Manufacturing method of electrode sheet and manufacturing device of electrode sheet
By forming cuts in the coating film before removal, the method addresses the issue of edge damage from chip adhesion, achieving enhanced linearity and dimensional accuracy in the electrode layer.
Patent Information
- Application Number
- JP2023075030
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for intermittently transferring a coating film of an electrode mixture onto a current collector foil using a drive roll result in damaged edge straightness due to sticky chips generated during film scraping, leading to poor linearity of the electrode layer.
Forming cuts in the coating film before removal to minimize chip generation, using a blade or wire to create notches, and then transferring the uncut portion to the current collector foil.
The method ensures excellent linearity at the edges of the electrode layer by reducing chip adhesion, resulting in improved dimensional accuracy and edge straightness.
Smart Images

Figure 2024159191000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method and an apparatus for manufacturing an electrode sheet. [Background technology]
[0002] 2. Description of the Related Art Known manufacturing devices for electrode sheets having an electrode layer on the surface of a current collector foil include devices that use a drive roll to continuously manufacture the sheets (see, for example, Patent Document 1). In a method for manufacturing an electrode sheet using this device, an electrode mixture containing an electrode active material is supplied between a first roll and a second roll rotating opposite to each other to form a coating film of the electrode mixture, and this coating film is adhered to the surface of the second roll. Furthermore, the coating film adhered to the surface of the second roll is transferred onto a current collecting foil conveyed by a third roll rotating opposite to the second roll. Through the above steps, an electrode sheet is manufactured in a state in which an electrode layer made of a coating film of the electrode mixture is disposed on the current collecting foil. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-184690 A Summary of the Invention [Problem to be solved by the invention]
[0004] Depending on the application of the electrode sheet, it is desirable that the coating film of the electrode mixture is intermittently transferred to the current collector (i.e., the coating film cut to a predetermined size is spaced apart). As a method for intermittently transferring the coating film of the electrode mixture to the current collector foil using a device equipped with a driving roll, for example, a method for removing a part of the coating film by contacting the second roll with a blade for scraping the coating film formed on the second roll is considered. However, in the above method, highly adhesive chips generated when scraping off a part of the coating film with a blade may adhere to the end surface of the coating film, which may impair the linearity of the end of the electrode layer transferred to the current collector. The problem to be solved by one embodiment of the present disclosure is to provide a method for manufacturing an electrode sheet having excellent linearity of the end of the electrode layer. [Means for solving the problem]
[0005] Means for solving the above problems include the following embodiments. A step of supplying an electrode mixture between the first roll and the second roll to form a coating film of the electrode mixture on the surface of the second roll; forming a notch in the coating film formed on the surface of the second roll; removing a portion of the coating film in which the notch is formed; and transferring the coating film that is not removed in the removing step onto the current collecting foil that is transported by a third roll. Effect of the Invention
[0006] According to one embodiment of the present disclosure, there is provided a method for manufacturing an electrode sheet having excellent linearity at the edge of an electrode layer. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic side view showing one embodiment of an electrode sheet manufacturing apparatus. FIG. [Diagram 2] FIG. 2 is a partially enlarged view of the electrode sheet manufacturing apparatus shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The method for producing an electrode sheet according to the present disclosure includes: A step of supplying an electrode mixture between the first roll and the second roll to form a coating film of the electrode mixture on the surface of the second roll; forming a notch in the coating film formed on the surface of the second roll; removing a portion of the coating film in which the notch is formed; and transferring the coating film that is not removed in the removing step onto the current collecting foil that is transported by a third roll.
[0009] Hereinafter, the process of supplying an electrode mixture between the first roll and the second roll and forming a coating film of the electrode mixture on the surface of the second roll is also referred to as the "coating film forming process." The process of forming a notch in the coating film formed on the surface of the second roll is also referred to as the "notch forming process." The process of removing a part of the coating film in which a notch has been formed is also referred to as the "removing process." The process of transferring the coating film that is not removed in the removing process to the current collecting foil transported by the third roll is also referred to as the "transferring process."
