R-t-b based sintered magnet
By optimizing the composition and internal structure of R-T-B sintered magnets with controlled grain boundary phases and reduced heavy rare earth element use, the magnets achieve enhanced magnetic properties and stability, addressing the challenges of resource scarcity and performance fluctuations.
Patent Information
- Application Number
- JP2024066871
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-08
AI Technical Summary
R-T-B sintered magnets face challenges in maintaining high coercive force (HcJ) at high temperatures while reducing the use of heavy rare earth elements like Tb, which are scarce and volatile in supply, leading to fluctuations in magnetic properties such as residual magnetic flux density (Br) and coercive force (HcJ).
The magnet composition includes specific ranges of rare earth elements (R), additional elements (M) like Cu, and controlled grain boundary phases with varying concentrations of Pr and Cu, forming a two-phase structure to enhance magnetic properties without relying heavily on heavy rare earths, using a controlled diffusion process to optimize internal organization.
This approach results in R-T-B sintered magnets with improved magnetic properties, including higher Br and HcJ, while minimizing the use of heavy rare earth elements, thus stabilizing performance and reducing resource dependency.
Smart Images

Figure 2024159586000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an RTB based sintered magnet. [Background technology]
[0002] RTB sintered magnets (R is at least one of rare earth elements, T is Fe or Fe and Co, and B is boron) are known as the most high-performance permanent magnets. For this reason, RTB sintered magnets are used in a variety of motors in the automotive field, such as electric vehicles (EV, HV, PHV), renewable energy fields such as wind power generation, home appliances, and industrial fields. RTB sintered magnets are an essential material for making these motors smaller and lighter, more efficient, and more energy-efficient (improving energy efficiency). RTB sintered magnets are also used in the drive motors of electric vehicles, and by replacing internal combustion engine vehicles with electric vehicles, they also contribute to preventing global warming by reducing greenhouse gases such as carbon dioxide (reducing fuel and exhaust gas). In this way, RTB sintered magnets are making a significant contribution to the realization of a clean energy society.
[0003] RTB sintered magnets are mainly R2T 14 It is composed of crystal grains made of B-type compounds and a grain boundary phase located at the grain boundaries of these crystal grains (for example, Patent Document 1). 14 B main phase grain and two adjacent R2T 14 The present invention discloses a rare earth sintered magnet comprising a two-particle grain boundary phase between main phase crystal grains, the thickness of which is 5 nm or more and 500 nm or less, and which is characterized by being composed of a phase having a magnetic property different from that of the ferromagnetic material. R2T that constitutes the grains 14 B-type compounds are ferromagnetic materials with high saturation magnetization and anisotropic magnetic field, and determine the properties of RTB sintered magnets.
[0004] RTB sintered magnets have a coercive force H cJ (Hereafter, simply "H cJThis causes a problem of irreversible thermal demagnetization due to the decrease in the magnetization temperature (H), which is particularly important for RTB sintered magnets used in electric vehicle motors. cJ i.e., higher H at room temperature cJ It is required that the applicant have: [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2014-209546 Summary of the Invention [Problem to be solved by the invention]
[0006] R2T 14 When the light rare earth elements RL (mainly Nd, Pr) in B-type compounds are replaced by heavy rare earth elements RH (mainly Tb, Dy), H cJ However, H cJ While R2T 14 The saturation magnetization of the B-type compound phase decreases, so the residual magnetic flux density B r (Hereinafter, simply "B r In particular, Tb has problems such as unstable supply and price fluctuations due to the fact that the resource is originally small and the production areas are limited. For this reason, it is recommended to use as little Tb as possible (use as little as possible) and to use B r While suppressing the decline of cJ It is required to obtain
[0007] The rare earth sintered magnet disclosed in Patent Document 1 has a low content of heavy rare earth elements RH such as Tb, and is excellent in H at high temperatures. cJ However, compared with sintered magnets containing heavy rare earth elements RH, the magnetic properties (B r and H cJ In recent years, especially in electric vehicle motors, r and HcJ Further improvement is required.
[0008] Therefore, one embodiment of the present invention is to reduce the amount of heavy rare earth elements RH such as Tb while increasing the amount of B r and H cJ The object of the present invention is to provide an RTB based sintered magnet that can further improve the above. [Means for solving the problem]
[0009] Aspect 1 of the present invention is R: 26.8% by mass or more and 31.5% by mass or less (R is a rare earth element, and always includes Pr); M: 0.05% by mass or more and 2.00% by mass or less (M is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si, and must contain Cu); B: 0.84% by mass or more and 0.94% by mass or less, and T: 61.5 mass% or more (T is Fe and Co, and 90% or more of T is Fe by mass ratio), The internal organization The crystal grains and Between two adjacent crystal grains, a first phase and A second phase having a higher Cu concentration and Pr concentration than the first phase is included between one or both of the two crystal grains and the first phase, The second phase is an RTB sintered magnet containing Pr in the range of 20 mass % to 65 mass %.
[0010] Aspect 2 of the present invention is The RTB based sintered magnet according to aspect 1 further includes the second phase between each of the two crystal grains and the first phase.
[0011] Aspect 3 of the present invention is The first phase is R: 15% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: Contains 20% by mass or more and 80% by mass or less, The second phase is R: 20% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: Contains 20% by mass or more and 80% by mass or less, and has a higher concentration of M than the first phase; The RTB based sintered magnet according to embodiment 1 or 2.
