Piezoelectric material film, manufacturing method thereof and vibration power generation element

By manufacturing the piezoelectric material film with controlled parameters, the surface smoothness and electrode accuracy are improved, leading to enhanced performance of vibration power generation elements.

JP2024158525APending Publication Date: 2024-11-08RESEARCH INSTITUTE FOR ELECTROMAGNETIC MATERIALS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023073787
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Low surface smoothness of the piezoelectric material film leads to decreased shape accuracy of comb-teeth electrodes, affecting the performance of vibration power generation elements.

Method used

The piezoelectric material film is manufactured with specific parameters: average crystal grain size of 0.05 to 2.0 μm, average pore diameter of 0.01 to 2 μm, porosity of 0.005 to 0.05 (0.5 to 5%), compressive residual stress of 10 to 300 MPa, and surface roughness Ra of 0.01 to 0.5 μm, using granulated powder with a median diameter of 10 to 100 μm and a coefficient of variation of 0.1 to 0.6, and a deposition method followed by heat-treatment.

Benefits of technology

Improves the surface smoothness and shape precision of the electrodes, enhancing the performance of the vibration power generation element by aligning polarization direction and reducing the need for noble metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158525000001_ABST
    Figure 2024158525000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a piezoelectric material film, etc., capable of attaining improvement of surface smoothness.SOLUTION: On a surface of a substrate 10, an as-deposited film is formed by an aerosol deposition method using a granulated powder of a piezoelectric ceramic material as a raw material powder. The granulated powder has a median diameter D50 included in a range of 10 to 100 μm and a variation coefficient CV value included in a range of 0.1 to 0.6. Heat treatment is performed on the as-deposited film so as to include an average crystal grain diameter of a piezoelectric material film 20 in a range of 0.05 to 2.0 μm, include an average pore diameter in a range of 0.5 to 2 μm, include porosity in a range of 0.01 to 0.05 (0.5 to 5%), include a compression residual stress in a range of 30 to 300 MPa, and include surface roughness Ra in a range of 0.05 to 0.3 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piezoelectric material film having piezoelectricity, a method for manufacturing the piezoelectric material film, and a vibration power generating element using the piezoelectric material film. [Background technology]

[0002] The present inventor has proposed a vibration power generation element that can reduce costs while improving characteristics and mechanical robustness (see, for example, Patent Document 1). This vibration power generation element includes a substrate made of an elastically deformable metal that is supported in a cantilevered state by a support member and extends with the support member as a reference, a piezoelectric material film formed on the substrate via a dielectric material film, and a first comb-tooth electrode and a second comb-tooth electrode formed on the piezoelectric material film. A plurality of first comb-tooth portions constituting the first comb-tooth electrode and a plurality of second comb-tooth portions constituting the second comb-tooth electrode are arranged so as to be alternately adjacent to each other in the longitudinal direction of the substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-010828 Summary of the Invention [Problem to be solved by the invention]

[0004] However, if the surface of the piezoelectric material film is not smooth, the shape precision of the first comb-tooth electrode and the second comb-tooth electrode may decrease, which may result in a decrease in the performance of the vibration power generation element.

[0005] Therefore, an object of the present invention is to provide a method for producing a piezoelectric material film that can improve the surface smoothness. [Means for solving the problem]

[0006] The piezoelectric material film of the present invention is The average grain size is in the range of 0.05 to 2.0 μm. The average pore size is in the range of 0.01 to 2 μm. The porosity is in the range of 0.005 to 0.05 (0.5 to 5%). The compressive residual stress is in the range of 10 to 300 MPa, and The surface roughness Ra is in the range of 0.01 to 0.5 μm.

[0007] The method for producing the piezoelectric material film of the present invention includes the steps of: forming an as-deposited film on a surface of a substrate by an aerosol deposition method using, as a raw material powder, a granulated powder of a piezoelectric ceramic material having a median diameter D50 in the range of 10 to 100 μm and a coefficient of variation CV value in the range of 0.1 to 0.6; and heat treating the as-deposited film.

[0008] According to the method of this configuration, as the raw material powder when forming an as-deposited film by the aerosol deposition method, granulated powder (secondary particles) of a piezoelectric ceramic material having a median diameter D50 in the range of 10 to 100 μm and a coefficient of variation CV value (= standard deviation / D50) in the range of 0.1 to 0.6 is used, instead of primary particles of the piezoelectric ceramic material. This improves the surface smoothness so that the surface roughness Ra of the piezoelectric material film obtained as a result of heat treatment of the as-deposited film falls in the range of 0.01 to 0.5 μm.

[0009] The vibration power generating element of the present invention is A substrate made of an elastically deformable metal, the substrate being supported in a cantilevered state by a support member and extending with respect to the support member; a piezoelectric material film formed on the substrate via a dielectric material film; a first electrode and a second electrode arranged so as to be able to apply a voltage to the piezoelectric material film; The average crystal grain size of the piezoelectric material film is in the range of 0.05 to 2.0 μm, the average pore diameter is in the range of 0.01 to 2 μm, the porosity is in the range of 0.005 to 0.05 (0.5 to 5%), the compressive residual stress is in the range of 10 to 300 MPa, and the surface roughness Ra is in the range of 0.03 to 0.5 μm.

