Thermoplastic elastomer composition and molded article
A thermoplastic elastomer composition with a specific polyamide resin, block copolymer, and hydrogenated petroleum resin blend addresses reactivity issues, achieving high-temperature rigidity and vibration damping, suitable for various applications.
Patent Information
- Application Number
- JP2023123978
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2023-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermoplastic resin compositions, such as those described in Patent Document 1, suffer from low reactivity between isobutylene-based block copolymers and polyamide 6, resulting in low loss tangent and inadequate high-temperature rigidity and vibration damping properties.
A thermoplastic elastomer composition is formulated with a specific ratio of polyamide resin (A) and block copolymer (B) containing aromatic vinyl and isobutylene blocks, along with a hydrogenated petroleum resin (C), ensuring a melting point of 200°C or higher, amino terminal groups of 3.0×10^-5 mol/g or more, and a loss tangent of 0.10 or more at 100 Hz and 23°C, enhancing reactivity and properties.
The composition exhibits excellent moldability, high-temperature rigidity, vibration damping properties, and spinnability, suitable for applications in automotive, electrical, and electronic products.
Smart Images

Figure 2024159392000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic elastomer composition comprising a polyamide resin (A), a block copolymer (B) containing a polymer block mainly composed of an aromatic vinyl compound having a reactive functional group and a polymer block mainly composed of isobutylene, and a hydrogenated petroleum resin (C), and a molded article using the same. [Background technology]
[0002] Conventionally, flexible polymeric materials have been widely used in which rubbers such as natural rubber or synthetic rubber are mixed with crosslinking agents and reinforcing agents and crosslinked under high temperature and pressure. However, such rubbers require a process of crosslinking and molding under high temperature and pressure for a long period of time, and have problems such as poor processability. In addition, since crosslinked rubber does not exhibit thermoplasticity, it is generally impossible to recycle it like thermoplastic resins. For this reason, various thermoplastic elastomers have been developed in recent years that can be easily manufactured into molded products using general-purpose melt molding techniques such as injection molding, hot press molding, and extrusion molding in the same way as ordinary thermoplastic resins.
[0003] Patent Document 1 discloses a thermoplastic resin composition having excellent impact resistance, gas barrier properties, and vibration damping properties, which contains a polar thermoplastic resin, an isobutylene-based block copolymer composed of a polymer block mainly composed of isobutylene and a polymer block composed of a monomer component not mainly composed of isobutylene, and a modified block polymer having at least one functional group selected from the group consisting of an acid anhydride group, a carboxyl group, a hydroxyl group, an amino group, and an epoxy group in at least one polymer block. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-225899 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the resin composition specifically disclosed in Patent Document 1 above, which is composed of an isobutylene-based block copolymer having a reactive functional group and polyamide 6, has low reactivity between the isobutylene-based block copolymer and polyamide 6, and the loss tangent of the resin composition at 23°C is low, so that excellent high-temperature rigidity and vibration damping properties could not be obtained.
[0006] An object of the present invention is to provide a thermoplastic elastomer composition which can be easily molded and has improved high-temperature rigidity and vibration damping properties. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention has the following configuration. (1) A melting point of 200°C or higher as measured by differential scanning calorimetry (DSC) and an amino end group content of 3.0 x 10 -5 mol / g or more, a block copolymer (B) including a polymer block mainly made of an aromatic vinyl compound having 0.1% by weight or more of reactive functional groups and a polymer block mainly made of isobutylene, and a hydrogenated petroleum resin (C), wherein the composition ratio (weight ratio) of the polyamide resin (A) to the copolymer (B) is (A):(B)=40:60 to 90:10, and the hydrogenated petroleum resin (C) is 0.01 to 20 parts by weight per 100 parts by weight of the total of the polyamide resin (A) and the copolymer (B). (2) The thermoplastic elastomer composition according to (1), characterized in that the loss tangent of the thermoplastic elastomer composition at a frequency of 100 Hz and a temperature of 23°C is 0.10 or more. (3) A molded article made of the thermoplastic elastomer composition according to (1) or (2). (4) Fibers made of the thermoplastic elastomer composition according to (1) or (2). (5) A sheet made of the thermoplastic elastomer composition according to (1) or (2). (6) A foam-molded article comprising the thermoplastic elastomer composition according to any one of (1) and (2). Effect of the Invention
[0008] The thermoplastic elastomer composition of the present invention can be easily molded using a general-purpose melt molding technique. In addition, the thermoplastic elastomer composition of the present invention has excellent vibration damping properties, high-temperature rigidity, blocking resistance, and spinnability, and can be used in, for example, automobile applications, electrical and electronic applications, fiber applications, film applications, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will now be described in further detail.
[0010] The present invention is a compound having a melting point of 200° C. or higher as measured by differential scanning calorimetry (DSC) and an amino terminal group content of 3.0×10 -5 The thermoplastic elastomer composition is a blend of a polyamide resin (A) having a molecular weight of 0.1 mol / g or more (hereinafter may be abbreviated as polyamide resin (A)), a block copolymer (B) (hereinafter may be abbreviated as copolymer (B)) containing a polymer block mainly made of an aromatic vinyl compound having 0.1 weight % or more of reactive functional groups and a polymer block mainly made of isobutylene, and a hydrogenated petroleum resin (C).
