Glass composition and x-ray radiopaque composition

By integrating rubidium into glass compositions, high X-ray contrastability and low refractive index are achieved, addressing the balance challenge in conventional glass, suitable for dental and optical applications.

JP2024158865APending Publication Date: 2024-11-08GC CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023074448
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional glass compositions face a challenge in achieving both high X-ray contrast properties and a low refractive index, making it difficult to balance these properties effectively.

Method used

Incorporating rubidium (Rb) into the glass composition, which enhances X-ray contrastability while minimizing the increase in refractive index, and optionally combining with other elements like cesium (Cs), silicon (Si), and potassium (K) to maintain chemical durability and adjust refractive index.

Benefits of technology

The glass composition achieves high X-ray contrastability with a refractive index of 1.564 or less, ensuring good X-ray contrast properties and chemical durability, suitable for dental and optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158865000001
    Figure 2024158865000001
  • Figure 2024158865000002
    Figure 2024158865000002
  • Figure 2024158865000003
    Figure 2024158865000003
Patent Text Reader

Abstract

To provide a glass composition capable of yielding glass with both high X-ray radiopacity and low refractive index.SOLUTION: This glass composition contains rubidium (Rb).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass composition and an X-ray contrast composition. [Background technology]

[0002] In the field of dentistry, Cs 2 O, BaO and / or SnO 2 An X-ray opaque glass containing any fluorine is known (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-131457 A Summary of the Invention [Problem to be solved by the invention]

[0004] With conventional glass, as the X-ray contrast property increases, the refractive index also tends to increase, making it difficult to achieve both high X-ray contrast property and a low refractive index.

[0005] An object of the present invention is to provide a glass composition which can provide a glass which has both high X-ray contrast properties and a low refractive index. [Means for solving the problem]

[0006] A glass composition according to one embodiment of the present invention contains rubidium (Rb). Effect of the Invention

[0007] According to one aspect of the present invention, it is possible to provide a glass composition which can give a glass which has both high X-ray contrast properties and a low refractive index. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described in detail.

[0009] The glass composition according to this embodiment contains rubidium (Rb).

[0010] Rubidium (Rb) has an atomic number (number of electrons) of 37, which is approximately the same as that of strontium (Sr), which has an atomic number (number of electrons) of 38 and exhibits high X-ray contrast in glass. Therefore, rubidium (Rb) exhibits high X-ray contrast in glass, equivalent to that of strontium (Sr).

[0011] Here, X-ray contrast is a property in which the shade of an X-ray image changes depending on the amount of X-ray absorption by the object, such as a biological tissue or material, making it possible to visualize or distinguish the object. In particular, in dental treatment, it is necessary to clarify the postoperative treatment area using dental materials, including dental filling materials, and dental materials are required to have X-ray contrast. In dental materials, the resin matrix is ​​an organic material and does not have X-ray contrast, and the filler made of an inorganic material such as glass is responsible for the X-ray contrast. Therefore, X-ray contrast is an important property for dental glass.

[0012] Incidentally, rubidium (Rb) has an effective ionic radius of 152 pm, which is larger than that of strontium (Sr), which has an effective ionic radius of 118 pm. The larger the effective ionic radius, the lower or sparser the electron density within the atom becomes relatively, so rubidium (Rb) can suppress the increase in the refractive index of glass compared to strontium (Sr).

[0013] Furthermore, rubidium (Rb), with an effective ionic radius of 152 pm, is smaller than cesium (Cs), an alkali metal with an effective ionic radius of 167 pm. The smaller the effective ionic radius of an element in the same group, the greater the single bond strength between the alkali metal and oxygen, and the greater the tendency for chemical stability to increase. Therefore, rubidium (Rb) is less likely to reduce the chemical durability (e.g., water resistance) of glass compared to cesium (Cs).

[0014] Rubidium (Rb) is contained in the glass composition in the form of an oxide of rubidium (Rb) (rubidium oxide (Rb 2 O)).