[0010] According to the vibration power generating element having this configuration, the smoothness of the surface of the piezoelectric material film is improved, so that the shape precision of each of the first electrode and the second electrode is improved, and thus the performance of the vibration power generating element is improved.

[0011] In the vibration power generating element having the above configuration, the first electrode is constituted by a first comb-teeth electrode, the second electrode is constituted by a second comb-teeth electrode, the first comb-tooth electrode and the second comb-tooth electrode are arranged such that a plurality of first comb-tooth portions constituting the first comb-tooth electrode and a plurality of second comb-tooth portions constituting the second comb-tooth electrode are alternately adjacent to each other in a longitudinal direction of the substrate, a width b of each of the first comb tooth portion and the second comb tooth portion is smaller than a thickness t1 of the piezoelectric material film, a ratio r=(ε1 / ε2) of the dielectric constant ε1 of the piezoelectric material film to the dielectric constant ε2 of the dielectric material film is within a range of 50 to 300; The thickness t1 of the piezoelectric material film is in the range of 10 to 50 μm, The thickness t2 of the dielectric material film is in the range of 1 to 3 μm, The distance a between the first comb tooth portion and the second comb tooth portion is within a range greater than 2t1 and smaller than t1+rt2.

[0012] In the vibration power generating element having this configuration, a dielectric material film is formed between the substrate and the piezoelectric material film (ferroelectric material film). Therefore, when a voltage is applied between the first comb-tooth electrode and the second comb-tooth electrode, it is possible to prevent the electric field component parallel to the thickness direction of the piezoelectric material film from becoming the main component. Therefore, when an electric field sufficiently stronger than the coercive electric field of the piezoelectric material film is applied between at least a part of the first electrode (or the first comb-tooth portion of the first comb-tooth electrode) and at least a part of the first electrode (or the second comb-tooth portion of the second comb-tooth electrode) adjacent to each other on the piezoelectric material film, it is possible to align the direction of spontaneous polarization inside the piezoelectric material film in a surface direction perpendicular to the thickness direction of the piezoelectric material film or in the extension direction of the substrate.

[0013] This allows the piezoelectric material film to function as a piezoelectric body with polarization oriented in the plane direction. Then, stress is applied to the piezoelectric material film in parallel with the polarization direction in response to bending deformation of the metal substrate constituting the cantilever beam, which enables a voltage to be generated between the first comb electrode having a plurality of first comb teeth and the second comb electrode having a plurality of second comb teeth due to the piezoelectric longitudinal effect.

[0014] In this way, with the vibration power generation element of this configuration, it is possible to form a piezoelectric layer by forming electrodes only on the film surface of the ferroelectric material film, and it is possible to perform heat treatment without using precious metals as electrodes. In addition to the above, it goes without saying that the improvement of the surface smoothness and film quality also contributes to the improvement of the transverse effect characteristics that align the polarization direction in the film thickness direction. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a top view of the vibration power generating element according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the vibration power generation element taken along the line II-II in FIG. [Diagram 3] FIG. 4 is a schematic diagram showing an electric field in a piezoelectric material film when a voltage is applied between comb-tooth electrodes. [Figure 4A] FIG. 4 is an explanatory diagram of particle size distribution of secondary particles. [Figure 4B] FIG. 2 is an explanatory diagram of the particle size distribution of primary particles. [Figure 5A] FIG. 13 is a diagram showing the surface properties of a piezoelectric material film derived from an AD film using secondary particles. [Figure 5B] FIG. 13 is a diagram showing the surface properties of a piezoelectric material film derived from an AD film using primary particles. [Figure 6] FIG. 11 is a diagram illustrating the configuration of a vibration power generating element according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] (composition) The vibration power generation element according to one embodiment of the present invention shown in Figures 1 and 2 comprises a substrate 10, a piezoelectric material film 20 formed on the substrate 10 via a dielectric material film 102, and a first comb-tooth electrode 41 and a second comb-tooth electrode 42 formed on the piezoelectric material film 20.

[0017] (substrate) The substrate 10 is made of, for example, a flexible or elastically deformable, generally rectangular metal plate material having a thickness of 20 to 200 μm. The substrate 10 is preferably made of heat-resistant stainless steel containing Al, and a dielectric material film 102 having a thickness of 1 μm or more and mainly composed of aluminum oxide (Al2O3) is formed on the surface. This dielectric material film 102 can prevent the components of the substrate 10 and the piezoelectric material film 20 from diffusing, even when the piezoelectric material film 20 is subjected to a heat treatment together with the substrate 10.

[0018] (Fixing method) The substantially rectangular plate-like substrate 10 is joined or adhered to a support member 11 at one end of its lower surface (the other main surface opposite to the one main surface on which the piezoelectric material film 20 is formed), so that the substrate 10 is supported in a cantilevered state by the support member 11 and extends in a first specified direction (X direction) with the support member 11 as a reference. The support member 11 may be constituted by a resin clamp that holds the substrate 10 on which the piezoelectric material film 20 is formed, or a mechanical fixing mechanism such as a base and screws for attaching the substrate 10 to the base.

