Positive electrode active material and lithium ion secondary battery
A Li-containing oxide with an O2 type structure and controlled I1/I2 ratio, incorporating Mn, Ni, and Co, addresses capacity limitations in conventional O2 type materials, enhancing lithium ion secondary battery performance.
Patent Information
- Application Number
- JP2023074743
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Conventional positive electrode active materials with an O2 type structure have limited capacity.
A positive electrode active material containing a Li-containing oxide with specific elemental composition and crystal structure, characterized by an O2 type structure, reduced X-ray diffraction peak intensity ratio I1/I2 ≤ 0.30, and inclusion of elements like Mn, Ni, and Co, is developed.
The new active material exhibits enhanced capacity due to reduced T#2 type structure intensity, improving lithium ion secondary battery performance.
Smart Images

Figure 2024159021000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a positive electrode active material and a lithium ion secondary battery. [Background technology]
[0002] Positive electrode active materials having an O2 type structure are known. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a part of Na in a Na-containing oxide having a P2 type structure with Li. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-170994 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional positive electrode active materials having an O2-type structure have room for improvement in terms of capacity. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A positive electrode active material comprising a Li-containing oxide, The Li-containing oxide has an O2 type structure, The Li-containing oxide contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O; The X-ray diffraction pattern of the Li-containing oxide is 0≦I 1 / I 2 ≦0.30, Above I 1 is the X-ray diffraction peak intensity originating from the (002) plane of the T#2 structure, Above I2 is the X-ray diffraction peak intensity derived from the (002) plane of the O2-type structure, the positive electrode active material. <Aspect 2> The positive electrode active material of Aspect 1, wherein the Li-containing oxide is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (where 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by the positive electrode active material. <Aspect 3> The positive electrode active material of Aspect 1 or 2, wherein the Li-containing oxide contains at least Li, Mn, Ni, Co, and O as constituent elements, the positive electrode active material. <Aspect 4> A lithium-ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains the positive electrode active material of any one of Aspects 1 to 3, the lithium-ion secondary battery.
Advantages of the Invention
[0006] The positive electrode active material of the present disclosure has an O2-type structure and a large capacity.
Brief Description of the Drawings
[0007] [Figure 1] An example of the flow of a method for manufacturing a Li-containing oxide having an O2-type structure is shown. [Diagram 2] An example of the configuration of a lithium-ion secondary battery is schematically shown. [Diagram 3]1 shows the X-ray diffraction patterns of Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 4] This shows the relationship between I1 / I2 and capacitance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1.Cathode active material The positive electrode active material according to the embodiment includes a Li-containing oxide. The Li-containing oxide has an O2 type structure. The Li-containing oxide includes, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. The X-ray diffraction pattern of the Li-containing oxide has a range of 0≦I 1 / I 2 ≦0.30. 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity originating from the (002) plane of the O2 type structure.
[0009] 1.1 Crystal structure The Li-containing oxide according to the embodiment has at least an O2 type structure (belonging to space group P63mc) as a crystal structure. The Li-containing oxide according to the embodiment has an O2 type structure and may have a crystal structure other than the O2 type structure. Examples of crystal structures other than the O2 type structure include a T♯2 type structure (belonging to space group Cmca) formed when Li is de-inserted from the O2 type structure and an O6 type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, and different from the O3 type structure also belonging to space group R-3m). However, as described later, the Li-containing oxide according to the embodiment has a small amount of the T♯2 type structure. The Li-containing oxide according to the embodiment may have an O2 type structure as a main phase, or may have a crystal structure other than the O2 type structure (for example, an O6 type structure) as a main phase. However, the Li-containing oxide according to the embodiment may have a crystal structure serving as a main phase that changes depending on the charge / discharge state.
[0010] 1.1.1 X-ray diffraction peak intensity The X-ray diffraction pattern of the Li-containing oxide according to the embodiment is 0≦I 1 / I 2 ≦0.30. 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity originating from the (002) plane of the O2 type structure.
[0011] In conventional O2-type positive electrode active materials, the T#2-type structure is inevitably generated along with the O2-type structure, and the X-ray diffraction peak intensity derived from the T#2 structure is large. In the conventional technology, sufficient consideration has not been given to reducing this T#2-type structure. In contrast, the Li-containing oxide according to the embodiment adopts the synthesis conditions described below, thereby reducing the X-ray diffraction peak intensity I derived from the O2-type structure. 2 However, the X-ray diffraction peak intensity I 1 Here, according to the findings of the present inventors, in the X-ray diffraction pattern of a Li-containing oxide, the lower the X-ray diffraction peak derived from the T♯2 type structure is relative to the X-ray diffraction peak derived from the O2 type structure, the higher the capacity as a positive electrode active material.
[0012] In the X-ray diffraction pattern of the Li-containing oxide according to the embodiment, the X-ray diffraction peak intensity I 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the O2 type structure 2 Comparison with I 1 / I 2 However, 0≦I 1 / I 2 ≦0.30. The X-ray diffraction pattern satisfies 0≦I 1 / I 2 ≦0.27, 0≦I 1 / I 2 ≦0.25, 0≦I 1 / I 2 ≦0.23, 0≦I 1 / I 2 ≦0.20, 0≦I 1 / I 2≦0.17, 0≦I 1 / I 2 ≦0.15, 0≦I 1 / I 2 ≦0.13, 0≦I 1 / I 2 ≦0.10, 0≦I 1 / I 2 ≦0.05, 0≦I 1 / I 2 ≦0.01 or I 1 / I 2 =0 may be satisfied.
[0013] 1.1.2 Method for measuring X-ray diffraction peak intensity In the present application, the "X-ray diffraction pattern of the Li-containing oxide" and the "X-ray diffraction peak intensity" refer to those obtained under the following conditions. That is, an X-ray diffraction pattern is obtained for the Li-containing oxide by using an X-ray diffractometer (Rigaku, fully automatic multipurpose X-ray diffractometer SmartLab) with CuKα as the radiation source, a tube voltage of 45 kV, a tube current of 200 mA, a step width of 0.02°, and a scan speed of 1° / min. In the X-ray diffraction pattern, an X-ray diffraction peak derived from the (002) plane of the T♯2 type structure and an X-ray diffraction peak derived from the (002) plane of the O2 type structure are identified, and the background value near the peaks is subtracted from the X-ray diffraction pattern, and the above I is calculated from the intensity of each X-ray diffraction peak. 1 / I 2 can be sought.
