Separator, manufacturing method thereof and secondary battery including the same

A separator with a coating layer of inorganic and hollow adhesive particles addresses the low bonding force issue, ensuring strong adhesion and swelling prevention, allowing for larger and more capable secondary batteries.

JP2024159614APending Publication Date: 2024-11-08SK INNOVATION CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024069342
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing secondary batteries face issues with low bonding force between electrodes and separators, leading to separation defects, limiting the increase in size and capacity.

Method used

A separator with a coating layer containing inorganic particles and hollow adhesive particles is used, which allows for high adhesive strength with electrodes without the need for a separate adhesive layer, and includes a gradient distribution of hollow adhesive particles to enhance adhesion and accommodate electrolyte swelling.

Benefits of technology

The separator provides improved adhesion to electrodes, prevents swelling and electrolyte elution, and maintains alignment, enabling larger and higher-capacity batteries with enhanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159614000001_ABST
    Figure 2024159614000001_ABST
Patent Text Reader

Abstract

To provide a separator, a manufacturing method thereof, and a secondary battery including the same, and specifically, provide a separator including hollow adhesive particles, a manufacturing method thereof, and a secondary battery including the same.SOLUTION: A separator according to an embodiment of the present disclosure includes a porous substrate and at least one coating layer located on one or both sides of the porous substrate, the coating layer including inorganic particles and hollow adhesive particles. The separator according to the present disclosure has improved surface adhesion and can be bonded to an electrode with high adhesion.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a separator, a manufacturing method thereof, and a secondary battery including the same. Specifically, the present disclosure relates to a separator including hollow adhesive particles, a manufacturing method thereof, and a secondary battery including the same. [Background technology]

[0002] Recently, secondary batteries have become larger and have higher capacity for use in electric vehicles and the like. As part of this, technology has been developed for electrode-separator combinations in which electrodes and separators are laminated and integrated. However, secondary batteries with existing electrode-separator combination structures have the disadvantage that the bonding strength between the electrodes and separators is low, resulting in defects in which the electrodes and separators are separated. This means that there is a problem in that it is practically impossible to increase the size and capacity of such batteries.

[0003] To solve this problem, a technology has been developed to provide a separator with improved adhesive strength by coating the surface that comes into contact with the electrode with an adhesive material, for example, a polymer resin. Such separators are usually manufactured by forming an inorganic particle layer and a polymer resin layer on a porous substrate to improve heat resistance, or by coating a one-component coating liquid in which a polymer resin and inorganic particles are mixed on a porous substrate.

[0004] However, in the case of a separator in which a polymer resin layer is separately formed on an inorganic particle layer, each layer must be manufactured separately, which results in a long manufacturing time and low process efficiency, resulting in reduced productivity.

[0005] In addition, in the case of a separator in which a coating layer is formed in one component by mixing polymer resin particles and inorganic particles, the manufacturing process is simplified, but there is a disadvantage in that the adhesive strength is reduced because inorganic particles and polymer resin are mixed on the surface that comes into contact with the electrode.

[0006] To solve this problem, a separator with improved adhesive performance can be used by adding a large amount of polymer resin. However, such a separator causes various problems that degrade battery performance, such as the polymer resin dissolving and eluting in the electrolyte during charging and discharging of the secondary battery, or the polymer resin swelling due to the electrolyte causing the pore layer in the separator to close.

[0007] To solve this problem, there is an urgent need to develop a new separator that can have high adhesion even with a small amount of adhesive material, can suppress swelling by acting as a buffer against swelling, and reduces electrolyte elution. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 10-2019-0036724 (April 5, 2019) Summary of the Invention [Problem to be solved by the invention]

[0009] One object of the present disclosure is to provide a separator that can be adhered to an electrode with high adhesive strength even with only a small amount of adhesive substance.

[0010] Another object of the present invention is to provide a new separator that provides an adhesive function for the separator and has the ability to internally accommodate swelling caused by an electrolyte or the like.

[0011] Another object of the present invention is to provide a method for producing a separator with improved adhesion to an electrode, without the need for a separate adhesive layer, and with only a simple process. Specifically, in the process of forming a coating layer by applying a coating composition containing inorganic particles and hollow adhesive particles, the hollow adhesive particles, which have a relatively low specific gravity compared to the inorganic particles, form an adhesive layer while floating, eliminating the need for a coating process for forming a separate adhesive layer, and providing electrode adhesion with a single coating process. Another object of the present invention is to provide a separator with excellent electrode adhesion, even when using a smaller content of hollow adhesive particles than in the past, by using a smaller content than in the past, as compared to the conventional case of forming a separate adhesive layer.

[0012] Another object of the present invention is to provide a novel separator in which the hollow adhesive particles function as a buffer capable of internally accommodating swelling caused by an electrolyte, thereby suppressing swelling and preventing elution of the electrolyte.

[0013] Another object of the present invention is to provide a new separator that suppresses swelling and has excellent adhesive strength, thereby maintaining good alignment even when electrodes and separators are laminated many times, and a battery using the same.

[0014] Another object of the present invention is to provide a secondary battery that can have a high capacity and a large size by including a separator with improved adhesive strength. [Means for solving the problem]

[0015] One aspect of the present disclosure provides a separator comprising a porous substrate and a coating layer located on one or both sides of the porous substrate, the coating layer comprising inorganic particles and hollow adhesive particles.

[0016] In one embodiment, the coating layer may have a first surface facing the porous substrate and a second surface opposite the first surface, and the second surface may have a higher content of the hollow adhesive particles than the first surface.

[0017] In one embodiment, the coating layer may have a gradient in which the content of the hollow adhesive particles increases from the first surface to the second surface.

[0018] In one embodiment, the coating layer may include an inorganic particle layer including inorganic particles and an adhesive layer formed by suspending hollow adhesive particles on the inorganic particle layer.

[0019] In one embodiment, the coating layer may be laminated in at least one layer.

[0020] In one embodiment, the hollow adhesive particles may have a hollow ratio of 5 to 97%, but is not limited thereto.

[0021] In one embodiment, the hollow adhesive particles may have an average outer diameter of 10 nm to 10 μm, but is not limited thereto.

[0022] In one embodiment, the hollow adhesive particle includes a hollow core having a hollow structure with an open interior and a shell layer made of an adhesive material, and the adhesive material may include an adhesive resin having adhesive strength at room temperature or at a temperature equal to or higher than the glass transition temperature (Tg).

[0023] In one embodiment, the adhesive resin may include, but is not limited to, an acrylic resin, a fluorine resin, an amide resin, a copolymer thereof, or a mixture thereof.

[0024] In one embodiment, the adhesive resin can be crosslinked.

[0025] In one embodiment, the hollow adhesive particle may further include a structural material layer between the hollow core and the shell layer to maintain the hollow structure.