[0011] By blending a specific ratio of a copolymer (B) having 0.1% by weight or more of reactive functional groups with a polyamide resin (A) having excellent properties of high-temperature rigidity and moldability, the polyamide resin (A) and the copolymer (B) react appropriately, improving the flexibility of the polyamide. Furthermore, by blending a specific amount of a hydrogenated petroleum resin (C), the peak temperature of the loss tangent of the softened thermoplastic elastomer composition can be shifted to any temperature, thereby imparting vibration damping properties to the thermoplastic elastomer composition.
[0012] The polyamide resin (A) used in the present invention is a polyamide resin having a melting point of 200° C. or higher as measured by DSC.
[0013] The melting point of the polyamide resin (A) in the present invention by DSC can be determined by the following method. First, a differential scanning calorimeter (DSC-7 manufactured by PerkinElmer) is used, and two-point calibration (indium, lead) and baseline correction are performed. 8 to 10 mg of a polyamide resin sample is weighed out, and the sample is heated at a heating rate of 20°C / min, and the melting endothermic peak observed during the heating process is taken as the melting point.
[0014] If the melting point of the polyamide resin (A) is lower than 200° C., the high-temperature rigidity of the thermoplastic elastomer composition of the present invention decreases. The melting point of the polyamide resin (A) is preferably 205° C. or higher, and more preferably 210° C. or higher.
[0015] On the other hand, the upper limit of the melting point of the polyamide resin (A) is not particularly limited, but is preferably 350°C or less since this tends not to deteriorate the mechanical properties of the copolymer (B), more preferably 320°C or less, and even more preferably 300°C or less.
[0016] Examples of means for adjusting the melting point of the polyamide resin (A) within the above range include a method of selecting one having a desired melting point from polyamide resins having different melting points, and a method of adjusting the polymerization degree or copolymerization ratio of the polyamide resin.
[0017] There are no particular limitations on the polyamide resin (A) so long as it is a polyamide resin whose melting point satisfies the above-mentioned condition, but it can generally be obtained using amino acids, lactams or diamines and dicarboxylic acids as main raw materials. Representative examples of the raw material include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid; lactams such as ε-caprolactam and ω-laurolactam; aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, and 5-methylnonamethylenediamine; aromatic diamines such as metaxylylenediamine and paraxylylenediamine; 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis Alicyclic diamines such as (4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine; aliphatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodiumsulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid; and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid. In the present invention, polyamide homopolymers or copolymers derived from these raw materials can be used. Two or more of such polyamide resins may be used.
[0018] Specific examples of the polyamide resin (A) preferably used in the present invention include polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polytetramethylene adipamide (polyamide 46), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polyhexamethylene terephthalamide / polycaproamide copolymer (polyamide 6T / 6), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (polyamide 66 / 6T), polyhexamethylene adipamide / polyhexamethylene Examples of the polyamide include polyamide 66 / 6I, polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (polyamide 66 / 6T / 6I), polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (polyamide 6T / 6I), polyhexamethylene terephthalamide / poly(2-methylpentamethylene) terephthalamide copolymer (polyamide 6T / M5T), polyxylylene adipamide (polyamide XD6), and mixtures or copolymers thereof. Particularly preferred are polyamide 6, polyamide 610, and polyamide 66, and more preferred is polyamide 6.
[0019] The amount of amino terminal groups in the polyamide resin (A) is 3.0×10 -5 mol / g or more. The amount of amino end groups is 3.0×10 -5 If the amount of the amino terminal group of the polyamide resin (A) is 3.5×10 mol / g or more, the reactivity with the copolymer (B) can be increased. -5 mol / g or more is preferable, and 4.0×10 -5 The upper limit of the amount of amino terminal groups is 12.0×10 -5 mol / g or less, 11.5×10 -5 mol / g is preferred, 11.0×10 -5 mol / g is more preferable, 10.8×10 -5mol / g is more preferable. The amount of amino terminal groups in polyamide resin (A) can be determined by dissolving polyamide resin (A) in a phenol-ethanol mixed solvent (volume ratio of 83.5:16.5) and titrating with 0.02N aqueous hydrochloric acid. The amount of amino terminal groups can be determined by adjusting the ratio of diamine and dicarboxylic acid during polymerization or by reacting terminal carboxylic acid with diamine.
[0020] Although there is no particular restriction on the degree of polymerization of the polyamide resin (A), it is preferable that the relative viscosity measured at 25°C in a 98% concentrated sulfuric acid solution with a resin concentration of 0.01 g / ml is in the range of 1.5 to 7.0. If the relative viscosity is 1.5 or more, the melt viscosity of the thermoplastic elastomer composition during molding is appropriately high, which can suppress air entrapment during molding and further improve moldability. On the other hand, if the relative viscosity is 7.0 or less, the melt viscosity of the thermoplastic elastomer composition during molding is appropriately low, which can further improve moldability. By making the relative viscosity of the polyamide resin (A) 7.0 or less, the amount of amino terminal groups can be reduced to 3.0 x 10 -5 It can be mol / g or more.
[0021] The copolymer (B) used in the present invention is a block copolymer containing a polymer block mainly composed of an aromatic vinyl compound having 0.1% by weight or more of reactive functional groups and a polymer block mainly composed of isobutylene.