[0014] 1.1.3 Crystallites The Li-containing oxide according to an embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites. For example, the Li-containing oxide according to an embodiment may have a surface consisting of a plurality of crystallites. In other words, the Li-containing oxide may have a structure in which a plurality of crystallites are connected to each other on the surface. When the surface of the Li-containing oxide is consisting of a plurality of crystallites, a crystal grain boundary is present on the surface. Here, the crystal grain boundary may be an inlet and an outlet of intercalation. That is, when the Li-containing oxide is a polycrystal having a plurality of crystallites, the effect of increasing the number of inlets and outlets of intercalation to reduce the reaction resistance, the effect of shortening the distance of movement of lithium ions to reduce the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging to reduce the occurrence of cracks, and the like can be expected. The size of the crystallite may be large or small, but it is considered that the smaller the size of the crystallite, the more the crystal grain boundaries will be, and the more likely the above-mentioned advantageous effects will be exhibited. For example, when the diameter of the crystallite constituting the Li-containing oxide is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "diameter of the crystallite" can be determined by observing the surface of the Li-containing oxide with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the Li-containing oxide is observed and one closed region surrounded by the grain boundary is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined and regarded as the "diameter of the crystallite". If the Li-containing oxide is composed of a single crystal, the particle itself can be said to be one crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be determined by EBSD or XRD. For example, the diameter of the crystallite can be determined based on the Scherrer formula from the half-width of the diffraction line of the XRD pattern. If the diameter of the crystallite specified by any method is less than 1 μm, the Li-containing oxide is likely to exhibit higher performance. The crystallite constituting the Li-containing oxide may have a first surface exposed on the surface of the oxide, and the first surface may be planar. That is, the surface of the Li-containing oxide may have a structure in which a plurality of planes are connected.As described later, when producing a Na-containing oxide that is a raw material for a Li-containing oxide, crystallites having a planar first surface can be easily obtained by growing the crystallites on the surface of the particles until one crystallite and another crystallite are connected to each other.
[0015] 1.2 Chemical composition A Li-containing oxide according to one embodiment contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O. When the Li-containing oxide contains, as constituent elements, at least Li, Mn, one or both of Ni and Co, and O, in particular, when the Li-containing oxide contains, as constituent elements, at least Li, Mn, Ni, Co, and O, higher performance is likely to be obtained.
[0016] In one embodiment, the Li-containing oxide having an O2 type structure is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2(Here, 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) It may have a chemical composition represented by. When the Li-containing oxide has such a chemical composition, the O2-type structure is easily maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, or 0.70 or less. In the above chemical composition, b is 0 or more, and may be 0.01 or more, 0.02 or more, or 0.03 or more, and is at most 0.20, and may be 0.15 or less, or 0.10 or less. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more, or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, since p + q + r is less than 0.17, a high charge and discharge capacity is easily ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when the element M is included, the O2-type structure is easily stabilized. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more.)The composition of O is approximately 2, but is not necessarily exactly 2.0 and is variable.
[0017] 1.3 Shape As described later, a Li-containing oxide having an O2 type structure can be obtained by substituting Li for Na in a Na-containing oxide having a P2 type structure. Here, the P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is prone to crystal growth in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystal is prone to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide having a P2 type structure is usually a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction. The Li-containing oxide according to one embodiment may be obtained based on such plate-like Na-containing oxide particles, or, as described later, may be obtained based on spherical Na-containing oxide particles. That is, the shape of the Li-containing oxide may be a plate-like particle or a spherical particle. When the Li-containing oxide is a spherical particle, the reaction resistance is reduced by reducing the crystallite size, and the diffusion resistance inside the particle is likely to be reduced. Furthermore, when applied to a secondary battery or the like, it is considered that the degree of curvature is reduced by spheroidization, and the lithium ion conduction resistance is reduced. This, for example, improves the rate characteristics and tends to increase the reversible capacity. In the present application, the term "spherical particles" refers to particles having a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is 4πS / L 2 Here, S is the orthogonal projected area of the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When the particle is made up of more than 100 particles, the circularity is measured, for example, as an average value as follows.
[0018] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles are randomly selected that have an equivalent circle diameter (the diameter of a circle having the same area as the orthogonal projected area of the particle) of not less than D10 and not more than D90, as determined in (1). (3) The circularity of each extracted particle is determined by image processing, and the average value is regarded as the "circularity of the particle."
[0019] The Li-containing oxide according to an embodiment may be a solid particle, a hollow particle, or a particle having a void. The size of the Li-containing oxide particles is not particularly limited, but it is considered that a smaller size is more advantageous. For example, the average particle diameter (D50) of the Li-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is a particle diameter (D50, median diameter) at an integrated value of 50% in a volume-based particle size distribution by a laser diffraction / scattering method.
[0020] 1.4 Other As described above, the positive electrode active material according to the embodiment has a large capacity by containing the specific Li-containing oxide. The positive electrode active material according to the embodiment may be composed of only the Li-containing oxide, or may contain the Li-containing oxide and other positive electrode active materials (other positive electrode active materials). From the viewpoint of further enhancing the above effect, the ratio of other positive electrode active materials in the entire positive electrode active material may be small. For example, the content of the Li-containing oxide may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, based on the entire positive electrode active material being 100% by mass.
[0021] 2. Manufacturing method of positive electrode active material The Li-containing oxide according to the above embodiment can be produced, for example, by the following method. As shown in FIG. 1, the method for producing a Li-containing oxide having an O2 type structure according to one embodiment is as follows: S1: Obtaining a precursor comprising at least one element of Mn, Ni and Co; S2: Coating the surface of the precursor with a Na source to obtain a composite; S3: Calcining the composite to obtain a Na-containing oxide having a P2 type structure; and S4: At least a part of the Na in the Na-containing oxide is ion-exchanged with Li to obtain a Li-containing oxide having an O2 type structure. S3-1: Pre-firing the composite at a temperature of 300° C. or more and less than 700° C. for 2 hours or more and 10 hours or less; S3-2: Following the preliminary firing, the composite is subjected to a main firing at a temperature of 700° C. or more and 1100° C. or less for a period of 30 minutes to 48 hours or less; and S3-3: Following the main sintering, the composite is heated to a temperature T 1 from 100°C or less T 2 and rapidly cooling until the temperature reaches a temperature of 100.degree.
[0022] 2.1 S1 In S1, a precursor containing at least one element of Mn, Ni, and Co is obtained. The precursor may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may have various shapes. For example, the precursor may be particulate, or may be spherical particles as described later. The particle size of the particles made of the precursor is not particularly limited.