[0026] In one embodiment, an inorganic particle layer may be further included between the porous substrate and the coating layer. Here, the inorganic particle layer refers to a layer made of inorganic particles that is generally used in the art to be distinguished from the coating layer, i.e., a ceramic layer. Specifically, for example, the inorganic particle layer may be a layer made of only inorganic particles with pores formed therebetween, or a layer in which the inorganic particles are bound by a binder to form pores therebetween. Here, the inorganic particle layer may not include the hollow adhesive particles.

[0027] Yet another aspect of the present disclosure provides a method for producing a separator, the method including: applying a coating composition including inorganic particles and hollow adhesive particles onto one or both sides of a porous substrate to form a coating layer; and drying the coating layer.

[0028] In one embodiment, the method may further include a step of applying vibration before or simultaneously with the drying step.

[0029] In one embodiment, the method may further include a step of leaving the separator coated with the coating composition unattended after the coating step and before drying.

[0030] In one embodiment, after the coating step and the drying step, the hollow adhesive particles may float on the surface of the coating layer to form a gradient, or an adhesive layer made of the hollow adhesive particles may be formed on the surface.

[0031] In one embodiment, the coating composition may have a solid content of 10 to 60 wt %, but is not limited thereto.

[0032] In one embodiment, the coating composition may include, but is not limited to, 0.2 to 20 parts by weight of the hollow adhesive particles based on 100 parts by weight of the inorganic particles.

[0033] In one embodiment, the drying can be performed by using hot air at 25 to 100°C.

[0034] Yet another aspect of the present disclosure provides a secondary battery including the separator according to the above aspect.

[0035] Also provided is a method for manufacturing a secondary battery, the method including the steps of: positioning the separator according to the embodiment between a positive electrode and a negative electrode; and then applying heat, pressure, or both to integrate the separator and the electrodes. Effect of the Invention

[0036] A separator according to one embodiment of the present disclosure contains hollow adhesive particles, and the surface adhesive strength of the separator is improved in accordance with the content of the hollow adhesive particles, enabling the separator to be bonded to an electrode with high adhesive strength.

[0037] Furthermore, the method for producing a separator according to one embodiment of the present disclosure can easily produce a separator having improved adhesion to the electrodes simply by forming a coating layer on a porous substrate.

[0038] Furthermore, a secondary battery including a separator according to one embodiment of the present disclosure can have a high capacity and a large size due to improved adhesive strength between the electrodes and the separator, and can be substantially industrially applicable.

[0039] Moreover, according to one embodiment of the present disclosure, it is possible to provide a novel separator that provides an excellent adhesive function between the separator and electrodes and has the ability to internally accommodate swelling caused by an electrolyte or the like.

[0040] Moreover, according to one embodiment of the present disclosure, a new separator can be provided that functions as a buffer capable of internally accommodating swelling caused by an electrolyte, thereby suppressing swelling and preventing the adhesive from dissolving into the electrolyte due to the electrolyte.

[0041] Moreover, according to one embodiment of the present disclosure, it is possible to provide a new separator and a battery using the same, which suppress swelling and maintain the adhesive strength with the electrode, i.e., prevent loss of adhesive strength due to swelling, and thereby maintain the alignment of the electrode module well even when the electrodes and separators are stacked many times. [Brief description of the drawings]

[0042] [Figure 1] FIG. 1 is a diagram illustrating one embodiment of a hollow adhesive particle consisting of a hollow core 11 with a void inside and a shell layer 12 made of an adhesive material. [Diagram 2] This is a diagram illustrating one embodiment of a hollow adhesive particle consisting of a hollow core 11, a structural material layer 13 for forming and maintaining the hollow structure, and a shell layer 12 made of an adhesive material. [Diagram 3] 1A to 1C are diagrams illustrating one embodiment of a method for manufacturing a separator. [Figure 4] FIG. 1 illustrates a method for evaluating stacking adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] Unless otherwise defined, technical and scientific terms used in this specification have the meanings commonly understood by a person of ordinary skill in the art to which this disclosure belongs, and in the following description and the accompanying drawings, descriptions of known functions and configurations that may obscure the gist of this disclosure will be omitted.

[0044] Also, as used herein, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context indicates otherwise.

[0045] Furthermore, in this specification, units used without special reference are based on weight, and as an example, a unit of % or ratio means % by weight or weight ratio, and % by weight means the weight % that any one component of the total composition occupies in the composition, unless otherwise defined.

[0046] In addition, the numerical ranges used herein include lower and upper limits, all values ​​within the range, increments logically derived from the form and width of the ranges defined, all values ​​that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are limited in different forms. Unless otherwise specified in the specification of this disclosure, values ​​outside the numerical ranges that may occur due to experimental error or rounding of values ​​are also included in the defined numerical ranges.

[0047] As used herein, the term "comprising" is an open-ended term having the same meaning as expressions such as "comprising," "containing," "having," or "characterized by," and does not exclude further unrecited elements, materials, or steps.

[0048] Unless otherwise specified in this specification, when a layer or member is said to be "on" another layer or member, this includes not only the case where a layer or member is in contact with the other layer or member, but also the case where another layer or member exists between two layers or two members.

[0049] In the present specification, "hollow adhesive particles" refers to particles that are hollow and have adhesive properties. Specifically, as shown in Figs. 1 and 2, the hollow adhesive particles are composed of a hollow core 11 that is hollow and a shell layer 12 made of an adhesive material, and the shell layer may be composed of at least one layer. Also, as shown in Fig. 2, a structural material layer 13 for forming and maintaining a hollow structure may be further included between the hollow core 11 and the shell layer 12. Figs. 1 and 2 are intended to specifically illustrate hollow adhesive particles according to one embodiment of the present disclosure, and are not limited thereto.

[0050] In addition, the term "adhesive particles" refers to particles that increase the peel strength or the skid resistance when the separator is in contact with or pressed against the negative or positive electrode of a battery, compared to when the particle is not included.

[0051] Conventionally, when laminating an electrode and a separator, a separator with improved adhesive strength was provided by coating the surface that contacts the electrode with an adhesive material. However, in the case of a separator in which an adhesive material and inorganic particles are mixed to form a coating layer, there is a disadvantage that the adhesive strength is poor relative to the amount of adhesive material contained, since the inorganic particles and adhesive material are mixed on the surface that contacts the electrode. To solve this, it is necessary to put a large amount of adhesive material into the coating layer, but in this case, when applied to a secondary battery, a problem may occur in which the adhesive material reduces the battery performance.

[0052] One embodiment of a separator according to the present disclosure can include a porous substrate and a coating layer located on one or both sides of the porous substrate and including inorganic particles and hollow adhesive particles.

[0053] In one aspect of the present disclosure, the hollow adhesive particles have a hollow structure and therefore have a relatively low specific gravity compared to the inorganic particles, and can float on the surface. Therefore, in order to form an electrode adhesive layer, it is not necessary to have a separate process of applying an adhesive composition to form a coating layer, and the hollow adhesive particles can be mixed with the inorganic particles and simultaneously applied to form a coating layer, thereby imparting electrode adhesiveness to the hollow adhesive particles that naturally float on the surface layer.

