Carbon nanotube dispersion liquid, and resin composition, conductive film, mixture slurry, electrode, and non-aqueous electrolyte secondary battery using the same
A carbon nanotube dispersion with bundle-shaped carbon nanotubes addresses the challenge of achieving stable and efficient battery performance by enhancing cycle characteristics and reducing resistivity, forming conductive films and electrodes for non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2024139880
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-26
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
Stable production of carbon nanotubes in a bundle shape for use in batteries is challenging, particularly when silicon is used as the negative electrode active material, leading to difficulties in achieving excellent cycle characteristics.
A carbon nanotube dispersion containing bundle-shaped carbon nanotubes with specific diameter and length ratios, along with a solvent and optionally a dispersant, is formulated to enhance stability and conductivity, forming conductive films and electrodes for non-aqueous electrolyte secondary batteries.
The solution improves the cycle characteristics and maintains film thickness, enhances electrode toughness, and reduces resistivity, resulting in improved battery performance.
Smart Images

Figure 2024159893000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a carbon nanotube dispersion containing bundle-shaped carbon nanotubes, and more particularly to a resin composition containing the carbon nanotube dispersion and a resin, a composite slurry containing the carbon nanotube dispersion, a resin, and an active material, a conductive film and an electrode film formed by forming them into a film shape, and a nonaqueous electrolyte secondary battery including the electrode film and an electrolyte. [Background technology]
[0002] In recent years, electronics has developed remarkably, and there is a demand for conductive materials used in various electronic devices and batteries to be smaller, lighter, and less expensive, while also having a longer life under various operating environments. To date, conductive carbon materials with low volume resistivity, such as various graphites and carbon nanotubes, have been investigated.
[0003] On the other hand, when a conductive material is used in various electronic devices or batteries, a dispersion in which the conductive material is dispersed in a solvent is often used, but this has a major problem in that the dispersion leads to a decrease in properties such as a decrease in conductivity, etc. Therefore, it is very important to prepare a dispersion that can obtain the desired properties.
[0004] For example, in the case of lithium-ion secondary batteries, carbon materials such as graphite, which have a large charge / discharge capacity per unit mass at a base potential close to that of lithium, are used as negative electrode materials in lithium-ion secondary batteries. However, these electrode materials are used to the extent that the charge / discharge capacity per mass is close to the theoretical value, and the energy density per mass of the battery is approaching its limit. Therefore, in order to increase the utilization rate of the electrode, attempts are being made to reduce the conductive additives and binders that do not contribute to the discharge capacity.
[0005] As the conductive assistant, carbon black, Ketjen black, graphene, fine carbon materials, etc. are used, and in particular, carbon nanotubes, which are a type of fine carbon fiber, are widely used. For example, Patent Documents 1 to 3 disclose that adding carbon nanotubes to graphite or silicon, which is a negative electrode active material, reduces the electrode resistance value, improves the internal resistance of the battery, improves the strength of the electrode, and improves the expansion and contraction properties of the electrode, thereby improving the cycle life of the lithium ion secondary battery. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 4-155776 [Patent Document 2] Japanese Patent Application Publication No. 4-237971 [Patent Document 3] JP 2004-178922 A [Patent Document 4] Special Publication No. 2018-534731 [Patent Document 5] Special Publication No. 2018-534747
[0007] However, it is difficult to stably obtain carbon nanotubes having a bundle shape as shown in Patent Documents 4 and 5, and it is also difficult to obtain excellent cycle characteristics, particularly in batteries using silicon as the negative electrode active material. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present disclosure is to provide a carbon nanotube dispersion that has excellent cycle characteristics when used as a battery, and a resin composition, a conductive film, a composite slurry, an electrode, and a nonaqueous electrolyte secondary battery that use the dispersion. [Means for solving the problem]
[0009] A carbon nanotube dispersion according to one embodiment of the present invention is a carbon nanotube dispersion comprising bundled carbon nanotubes using carbon nanotubes having an average diameter of 3 nm to 30 nm and a solvent, and is characterized in that, based on the number of carbon nanotubes with an outer diameter of 10 nm or more contained in the carbon nanotube dispersion, the proportion of bundled carbon nanotubes having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% or more.
[0010] The carbon nanotube dispersion according to one embodiment of the present invention is characterized in that the bundle-shaped carbon nanotubes have an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm and have an average aspect ratio of 5 to 100.
[0011] The carbon nanotube dispersion liquid according to one aspect of the present invention is characterized by further containing a dispersant.
[0012] A conductive film according to one aspect of the present invention is a coating film of the carbon nanotube dispersion liquid.
[0013] A carbon nanotube resin composition according to one aspect of the present invention is characterized by containing the above carbon nanotube dispersion liquid and a binder.
[0014] A composite slurry according to one aspect of the present invention is characterized by containing the above carbon nanotube resin composition and an active material.
[0015] An electrode film according to one aspect of the present invention is a coating film of the above-mentioned composite slurry.
[0016] A nonaqueous electrolyte secondary battery according to one embodiment of the present invention is a nonaqueous electrolyte secondary battery including a positive electrode, a negative electrode, and an electrolyte, wherein at least one of the positive electrode and the negative electrode includes the above-described electrode film. Effect of the Invention
[0017] The present disclosure makes it possible to provide a carbon nanotube dispersion that has excellent cycle characteristics when used in a battery, as well as a resin composition, a conductive film, a composite slurry, an electrode, and a nonaqueous electrolyte secondary battery that use the dispersion. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 shows an image of the carbon nanotube dispersion liquid described in Example 1 observed with a scanning electron microscope at a magnification of 20,000 times, which was processed using image analysis software (WINROOF2015: manufactured by Mitani Shoji Co., Ltd.). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Carbon nanotube dispersion liquid> The carbon nanotube dispersion of the present disclosure contains bundled carbon nanotubes made of carbon nanotubes having an average diameter of 3 nm to 30 nm and a solvent, and is characterized in that, based on the number of carbon nanotubes with an outer diameter of 10 nm or more contained in the carbon nanotube dispersion, the proportion of bundled carbon nanotubes (X) having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% or more. By containing a certain amount of such bundled carbon nanotubes (X) having a predetermined shape, not only the resistivity of the composite layer is reduced, but also the ability to follow expansion and contraction is improved. This strengthens the electrode film and improves the peel strength. Furthermore, the stability of the coating film is increased during charging and discharging, which is subject to large stress, and the film thickness can be maintained. In addition, excellent cycle characteristics can be exhibited. The carbon nanotube dispersion, resin composition, conductive film, composite slurry, electrode, and nonaqueous electrolyte secondary battery of the present disclosure will be described in detail below. In this specification, carbon nanotubes may be abbreviated as CNT.
[0020] <Bundled carbon nanotubes> The bundled carbon nanotubes contained in the carbon nanotube dispersion liquid of the present disclosure are carbon nanotubes having a bundle shape and made of carbon nanotubes having an average diameter of 3 nm to 30 nm. The bundled carbon nanotubes are a bundle in which a plurality of carbon nanotubes are aligned or arranged in a certain direction, and the outer diameter and fiber length refer to the outer diameter (minor diameter) and fiber length (major diameter) of the bundle. The dispersion of the present disclosure contains a predetermined amount of bundled carbon nanotubes (X) having a predetermined outer diameter and fiber length. The outer diameter and fiber length of the bundled carbon nanotubes in the dispersion can be determined by observing a sample obtained by drying the dispersion, which has been diluted as necessary so that the individual carbon nanotubes do not overlap and their sizes can be easily distinguished, using a scanning electron microscope (SEM) and performing image analysis. In addition, if the carbon nanotubes aggregate due to dilution of the carbon nanotube dispersion, additives such as a dispersant or a water-soluble solvent may be added at 0.01 to 2% by mass relative to the solid content of the carbon nanotubes, and after uniformly mixing using ultrasonic waves, the mixture may be diluted to 1000 times. In addition, a sample for SEM observation obtained by drying the dispersion can be specifically prepared by applying the above-mentioned diluted carbon nanotube dispersion onto a mica substrate, drying the solvent in an oven, and then sputtering the substrate surface on the coated side with platinum.
[0021] Specifically, in order to observe carbon nanotubes more appropriately using a scanning electron microscope, the outer diameter (minor diameter), fiber length (major diameter), and area of each particle of carbon nanotubes imaged at a magnification of 10,000 or 20,000 are measured using image analysis software (WINROOF2015: manufactured by Mitani Shoji Co., Ltd.) Note that the shape of a bundled carbon nanotube is indefinite, and in this specification, since the outer diameter value has a range within one carbon nanotube, the value obtained by dividing the area value by the fiber length (major diameter) is used as the outer diameter. Next, 1000 carbon nanotube particles having an outer diameter of 10 nm or more obtained as described above are randomly selected, and among the 1000 carbon nanotube particles, particles having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm are identified, the number A of particles is counted, and the percentage (%) of the number of bundled carbon nanotubes (X) is calculated using the following formula. (Formula) The percentage of bundled carbon nanotubes (X) (%) = A / 1000 x 100
[0022] The proportion of the number of bundled carbon nanotubes (X) is preferably 0.5% or more. Also, it is preferably 20% or less, more preferably 10% or less, and further preferably 5% or less. For example, this proportion may be 0.5% to 20%. Particularly from the viewpoint of cycle characteristics and the rate of change in film thickness, the range is preferably 0.5% to 20%.
[0023] In this specification, the average outer diameter and average fiber length of particles having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm specified as above are referred to as the average outer diameter and average fiber length, respectively. The ratio of the average outer diameter and average fiber length is referred to as the average aspect ratio. In the dispersion of the present disclosure, the bundled carbon nanotubes have an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm, and the average outer diameter is preferably 50 nm to 1 μm, and more preferably 50 nm to 500 nm. The average fiber length is preferably 1 μm to 50 μm, more preferably 1 μm to 10 μm, and the average aspect ratio is preferably 5 to 200, more preferably 10 to 150.