[0019] (Piezoelectric materials) From the viewpoint of its application in a living body and the environmental load at the time of disposal, the piezoelectric material film 20 is preferably made of a lead-free piezoelectric ceramic material. x Na 1-x )NbO3 system, (Bi 0.5 Na 0.5 )TiO3 system, (Bi 0.5 K 0.5 ) It is composed of a thin film of lead-free piezoelectric material whose main component is TiO3.

[0020] (Composition of piezoelectric and dielectric material films) The thickness t1 of the piezoelectric material film 20 is adjusted to be within the range of 10 to 50 μm, for example. This is because if the thickness t1 of the piezoelectric material film 20 exceeds 50 μm, mechanical damage such as cracks is likely to occur in the piezoelectric material film 20 due to bending deformation of the substrate 10. Also, if the thickness t1 of the piezoelectric material film 20 is less than 10 μm, the power generation energy decreases.

[0021] It is preferable to form the dielectric material film 102 having a dielectric constant ε2 lower than the dielectric constant ε1 of the piezoelectric material film 20. This is because, during polarization processing of the piezoelectric material film 20, the electric field strength in the surface direction (direction parallel to the main surface) is smaller than the coercive electric field E c This is to prevent the electric field component in the thickness direction (Z direction) of the piezoelectric material film 20 from becoming the main component when a voltage is applied between the first comb tooth electrode 41 and the second comb tooth electrode 42, and therefore between the adjacent first comb tooth portion 412 and second comb tooth portion 422.

[0022] The thickness t2 of the dielectric material film 102 is adjusted to fall within the range of 0.5 to 3 μm. This is to facilitate its formation while achieving the effect of controlling the electric field components. In Fig. 3, the electric field direction components in the piezoelectric material film 20 when a voltage is applied between the adjacent first comb tooth portion 412 and second comb tooth portion 422 are diagrammatically shown by arrows pointing in the corresponding direction.

[0023] The average crystal grain size of the piezoelectric material film 20 is in the range of 0.05 to 2.0 μm. The average crystal grain size of the piezoelectric material film 20 is preferably in the range of 0.1 to 1.5 μm, and more preferably in the range of 0.3 to 1.5 μm.

[0024] The average pore size of the piezoelectric material film 20 is in the range of 0.01 to 2 μm. The average pore size of the piezoelectric material film 20 is preferably in the range of 0.1 to 1.8 μm, and more preferably in the range of 0.3 to 1.5 μm.

[0025] The porosity of the piezoelectric material film 20 is in the range of 0.005 to 0.05 (0.5 to 5%). It is preferable that the porosity of the piezoelectric material film 20 is in the range of 0.01 to 0.04 (1 to 4%).

[0026] The compressive residual stress of the piezoelectric material film 20 is in the range of 10 to 300 MPa. The compressive residual stress of the piezoelectric material film 20 is preferably in the range of 30 to 250 MPa, and more preferably in the range of 50 to 150 MPa. The compressive residual stress of the as-deposited film calculated from the half-width and peak shift of the XRD peak is relatively large. The as-deposited film is heat-treated to promote the growth of crystal grains, improving the crystallinity of the piezoelectric material film 20 (or the unfinished film during heat treatment), so that the compressive residual stress is slightly smaller than that of the as-deposited film. However, when the heat treatment temperature of the as-deposited film is increased, the difference in the linear expansion coefficient between the substrate 10 and the piezoelectric material film 20 (or the unfinished film during heat treatment) becomes a thermal stress, and the compressive residual stress of the piezoelectric material film 20 increases. When the heat treatment temperature of the as-deposited film is further increased and the grain size of the piezoelectric material film 20 (or the unfinished film during heat treatment) becomes larger, domains with different spontaneous polarization (long axis direction of the lattice) are formed within the grains, and the residual stress is alleviated.

[0027] The surface roughness Ra of the piezoelectric material film 20 is in the range of 0.03 to 0.5 μm. If the surface roughness Ra is less than 0.03 μm, it is difficult to form a piezoelectric material film 20 with such high surface smoothness, and if the surface roughness Ra exceeds 0.5 μm, the surface smoothness of the piezoelectric material film 20 is low, which affects the shape accuracy of the first comb-tooth electrode 41 and / or the second comb-tooth electrode 42. The surface roughness Ra of the piezoelectric material film 20 is preferably in the range of 0.05 to 0.3 μm, and more preferably in the range of 0.1 to 0.25 μm.