[0022] The reactive functional group in the copolymer (B) is not particularly limited, and examples thereof include at least one selected from an amino group, a carboxyl group, a carboxyl metal salt, a hydroxyl group, an acid anhydride group, an epoxy group, an isocyanate group, a mercapto group, an oxazoline group, a sulfonic acid group, etc. Among these, an amino group, a carboxyl group, a carboxyl metal salt, an epoxy group, an acid anhydride group, and an oxazoline group are preferably used because they have high reactivity and cause few side reactions such as decomposition and crosslinking.
[0023] Examples of the acid anhydride constituting the above-mentioned acid anhydride group include maleic anhydride, itaconic anhydride, endic anhydride, citraconic anhydride, and 1-butene-3,4-dicarboxylic anhydride. Two or more of these may be used simultaneously. Of these, maleic anhydride and itaconic anhydride are preferably used.
[0024] The polymer block mainly composed of an aromatic vinyl compound is a polymer block composed of 60% by weight or more, preferably 70% by weight or more, and more preferably 80% by weight or more of units derived from an aromatic vinyl compound.
[0025] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,6-dimethylstyrene, 2,4-dimethylstyrene, α-methyl-o-methylstyrene, α-methyl-m-methylstyrene, α-methyl-p-methylstyrene, β-methyl-o-methylstyrene, β-methyl-m-methylstyrene, β-methyl-p-methylstyrene, 2,4,6-trimethylstyrene, α-methyl-2,6-dimethylstyrene, α-methyl-2,4-dimethylstyrene, β-methyl-2,6-dimethylstyrene, β-methyl-2,4-dimethylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,6-dichlorostyrene, 2,4-dichlorostyrene, and α-chloro-o-chlorostyrene. , α-chloro-m-chlorostyrene, α-chloro-p-chlorostyrene, β-chloro-o-chlorostyrene, β-chloro-m-chlorostyrene, β-chloro-p-chlorostyrene, 2,4,6-trichlorostyrene, α-chloro-2,6-dichlorostyrene, α-chloro-2,4-dichlorostyrene, β-chloro-2,6-dichlorostyrene, β-chloro-2,4-dichlorostyrene, ot-butylstyrene, mt-butylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chloromethylstyrene, m-chloromethylstyrene, p-chloromethylstyrene, o-bromomethylstyrene, m-bromomethylstyrene, p-bromomethylstyrene, styrene derivatives substituted with silyl groups, indene, vinylnaphthalene, etc. Among these, styrene, α-methylstyrene, and mixtures thereof are preferred from the viewpoints of industrial availability and glass transition temperature.
[0026] The polymer block mainly composed of isobutylene is a polymer block composed of 60% by weight or more, preferably 70% by weight or more, and more preferably 80% by weight or more of units derived from isobutylene.
[0027] Both the polymer block mainly made of an aromatic vinyl compound and the polymer block mainly made of isobutylene can use the mutual monomers as copolymerization components, and can also use other cationic polymerizable monomer components. Examples of such monomer components include dienes, aliphatic olefins, silanes, vinyl ethers, vinylcarbazole, β-pinene, acenaphthylene, and other monomers. These can be used alone or in combination of two or more.
[0028] Examples of the diene monomer include butadiene, isobutylene, hexadiene, cyclopentadiene, cyclohexadiene, dicyclopentadiene, divinylbenzene, and ethylidenenorbornene.
[0029] Examples of the aliphatic olefin monomer include ethylene, propylene, 1-butene, 2-methyl-1-butene, 3-methyl-1-butene, pentene, hexene, cyclohexene, 4-methyl-1-pentene, vinylcyclohexane, octene, and norbornene.
[0030] Examples of the silane compound include vinyltrichlorosilane, vinylmethyldichlorosilane, vinyldimethylchlorosilane, vinyldimethylmethoxysilane, vinyltrimethylsilane, divinyldichlorosilane, divinyldimethoxysilane, divinyldimethylsilane, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, trivinylmethylsilane, γ-methacryloyloxypropyltrimethoxysilane, and γ-methacryloyloxypropylmethyldimethoxysilane.
[0031] Examples of the vinyl ether monomer include methyl vinyl ether, ethyl vinyl ether, (n-, iso)propyl vinyl ether, (n-, sec-, tert-, iso)butyl vinyl ether, methyl propenyl ether, and ethyl propenyl ether.
[0032] There is no particular restriction on the ratio of the polymer block mainly made of an aromatic vinyl compound to the polymer block mainly made of isobutylene, but from the viewpoint of loss tangent, the content of the polymer block mainly made of an aromatic vinyl compound in the copolymer (B) is preferably 10 to 50% by weight, more preferably 10 to 40% by weight. When the content of the polymer block mainly made of an aromatic vinyl compound is 10% by weight or more, sufficient mechanical properties are exhibited, and when it is 50% by weight or less, vibration damping properties can be obtained.
[0033] The molecular weight of the copolymer (B) is not particularly limited, but in terms of moldability, fluidity, rubber elasticity, etc., the weight average molecular weight measured by GPC is preferably 5,000 to 400,000, and more preferably 10,000 to 200,000. If the weight average molecular weight is 5,000 or more, sufficient mechanical properties are exhibited, while if it is 400,000 or less, the molded product will have excellent processability and fluidity.
[0034] The reactive functional group of the copolymer (B) is 0.1% by weight or more, when the copolymer (B) is 100% by weight. It is preferably 0.1% by weight or more, more preferably 0.15% by weight or more, and more preferably 0.2% by weight or more. There is no particular upper limit to the amount of the reactive functional group, but it is preferably 20% by weight or less, more preferably 18% by weight or less, and even more preferably 10% by weight or less.