[0015] The content of rubidium (Rb) is not particularly limited, and is, for example, 3 mass% or more, preferably 5 mass% or more, and more preferably 7 mass% or more, calculated as an oxide. The content of rubidium (Rb) calculated as an oxide is rubidium oxide (Rb 2 O) in the glass composition.

[0016] The upper limit of the content of rubidium (Rb) calculated as an oxide is not particularly limited, but from the viewpoint of suppressing a decrease in the chemical durability of the glass composition, the content of rubidium (Rb) is preferably 60 mass % or less, more preferably 50 mass % or less, and further preferably 40 mass % or less.

[0017] In this embodiment, the glass composition contains rubidium (Rb), which can improve the X-ray contrast of the resulting glass. In addition, the refractive index of the resulting glass increases little while maintaining high X-ray contrast, making it easy to control the refractive index. Furthermore, the glass composition contains rubidium (Rb), which makes it difficult for the chemical durability (e.g., water resistance) of the resulting glass to decrease.

[0018] The glass composition of the present embodiment is not particularly limited in type as long as it contains rubidium (Rb). Examples of the glass composition include silicate glass, borate glass, phosphate glass, borosilicate glass, silicophosphate glass, fluorophosphate glass, sulfophosphate glass, soda-lime glass, aluminosilicate glass, and aluminoborosilicate glass.

[0019] Among these, the types of glass compositions are preferably silicate glass, borate glass, and borosilicate glass. Note that the main component of silicate glass is silicon (Si).

[0020] That is, the glass composition of the present embodiment preferably contains silicon (Si). Silicon (Si) is contained in the glass composition in the form of an oxide of silicon (Si) (silicon oxide (SiO 2 )

[0021] The content of silicon (Si) is not particularly limited, and is, for example, preferably 10 mass% or more in terms of oxide, more preferably 15 mass% or more, and further preferably 20 mass% or more. The content of silicon (Si) in terms of oxide is silicon oxide (SiO 2 ) in the glass composition.

[0022] When the content of silicon (Si) calculated as oxide is 20 mass % or more, it becomes possible to adjust the viscosity of the glass composition, and also possible to increase the mechanical strength of the glass composition.

[0023] The upper limit of the content of silicon (Si) calculated as an oxide is not particularly limited. However, since an increase in silicon (Si) in the glass composition hardens the glass melt, from the viewpoint of reducing production costs, the upper limit is preferably 90 mass % or less, more preferably 85 mass % or less, and even more preferably 80 mass % or less.

[0024] The glass composition of the present embodiment may further contain cesium (Cs).

[0025] Cesium (Cs) has an atomic number (number of electrons) of 55, which is almost the same as barium (Ba), which has an atomic number (number of electrons) of 56 and exhibits high X-ray contrast, so it exhibits high X-ray contrast similar to barium (Ba). Therefore, even if cesium (Cs) is mixed with rubidium (Rb), the X-ray contrast of the resulting glass can be improved.

[0026] In addition, cesium (Cs) has an effective ionic radius of 167 pm, which is larger than that of barium (Ba) with an effective ionic radius of 135 pm (the electron density in the atom is low or sparse), so the increase in the refractive index can be suppressed compared to barium (Ba). Therefore, even if cesium (Cs) is mixed with rubidium (Rb), the increase in the refractive index of the resulting glass can be suppressed while maintaining high X-ray contrast.

[0027] Furthermore, although cesium (Cs) has inferior chemical durability (e.g., water resistance) compared to rubidium (Rb), mixing cesium (Cs) with rubidium (Rb) does not cause a decrease in chemical durability due to the inclusion of rubidium (Rb). Therefore, by replacing a part of rubidium (Rb), which has a relatively expensive raw material cost, with cesium (Cs), which has a relatively cheap raw material cost, it is possible to prevent an increase in the manufacturing cost of the glass composition.

[0028] Cesium (Cs) is dissolved in the glass composition as an oxide of cesium (Cs) (Cs oxide (Cs 2 O).