[0023] In S1, a precipitate as the precursor may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain a precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.
[0024] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have a function of stabilizing, for example, a P2 type structure or an O2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.
[0025] 2.2 S2 In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or may be a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.
[0026] In S2, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with the Na source. Here, when the precursor obtained by S1 is a spherical particle, and the composite obtained by S2 is obtained by covering 40 area% or more of the surface of the precursor with the Na source, the Na-containing oxide having the P2 type structure is likely to become a spherical particle in S3 described later. If the coverage of the Na source is small, when the composite is fired, P2 type crystals are likely to grow on the surface of the composite, and the Na-containing oxide is likely to become a plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystals are likely to become small, and the Na-containing oxide is likely to become a spherical particle corresponding to the shape of the precursor.
[0027] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of the surface of the precursor is coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method or a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the area of the surface of the precursor can be coated with the Na source.
[0028] In S2, the precursor may be coated with an M source together with a Na source. For example, in S2, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.
[0029] 2.3 S3 In S3, the composite obtained in S2 is calcined to obtain a Na-containing oxide having a P2 type structure. S3 includes the above S3-1, S3-2, and S3-3.
[0030] 2.3.1 S3-1 In S3-1, the composite is pre-fired at a temperature of 300° C. or more and less than 700° C. for 2 hours to 10 hours. In S3-1, the composite may be optionally molded and then pre-fired. The pre-fire is performed at a temperature lower than that of the main firing. If the pre-fire in S3-1 is insufficient, the formation of the P2 phase may be insufficient in the finally obtained Na-containing oxide. In S3-1, the pre-fire temperature is 300° C. or more and less than 700° C., and the pre-fire time is 2 hours to 10 hours, so that the composite can be pre-fired sufficiently, the heat uniformity is increased, the Na-containing oxide obtained through S3-2 and S3-3 described later becomes appropriate, and the Li-containing oxide having an O2 type structure obtained through S4 becomes the above-mentioned I phase. 1 / I 2The pre-firing temperature may be 400°C or more and less than 700°C, 450°C or more and less than 700°C, 500°C or more and less than 700°C, 550°C or more and less than 700°C, or 550°C or more and less than 650°C. The pre-firing time may be 2 hours or more and less than 8 hours, 3 hours or more and less than 8 hours, 4 hours or more and less than 8 hours, 5 hours or more and less than 8 hours, or 5 hours or more and less than 7 hours. The pre-firing atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.
[0031] 2.3.2 S3-2 In S3-2, following the above pre-firing, the composite is subjected to main firing at a temperature of 700°C to 1100°C for 30 minutes to 10 hours. In S3-2, the main firing temperature of the composite is 700°C to 1100°C, preferably 800°C to 1000°C. If the main firing temperature is too low, the P2 phase is not generated, and if the main firing temperature is too high, the O3 phase and the like are likely to be generated instead of the P2 phase. The temperature rise condition from the pre-firing temperature to the main firing temperature is not particularly limited. The main firing time is not particularly limited, and may be, for example, 30 minutes to 48 hours. However, the shape of the Na-containing oxide can be controlled by the main firing time. As described above, in the method of the present disclosure, when the coverage of the Na source in the composite is 40 area % or more, when the composite is fired, P2 type crystals with small crystallites are likely to be formed on the surface. In the method of the present disclosure, the P2 type crystals are grown along the surface of the particles so as to connect one P2 type crystallite with another P2 type crystallite, so that the shape of the Na-containing oxide corresponds to the shape of the precursor. For example, when the precursor is a spherical particle, the Na-containing oxide can also be a spherical particle. If the firing time is too short, the generation of the P2 phase is insufficient. On the other hand, if the firing time is too long, the P2 phase grows excessively, resulting in plate-like particles rather than spherical ones. As far as the present inventors have confirmed, spherical particles of the Na-containing oxide are easily obtained when the firing time is 30 minutes or more and 3 hours or less. The Na-containing oxide obtained after firing may have a structure in which a plurality of crystallites are present on the surface and the crystallites are connected to each other.
[0032] 2.3.3 S3-3 In S3-3, following the main sintering, the composite is heated to a temperature T 1 from 100°C or less T 2 The above pre-baking and main baking are performed, for example, in a heating furnace. In step S3-3, for example, after the main baking of the composite is performed in the heating furnace, the composite is heated to an arbitrary temperature T 1 Cool to the temperature T 1 After this, the baked product is removed from the furnace and heated to any temperature T below 100°C. 2 Rapid cooling is performed outside the furnace until the temperature T 1 is any temperature above 200° C., and may be any temperature above 250° C. 2 is any temperature below 100°C, may be any temperature below 50°C, or may be the cooling end temperature. 1 from temperature T 2 In a certain temperature range between the temperatures, moisture easily penetrates between the layers of the P2 type structure due to atomic vibrations and molecular motions. When cooling the composite (Na-containing oxide having a P2 type structure) after the main firing, it is considered that the amount of moisture that penetrates between the layers of the P2 type structure can be reduced by shortening the time during which the composite is in the temperature range in which moisture easily penetrates (i.e., by cooling quickly). In this regard, in step S3-3, when cooling the composite after the main firing, an arbitrary temperature T 1 Any temperature T below 100°C 2 For example, by cooling in a dry atmosphere outside the furnace, the temperature T 1 from temperature T 2 The cooling rate during the process is high (e.g., 20°C / min or more), which makes it difficult for moisture to penetrate between the layers of the P2 type structure, and the collapse of the P2 type structure can be suppressed. As a result, Na can be efficiently ion-exchanged with Li in S4, and the Li-containing oxide having an O2 type structure obtained through S4 has the above-mentioned I 1 / I 2 It is likely to satisfy the above.
[0033] By the above method, a Na-containing oxide having a P2 type structure and a predetermined chemical composition can be produced. The Na-containing oxide contains at least one transition metal element selected from Mn, Ni, and Co, Na, and O as constituent elements. In particular, when the constituent elements include at least Na, Mn, at least one of Ni and Co, and O, and especially when the constituent elements include at least Na, Mn, Ni, Co, and O, the performance of the positive electrode active material particles is more likely to be improved. The Na-containing oxide contains Na c Mn x-p Ni y-q Co z-r M p+q+r O 2It may have the chemical composition shown herein. Here, 0 < c ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the Na-containing oxide has such a chemical composition, the P2-type structure is more likely to be maintained. In the above chemical composition, c may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. x is 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, 0.10 or more, or 0.20 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The contribution of element M to charge and discharge is small. In this regard, in the above chemical composition, when p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when element M is included, the P2-type structure and the O2-type structure are likely to be stabilized. In the above chemical composition, p + q + r is 0 or more, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but it is not necessarily exactly 2.0 and is indefinite.