[0054] In this way, by including hollow adhesive particles in the coating layer, the hollow structure of the hollow adhesive particles gives them a lower specific gravity than inorganic particles, so that the hollow adhesive particles can be easily guided toward the surface of the coating layer when the coating layer is formed. As a result, there is no need to form a separate adhesive layer, so that a smaller amount of adhesive substance, i.e., a smaller amount of hollow adhesive particles, can be included compared to the conventional technology of forming a separate adhesive layer, and even if a small amount is included, adhesive strength with the electrode can be exhibited.

[0055] In addition, when swelling occurs due to an electrolyte, etc., the coating layer can internally accommodate the electrolyte, thereby preventing external swelling. In addition, a secondary battery including a separator according to an embodiment of the present disclosure exhibits adhesion between the electrodes and the separator during battery assembly, improving cell assembly processability, and prevents separation between the electrodes and the separator during charging and discharging, thereby preventing various problems such as increased resistance or reduced cycle life due to separation between the electrodes and the separator. In addition, the battery expansion phenomenon can be prevented.

[0056] In other words, when the separator has a coating layer containing the hollow adhesive particles, it is possible to provide a new separator that provides excellent adhesion between the separator and electrodes and has the effect of preventing external swelling by internally accommodating swelling caused by electrolytes, etc.

[0057] Furthermore, the separator can provide a new separator that internally accommodates swelling caused by the electrolyte, suppresses external swelling, and prevents the adhesive from dissolving into the electrolyte due to the electrolyte.

[0058] In addition, the separator suppresses swelling due to the electrolyte and minimizes loss of adhesion with the electrode, i.e., prevents loss of adhesion due to swelling, and therefore provides a new separator and a battery using the same that maintain good alignment of the electrode module even when the electrodes and separators are stacked many times. In addition, the suppression of swelling and dissolution can improve electrode performance.

[0059] Specifically, the separator may include hollow adhesive particles made of a polymer as an adhesive for fixing the inorganic particles in a coating layer in which the inorganic particles are connected to each other and form pores by the inorganic particles, and for adhering to the electrodes.

[0060] In the case of the separator, compared to a separator conventionally manufactured using inorganic particles and a thermoplastic resin adhesive, such as a thermoplastic resin adhesive such as polyacrylate or polyamide, it is possible to impart effects such as the suppression of swelling, the increase in electrode adhesive strength, the ability to maintain alignment, and the prevention of loss of adhesive strength.

[0061] In addition, due to the difference in specific gravity between the hollow adhesive particles and inorganic particles in the coating layer, the hollow adhesive particles having a low specific gravity or density can be concentrated on the surface in contact with the electrode, so that the adhesive strength of the surface of the coating layer in contact with the electrode can be improved even if the content of adhesive particles exhibiting adhesiveness is minimized. Also, it goes without saying that the content of adhesive materials can be minimized, preventing the problem of deterioration of battery performance due to adhesive materials.

[0062] In a separator according to one embodiment of the present disclosure, when the surface facing the porous substrate is designated as a first surface and the surface opposite the first surface is designated as a second surface, the second surface can have a higher content of the hollow adhesive particles than the first surface.

[0063] In addition, the coating layer may have a gradient in which the content of the hollow adhesive particles increases from the first surface to the second surface.

[0064] Also, the coating layer may be composed of an inorganic particle layer containing inorganic particles and an adhesive layer formed by floating hollow adhesive particles on the inorganic particle layer, that is, as shown in Fig. 3, the hollow adhesive particles may be suspended to form a layer separate from the layer composed of the inorganic particles.

[0065] In the present disclosure, the separator may include a single coating layer, or alternatively, multiple coating layers may be stacked. In this case, multiple stacks may be used to vary the content of hollow adhesive particles relative to inorganic particles in each layer, thereby increasing the content of hollow adhesive particles on the surface that adheres to the electrode, thereby further improving electrode adhesion.

[0066] That is, when the coating layer has a single layer structure, the hollow adhesive particles may naturally rise to the surface to have a concentration gradient or form a separate adhesive layer during the process of coating the surface of the porous substrate with a slurry containing the hollow adhesive particles and the inorganic particles and drying the slurry, depending on the difference in specific gravity between the hollow adhesive particles and the inorganic particles. Alternatively, after coating the slurry, a process of maintaining the slurry for a predetermined time so that the hollow adhesive particles rise sufficiently to the surface and the inorganic particles sink toward the porous substrate may be introduced, and the concentration gradient of the hollow adhesive particles may be intentionally formed by adjusting the time of standing. That is, when the surface of the coating layer facing the porous substrate is the first surface and the surface opposite to the first surface is the second surface, the concentration of the hollow adhesive particles may be continuously increased from the first surface to the second surface, or the time of standing may be adjusted so that more hollow adhesive particles are distributed on the second surface. Alternatively, an adhesive layer may be formed on the second surface in the form of suspended hollow adhesive particles.

[0067] The coating layer may have a multi-layer structure in which at least one layer is laminated.

[0068] For example, the coating layer may have a multi-layer structure in which the content of the inorganic particles and the hollow adhesive particles is changed to form a plurality of layers with different contents of the hollow adhesive particles. In particular, the coating layer may have a structure divided into n (n≧2, a natural number) layers with different concentrations of the hollow adhesive particles. Specifically, n may be 2 to 5.

[0069] The coating layer may include a first coating layer having a first surface in contact with the porous substrate and a second surface opposite to the first surface, the first coating layer containing a first amount of hollow adhesive particles, a third surface in contact with the second surface and a fourth surface opposite to the third surface, the second coating layer containing a second amount of hollow adhesive particles, and an nth coating layer containing an nth amount of hollow adhesive particles. For example, when the coating layer is divided into two layers, the first coating layer containing a first amount of hollow adhesive particles and the second coating layer containing a second amount of hollow adhesive particles may be divided. Also, each coating layer may be in direct contact with each other.

[0070] In the present disclosure, the separator has a porous structure, and thus may have pores and porosity. The size and porosity of the pores formed in the separator may be appropriately adjusted according to the porosity of the porous substrate and the thickness of the coating layer. As an example, the average size of the pores formed in the separator, i.e., the average diameter of the pores, may be 0.001 to 10 μm, and the porosity may be 10 to 70%.

[0071] The separator according to one embodiment of the present disclosure may have a gas permeability of 500 sec / 100 cc or less, 400 sec / 100 cc or less, 300 sec / 100 cc or less, 200 sec / 100 cc or less, or 100 sec / 100 cc or less. The gas permeability is measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard.

[0072] In addition, the change in Gurley permeability ΔG according to the following formula can be 50 sec / 100 cc or less, 45 sec / 100 cc or less, 40 sec / 100 cc or less, 35 sec / 100 cc or less, or 30 sec / 100 cc or less.