[0029] When cesium (Cs) is contained, the content of cesium (Cs) is not particularly limited, and is, for example, 3 mass% or more, preferably 5 mass% or more, and more preferably 10 mass% or more, calculated as an oxide. The content of cesium (Cs) calculated as an oxide is cesium oxide (Cs 2 O) in the glass composition.

[0030] By making the content of cesium (Cs) calculated as oxide 3% or more by mass, in combination with rubidium (Rb), the X-ray contrast property of the obtained glass can be improved and an increase in the refractive index can be suppressed. The upper limit of the content of cesium (Cs) calculated as oxide is not particularly limited, but from the viewpoint of not decreasing the content of rubidium (Rb), it is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0031] The glass composition of the present embodiment may further contain potassium (K). In the glass composition, potassium (K) is contained in the form of an oxide of potassium (K) (potassium oxide (K 2 O).

[0032] When potassium (K) is contained, the content of potassium (K) is 1 mass% or more and 15 mass% or less, preferably 3 mass% or more and 12 mass% or less, and more preferably 5 mass% or more and 10 mass% or less, calculated as an oxide. The content of potassium (K) calculated as an oxide is potassium oxide (K 2 O) in the glass composition.

[0033] When potassium (K) is contained, the content of potassium (K) calculated as oxide is 1 mass %, which can lower the melting temperature of the glass composition, making it easier to manufacture and process the glass composition and allowing it to be used as a material in various fields. In addition, the content of potassium (K) calculated as oxide is 15 mass % or less, which can suppress a decrease in the chemical durability of the glass composition.

[0034] The glass composition of the present embodiment may further contain sodium (Na). Sodium (Na) is contained in the glass composition in the form of an oxide of sodium (Na) (sodium oxide (Na 2 O).

[0035] When sodium (Na) is contained, the content of sodium (Na) is 1 mass% or more and 15 mass% or less, preferably 1.5 mass% or more and 12 mass% or less, and more preferably 2 mass% or more and 10 mass% or less, calculated as an oxide. The content of sodium (Na) calculated as an oxide is sodium oxide (Na 2 O) in the glass composition.

[0036] When sodium (Na) is contained, the content of sodium (Na) calculated as oxide is 1 mass %, which can lower the melting temperature of the glass composition, making it easier to manufacture and process the glass composition and allowing it to be used as a material in various fields. In addition, the content of sodium (Na) calculated as oxide is 15 mass % or less, which can suppress a decrease in the chemical durability of the glass composition.

[0037] In order to reliably suppress the deterioration of the chemical durability of the glass composition, it is preferable that the glass composition of the present embodiment does not contain at least one of potassium (K) and sodium (Na) in order to reduce the total amount of alkali metals. In this specification, "not containing at least one of potassium (K) and sodium (Na)" means that the glass composition does not substantially contain potassium (K) and / or sodium (Na) except for inevitable impurities.

[0038] When potassium (K) is contained in the glass composition as an inevitable impurity, the content of potassium (K) calculated as oxide is 0.5 mass % or less, preferably 0.3 mass % or less, and more preferably 0.1 mass % or less.

[0039] When sodium (Na) is contained in the glass composition as an inevitable impurity, the content of sodium (Na) is 0.5 mass % or less, preferably 0.3 mass % or less, and more preferably 0.1 mass % or less, calculated as an oxide.

[0040] The glass composition of the present embodiment may contain other elements as long as the object of the present invention is not impaired. Examples of other elements include boron (B), fluorine (F), aluminum (Al), zinc (Zn), strontium (Sr), zirconium (Zr), tin (Sn), barium (Ba), lanthanum (La), and gadolinium (Gd) from the viewpoint of improving X-ray contrast and chemical durability. The other elements, except for fluorine (F), may be present as oxides in the glass composition. The content of the other elements is not particularly limited, and they may be contained in the glass composition at any mass.

[0041] In the glass composition, boron (B) is present in the form of an oxide of boron (B) (boron oxide (B 2 O 3 )

[0042] When boron (B) is contained, the content of boron (B) is not particularly limited, but is preferably 40 mass% or less, more preferably 35 mass% or less, and further preferably 30 mass% or less, calculated as an oxide. The content of boron (B) calculated as an oxide is boron oxide (B 2 O 3 ) in the glass composition.