[0024] The carbon nanotube dispersion of the present disclosure may further contain bundled carbon nanotubes (Y) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 1 μm to 5 μm. Such bundled carbon nanotubes (Y) mainly play a role in forming a network of conductive paths, improving cycle characteristics. Based on the number of carbon nanotubes having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion, the proportion of the number of the bundled carbon nanotubes (Y) is preferably 10% to 60% from the viewpoint of improving cycle characteristics. The method of calculating the number ratio will be described below. The outer diameter (minor diameter), fiber length (major diameter), and area of each particle of carbon nanotube, which is imaged with a scanning electron microscope at a magnification of 5,000 times in accordance with the fiber length of the carbon nanotube, are measured using image analysis software (WINROOF2015: manufactured by Mitani Shoji Co., Ltd.). Note that the shape of the bundled carbon nanotube is indefinite, and in this specification, since the outer diameter value has a width within one carbon nanotube, the value obtained by dividing the area value by the fiber length (major diameter) is used as the outer diameter. Next, 1000 carbon nanotube particles having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more obtained as described above are randomly selected, and among the 1000 carbon nanotube particles, particles having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 1 μm to 5 μm are identified, the number B of particles is counted, and the percentage (%) of the number of bundled carbon nanotubes (Y) is calculated using the following formula. (Formula) The ratio (%) of the number of bundled carbon nanotubes (Y) = B / 1000 x 100
[0025] From the viewpoint of cycle characteristics, the proportion of the number of bundled carbon nanotubes (Y) is preferably 10% or more, more preferably 20% or more, and is preferably 60% or less, more preferably 35% or less.
[0026] The carbon nanotube dispersion of the present disclosure may further contain bundled carbon nanotubes (Z) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 0.2 μm or more and less than 1 μm. It is presumed that such bundled carbon nanotubes (Z) not only reduce the volume resistivity but also contribute to improving cycle characteristics by penetrating into the vicinity of the surface of the active material or the like described later or into the gaps of the conductive network. Based on the number of carbon nanotubes having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion, the proportion of the number of the bundled carbon nanotubes (Z) is preferably 50% to 80% from the viewpoint of improving cycle characteristics. The method of calculating the number ratio will be described below. The outer diameter (minor diameter), fiber length (major diameter), and area of each particle of carbon nanotube, which is imaged with a scanning electron microscope at a magnification of 5,000 times in accordance with the fiber length of the carbon nanotube, are measured using image analysis software (WINROOF2015: manufactured by Mitani Shoji Co., Ltd.). Note that the shape of the bundled carbon nanotube is indefinite, and in this specification, since the outer diameter value has a width within one carbon nanotube, the value obtained by dividing the area value by the fiber length (major diameter) is used as the outer diameter. Next, the carbon nanotube particles having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more obtained as described above are observed, and 1,000 particles are randomly selected. Among the 1,000 carbon nanotube particles, particles having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 0.2 μm or more and less than 1 μm are identified, the number C of these particles is counted, and the percentage (%) of the number of bundled carbon nanotubes (Z) is calculated using the following formula. (Formula) The percentage of bundled carbon nanotubes (Z) (%) = C / 1000 x 100
[0027] The proportion of the number of bundled carbon nanotubes (Z) is preferably 30% or more, more preferably 50% or more, from the viewpoint of volume resistivity, and is preferably 90% or less, more preferably 70% or less.
[0028] The dispersion of the present disclosure contains bundled carbon nanotubes (X), (Y), and (Z) having different outer diameters and fiber lengths in an optimal balance, thereby improving cycle characteristics and film thickness retention. From the viewpoint of cycle characteristics and film thickness retention, the ratio of the number of bundled carbon nanotubes (Y) to the number of bundled carbon nanotubes (Z) (the ratio of the number of (Y) / the ratio of the number of (Z)) is preferably 0.1 or more, more preferably 0.3 or more. It is also preferably 1.3 or less, more preferably 1.0 or less, and even more preferably 0.6 or less. For example, this ratio may be 0.3 to 0.6.
[0029] A dispersion liquid containing such bundled carbon nanotubes can be obtained, for example, by promoting the interaction between carbon nanotubes and then dispersing them in a solvent (also called a dispersion solvent). In order to promote the interaction between carbon nanotubes, it is preferable to apply shear (force) or impact (force) to the carbon nanotubes and to perform wet mixing using a solvent (also called a processing solvent), but this is not limited thereto. An example of such a method is to disperse treated carbon nanotubes obtained by wet mixing and then calcining the treated carbon nanotubes in the presence of a dispersion solvent, in which shear or impact force is applied using an optimal device in the presence of an optimal treatment solvent so as to cause selective aggregation between carbon nanotubes having an average diameter of 3 nm to 30 nm. By dispersing the treated carbon nanotubes obtained as described above, a dispersion liquid containing a predetermined amount of bundled carbon nanotubes (X) having a predetermined shape as specified in the present disclosure can be obtained.
[0030] [Raw carbon nanotubes] The raw carbon nanotubes used to form the bundled carbon nanotubes refer to carbon nanotubes that are structural units that constitute the bundled carbon nanotubes (bundles), and it is important that the raw carbon nanotubes have an average diameter of 3 nm to 30 nm. Carbon nanotubes with such an average diameter are not only inexpensive and easy to obtain, but also, by using carbon nanotubes with such an average diameter, bundled carbon nanotubes that are long and have excellent flexibility can be obtained, and excellent cycle characteristics can be exhibited. The diameter of the raw carbon nanotubes can be measured, for example, at a magnification of 5 million times using a transmission electron microscope (TEM). The average diameter of the raw carbon nanotubes is the average value obtained by measuring the diameter at any 10 points in the carbon nanotube fiber. The average diameter of the raw carbon nanotubes is preferably 5 nm to 20 nm.
[0031] A carbon nanotube has a cylindrical shape of planar graphite, and a multi-walled carbon nanotube has a structure in which two or more layers of graphite are wound. The sidewall of the carbon nanotube does not have to have a graphite structure. For example, a carbon nanotube having a sidewall with an amorphous structure can be used as the carbon nanotube. These carbon nanotubes may also be a mixture of carbon nanotubes having multiple layers. The raw carbon nanotubes used in the present disclosure are not particularly limited as long as they have an average diameter of 3 nm to 30 nm, but the number of walls is preferably 2 or more, more preferably 3 or more, and preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0032] The shape of the raw carbon nanotubes is not limited, and various shapes including needle-like, cylindrical tube-like, fishbone-like (fishbone or cup stacked type), and coil-like can be used. In addition, the raw carbon nanotubes may be plate-like or platelet-like secondary aggregates obtained by dry processing of cylindrical tube-like carbon nanotubes. The shape of the raw carbon nanotubes used in the present disclosure is preferably needle-like or cylindrical tube-like. The carbon nanotubes may be a single shape or a combination of two or more shapes.
[0033] Examples of the form of the raw carbon nanotubes include, but are not limited to, graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers. The carbon nanotubes may have a single form or a combination of two or more of these forms.
[0034] The BET specific surface area of the raw carbon nanotubes is 10 to 1500 m 2 / g is preferable, and 150 to 800m 2 / g is more preferable, and 200 to 700m 2 It is more preferred that the molecular weight is / g.
[0035] The volume resistivity of the raw carbon nanotubes is 1.0×10 -2 It is preferable that the resistance is 5.0×10 -3 More preferably, it is 3.0×10 -3 It is more preferable that the volume resistivity is Ω·cm or less. The volume resistivity of the carbon nanotubes can be measured using a powder resistivity measuring device (Loresta GP-powder resistivity measuring system MCP-PD-51, manufactured by Nitto Seiko Analytech Co., Ltd.).
[0036] The carbon purity of the raw carbon nanotubes is expressed as the content (%) of carbon atoms in the carbon nanotubes. The carbon purity is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more, relative to 100% by mass of the carbon nanotubes. The amount of metal contained in the raw carbon nanotube is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of the carbon nanotube. Metals contained in the carbon nanotube include metals and metal oxides used as catalysts when synthesizing carbon nanotubes. Specific examples include metals such as cobalt, nickel, aluminum, magnesium, silica, manganese, and molybdenum, metal oxides, and composite oxides thereof.
[0037] Raw carbon nanotubes are usually present as secondary particles. The shape of these secondary particles may be, for example, a state in which carbon nanotubes, which are general primary particles, are intricately entangled, or may be an aggregate of linear carbon nanotubes. Secondary particles that are an aggregate of linear carbon nanotubes are easier to disentangle than entangled ones. Furthermore, linear ones have better dispersibility than entangled ones, so they can be suitably used as carbon nanotubes.
[0038] The raw carbon nanotubes may be surface-treated carbon nanotubes, or may be carbon nanotube derivatives to which a functional group such as a carboxyl group has been added, or may be carbon nanotubes encapsulating a substance such as an organic compound, a metal atom, or a fullerene.
[0039] The raw carbon nanotubes may be carbon nanotubes produced by any method. Carbon nanotubes can generally be produced by, but are not limited to, laser ablation, arc discharge, thermal CVD, plasma CVD, and combustion methods. For example, carbon nanotubes can be produced by contacting a carbon source with a catalyst at 500 to 1000°C in an atmosphere with an oxygen concentration of 1% by volume or less. The carbon source may be at least one of a hydrocarbon and an alcohol.
[0040] The raw material gas that is the carbon source of the raw carbon nanotubes can be any conventionally known gas. For example, the raw material gas containing carbon can be, but is not limited to, hydrocarbons such as methane, ethylene, propane, butane, and acetylene, carbon monoxide, and alcohol. In particular, from the viewpoint of ease of use, it is desirable to use at least one of the hydrocarbons and the alcohol as the raw material gas.
[0041] [Processing solvent] As a treatment solvent for wet-mixing carbon nanotubes having an average diameter of 3 nm to 30 nm, a highly polar alcohol-based solvent or water is preferred. Treatment with a highly polar alcohol-based solvent or water increases the difference in polarity with the hydrophobic surface of the carbon nanotubes, which is advantageous for the carbon nanotubes to aggregate and form bundles. High polarity refers to a Hansen solubility parameter (SP value) at 25°C of 10 or more. The Hansen solubility parameter (SP value) at 25°C can be calculated using the Hansen Solubility Parameters in Practice (HSPiP) Ver.5.1.05, developed by Dr. Hansen, Prof. Abbott, and Dr. Yamamoto.
[0042] Examples of the alcohol-based solvent with high polarity include ethanol, propyl alcohol, and butyl alcohol, but are not limited to these examples, and any solvent that can be mixed with carbon nanotubes in an optimal state may be used. The SP values of monohydric aliphatic alcohols are shown below. Methanol (SP value: 14.4, the same applies below), ethanol (13.0), 2-propanol (isopropyl alcohol, IPA) (11.5), 1-butanol (11.3), 2-butanol (10.8), 2-methyl-1-propanol (11.1), 2-methyl-2-propanol (10.6), 1-pentanol (10.7), 2-pentanol (10.5), isopentanol (10.4), and t-pentanol (10.3).