[0012] A fourth aspect of the present invention is The RTB based sintered magnet according to any one of aspects 1 to 3, wherein the Pr concentration and Cu concentration gradually decrease from the surface in the depth direction within a range of 200 μm from the surface.
[0013] A fifth aspect of the present invention is The RTB based sintered magnet according to any one of aspects 1 to 4, wherein M necessarily further contains Ga.
[0014] A sixth aspect of the present invention is The RTB based sintered magnet according to any one of aspects 1 to 5 satisfies the following formula (1): 26.0 mass%≦([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≦27.7 mass% (1) Here, [Nd], [Pr], [Ce], [La], [Dy], [Tb], [O] and [C] are the contents of Nd, Pr, Ce, La, Dy, Tb, O and C, respectively, expressed in mass%.
[0015] A seventh aspect of the present invention is The RTB sintered magnet according to any one of aspects 1 to 6, wherein the Ga content of M is 0.3 mass % or more, and the Ga concentration does not decrease gradually from the surface to a depth of 200 μm. Effect of the Invention
[0016] According to an embodiment of the present invention, the amount of heavy rare earth element RH such as Tb is reduced while B r and H cJIt is therefore possible to provide an RTB sintered magnet with further improved properties. [Brief description of the drawings]
[0017] [Figure 1A] FIG. 1A is a cross-sectional view showing a schematic enlargement of a portion of an RTB based sintered magnet. [Figure 1B] FIG. 1B is a cross-sectional view showing a further enlarged schematic view of the dashed rectangular region in FIG. 1A. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic diagram of a two-particle grain boundary. [Figure 3A] FIG. 3A is a TEM photograph of a cross section of an RTB sintered body produced in an example. [Figure 3B] FIG. 3B is an enlarged TEM photograph of a portion (encircled in a square) of FIG. 3A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The inventors have developed a method for improving the magnetic properties (especially B r and H cJ We have conducted extensive research to improve the R2T 14 It was found that the effect of improving the magnetic properties due to the grain boundary diffusion of R and M is enhanced in the case of a "low boron" composition, which is lower than the stoichiometric composition of the B compound. 14 It was found that the same effect can be obtained even if part of the B in the B compound is replaced by carbon (C). 14 It was found that the C that replaced the B in the B compound combined with the rare earth oxides in the grain boundaries during the sintering process to form rare earth oxygen carbon compounds (ROC compounds) in the grain boundaries. It was also found that the atomic ratio in this case was R:(C,O)=1:1. When such ROC compounds were formed in the grain boundaries, the R2T compound, which is the main phase, was reduced in proportion to the amount of the rare earth oxides in the grain boundaries. 14 The content of C in the B compound decreases. As mentioned above, R2T 14Even if a part of B in the B compound is substituted by C, the effect of "low boron" can be obtained. Therefore, in the main phase R2T 14 A decrease in the content of C constituting the B compound effectively reduces the total amount of B and C. Further, the formation of R-O-C compounds at the grain boundaries means that a part of the rare earth element R contained in the raw material alloy is consumed in the formation of the R-O-C compounds. Note that the R-O-C compounds (rare earth oxycarbides) include R-O compounds (rare earth oxides) and R-C compounds (rare earth carbides).
[0019] As a result of investigations based on these findings, it has been found that an R-T-B sintered magnet satisfying a specific component composition, in which the grain boundary phase between the crystal grains includes a first phase and a second phase disposed between the crystal grains and the first phase and having a higher Cu concentration and Pr concentration than the first phase, and the second phase contains Pr in the range of 20% by mass or more and 65% by mass or less, has excellent magnetic properties, and the invention according to the embodiment of the present application has been completed.
[0020] Hereinafter, the R-T-B sintered magnet according to the embodiment (hereinafter sometimes simply referred to as "sintered magnet") will be described in detail.
[0021] <R-T-B Sintered Magnet> The R-T-B sintered magnet is R: 26.8% by mass or more and 31.5% by mass or less (R is a rare earth element and includes Pr), M: 0.05% by mass or more and 2.00% by mass or less (M is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si and necessarily includes Cu), B: 0.84% by mass or more and 0.94% by mass or less, and T: 61.5% by mass or more (T is Fe and Co, and 90% or more of T is Fe by mass ratio).
[0022] As shown in FIGS. 1A and 1B, the internal structure of the sintered magnet 10 mainly consists of R2T 14It includes crystal grains 12 made of a B compound and a grain boundary phase 14 located between the crystal grains 12 . The grain boundary phase 14 includes a two-particle grain boundary phase 14a present between two adjacent crystal grains 12, and a grain boundary triple junction 14b where three two-particle grain boundary phases 14a intersect.
[0023] 2, in the sintered magnet 10 according to the embodiment, the two-particle grain boundary phase 14a includes a first phase 141 and a second phase 142 between the first phase 141 and one or both of the two crystal grains 12. Note that the second phase 142 may be formed only between one of the two crystal grains 12 and the first phase 141, but is preferably formed between both of the two crystal grains 12 and the first phase 141. The Cu concentration and Pr concentration of the second phase 142 are higher than the Cu concentration and Pr concentration of the first phase 141. That is, the embodiment of the present invention has a first phase and a second phase with different Cu and Pr contents from each other. The Pr concentration of the second phase 142 is in the range of 20 mass % to 65 mass %. The Pr concentration of the first phase 141 may also be in the range of 20 mass % to less than 65 mass %.