[0073] ΔG=G1-G2

[0074] In the above formula, G1 is the Gurley permeability of a separator having coating layers formed on both sides of a porous substrate, and G2 is the Gurley permeability of the porous substrate itself. The Gurley permeability was measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard, and the unit is sec / 100cc.

[0075] The heat shrinkage rate can be 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, 2% or less, or 1% or less at 150° C. The heat shrinkage rate can be 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, or 2% or less at 170° C.

[0076] After the battery is assembled, the thickness deformation rate may be 5% or less, 4% or less, 3% or less, 2% or less, or 1% or less when charged and discharged 100 times. 2 After pressure bonding for 10 seconds or more at the above pressure, when peeled at 180° using an INSTRON UTM device in accordance with ASTM D 903, the adhesive strength between the separator and the electrode may be 0.5 gf / 15 mm or more, 1 gf / 15 mm or more, for example, 0.5 to 4 gf / 15 mm.

[0077] In addition, the electrode adhesive strength was evaluated as excellent in the electrode adhesive strength described later. Specifically, as shown in FIG. 4, the separator was stacked alternately with three positive electrodes and three negative electrodes of 4×6 cm size, and then subjected to 1 kgf / cm2 pressure in a 60°C atmosphere. 2After adhesion for 10 seconds, the device was unfolded and the number of electrodes still attached was evaluated. All six electrodes were able to maintain adhesion without coming apart.

[0078] [Porous base material] For example, the porous substrate of the separator is not limited as long as it is a substrate that has been used in the past for separators. Specifically, it may be a film, sheet, nonwoven fabric, or woven fabric made of a polymer material. Specifically, the porous substrate may include a porous substrate made of a polyolefin resin. The polyolefin resin may be, but is not limited to, at least one selected from the group consisting of high density polyethylene, low density polyethylene, linear low density polyethylene, ultra-high molecular weight polyethylene, polypropylene, and copolymers thereof.

[0079] The thickness of the porous substrate is not particularly limited, and may be in the range of 1 to 100 μm, 5 to 60 μm, 5 to 40 μm, 5 to 20 μm, or 5 to 10 μm. The porous substrate may be in the form of a porous film.

[0080] The pores formed in the porous substrate are not limited as long as they are of a size that allows smooth movement of lithium ions, but an average diameter of 0.01 to 20 μm, 0.05 to 5 μm, or 0.05 to 1 μm can be advantageous for smooth movement of lithium ions and impregnation with an electrolyte. In addition, although not particularly limited, the porosity can be 5 to 95%, or 30 to 60%. The porosity can be calculated by cutting a sample into a rectangle (thickness T μm) of A cm x B cm, measuring the mass, and calculating the ratio of the weight of the resin and the weight of the separator (Mg) of the same volume using the following formula: Porosity (%) = 100 x {1-M x 10000 / (A x B x T x ρ)}, where ρ (g / cm 2 ) is the density of the resin.

[0081] [Coating layer] For example, the coating layer may be formed on one or both sides of the porous substrate, and may be a layer having a porous structure in which inorganic particles and hollow adhesive particles are connected to each other to form pores. Alternatively, the coating layer may be a laminated structure in which an inorganic particle layer in which inorganic particles are connected to each other to form pores and an adhesive layer in which hollow adhesive particles are suspended on the inorganic particle layer are formed. The coating layer may be formed in direct contact with the porous substrate. Alternatively, another layer that is usually used in a separator, specifically an inorganic particle layer in which pores are formed between inorganic particles, may be further provided between the porous substrate and the coating layer, but is not limited thereto.

[0082] As described above, the coating layer allows the hollow adhesive particles to be concentrated on the surface that contacts the electrode, thereby solving the problems of the conventional separator.

[0083] The thickness of the coating layer is not particularly limited, but for example, the thickness of the coating layer formed on one side of the porous substrate may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, 1.5 μm or more, 2 μm or more, 3 μm or more, or 5 μm or more, for example, 0.1 to 10 μm, 0.2 to 5 μm, or 0.2 to 3 μm, but is not limited thereto. In addition, the coating layer may include an adhesive layer formed by suspending the hollow adhesive particles, and the thickness of the adhesive layer may be, but is not limited to, 0.01 to 20 μm. The thickness of the adhesive layer may be adjusted by adjusting the content of the hollow adhesive particles used, but is not limited thereto.

[0084] As an example, the thickness ratio of the porous substrate of the separator to the coating layer may be, but is not limited to, 1:0.01-1, or 1:0.05-0.5, as long as the object of the present disclosure can be achieved. This range is preferable because excellent battery stability, suppression of swelling, improvement of battery performance, and excellent adhesion to the electrode can be secured within the above range, but is not limited thereto. As an example, the coating layer may be formed on 90% or more of the total area of ​​each surface of the porous substrate, and 95% or more, or 100% of the total area of ​​each surface of the porous substrate, except in the case where micro defects occur.

[0085] The coating layer may further contain other commonly known additives in addition to the inorganic particles and hollow adhesive particles described above, such as dispersants, lubricants, antifoaming agents, thickeners, etc., and the content thereof may be about the same as that of commonly used additives.

[0086] In addition, the coating layer may further include a conventional binder, instead of hollow adhesive particles, as an adhesive for fixing the particles of the inorganic particle layer, which may be used in an amount significantly smaller than that used in the past. Such a conventional binder is not particularly limited, but may include, for example, any one or a mixture of two or more selected from acrylic polymers, styrene polymers, vinyl alcohol polymers, vinylpyrrolidone polymers, and fluorine polymers.

[0087] For example, the polyacrylamide, poly(meth)acrylate, acrylic acid-methacrylic acid copolymer, polystyrene, polyvinyl alcohol, polyvinyl acetate, polyvinyl acetate-polyvinyl alcohol copolymer, polyvinylpyrrolidone, polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, hexafluoropropylene, polyvinylidene fluoride-hexafluoropropylene, polychlorotrifluoroethylene, etc., or a mixture of two or more thereof, or a copolymer thereof, may be used, but is not limited thereto.

[0088] The binder and additives may be further included in an appropriate minimum amount, and as a non-limiting example, the binder may be 0.1 to 5 parts by weight and the additive may be 0.1 to 3 parts by weight per 100 parts by weight of inorganic particles. This is an example and is not limited thereto.

[0089] The inorganic particles contained in the coating layer may be, for example, one or more selected from metal oxides, metal nitrides, metal carbides, metal carbonates, metal hydrates, and metal carbonitrides. For example, boehmite, Ga 2 O 3 , SiC, SiC 2 , Quartz, NiSi, Ag, Au, Cu, Ag-Ni, ZnS, Al 2 O 3 , TiO 2 , CEO 2 , MgO, NiO, Y 2 O 3 , CaO, SrTiO 3 , SnO 2 , ZnO, and ZrO 2 However, the present invention is not limited to these, so long as the material is electrochemically unstable and does not significantly affect the battery performance.