[0028] (Explanation of comb electrodes) The first comb-tooth electrode 41 has a first base portion 411 extending in the extension direction (+X direction) of the substrate 10 based on a support point by the support member 11, and a plurality of first comb-tooth portions 412 extending from the first base portion 411 in a direction (-Y direction) perpendicular to the extension direction of the substrate 10. The second comb-tooth electrode 42 has a second base portion 421 extending in the extension direction (+X direction) of the substrate 10 based on a support point by the support member 11, and a plurality of second comb-tooth portions 422 extending from the second base portion 421 in a direction (+Y direction) perpendicular to the extension direction of the substrate 10. The first comb-tooth electrode 41 and the second comb-tooth electrode 42 are made of a conductor such as a metal. Since the first comb-tooth electrode 41 and the second comb-tooth electrode 42 do not cover the entire upper surface of the piezoelectric material film 20, the material costs are reduced even if the first comb-tooth electrode 41 and / or the second comb-tooth electrode 42 are made of a precious metal.

[0029] (Relationship between piezoelectric vibration energy generation and dimensional parameters) The beam length L of the substrate 10 is the length of the range in which the multiple first comb tooth portions 412 and the multiple second comb tooth portions 422 exist in the longitudinal direction (X direction) of the substrate 10, and the overlap length w of the first comb tooth portions 412 and the second comb tooth portions 422 in the lateral direction (Y direction) of the substrate 10. e , the piezoelectric constant d of the piezoelectric longitudinal effect of the piezoelectric material film 20 33, the thickness t1 and dielectric constant ε1 of the piezoelectric material film 20, the dielectric constant ε0 of a vacuum, the width b of each of the first comb-tooth portion 412 and the second comb-tooth portion 422, the distance a between the first comb-tooth portion 412 and the second comb-tooth portion 422, and the stress T applied to the piezoelectric material film 40 due to bending deformation in the extension direction of the substrate 10 and the generated energy U corresponding to the potential difference between the first comb-tooth electrode 41 and the second comb-tooth electrode 42 corresponding to the stress T. 33 There is a relationship between them, as expressed by equation (01).

[0030] U 33 ={d 33 2 / (2ε1ε0)}(w e t1L)T 2 {a / (a+b)} ‥(01).

[0031] Relational formula (01) represents the generated energy due to the piezoelectric stiffness effect since the substrate 10 has a cantilever structure in which stress is applied in a direction parallel to the polarization axis of the piezoelectric material film 20 (second specified direction).

[0032] The vibration power generation element as a piezoelectric transverse effect element has a structure in which a piezoelectric material film is sandwiched between a pair of electrodes from above and below. The polarization direction is the thickness direction of the piezoelectric material film, while the direction in which stress is applied to the piezoelectric material film is perpendicular to the polarization direction. This is a piezoelectric transverse effect element, and the power generation energy of the piezoelectric transverse effect is calculated when the piezoelectric constant in the relational expression (01) is d 31 Therefore, the term a / (a+b) is unnecessary. Therefore, the generated energy U 31 is expressed by the relation (02).

[0033] U 31 ={d 31 2 / (2ε1ε0)}T 2 (w e t1L) ‥(02).

[0034] In the case of piezoelectric ceramics, the piezoelectric constant d 33 ≒2×d 31Therefore, when the same stress is applied to the substrate 10 and the piezoelectric material film 20, the generated energy U due to the piezoelectric stiffness effect is 33 is the power generation energy U due to the piezoelectric transverse effect. 31 For U to be greater than 1, the inequality 4a / (a+b)>1 must hold, based on equation (01) and equation (02). That is, U 33 >U 31 In order for this relationship to hold, a relationship expressed by the inequality b / a<3 must hold between the electrode width b of each of the first comb tooth portion 412 of the first comb tooth electrode 41 and the second comb tooth portion 422 of the second comb tooth electrode 42 and the spacing a between the first comb tooth portion 412 and the second comb tooth portion 422.

[0035] (Effect of dielectric material film) By noting that the dielectric constant ε2 of the dielectric material film 102 (diffusion barrier layer) when the piezoelectric material film 20 formed on the substrate 10 is heat-treated is smaller than the dielectric constant ε1 of the piezoelectric material film 20, the piezoelectric material film 20 formed on the substrate 10 can be made to function as a piezoelectric longitudinal effect element as a whole by controlling the thickness t2.

[0036] The ratio r=(ε1 / ε2) of the dielectric constant ε1 of the piezoelectric material film 20 to the dielectric constant ε2 of the dielectric material film 102 is within the range of 50 to 300. The width b of each of the first comb-tooth portion 412 and the second comb-tooth portion 422 (the size in the longitudinal direction of the substrate 10) is smaller than the thickness t1 of the piezoelectric material film 20.

[0037] During polarization processing for aligning the polarization direction of the piezoelectric material film 20 formed on the main surface of the metal substrate 10 via the dielectric material film 102 in an in-plane direction (X direction), a voltage is applied between the first comb-tooth electrode 41 and the second comb-tooth electrode 42 formed on the surface of the piezoelectric material film 20. At this time, a potential difference is also generated between the first comb-tooth electrode 41 and the second comb-tooth electrode 42 and the substrate 10. For this reason, it is necessary to align the direction of the electric field between the first comb-tooth electrode 41 and the second comb-tooth electrode 42 in the in-plane direction of the piezoelectric material film 20.