[0024] The present inventors have confirmed that the two-particle grain boundary phase 14a of the sintered magnet 10 has an internal structure including the first phase 141 and the second phase 142 as described above, thereby achieving high magnetic properties. Although the reason why the two-particle grain boundary phase 14a can achieve high magnetic properties is unclear, it is believed that the second phase 142 has a lower melting point than the first phase 141 because the second phase 142 has a higher Cu concentration and Pr concentration than the first phase 141. It is also believed that the final solidification of the second phase 142 improves the lattice matching between the main phase (crystal grains 12), the second phase 142, and the first phase 141.
[0025] In the sintered magnet according to the embodiment, R is a rare earth element, and necessarily contains Pr, and preferably further contains Nd. By including both Pr and Nd as R, it is possible to realize higher magnetic properties. Similar to Pr, the Nd concentration in the second phase 142 is preferably higher than the Nd concentration in the first phase 141 .
[0026] The sintered magnet 10 according to the embodiment has a two-phase structure in the two-particle grain boundary phase 14a, and therefore can achieve high magnetic properties even in a component composition that has a low content of heavy rare earth elements RH such as Tb or does not contain any heavy rare earth elements RH.
[0027] When the sintered magnet 10 contains the heavy rare earth element RH, it is preferable that the content of the heavy rare earth element RH is smaller than that of the conventional magnet. Tb: more than 0 mass% and 0.10 mass% or less, and Dy: more than 0 mass % and 0.20 mass % or less, is preferably limited to at least one selected from the group consisting of: The sintered magnet 10 according to the embodiment has the internal structure described above, and thus can achieve excellent magnetic properties even when the contents of the heavy rare earth elements RH, Tb and Dy, are restricted to 0.10 mass % or less and 0.20 mass % or less, respectively.
[0028] It is preferable that the sintered magnet 10 satisfies the following formula (1). 26.0 mass%≦([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≦27.7 mass% (1) Here, [Nd], [Pr], [Ce], [La], [Dy], [Tb], [O] and [C] are the contents of Nd, Pr, Ce, La, Dy, Tb, O and C, respectively, expressed in mass%. In addition, when the sintered magnet does not contain one or more of Nd, Pr, Ce, La, Dy, Tb, O, and C, the content of the element not contained is regarded as "0 mass%" and is substituted into formula (1).
[0029] The contents of R (particularly Nd, Pr, Ce, La, Dy, and Tb), O, and C in the sintered magnet 10 are adjusted, thereby satisfying the above formula (1). The C content can be adjusted by the amount of lubricant added during pulverization and molding. Preferably, formula (1) is 26.0 mass% or more and 27.5 mass% or less, more preferably 26.3 mass% or more and 27.3 mass% or less, and particularly preferably 27.0 mass% or more and 27.3 mass% or less. It is possible to achieve a high B while further reducing the amount of heavy rare earth element RH such as Tb used. r and H cJ can be obtained.
[0030] The composition of each phase contained in the two-particle grain boundary phase 14a is as follows: The first phase is R: 15% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: Contains 20% by mass or more and 80% by mass or less, The second phase is R: 20% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: It is preferable that the T phase contains 20% by mass or more and 80% by mass or less, and has a higher concentration of M than the first phase. Moreover, the first phase 141 and the second phase 142 contain F, and it is preferable that the F concentration of the second phase 142 is higher than the F concentration of the first phase 141. It is considered that the higher F concentration of the second phase 142 than the first phase 141 improves the lattice matching of the main phase (crystal grains 12), the second phase 142, and the first phase 141, and thus high magnetic properties are obtained.
[0031] The first phase 141 and the second phase 142 having such a component composition are both typically R6T 13 M crystal structure, R6T 12.5 M 1.5 At least Cu is contained as M, and the Cu concentration in the second phase 142 is made higher than the Cu concentration in the first phase 141. When the first phase 141 and the second phase 142 include such a crystal structure, a high H cJcan be obtained. The element concentrations in the first phase 141 and the second phase 142 can be measured by SEM-EDX analysis or TEM-EDX analysis.
[0032] The thickness of the first phase 141 is preferably 10 nm to 500 nm, more preferably 20 nm to 300 nm. By setting the thickness in such a range, it is possible to obtain the effect of reducing the magnetic interaction between the main phase particles (crystal grains 12) and to suppress the deterioration of the magnetic properties due to the decrease in the main phase ratio. The thickness of the second phase 142 is preferably 0.5 nm to 10 nm, more preferably 1.0 nm to 5.0 nm, inclusive. By setting the thickness in this range, it is possible to suppress the deterioration of the magnetic properties due to the decrease in the main phase ratio while satisfying the role of improving the lattice matching.
[0033] The composition of each component of the sintered magnet 10 will now be described in detail.
[0034] (R: 26.8% by mass or more and 31.5% by mass or less) R is a rare earth element, and always contains Pr, and preferably further contains Nd. The content of R is 26.8 mass% or more and 31.5 mass% or less. If the content of R is less than 26.8 mass%, it may be difficult to densify during sintering, and if it exceeds 31.5 mass%, the main phase ratio decreases and B r The content of R is preferably 26.8% by mass or more and 30.0% by mass or less. When R is in such a range, a higher B r can be obtained.