[0090] The shape of the inorganic particles is not particularly limited as long as the purpose of improving the durability and heat resistance of the porous substrate is achieved. Specifically, the inorganic particles may have one or more shapes selected from the group consisting of spherical, angular, and amorphous.

[0091] The size of the inorganic particles is not limited as long as the above-mentioned object is achieved, and specifically, the size of the inorganic particles, i.e., the average diameter, can be 0.001 to 100 μm, specifically 0.01 to 50 μm, and more specifically 0.01 to 10 μm. Within the above range, it is preferable to have the above-mentioned separator porosity, but it is not necessarily limited thereto.

[0092] The hollow adhesive particles used in the coating layer may be hollow organic particles or polymer particles, and as shown in FIG. 1 and FIG. 2, the hollowness is formed inside, so that the hollow adhesive particles have a lower density and buoyancy than inorganic particles. The hollowness of the hollow adhesive particles is not particularly limited as long as it achieves the above-mentioned purpose, i.e., the purpose of forming a lower density than inorganic particles. As an example, the hollowness of the hollow adhesive particles may be 5 to 97%, or 50 to 95%, but is not limited thereto. The hollowness can be calculated from the outer diameter and inner diameter of the hollow adhesive particles by the following formula. The outer diameter and inner diameter mean the average particle size, and can be measured using SEM, etc. Hollowness (%) = inner diameter / outer diameter x 100, the outer diameter means the average particle size of the hollow adhesive particles, i.e., the average outer diameter, and the inner diameter is calculated by subtracting the thickness of the shell layer from the average particle size by measuring the thickness of the shell layer using SEM, TEM, etc. In addition, when the hollow adhesive particles are hollow particles having a non-uniform hollow shape, the hollow ratio can be calculated based on the correlation between the density (apparent density) measured using a powder density measurement method and the theoretical density. In this case, the hollow ratio (%) can be calculated as (1-apparent density / theoretical density) x 100.

[0093] The hollow adhesive particle is composed of a hollow core 11 and a shell layer 12 made of an adhesive material as shown in Fig. 1, and the shell layer may be composed of at least one layer. Also, as shown in Fig. 2, the hollow core may further include a structural material layer 13 between the hollow core 11 and the shell layer 12 for forming and maintaining the hollow structure.

[0094] The shell layer of the hollow adhesive particle is preferably made of a material having adhesive properties to the porous substrate and the electrode, and is not particularly limited as long as it has adhesive properties such as those conventionally used as adhesive materials. As an example, the adhesive material may be an adhesive resin having adhesive properties at room temperature or at a temperature equal to or higher than the glass transition temperature (Tg). The adhesive resin may be a thermoplastic polymer, and may include, for example, but is not limited to, an acrylic resin, a fluorine resin, an amide resin, and copolymers or mixtures thereof. As an example, the shell layer of the hollow adhesive particle may be a shell layer in which the adhesive resin is crosslinked.

[0095] The structure material layer may be made of the same or different resin as the shell layer, and any material that can maintain the hollow core structure may be used without limitation. The structure material layer may be made of a material that has or does not have adhesive properties. For example, SiO 2 , Al 2 O 3 , ZnO, TiO 2 , SnO 2 The material may be selected from, but is not limited to, carbon, polystyrene, polyacrylate, PVDF, and the like.

[0096] The size of the hollow adhesive particles is not limited as long as the above-mentioned object is achieved, and the size of the hollow adhesive particles, i.e., the average outer diameter, can be, but is not necessarily limited to, 10 nm to 10 μm, or 50 nm to 5 μm, or 0.1 to 5 μm, or 0.2 to 2 μm.

[0097] As described above, the hollow adhesive particles are not particularly limited as long as they form a hollow. For example, they may be prepared by polymerizing acrylate, acrylic acid, and a multifunctional acrylic crosslinker. Here, they may contain a polar monomer such as acrylic acid, which is preferable because it can induce adhesion with the inorganic particles of the coating layer and improve adhesion with the active material or metal layer of the electrode, but is not limited thereto.

[0098] The hollow adhesive particles may be manufactured in various ways, for example, but not limited to, the method disclosed in Korean Patent Publication No. 2020-0138213 (Publication date: December 9, 2020, Zeon Corporation). It is preferable that such hollow adhesive particles have a crosslinked shell layer, for example, by increasing the crosslinking ratio of crosslinking monomers in the shell layer to prevent collapse in order to maintain the internal hollow shape.

[0099] The shell layer may be a single layer or may have multiple layers, but is not particularly limited thereto. Therefore, the coating layer may contain either one of the single-structure hollow adhesive particles and the double-structure hollow adhesive particles, or may contain both the single-structure hollow adhesive particles and the double-structure hollow adhesive particles. Also, the coating layer may contain all of the hollow particles exemplified in FIG. 1 and FIG. 2.

[0100] The coating layer may contain more inorganic particles than the hollow adhesive particles. The hollow adhesive particles may be used in a small amount that can exhibit adhesiveness, and for example, the hollow adhesive particles may be contained in an amount of 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, or 1.0 parts by weight or more, or 20 parts by weight or less, 19 parts by weight or less, 18 parts by weight or less, 17 parts by weight or less, 16 parts by weight or less, or 15 parts by weight or less, and may be used in these ranges. For example, the hollow adhesive particles may be contained in an amount of 0.1 to 20 parts by weight, 0.2 to 20 parts by weight, 1 to 20 parts by weight, 1 to 15 parts by weight, 1 to 10 parts by weight, 1 to 8 parts by weight, or 1 to 5 parts by weight, and although not limited thereto, sufficient electrode adhesive strength can be exhibited even in the above range. In addition, if necessary, the composition may further contain 0.1 to 5 parts by weight of a non-hollow polymer binder and 0.1 to 5 parts by weight of an additive, based on 100 parts by weight of the inorganic particles, but is not limited thereto.

[0101] [Separator manufacturing method] The method for producing the separator will be described in detail below.

[0102] In the present disclosure, the method for producing a separator includes a coating step of applying a coating composition including inorganic particles and hollow adhesive particles onto one or both sides of a porous substrate to form a coating layer, and a drying step of drying the coating layer.

[0103] 3, a coating composition including the inorganic particles 20 and hollow adhesive particles 10 may be applied to one side of a porous substrate 100 and then dried to produce a coating layer 200 having a higher content of the hollow adhesive particles on the surface, i.e., the surface not in contact with the porous substrate. Alternatively, the hollow adhesive particles may be substantially guided to the surface to form an adhesive layer.

[0104] As an example, when the surface facing the porous substrate is designated as a first surface and the surface opposite the first surface is designated as a second surface, the second surface may contain a higher content of the hollow adhesive particles than the first surface.