[0035] When the amount of reactive functional groups introduced is less than 0.1% by weight, the reactivity with the polyamide resin (A) is insufficient. On the other hand, when the amount of reactive functional groups is more than 20% by weight, the reaction between the polyamide resin (A) and the copolymer (B) proceeds excessively, and the blocking resistance of the thermoplastic elastomer composition decreases.
[0036] The blending amount of polyamide resin (A) and copolymer (B) in the present invention is 40:60 to 90:10 in the ratio (weight ratio) of polyamide resin (A) to copolymer (B). If the amount of copolymer (B) is more than 40:60 in the ratio of (A):(B), the reaction between polyamide resin (A) and copolymer (B) proceeds excessively, and the high-temperature rigidity of the polyamide resin is not expressed. On the other hand, if the amount of copolymer (B) is less than 90:10 in the ratio of (A):(B), the loss tangent of the thermoplastic elastomer composition is low, and vibration damping properties cannot be imparted. (A):(B) is 40:60 to 90:10, preferably 45:55 to 90:10, more preferably 45:55 to 85:15, and even more preferably 50:50 to 85:15.
[0037] The present invention comprises blending 0.01 to 20 parts by weight of hydrogenated petroleum resin (C) with 100 parts by weight in total of polyamide resin (A) and copolymer (B).
[0038] Hydrogenated petroleum resin (C) is a resin obtained by hydrogenating petroleum resin that is solidified using an acid catalyst without isolating unsaturated hydrocarbons from the remaining fractions, mainly the C5 and C9 fractions, which are obtained by thermally cracking petroleum naphtha to extract the necessary fractions.
[0039] Examples of the hydrogenated petroleum resins include hydrogenated dicyclopentadiene resins and partially hydrogenated aromatic modified dicyclopentadiene resins, which are hydrogenated resins of C5 petroleum resins obtained by copolymerizing C5 fractions such as pentene, isoprene, piperine, and 1,3-pentadiene produced by thermal decomposition of petroleum naphtha; C9 hydrogenated petroleum resins obtained by copolymerizing C9 fractions such as indene, vinyltoluene, and α- or β-methylstyrene produced by thermal decomposition of petroleum naphtha; and copolymerized hydrogenated petroleum resins of the C5 fraction and the C9 fraction.
[0040] Examples of commercially available hydrogenated dicyclopentadiene resins include Escolez (registered trademark) 5300 and 5400 series manufactured by Donex Co., Ltd. and Eastotac (registered trademark) H series manufactured by Eastman Chemical Japan Co., Ltd.
[0041] An example of a commercially available product of the partially hydrogenated aromatic modified dicyclopentadiene resin is the Escolez (registered trademark) 5600 series manufactured by Tonex Corporation.
[0042] Examples of commercially available C9 hydrogenated petroleum resins include Arcon (registered trademark) P and M series manufactured by Arakawa Chemical Industries, Ltd.; and Polystolyn manufactured by Eastman Chemical Company.
[0043] Examples of copolymerized hydrogenated petroleum resins of C5 fraction and C9 fraction include the Imab (registered trademark) series manufactured by Idemitsu Kosan Co., Ltd.
[0044] From the viewpoint of compatibility with the copolymer (B), C9 hydrogenated petroleum resin is preferred.
[0045] The amount of hydrogenated petroleum resin (C) in the present invention is 0.01 to 20 parts by weight based on 100 parts by weight of the total of polyamide resin (A) and copolymer (B). If the amount is less than 0.01 part by weight, the glass transition temperature of copolymer (B) cannot be shifted to a higher temperature, and the loss tangent of the thermoplastic elastomer composition at a frequency of 100 Hz and a temperature of 23°C does not reach 0.10 or more, resulting in poor vibration damping. On the other hand, if the amount exceeds 20 parts by weight, surface tack occurs due to bleed-out, which is not preferable. The amount of hydrogenated petroleum resin is preferably 0.01 to 15 parts by weight, more preferably 0.1 to 15 parts by weight, and even more preferably 1.5 to 15 parts by weight.
[0046] The loss tangent of the thermoplastic elastomer composition of the present invention is preferably 0.10 or more at a frequency of 100 Hz and a temperature of 23° C. By making the loss tangent at a frequency of 100 Hz and a temperature of 23° C. 0.10 or more, it is possible to impart vibration damping properties to a molded article made of the thermoplastic elastomer composition.
[0047] The loss tangent at a frequency of 100 Hz and a temperature of 23°C can be determined by the following method. Using a viscoelasticity measuring device (Seiko Instruments, DMS6100), measurements are taken under conditions of a nitrogen atmosphere, a heating rate of 2°C / min, and a frequency of 100 Hz to determine the storage modulus and loss modulus. The loss modulus at a temperature of 23°C is divided by the storage modulus to determine the loss tangent at a temperature of 23°C.
[0048] In order to achieve a loss tangent of 0.10 or more at a frequency of 100 Hz and a temperature of 23°C, the blending ratio of polyamide resin (A) and copolymer (B) should be 40:60 to 90:10 (weight ratio) (A):(B) and 0.01 to 20 parts by weight of hydrogenated petroleum resin (C) should be blended per 100 parts by weight of the total of polyamide resin (A) and copolymer (B).
[0049] The loss tangent at a frequency of 100 Hz and a temperature of 23° C. is preferably 0.10 or more, more preferably 0.13 or more, and even more preferably 0.15 or more.