[0038] By providing the dielectric material film 102 between the substrate 10 and the piezoelectric material film 20, the effective distance between the substrate 10 and the first comb-tooth electrode 41 and the second comb-tooth electrode 42 (or the effective thickness of the piezoelectric material film 20) becomes (1+n) times the thickness t1 of the piezoelectric material film 20 (n=(ε1 / t1) / (ε2 / t2)). In other words, the thickness t1 of the piezoelectric material film 20 appears to be increased by (1+n) times due to the presence of the dielectric material film 102. For example, when (ε1 / ε2)=50, t1=50 μm, and t2=1 μm, the effective distance (1+n)t1 between the substrate 10 and the comb-tooth electrodes 41, 42 becomes twice the thickness t1 of the piezoelectric material film 20 (n=1). Furthermore, when (ε1 / ε2)=300, t1=10 μm, and t2=3 μm, the effective distance (1+n)t1 between the substrate 10 and the comb-tooth electrodes 41, 42 is 91 times the thickness t1 of the piezoelectric material film 20 (n=90).

[0039] According to FEM analysis, when the electrode width b is smaller than the thickness t1 of the piezoelectric material film 20 and the electrode interval a is smaller than 2t1, the X-direction component E of the electric field intensity E between the first comb-tooth electrode 41 and the second comb-tooth electrode 42 is x becomes non-uniform depending on the depth from the upper surface of the piezoelectric material film 20 (the boundary surface between the piezoelectric material film 20 and the first comb-tooth electrode 41 and the second comb-tooth electrode 42). For example, at the midpoint between the adjacent first comb-tooth portion 412 and the second comb-tooth portion 422, the X-direction components E of the electric field E of the piezoelectric material film 20 at depths of 0.25t1, 0.50t1, and 0.75t1 from the upper surface of the piezoelectric material film 20 (the boundary surface between the piezoelectric material film 20 and the first comb-tooth electrode 41 and the second comb-tooth electrode 42) are x(0.25) , E x(0.50) and E x(0.75) It was confirmed that each of the above is non-uniform. Here, "non-uniform" means that max(E x(0.25) , E x(0.50) , E x(0.75) ) / min(E x(0.25) , E x(0.50) , E x(0.75) ) exceeds 1.20.

[0040] On the other hand, according to the FEM analysis, when the electrode width b is smaller than the thickness t1 of the piezoelectric material film 20 and the electrode interval a is included in the range of 2t1 or more, the X-direction component E of the electric field strength E between the first comb-shaped electrode 41 and the second comb-shaped electrode 42 x becomes substantially uniform regardless of the depth from the upper surface of the piezoelectric material film 20 (the interface between the piezoelectric material film 20 and the first comb-shaped electrode 41 and the second comb-shaped electrode 42). This condition is expressed by the relational expression (11).

[0041] b < t1 ≤ a / 2 ‥(11).

[0042] For example, at the intermediate point between the adjacent first comb-shaped portions 412 and second comb-shaped portions 422, the X-direction components E of the electric field E of the piezoelectric material film 20 at depths of 0.25t1, 0.50t1, and 0.75t1 from the upper surface of the piezoelectric material film 20 (the interface between the piezoelectric material film 20 and the first comb-shaped electrode 41 and the second comb-shaped electrode 42) x(0.25) , E x(0.50) and E x(0.75) were each confirmed to be non-uniform. Here, "substantially uniform" means that max(E x(0.25) , E x(0.50) , E x(0.75) ) / min(E x(0.25) , E x(0.50) , E x(0.75) ) is included in the range of 1.0 to 1.20.

[0043] Therefore, under the condition of b < t1, in order to make the directions of the spontaneous polarization of the piezoelectric material film 20 uniform in the thickness direction by the polarization treatment, the electric field E between the adjacent first comb-shaped portions 412 and second comb-shaped portions 422 may be adjusted so that the magnitude of the X-direction component E of the electric field E of the piezoelectric material film 20 is equal to or greater than the coercive electric field E x . c (Definition of the electric field strength E and explanation of the electric fields E

[0044] x , E z z ) When a voltage V is applied between the first comb-tooth electrode 41 and the second comb-tooth electrode 42, the electric field strength E between the first comb-tooth portion 412 and the second comb-tooth portion 422, which are adjacent to each other at a distance a in the longitudinal direction of the substrate 10, is V / a. The component of the electric field in the thickness direction (Z direction) of the piezoelectric material film 20 is defined as E z The component of the electric field in the longitudinal direction (X direction) of the piezoelectric material film 20 is E x Then, from the viewpoint of aligning the polarization direction of the piezoelectric material film 20 in the x direction, the X-direction component E x The magnitude of the coercive electric field E c It must be equal to or greater than E x and E z can be simulated using the finite element method.

[0045] (Definition of electric field strength ratio R) Here, the X-direction component E of the electric field E x is the X-direction component E of the electric field at multiple points on the piezoelectric material film 20 between the first comb tooth portion 412 and the second comb tooth portion 422 (for example, multiple depth points from the surface of the piezoelectric material film 20 between the first comb tooth portion 412 and the second comb tooth portion 422). x For example, the condition for aligning the polarization direction of the piezoelectric material film 20 in the x direction is E x >E c In the case of a comb-shaped electrode pattern, the size of Ex is smaller than E, so E x E c In order to perform the polarization process with E set to a value larger than the electric field strength in the structure in which the film is sandwiched between electrodes, the magnitude of E must be larger than the electric field strength in the structure in which the film is sandwiched between electrodes.