[0034] 2.4 S4 In S4, at least a part of Na in the Na-containing oxide obtained in S3 is ion-exchanged with Li to obtain a Li-containing oxide having an O2-type structure. For example, there are a method using an aqueous solution containing lithium halide and a method using a mixture of lithium halide and other lithium salts (for example, molten salt) for ion exchange. From the viewpoint that the P2-type structure is easily broken by the intrusion of water and from the viewpoint of crystallinity, the method using the molten salt is preferable among the above two methods. That is, by mixing the Na-containing oxide having the above-mentioned P2-type structure with the molten salt and heating it to a temperature equal to or higher than the melting point of the molten salt, at least a part of Na in the Na-containing oxide can be replaced with Li by ion exchange.
[0035] The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide, and lithium iodide. The other lithium salt constituting the molten salt is preferably lithium nitrate. By using the molten salt, the melting point becomes lower than when the lithium halide or other lithium salt is used alone, and ion exchange can be performed at a lower temperature.
[0036] The temperature in the ion exchange may be, for example, above the melting point of the molten salt and below 600°C, below 500°C, below 400°C, or below 300°C. If the temperature in the ion exchange is too high, the stable O3 structure is likely to be formed instead of the O2 structure. On the other hand, from the viewpoint of shortening the time required for the ion exchange, it is preferable that the temperature in the ion exchange is as high as possible.
[0037] 3. Lithium-ion secondary battery The positive electrode active material according to the embodiment includes the specific Li-containing oxide described above. The positive electrode active material according to the embodiment can be used, for example, as a positive electrode active material of a lithium ion secondary battery. FIG. 2 shows a schematic configuration of a lithium ion secondary battery according to an embodiment. As shown in FIG. 2, a lithium ion secondary battery 100 according to an embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. Here, the positive electrode active material layer 10 includes the positive electrode active material according to the embodiment described above.
[0038] 3.1 Cathode active material layer The positive electrode active material layer 10 includes at least the positive electrode active material according to the above embodiment, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the positive electrode active material layer 10 may further include various additives. The content of each of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 10 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 10 (total solid content) being 100 mass%. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 10 having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0039] 3.1.1 Cathode active material The positive electrode active material is as described above. That is, the positive electrode active material contains a Li-containing oxide, and the Li-containing oxide has an O2 type structure and contains at least one element selected from Mn, Ni, and Co, Li, and O as constituent elements. 1 / I 2satisfies the relationship described above. As described above, the positive electrode active material may consist only of the above Li-containing oxide, or may include, together with the above Li-containing oxide, other positive electrode active materials (other positive electrode active materials). From the viewpoint of further enhancing the effects of the technology of the present disclosure, the proportion of other positive electrode active materials in the entire positive electrode active material may be small. For example, assuming the total amount of the positive electrode active material is 100% by mass, the content of the above Li-containing oxide may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.
[0040] Any of the other positive electrode active materials known as positive electrode active materials for lithium ion secondary batteries can be adopted. The other positive electrode active materials may be, for example, at least one selected from various lithium compounds other than the above Li-containing oxide, elemental sulfur, sulfur compounds, etc. The lithium compound as the other positive electrode active material may be a Li-containing oxide containing at least one element M, Li, and O. Element M may be, for example, at least one selected from Mn, Ni, Co, Al, Mg, Ca, Sc, V, Cr, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, Bi, Fe, and Ti, or at least one selected from the group consisting of Mn, Ni, Co, Al, Fe, and Ti. More specifically, the Li-containing oxide as the other positive electrode active material is lithium cobaltate, lithium nickelate, lithium manganate, lithium nickel cobaltate, lithium nickel manganate, lithium cobalt manganate, lithium nickel cobalt manganate (Li 1±α Ni x Co y Mn z O 2±δ (for example, 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), spinel-type lithium compounds (Li 1+x Mn 2-x-y M y O 4(M is one or more selected from Al, Mg, Co, Fe, Ni, and Zn)), lithium nickel cobalt aluminate (e.g., Li 1±α Ni p Co q Al r O 2±δ (e.g., p+q+r=1), lithium titanate, lithium metal phosphate (LiMPO 4 and the like, M may be at least one selected from Fe, Mn, Co, and Ni). In particular, when the other positive electrode active material contains at least one of Ni, Co, and Mn as a constituent element, and a Li-containing oxide containing Li and O, the performance of the secondary battery is more likely to be improved. Alternatively, when the other positive electrode active material contains at least one of Ni, Co, and Al as a constituent element, and a Li-containing oxide containing Li and O, the performance of the secondary battery is more likely to be improved. Only one type of the other positive electrode active material may be used alone, or two or more types may be used in combination. The shape of the other positive electrode active material may be a general shape as a positive electrode active material for a secondary battery. The other positive electrode active material may be, for example, particulate. The other positive electrode active material may be solid or may have voids, for example, may be porous or may be hollow. The other positive electrode active material may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle diameter D50 of other positive electrode active materials may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less.
[0041] 3.1.2 Protective layer An ion-conductive protective layer may be formed on the surface of the positive electrode active material. That is, the positive electrode active material layer 10 may include a complex of the positive electrode active material and the protective layer, and at least a part of the surface of the positive electrode active material in the complex may be covered with the protective layer. This makes it easier to suppress, for example, the reaction between the positive electrode active material and other battery materials (such as the sulfide solid electrolyte described below). The ion-conductive protective layer may include various ion-conductive compounds. The ion-conductive compound may be, for example, at least one selected from ion-conductive oxides and ion-conductive halides.
[0042] The ion conductive oxide may contain, for example, at least one element selected from B, C, Al, Si, P, S, Ti, La, Zr, Nb, Mo, Zn, and W, Li, and O. The ion conductive oxide may be an oxynitride containing N. More specifically, the ion conductive oxide may contain Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , LiAlO 2 , Li 4 SiO 4 , Li 2 SiO 3 , Li 3 PO 4 , Li 2 SO 4 , Li 2 TiO 3 , Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , Li 2 ZrO 3 , LiNbO 3 , Li 2 MoO 4 , Li 2 WO 4 , LiPON, Li 2 O-LaO 2 , Li 2 O-ZnO 2etc. The ion conductive oxide may be one in which some elements are substituted with various doping elements.