[0010] In the method of the present disclosure, before removing a portion of the coating film formed on the surface of the second roll, a notch is formed in the coating film. That is, in the method of the present disclosure, the coating film is removed along the notch formed in the coating film in advance. Therefore, chips are less likely to be generated when removing a portion of the coating film compared to removing a portion of the coating film without a notch. Therefore, adhesion of chips to the edge when removing a portion of the coating film is suppressed, and the straightness of the edge of the coating film is excellent.
[0011] Hereinafter, an embodiment of the manufacturing method of the electrode sheet of the present disclosure will be described with reference to the drawings. Note that the manufacturing method of the electrode sheet of the present disclosure is not limited thereto.
[0012] FIG. 1 is a schematic side view showing one embodiment of an electrode sheet manufacturing apparatus that can be used in the electrode sheet manufacturing method of the present disclosure. The electrode sheet manufacturing apparatus 10 shown in FIG. 1 includes a first roll 11, a second roll 12, a third roll 13, and an electrode mixture supply unit 15. The first roll 11, the second roll 12, and the third roll 13 rotate in the directions indicated by the arrows. The electrode mixture 16 supplied from the supply unit 15 to between the first roll 11 and the second roll 12 forms a coating film 16A on the surface of the second roll 12. The coating film 16A is transferred onto a current collector foil 17 conveyed in the CD direction by the third roll 13 in the state of a coating film 16B with the end cut.
[0013] Fig. 2 is a partial enlarged view of the electrode sheet manufacturing apparatus 10 shown in Fig. 1. As shown in Fig. 2, a slit is formed in the coating film 16A formed on the surface of the second roll 12 at the position indicated by the arrow X. A part of the coating film 16A where the slit is formed is removed from the second roll 12 at the position indicated by the arrow Y. The part of the coating film 16A that is not removed is transferred to the current collector 17 on the third roll 13 as the coating film 16B.
[0014] As described above, part of coating film 16A formed on second roll 12 is removed before being transferred to current collecting foil 17. Therefore, current collecting foil 17 has alternating regions where coating film 16B is transferred and regions where coating film 16B is not transferred.
[0015] 1 and 2, the axes of the first roll 11, the second roll 12, and the third roll 13 are arranged on a straight line, but the present disclosure is not limited to such an arrangement. For example, the angle formed by the line connecting the axis of the first roll 11 and the axis of the second roll 12 and the line connecting the axis of the second roll 12 and the axis of the third roll 13 may be selected from the range of 0° to 90°.
[0016] In the coating film forming step, the electrode mixture is supplied between the first roll and the second roll, and a coating film of the electrode mixture is formed on the surface of the second roll. The thickness of the coating film formed in the coating film forming step is not particularly limited and can be set according to the application of the electrode sheet. For example, the thickness of the coating film can be 50 μm to 600 μm. The electrode mixture used to form the coating film contains at least an active material and a solvent. The electrode mixture may further contain components such as a binder and a conductive material.
[0017] In the slit forming step, slits are formed in the coating film formed on the surface of the second roll. The direction of the slits when observed from above the coating film is preferably along the width direction of the coating film (i.e., the direction perpendicular to the conveying direction of the coating film). Specifically, the angle between the width direction of the coating film and the direction of the slits is preferably within the range of 0°±20°, more preferably within the range of 0°±10°, and even more preferably 0°.
[0018] The intervals between the slits formed in the coating film may or may not be equal. For example, the intervals between the slits formed in the coating film may be alternately repeated between intervals corresponding to the dimensions of the area where the coating film is transferred onto the current collecting foil (i.e., the transfer area) and intervals corresponding to the dimensions of the area where the coating film is not transferred onto the current collecting foil (i.e., the non-transfer area).
[0019] The direction of the cuts when observed from the side of the coating film is preferably formed along the thickness direction of the coating film (i.e., the direction perpendicular to the tangent line of the second roll). Specifically, the angle between the thickness direction of the coating film and the direction of the cuts is preferably within the range of 0°±20°, more preferably within the range of 0°±10°, and even more preferably 0°.