[0043] [Wet mixing] Examples of equipment used for wet mixing include mixers such as a Disper, Homomixer, or Planetary Mixer; homogenizers such as M-Technique's "Clearmix" or PRIMIX's "Filmix"; sand mills such as Red Devil's paint conditioner, ball mill, and Shinmaru Enterprises' "Dynomill"; media-type dispersers such as an Attritor or Coball Mill; wet jet mills such as Genus' "Genus PY," Sugino Machine's "Starburst," and Nanomizer's "Nanomizer," media-less dispersers such as M-Technique's "Clear SS-5" or Nara Machinery's "Micros," and other roll mills and kneaders, but are not limited to these. In addition, it may be preferable to use a wet mixing device that has been treated to prevent metal from being mixed in from the device. For example, when using a media-type dispersing machine, it is preferable to use a method in which a dispersing machine with an agitator and a vessel made of ceramic or resin is used, or a dispersing machine in which the surface of a metal agitator and a vessel is treated with tungsten carbide spraying or resin coating, etc. is used. As the media, it is preferable to use ceramic beads such as glass beads, zirconia beads, or alumina beads. Also, when using a roll mill, it is preferable to use a ceramic roll. Only one type of dispersing device may be used, or multiple types of devices may be used in combination.
[0044] [Boron source] When carbon nanotubes are wet-mixed using a treatment solvent, a boron source may be included. It is presumed that wet-treatment in the presence of a boron source and a treatment solvent allows the boron source and carbon nanotubes to be uniformly mixed, and that a baking process promotes the formation of a bundle-like structure in which multiple carbon nanotubes are connected. The treated carbon nanotubes thus obtained maintain their bundle shape even after dispersion, and a carbon nanotube dispersion that exhibits excellent cycle characteristics can be obtained. When a boron source is used, it is preferable to dissolve the boron source in a treatment solvent and then treat the raw carbon nanotubes with the boron source, which allows the boron source and the carbon nanotubes to be mixed more uniformly, thereby achieving excellent cycle characteristics.
[0045] The boron source is not particularly limited, and examples thereof include boron carbide, boron oxide, boron nitride, metal borides, boron oxoacids, boranes, and boron-containing organic compounds. Specifically, in the case of boron carbide, B4C(B 12 C3), B 12Examples of boron oxyacids include orthoboric acid, metaboric acid, tetraboric acid, and the like; boranes include monoborane, diborane, decaborane, and the like; boron-containing organic compounds include boric acid esters such as trimethyl borate and triethyl borate, substituted boranes such as triethylborane and triphenylborane, and boronic acids such as phenylboronic acid and phenylboronic acid esters. From the viewpoint of forming a bundle shape, it is preferable that the boron source has high solubility in the treatment solvent, and it is more preferable to use boric acid. The raw carbon nanotubes are wet-treated in the presence of the treatment solvent or the treatment solvent and the boron source, and then heat-treated (calcined) to obtain treated carbon nanotubes.
[0046] When a boron source is used, the mass ratio between the raw carbon nanotubes and the boron source is not particularly limited, but the ratio of the boron source to 100 parts by mass of the raw carbon nanotubes is preferably 0.01 to 300 parts by mass, more preferably 0.05 to 100 parts by mass, and even more preferably 0.1 to 50 parts by mass.
[0047] Furthermore, if the raw materials are not uniformly dissolved or dispersed, a dispersant may be added as necessary to improve the wettability and dispersibility of each raw material in the solvent, thereby dispersing and mixing the raw materials.
[0048] The temperature conditions for heat-treating the mixture of the raw carbon nanotubes and the boron source vary depending on the types and amounts of the raw carbon nanotubes and the boron source, and are not particularly limited, but are preferably 1000 to 3000° C., more preferably 1100 to 2500° C., and further preferably 1200 to 2000° C. In addition, the heating time is not particularly limited, but is preferably 10 minutes to 72 hours, and more preferably 30 minutes to 10 hours. The atmosphere in the heat treatment step is preferably an inert gas atmosphere such as nitrogen or argon, or a vacuum atmosphere, in order to prevent side reactions such as oxidation of the raw materials. The heat treatment step may be not only a treatment step performed in one stage at a constant atmosphere, temperature and time, but also a treatment step performed in multiple stages with different atmospheres, temperatures and times.
[0049] <Solvent> Next, the solvent used in the carbon nanotube dispersion liquid of the present disclosure will be described. The solvent is not particularly limited as long as it is a solvent in which carbon nanotubes can be dispersed, but is preferably water or a mixed solvent consisting of one or more organic solvents, and more preferably water or a solvent consisting of one or more water-soluble organic solvents, or a mixed solvent consisting of two or more water-soluble organic solvents. In addition, when a dispersant described later is used, it is preferable that the solvent is capable of partially or completely dissolving the dispersant, and although the solvent is not particularly limited, it is preferable that the solvent contains water or a water-soluble organic solvent.
[0050] Examples of organic solvents that can be used include alcohols (e.g., methanol), polyhydric alcohols (e.g., ethylene glycol), polyhydric alcohol ethers (e.g., ethylene glycol monomethyl ether), amines (e.g., ethanolamine), amides (e.g., N-methyl-2-pyrrolidone (NMP)), heterocyclic compounds (e.g., γ-butyrolactone), sulfoxides (e.g., dimethyl sulfoxide), sulfones (e.g., sulfolane), aromatic compounds (e.g., toluene, xylene), hydrocarbons (e.g., hexane), lower ketones (e.g., acetone), and esters (e.g., ethyl acetate).
[0051] Preferred water-soluble organic solvents include amides (N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone (NEP), N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N-methylcaprolactam, etc.), heterocyclics (cyclohexylpyrrolidone, 2-oxazolidone, 1,3-dimethyl-2-imidazolidinone, γ-butyrolactone, etc.), sulfoxides (dimethyl sulfoxide, etc.), sulfones (hexamethylphosphorotriamide, sulfolane, etc.), alcohols (methanol, ethanol, etc.), polyhydric alcohols (ethylene glycol, diethylene glycol, etc.), lower ketones (acetone, methyl ethyl ketone, etc.), and others, such as tetrahydrofuran, urea, and acetonitrile.
[0052] <Dispersant> The carbon nanotube dispersion of the present disclosure may further contain a dispersant. The dispersant plays a role of breaking up the aggregates of carbon nanotubes and improving the stability of the dispersion. The dispersant is not particularly limited as long as it can disperse and stabilize the carbon nanotubes, and for example, a surfactant or a resin-type dispersant can be used. The surfactants are mainly classified into anionic, cationic, nonionic, and amphoteric. Depending on the characteristics required for dispersing the carbon nanotubes, a suitable type of dispersant can be used in a suitable amount.
[0053] Examples of anionic surfactants include, but are not limited to, fatty acid salts, polysulfonates, polycarboxylates, alkyl sulfates, alkylarylsulfonates, alkylnaphthalenesulfonates, dialkylsulfonates, dialkylsulfosuccinates, alkyl phosphates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkylaryl ether sulfates, naphthalenesulfonic acid formalin condensates, polyoxyethylene alkyl phosphate sulfonates, glycerol borate fatty acid esters, and polyoxyethylene glycerol fatty acid esters.Furthermore, specific examples include sodium dodecylbenzenesulfonate, sodium lauric acid sulfate, sodium polyoxyethylene lauryl ether sulfate, polyoxyethylene nonylphenyl ether sulfate, and the sodium salt of β-naphthalenesulfonic acid formalin condensates.
[0054] Examples of cationic surfactants include alkylamine salts and quaternary ammonium salts, specifically stearylamine acetate, trimethyl coconut ammonium chloride, trimethyl beef tallow ammonium chloride, dimethyldioleyl ammonium chloride, methyl oleyl diethanol chloride, tetramethyl ammonium chloride, lauryl pyridinium chloride, lauryl pyridinium bromide, lauryl pyridinium disulfate, cetyl pyridinium bromide, 4-alkyl mercaptopyridine, poly(vinylpyridine)-dodecyl bromide, and dodecylbenzyl triethyl ammonium chloride.
[0055] Examples of nonionic surfactants include, but are not limited to, polyoxyethylene alkyl ethers, polyoxyalkylene derivatives, polyoxyethylene phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and alkyl allyl ethers.Specific examples include polyoxyethylene lauryl ethers, sorbitan fatty acid esters, and polyoxyethylene octylphenyl ethers. Examples of amphoteric surfactants include aminocarboxylates.
[0056] The surfactant may be used alone or in combination of two or more kinds. For example, a combination of an anionic surfactant and a nonionic surfactant, or a combination of a cationic surfactant and a nonionic surfactant may be used. In this case, it is preferable to use an appropriate amount for each surfactant component. A combination of an anionic surfactant and a nonionic surfactant is preferable. The anionic surfactant is preferably a polycarboxylate. The nonionic surfactant is preferably polyoxyethylene phenyl ether.
[0057] Examples of resin-type dispersants include cellulose derivatives (cellulose acetate, cellulose acetate butyrate, cellulose butyrate, cyanoethyl cellulose, ethylhydroxyethyl cellulose, nitrocellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, etc.), polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, polyacrylonitrile polymers, polyacrylic acid, and various rubbers. Particularly preferred are methyl cellulose, ethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinylpyrrolidone, polyacrylonitrile polymers, polyacrylic acid, and various rubbers (for example, partially hydrogenated nitrile rubber).
[0058] In particular, the resin-type dispersant is more preferably made of a polymer containing one or more structural units selected from the group consisting of a nitrile group-containing structural unit, a carboxy group-containing structural unit, a hydroxy group-containing structural unit, and a heterocyclic ring-containing structural unit, which enhances the adsorption to boron-containing carbon nanotubes and the affinity to the medium. The polymer preferably contains an alkylene structure in the main chain, and has a structure of any one of a nitrile group, a carboxy group, a hydroxy group, and a heterocyclic ring, which has strong polarization, which enhances the adsorption to carbon nanotubes and the affinity to the medium, and allows the carbon nanotubes to be present stably in the medium. In addition, the polymer is more preferably made of two or more structural units selected from the group consisting of a nitrile group-containing structural unit, a carboxy group-containing structural unit, a hydroxy group-containing structural unit, and a heterocyclic ring-containing structural unit, which enhances the adsorption to carbon nanotubes and the affinity to the medium.