[0043] The ion conductive halide may be, for example, at least one of various compounds exemplified as the halide solid electrolyte described later. The ion conductive halide may include, for example, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm, at least one halogen element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may include at least one element selected from the group consisting of Ti, Al, Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also include at least one element selected from the group consisting of Ti and Al, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also be, for example, a complex halide of Li, Ti, Al and F.
[0044] The coverage (area ratio) of the protective layer with respect to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less, or 20 nm or less.
[0045] 3.1.2 Electrolytes The positive electrode active material layer 10 may contain an electrolyte. The electrolyte that may be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte, or a combination thereof.
[0046] 3.1.2.1 Solid electrolyte As the solid electrolyte, a solid electrolyte known for lithium ion secondary batteries may be used. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte is excellent in ion conductivity and heat resistance. Examples of the inorganic solid electrolyte include oxide solid electrolytes, sulfide solid electrolytes, and ion-bonded inorganic solid electrolytes. Among inorganic solid electrolytes, sulfide solid electrolytes, and sulfide solid electrolytes containing at least Li, S, and P as constituent elements, have high performance. Alternatively, among inorganic solid electrolytes, ion-bonded solid electrolytes, and solid electrolytes containing at least Li, Y, and halogen (at least one of Cl, Br, I, and F) as constituent elements, have high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. The average particle diameter (D50) of the solid electrolyte may be, for example, 10 nm or more and 10 μm or less. The ion conductivity of the solid electrolyte at 25° C. is, for example, 1×10 -5 S / cm or more, 1×10 -4 S / cm or more, or 1×10 -3 The solid electrolyte may have a specific surface area of 100 nm or more and may have a specific surface area of 100 nm or more.
[0047] The oxide solid electrolyte is lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X (PO 4 ) 3 , Li-SiO-based glass, Li-Al-SO-based glass, etc. In addition, when an oxide solid electrolyte is combined with a liquid electrolyte, ion conductivity can be improved.
[0048] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase. The sulfide solid electrolyte may be particulate. The average particle diameter (D50) of the sulfide solid electrolyte may be, for example, 10 nm or more and 100 μm or less.
[0049] The sulfide solid electrolyte may contain, for example, Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S element. The sulfide solid electrolyte may further contain at least one of O element and halogen element. The sulfide solid electrolyte may contain S element as a main component of anion element.
[0050] The sulfide solid electrolyte is, for example, Li 2 SP 2 S 5 , Li 2 SP 2 S 5 - LiI, Li 2 SP 2 S 5 -GeS 2 , Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 SP 2 S 5 -LiI-LiBr, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B. 2 S 3 , Li 2 SP 2 S 5 -ZmSn (where m and n are positive numbers. Z is Ge, Zn, or Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (wherein x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In).
[0051] The composition of the sulfide solid electrolyte is not particularly limited, but may be, for example, xLi 2 S·(100-x)P 2 S 5 (70≦x≦80), yLiI・zLiBr・(100-yz)(xLi 2 S (1-x)P 2 S 5 ) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30) and the like. Alternatively, the sulfide solid electrolyte may be represented by the general formula: Li 4-x Ge 1-x P x S 4It may have a composition represented by (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte is Li 7-a PS 6-a X a (X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0, or may be greater than 0. In the latter case, a may be 0.1 or more, may be 0.5 or more, or may be 1 or more. Also, a may be 1.8 or less, may be 1.5 or less.
[0052] The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm. These elements may generate cations in water. The ion-bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I and F. These elements may generate anions in water. The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion-bonded solid electrolyte may contain Li and Y, and at least one element selected from the group consisting of Cl, Br, I and F. More specifically, the ionically bonded solid electrolyte may contain Li, Y, Cl, and Br, or may contain Li, Ca, Y, Gd, Cl, and Br, or may contain Li, Zr, Y, and Cl. 3 YBr 2 Cl 4 , Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br 2 Cl 4 , and Li 2.5 Y 0.5 Zr 0.5 Cl 6 It may be at least one of the above.
[0053] The ionically bonded solid electrolyte may be a halide solid electrolyte. The halide solid electrolyte has excellent ion conductivity. Examples of the halide solid electrolyte include those represented by the formula (A): Li α M β X γ (A) It may have a composition represented by the following. Here, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements other than Li and metalloid elements, and X is at least one selected from the group consisting of Cl, Br, and I. Note that the "metalloid element" may be at least one selected from the group consisting of B, Si, Ge, As, Sb, and Te. Also, the "metal element" may include (i) all elements (excluding hydrogen) contained in Groups 1 to 12 of the periodic table and (ii) all elements (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se) contained in Groups 13 to 16 of the periodic table. The metal element can form an inorganic compound with a halide ion and become a cation.
[0054] In formula (A), M may contain Y (i.e., yttrium). The halide solid electrolyte containing Y is Li a Me b Y c X 6 (where a + mb + 3c = 6, c > 0, Me is at least one selected from the group consisting of metal elements and metalloid elements other than Li and Y, and m is the valence of Me) may have a composition represented by the following. Me may be, for example, at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.