[0046] Therefore, a sufficiently large E x The electric field strength E is the manufacturing condition for applying c In reality, E may be selected so that an electric field is applied to the piezoelectric material film 20 without discharging between the first comb-tooth electrode 41 and the second comb-tooth electrode 42. x Since the size of E varies depending on the electrode pattern dimensions of the comb-tooth electrode and the shape and dimensions of the piezoelectric material film 20, x E cIt is necessary to determine the shapes of the electrodes and the piezoelectric material film 20 so that the electric field strength ratio R=E x If we define / E as E ≥ 3E c In order to meet the manufacturing requirements, the electric field strength ratio R = E x The condition that / E is 1 / 3 or more is adopted.

[0047] Here, the distance a between the first comb-tooth portion 412 and the second comb-tooth portion 422 is designed to be smaller than the effective distance (1+n)t1 or t1+r·t2 (r=(ε1 / ε2)) between the substrate 10 and the comb-tooth electrodes 41, 42. This condition is expressed by relational expression (12).

[0048] a < (1 + n) t1 = t1 + r t2 ... (12).

[0049] This is because, when the distance a between the first comb tooth portion 412 and the second comb tooth portion 422 is equal to or greater than the effective distance (1+n)t1 between the substrate 10 and the comb tooth electrodes 41 and 42, the X-direction component E x The electric field strength ratio R = (E x / E) is less than 1 / 3.

[0050] (Manufacturing method) A method for manufacturing a vibration power generating element according to one embodiment of the present invention will be described.

[0051] (Deposition by AD method) In a vacuum, a lead-free piezoelectric ceramic powder having a particle size of, for example, about 1 μm, specifically, barium titanate (BaTiO3) powder as a raw material powder is sprayed from a nozzle onto a substantially rectangular plate-shaped substrate 10 made of heat-resistant stainless steel containing Al, and is caused to collide with the substrate 10, thereby forming a film by aerosol deposition (AD). A piezoelectric material film 20 having a desired thickness of 10 to 50 μm is formed by this AD method. From the viewpoint of improving the surface smoothness of the as-deposited film (AD film) and therefore the surface smoothness of the piezoelectric material film 20, the substrate 10 may be subjected to a physical and / or chemical surface treatment so that the surface roughness Ra of the substrate 10 is in the range of 0.01 to 0.5 μm (or 0.1 to 0.4 μm, or 0.15 to 0.3 μm).

[0052] When an unpolished substrate (Rax (x: direction perpendicular to rolling) = 0.25 μm, Ray (y: direction of rolling) = 0.12 μm)) was used as the substrate 10, the Rax of the 3 μm-thick barium titanate film as the piezoelectric material film 20 was 0.233 μm and the Ray was 0.239 μm. In contrast, when a polished substrate (Rax = 0.032 μm, Ray = 0.034 μm) was used as the substrate 10, the Rax of the 3 μm-thick barium titanate film as the piezoelectric material film 20 was 0.211 μm and the Ray was 0.233 μm.

[0053] The raw powder used here is not primary particles, but secondary particles (granulated powder) obtained by granulating the primary particles by a spray-drying method. During the spray-drying, about 1 to 2% of PVA was added as a binder. FIG. 4A shows the particle size distribution (particle diameter distribution) of the secondary particles. The particle size distribution of the secondary particles shown in FIG. 4A has a median diameter D50 in the range of 10 to 100 μm (preferably 10 to 80 μm, more preferably 10 to 60 μm) and a coefficient of variation CV value (=standard deviation / D50) in the range of 0.1 to 0.6 (preferably 0.2 to 0.5, more preferably 0.25 to 0.4). FIG. 4B shows the particle size distribution of the primary particles for reference.

[0054] It is preferable that the barium titanate (BaTiO3) powder is produced by a method that reduces the amount of residual BaCO3. If BaCO3 remains, CO2 gas is generated during the heat treatment process, which can cause film peeling (peeling of the piezoelectric material film 20 from the substrate 10).

[0055] (Flexibility and adhesion strength of AD membrane) The film formed by the AD method (as-deposited film) is firmly bonded to the substrate 10 due to the anchor effect. This strong bond is maintained even in the piezoelectric material film 20 in its final state. This reduces the possibility that the piezoelectric material film 20 will crack or peel off from the substrate 10 when the vibration power generation element is bent and deformed. Thus, the AD method is a suitable method for obtaining a piezoelectric material film 20 that has flexibility.