[0043] When the content of boron (B) calculated as oxide is 40 mass% or less, the melting point of the glass of the glass composition can be lowered and manufacturing can be facilitated. In addition, the lower limit of the content of boron (B) calculated as oxide when boron (B) is contained is not particularly limited, but from the viewpoint of chemical durability and ease of manufacturing of the glass composition, it is preferably 1 mass% or more, more preferably 2 mass% or more, and further preferably 3 mass% or more.

[0044] Fluorine (F) may be present in the glass composition as a fluoride or a fluoride salt.

[0045] When fluorine (F) is contained, the content of fluorine (F) is not particularly limited, but is preferably 6 mass% or less, more preferably 5.5 mass% or less, and further preferably 5 mass% or less. The content of fluorine (F) indicates the mass content of fluorine (F) as a simple substance in the glass composition.

[0046] The refractive index of the resulting glass can be adjusted by making the content of fluorine (F) 6% by mass or less. The lower limit of the content of fluorine (F) when fluorine (F) is contained is not particularly limited, but from the viewpoint of reducing the viscosity of the glass composition and improving the handleability of the glass composition, it is preferably 0.1% by mass or more, more preferably 1% by mass or more, and further preferably 2% by mass or more.

[0047] In the glass composition, aluminum (Al) is present in the form of an oxide of aluminum (Al) (aluminum oxide (Al 2 O 3 )

[0048] When aluminum (Al) is contained, the content of aluminum (Al) is not particularly limited, but is preferably 35 mass% or less, more preferably 30 mass% or less, and further preferably 25 mass% or less, calculated as an oxide. The content of aluminum (Al) calculated as an oxide is aluminum oxide (Al 2 O 3 ) in the glass composition.

[0049] By making the content of aluminum (Al) calculated as oxide 35% by mass or less, the chemical durability of the glass composition can be improved and devitrification of the glass can be suppressed. In addition, the lower limit of the content of aluminum (Al) calculated as oxide when aluminum (Al) is contained is not particularly limited, but from the viewpoint of the chemical durability of the glass composition and suppression of devitrification of the glass, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 1% by mass or more.

[0050] Zinc (Zn) may be present in the glass composition as an oxide of zinc (Zn), such as zinc oxide (ZnO).

[0051] When zinc (Zn) is contained, the content of zinc (Zn) is not particularly limited, but is preferably 20 mass% or less, more preferably 15 mass% or less, and further preferably 10 mass% or less, calculated as oxide. The content of zinc (Zn) calculated as oxide indicates the mass content of zinc oxide (ZnO), which is an oxide of zinc (Zn), in the glass composition.

[0052] By making the content of zinc (Zn) calculated as oxide 35% by mass or less, devitrification can be prevented and manufacturing can be facilitated without decreasing the chemical durability of the obtained glass. In addition, when zinc (Zn) is contained, the lower limit of the content of zinc (Zn) calculated as oxide is not particularly limited, but from the viewpoint of the chemical durability of the glass composition and suppressing devitrification of the glass, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more.

[0053] Strontium (Sr) may be present in the glass composition as an oxide of strontium (Sr), such as strontium oxide (SrO).

[0054] When strontium (Sr) is contained, the content of strontium (Sr) is not particularly limited, but is preferably 20 mass% or less, more preferably 15 mass% or less, and further preferably 10 mass% or less, calculated as oxide. The content of strontium (Sr) calculated as oxide indicates the mass content of strontium oxide (SrO), which is an oxide of strontium (Sr), in the glass composition.

[0055] By making the content of strontium (Sr) calculated as oxide 20% by mass or less, it is possible to improve the X-ray contrast property while maintaining a low refractive index of the obtained glass. Note that, when strontium (Sr) is contained, the lower limit of the content of strontium (Sr) calculated as oxide is not particularly limited, but from the viewpoint of improving the X-ray contrast property while maintaining a low refractive index, it is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more.