[0055] The halide solid electrolyte may have a composition represented by formula (A1): Li 6-3d Y d X 6 In formula (A1), X is one or more elements selected from the group consisting of Cl, Br, and I. d may satisfy 0 < d < 2, or d may be 1. The halide solid electrolyte may have a composition represented by formula (A2): Li 3-3δ Y 1+δ Cl 6It may have a composition represented by. In formula (A2), 0 < δ ≦ 0.15 may be satisfied. The halide solid electrolyte has the formula (A3): Li 3-3δ Y 1+δ Br 6 It may have a composition represented by. In formula (A3), 0 < δ ≦ 0.25 may be satisfied. The halide solid electrolyte has the formula (A4): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y It may have a composition represented by. In formula (A4), Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. In formula (A4), for example, -1 < δ < 2, 0 < a < 3, 0 < (3 - 3δ + a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 are satisfied. The halide solid electrolyte has the formula (A5): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y It may have a composition represented by. In formula (A5), Me may be at least one selected from the group consisting of Al, Sc, Ga, and Bi. In formula (A5), -1 < δ < 1, 0 < a < 2, 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may be satisfied. The halide solid electrolyte has the formula (A6): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y It may have a composition represented by. In formula (A6), Me may be at least one selected from the group consisting of Zr, Hf, and Ti. In formula (A6), -1 < δ < 1, 0 < a < 1.5, 0 < (3 - 3δ - a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may be satisfied. The halide solid electrolyte has the formula (A7): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Brx I y In formula (A7), Me may be at least one selected from the group consisting of Ta and Nb. In formula (A7), -1<δ<1, 0 <a<1.2、0<(3-3δ-2a)、0<(1+δ-a)、0≦x≦6、0≦y≦6、かつ、(x+y)≦6であってもよい。
[0056] The ionically bonded solid electrolyte may be a complex hydride solid electrolyte. The complex hydride solid electrolyte may be composed of Li ions and complex ions containing H. The complex ion containing H may have, for example, an element M containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element M. In addition, the complex ion containing H may have the element M as a central element and H surrounding the element M bonded to each other via a covalent bond. In addition, the complex ion containing H may be (M m H n ) α- In this case, m is any positive number, and n and α can be any positive number depending on m and the valence of element M. Element M may be a nonmetallic element or a metallic element capable of forming a complex ion. For example, element M may contain at least one of B, C, and N as a nonmetallic element, or may contain B. Also, for example, element M may contain at least one of Al, Ni, and Fe as a metallic element. In particular, when the complex ion contains B, or contains C and B, higher ionic conductivity is likely to be ensured. Specific examples of complex ions containing H include (CB 9 H 10 ) - , (C.B. 11 H 12 ) - , (B 10 H 10 ) 2- , (B 12 H 12 ) 2- , (BH 4 ) - , (NH 2 ) - , (AlH 4 ) -, and combinations thereof. In particular, (CB 9 H 10 ) - , (C.B. 11 H 12 ) - In other words, the complex hydride solid electrolyte may contain Li, C, B, and H.
[0057] 3.1.2.2 Liquid electrolyte The liquid electrolyte (electrolytic solution) is a liquid containing lithium ions as carrier ions. The electrolytic solution may be an aqueous electrolytic solution or a non-aqueous electrolytic solution. The composition of the electrolytic solution may be the same as that of the electrolytic solution of a lithium ion secondary battery known in the art. The electrolytic solution may be a solution in which a lithium salt is dissolved in water or a non-aqueous solvent. Examples of the non-aqueous solvent include various carbonate-based solvents. Examples of the lithium salt include lithium amide salt and LiPF 6 etc.
[0058] 3.1.3 Conductive additives Examples of the conductive assistant that may be included in the positive electrode active material layer 10 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, titanium, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size thereof is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.
[0059] 3.1.4 Binders Examples of binders that can be included in the positive electrode active material layer 10 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.
[0060] 3.1.5 Other The positive electrode active material layer 10 may contain various additives in addition to the above components, such as a dispersant and a lubricant.
[0061] 3.2 Electrolyte layer The electrolyte layer 20 is disposed between the positive electrode active material layer 10 and the negative electrode active material layer 30. The electrolyte layer 20 includes at least an electrolyte. The electrolyte layer 20 may include at least one of a solid electrolyte and an electrolytic solution, and may further include a binder or the like. The content of the electrolyte and the binder or the like in the electrolyte layer 20 is not particularly limited. Alternatively, the electrolyte layer 20 may have a separator or the like for holding the electrolytic solution and preventing contact between the positive electrode active material layer 10 and the negative electrode active material layer 30. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0062] The electrolyte layer 20 may be composed of one layer or may be composed of multiple layers. For example, the electrolyte layer 20 may include a first layer disposed on the positive electrode active material layer 10 side and a second layer disposed on the negative electrode active material layer 30 side, and the first layer may include the first electrolyte, and the second layer may include the second electrolyte. The first electrolyte and the second electrolyte may be different from each other. The first electrolyte and the second electrolyte may each be at least one selected from the above-mentioned oxide solid electrolyte, sulfide solid electrolyte, and ionic solid electrolyte. For example, the first layer may include an ionic solid electrolyte, and the second layer may include at least one of an ionic solid electrolyte and a sulfide solid electrolyte.
[0063] The electrolyte contained in the electrolyte layer 20 may be appropriately selected from those exemplified as electrolytes that can be contained in the above-mentioned positive electrode active material layer 10 (solid electrolytes and / or liquid electrolytes). The binder that can be contained in the electrolyte layer 20 may also be appropriately selected from those exemplified as binders that can be contained in the above-mentioned positive electrode active material layer. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator that is normally used in lithium ion secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multilayer structure. Examples of the multilayer separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.
[0064] 3.3 Negative electrode active material layer The negative electrode active material layer 30 includes at least a negative electrode active material. The negative electrode active material layer 30 may also include an electrolyte, a conductive assistant, a binder, various additives, and the like. The content of each component in the negative electrode active material layer 30 may be appropriately determined according to the intended battery performance. For example, the content of the negative electrode active material may be 40% by mass or more, 50% by mass or more, 60% by mass or more, or 70% by mass or more, or 100% by mass or less, less than 100% by mass, 95% by mass or less, or 90% by mass or less, based on the entire solid content of the negative electrode active material layer 30 being 100% by volume. Alternatively, the negative electrode active material and optionally the electrolyte, the conductive assistant, and the binder may be included in a total amount of 85% by volume or more, 90% by volume or more, or 95% by volume or more, based on the entire negative electrode active material layer 30 being 100% by volume, and the remainder may be voids or other components. The shape of the negative electrode active material layer 30 is not particularly limited, and may be, for example, a sheet having a substantially flat surface. The thickness of the negative electrode active material layer 30 is not particularly limited, and may be, for example, 0.1 μm or more, 1 μm or more, 10 μm or more, or 30 μm or more, and may be 2 mm or less, 1 mm or less, 500 μm or less, or 100 μm or less.
[0065] 3.3.1 Negative electrode active material The negative electrode active material may be any of those known as negative electrode active materials for lithium ion secondary batteries. Of the known active materials, various materials may be used that have a potential (charge / discharge potential) for absorbing and releasing lithium ions that is lower than the above-mentioned positive electrode active material. For example, silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like may be used. Among them, when the negative electrode active material layer 30 contains Si as the negative electrode active material, the performance of the lithium ion secondary battery 100 is likely to be improved. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be any shape that is common as a negative electrode active material for secondary batteries. For example, the negative electrode active material may be in the form of particles. The negative electrode active material particles may be primary particles, or may be secondary particles formed by agglomerating a plurality of primary particles. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in the form of a sheet (foil or film) such as a lithium foil. That is, the negative electrode active material layer 30 may be made of a sheet of the negative electrode active material.