[0059] The nitrile group-containing structural unit is a structural unit containing a nitrile group, and preferably contains a structural unit containing an alkylene structure substituted with a substituent containing a nitrile group. The alkylene structure is preferably a linear or branched alkylene structure. The number of nitrile groups contained in the nitrile group-containing structural unit is preferably one or two, more preferably one. The method of introducing the nitrile group-containing structural unit into a polymer is not particularly limited, but for example, a method of preparing a polymer by polymerization reaction of a monomer containing a nitrile group can be preferably used.
[0060] Examples of monomers containing a nitrile group include acrylonitrile, methacrylonitrile, and fumaronitrile, and one type can be used alone or two or more types can be used in combination. In particular, from the viewpoint of increasing the intermolecular force between polymers and / or between a polymer and a dispersed substance (adsorbed substance), availability of raw materials, and reactivity, it is preferable that the monomer containing a nitrile group is acrylonitrile. The content of the nitrile group-containing structural unit is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the mass of the polymer (i.e., when the mass of the polymer is 100% by mass). In addition, it is preferably 100% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. It is believed that by setting the content of the nitrile group-containing structural unit within the above range, it is possible to control the adsorption to the dispersed substance and the affinity to the dispersion medium, and the dispersed substance can be stably present in the dispersion medium. In addition, the affinity of the polymer for the electrolyte can be controlled, which is believed to prevent problems such as the polymer dissolving in the electrolyte inside the battery and increasing the resistance of the electrolyte.
[0061] The carboxyl group-containing structural unit is a structural unit containing a carboxyl group, and preferably contains a structural unit containing an alkylene structure substituted with a substituent containing a carboxyl group. The alkylene structure is preferably a linear or branched alkylene structure. The number of carboxyl groups contained in the carboxyl group-containing structural unit is preferably one or two, more preferably one. The method of introducing the carboxyl group-containing structural unit into the polymer is not particularly limited, but examples thereof include a method of preparing a polymer by polymerization reaction of a monomer containing a carboxyl group, or a method of preparing a polymer by polymerization reaction of a monomer containing a functional group other than a carboxyl group, and modifying the polymer into a carboxyl group.
[0062] Examples of monomers containing a carboxy group include unsaturated fatty acids such as (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, and citraconic acid, 2-(meth)acryloyloxyethyl phthalate, and 2-(meth)acryloyloxypropyl phthalate. A carboxy group-containing monomer may be obtained by hydrolyzing the carbamoyl group of a polymer obtained by polymerization of a monomer containing a carbamoyl group such as (meth)acrylamide. The carboxy group-containing monomer is preferably an unsaturated fatty acid, more preferably (meth)acrylic acid, and even more preferably acrylic acid.
[0063] The content of the carboxyl group-containing structural unit is preferably 60% by mass or more, more preferably 80% by mass or more, and preferably 98% by mass or less, and may be 100% by mass, based on the mass of the polymer (i.e., when the mass of the polymer is 100% by mass), from the viewpoint of having a suitable affinity with the solvent. In addition, if one or more selected from the group of nitrile group-containing structural units, hydroxyl group-containing structural units, and heterocyclic ring-containing structural units are further contained, the affinity between the carbon nanotube and the medium is increased, which is more preferable. When one or more selected from the group of nitrile group-containing structural units, hydroxyl group-containing structural units, and heterocyclic ring-containing structural units are further contained, the content of the carboxyl group-containing structural unit is preferably 3% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, based on the mass of the polymer (i.e., when the mass of the polymer is 100% by mass). In addition, from the viewpoint of electrolyte resistance, it is preferably 50% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.
[0064] The hydroxyl group-containing structural unit is a structural unit containing a hydroxyl group, and preferably contains a structural unit containing an alkylene structure substituted with a substituent containing a hydroxyl group. The alkylene structure is preferably a linear or branched alkylene structure. The number of hydroxyl groups contained in the hydroxyl group-containing structural unit is preferably one or two, more preferably one. The method of introducing the hydroxyl group-containing structural unit into the polymer is not particularly limited, but examples thereof include a method of preparing a polymer by polymerization reaction of a monomer containing a hydroxyl group, or a method of preparing a polymer by polymerization reaction of a monomer containing a functional group other than a hydroxyl group, and modifying the polymer into a hydroxyl group.
[0065] Examples of monomers containing a hydroxy group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 2-hydroxy-3-phenoxypropyl acrylate, and caprolactone adducts of these monomers (the number of moles added is 1 to 5), etc. The monomer containing a hydroxy group is preferably a hydroxyalkyl (meth)acrylate, more preferably 2-hydroxyethyl (meth)acrylate, and even more preferably 2-hydroxyethyl acrylate.
[0066] As a method for preparing a polymer by polymerization reaction of a monomer containing a functional group other than a hydroxyl group and modifying it to a hydroxyl group, for example, there is a method in which the acetyl group of polyvinyl acetate obtained by polymerization of vinyl acetate is saponified with an alkali such as sodium hydroxide to convert it to a hydroxyl group (saponification reaction). The saponification reaction rate (degree of saponification) can be controlled as desired by changing the concentration of sodium hydroxide and the treatment time.
[0067] In addition, for the purpose of increasing the affinity between the carbon nanotube and the medium, the hydroxyl group in the polymer may be reacted with an aldehyde compound to be modified into an acetal group (acetalization). The aldehyde compound used in the acetalization reaction may be, for example, a linear, branched, cyclic saturated, unsaturated, or aromatic aldehyde compound having 1 to 15 carbon atoms, but is not limited thereto. Specific examples include formaldehyde, acetaldehyde, propionyl aldehyde, n-butyl aldehyde, isobutyl aldehyde, tert-butyl aldehyde, and benzaldehyde. These aldehyde compounds may be used alone or in combination of two or more kinds. From the viewpoint of versatility, a linear, branched, cyclic saturated, unsaturated, or aromatic aldehyde compound having 1 to 10 carbon atoms is preferred, and a linear aldehyde compound having 1 to 4 carbon atoms is more preferred. By changing the aldehyde compound and the treatment time, the reaction rate of acetalization (degree of acetalization) can be controlled as desired.
[0068] The content of the hydroxyl group-containing structural unit is preferably 80% by mass or more, more preferably 85% by mass or more, and more preferably 99.8% by mass or less, based on the mass of the polymer (i.e., when the mass of the polymer is 100% by mass). However, when one or more selected from the group consisting of a nitrile group-containing structural unit, a hydroxyl group-containing structural unit, and a heterocyclic ring-containing structural unit are further contained, the content is preferably 5% by mass or more, more preferably 95% by mass or less, and more preferably 85% by mass or less. By setting it in the above range, it is possible to strengthen the polarization and increase the affinity to the carbon nanotube and the medium. It is also preferable from the viewpoint of electrolyte resistance. For the same reason as the content of the hydroxyl group-containing structural unit, the content of the acetal group is preferably set within the preferred range of the content of the hydroxyl group-containing structural unit.
[0069] The heterocycle-containing structural unit is a structural unit containing a heterocycle, and more preferably a structural unit containing an alkylene structure substituted with a substituent containing a heterocycle. The alkylene structure is preferably a linear or branched alkylene structure. The heterocycle contained in the heterocycle-containing structural unit may be a monocyclic structure or a condensed ring structure, but is preferably a monocyclic structure. The number of heterocycles contained in the heterocycle-containing structural unit is preferably one or two, more preferably one. The heterocycle contains an atom other than carbon in the ring-constituting atom, for example, one or more nitrogen, oxygen, sulfur atoms, etc. As the atom other than carbon constituting the ring, nitrogen or oxygen is preferable, and nitrogen is more preferable. When the atom constituting the ring contains an atom other than carbon, polarization occurs in the heterocycle, and it becomes possible to strongly act on the carbon nanotube. The method of introducing the heterocycle into the polymer is not particularly limited, but for example, a method of preparing a polymer by polymerization reaction of a monomer containing a heterocycle can be used.
[0070] As the monomer containing a heterocycle, an N-vinyl cyclic amide structural unit is preferred, and examples thereof include N-vinyl-2-pyrrolidone, N-vinyl-ε-caprolactam, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, and N-vinyl-3,5-morpholinedione. In particular, N-vinyl-2-pyrrolidone is preferred from the viewpoint of improving battery characteristics. These may be used alone or in combination of two or more kinds.
[0071] The content of the heterocycle-containing structural unit is, based on the mass of the polymer (i.e., when the mass of the polymer is 100 mass%), preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and may be 100 mass%, from the viewpoint of enhancing the effect on the carbon nanotubes.
[0072] The polymer may further contain, as other structural units, one or more structural units selected from the group consisting of active hydrogen group-containing structural units (excluding carboxyl groups and hydroxyl groups), basic group-containing structural units, and ester group-containing structural units. The conductive material dispersion of the present disclosure can be applied to various applications by selecting and containing the above structural units according to the properties such as hydrophilicity, hydrophobicity, acidity, and basicity of the substrate to which the conductive material dispersion of the present disclosure is applied or the material to be mixed.
[0073] The active hydrogen group-containing structural unit is a structural unit having, for example, a primary amino group, a secondary amino group, a mercapto group, etc. as an active hydrogen group. Here, the "primary amino group" means -NH2 (amino group), and the "secondary amino group" means a group in which one hydrogen atom on the primary amino group is replaced with an organic residue such as an alkyl group. However, the primary amino group and the secondary amino group in the acid amide are not included in the active hydrogen group in this specification.
[0074] The basic group-containing structural unit is a structural unit having a basic group. Examples of the basic group include tertiary amino group, amide group, etc. Note that the structural unit having a primary amino group and the structural unit having a secondary amino group can also be included in the basic group-containing structural unit, but in the present disclosure, they are treated as the active hydrogen group-containing structural unit and are not included in the basic group-containing structural unit.
[0075] The ester group-containing structural unit is a structural unit having a structure represented by (R1)2C=CH-CO-O-R2 (wherein R1 is a hydrogen atom or a methyl group, at least one of which is a hydrogen atom, and R2 is an alkyl group which may have a substituent). In addition, those containing the active hydrogen group or the basic group as a substituent of an alkyl group are treated as the active hydrogen group-containing structural unit or the basic group-containing structural unit, and are not included in the ester group-containing structural unit.
[0076] When a polymer is used as a dispersant in the carbon nanotube dispersion, the polymer content is preferably determined according to the specific surface area and wettability of the carbon nanotubes, and is preferably 2% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and is preferably 250% by mass or less, more preferably 150% by mass or less, and even more preferably 100% by mass or less, assuming the mass of the treated carbon nanotubes to be 100% by mass.