[0056] Zirconium (Zr) is contained in the glass composition as an oxide of zirconium (Zr) (zirconium oxide (ZrO 2 )

[0057] When zirconium (Zr) is contained, the content of zirconium (Zr) is not particularly limited, but is preferably 20 mass% or less, more preferably 15 mass% or less, and further preferably 10 mass% or less, calculated as an oxide. The content of zirconium (Zr) calculated as an oxide is zirconium oxide (ZrO 2 ) in the glass composition.

[0058] By making the content of zirconium (Zr) calculated as oxide 20% by mass or less, it is possible to improve the X-ray contrast property of the obtained glass and increase the water resistance while maintaining the meltability of the glass. Note that, when zirconium (Zr) is contained, the lower limit of the content of zirconium (Zr) calculated as oxide is not particularly limited, but from the viewpoint of increasing the water resistance while maintaining the X-ray contrast property, it is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more.

[0059] Tin (Sn) is contained in the glass composition as an oxide of tin (Sn) (stannic oxide (SnO 2 )).

[0060] When tin (Sn) is contained, the content of tin (Sn) is not particularly limited, but is preferably 25 mass% or less, more preferably 20 mass% or less, and further preferably 15 mass% or less, calculated as an oxide. The content of tin (Sn) calculated as an oxide is tin oxide (SnO 2 ) in the glass composition.

[0061] By making the content of tin (Sn) calculated as oxide 25% by mass or less, it is possible to maintain the meltability of the glass, improve the X-ray contrast property of the obtained glass, and increase the water resistance. In addition, when tin (Sn) is contained, the lower limit of the content of tin (Sn) calculated as oxide is not particularly limited, but from the viewpoint of improving the water resistance while maintaining the X-ray contrast property, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more.

[0062] Barium (Ba) may be present in the glass composition as an oxide of barium (Ba), such as barium oxide (BaO).

[0063] When barium (Ba) is contained, the content of barium (Ba) is not particularly limited, but is preferably 30 mass% or less, more preferably 25 mass% or less, and further preferably 20 mass% or less, calculated as an oxide. The content of barium (Ba) calculated as an oxide indicates the mass content of barium oxide (BaO), which is an oxide of barium (Ba), in the glass composition.

[0064] By making the content of barium (Ba) calculated as oxide 30% by mass or less, it is possible to improve the X-ray contrast property of the obtained glass while suppressing the decrease in water resistance. In addition, the lower limit of the content of barium (Ba) calculated as oxide when barium (Ba) is contained is not particularly limited, but from the viewpoint of imparting high X-ray contrast property, it is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more.

[0065] In the glass composition, lanthanum (La) is contained in the form of an oxide of lanthanum (La) (lanthanum oxide (La 2 O 3 )).

[0066] When lanthanum (La) is contained, the content of lanthanum (La) is not particularly limited, but is preferably 40 mass% or less, more preferably 45 mass% or less, and even more preferably 30 mass% or less, calculated as an oxide. The content of lanthanum (La) calculated as an oxide is lanthanum oxide (La 2 O 3 ) in the glass composition.

[0067] By making the content of lanthanum (La) calculated as oxide 40% by mass or less, it is possible to improve the X-ray contrast property of the obtained glass and increase the water resistance while maintaining the meltability of the glass. Note that, when lanthanum (La) is contained, the lower limit of the content of lanthanum (La) calculated as oxide is not particularly limited, but from the viewpoint of increasing the water resistance while maintaining the X-ray contrast property, it is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more.

[0068] Gadolinium (Gd) is the oxide of gadolinium (Gd) (Gd 2 O 3 )

[0069] When gadolinium (Gd) is contained, the content of gadolinium (Gd) is not particularly limited, but is preferably 30 mass% or less, more preferably 25 mass% or less, and further preferably 20 mass% or less, calculated as an oxide. The content of gadolinium (Gd) calculated as an oxide is gadolinium oxide (Gd 2 O 3 The mass content in the glass composition is shown.