[0035] (M: 0.05 mass% or more and 2.00 mass% or less) M is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si, and must contain Cu. The content of M (the total content of Ga, Cu, Zn, Al, and Si) is 0.05 mass% or more and 2.00 mass% or less. When M is in this range, the temperature coefficient is improved, and high H cJ can be achieved. The sintered magnet 10 necessarily contains Cu as M, but preferably also contains Ga, and further contains H cJ can be improved.
[0036] Cu is contained in both the crystal grains 12 and the two-particle grain boundary phase 14a. In particular, the Cu concentration in the second phase 142 of the two-particle grain boundary phase 14a is high, and can be in the range of 2 mass % to 20 mass % as described below. In other words, Cu is concentrated in the second phase 142 of the sintered magnet 10. The first phase 141 may also contain Cu, but the Cu concentration is lower than that of the second phase 142. The Cu may be derived from the raw material, or may be derived from Cu diffused from the surface of the sintered body in a diffusion step carried out after the sintering step.
[0037] (B: 0.84 mass% or more and 0.94 mass% or less) The content of B is 0.84% by mass or more and 0.94% by mass or less. By including B in the range of the present disclosure in the sintered magnet 10, the temperature coefficient is improved and a high H cJ The B content is preferably 0.85% by mass or more and 0.94% by mass or less.
[0038] (T: 61.5% by mass or more) T is Fe and Co, and 90% or more of T is Fe by mass ratio. The inclusion of Co can improve corrosion resistance, but if the amount of Co substituted exceeds 10% by mass of T, high B r The T content is 61.5 mass% or more. If the T content is less than 61.5 mass%, the B r The content of T may be 70.0 mass % or less, and preferably T is the balance.
[0039] The sintered magnet 10 may contain Cr, Mn, La, Ce, Sm, Ca, Mg, etc., as inevitable impurities that are usually contained in didymium alloys (Nd-Pr), electrolytic iron, ferroboron, etc. Furthermore, examples of inevitable impurities that are contained during the manufacturing process include O (oxygen), N (nitrogen), and C (carbon). The sintered magnet 10 according to the embodiment may also contain one or more other elements. For example, small amounts (about 0.1% by mass each) of such elements as Ag, Zn, In, Sn, Ti, Ge, Y, H, F, P, S, V, Ni, Mo, Hf, Ta, W, Nb, Zr, Pb, and Bi may be contained. Such elements may be contained in a total amount of, for example, about 1.0% by mass. If the amount is at this level, high H cJ It is quite possible to obtain an RTB based sintered magnet having the above properties.
[0040] Of these elements contained in small amounts, F is an essential element that is always contained in the first phase 141 of the two-particle grain boundary phase 14a of the sintered magnet 10, but is hardly contained in the crystal grains 12, and is therefore treated as an element contained in small amounts in the composition of the sintered magnet 10. However, as described above, the presence of a predetermined amount of F in the second phase 142 can be confirmed by subjecting the two-particle grain boundary phase 14a to SEM-EDX analysis or TEM-EDX analysis. F element may be intentionally added to the raw material so that the second phase 142 and, if necessary, the first phase 141 contain F in a predetermined amount.
[0041] In the sintered magnet 10 according to the embodiment, the Pr concentration and Cu concentration may gradually decrease from the surface to a depth of 200 μm. The sintered magnet 10 having such a concentration distribution can be obtained by carrying out a diffusion process from the magnet surface to the inside of the magnet using a diffusion source containing Pr and Cu during the manufacture of the sintered magnet 10. By carrying out such a diffusion process, it is possible to more reliably obtain an RTB sintered magnet that includes a second phase 142 between one or both of the two crystal grains 12 and the first phase 141, the second phase 142 having a higher Cu concentration and Pr concentration than the first phase, and the second phase 142 containing Pr in the range of 20% by mass to 65% by mass.
[0042] Furthermore, as a result of the study by the present inventors, compared with a sintered magnet produced by diffusing Pr, Cu, and part or all of Ga in a diffusion process, the sintered body contains 0.3 mass% or more of Ga, and after manufacturing all of the Ga from the raw material (that is, contained in the alloy for the sintered magnet), by performing diffusion of Pr and Cu, it was newly found that significantly higher H cJ can be achieved. That is, the sintered magnet of the present disclosure necessarily contains Cu and Ga as M, the content of Ga is 0.3 mass% or more, and in the range from the surface to a depth of 200 μm, it is preferable that the Ga concentration does not gradually decrease in the depth direction from the surface. The fact that the Ga concentration does not gradually decrease in the depth direction from the surface indicates that the process of diffusing from the magnet surface toward the magnet interior using a diffusion source containing Ga has not been performed. As a result, it is considered that the first phase is more uniformly formed in the sintered magnet and high H cJ is obtained.
[0043] The concentrations of Pr and Cu in the range from the surface to a depth of 200 μm can be confirmed by performing line analysis (line analysis) on the cross section of the sintered magnet 10 in the range from the magnet surface to near the magnet center up to a depth of 200 μm by an energy dispersive X-ray spectroscopy method (EDX). It is preferable to measure at a cross section perpendicular to the surface and more than 200 μm away from the end of the surface. When performing line analysis, the measurement is performed in a direction orthogonal to the surface (the outer periphery of the measurement cross section) within a region more than 200 μm away from the end of the measurement cross section so as not to measure the range within 200 μm from the outer periphery of the measurement cross section. The concentration of Ga can also be confirmed by performing the same measurement.