[0105] For example, the coating layer may be manufactured to have a gradient in which the content of the hollow adhesive particles increases from the first surface to the second surface, or the coating layer may be composed of an inorganic particle layer containing inorganic particles and an adhesive layer in which hollow adhesive particles are suspended on the inorganic particle layer.

[0106] In one embodiment, before the drying step, in order to artificially induce the formation of a gradient or another adhesive layer due to the difference in specific gravity between the hollow adhesive particles and the inorganic particles, the coating may be left to stand for a predetermined time, vibrated, or both may be applied simultaneously or successively, and then dried. That is, the coating composition may be applied and then left to stand for a predetermined time, and then dried. Alternatively, the coating composition may be applied and then left to stand for a predetermined time, and then vibrated, and then dried. Alternatively, the coating composition may be applied and then left to stand for a predetermined time, and then vibrated and then dried. Alternatively, the coating composition may be applied and then vibrated, and then dried. Alternatively, the coating composition may be applied and then vibrated, and then dried. In one embodiment, the time for leaving to stand for a predetermined time may be adjusted to adjust the gradient of the hollow adhesive particles, or an adhesive layer formed by floating hollow adhesive particles may be formed.

[0107] In one embodiment, when the coating layer is formed on both sides of the porous substrate, a coating layer may be formed on one side and then a coating layer may be formed on the other side. Although both sides may be simultaneously coated, as intended in the present disclosure, it is preferable to coat each side on the side on which the hollow adhesive particles are guided to the surface.

[0108] As described above, the hollow adhesive particles migrate to the air surface (the surface opposite to the surface in contact with the porous substrate) due to the difference in specific gravity and dry there, so that the hollow adhesive particles having adhesive properties are present in large amounts on the surface, and therefore even if a small amount of hollow adhesive particles is used, adhesive strength with the electrode can be exhibited.

[0109] The hollow adhesive particles can adjust the strength, particularly the compressive strength, by adjusting the degree of crosslinking, and can also induce an increase in heat resistance.

[0110] In this method for producing a separator, a separator having excellent adhesive strength with an electrode can be easily produced simply by forming a coating layer containing the hollow adhesive particles on a porous substrate.

[0111] In one embodiment, the coating layer may further include a non-hollow organic binder as the conventional organic binder described above, but the content can be significantly reduced by using hollow adhesive particles.

[0112] In the preparation method, the porous substrate, the inorganic particles, the hollow adhesive particles, and the prepared separator have been described above, and detailed description will be omitted below, and each step will be described in detail.

[0113] The coating composition may be in the form of a slurry in which inorganic particles and hollow adhesive particles are dispersed in a solvent. In addition, the coating composition may further include a non-hollow polymer binder as necessary, and may further include additives that are generally used in the relevant field.

[0114] The solvent is not particularly limited as long as it can disperse the inorganic particles and hollow adhesive particles, which are solids. For example, the solvent may be water, lower alcohols such as ethanol, methanol, and propanol, dimethylformamide, acetone, tetrahydrofuran, diethyl ether, methylene chloride, N-methyl-2-pyrrolidone, hexane, cyclohexane, or a mixture thereof, but is not necessarily limited thereto.

[0115] The content of the solid matter in the slurry-like coating composition can be appropriately adjusted so that it is easy to apply and can induce a layer separation phenomenon due to the difference in density between the inorganic particles and the hollow adhesive particles when dried. Specifically, the content of the solid matter in the coating composition can be 10 to 60% by weight, or 20 to 50% by weight, but is not limited thereto. The solid matter includes inorganic particles and hollow adhesive particles, and can further include a non-hollow polymer binder as necessary. For example, the content of the solid matter can include 0.1 to 20 parts by weight, 0.1 to 15 parts by weight, 0.1 to 10 parts by weight, 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, or 0.1 to 2 parts by weight of hollow adhesive particles relative to 100 parts by weight of inorganic particles. In addition, the composition can further include 0.1 to 5 parts by weight of a non-hollow polymer binder and 0.1 to 5 parts by weight of an additive relative to 100 parts by weight of the inorganic particles as necessary, but is not limited thereto.

[0116] In addition, the coating composition may further include additives within a range that does not significantly deteriorate the coating property or the battery performance. Specifically, for example, the additives may include dispersants, lubricants, antifoaming agents, thickeners, etc., but are not limited thereto, and since they have been described above, further description will be omitted.

[0117] The coating method for coating the coating composition on one or both sides of the porous substrate is not limited, and specifically, may be a common coating method such as bar coating, dip coating, flow coating, knife coating, roll coating, gravure coating, spray coating, etc.

[0118] In the drying step, the drying means is not particularly limited as long as it can remove 90% or more of the solvent. The drying temperature can be changed depending on the solvent, and can be, for example, 20 to 200°C, and is not limited as long as the surface structure is not changed by the sudden evaporation of the solvent or the hollow adhesive particles are not melted and collapsed. As a specific example, it can be dried with hot air at 25°C to 100°C, and the drying time is not limited, but can be, for example, 5 seconds to 300 seconds. In addition, drying methods using infrared rays, near infrared rays, heat rolls, and hybrid forms thereof are also possible. Within the above range, the hollow adhesive particles can be smoothly suspended, and a larger amount of the hollow adhesive particles can be located in the upper region, adhesive layer, or n-th coating layer.

[0119] In one embodiment, the drying step may involve vibration or artificial standing time before drying, or these mixing means may be used to provide a concentration gradient of the hollow adhesive particles.

[0120] When the vibration is further applied, the floating phenomenon of the hollow adhesive particles due to the difference in specific gravity between the inorganic particles and the hollow adhesive particles can be more smoothly performed. The vibration is not particularly limited as long as it can be applied to the coating composition. For example, the vibration can be applied directly to the coating composition by applying energy such as ultrasonic waves. Alternatively, the vibration can be applied to the coating composition by applying physical vibration such as a motor to the porous substrate.

[0121] In one embodiment, the method may further include a step of leaving the coating composition to allow the hollow adhesive particles to have a sufficient gradient before the drying step. Specifically, the coating composition may be left to stand for about 30 seconds to 1 hour after being applied onto a porous substrate, so that the hollow adhesive particles are sufficiently suspended on the surface of the coating layer. The temperature at which the coating composition is left to stand is preferably 0 to 50°C, and more preferably room temperature (25±5°C), but is not limited thereto.

[0122] [Secondary battery] The secondary battery will be described in detail below.

[0123] In the present disclosure, the secondary battery includes the above-mentioned separator, and specifically, the secondary battery can have a structure in which the above-mentioned separator is interposed between and bonded to a negative electrode and a positive electrode.

[0124] In particular, the positive and negative electrodes are not limited as long as they are materials normally used as positive and negative electrodes of secondary batteries.