[0050] There is no particular upper limit to the loss tangent at a frequency of 100 Hz and a temperature of 23° C., but from the viewpoint of maintaining the shape of the molded product, it is preferably 5.0 or less.
[0051] The thermoplastic elastomer composition of the present invention has excellent blocking resistance. Here, blocking resistance indicates the adhesion of pellets. The better the blocking resistance, the better the handling properties of the pellets.
[0052] The blocking resistance can be confirmed by the following method: Pellets made of a thermoplastic elastomer composition are vacuum dried at 80° C. for 15 hours. At that time, adhesion (blocking) between the pellets is confirmed.
[0053] Blocking resistance can be achieved by setting the blending ratio of polyamide resin (A) and copolymer (B) to a ratio (weight ratio) of polyamide resin (A) to copolymer (B) (A):(B) of 40:60 to 90:10, and blending 0.01 to 20 parts by weight of hydrogenated petroleum resin (C) per 100 parts by weight of the total of polyamide resin (A) and copolymer (B).
[0054] The thermoplastic elastomer composition of the present invention has excellent spinnability.
[0055] Spinnability can be confirmed by the following method. Thermoplastic elastomer composition pellets are vacuum dried at 80°C for 15 hours. The vacuum dried pellets are filled into a cylinder set at a test temperature of 280°C using a Toyo Seiki Co., Ltd. Capillograph 1C (cylinder diameter 9.55 mm, orifice length 10.0 mm, inner diameter 1.0 mm), and the thermoplastic elastomer composition is compressed and held for 30 minutes to melt the pellets. The pellets are then heated at a shear rate of 24.3 sec. -1 The mixture is discharged under the above conditions, and taken up at a take-up speed of 200 m / min, and spinnability is confirmed.
[0056] In order to have excellent spinnability, it is preferable that the blending ratio of polyamide resin (A) and copolymer (B) is 40:60 to 90:10 (weight ratio) (A):(B), and that 0.01 to 20 parts by weight of hydrogenated petroleum resin (C) is blended per 100 parts by weight of the total of polyamide resin (A) and copolymer (B).
[0057] The thermoplastic elastomer composition of the present invention has excellent sheet moldability.
[0058] Sheet moldability can be confirmed by the following method. Thermoplastic elastomer composition pellets are vacuum dried at 80°C for 15 hours. The vacuum dried pellets are melted and kneaded in an extruder, and the resin is extruded in a certain direction from a die and fixed on a roll to form into a sheet.
[0059] In order to have excellent sheet formability, it is preferable that the blending ratio of polyamide resin (A) and copolymer (B) is 40:60 to 90:10 (weight ratio) (A):(B), and that 0.01 to 20 parts by weight of hydrogenated petroleum resin (C) is blended per 100 parts by weight of the total of polyamide resin (A) and copolymer (B).
[0060] The thermoplastic elastomer composition of the present invention may contain other components than the components (A), (B) and (C) as necessary, provided that the properties of the composition are not impaired. Examples of such other components include fillers, copper compounds, potassium compounds, thermoplastic resins other than the component (A), rubbery polymers other than the component (B), and various additives.
[0061] For example, by blending a filler, the strength and dimensional stability of the molded product can be improved. The shape of the filler may be fibrous or non-fibrous, and a combination of a fibrous filler and a non-fibrous filler may be used. Examples of fibrous fillers include glass fiber, glass middle fiber, carbon fiber, potassium titanate whisker, zinc oxide whisker, aluminum nitrate whisker, aramid fiber, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber. Examples of non-fibrous fillers include silicates such as wollastonite, zeolite, sericite, kaolin, mica, pyrophyllite, bentonite, asbestos, and alumina silicate; metal oxides such as alumina, magnesium oxide, zirconium oxide, titanium oxide, and iron oxide; metal carbonates such as calcium carbonate, magnesium carbonate, and dolomite; metal sulfates such as calcium sulfate and barium sulfate; metal hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide; glass beads, ceramic beads, boron nitride, and silicon carbide. These may be hollow. In addition, it is preferable to pretreat these fibrous and / or non-fibrous fillers with a coupling agent before use in order to obtain better mechanical properties. Examples of the coupling agent include isocyanate compounds, organic silane compounds, organic titanate compounds, organic borane compounds, and epoxy compounds.
[0062] Examples of copper compounds include copper chloride, copper bromide, copper iodide, copper acetate, copper acetylacetonate, copper carbonate, copper fluoroborate, copper citrate, copper hydroxide, copper nitrate, copper sulfate, and copper oxalate. The copper compound may contain two or more of these. Among these copper compounds, those that are industrially available are preferred, and copper halides are suitable. Examples of copper halides include copper iodide, copper bromide, copper bromide, and copper chloride. The copper compound is more preferably copper iodide.
[0063] Examples of potassium compounds include potassium iodide, potassium bromide, potassium chloride, potassium fluoride, potassium acetate, potassium hydroxide, potassium carbonate, and potassium nitrate. The potassium compound may contain two or more of these. Among these potassium compounds, potassium iodide is preferred. By containing a potassium compound, the surface appearance, weather resistance, and mold corrosion resistance of the molded product can be improved.
[0064] The potassium compound inhibits the liberation and precipitation of copper, and therefore, it is believed that the combined use of a copper compound and a potassium compound has the effect of promoting the reaction between the copper compound and the polyamide resin (A).