[0020] The method of forming the slits in the coating film is not particularly limited. For example, the method may be performed by alternately moving the means for forming the slits in the coating film close to the second roll and moving it away from the second roll. These operations may be performed manually or using a driving device or the like. From the viewpoint of the accuracy of the intervals between the slits, it is preferable to form the slits using a servo motor.
[0021] The means for forming the slits in the coating film is not particularly limited. From the viewpoint of linearity of the end of the coating film transferred to the current collector foil, it is preferable to form the slits using a blade or a wire. The material of the blade or wire used to form the slits is not particularly limited, and may include resin, metal, etc. From the viewpoint of suppressing adhesion of the electrode mixture to the blade or wire, it is preferable that the blade or wire contains a resin.
[0022] When the blade or wire contains a resin, examples of the resin include fluororesin, nylon resin, fluorocarbon resin, polyester resin, polyolefin resin, polystyrene resin, and polyether ketone ketone resin. From the viewpoint of suppressing adhesion of the electrode mixture, the resin is preferably one or more resins selected from fluororesin, polyolefin resin, and polyolefin resin, and more preferably fluororesin. As the fluororesin, one or more resins selected from polyvinylidene fluoride and Teflon resin are preferred, and more preferably polyvinylidene fluoride. From the viewpoint of chemical resistance, the resin is preferably polyolefin resin, and more preferably polypropylene resin. When the blade or wire comprises a metal, the metal may be iron, manganese, nickel, chromium, molybdenum, magnesium, silicon, aluminum, titanium, alloys thereof, or the like.
[0023] From the viewpoint of suppressing adhesion of the electrode mixture, it is preferable that the means for forming the notches in the coating film has a small contact area with the coating film, and therefore a wire is preferable as the means for forming the notches in the coating film.
[0024] From the viewpoint of dimensional accuracy of the notch formed in the coating film, the wire thickness is preferably 0.17 mm to 4.00 mm, more preferably 0.20 mm to 1.00 mm, and even more preferably 0.25 mm to 0.50 mm. In addition, by setting the wire thickness within the above numerical range, adhesion of the coating film to the wire can be effectively prevented. In the present disclosure, the wire thickness means the diameter of a circle that has the smallest area when a circle that can surround the entire wire observed in the cross-sectional image of the wire is drawn. When the wire thickness is not constant, the arithmetic average value of the thicknesses measured at five points is taken as the wire thickness.
[0025] From the viewpoint of suppressing breakage of the wire, the tensile strength of the wire is preferably 21 MPa to 2600 MPa, more preferably 50 MPa to 500 MPa, and further preferably 50 MPa to 200 MPa. In the present disclosure, the tensile strength of the wire is measured by an AllroundLine manufactured by Zwick Roell.
[0026] When a blade is used to form a cut in the coating film, the thickness of the tip of the blade is preferably 5 mm or less, more preferably 1 mm or less, from the viewpoint of dimensional accuracy of the cut, and is preferably 50 μm or more, from the viewpoint of durability.
[0027] In the removing step, a part of the coating film in which the slit is formed is removed. In the method of the present disclosure, the removal of the coating film is performed on the area partitioned by the slit formed in the coating film. Therefore, the linearity of the end of the coating film that remains without being removed is excellent. The method of removing a part of the coating film is not particularly limited. For example, the coating film may be removed by inserting a means for removing the coating film into the coating film at a position corresponding to the slit formed in the coating film, and separating the area of the coating film from this slit to the adjacent slit from the second roll. As the means for removing the coating film, the blade or wire described above as the means for forming the slit may be used.
[0028] In the transfer step, the coating film that is not removed in the removal step is transferred to a current collector foil conveyed by a third roll. The current collector foil to which the coating film is transferred may be a conventionally known one. For example, an aluminum foil may be used as the current collector foil when producing a positive electrode sheet. For example, a copper foil may be used as the current collector foil when producing a negative electrode sheet. EXAMPLES
[0029] The present disclosure will be described in more detail below with reference to examples, but the invention of the present disclosure is not limited to these examples.