[0070] By making the content of gadolinium (Gd) calculated as oxide 30% by mass or less, it is possible to improve the X-ray contrast property of the obtained glass while maintaining the meltability of the glass. In addition, when gadolinium (Gd) is contained, the lower limit of the content of gadolinium (Gd) calculated as oxide is not particularly limited, but from the viewpoint of imparting high X-ray contrast property, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more.

[0071] The glass composition of the present embodiment may contain other inevitable impurities, such as nickel (Ni).

[0072] The form of the glass composition is not particularly limited, and may be, for example, a powder (or powder), plate, column, thread, or fiber. When the glass composition is in the form of a powder, it becomes easy to blend and mix each component of the glass composition. When the glass composition is in the form of a plate or column, the glass composition can be used for optical elements (for example, lenses, prisms, filters, etc.).

[0073] The particle size of the powdered glass composition is not particularly limited, but is preferably 0.01 μm to 20 μm in median diameter, more preferably 0.02 μm to 10 μm in median diameter, and further preferably 0.1 μm to 1 μm in median diameter. Here, the particle size means the average particle size defined by the median diameter.

[0074] When the particle size of the glass composition is 0.01 μm or more, the handling property of the glass composition is improved when the glass composition is used as a powder, and when the particle size of the glass composition is 20 μm or less, the mechanical strength of the dental composition obtained when applied to a dental material is improved.

[0075] The glass composition of the present embodiment can make the refractive index (nd) of the glass containing the glass composition equal to or less than 1.564. In this specification, the refractive index (nd) means the refractive index at the D line (light having a wavelength of 589 nm).

[0076] When the refractive index (nd) of the glass composition of the present embodiment is 1.564 or less, when the glass composition is used as a dental composition, the difference in refractive index between the glass composition and a dental resin is small, and the transparency of the dental composition obtained is high. The lower limit of the refractive index (nd) is not particularly limited, but is preferably 1.40 or more as a feasible range, more preferably 1.45 or more, and even more preferably 1.47 or more.

[0077] The glass composition of the present embodiment can provide a glass containing the glass with an X-ray contrast property of 200% or more relative to aluminum. In this specification, the X-ray contrast property refers to the X-ray contrast property measured by a test method for X-ray contrast property of dental materials in accordance with ISO 4049:2019.

[0078] In this embodiment, the X-ray contrast property of the glass containing the glass composition is 200% or more relative to aluminum, so that a glass composition exhibiting good X-ray contrast property can be provided. The upper limit of the X-ray contrast property is not particularly limited, but is preferably 1000% or less relative to aluminum as a feasible range, more preferably 900% or less, and even more preferably 800% or less.

[0079] The use of the glass composition of the present embodiment is not particularly limited, but since the glass composition exhibits high X-ray contrast properties, it can be used as an X-ray contrast composition containing the glass composition.

[0080] In addition, the glass composition of the present embodiment can be used as a dental material (dental composition) by utilizing its high X-ray contrast property. Examples of such dental materials include dental composite resins, dental cements, dental adhesives, dental temporary sealing materials, dental primers, dental coating materials, dental hard resins, dental cutting resin materials, dental temporary restorative materials, dental filling materials, and dentifrices.

[0081] In addition, the dental composition of the present embodiment has high X-ray contrast and transparency for the glass containing the dental composition, so that a dental composition that has both good X-ray contrast and excellent aesthetics can be obtained. In addition, the dental composition of the present embodiment has good X-ray contrast, so that the repaired part can be clearly identified in diagnosis or examination by X-ray images after treatment.

[0082] In addition, the glass composition contained in the dental composition of this embodiment is adjusted to a sufficiently suitable refractive index range, so that the refractive index difference with dental resins is small and the composition can be suitably used for dental materials that require aesthetics (e.g., dental composite resins, dental coating agents, dental hard resins, dental cutting resin materials, etc.).

[0083] Furthermore, the glass composition contained in the dental composition of this embodiment has good chemical durability (particularly, water resistance), and therefore can be suitably used as a general dental material applied in the oral cavity.