[0044] <Manufacturing method of R-T-B system sintered magnet> Hereinafter, embodiments of the manufacturing method of the R-T-B system sintered magnet of the present disclosure will be described.
[0045] The manufacturing method in this embodiment may include a step of preparing an RTB sintered body, a step of preparing an R1-M alloy, a step of performing a first heat treatment, and a step of performing a second heat treatment. The step of performing the first heat treatment is a step (diffusion step) of bringing at least a part of the R1-M alloy into contact with at least a part of the surface of the RTB sintered body, and performing the first heat treatment at a temperature of 700°C or higher and 950°C or lower in a vacuum or inert gas atmosphere, thereby diffusing R1 and M into the magnet. The step of performing the second heat treatment is a step of performing a second heat treatment on the RTB sintered magnet that has been subjected to the first heat treatment in a vacuum or inert gas atmosphere at a temperature of 400°C or higher and 750°C or lower, which is a temperature lower than the first heat treatment temperature. Each of these steps will be described in more detail below.
[0046] (Preparation of RTB-based sintered body) First, the composition of the RTB sintered body will be described.
[0047] One of the features of the RTB sintered body used in this embodiment is that the R, oxygen, carbon, etc. contained in the RTB sintered body are adjusted to finally produce an RTB sintered magnet that satisfies the above formula (1). For this reason, it is preferable to prepare an RTB sintered body that satisfies the following relationships: 0.84 mass%≦[B]≦0.94 mass%, 25.8 mass%≦([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≦27.5 mass%, and 0.05 mass%≦[O]≦0.30 mass%. It is also preferable to prepare an RTB sintered body that satisfies the following relationship: 0.05 mass%≦[C]≦0.18 mass%. By carrying out a diffusion process described later on such an RTB sintered body, it is possible to prevent R, M, etc. from being excessively diffused inside the magnet inside the RTB sintered body and to greatly promote grain boundary diffusion.
[0048] The RTB sintered body prepared in this step has, for example, the following composition. R: 26.6% by mass or more and 31.3% by mass or less (R is a rare earth element and necessarily contains Pr), and preferably further contains Nd. B: 0.84% by mass or more and 0.94% by mass or less, M: 0% by mass or more and 1.5% by mass or less (M is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si); Q: 0% by mass or more and 2.0% by mass or less (Q is at least one selected from the group consisting of Ti, V, Cr, Mn, Ni, Zr, Nb, Mo, Ag, In, Sn, Hf, Ta, W, Pb, and Bi) The balance consists of T (T is Fe or Fe and Co) and unavoidable impurities.
[0049] The RTB-based sintered body also satisfies the above formula (1).
[0050] Next, a method for preparing the RTB sintered body will be described.
[0051] First, an alloy for an RTB sintered magnet is prepared, and then this alloy is roughly crushed by, for example, a hydrogen crushing method.
[0052] The following is an example of a method for producing an alloy for an RTB sintered magnet. An alloy ingot can be obtained by an ingot casting method in which a metal or alloy previously adjusted to have the above-mentioned composition is melted and poured into a mold to solidify. Alternatively, the alloy may be produced by a strip casting method in which a molten metal or alloy previously adjusted to have the above-mentioned composition is brought into contact with a single roll, twin rolls, rotating disk, or rotating cylindrical mold, etc., and quenched to produce a rapidly solidified alloy. Alternatively, flake-shaped alloys may be produced by other quenching methods, such as centrifugal casting.
[0053] In the embodiment of the present invention, alloys manufactured by either the ingot method or the quenching method can be used, but it is preferable to use alloys manufactured by a quenching method such as a strip casting method. The thickness of the alloy manufactured by the quenching method is usually in the range of 0.03 mm to 1 mm, and it is in a flake shape. The molten alloy starts to solidify from the surface (roll contact surface) that contacts the cooling roll, and crystals grow columnarly in the thickness direction from the roll contact surface. The quenched alloy is cooled in a short time compared to the alloy (ingot alloy) manufactured by the conventional ingot casting method (mold casting method), so the structure is finer and the crystal grain size is smaller. In addition, the area of the grain boundary is large. Since the R-rich phase spreads widely within the grain boundary, the quenching method has excellent dispersibility of the R-rich phase. Therefore, it is easy to break at the grain boundary by the hydrogen pulverization method. By hydrogen pulverizing the quenched alloy, the size of the hydrogen pulverized powder (coarse pulverized powder) can be reduced to, for example, 1.0 mm or less. The coarse pulverized powder obtained in this manner is pulverized, for example, by a jet mill.
[0054] In this embodiment, the pulverization conditions are adjusted so that the oxygen content of the finally obtained RTB based sintered magnet falls within a specific range (0.05% by mass≦[O]≦0.30% by mass). In jet mill pulverization, pulverization is performed in an inert atmosphere such as nitrogen. Pulverization may be performed, for example, by jet mill pulverization in a humidified atmosphere. Preferably, the powder particles are made small (average particle size d50 is 2.0 μm or more and 10.0 μm or less, more preferably d50 is 2.0 μm or more and 8.0 μm or less, even more preferably d50 is 2.0 μm or more and 4.5 μm or less, and even more preferably d50 is 2.0 μm or more and 3.5 μm or less). By making the powder particles small, a high H cJ can be obtained.