[0077] The dispersant preferably contains at least a polymer. The dispersant may further contain any polymer, any copolymer, etc. The polymer content in the dispersant is preferably 50% by mass or more, more preferably 80% by mass or more, and more preferably 90% by mass or more. The polymer content in the dispersant may be 100% by mass, in which case the dispersant consists of only the polymer.
[0078] The pH of the carbon nanotube dispersion liquid of the present disclosure can usually be in the range of 4 to 12. It is preferably in the range of 4 to 6. It is believed that adjusting the pH to within the above range can improve the wettability of the carbon nanotubes and further enhance the action as a dispersant for the polymer. If the pH is outside the above range, the dispersibility of the carbon nanotubes may decrease or the binder may gel. In addition, when used for battery applications, problems such as corrosion of various raw materials and exterior materials in the battery may easily occur. The pH of the carbon nanotube dispersion liquid can be measured using a general pH meter when it contains water as a solvent. On the other hand, when it does not substantially contain water as a solvent, for example, when only NMP is selected as the solvent, the carbon nanotube dispersion liquid is prepared by adding water to the carbon nanotube dispersion liquid so that the solid concentration after adding water is 50% when the solid concentration before adding water is 100%, and the pH value is measured using a general pH meter, and can be measured, for example, by the following method. While stirring the carbon nanotube dispersion with a solids concentration of 5% using a disperser, add water so that the solids concentration of the carbon nanotube dispersion becomes 2.5%. After stirring uniformly, the pH of the carbon nanotube dispersion can be measured at 25℃ using a benchtop pH meter (Seven Compact S220 Expert Pro, manufactured by Mettler Toledo). In the present disclosure, "substantially free of water" means that water is not intentionally added. The water content is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, based on the mass of the solvent.
[0079] The pH of the carbon nanotube dispersion is not particularly limited, but can be adjusted by (1) the amount of metal hydroxide contained in the carbon nanotubes, (2) the type and amount of functional groups on the carbon nanotube surface, and (3) the type and amount of base added. By adjusting the pH by combining the above factors (1) to (3), it is possible to obtain a carbon nanotube dispersion that not only improves the wettability of carbon nanotubes but also has excellent dispersibility and stability.
[0080] As described above, metals, metal oxides, and metal hydroxides used as catalysts in the manufacturing process remain in the carbon nanotubes. The pH can be adjusted by appropriately adjusting the amount of metals remaining in the carbon nanotubes, particularly the content of the metal hydroxides (1) above. The amount of remaining metals and carbon purity of carbon nanotubes, as well as the pH of the carbon nanotube dispersion containing them, can be adjusted by a conventionally known purification method.
[0081] The functional group on the carbon nanotube surface in (2) above is not particularly limited, but may be a carboxy group, a sulfo group, or a hydroxyl group. The method of introducing the functional group into the carbon nanotube is not particularly limited. For example, in order to introduce a carboxy group into the carbon nanotube, it is sufficient to heat the carbon nanotube together with an acid having an oxidizing effect. This operation is relatively easy, and is preferable because it can add a highly reactive carboxy group. Examples of the acid having an oxidizing effect include concentrated nitric acid, hydrogen peroxide, a mixture of sulfuric acid and nitric acid, and aqua regia. In particular, when concentrated nitric acid is used, the concentration is preferably 5% by mass or more, and more preferably 60% by mass or more. Heating may be performed by a conventional method, and the temperature is preferably below the boiling point of the acid used. For example, the range of 50 to 130°C is preferable for concentrated nitric acid. In addition, the heating time is preferably in the range of 30 minutes to 20 hours, and more preferably in the range of 1 hour to 8 hours. It is preferable that the carbon nanotube does not have an acidic functional group such as a carboxy group or a sulfo group. If the carbon nanotube contains a large number of acidic functional groups, the carbon nanotube dispersion liquid may gel during storage.
[0082] The base added for adjusting the pH in (3) above is not particularly limited, and specifically, at least one base selected from the group consisting of inorganic bases, inorganic metal salts, organic hydroxides, and other organic bases can be used.
[0083] Examples of inorganic bases and inorganic metal salts include chlorides, hydroxides, carbonates, nitrates, sulfates, phosphates, tungstates, vanadates, molybdates, niobates, or borates of alkali metals or alkaline earth metals; and ammonium hydroxide. Among these, chlorides, hydroxides, carbonates, and alkoxides of alkali metals and alkaline earth metals are preferred from the viewpoint of easily supplying cations. Examples of hydroxides of alkali metals include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of hydroxides of alkaline earth metals include calcium hydroxide and magnesium hydroxide. Examples of carbonates of alkali metals include lithium carbonate, lithium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and potassium hydrogen carbonate. Examples of the alkoxide of an alkali metal include lithium methoxide, lithium ethoxide, lithium n-butoxide, lithium t-butoxide, potassium methoxide, potassium ethoxide, potassium n-butoxide, potassium t-butoxide, sodium methoxide, sodium ethoxide, sodium n-butoxide, and sodium t-butoxide. The number of carbon atoms of the alkoxide may be 5 or more. Examples of the alkoxide of an alkaline earth metal include magnesium methoxide, magnesium ethoxide, magnesium n-butoxide, and magnesium t-butoxide. The number of carbon atoms of the alkoxide may be 5 or more. Among these, lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, lithium t-butoxide, potassium t-butoxide, and sodium t-butoxide are more preferable. Note that the metal contained in the inorganic base of the present disclosure may be a transition metal.
[0084] The organic hydroxide is a salt containing an organic cation and a hydroxide ion. Examples of the organic hydroxide include trimethyl-2-hydroxyethyl ammonium hydroxide, tetramethyl ammonium hydroxide, cetyl trimethyl ammonium hydroxide, hexadecyl trimethyl ammonium hydroxide, trimethyl phenyl ammonium hydroxide, 3-trifluoromethyl-phenyl trimethyl ammonium hydroxide, and benzyl trimethyl ammonium hydroxide. Among these, trimethyl-2-hydroxyethyl ammonium hydroxide and tetramethyl ammonium hydroxide are particularly preferred.
[0085] Other organic bases include methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, dioctylamine, trioctylamine, aminoethanol, aminopropanol, aminobutanol, and 2-methoxyethylamine. These organic bases have high solubility in the electrolyte, so if they are used in excess, they may reduce battery performance. In addition, these compounds are prone to decomposition, so the decomposition products may remain in the coating film, and if they are present in the battery, they may reduce the initial capacity.
[0086] The amount of the base used is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the mass of the polymer. The amount of the base used is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on the mass of the polymer. If the amount used is too large, the stability of the resulting carbon nanotube dispersion liquid may be poor. Furthermore, it may cause corrosion of the dispersion device and / or the inside of the battery.
[0087] The reason why the dispersibility is improved by adjusting the pH to a predetermined value is unclear, but the following factors are considered. The reasons why the dispersibility is improved are not limited to the factors (1) to (3) listed below. (1) Improve the dispersibility of the polymer. By adjusting pH to a predetermined value, the polymer containing one or more selected from the group consisting of nitrile group-containing structural unit, carboxy group-containing structural unit, hydroxy group-containing structural unit, and heterocyclic ring-containing structural unit can increase the adsorption power to the dispersed material.In addition, since the functional group of the structural unit can form hydrogen bond, a crosslinked structure by hydrogen bond is introduced into the polymer molecule, which can be three-dimensionally adsorbed to the dispersed material, and it is believed that a dispersion liquid excellent in not only dispersibility but also stability can be obtained. (2) It reduces the solution viscosity of the polymer. When a polymer is dissolved in a solvent and used, if the viscosity of the polymer solution is low, the dispersant can easily penetrate into the carbon nanotubes, which have strong cohesive forces, and it is believed that a uniform dispersion can be obtained. (3) Improve the wettability of carbon nanotubes. When dispersing carbon nanotubes, the carbon nanotubes are wetted with a solvent to reduce the cohesive force between the carbon nanotubes, and then crushed and stabilized so that they can exist as a dispersion liquid. Carbon nanotubes have significantly lower wettability than other conductive materials, so they need to be pretreated to improve their wettability by chemical treatment or mechanical crushing, but these treatments may reduce the conductivity. It is believed that by adjusting the pH to a specified value, the wettability of carbon nanotubes can be dramatically improved without compromising their conductivity.
[0088] The carbon nanotube dispersion of the present disclosure may contain an antifoaming agent in addition to the dispersant. Any antifoaming agent having an antifoaming effect, such as a commercially available antifoaming agent, a wetting agent, a hydrophilic organic solvent, a water-soluble organic solvent, etc., may be used, and one or more of them may be used in combination. For example, alcohols: ethanol, propanol, isopropanol, butanol, octyl alcohol, hexadecyl alcohol, acetylene alcohol, ethylene glycol monobutyl ether, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, acetylene glycol, polyoxyalkylene glycol, propylene glycol, other glycols, etc.; fatty acid esters: diethylene glycol laurate, glycerin monoricinoleate, alkenylsuccinic acid derivatives, sorbitol monolaurate, sorbitol trioleate. esters, tributyl phosphate, sodium octyl phosphate, metal soaps, aluminum stearate, calcium oleate, etc.; oils and fats, animal and vegetable oils, sesame oil, castor oil, etc.; mineral oils: kerosene, paraffin, etc.; silicones, dimethyl silicone oil, silicone paste, silicone emulsion, organic modified polysiloxane, fluorosilicone oil, etc.
[0089] <Other conductive materials> The carbon nanotube dispersion of the present disclosure may contain other conductive materials in addition to the carbon nanotubes. Examples of the other conductive materials include metal powders such as gold, silver, copper, silver-plated copper powder, silver-copper composite powder, silver-copper alloy, amorphous copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, malbutene, and platinum, inorganic powders coated with these metals, powders of metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, and ruthenium oxide, inorganic powders coated with these metal oxides, and carbon materials such as carbon black and graphite. The other conductive materials may be used alone or in combination of two or more. When using the other conductive materials, carbon black is preferred from the viewpoint of the adsorption performance of the dispersant. The other conductive materials are substances (materials) different from the electrode active material described later.
[0090] Examples of carbon black include acetylene black, furnace black, hollow carbon black, channel black, thermal black, ketjen black, etc. Carbon black may be neutral, acidic, or basic, and oxidation-treated carbon black or graphitization-treated carbon black may be used.
[0091] <Production of Carbon Nanotube Dispersion> The carbon nanotube dispersion of the present disclosure contains bundled carbon nanotubes and a solvent, and preferably further contains a dispersant. In order to obtain the carbon nanotube dispersion of the present disclosure, it is preferable to carry out a process for dispersing the treated carbon nanotubes described above in a solvent. The dispersing device used for such a process is not particularly limited.