[0084] The glass composition of the present embodiment can also be used in fields other than dental materials, for example, optical elements such as optical lenses, prisms, and optical filters, ultraviolet and infrared ray blocking glass, and radiation shielding glass. EXAMPLES

[0085] The present invention will be further described below with reference to examples. In the following, numerical values ​​without units or "%" are based on mass (% by mass) unless otherwise specified.

[0086] <Glass preparation> Glasses (Examples 1-1 to 1-3, Examples 2-1 to 2-4, Examples 3-1 to 3-2, Examples 4-1 to 4-6, Comparative Examples 1-1 to 1-3, and Comparative Example 3-1) were prepared with the compositions shown in Tables 1 to 4. A raw material batch obtained by mixing various raw materials was placed in a platinum crucible, and then was held in an electric furnace preheated to 1400 to 1500°C for 30 to 60 minutes, and poured into a carbon mold to obtain a bulk body. Alternatively, after melting in the same manner, the glass melt was dropped into a water tank to obtain granulated glass. The glass was pulverized in an alumina magnetic mortar to obtain glass powder with a median diameter (average particle size) of 20 to 300 μm.

[0087] The refractive index of the obtained glass powder (glass) was measured. The obtained bulk glass was heated in an electric furnace from room temperature to 600°C at a heating rate of 20°C / min, held at 600°C for 30 minutes, and then slowly cooled to room temperature. The bulk glass after the heat treatment was sliced ​​to obtain slices.

[0088] <Refractive index> A liquid having a specific refractive index and the prepared glass powder were mixed at a ratio of 1:1 (mass ratio) and filled into a transparent tube. Next, the transparent tube was held in front of a white LED, and the color of the transmitted light through the transparent tube was visually observed. Then, the refractive index of the liquid that made the transmitted light through the transparent tube turn green was adopted as the refractive index of the glass powder. Note that when the refractive index of the liquid is lower than that of the glass powder, the color of the transmitted light through the transparent tube becomes blue. Also, when the refractive index of the liquid is higher than that of the glass powder, the color of the transmitted light through the transparent tube becomes red or yellow. The evaluation of the refractive index of the glass was judged to be good when the refractive index was 1.564 or less and bad when the refractive index exceeded 1.564. The results of the refractive index of the glass are shown in Tables 1 to 4.

[0089] <X-ray contrastability> For the obtained glass slice, the X-ray contrastability (relative to Al%) was measured. The X-ray contrastability was measured by the X-ray contrastability test method for dental materials in accordance with ISO 4049:2019. Specifically, the optical density or gray value of a test piece (plate-shaped glass composition) with a thickness Ts (unit: mm) was measured. Next, the thickness Ta (unit: mm) of an aluminum plate showing the same optical density or gray value as the test piece with a thickness Ts was determined. Then, the ratio of Ta to Ts (unit: relative to Al%) was used as the value of the X-ray contrastability. The evaluation of the X-ray contrastability was judged to be good when the aluminum ratio was 200% or more and bad when the aluminum ratio was less than 200%. The results of the refractive index of the glass are shown in Tables 1 to 4.

[0090] <Water resistance> 2.0 g of glass powder (median diameter 20 to 300 μm) was weighed. The glass powder was added to a Duran glass bottle (manufactured by SCHOTT, "Duran" is a registered trademark), and then 50 mL of distilled water was added and shaken. The glass bottle was placed in a thermostatic chamber preheated to 98°C and left to stand for 1 hour. After being removed from the thermostatic chamber, it was allowed to cool to room temperature, and the electrical conductivity of the immersion liquid was measured using an electrical conductivity meter (manufactured by Horiba, Ltd.). In the water resistance test, the amount of ions dissolved from the glass powder into the immersion liquid was measured and evaluated. Therefore, the smaller the amount of ion dissolved, that is, the smaller the evaluation value of water resistance (unit: μS), the better the water resistance of the glass composition was evaluated. Specifically, the evaluation of water resistance was judged to be good when it was 800 μS or less, and poor when it exceeded 800 μS. The results of water resistance are shown in Tables 1, 3, and 4.

