids content 30% solution)

[0123] [Table 3]

[0124] [Light-shielding ink preparation example 4-1] (Preparation of ink D1) 10 parts of carbon black, 10 parts of urethane resin B1 solution, and 20 parts of a mixed solvent (n-propyl acetate / IPA = 70 / 30 (mass ratio)) were stirred and mixed and dispersed using a sand mill, and then 20 parts of the urethane resin B1 solution and 40 parts of a mixed solvent (propyl acetate / isopropyl alcohol = 70 / 30 (mass ratio)) were stirred and mixed to obtain light-shielding ink D1.

[0125] [Light-shielding ink preparation examples 4-2 to 4-11] (Preparation of inks D2 to D11) Except for changing the raw materials and charging ratios as shown in Table 4, light-shielding inks D2 to D11 were obtained in the same manner as in Light-shielding ink Preparation Example 4-1. Vinyl chloride-vinyl acetate resin solution (a 30% solids solution of vinyl chloride-vinyl acetate copolymer resin with a hydroxyl value of 140 mgKOH / g and a mass average molecular weight of 50,000) Zinc oxide: Zinc oxide particles (average particle size 200 nm, primary particle size 25 nm, oil absorption 24 ml / 100 g) Iron oxide: Iron(III) oxide particles (average particle size 200 nm)

[0126] [Comparative Preparation Examples 4-12 to 4-13] (Preparation of Inks D12 to D13) Except for changing the raw materials and charging ratios as shown in Table 4, light-shielding inks D12 to D13 were obtained in the same manner as in Light-shielding Ink Preparation Example 4-1. Polyether urethane resin (mass average molecular weight 70,000, solids content 30% solution)

[0127] [Table 4]

[0128] [Example 1] (Preparation of packaging material E1) White ink C1 and light-shielding ink D1 were gravure printed on the inner surface treatment layer of a 12 μm thick plastic film G1 (polyethylene terephthalate film E5100 manufactured by Toyobo Co., Ltd.) and dried to obtain a printed matter having a printed layer with a dry thickness of 1.5 μm including the white printed layer and the light-shielding printed layer. In addition to a solid plate with a plate depth of 100%, printing was also performed on a gradation plate with a plate depth of 0 to 100% to evaluate trapping properties. Using this printed matter, the adhesion to the substrate and the appearance were evaluated.

[0129] Next, 8 parts of polyol resin H1 (TM-250HV, manufactured by Toyo Morton Co., Ltd.) and 1 part of isocyanate compound I1 (CAT-RT86-60, manufactured by Toyo Morton Co., Ltd.) were mixed, and ethyl acetate was added to adjust the non-volatile content to 30% to prepare a laminate adhesive solution, which was then applied onto the printed layer, dried, and laminated with an intermediate substrate layer J1 (oriented nylon (Ny), thickness 15 μm) using a laminator. Next, the laminate adhesive solution was applied to the surface of the intermediate substrate layer, dried, and laminated with a sealant K1 (CPP, unoriented polypropylene film, thickness 60 μm, surface corona discharge treatment) using a laminator, and the mixture was kept at 40 ° C. for 1 day to prepare a packaging material E1. The packaging material E1 of Example 1 has, from the outer layer side, a substrate, a white printed layer, a light-shielding printed layer, a first adhesive layer, an intermediate substrate layer, a second adhesive layer, and a sealant, in this order.

[0130] [Examples 2 to 23] (Preparation of packaging materials E2 to E23) The printed matter of Examples 2 to 23 and packaging materials E2 to 23 were obtained in the same manner as in Example 1, except that the raw materials and inks having the compounding ratios shown in Table 5 were used. In Examples 15, 16, and 17, an isocyanate curing agent (TLA-100, isocyanurate type manufactured by Asahi Kasei Corporation, solid content 70 mass%) was mixed with the ink so that the mass ratio of the ink to the isocyanate curing agent was ink / isocyanate curing agent = 100 / 1, and printing was performed.

[0131] [Comparative Examples 1 to 5] (Preparation of Packaging Materials F1 to F5) The printed matters and packaging materials F1 to F5 of Comparative Examples 1 to 5 were obtained in the same manner as in Example 1, except that the raw materials and inks having the blending ratios shown in Table 6 were used.

[0132] (Measurement and Evaluation) The following measurements and evaluations were carried out on the printed matter and packaging materials of the Examples and Comparative Examples. The results are shown in Tables 5 and 6.

[0133] (Light blocking property) For the packaging materials obtained in the Examples and Comparative Examples, the maximum transmittance in the 380 to 780 nm region was measured using a UV3600 ultraviolet-visible-near infrared spectrophotometer manufactured by Shimadzu Corporation to evaluate the light blocking ability in the visible region. <Evaluation criteria> 5 (Excellent): Maximum transmittance is less than 1.0% 4 (Good): Maximum transmittance is 1.0% or more, but less than 2.0% 3 (Acceptable): Maximum transmittance is 2.0% or more and less than 3.0% 2 (Not acceptable): Maximum transmittance is 3.0% or more and less than 4.0% 1 (Poor): Maximum transmittance is 4.0% or more Incidentally, 3 to 5 is within the range where no practical problems arise.