[0066] 3.3.2 Other Examples of the electrolyte that can be contained in the negative electrode active material layer 30 include the above-mentioned solid electrolyte, electrolytic solution, or a combination thereof. The conductive assistant that can be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, those exemplified as the conductive assistant that can be contained in the above-mentioned positive electrode active material layer. The binder that can be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, those exemplified as the binder that can be contained in the above-mentioned positive electrode active material layer. Each of the electrolyte, conductive assistant, and binder may be used alone or in combination of two or more kinds.
[0067] 3.4 Positive electrode current collector As shown in FIG. 2, the lithium ion secondary battery 100 may include a positive electrode collector 40 in contact with the positive electrode active material layer 10. The positive electrode collector 40 may be any of those commonly used as a positive electrode collector for secondary batteries. The positive electrode collector 40 may have at least one shape selected from a foil shape, a plate shape, a mesh shape, a punched metal shape, and a foam. The positive electrode collector 40 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of handling and the like. The positive electrode collector 40 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 40 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 40 may contain Al. The positive electrode collector 40 may have some kind of coating layer on its surface for the purpose of adjusting the resistance or the like. For example, the positive electrode collector 40 may have a carbon coating layer. The positive electrode collector 40 may be a metal foil or a substrate on which the above-mentioned metal is plated or vapor-deposited. When the positive electrode collector 40 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the positive electrode collector 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0068] 3.5 Negative electrode current collector As shown in FIG. 2, the lithium ion secondary battery 100 may include a negative electrode current collector 50 in contact with the negative electrode active material layer 30. The negative electrode current collector 50 may be any of those commonly used as negative electrode current collectors for secondary batteries. The negative electrode current collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, a metal foil is excellent in terms of ease of handling. The negative electrode current collector 50 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 50 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 50 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. For example, the negative electrode current collector 50 may have a carbon coating layer. The negative electrode current collector 50 may be an aluminum foil having a carbon coating layer. The negative electrode current collector 50 may also be a metal foil or a base material on which the above metal is plated or vapor-deposited. In addition, when the negative electrode current collector 50 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 50 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.
[0069] 3.6 Other configurations The lithium ion secondary battery 100 may have a general configuration as a secondary battery in addition to the above configuration. For example, a tab, a terminal, etc. The lithium ion secondary battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be adopted as the exterior body. In addition, a plurality of secondary batteries 100 may be electrically connected in any way and stacked in any way to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The shape of the lithium ion secondary battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, etc.
[0070] The lithium ion secondary battery 100 can be manufactured by applying a known method, except for using the above-mentioned specific positive electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the lithium ion secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, thereby forming a positive electrode. (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is applied to the surface of the negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).
[0071] 4. Method for increasing the capacity of lithium-ion secondary batteries The technology of the present disclosure also has an aspect of being a method for increasing the capacity of a lithium ion secondary battery. That is, the method for increasing the capacity of a lithium ion secondary battery of the present disclosure is characterized in that the positive electrode active material of the present disclosure is used in a positive electrode active material layer of the lithium ion secondary battery.
[0072] 5. Vehicles equipped with lithium-ion secondary batteries As described above, the positive electrode active material of the present disclosure has a large capacity and is suitable as a positive electrode active material for a lithium ion secondary battery. Such a lithium ion secondary battery having a large capacity can be suitably used in at least one vehicle selected from, for example, a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV), and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a lithium ion secondary battery, the lithium ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and the positive electrode active material layer contains the positive electrode active material of the present disclosure. EXAMPLES
[0073] As described above, one embodiment of the positive electrode active material and the lithium ion secondary battery has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.
[0074] 1. Preparation of Positive Electrode Active Material 1.1 Example 1 1.1.1 Preparation of precursor (1) MnSO4 5H 2 O, NiSO 4 6H 2 O, CoSO 4 7H 2 The first solution was obtained by weighing out the desired composition ratio of O and dissolving it in distilled water to a concentration of 1.2 mol / L. 2 CO 3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then separated into coarse particles and fine particles by air classification. Here, both the coarse particles and the fine particles were composite salts containing Mn, Ni, and Co. The coarse particles were spherical particles having an average particle diameter D50 of 3.8 μm and a circularity of 0.86. The fine particles were spherical particles having an average particle diameter D50 of 1.4 μm and a circularity of 0.80. In Example 1, the above coarse particles were used as precursor particles.
[0075] 1.1.2 Preparation of the complex (1) Na to 1150g / L 2 CO 3 After weighing out and distilled water, stir using a stirrer until completely dissolved. 2 CO 3 An aqueous solution was prepared. (2) The above Na 2 CO 3 The aqueous solution and the above-mentioned precursor particles are mixed together to obtain a mixture having a composition of Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2The components were weighed and mixed so as to obtain a slurry. (3) The above slurry was air-dried by spray drying to obtain a composite. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 The above slurry was dried by air flow under the conditions of 0.3 MPa spray pressure at 1000 rpm, and the surface of the precursor particles was coated with Na. 2 CO 3 The precursor particles were coated with Na to obtain a composite. In the composite, 77% of the surface area of the precursor particles was Na 2 CO 3 It was covered with.
[0076] 1.1.3 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 900°C in 100 minutes. (5) The temperature in the heating furnace is kept at 900°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C in 120 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0077] The fired product after cooling was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles A having a P2 type structure.
[0078] 1.1.4 Ion exchange (1) LiNO 3and LiCl were weighed out to have a molar ratio of 50:50, and mixed with the above P2 type particles A in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. (2) Using an alumina crucible, ion exchange was carried out in air at 280°C for 1 hour to obtain a product containing Li-containing oxide. (3) The salt remaining in the product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. (4) The obtained precipitate was dried overnight at 120° C. to obtain the positive electrode active material according to Example 1.
[0079] 1.2 Example 2 1.2.1 Preparation of precursor Coarse particles and fine particles were obtained in the same manner as in Example 1, and the fine particles were used as precursor particles.
[0080] 1.2.2 Preparation of the complex A composite was obtained by spray drying in the same manner as in Example 1, except that fine particles were used as the precursor particles. In the composite, 73% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with.
[0081] 1.2.3 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 1000°C in 160 minutes. (5) The temperature in the heating furnace is kept at 1000°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 1000°C to 250°C in 160 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0082] The fired product after cooling was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles B having a P2 type structure.
[0083] 1.2.4 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles B were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Example 2.
[0084] 1.3 Comparative Example 1 1.3.1 Preparation of precursor particles As in Example 2, fine particles were used as precursor particles.