[0091] [Table 1]

[0092] [Table 2]

[0093] [Table 3]

[0094] [Table 4]

[0095] As can be seen from Tables 1 to 4, the glass compositions containing rubidium (Rb) had good refractive index, X-ray contrast properties, and water resistance of the resulting glasses (Examples 1-1 to 1-3, Examples 3-1 to 3-2, Examples 4-1 to 4-6).

[0096] In contrast, glass compositions not containing rubidium (Rb) were poor in any one of the refractive index, X-ray contrast property, and water resistance of the resulting glasses (Comparative Examples 1-1 to 1-3, Comparative Example 3-1).

[0097] Furthermore, Table 1 shows that even when Na and Cs are contained, the inclusion of Rb results in excellent physical properties (low refractive index, high X-ray contrast, and high water resistance) (Examples 1-2 and 1-3).

[0098] Furthermore, from Table 2, it was found that as the amount of Rb added increased, the X-ray contrast increased with a slight increase in the refractive index. In other words, by increasing the amount of Rb added, it is possible to improve the X-ray contrast while suppressing the increase in the refractive index. In other words, it was found that the X-ray contrast can be adjusted as desired by changing the amount of Rb added (Examples 2-1 to 2-4).

[0099] Furthermore, from Table 3, by not including Na and K, good water resistance was shown (Examples 3-1 to 3-2). In contrast, when Na was included, the water resistance was deteriorated (Comparative Example 3-1). In other words, it was found that by making the composition free of Na and / or K, the water resistance can be further improved in the glass composition containing Rb.

[0100] Furthermore, from Tables 3 and 4, the glass composition containing Rb, even when combined with elements such as F, Zn, Sn, Sr, Zr, Ba, La, and Gd, had excellent physical properties (low refractive index, high X-ray contrast, and high water resistance) due to the inclusion of Rb. In particular, the inclusion of Sn, Sr, Zr, Ba, La, and Gd further improved the X-ray contrast (Examples 3-1 to 3-2, Examples 4-1 to 4-6). In addition, the inclusion of Sn, Zr, and La improved the X-ray contrast and also improved the water resistance. Furthermore, the inclusion of F and Zn provided a glass composition with a low refractive index while exhibiting both good X-ray contrast and sufficient water resistance (Examples 4-1 and 4-6).

[0101] The above disclosed embodiments include, for example, the following aspects.

[0102] (Appendix 1) A glass composition comprising rubidium (Rb).

[0103] (Appendix 2) 2. The glass composition of claim 1, comprising silicon (Si).

[0104] (Appendix 3) 3. The glass composition according to claim 1 or 2, comprising cesium (Cs).

[0105] (Appendix 4) 4. The glass composition according to claim 1, wherein the glass composition does not contain at least one of potassium (K) and sodium (Na).

[0106] (Appendix 5) 5. An X-ray contrast composition comprising a glass composition according to any one of claims 1 to 4.

[0107] (Appendix 6) A dental composition comprising the X-ray contrast composition described in Appendix 5.

[0108] Although an embodiment of the present invention has been described above, the present invention is not limited to a specific embodiment, and various modifications and changes are possible within the scope of the invention described in the claims.

Claims

1. Including rubidium (Rb), Glass composition.

2. Contains silicon (Si); The glass composition of claim 1 .

3. Contains cesium (Cs) The glass composition of claim 1 .

4. Does not contain at least one of potassium (K) and sodium (Na); The glass composition of claim 1 .

5. The glass composition according to any one of claims 1 to 4, X-ray contrast composition.

6. The radiographic contrast composition according to claim 5, Dental compositions.

Citation Information

Patent Citations

  • CAD / CAM engravable lithium disilicate microcrystalline glass for dentistry and preparation method thereof

    CN107698167A

  • Glass composition

    JP1983208151A

  • Cao-al2o3-p2o5 crystallized glass

    JP1987128947A

  • Glass for ultrasonic delay line

    JP1988166735A

  • Optical functional glass, optical fiber, amplifier and laser

    JP1992160031A