[0056] (Adjustment of crystal grain size of piezoelectric material film) The microstructure of the as-deposited film is smaller than the grain size of the raw material powder (primary particles) used in the AD method, and is finely sized to about several tens of nm, so that the piezoelectricity is low, and therefore it is necessary to promote the growth of crystal grains by heat treatment. On the other hand, since destruction of ceramics generally occurs at grain boundaries, a microcrystalline structure with many grain boundaries is preferable to improve the strength of the piezoelectric material film 20. From the viewpoint of improving the piezoelectric properties, the as-deposited film is heat-treated at 800 to 1200°C for 1 to 4 hours so that the average crystal grain size of the crystals constituting the piezoelectric material film 20 is 100 nm or more, and from the viewpoint of ensuring the strength of the piezoelectric material film 20, the average crystal grain size of the crystals constituting the piezoelectric material film 20 is 2000 nm or less.

[0057] In this case, the heat treatment temperature (pattern of change in heat treatment temperature over time) and heat treatment time are controlled so that the average crystal grain size of the piezoelectric material film 20 falls within the range of 0.05 to 2.0 μm, the average pore diameter falls within the range of 0.01 to 2 μm, the porosity falls within the range of 0.005 to 0.05, the compressive residual stress falls within the range of 10 to 300 MPa, and the surface roughness Ra falls within the range of 0.03 to 0.3 μm. The average pore diameter and porosity were determined by image processing of electron microscope photographs.

[0058] FIG. 5A shows a photograph showing the surface state of the piezoelectric material film 20 of the Example derived from an as-deposited film (AD film) made using secondary particles of barium titanate having the particle size distribution shown in FIG. 4A. FIG. 5B shows a photograph showing the surface state of the piezoelectric material film 20 of the Reference Example derived from an as-deposited film (AD film) made using primary particles of barium titanate having the particle size distribution shown in FIG. 4B. As shown in FIG. 5B, the surface of the piezoelectric material film 20 of the Reference Example has crater-like dents having an extent of about 50 to 100 μm derived from the primary particles. On the other hand, as shown in FIG. 5A, the surface of the piezoelectric material film 20 of the Example does not have such dents and has high surface smoothness.

[0059] (Formation of dielectric material film (diffusion barrier layer)) In the heat treatment process, a dielectric material film 102 containing an oxide of Al (Al2O3) as a main component is formed between the substrate 10 and the piezoelectric material film 20. This allows the dielectric material film 102 to function as a diffusion barrier layer that suppresses component diffusion between the stainless steel substrate 10 and the piezoelectric material film 20, and prevents the substrate 10 and the piezoelectric material film 20 from reacting when heat treated at a high temperature of 900°C or more. The dielectric material film 102 having a thickness of 1 μm or more may be formed in advance on the main surface of the stainless steel substrate 10, or the piezoelectric material film 20 may be directly formed on the main surface of the stainless steel substrate 10 containing Al, and then the piezoelectric material film 20 may be heat treated to form the dielectric material film 102.

[0060] (Formation of comb-tooth electrodes) A first comb-tooth electrode 41 and a second comb-tooth electrode 42 are formed on the piezoelectric material film 20 after the heat treatment. The first comb-tooth electrode 41 and the second comb-tooth electrode 42 are made of a conductive film and have a thickness of, for example, 0.4 to 0.6 μm. The conductive film can be formed by, for example, a sputtering method or a vapor deposition method. The first comb-tooth electrode 41 and the second comb-tooth electrode 42 are not limited to an Au film, and may be a metal film made of other metals, such as a Cu film or a Cu alloy film, or may have a multi-layer structure such as Au / Ni / Ti.

[0061] (Polarization treatment) The as-deposited film and the heat-treated film obtained by heat-treating the as-deposited film are polycrystalline structures, so that the direction of electric polarization is random as it is. Therefore, in order to align the direction of polarization, a voltage (predetermined voltage) equal to or greater than the electric field strength at which polarization is inverted is applied to the heat-treated film between the first comb-tooth electrode 41 and the second comb-tooth electrode 42. If the dielectric material film 102 is not formed between the substrate 10 and the piezoelectric material film 20, and if the thickness t2 of the dielectric material film 102 is excessively small compared to the thickness t1 of the piezoelectric material film 20, the thickness direction (Z direction) component of the electric field of the piezoelectric material film 20 tends to be the main component, so it is desirable that the thickness t2 of the dielectric material film 102 is 1 μm or more. By making the dielectric constant ε2 of the dielectric material film 102 (diffusion barrier layer) smaller than the dielectric constant ε1 of the piezoelectric material film 20, the surface direction component or the second specified direction component (Y direction component) of the electric field in the piezoelectric material film 20 becomes the main component.

[0062] In addition, in order to form a dielectric material film 102 having a thickness of more than 3 μm on the main surface of a substrate 10 made of a metal such as stainless steel, the thin film formation method has a slow film formation rate, which is not realistic in terms of production efficiency. Although it is possible to form a dielectric material film 102 having a thickness of more than 3 μm by a thick film formation method such as the AD method, from the viewpoint of improving power generation energy, thickening the piezoelectric material film 20 has a greater effect on improving performance than thickening the dielectric material film 102. For this reason, the thickness of the dielectric material film 102 is adjusted to 3 μm or less. In addition, by using a stainless steel base material containing Al as a method for forming the dielectric material film 102, it is possible to form the dielectric material film 102 by thermal oxidation of Al contained in the base material, and the coating grows thick even during the heat treatment process of the piezoelectric material film 20, and the effect of improving the adhesion strength between the piezoelectric material film 20 and the dielectric material film 102 is achieved.