[0055] The average particle size (d50) can be measured by an airflow dispersion laser diffraction method (based on JIS Z 8825: revised in 2013). That is, in this specification, the average particle size means the particle size (median diameter) at which the cumulative particle size distribution (volume basis) from the small particle size side is 50%.
[0056] As long as the fine powder used to produce the RTB-based sintered body satisfies the above-mentioned conditions, it may be produced from one type of raw material alloy (single raw material alloy) or may be produced by using two or more types of raw material alloys and mixing them (blending method).
[0057] In a preferred embodiment, a powder compact is produced from the above fine powder by pressing in a magnetic field, and then the powder compact is sintered to obtain an RTB type sintered body.
[0058] In terms of suppressing oxidation in the case of pressing in a magnetic field, it is preferable to form the powder compact by pressing in an inert gas atmosphere or wet pressing. In particular, in wet pressing, the surface of the particles constituting the powder compact is covered with a dispersant such as an oil agent, and contact with oxygen in the air or water vapor is suppressed. Therefore, it is possible to prevent or suppress the particles from being oxidized by the air before, during, or after the pressing process. Therefore, it is easy to control the oxygen content of the sintered magnet within a predetermined range. When performing wet pressing in a magnetic field, a slurry is prepared by mixing a fine powder with a dispersion medium, and the slurry is supplied to the cavity of a die of a wet pressing device and press-molded in a magnetic field. Note that the RTB sintered compact may be prepared by using a known method such as the PLP (Press-Less Process) method described in JP-A-2006-19521 without molding.
[0059] The powder compact is preferably sintered at a temperature in the range of 950°C to 1150°C. To prevent oxidation due to sintering, residual gas in the atmosphere may be replaced with an inert gas such as helium or argon. The obtained sintered compact may be subjected to a heat treatment. Known conditions may be adopted for the heat treatment temperature, heat treatment time, and other heat treatment conditions.
[0060] (The process of preparing the R1-M alloy) In this embodiment, R1, or R1 and M, are diffused from the surface of the RTB sintered body to the inside. For this purpose, an alloy containing the elements to be diffused (hereinafter referred to as an "R1-M alloy") is prepared.
[0061] First, the composition of the R1-M alloy will be described. R1 in the R1-M alloy is at least one of rare earth elements, and the content of R1 is preferably 65% by mass to 100% by mass, more preferably 70% by mass to 95% by mass, of the entire R1-M alloy. M in the R1-M alloy is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si, and the content of M is preferably 0% by mass to 35% by mass, more preferably 5% by mass to 30% by mass, of the entire R1-M alloy. In the R1-M alloy, R1 preferably contains at least one of Nd and Pr, and more preferably R1 always contains Pr. The Pr content is preferably 65 mass% or more and 86 mass% or less of the entire R1-M alloy. The Pr content is preferably 50 mass% or more of the entire R1, and more preferably 65 mass% or more of the entire R1. The inclusion of Pr facilitates diffusion in the grain boundary phase, which can promote grain boundary diffusion and result in a higher H cJ can be obtained.
[0062] The shape and size of the R1-M alloy are not particularly limited and can be any shape. The R1-M alloy can be in the form of a film, foil, powder, block, particle, etc.
[0063] Next, a method for producing the R1-M alloy will be described.
[0064] The R1-M alloy can be prepared by a raw material alloy production method employed in a general method for producing RTB sintered magnets, such as die casting, strip casting, single roll rapid cooling (melt spinning), atomization, etc. The R1-M alloy may be prepared by pulverizing the alloy obtained by the above method using a known pulverizing means such as a pin mill.
[0065] (Step of carrying out first heat treatment (diffusion step)) At least a part of the R1-M alloy is brought into contact with at least a part of the surface of the RTB sintered body prepared by the above-mentioned method, and a first heat treatment is carried out in a vacuum or inert gas atmosphere at a temperature of 700° C. to 950° C. (first heat treatment temperature). The first heat treatment is a process for diffusing R1 and M into the interior of the sintered body (i.e., a diffusion process), and a liquid phase containing R1 and M is generated from the R1-M alloy by the heat treatment, and the liquid phase is diffused from the surface of the RTB sintered body through the grain boundaries in the sintered body into the interior of the sintered body.
[0066] If the first heat treatment temperature is less than 700°C, the amount of liquid phase containing R1 and M is too small, resulting in high H cJ On the other hand, when the temperature exceeds 950℃, H cJ The first heat treatment temperature is preferably 850° C. or higher and 950° C. or lower, and the higher H cJ It is also preferable to cool the RTB sintered body that has been subjected to the first heat treatment (700° C. or more and 950° C. or less) from the first heat treatment temperature to 300° C. at a cooling rate of 5° C. / min or more, and a higher H cJ More preferably, the cooling rate is 15° C. / min or more.