[0030] <Example> An electrode sheet manufacturing apparatus having the configuration shown in Figures 1 and 2 was prepared. The minimum gap between the first roll and the second roll was 220 µm, and the minimum gap between the second roll and the third roll was 130 µm. The rotation speed of the first roll was 0.75 rpm, the rotation speed of the second roll was 2 rpm, and the rotation speed of the third roll was 5 rpm.
[0031] The incision forming part for forming incisions in the coating film was made of polyvinylidene fluoride, and was a wire (cross-sectional shape: circular) with a thickness of 0.30 mm and a tensile strength of 66.5 MPa. The removal part for removing a part of the coating film was made of polyvinylidene fluoride, and was a blade (tip thickness: 500 μm) with a shape capable of scraping off the coating film on the second roll.
[0032] An electrode sheet was produced using the above-mentioned device through the following steps (1) to (5). The electrode mixture was a mixture of 97.3% by mass of lithium nickel manganese composite oxide (positive electrode active material), 1.5% by mass of carbon nanotubes (conductive material), 1.2% by mass of polyvinylidene fluoride (binder), and further mixed with N-methyl-2-pyrrolidone (solvent) (solid concentration 89% by mass). The electrode mixture was a wet granule.
[0033] (1) An electrode mixture was supplied between the first roll and the second roll, and a coating film having a thickness of 200 μm was formed on the surface of the second roll. The formed coating film was transported by the rotation of the second roll.
[0034] (2) A slit was formed in the coating film on the second roll using a wire. The slits were formed so that the coating film divided by the slits alternated between areas with dimensions of 310 mm and areas with dimensions of 30 mm.
[0035] (3) The coating film in the area defined by the slits and measuring 30 mm was removed using a blade. The coating film was removed intermittently at intervals measuring 310 mm in the conveying direction. The removed coating film was collected by a collection device.
[0036] (4) The coating film that was not removed by the blade was transferred to the current collector foil transported by the second roll to the third roll. An aluminum foil with a thickness of 30 μm was used as the current collector foil. The thickness of the coating film that passed between the second roll and the third roll was 100 μm.
[0037] (5) The laminate of the current collecting foil and the coating film was transported to a drying device by the third roll, and the coating film was dried by passing through the device to obtain an electrode sheet in which an electrode layer was formed on the current collecting foil.
[0038] <Comparative Example> An electrode sheet was obtained in the same manner as in Example 1, except that a step of removing a part of the coating film using a wire was carried out without forming a cut in the coating film.
[0039] <Evaluation> The electrode sheets produced in the examples and the electrode sheets produced in the comparative examples were observed from the top surface of the electrode layer, and the dimensional variation at the starting end (the end corresponding to the downstream side in the conveying direction) and the ending end (the end corresponding to the upstream side in the conveying direction) of the electrode layer was evaluated. Specifically, a straight line corresponding to the design values of the start and end of the electrode layer was set as a reference line, and the maximum amount of protrusion of the electrode layer from the reference line (absolute value, mm) was measured. As a result, the maximum protruding amount of the electrode layer at the start and end of the electrode sheets produced in the examples was 0.5 mm or less, while the maximum protruding amount of the electrode layer at the start and end of the electrode sheets produced in the comparative examples was 2 mm or more. As shown by the above results, the electrode sheets of the examples in which notches were formed in the coating film before it was removed had smaller dimensional variation at the ends of the electrode layer and were more linear than the electrode sheets of the comparative examples in which notches were formed in the coating film before it was removed. [Explanation of symbols]
[0040] 10: electrode sheet manufacturing device, 11: first roll, 12: second roll, 13: third roll, 15: supply unit, 16: electrode mixture, 16A, 16B: coating film, 17: current collector foil
Claims
[Claim 1] A step of supplying an electrode mixture between the first roll and the second roll to form a coating film of the electrode mixture on the surface of the second roll; forming a notch in the coating film formed on the surface of the second roll; removing a portion of the coating film in which the notch is formed; and transferring the coating film that is not removed in the removing step onto the current collecting foil that is transported by a third roll.
Citation Information
Patent Citations
Electrode layer molding method and electrode layer molding apparatus
JP2022184690A