[0085] 1.3.2 Preparation of the complex Precursor particles and Na 2 CO 3 And, Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O 2 The precursor and Na were weighed out to have the following composition: 2 CO 3 The composite was obtained by mixing the above in a mortar. In the composite, 24% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with.
[0086] 1.3.3 Firing of the composite The composite was placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) An alumina crucible containing the above composite is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 950°C in 120 minutes. (5) The temperature in the heating furnace is kept at 950°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 950°C to 250°C in 140 minutes. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool outside the furnace in a dry atmosphere until it reaches 25°C in 10 minutes.
[0087] The fired product after cooling was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles C having a P2 type structure.
[0088] 1.3.4 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles C were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 1.
[0089] 1.4 Comparative Example 2 1.4.1 Preparation of precursor particles As in Example 1, coarse particles were used as precursor particles.
[0090] 1.4.2 Preparation of the complex A composite was obtained in the same manner as in Comparative Example 1, except that coarse particles were used as the precursor particles. In the composite, 26% by area of the surface of the precursor particles was Na 2 CO 3 It was covered with.
[0091] 1.4.3 Firing of the composite The composite was placed in an alumina crucible and sintered under air atmosphere to obtain a Na-containing oxide having a P2 structure. The sintering conditions were the same as those in Example 2.
[0092] The fired product after cooling was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles D having a P2 type structure.
[0093] 1.4.4 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that Na-containing oxide particles D were used instead of Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 2.
[0094] 2. Evaluation of positive electrode active material 2.1 Elemental analysis Elemental analysis was carried out to identify the chemical composition of each of the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The results are shown in Table 1 below.
[0095] 2.2 Identification of crystal structure by X-ray diffraction measurement For each of the positive electrode active materials of Examples 1-2 and Comparative Examples 1-2, an X-ray diffraction measurement was performed using CuKα as a radiation source to obtain an X-ray diffraction pattern. FIG. 3 shows the X-ray diffraction patterns of Examples 1-2 and Comparative Examples 1-2. As shown in FIG. 3, it can be seen that all of the positive electrode active materials of Examples 1-2 and Comparative Examples 1-2 have an O2 type structure. Also, as shown in FIG. 3, it can be seen that the positive electrode active materials of Examples 1-2 have a lower X-ray diffraction peak intensity derived from the (002) plane of the T♯2 structure compared to the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure, compared to the positive electrode active materials of Comparative Examples 1-2. Table 1 below shows the X-ray diffraction peak intensity I derived from the (002) plane of the T♯2 structure for each of Examples 1-2 and Comparative Examples 1-2. 1 and the X-ray diffraction peak intensity I originating from the (002) plane of the O2 type structure 2 Comparison with I 1 / I 2 Shows.
[0096] 3. Preparation of evaluation cells Coin cells were produced using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The coin cell was produced as follows. (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) LiPF6 was dissolved at a concentration of 1 M in a mixed solvent of trifluoropropylene carbonate (TFPC) and trifluoroethyl methyl carbonate (TFEMC) in a ratio of TFPC:TFEMC = 30 vol%:70 vol% to obtain an electrolyte solution. (3) Metallic lithium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.
[0097] 4.Charge / Discharge Characteristics Evaluation The capacity of each coin cell was measured by charging and discharging at 0.1 C (1 C = 220 mA / g) in a voltage range of 2.0 to 4.8 V in a thermostatic chamber maintained at 25° C. The results are shown in Table 1 below.
[0098] 5. Evaluation Results For each of Examples 1 and 2 and Comparative Examples 1 and 2, the chemical composition of the positive electrode active material and the I identified from the X-ray diffraction pattern were 1 / I 2 The capacity of the evaluation cell is shown in Fig. 4. 1 / I 2 The relationship between the capacitance and the
[0099] [Table 1]
[0100] As is clear from the results shown in Table 1 and Figure 4, I 1 / I 2 The positive electrode active materials according to Examples 1 and 2, in which I is 0.30 or less, 1 / I 2The positive electrode active material according to Comparative Examples 1 and 2 has a larger capacity than the positive electrode active material according to Comparative Examples 1 and 2, in which the X-ray diffraction peak intensity derived from the O2 type structure is higher and the X-ray diffraction peak intensity derived from the T♯2 structure is lower, so that the capacity of the positive electrode active material is increased.
[0101] 6. Supplementary Information In the above examples, the precursor is obtained by coprecipitation, but the precursor can be obtained by other methods. In the above examples, the surface of the precursor is coated with a Na source by spray drying to obtain a composite, but the composite can be obtained by other methods. In the above examples, the Na-containing oxide having a P2 type structure and the Li-containing oxide having an O2 type structure are exemplified as those having a predetermined chemical composition, but the chemical composition of the Na-containing oxide and the Li-containing oxide is not limited to this. In addition, the Na-containing oxide and the Li-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.
[0102] 7. Summary As described above, in a positive electrode active material containing a Li-containing oxide, if the Li-containing oxide satisfies the following requirements (1) to (3), it can be said that the capacity of the positive electrode active material is large. (1) The Li-containing oxide has an O2 type structure. (2) The Li-containing oxide contains at least one element selected from the group consisting of Mn, Ni, and Co, Li, and O as constituent elements. (3) The X-ray diffraction pattern of the Li-containing oxide is 0≦I 1 / I 2 ≦0.30. Here, the above I 1 is the X-ray diffraction peak intensity derived from the (002) plane of the T#2 type structure, and 2 is the X-ray diffraction peak intensity originating from the (002) plane of the O2 type structure. [Explanation of symbols]
[0103] 100 Lithium-ion secondary battery 10 Cathode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector
Claims
1. A positive electrode active material comprising a Li-containing oxide, The Li-containing oxide has an O2 type structure, The Li-containing oxide contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Li, and O, The X-ray diffraction pattern of the Li-containing oxide is 0≦I 1 / I 2 ≦0.30 is satisfied, I 1 is the X-ray diffraction peak intensity originating from the (002) plane of the T#2 type structure, I 2 is the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure; Cathode active material.
2. The positive electrode active material according to claim 1 , The Li-containing oxide is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Cathode active material.
3. The positive electrode active material according to claim 1 , The Li-containing oxide contains at least Li, Mn, Ni, Co, and O as constituent elements. Cathode active material.
4. A lithium ion secondary battery, A positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 3. Lithium-ion secondary battery.
Citation Information
Patent Citations
Secondary battery
JP2016095934A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068555A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068556A
Composite compound, lithium-containing composite oxide, and methods respectively for producing said products
WO2014175191A1
Nonaqueous-electrolyte secondary battery
WO2015115025A1