[0092] As the dispersing device, a dispersing machine generally used for dispersing pigments, etc., can be used. For example, a mixer such as a disperser, a homomixer, or a planetary mixer, a homogenizer (Advanced Digital Homogenizer manufactured by Branson, Inc.) Examples of media-type dispersers include media-type dispersers such as Sonifer (registered trademark), MODEL450DA, M-Technique's "Clearmix," PRIMIX's "Filmix," Silverson's "Abramix," etc.), paint conditioners (manufactured by Red Devil), colloid mills (PUC's "PUC Colloid Mill," IKA's "Colloid Mill MK"), cone mills (IKA's "Cone Mill MKO," etc.), ball mills, sand mills (Shinmaru Enterprises' "Dyno Mill," etc.), attritors, pearl mills (Eirich's "DCP Mill," etc.), and Coball mills; wet jet mills (Zenus' "Zenus PY," Sugino Machine's "Starburst," Nanomizer's "Nanomizer," etc.); media-less dispersers such as M-Technique's "Clear SS-5" and Nara Kikai's "MICROS," and other roll mills, but are not limited to these.
[0093] The amount of carbon nanotubes in the carbon nanotube dispersion of the present disclosure is preferably 0.2 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and further preferably 0.5 to 3.0 parts by mass, based on 100 parts by mass of the carbon nanotube dispersion.
[0094] The viscosity of the carbon nanotube dispersion of this embodiment, measured at 60 rpm using a Brookfield viscometer, is preferably 10 mPa·s or more and 10,000 mPa·s or less, more preferably 10 mPa·s or more and 5,000 mPa·s or less, and even more preferably 10 mPa·s or more and 2,000 mPa·s or less.
[0095] The carbon nanotube dispersion of the present disclosure not only achieves both excellent dispersibility and conductivity, but also improves durability against external forces such as impact and coating strength, and therefore can be suitably used as a dispersion for forming conductive wiring or transparent conductive films, and as a dispersion for forming electrochemical devices such as secondary batteries, capacitors, and sensors.
[0096] <Carbon nanotube resin composition> The carbon nanotube resin composition of the present disclosure contains a carbon nanotube dispersion and a binder, and can be obtained by mixing and homogenizing the carbon nanotube dispersion and the binder. As a mixing method, a conventionally known method can be used, and the dispersing device described above for the carbon nanotube dispersion can be used.
[0097] <Binder> The binder in this disclosure is a resin for binding substances such as carbon nanotubes together. The binder resin can be appropriately selected according to the desired physical properties, and examples of the binder resin include polymers or copolymers containing ethylene, propylene, vinyl chloride, vinyl acetate, vinyl alcohol, maleic acid, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, acrylonitrile, styrene, vinyl butyral, vinyl acetal, vinyl pyrrolidone, etc. as structural units; polyurethane resins, polyester resins, phenolic resins, epoxy resins, phenoxy resins, urea resins, melamine resins, alkyd resins, acrylic resins, formaldehyde resins, silicone resins, fluororesins; cellulose resins such as carboxymethylcellulose; rubbers such as styrene butadiene rubber and fluororubber; and conductive resins such as polyaniline and polyacetylene. Modified bodies, mixtures, and copolymers of these resins may also be used. Among these, when used as a binder resin for a positive electrode film, polymers or copolymers having fluorine atoms in the molecule such as polyvinylidene fluoride, polyvinyl fluoride, tetrafluoroethylene, etc. are preferred from the viewpoint of durability, while when used as a binder resin for a negative electrode film, carboxymethyl cellulose, styrene butadiene rubber, polyacrylic acid, etc., which have good adhesion, are preferred.
[0098] Carboxymethyl cellulose preferably has a high viscosity, and for example, when made into a 1% by mass aqueous solution, the viscosity is preferably 500 to 6000 mPa s, more preferably 1000 to 3000 mPa s. The above viscosity can be measured using a Brookfield viscometer at 25° C. with a rotor rotation speed of 60 rpm.
[0099] Carboxymethyl cellulose preferably has a high degree of etherification. For example, the degree of etherification is preferably 0.6 to 1.5, and more preferably 0.8 to 1.2.
[0100] The type and amount of the binder are appropriately selected according to the properties of the coexisting materials such as carbon nanotubes, active material, etc. For example, when carboxymethyl cellulose is used, the ratio of carboxymethyl cellulose is preferably 0.5 to 3.0% by mass, more preferably 1.0 to 2.0% by mass, based on 100% by mass of the active material.
[0101] The styrene-butadiene rubber may be any rubber generally used as a binder for electrodes, so long as it is an oil-in-water emulsion. When using styrene-butadiene rubber, the proportion of the styrene-butadiene rubber is preferably 0.5 to 3.0% by mass, more preferably 1.0 to 2.0% by mass, based on 100% by mass of the active material.
[0102] When polyacrylic acid is used, the proportion of polyacrylic acid is preferably 1 to 25% by mass, and more preferably 5 to 20% by mass, relative to 100% by mass of the active material.
[0103] The weight average molecular weight of these binder resins is preferably 10,000 to 2,000,000, more preferably 100,000 to 1,000,000, and further preferably 200,000 to 1,000,000.
[0104] <Compound slurry> The composite slurry of the present disclosure contains the above-described carbon nanotube resin composition and an active material.
[0105] [Active material] In this disclosure, the active material refers to a material that is the basis of a battery reaction. Active materials are divided into positive electrode active materials and negative electrode active materials based on their electromotive force.
[0106] As the positive electrode active material, there is no particular limitation, but metal compounds such as metal oxides and metal sulfides capable of doping or intercalating lithium ions, and conductive polymers can be used. For example, oxides of transition metals such as Fe, Co, Ni, Mn, composite oxides with lithium, inorganic compounds such as transition metal sulfides, etc. can be mentioned. Specifically, transition metal oxide powders such as MnO, V2O5, V6O 13 , TiO2, etc., composite oxide powders of lithium and transition metals such as layered lithium nickelate, lithium cobaltate, lithium manganate, spinel-structured lithium manganate, lithium iron phosphate-based materials which are olivine-structured phosphate compounds, transition metal sulfide powders such as TiS2, FeS, etc. can be mentioned. Also, conductive polymers such as polyaniline, polyacetylene, polypyrrole, polythiophene can be used. Further, the above inorganic compounds and organic compounds may be mixed and used.
[0107] As the negative electrode active material, there is no particular limitation as long as it can dope or intercalate lithium ions. For example, metal Li, alloy systems such as its alloys like tin alloy, silicon alloy, lead alloy, etc., Li X Fe2O3, Li X Fe3O4, Li X WO2 (x is a number where 0 < x < 1.), metal oxide systems such as lithium titanate, lithium vanadate, lithium silicate, etc., conductive polymer systems such as polyacetylene, poly-p-phenylene, etc., amorphous carbonaceous materials such as soft carbon and hard carbon, artificial graphite such as highly graphitized carbon materials, or carbonaceous powders such as natural graphite, carbon black, mesophase carbon black, resin-fired carbon materials, gas-phase grown carbon fibers, carbon fibers, etc. can be mentioned. These negative electrode active materials can also be used alone or in combination of two or more.
[0108] As the negative electrode active material of the present disclosure, a silicon-based negative electrode active material which is a negative electrode active material containing silicon such as a silicon alloy or lithium silicate is preferable.
[0109] Examples of silicon-based negative electrode active materials include so-called metallurgical grade silicon produced by reducing silicon dioxide with carbon; industrial grade silicon obtained by reducing impurities in metallurgical grade silicon by acid treatment, unidirectional solidification, or the like; high-purity silicon having different crystalline states, such as high-purity single crystal, polycrystalline, and amorphous, produced from silane obtained by reacting silicon; and silicon obtained by making industrial grade silicon highly pure by a sputtering method, EB deposition (electron beam deposition) method, or the like, while simultaneously adjusting the crystalline state or precipitation state.
[0110] Other examples include silicon oxide, which is a compound of silicon and oxygen, silicon and various alloys, and silicon compounds in which the crystalline state of these alloys is adjusted by a quenching method, etc. Among these, a silicon-based negative electrode active material having a structure in which silicon nanoparticles are dispersed in silicon oxide and the outside is coated with a carbon film is preferred.
[0111] In addition to the silicon-based negative electrode active material, the negative electrode active material of the present disclosure preferably uses amorphous carbonaceous materials such as soft carbon and hard carbon, artificial graphite such as highly graphitized carbon materials, or carbonaceous powder such as natural graphite. Among them, it is preferable to use carbonaceous powder such as artificial graphite or natural graphite.
[0112] The amount of the silicon-based negative electrode active material is preferably 3 to 50 mass %, and more preferably 5 to 25 mass %, based on 100 mass % of carbonaceous powder such as artificial graphite or natural graphite.
[0113] The BET specific surface area of the active material of the present disclosure is 0.1 to 10 m 2 / g is preferable, and 0.2 to 5m 2 / g is more preferable, and 0.3 to 3m 2 / g is more preferred.
[0114] The average particle size of the active material of the present disclosure is preferably within a range of 0.5 to 50 μm, and more preferably 2 to 20 μm. The average particle size of the active material in this specification refers to the average value of particle sizes measured by an electron microscope.
[0115] [Method of manufacturing composite slurry] The composite slurry of the present disclosure can be prepared by various conventionally known methods, such as a method of adding an active material to a carbon nanotube resin composition, or a method of adding an active material to a carbon nanotube dispersion and then adding a binder.
[0116] In order to obtain the composite slurry of the present disclosure, it is preferable to add an active material to a carbon nanotube resin composition and then perform a dispersion process. The dispersion device used for such a process is not particularly limited. The composite slurry can be obtained using the dispersion device described for the carbon nanotube dispersion liquid.
[0117] The amount of the active material in the composite slurry of the present disclosure is preferably 20 to 85 parts by mass, more preferably 30 to 75 parts by mass, and even more preferably 40 to 70 parts by mass, per 100 parts by mass of the composite slurry.
[0118] The amount of carbon nanotubes in the composite slurry of the present disclosure is preferably 0.01 to 10 parts by mass, more preferably 0.02 to 5 parts by mass, and even more preferably 0.03 to 1 part by mass, relative to 100 parts by mass of the active material.