[0065] Examples of the thermoplastic resins include polyamide resins other than the component (A), polyester resins, polyphenylene sulfide resins, polyphenylene oxide resins, polycarbonate resins, polylactic acid resins, polyacetal resins, polysulfone resins, tetrafluoroethylene resins, polyetherimide resins, polyamideimide resins, polyimide resins, polyethersulfone resins, polyetherketone resins, polythioetherketone resins, polyetheretherketone resins, styrene-based resins such as polystyrene resins and ABS resins, and polyalkylene oxide resins. Two or more of such thermoplastic resins can be blended. When blending a polyamide resin other than the polyamide resin (A), it is preferable that the amount of the polyamide resin is 5 parts by weight or less relative to 100 parts by weight of the polyamide resin (A).
[0066] Examples of the rubber polymer of component (B) include styrene-based rubber, olefin-based resin, acrylic rubber, silicone-based rubber, fluorine-based rubber, nitrile-based rubber, vinyl-based rubber, urethane-based rubber, polyamide elastomer, polyester elastomer, ionomer, etc. These may have a reactive functional group, and two or more of these may be blended together.
[0067] The structure of the rubbery polymer is not particularly limited, and may be, for example, a so-called core-shell type multilayer structure consisting of at least one layer made of rubber and one or more layers made of a different type of polymer. The number of layers constituting the multilayer structure may be two or more, and may be three or more or four or more, but it is preferable to have one or more rubber layers (core layers) inside. The type of rubber constituting the rubber layer of the multilayer structure is not particularly limited, and examples thereof include rubbers obtained by polymerizing acrylic components, silicone components, styrene components, nitrile components, conjugated diene components, urethane components, ethylene components, propylene components, isobutene components, etc. The type of different polymers constituting the layers other than the rubber layer of the multilayer structure is not particularly limited as long as they are polymers having thermoplasticity, but polymers having a higher glass transition temperature than the rubber layer are preferred. Examples of polymers having thermoplasticity include polymers containing unsaturated carboxylic acid alkyl ester units, unsaturated carboxylic acid units, unsaturated glycidyl group-containing units, unsaturated dicarboxylic acid anhydride units, aliphatic vinyl units, aromatic vinyl units, vinyl cyanide units, maleimide units, unsaturated dicarboxylic acid units, and other vinyl units.
[0068] Examples of the various additives include color inhibitors, antioxidants such as hindered phenols and hindered amines, release agents such as ethylene bisstearylamide and higher fatty acid esters, plasticizers, heat stabilizers, lubricants, ultraviolet protection agents, colorants, flame retardants, and foaming agents.
[0069] The thermoplastic elastomer composition of the present invention has excellent high-temperature rigidity. Here, the melting point of the thermoplastic elastomer composition is used as an index of high-temperature rigidity. The higher the melting point of the thermoplastic elastomer composition, the more excellent the high-temperature rigidity is judged to be.
[0070] From the viewpoint of shape retention of a molded product, it is preferable that the melting point of the thermoplastic elastomer composition is 200° C. or higher. The melting point of the thermoplastic elastomer is preferably 200° C. or higher, more preferably 205° C. or higher, and even more preferably 210° C. or higher.
[0071] On the other hand, there is no particular upper limit to the melting point of the thermoplastic elastomer composition, but from the viewpoint of productivity, it is preferably 350° C. or lower, more preferably 320° C. or lower, and even more preferably 300° C. or lower.
[0072] The melting point of the thermoplastic elastomer composition can be adjusted to fall within the above range, for example, by using a polyamide resin (A) having a melting point of 200° C. or higher as measured by DSC.
[0073] Next, a method for producing the thermoplastic elastomer composition of the present invention will be described. The method for producing the thermoplastic elastomer composition of the present invention includes, for example, a method of kneading polyamide resin (A), copolymer (B), hydrogenated petroleum resin (C), and other components as necessary, all at once. As the kneading device, for example, a known kneading device such as a Banbury mixer, roll, extruder, etc. can be adopted. When other components such as various additives are blended into the thermoplastic elastomer composition of the present invention, they can be blended at any stage. For example, when the thermoplastic elastomer composition of the present invention is produced using a twin-screw extruder, there are a method of blending other components simultaneously when blending polyamide resin (A), copolymer (B), and hydrogenated petroleum resin (C), a method of blending other components by a method such as side feed during melt-kneading of polyamide resin (A), copolymer (B), and hydrogenated petroleum resin (C), and a method of blending other components with polyamide resin (A) and copolymer (B) in advance, melt-kneading, and then blending hydrogenated petroleum resin (C).
[0074] The thermoplastic elastomer composition of the present invention can be molded by any method to obtain a molded product, and the molded shape can be any shape. Examples of the molding method include extrusion molding, injection molding, blow molding, calendar molding, compression molding, vacuum molding, foam molding, blow molding, and rotational molding. Examples of the molded shape include pellets, plates, fibers, strands, films or sheets, pipes, hollows, boxes, and the like.