[0067] The first heat treatment can be performed by placing an R1-M alloy of any shape on the surface of the RTB sintered compact and using a known heat treatment device. For example, the surface of the RTB sintered compact can be covered with a powder layer of the R1-M alloy and then the first heat treatment can be performed. For example, a slurry in which the R1-M alloy is dispersed in a dispersion medium can be applied to the surface of the RTB sintered compact, and then the dispersion medium can be evaporated to bring the R1-M alloy layer into contact with the RTB sintered compact and then the first heat treatment can be performed. Examples of the dispersion medium include alcohol (ethanol, etc.), aldehyde, and ketone. Also, for example, an R1-M alloy film can be formed on the surface of the RTB sintered compact using a known sputtering device, and then the first heat treatment can be performed. In addition, when introducing a heavy rare earth element RH into the RTB sintered compact, not only a method using an R1-M alloy containing RH, but also a fluoride, oxide, acid fluoride, etc. of the heavy rare earth element RH can be placed on the surface of the RTB sintered compact together with the R1-M alloy and the first heat treatment can be performed. Examples of the fluorides, oxides, and oxyfluorides of the heavy rare earth element RH include TbF3, DyF3, Tb2O3, Dy2O3, TbOF, and DyOF.
[0068] The position of the R1-M alloy is not particularly important as long as at least a part of the R1-M alloy is in contact with at least a part of the RTB sintered compact.
[0069] (Step of carrying out second heat treatment) The RTB sintered body that has been subjected to the first heat treatment is then heat treated in a vacuum or inert gas atmosphere at a temperature between 400° C. and 750° C., both inclusive, and lower than the temperature of the first heat treatment. In the present disclosure, this heat treatment is referred to as the second heat treatment. By performing the second heat treatment, a high H cJ When the temperature at which the second heat treatment is performed (second heat treatment temperature) is higher than the first heat treatment temperature, or when the second heat treatment temperature is lower than 400° C. or higher than 750° C., a high H cJ may not be obtained. EXAMPLES
[0070] The raw materials of each element were weighed so that the RTB-based sintered bodies had the compositions shown in No. A to D in Table 1, and alloys were produced by strip casting. The obtained alloys were coarsely pulverized by hydrogen pulverization to obtain coarsely pulverized powder. Next, zinc stearate was added as a lubricant at 0.04 mass% relative to 100 mass% of the coarsely pulverized powder to the obtained coarsely pulverized powder, and mixed. After that, the mixture was dry-pulverized in a nitrogen gas stream using an airflow pulverizer (jet mill device) to obtain finely pulverized powder (alloy powder) with an average particle size d50 of 3 μm.
[0071] The finely pulverized powder was mixed with zinc stearate as a lubricant at 0.05% by mass relative to 100% by mass of the finely pulverized powder, and then molded in a magnetic field to obtain a powder compact. The molding device used was a so-called perpendicular magnetic field molding device (horizontal magnetic field molding device) in which the magnetic field application direction and the pressure direction are perpendicular to each other. The obtained powder compact was sintered in a vacuum at 1060°C to 1090°C (a temperature at which sufficient densification by sintering occurs for each sample) for 4 hours to obtain an RTB-based sintered body. The density of the obtained RTB-based sintered body was 7.5 Mg / m 3 That was all. The composition of the obtained RTB-based sintered body is shown in Table 1. Each component in Table 1 was measured using inductively coupled plasma optical emission spectroscopy (ICP-OES). The O (oxygen) content was measured using a gas analyzer that uses the gas fusion-infrared absorption method, and the C (carbon) content was measured using a gas analyzer that uses the combustion-infrared absorption method. The composition of the R1-M alloy (Table 2) was also measured using the same measurement method.
[0072] [Table 1]
[0073] The raw materials of each element were weighed so that the R1-M alloy had the composition shown in Table 2, No. a and b. The raw materials were melted and a ribbon or flake-shaped alloy was obtained by single-roll ultra-quenching (melt spinning). The obtained alloy was pulverized in an argon gas atmosphere using a mortar, and then passed through a sieve with 425 μm openings to prepare the R1-M alloy. The composition of the obtained R1-M alloy is shown in Table 2.
[0074] [Table 2]
[0075] The RTB sintered compacts No. A to D in Table 1 were cut and ground to obtain cubes of 7.4 mm x 7.4 mm x 7.4 mm. Next, 3 mass% of R1-M alloy (No. a, b) was sprayed on the entire surface of the RTB sintered compacts No. A to D with respect to 100 mass% of the RTB sintered compact. After that, heat treatment (first heat treatment) was performed at 900°C for 4 hours in reduced pressure argon gas controlled at 50 Pa, and then cooled to room temperature. Further, heat treatment (second heat treatment) was performed at 500°C for 1 hour in reduced pressure argon gas controlled at 50 Pa, and then cooled to room temperature to produce RTB sintered magnets (No. 1 to 4).
[0076] Table 3 shows the composition of the obtained RTB sintered magnet and the value of the middle part of formula (1) (i.e., ([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])). It was confirmed that Nos. 1 to 3 all satisfy formula (1) of the present disclosure. Each component in Table 3 was measured using inductively coupled plasma optical emission spectroscopy (ICP-OES). The O (oxygen) content was measured using a gas analyzer using gas fusion-infrared absorption method, and the C (carbon) content was measured using a gas analyzer using combustion-infrared absorption method.
[0077] The obtained RTB sintered magnets were machined to produce magnet samples of 7 mm x 7 mm x 7 mm, and the magnetic properties (B r and H cJ ) was measured. The measurement results are shown in Table 4. Furthermore, each of magnet samples No. 1 to 4 was cut along a plane that was parallel to one of the surfaces and passed near the center of the magnet, and a line analysis was performed on the cross section using EDX from the magnet surface to near the center of the magnet. It was confirmed that in all samples, the Pr concentration and Cu concentration each gradually decreased (gradually became lower) in the depth direction from the surface, in the range from the magnet surface to a depth of 200 μm.