[0125] A secondary battery including the above separator has improved adhesive strength between the electrode and the separator, and can prevent the electrode and the separator from being separated during charging and discharging. This can solve various problems such as an increase in resistance or a decrease in cycle life due to the separation between the electrode and the separator, and can achieve high capacity and large size, making it practically highly industrially applicable. In addition, despite the high adhesive strength, the battery contains a relatively small amount of adhesive material, and can prevent the problem of battery performance degradation due to adhesive material.

[0126] The method for producing the secondary battery will be described in detail below.

[0127] In the present disclosure, a method for manufacturing a secondary battery is a method for manufacturing the above-mentioned secondary battery, which includes a step of positioning the above-mentioned separator between two electrodes and then applying heat, pressure, or heat and pressure to attach the electrodes to the separator. Such a method for manufacturing a secondary battery can easily manufacture a secondary battery having very high durability.

[0128] The adhesion can be performed by applying heat, pressure, or both heat and pressure as described above, and specifically, it can be heat fusion, in which both heat and pressure are applied. When such adhesion is performed, the hollow adhesive particles can be broken, which can provide a higher adhesive strength.

[0129] Specifically, the adhesion can be performed by applying heat to a temperature above the glass transition temperature (Tg) of the hollow adhesive particles, more specifically, at Tg or 1.2Tg of the hollow adhesive particles, but is not limited thereto, provided that within this range, the hollow adhesive particles can be damaged while maintaining a high adhesive strength.

[0130] The present disclosure will be described in more detail below based on examples and comparative examples. However, the following examples and comparative examples are merely examples for describing the present disclosure in more detail, and the present disclosure is not limited by the following examples and comparative examples.

[0131] The physical properties were measured as follows.

[0132] 1) Adhesion force to electrode The separator thus produced was placed between the positive and negative electrodes and subjected to a test at 60°C and 1 kgf / cm 2 After adhesion for 10 seconds, the adhesive strength to the electrode was evaluated.

[0133] The positive and negative electrodes used in the evaluation were prepared as follows.

[0134] Positive electrode production: Lithium cobalt oxide (LiCoO 2 A positive electrode mixture slurry was prepared by adding 92% by weight of ZnO, 4% by weight of carbon black as a conductive material, and 4% by weight of polyvinylidene fluoride (PVDF) as a binder to a solvent, N-methyl-2-pyrrolidone (NMP). The prepared slurry was applied to a 30 μm-thick aluminum (Al) thin film, dried at a temperature of 120°C, and then roll-pressed to prepare a positive electrode with a thickness of 140 μm.

[0135] Preparation of negative electrode: Graphite carbon, PVDF as a binder, and carbon black as a conductive agent were added at 96 wt%, 3 wt%, and 1 wt%, respectively, to NMP as a solvent to prepare a negative electrode mixture slurry. The prepared slurry was applied to a copper (Cu) thin film with a thickness of 20 μm, dried at 120°C, and pressed with a roll press to prepare a negative electrode with a thickness of 150 μm.

[0136] The electrode adhesion was measured by peeling at 180° using an Instron UTM instrument according to ASTM D 903. The unit of adhesion is gf / 15 mm.

[0137] 2) Stacking Adhesiveness The electrodes used in the adhesive evaluation were cut into pieces 4 cm wide and 6 cm long, and three cut pieces of the positive electrode and three cut pieces of the negative electrode were stacked alternately on the surface of the separator as shown in Figure 4. Then, they were subjected to 1 kgf / cm2 pressure in a 60°C atmosphere. 2 After adhesion for 10 seconds, the plate was unfolded and the number of electrodes attached was counted.

[0138] 3) Gas permeability The gas permeability was measured using a Gurley type densometer manufactured by Toyoseiki Co., Ltd. in accordance with JIS P8117. The measured value was corrected to a thickness value and converted to a value that does not vary depending on the thickness.

[0139] 4) Change in Gurley transmittance The change in Gurley permeability, ΔG, is calculated as follows:

[0140] ΔG=G1-G2

[0141] In the above formula, G1 is the Gurley permeability of a separator having coating layers formed on both sides of a porous substrate, and G2 is the Gurley permeability of the porous substrate itself. The Gurley permeability was measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard, and the unit is sec / 100cc.

[0142] 5) Heat shrinkage rate Separators of 10 cm×10 cm were left to stand at 130° C., 150° C. and 170° C. for 1 hour, respectively, and then the reduction in area was measured and the thermal shrinkage was calculated by the following formula.

[0143] Heat shrinkage rate (%) = ((length before heating - length after heating) / length before heating) x 100

[0144] 6) Battery performance and battery deformation rate The separator was used to assemble pouch-type batteries in a stacking manner between the positive and negative electrodes, and 1M lithium hexafluorophosphate (LiPF 6A lithium secondary battery was manufactured by injecting an electrolyte solution of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) = 3:5:2 (volume ratio) in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) was dissolved. As a result, a pouch-type lithium ion secondary battery with a capacity of 2 Ah was manufactured. The resistance (DC-IR) of the lithium secondary battery was evaluated using the J-pulse (Japan Electric Vehicle Association Standards, JEVS D 713) method, which evaluates discharge and charge characteristics for 10 seconds at 0.25C, 0.5C, 1.0C, 1.5C, 2.0C, and 2.5C. The average impedance of three batteries was calculated using the above method, and the initial resistance and its standard deviation were calculated. The relative comparison value of the initial resistance means an increased value compared to the initial resistance of an uncoated porous substrate (Comparative Example 2).

[0145] Relative comparison with Ref.(%)=((Impedance-Impedance base material) / Impedance base material)×100

[0146] For the cycle life, after 100 charge / discharge cycles at 0.5C, the impedance was calculated using J-pulse in the same manner as in the initial resistance measurement method, and the average and standard deviation of the three values ​​were calculated.

[0147] After 100 charge / discharge cycles, the change in resistance was calculated as follows:

[0148] Relative changes in impedance(%)=((Impedance 100サイクル -Impedance 初期 ) / Impedance 初期 ) x 100

[0149] The battery deformation rate was calculated by measuring the thickness change of the battery after 100 charge / discharge cycles.

[0150] The thickness of the battery was measured at five points (four points at the corners and one point at the center) and the average value was calculated.

[0151] ΔTh(%)=((Thn-Th0) / Th0)×100

[0152] In the above formula, Th0 is the initial battery thickness, and Thn is the battery thickness measured after the secondary battery was charged and discharged 100 times.

[0153] 7) Average particle size and average outer diameter According to the ISO 13320-1 standard, the average particle size (D 50 ), D 10 and D. 90 was measured.