[0075] The thermoplastic elastomer composition of the present invention can be foamed. Examples of the foaming method include a method of adding a foaming agent for foaming the thermoplastic elastomer when melt-kneading the thermoplastic elastomer composition, and then molding after melt-kneading; a method of dry-blending a foaming agent for foaming the thermoplastic elastomer composition with the thermoplastic elastomer composition of the present invention before molding, and then molding; a method of impregnating a thermoplastic elastomer composition with a supercritical gas and molding it; a method of impregnating a thermoplastic elastomer composition molded in an autoclave with a supercritical gas and foaming it; and a method of impregnating a thermoplastic elastomer composition with a supercritical gas when melt-kneading it, and then foaming it; and a physical foaming method of impregnating a thermoplastic elastomer composition with a supercritical gas and foaming it when melt-kneading it. From the viewpoint of productivity and quality, physical foaming is preferred.
[0076] The supercritical gas used in physical foaming is not particularly limited as long as it can dissolve in the thermoplastic elastomer composition and is inactive, but carbon dioxide and nitrogen are preferred from the standpoint of safety and cost. The supercritical gas is preferably used in an amount of 0.01 to 20 parts by weight, more preferably 0.05 to 10 parts by weight, per 100 parts by weight of the thermoplastic elastomer composition.
[0077] The molded article of the present invention has excellent vibration-damping properties, high-temperature rigidity, blocking resistance, and spinnability, and can therefore be used in a wide range of applications, including automobiles, electrical and electronic applications, fibers, and films. EXAMPLES
[0078] The effects of the present invention will be described more specifically below with reference to examples. Note that the present invention is not limited to the following examples. Evaluations in each example and comparative example were performed by the following methods.
[0079] (1) Melting point of polyamide resin The melting point of the polyamide resin used in each Example and Comparative Example was determined by DSC. First, a differential scanning calorimeter (PerkinElmer DSC-7) was used, and two-point calibration (indium, lead) and baseline correction were performed. 8 to 10 mg of the polyamide resin was weighed and heated at a heating rate of 20°C / min, and the melting endothermic peak temperature observed during the heating process was taken as the melting point.
[0080] (2) High temperature stiffness: Melting point The melting point of the thermoplastic elastomer composition pellets obtained in each of the Examples and Comparative Examples was determined by DSC measurement. First, a differential scanning calorimeter (PerkinElmer DSC-7) was used, and two-point calibration (indium, lead) and baseline correction were performed. 8 to 10 mg of the thermoplastic elastomer composition was weighed and heated at a heating rate of 20°C / min, and the melting endothermic peak temperature observed during the heating process was taken as the melting point.
[0081] (3) Vibration damping: loss tangent (tan δ) Using the thermoplastic elastomer compositions obtained in each of the Examples and Comparative Examples, strips of 40 mm x 8 mm x 1 mm were cut out from the prepared 80 mm x 80 mm x 1 mm flat plates. The cut strips were used to determine the storage modulus and loss modulus under conditions of a nitrogen atmosphere, a heating rate of 2°C / min, and a frequency of 100 Hz using a viscoelasticity measuring device (Seiko Instruments, DMS6100). The loss modulus at a temperature of 23°C was divided by the storage modulus to determine the loss tangent (tan δ) at a temperature of 23°C.
[0082] (4) Productivity: Blocking The thermoplastic elastomer composition pellets obtained in each of the Examples and Comparative Examples were vacuum dried at 80° C. for 15 hours, during which adhesion (blocking) between the pellets was confirmed.
[0083] (5) Spinnability: High-speed take-up The thermoplastic elastomer composition pellets obtained in each of the Examples and Comparative Examples were vacuum dried at 80° C. for 15 hours. The vacuum dried pellets were filled into a cylinder (Cylinder diameter 9.55 mm, Orifice length 10.0 mm, inner diameter 1.0 mm) manufactured by Toyo Seiki Seisakusho Co., Ltd., with the test temperature set to 280° C., compressed, and held for 30 minutes to melt, and then heated at a shear rate of 24.3 sec -1 The fibers were discharged under the above conditions and taken up at a take-up speed of 200 m / min. Those that could be taken up were rated ◯ (good spinnability), and those that could not be taken up were rated × (poor spinnability).
[0084] (6) Sheet formability Thermoplastic elastomer composition pellets obtained in each Example and Comparative Example were vacuum dried at 80°C for 15 hours. The vacuum dried pellets were melted and kneaded in an extruder, and the resin was extruded in a certain direction from a mold and fixed on a roll to form a sheet. Those that could be molded into a sheet were rated ◯ (good sheet moldability), and those that could not were rated × (poor sheet moldability).
[0085] The raw materials and their abbreviations used in each of the Examples and Comparative Examples are shown below.
[0086] [SIBS-g-MAH-1] SIBS (SIBSTAR102T), maleic anhydride (FUJIFILM Wako Pure Chemical Industries, Ltd.), Perhexa 25B (NOF Corporation, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, organic peroxide), and Irganox1010 (BASF Japan, antioxidant) were premixed in a Henschel mixer at a weight ratio of 100:1.0:0.5:0.5 for SIBS:maleic anhydride:organic peroxide:antioxidant. This premix was fed to a twin-screw extruder (cylinder temperature: 200°C) and graft-modified under melt conditions to obtain SIBS-g-MAH-1. The amount of maleic anhydride bonded to SIBS-g-MAH-1 at that time was 0.65% by weight.