[0134] (Adhesion to substrate) For the prints obtained in the Examples and Comparative Examples, 3 hours after printing, a 12 mm wide adhesive tape (cellophane tape manufactured by Nichiban Co., Ltd.) was applied to the printed surface, and the appearance of the printed surface was visually judged when the tape was quickly peeled off. The judging criteria were as follows: <Evaluation criteria> 5 (Excellent): The ink film on the printed surface does not peel off at all. 4 (Good): The area of ​​the ink film peeling off is between 1% and 5%. 3 (Acceptable): The area of ​​the ink film peeling is between 5% and 20%. 2 (Not acceptable): The area of ​​the ink film peeling off is between 20% and 50%. 1 (Poor): The ink film peels off by 50% or more. Incidentally, 3 to 5 is within the range where no practical problems arise.

[0135] (Appearance (trapping ability)) The appearance (trapping property) of the overlapping portion of the white ink layer / light-shielding ink layer of the printed matter obtained in the examples and comparative examples was evaluated using a microscope (VHX-5000) manufactured by Keyence Corporation. The evaluation was performed on the gradation printed matter. It should be noted that Comparative Examples 4 and 5 were not evaluated because they did not have the overlapping portion. <Evaluation criteria> 5 (Excellent): Print unevenness occurs at less than 70% plate depth. 4 (Good): Print unevenness occurs at a plate depth of 70% or more but less than 80%. 3 (OK): Print unevenness occurs at a plate depth of 80% or more but less than 90%. 2 (Not acceptable): Print unevenness occurs when the plate depth is 90% or more but less than 100%. 1 (Poor): All the overlapping light-shielding inks are halftone dots and do not spread at all. Incidentally, 3 to 5 is within the range where no practical problems arise.

[0136] (Hot lamination strength) The packaging materials obtained in the examples and comparative examples were cut into 15 mm widths, and the printed layer was peeled off from the substrate surface. The peel strength (lamination strength) was then measured in an environment of 60°C using an Intesco 201 universal tensile tester. <Evaluation criteria> 5 (Excellent): Tensile strength is 1.0N / 15mm or more 4 (Good): Tensile strength is 0.6N / 15mm or more and less than 1.0N / 15mm 3 (Acceptable): Tensile strength is 0.4N / 15mm or more and less than 0.6N / 15mm 2 (Not acceptable): Tensile strength is 0.2N / 15mm or more and less than 0.4N / 15mm 1 (Poor): Tensile strength is less than 0.2N / 15mm Incidentally, 3 to 5 is within the range where no practical problems arise.

[0137] [Table 5]

[0138] [Table 5]

[0139] [Table 6]

[0140] From the above results, the object of the present application could be achieved by using the packaging material of the present invention. Note that when there was no white printed layer or light-shielding printed layer, the light-shielding property or hot lamination strength was inferior, and when the white printed layer and the light-shielding printed layer did not contain a urethane resin containing a structural unit derived from sebacic acid, succinic acid, or a dimer acid-based polyester polyol, at least one of the adhesion to the substrate, the appearance, and the hot lamination strength was inferior.

Claims

1. A packaging material having a substrate, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant in this order, The white printing layer contains a white pigment, the light-shielding printed layer contains at least one pigment selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide, the white printed layer and the light-shielding printed layer contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, The packaging material, wherein the dibasic acid comprises at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid.

2. 2. The packaging material of claim 1, wherein the dibasic acid comprises sebacic acid.

3. The packaging material according to claim 1 or 2, wherein the white printed layer and / or the light-shielding printed layer comprises a cured product derived from an isocyanate-based curing agent.

4. A method for producing a packaging material having a substrate, a white printed layer, a light-shielding printed layer, an adhesive layer, and a sealant in this order, comprising: A step of forming a white printing layer by gravure printing or flexographic printing with white ink; and forming a light-shielding printed layer by gravure printing or flexographic printing a light-shielding ink on the white printed layer, the light-shielding ink contains at least one selected from the group consisting of carbon black, aluminum particles, iron oxide, and zinc oxide; the white ink and the light-shielding ink contain a urethane resin, the urethane resin contains a structural unit derived from a polyester polyol which is a condensation product of a dibasic acid and a diol, The method for producing a packaging material, wherein the dibasic acid comprises at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid.

5. The amount of light-shielding ink applied by printing is 0.5 g / m 2 5g / m or more 2 The method for producing the packaging material according to claim 4, wherein the

Citation Information

Patent Citations

  • Laminate and package

    JP2017202613A

  • White sealant film and package comprising the same

    JP2018020545A

  • Gravure ink for easy-tearing laminate, and easy-tearing laminate

    JP2019199509A

  • Light-shielding printed material, laminate, method for manufacturing light-shielding printed material, method for manufacturing laminate, and packaging bag, lid material, label

    JP6864774B1

  • Reactive adhesive agent, laminated film, and packaging body

    WO2020246241A1

Cited By

  • Laminate, method for manufacturing a laminate, packaging, packaging container

    JP7950616B1