[0063] In this way, a vibration power generating element according to one embodiment of the present invention is manufactured (see FIGS. 1 and 2).

[0064] (Another embodiment of the present invention) The vibration power generating element as another embodiment of the present invention shown in Fig. 6 has a common configuration with the vibration power generating element of the embodiment shown in Fig. 1 and Fig. 2, and the common configuration is designated by the same reference numerals and detailed description thereof is omitted. As shown in Fig. 6, this vibration power generating element includes a substrate 10, a first electrode 410 formed on the substrate 10 via a dielectric material film 102, a piezoelectric material film 20 formed on the first electrode 410, and a second electrode 420 formed on the piezoelectric material film 20. The vibration power generating element is a piezoelectric transverse effect element, and has a structure in which the piezoelectric material film 20 is sandwiched between a pair of electrodes 410 and 420, and the polarization direction is the thickness direction of the piezoelectric material film 20, while the direction in which stress is applied to the piezoelectric material film 20 is perpendicular to the polarization direction. The pair of electrodes 410 and 420 may be made of a metal having a thickness similar to that of the first comb-tooth electrode 41 and / or the second comb-tooth electrode 42 in the embodiment.

[0065] 6, the second electrode 420 is formed in a substantially rectangular shape, but as long as it at least partially faces the first electrode 410, the shape may be any shape, such as a substantially circular shape, a substantially elliptical shape, a substantially parallelogram shape, a substantially trapezoid shape, or a substantially regular N-sided polygon. "Substantially" means that the shape is mathematically exact, excluding minor differences such as rounded corners.

[0066] Instead of the first comb tooth electrode 41 and the second comb tooth electrode 42 in the above embodiment, a first electrode and a second electrode arranged at least partially opposite each other in the longitudinal direction of the substrate 10, such as a first comb tooth portion 412 and a second comb tooth portion 422, may be formed on the surface of the piezoelectric material film 20. [Explanation of symbols]

[0067] 10. Circuit board 11. Support member 20. Piezoelectric material film (ferroelectric material film) 41‥1st comb electrode 42‥Second comb electrode 102...Dielectric material film (diffusion barrier layer) 410‥1st electrode 411‥1st foundation part 412‥1st comb tooth part 420‥Second electrode 421‥Second foundation part 422‥2nd comb teeth part

Claims

1. The average crystal grain size is in the range of 0.05 to 2.0 μm, The average pore size is in the range of 0.01 to 2 μm, The porosity is in the range of 0.005 to 0.05; The compressive residual stress is in the range of 10 to 300 MPa, and Surface roughness Ra is in the range of 0.03 to 0.5 μm Piezoelectric material film.

2. A method for producing the piezoelectric material film according to claim 1, comprising the steps of: forming an as-deposited film on a surface of a substrate by an aerosol deposition method using, as a raw material powder, a granulated powder of a piezoelectric ceramic material having a median diameter D50 in the range of 10 to 100 μm and a coefficient of variation CV value in the range of 0.1 to 0.6; and heat treating the as-deposited film.

3. A substrate made of an elastically deformable metal, the substrate being supported in a cantilevered state by a support member and extending with respect to the support member; a piezoelectric material film formed on the substrate via a dielectric material film; a first electrode and a second electrode arranged so as to be able to apply a voltage to the piezoelectric material film; The average crystal grain size of the piezoelectric material film is in the range of 0.05 to 2.0 μm, the average pore size is in the range of 0.01 to 2 μm, the porosity is in the range of 0.005 to 0.05, the compressive residual stress is in the range of 10 to 300 MPa, and the surface roughness Ra is in the range of 0.03 to 0.5 μm. Vibration power generation element.

4. The vibration power generating element according to claim 3 , the first electrode is constituted by a first comb-teeth electrode, the second electrode is constituted by a second comb-teeth electrode, the first comb-tooth electrode and the second comb-tooth electrode are arranged such that a plurality of first comb-tooth portions constituting the first comb-tooth electrode and a plurality of second comb-tooth portions constituting the second comb-tooth electrode are alternately adjacent to each other in a longitudinal direction of the substrate; The width b of each of the first comb teeth portion and the second comb teeth portion is equal to the thickness t of the piezoelectric material film. 1 Smaller, The dielectric constant ε of the dielectric material film 2 The dielectric constant ε of the piezoelectric material film 1 The ratio r = (ε 1 / ε 2 ) is in the range of 50 to 300, The thickness t of the piezoelectric material film 1 is in the range of 10 to 50 μm, The thickness t of the dielectric material film 2 is in the range of 0.5 to 3 μm, The distance a between the first comb tooth portion and the second comb tooth portion is 2t 1 Greater than and t 1 +rt 2 Included in a smaller range Vibration power generation element.

Citation Information

Patent Citations

  • Vibration power generation element

    JP2022010828A