[0154] [Example 1] 100 parts by weight of boehmite (γ-AlO(OH)) with an average particle size of 300 nm was added to water, and 3 parts by weight of polyacrylamide (Mw 150,000 g / mol, Sigma Aldrich) was added, and 0.7 parts by weight of a dispersant (BYK-2018) was added to the boehmite, and the mixture was stirred to produce a uniform aqueous slurry with a solid content of 30 wt%. 1 part by weight of hollow acrylic particles with an average outer diameter of 0.9 μm and a hollow ratio of 78% produced according to Example 5 of Korean Patent Publication No. 2020-138213A (publication date: December 9, 2020) was added to the boehmite, and water was further added to produce a slurry composition with a final solid content of 25 wt%. The prepared slurry composition was coated on both sides of a 9 μm thick polyolefin microporous membrane (ENPASS, SK Innovation, average pore size: 40 nm) at a speed of 10 m / min and dried with hot air at 45° C. Drying was continued until there was no further weight loss. Then, the membrane was wound up. After drying, the thickness of the coating layers on both sides was 3.0 μm. The physical properties of the prepared separator were evaluated and are shown in Table 1, and the physical properties of a cell using the prepared separator were evaluated and are shown in Table 2.

[0155] When the manufactured separator was observed using an Energy Dispersive Spectrometer (EDS) attached to a SEM (scanning electron microscope), it was confirmed that hollow acrylic particles floated on the surface and formed an adhesive layer.

[0156] [Example 2] The same procedure as in Example 1 was repeated except that the slurry composition was applied to one side of a polyolefin microporous membrane fixed to a glass plate of 0.2 m x 0.2 m size using a bar coating method, and then the plate was left to stand for 3 minutes, and then ultrasonic vibration was applied to the glass plate, and the plate was dried with hot air at 45°C for a period of time until no further weight loss occurred. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of a cell using the produced separator were evaluated and are shown in Table 2.

[0157] The manufactured separator was observed using an EDS attached to a SEM (scanning electron microscope), and it was confirmed that the hollow acrylic particles floated on the surface and formed an adhesive layer. In addition, it was confirmed that more hollow acrylic particles were floating on the surface compared to Example 1.

[0158] [Example 3] The same procedure was carried out as in Example 1, except that the hollow acrylic particles were added in an amount of 2 parts by weight relative to the boehmite. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of the cell using the produced separator were evaluated and are shown in Table 2.

[0159] [Example 4] The same procedure was carried out as in Example 1, except that 5 parts by weight of hollow acrylic particles were added relative to the boehmite. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of a cell using the produced separator were evaluated and are shown in Table 2.

[0160] [Comparative Example 1] A slurry was prepared in the same manner as in Example 1, except that hollow acrylic particles were not used, and a separator was prepared in the same manner. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of a cell using the produced separator were evaluated and are shown in Table 2.

[0161] [Comparative Example 2] The properties of the polyolefin microporous membrane (ENPASS, SK Innovation, average pore size: 40 nm) used in Example 1 were evaluated and are shown in Table 1. That is, the properties of the polyolefin microporous membrane itself without forming a coating layer were measured and shown in Table 1, and the properties of the cell using the same were measured and shown in Table 2.

[0162] [Table 1]

[0163] [Table 2]

[0164] As described above, the present disclosure has been described by citing specific matters and limited examples and comparative examples. However, these are provided to aid in a more general understanding of the present disclosure, and the present disclosure is not limited to the above examples. A person having ordinary knowledge in the field to which the present disclosure pertains can make various modifications and variations from such descriptions.

[0165] Therefore, the idea of ​​the present disclosure should not be limited to the above-described embodiments, and it can be said that not only the scope of the claims described below, but also all equivalent or similar variations to the scope of the claims fall within the scope of the idea of ​​the present disclosure. [Explanation of symbols]

[0166] 10 Hollow adhesive particles 20 Inorganic particles 11 Hollow-core 12 Shell layer 13 Structure material layer 100 Porous substrate 200 coating layers

Claims

1. A porous substrate; a coating layer located on one or both sides of the porous substrate, the coating layer comprising inorganic particles and hollow adhesive particles.

2. 2. The separator according to claim 1, wherein a surface of the coating layer facing the porous substrate is defined as a first surface and a surface opposite to the first surface is defined as a second surface, and the second surface has a higher content of the hollow adhesive particles than the first surface.

3. The separator according to claim 2 , wherein the coating layer has a gradient in which the content of the hollow adhesive particles increases from the first surface to the second surface.

4. The separator according to claim 3 , wherein the coating layer comprises an inorganic particle layer containing inorganic particles and an adhesive layer formed by suspending hollow adhesive particles on the inorganic particle layer.

5. The separator according to claim 1 , wherein the coating layer is a laminate of at least one layer.

6. 2. The separator according to claim 1, wherein the hollow adhesive particles have a hollow ratio of 5 to 97%.

7. The separator according to claim 1, wherein the hollow adhesive particles have an average outer diameter of 10 nm to 10 μm.

8. 2. The separator according to claim 1, wherein the hollow adhesive particle includes a hollow core having a hollow structure with an open interior and a shell layer made of an adhesive substance, and the adhesive substance includes an adhesive resin having adhesive strength at room temperature or at a temperature equal to or higher than the glass transition temperature.

9. The separator according to claim 8 , wherein the adhesive resin comprises an acrylic resin, a fluorine-based resin, an amide resin, a copolymer thereof, or a mixture thereof.

10. The separator of claim 9 , wherein the adhesive resin is crosslinked.

11. The separator according to claim 8 , wherein the hollow adhesive particle further comprises a structural material layer between the hollow core and the shell layer for maintaining the hollow structure.

12. The separator according to claim 1 , further comprising an inorganic particle layer between the porous substrate and the coating layer.

13. A coating step of applying a coating composition including inorganic particles and hollow adhesive particles onto one or both sides of the porous substrate to form a coating layer; and drying the coating layer.

14. The method for producing a separator according to claim 13, further comprising the step of applying vibration prior to or simultaneously with the drying step.

15. The method for producing a separator according to claim 13, further comprising the step of leaving the separator coated with the coating composition undisturbed after the coating step and before drying.

16. 14. The method for manufacturing a separator according to claim 13, wherein after the coating step and the drying step, the hollow adhesive particles float on the surface of the coating layer to form a gradient, or an adhesive layer made of the hollow adhesive particles is formed on the surface of the coating layer.

17. The method for producing a separator according to claim 13, wherein the coating composition has a solid content of 10 to 60 wt %.

18. The method for producing a separator according to claim 13, wherein the coating composition contains 0.2 to 20 parts by weight of the hollow adhesive particles based on 100 parts by weight of the inorganic particles.

19. The method for producing a separator according to claim 13, wherein the drying is performed with hot air at 25 to 100°C.

20. A secondary battery comprising the separator according to any one of claims 1 to 12.

21. After the separator according to any one of claims 1 to 12 is placed between the positive electrode and the negative electrode, A method for manufacturing a secondary battery, comprising the step of applying heat, pressure, or heat and pressure to integrate the separator and electrodes.

Citation Information

Patent Citations

  • Integral All-Solid State Rechargeable Batteries

    KR1020190036724A