[0119] The amount of binder in the composite slurry of the present disclosure is preferably 0.5 to 30 mass %, more preferably 1 to 25 mass %, and particularly preferably 2 to 20 mass %, relative to 100 mass % of the active material.
[0120] The amount of solid content in the composite slurry of the present disclosure is preferably 30 to 90 mass %, more preferably 30 to 80 mass %, and more preferably 40 to 75 mass %, relative to 100 mass % of the composite slurry.
[0121] <Conductive film and electrode film> The conductive film of the present disclosure is formed by forming a carbon nanotube dispersion into a film. For example, it is a coating film formed by coating and drying a carbon nanotube dispersion on a sheet-like substrate. The sheet-like substrate is not particularly limited, and a conductive or non-conductive substrate can be used. The conductive substrate can be a current collector as described below.
[0122] The electrode film of the present disclosure is formed by forming a composite material slurry into a film shape, for example, a coated film in which the composite material slurry is coated on a current collector and dried to form an electrode composite material layer. The material and shape of the current collector used in the electrode film are not particularly limited, and can be appropriately selected from those suitable for various secondary batteries. For example, the material of the current collector can be metals or alloys such as aluminum, copper, nickel, titanium, or stainless steel. In addition, as for the shape, a flat foil is generally used, but a current collector with a roughened surface, a perforated foil, or a mesh-shaped current collector can also be used.
[0123] The method for applying the composite slurry onto the current collector is not particularly limited, and any known method can be used. Specifically, examples of the method include die coating, dip coating, roll coating, doctor coating, knife coating, spray coating, gravure coating, screen printing, and electrostatic painting, and the drying method can be, but is not limited to, standing drying, a blower dryer, a hot air dryer, an infrared heater, or a far infrared heater.
[0124] After coating, the coating may be rolled using a lithographic press, a calendar roll, etc. The thickness of the electrode mixture layer is generally 1 μm or more and 500 μm or less, and preferably 10 μm or more and 300 μm or less.
[0125] <Nonaqueous electrolyte secondary battery> The nonaqueous electrolyte secondary battery of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte, and at least one of the positive electrode and the negative electrode includes the above-mentioned electrode film. When the positive electrode includes the electrode film of the present disclosure, a composite slurry including a positive electrode active material is coated on a current collector and dried to produce an electrode film. When the negative electrode includes the electrode film of the present disclosure, a composite slurry including a negative electrode active material is coated on a current collector and dried to produce an electrode film.
[0126] As the electrolyte, various conventionally known electrolytes capable of moving ions can be used. For example, those containing lithium salts such as LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, Li(CF3SO2)3C, LiI, LiBr, LiCl, LiAlCl, LiHF2, LiSCN, or LiBPh4 (wherein Ph is a phenyl group) can be mentioned, but are not limited thereto, and those containing sodium salts or calcium salts can also be used. It is preferable that the electrolyte is dissolved in a non-aqueous solvent and used as an electrolytic solution.
[0127] Examples of non-aqueous solvents include, but are not limited to, carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; lactones such as γ-butyrolactone, γ-valerolactone, and γ-octanoic lactone; glymes such as tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,2-methoxyethane, 1,2-ethoxyethane, and 1,2-dibutoxyethane; esters such as methyl formate, methyl acetate, and methyl propionate; sulfoxides such as dimethyl sulfoxide and sulfolane; and nitriles such as acetonitrile. These solvents may be used alone or in combination of two or more.
[0128] The nonaqueous electrolyte secondary battery of the present disclosure preferably includes a separator, such as, but not limited to, polyethylene nonwoven fabric, polypropylene nonwoven fabric, polyamide nonwoven fabric, and those that have been subjected to a hydrophilic treatment.
[0129] The structure of the nonaqueous electrolyte secondary battery of the present disclosure is not particularly limited, but is usually composed of a positive electrode and a negative electrode, and a separator that is provided as necessary, and can be in various shapes depending on the purpose of use, such as a paper type, a cylindrical type, a button type, or a laminated type. EXAMPLES
[0130] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples unless it exceeds the gist of the present invention. In addition, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass".
[0131] <Measurement of bundled CNTs in dispersion> The percentage by number, average outer diameter, average fiber length, and average aspect ratio of the bundled CNTs in the carbon nanotube dispersions of the Examples were determined by SEM image analysis according to the method described above in the section <Bundled Carbon Nanotubes>.
[0132] <Measurement of the average diameter of raw CNT> The average diameter of the carbon nanotubes used as the raw material was determined by TEM image analysis according to the method described in the above section [Raw material carbon nanotubes].
[0133] <Production of bundled CNTs> [Manufacturing example of raw CNT (A)] A catalyst for CNT synthesis was prepared by the method described in paragraph
[0117] of JP 2018-150218. Then, a quartz glass heat-resistant plate on which 1.5 g of the catalyst for CNT synthesis was spread was placed in the center of a horizontal reaction tube with an internal volume of 10 L, which can be pressurized and heated by an external heater. The air in the reaction tube was replaced with nitrogen gas while injecting nitrogen gas, and the atmosphere in the horizontal reaction tube had an oxygen concentration of 1% by volume or less. Next, the horizontal reaction tube was heated with an external heater until the central temperature in the horizontal reaction tube reached 680°C. After reaching 680°C, propane gas was introduced into the reaction tube as a carbon source at a flow rate of 2L per minute and reacted for 2 hours. After the reaction was completed, the gas in the reaction tube was replaced with nitrogen gas, and the reaction tube was cooled to 100°C or less and taken out to obtain CNT (A). The average diameter of CNT (A) is 9.1 nm.
[0134] [Manufacturing example (1)] 100 parts of 8S (JEIO carbon nanotube, average diameter 6.8 nm) as a carbon source was mixed with 9900 parts of ethyl alcohol as a processing solvent, and wet-mixed using Filmix (PRIMIX), then heated and dried at 65°C to remove the solvent, producing precursor (1). Next, precursor (1) was filled into a graphite crucible, and heated in a firing furnace in an argon atmosphere at a heating rate of 10°C / min until the temperature inside the furnace reached 1700°C, followed by heat treatment at 1700°C for 2 hours to obtain CNT (1).
[0135] [Manufacturing Examples (2) to (6)] CNTs (2) to (6) were obtained in the same manner as in Production Example (1), except that the raw carbon nanotubes, processing solvent, additives, and firing conditions were changed as shown in Table 1.
[0136] [Manufacturing Example (7)] 100 parts of 8S (carbon nanotubes manufactured by JEIO CO., LTD., average diameter 6.8 nm) as a carbon source and 9900 parts of a mixed solvent (a solvent obtained by mixing toluene and normal propyl alcohol at a mass ratio of 1:1) as a treatment solvent were mixed, and after performing wet mixing by ultrasonic waves, heating and drying were performed at 65°C to remove the solvent, thereby producing a precursor (7). Next, the precursor (7) was filled into a graphite crucible, heated in a firing furnace under an argon atmosphere at a heating rate of 10°C / min until the furnace temperature reached 1700°C, and then heat treatment was performed at 1700°C for 2 hours to obtain CNT (7).
[0137]
Table 1
[0138] <Manufacture of CNT dispersion liquid> [Example 1] CNT dispersion liquid (W1) 97.7 parts of ion-exchanged water, 0.45 parts of dispersant (1) (polyvinylpyrrolidone (manufactured by Nippon Shokubai Co., Ltd., K-30)), and 0.05 parts of antifoaming agent (A) (SN defoamer 1312 manufactured by San Nopco Ltd.) were added to a stainless steel container and stirred with a disper until uniform. Then, while stirring with a disper, 1.8 parts of treated CNT (1) were added and further stirred with a disper until uniform. Thereafter, dispersion treatment was performed using a high-pressure homogenizer (manufactured by Sugino Machine, Ltd., Starburst 10). The dispersion treatment was performed using a single nozzle chamber, with a nozzle diameter of 0.17 mm and a pressure of 100 MPa, and 6-pass treatment was performed to obtain CNT dispersion liquid (W1).
[0139] [Examples 3, 6, 7, 9, 10] CNT dispersion liquids (W3, 6, 7, 9, 10) CNT dispersion liquids (W3), (W6), (W7), (W9), and (W10) were obtained in the same manner as in Example 1, except that the types of treated CNT, CNT addition amounts, ion-exchanged water addition amounts, types of dispersants, dispersant addition amounts, antifoaming agent addition amounts, and number of passes were changed as shown in Table 2.
[0140] [Example 4] CNT dispersion liquid (W4) In a stainless steel container, 92.27 parts of ion-exchanged water, 3.2 parts of dispersant (4) (polyacrylic acid (Jurimer AC-10LP, manufactured by Toagosei Co., Ltd.)), 0.48 parts of sodium carbonate (Na2CO3), and 0.05 parts of defoamer (A) (SN Deformer 1312, manufactured by San Nopco Co., Ltd.) were added and stirred with a disperser until uniform. Then, while stirring with a disperser, 4 parts of treated CNT (2) were added and further stirred with a disperser until uniform. After that, a dispersion process was performed using a high-pressure homogenizer (Starburst 10, manufactured by Sugino Machine Co., Ltd.). The dispersion process was performed using a single nozzle chamber, with a nozzle diameter of 0.17 mm and a pressure of 100 MPa, and 4 passes were performed to obtain a CNT dispersion liquid (W4).
[0141] [Example 2] CNT dispersion (W2) A glass bottle was charged with 2 parts of the treated CNTs (1), 0.5 parts of the dispersant (7), 0.05 parts of the defoamer (A) (SN DEFORMER 1312 manufactured by San Nopco Ltd.), 97.45 parts of ion-exchanged water, and 140 parts of zirconia beads (bead diameter 0.3 mmφ), and a dispersion treatment was carried out for 4 hours using a paint conditioner manufactured by Red Devil Co., Ltd., after which the zirconia beads were separated to obtain a CNT dispersion (W2).
[0142] [Examples 5, 8, 16] CNT dispersions (W5), (W8), (W19) CNT dispersions (W5), (W8), and (W19) were obtained in the same manner as in Example 2, except that the type of treated CNT, amount of CNT added, amount of ion-exchanged water added, type of dispersant, amount of dispersant added, amount of antifoaming agent added, and dispersion time were changed as shown in Table 2.