[0078] Furthermore, it was confirmed that in magnet sample No. 3, which used diffusion source b containing Ga, the Ga concentration gradually decreased from the surface toward the depth in the range from the magnet surface to a depth of 200 μm, whereas in magnet samples No. 1, 2, and 4, which used diffusion source a not containing Ga, the Ga concentration did not gradually decrease from the surface toward the depth in the range from the magnet surface to a depth of 200 μm.
[0079] The cross sections of the RTB sintered magnets No. 1 to 4 were analyzed by FE-TEM / WDX·EDX (field emission transmission electron microscope / wavelength dispersive X-ray analysis·energy dispersive X-ray analysis). In order to eliminate the effects of elements diffused from the surface, the analysis was carried out at a position more than 3000 μm away from the surface. Figures 3A and 3B are cross-sectional TEM photographs of the RTB sintered magnet No. 1.
[0080] First, the cross section was observed by TEM, and a TEM image of the two-particle boundary phase 14a between two adjacent crystal grains 12 was obtained (FIG. 3A). When multiple two-particle boundaries were confirmed, one of the two two-particle boundaries was selected. Then, the vicinity of the interface between one of the two adjacent crystal grains 12 and the two-particle boundary phase 14a in contact with the crystal grain 12 was further observed by TEM (FIG. 3B). As can be seen from the TEM photograph in FIG. 3B, the two-particle boundary 14a included a first phase 141 that appeared whiter than the crystal grain 12, and a band-like second phase 142 that appeared black between the crystal grain 12 and the first phase 141.
[0081] Nos. 2 and 3 were also observed by TEM, and it was confirmed that the two-particle grain boundary phase 14a contained a first phase 141 and a second phase 142. As for No. 4, the two-particle grain boundary phase 14a was composed only of the first phase 141, and the second phase 142 could not be confirmed.
[0082] For Nos. 1 to 4, the first phase 141 and the second phase 142 identified in the TEM image were each subjected to point analysis by EDX to identify the amount of elements contained in each phase. For No. 4, the first phase 141 was subjected to point analysis by EDX. The results of the point analysis are shown in Table 4. As shown in Table 4, it was confirmed that Nos. 1 to 3 all contain a second phase having a higher Cu concentration and Pr concentration than the first phase, and that the second phase contains Pr in the range of 20 mass % to 65 mass %. As shown in Table 4, Nos. 1 to 3 which satisfy the conditions of the present disclosure have a larger B. r No drop in H cJ was obtained.
[0083] In addition, compared to sintered magnet No. 3, which was manufactured by diffusing Pr, Cu, and Ga in the diffusion process, sintered magnets No. 1 and 2, which were manufactured by diffusing Pr and Cu after the entire amount of Ga was contained in the sintered body, had a higher H cJ was achieved.
[0084] [Table 3]
[0085] [Table 4] [Explanation of symbols]
[0086] 10. RTB-based sintered magnet 12. Grain 14...grain boundary phase 14a...Two-grain grain boundary phase 141...Phase 1 142...2nd phase 14b...Grain boundary triple point
Claims
1. R: 26.8% by mass or more and 31.5% by mass or less (R is a rare earth element, and always contains Pr); M: 0.05% by mass or more and 2.00% by mass or less (M is at least one selected from the group consisting of Ga, Cu, Zn, Al, and Si, and must contain Cu); B: 0.84% by mass or more and 0.94% by mass or less, and T: 61.5 mass% or more (T is Fe and Co, and 90% or more of T is Fe by mass ratio), The internal organization The crystal grains and A first phase is present between two adjacent crystal grains. A second phase having a higher Cu concentration and Pr concentration than the first phase is included between one or both of the two crystal grains and the first phase, The second phase contains Pr in a range of 20 mass % to 65 mass %.
2. 2. The RTB based sintered magnet according to claim 1, wherein the second phase is present between each of the two crystal grains and the first phase.
3. The first phase is R: 15% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: Contains 20% by mass or more and 80% by mass or less, The second phase is R: 20% by mass or more and 65% by mass or less, M: 2% by mass or more and 20% by mass or less, T: Contains 20% by mass or more and 80% by mass or less and has a higher concentration of M than the first phase; The RTB based sintered magnet according to claim 1.
4. 2. The R-T-B based sintered magnet according to claim 1, wherein the Pr concentration and the Cu concentration gradually decrease from the surface in the depth direction within a range of 200 μm from the surface.
5. 2. The RTB based sintered magnet according to claim 1, wherein M further necessarily contains Ga.
6. The RTB based sintered magnet according to claim 1, which satisfies the following formula (1): 26.0 mass%≦([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≦27.7 mass% (1) Here, [Nd], [Pr], [Ce], [La], [Dy], [Tb], [O] and [C] are the contents of Nd, Pr, Ce, La, Dy, Tb, O and C, respectively, expressed in mass %.
7. The R-T-B system sintered magnet according to any one of claims 1 to 6, wherein the Ga content of M is 0.3 mass % or more, and the Ga concentration does not decrease gradually within a range from the surface to a depth of 200 µm.
Citation Information
Patent Citations
Rare earth magnet
JP2014209546A