[0087] [SIBS-g-MAH-2] SIBS (SIBSTAR102T), maleic anhydride (FUJIFILM Wako Pure Chemical Industries, Ltd.), Perhexa 25B (NOF Corporation, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, organic peroxide), and Irganox1010 (BASF Japan, antioxidant) were premixed in a Henschel mixer at a weight ratio of 100:0.1:0.05:0.5 for SIBS:maleic anhydride:organic peroxide:antioxidant. This premix was fed to a twin-screw extruder (cylinder temperature: 220°C) and graft-modified under melt conditions to obtain SIBS-g-MAH-2. The amount of maleic anhydride bonded to SIBS-g-MAH-2 at that time was 0.04% by weight. PA6: Polyamide 6 resin "Amilan" (registered trademark) manufactured by Toray Industries, Inc. (melting point 224°C, relative viscosity 2.70 at 25°C in a 98% concentrated sulfuric acid solution with a resin concentration of 0.01 g / ml, amino end group amount 7.0 x 10 -5 mol / g) (corresponding to polyamide resin (A)) PA12: Polyamide 12 resin "DAIAMID" (registered trademark) from Daicel Evonik Co., Ltd. (melting point 178°C, amino end group amount 1.0 x 10 -5 mol / g) SIBS-g-MAH-1: Maleic anhydride-modified styrene-isobutylene-styrene copolymer produced by the method described in [SIBS-g-MAH-1] (styrene content 15% by weight, maleic anhydride content 0.65% by weight, corresponds to copolymer (B)). SIBS-g-MAH-2: Maleic anhydride-modified styrene-isobutylene-styrene copolymer (styrene content 15 wt%, maleic anhydride content 0.04 wt%) produced by the method described in [SIBS-g-MAH-1]. Hydrogenated petroleum resin: C9 hydrogenated petroleum resin "Alcon" P-140 (Arakawa Chemical Industries, Ltd.) (corresponding to hydrogenated petroleum resin (C)).
[0088] [Examples 1 to 5, Comparative Examples 1 to 7] The raw materials shown in Table 1 were melt-kneaded by feeding them to a twin-screw extruder (TEX30XSSST manufactured by JSW) (L / D=45.5 (where L is the length from the raw material inlet to the outlet, and D is the screw diameter) with a cylinder temperature set to 250°C, a screw arrangement with two kneading zones, and a screw rotation speed of 250 rpm. The guts were then passed through a cooling bath filled with water adjusted to 10°C for 15 seconds to quench and solidify the structure. The mixture was pelletized with a strand cutter to obtain pellets. The pellets were molded into a flat plate of 80 mm x 80 mm x 1 mmt using an injection molding machine (SE-75DUZ-C250) manufactured by Sumitomo Heavy Industries, Ltd. under molding conditions of a mold temperature of 80°C, an injection speed of 40 mm / sec, and a cooling time of 60 sec. The temperature of the injection molding machine was set to 240°C-245°C-250°C-250°C from the bottom of the hopper to the tip. The results of evaluation of the obtained pellets or molded products by the above-mentioned methods are shown in Table 1.
[0089] [Table 1]
[0090] From the above results, it was found that the melting point measured by differential scanning calorimetry (DSC) was 200°C or higher and the amino terminal group amount was 3.0×10 -5 The thermoplastic elastomer composition is a mixture of polyamide resin (A) having a molecular weight of 0.1 mol / g or more, block copolymer (B) including a polymer block mainly made of an aromatic vinyl compound having a reactive functional group of 0.1 wt% or more and a polymer block mainly made of isobutylene, and hydrogenated petroleum resin (C), in which the composition ratio (weight ratio) of polyamide resin (A) and copolymer (B) is (A):(B)=40:60-90:10, and 0.01-20 parts by weight of hydrogenated petroleum resin (C) is mixed with 100 parts by weight of polyamide resin (A) and copolymer (B). These thermoplastic elastomer compositions have a loss tangent of 0.10 or more at a frequency of 100 Hz and a temperature of 23°C, and are found to be excellent in vibration damping properties, high temperature rigidity, blocking resistance, and spinnability. [Industrial Applicability]
[0091] The molded article made of the thermoplastic elastomer composition of the present invention has excellent vibration damping properties, high-temperature rigidity, blocking resistance, and spinnability, and can be easily produced. Taking advantage of these properties, the thermoplastic elastomer composition of the present invention can be widely used in various molded articles, and is particularly suitable for use in automobiles, electrical and electronic applications, and consumer applications.
Claims
1. A melting point of 200°C or higher as measured by differential scanning calorimetry (DSC) and an amino terminal group content of 3.0 x 10 -5 mol / g or more, a block copolymer (B) including a polymer block mainly made of an aromatic vinyl compound having 0.1% by weight or more of reactive functional groups and a polymer block mainly made of isobutylene, and a hydrogenated petroleum resin (C), wherein the composition ratio (weight ratio) of the polyamide resin (A) to the copolymer (B) is (A):(B)=40:60 to 90:10, and the hydrogenated petroleum resin (C) is blended in an amount of 0.01 to 20 parts by weight per 100 parts by weight of the total of the polyamide resin (A) and the copolymer (B).
2. The thermoplastic elastomer composition according to claim 1, wherein the thermoplastic elastomer composition has a loss tangent of 0.10 or more at a frequency of 100 Hz and a temperature of 23°C.
3. A molded article comprising the thermoplastic elastomer composition according to claim 1 or 2.
4. A fiber comprising the thermoplastic elastomer composition according to claim 1 or 2.
5. A sheet comprising the thermoplastic elastomer composition according to claim 1 or 2.
6. A foam-molded article comprising the thermoplastic elastomer composition according to claim 1 or 2.
Citation Information