[0143] [Example 11] CNT dispersion (W14) 96.44 parts of ion-exchanged water, 2.1 parts of dispersant (4) (polyacrylic acid (Toagosei Co., Ltd., Julimer AC-10LP)), 0.21 parts of sodium carbonate, and 0.05 parts of defoamer (A) (San Nopco Ltd., SN Deformer 1312) were added to a stainless steel container and stirred with a disperser until uniform. Then, while stirring with a disperser, 1.2 parts of treated CNT (1) were added and further stirred with a disperser until uniform. After that, dispersion treatment was performed using a high-pressure homogenizer (Sugino Machine Co., Ltd., Starburst 10). The dispersion treatment was performed using a single nozzle chamber, with a nozzle diameter of 0.17 mm and a pressure of 100 MPa, and five passes were performed. The resulting dispersion was centrifuged to remove precipitates. Furthermore, 80 parts of the above stirring liquid and 120 parts of zirconia beads (bead diameter 1 mmΦ) were placed in a glass bottle, and dispersion treatment was performed for 5 hours using a paint conditioner manufactured by Red Devil, after which the zirconia beads were separated to obtain a CNT dispersion liquid (W14).
[0144] [Example 12] CNT dispersion (W15) A CNT dispersion (W15) was obtained in the same manner as in Example 11, except that the type of treated CNT, amount of CNT added, amount of ion-exchanged water added, type of dispersant, amount of dispersant added, type of basic compound, amount of basic compound added, amount of antifoaming agent added, and dispersion time were changed as shown in Table 2.
[0145] [Example 13] CNT dispersion (W16) A CNT dispersion (W16) was obtained in the same manner as in Example 11, except that the type of treated CNT, amount of CNT added, amount of ion-exchanged water added, type of dispersant, amount of dispersant added, amount of defoamer added, and dispersion time were changed to those shown in Table 2, and no basic compound was used.
[0146] [Example 14] CNT dispersion (W17) A stainless steel container was charged with 97.95 parts of ion-exchanged water, 0.5 parts of dispersant (2) (carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., APP-084)), and 0.05 parts of defoamer (A) (manufactured by San Nopco Ltd., SN Deformer 1312), and the mixture was stirred with a disperser until uniform. Then, while stirring with a disperser, 1.2 parts of CNT (1) and 0.3 parts of CNT (8) (manufactured by Hamamatsu Carbonix Co., Ltd., NFT005) were added, and the mixture was further stirred with a disperser until uniform. After that, a dispersion treatment was performed with a high-pressure homogenizer (manufactured by Sugino Machine Co., Ltd., Starburst 10). The dispersion treatment was performed using a single nozzle chamber, with a nozzle diameter of 0.17 mm and a pressure of 100 MPa, with 20 passes being performed. The resulting dispersion was centrifuged to remove precipitates, and then 80 parts of the above stirring liquid and 120 parts of zirconia beads (bead diameter 1 mmΦ) were placed in a glass bottle and dispersion treatment was performed for 10 hours using a paint conditioner manufactured by Red Devil, after which the zirconia beads were separated to obtain a CNT dispersion liquid (W17).
[0147] [Example 15] CNT dispersion (W18) In a stainless steel container, 97.95 parts of ion-exchanged water, 0.5 parts of dispersant (2) (carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., APP-084)), and 0.05 parts of defoamer (A) (manufactured by San Nopco Ltd., SN Deformer 1312) were added, and the mixture was stirred with a disperser until it became uniform. Then, while stirring with a disperser, 1.35 parts of CNT (1) and 0.15 parts of CNT (8) (manufactured by Hamamatsu Carbonix Co., Ltd., NFT005) were added, and the mixture was further stirred with a disperser until it became uniform. After that, a dispersion treatment was performed with a high-pressure homogenizer (manufactured by Sugino Machine Co., Ltd., Starburst 10). The dispersion treatment was performed using a single nozzle chamber, with a nozzle diameter of 0.17 mm and a pressure of 100 MPa, and 10 passes were performed. The resulting dispersion was centrifuged to remove precipitates, and a CNT dispersion (W18) was obtained.
[0148] [Comparative Example 1] According to the composition shown in Table 2, a glass bottle was charged with treated CNT, ion-exchanged water, a dispersant, an antifoaming agent, and 140 parts of zirconia beads (bead diameter: 0.3 mmφ), and after performing a dispersion treatment for 20 hours using a paint conditioner manufactured by Red Devil, the zirconia beads were separated to obtain a CNT dispersion (W11).
[0149] [Comparative Example 2] According to the composition shown in Table 2, a glass bottle was charged with treated CNT, ion-exchanged water, a dispersant, an antifoaming agent, and 140 parts of zirconia beads (bead diameter: 0.3 mmφ), and after performing a dispersion treatment for 0.5 hour using a paint conditioner manufactured by Red Devil, the zirconia beads were separated to obtain a CNT dispersion (W13).
[0150] Table 2 shows a list of the compounding compositions. The compounding amounts of the treated CNT, dispersant, and antifoaming agent in the table are all values converted to solid content.
[0151] [Evaluation of CNT Dispersion] The following evaluations were performed using the obtained CNT dispersion. The results are shown in Table 2.
[0152] (Viscosity) After allowing the CNT dispersion to stand in a constant temperature bath at 25°C for 1 hour or more, the CNT dispersion was sufficiently stirred, and then immediately measured at a rotational speed of 60 rpm using a B-type viscometer rotor. The rotor used for the measurement was No. 1 when the viscosity value was less than 100 mPa·s, No. 2 when it was 100 or more and less than 500 mPa·s, No. 3 when it was 500 or more and less than 2000 mPa·s, and No. 4 when it was 2000 or more and less than 10000 mPa·s, respectively. [Judgment Criteria] ◎: Less than 2000 mPa·s (excellent) ○: 2000 mPa·s or more and less than 5000 mPa·s (good) △: 5000 mPa·s or more and less than 10000 mPa·s (fair) ×: 10000 mPa·s or more, sedimentation or separation (poor)
[0153] (Storage Stability) The CNT dispersion was left to stand at 50°C for 7 days, and the change in the liquid properties (ease of stirring when stirred with a spatula) was checked before and after storage, and evaluated according to the following criteria. 〔Judgment criteria〕 ○: Viscosity did not increase. No problem (good). △: Viscosity has increased but gelation has not occurred (passable) ×: Gelled (very poor)
[0154] (Volume resistivity) The CNT dispersion was applied to a PET substrate using an applicator, and then dried in an oven at 120°C for 30 minutes to obtain a CNT coating film (film thickness 3μm). The surface resistivity (Ω / □) of the coating film after drying was then measured using a Loresta GP, MCP-T610 (manufactured by Nitto Seiko Analytech Co., Ltd.). After measurement, the surface resistivity was multiplied by the thickness of the CNT coating film formed on the PET substrate to obtain the volume resistivity (Ω·cm) of the coating film. The thickness of the coating film was calculated by subtracting the film thickness of the PET substrate from the average value measured at five points in the film using a film thickness meter to calculate the volume resistivity (Ω·cm) of the coating film. The evaluation criteria are as follows: 〔Judgment criteria〕 ◎: Volume resistivity (Ω cm) of the CNT coating is 7×10 -3 Less than (Excellent) 〇: The volume resistivity (Ω cm) of the CNT coating is 7×10 -3 More than 1×10 -2 Less than (good) △: The volume resistivity (Ω cm) of the CNT coating is 1×10 -2 More than 2×10 -2 Less than (OK) ×: Volume resistivity (Ω cm) of the CNT coating is 2×10 -2 or more (defect)
[0155] (Volume resistivity of negative electrode film) First, the obtained CNT dispersion liquid, ion-exchanged water, and 12.5 parts of a 2% aqueous solution of CMC (manufactured by Daicel FineChem Co., Ltd., #1190) were mixed and stirred at 2000 rpm for 30 seconds using a planetary centrifugal mixer to obtain a CNT resin composition. At this time, the amount of CNT dispersion liquid was adjusted so that the amount of CNT in 100 parts of the composite slurry was 0.27 parts. Then, 2.4 parts of silicon monoxide (manufactured by Osaka Titanium Technology Co., Ltd., SILICON MONOOXIDE, SiO 1.3C 5μm) was added, and the mixture was stirred for 30 seconds at 2000 rpm using a planetary mixer. Furthermore, 21.9 parts of artificial graphite (manufactured by Nippon Graphite Industries Co., Ltd., CGB-20) was added, and the mixture was stirred for 30 seconds at 2000 rpm using a planetary mixer. Then, 0.78 parts of styrene butadiene emulsion (manufactured by JSR Corporation, TRD2001) was added, and the mixture was stirred for 30 seconds at 2000 rpm using a planetary mixer to obtain a negative electrode composite slurry.
[0156] The obtained negative electrode composite slurry was used to prepare an electrode with a coating weight of 8 mg / cm 2 After coating on a PET substrate so that the thickness was as shown in the figure, the negative electrode was obtained by drying in an electric oven at 120°C for 30 minutes. The surface resistivity (Ω / □) of the coating film after drying was then measured using a Loresta GP, MCP-T610 (manufactured by Nitto Seiko Analytech Co., Ltd.). Meanwhile, the thickness of the negative electrode composite layer was calculated by subtracting the film thickness of the PET substrate from the average value measured at five points in the electrode film using a film thickness meter. The surface resistivity of the coating film thus obtained was multiplied by the thickness of the negative electrode mixture layer to calculate the volume resistivity (Ω·cm) of the negative electrode mixture layer, and the volume resistivity was evaluated according to the following criteria. 〔Judgment criteria〕 ◎: Volume resistivity (Ω·cm) of the negative electrode mixture layer is less than 0.12 (excellent) ○: The volume resistivity (Ω·cm) of the negative electrode mixture layer is 0.12 or more and less than 0.15 (good) △: Volume resistivity (Ω·cm) of the negative electrode mixture layer is 0.15 or more and less than 0.25 (acceptable) ×: The volume resistivity (Ω·cm) of the negative electrode mixture layer is 0.25 or more (defective)
[0157] (Peel strength of negative electrode film) The obtained negative electrode composite slurry was applied to the electrode with an applicator so that the coating amount was 8 mg / cm 2 After coating on copper foil so that the coating was as shown in the figure, the coating was dried in an oven at 120°C for 30 minutes. After that, the strip was cut into two 90mm x 20mm rectangles with the coating direction as the long axis. The peel strength was measured using a tensile tester and evaluated by the 180-degree peel test method. Specifically, a double-sided tape measuring 100mm x 30mm was attached to a stainless steel plate, the prepared battery electrode composite layer was attached to the other side of the double-sided tape, and the layer was peeled off while being pulled from the bottom to the top at a constant speed (50mm / min). The average value of the stress at this time was taken as the peel strength. The evaluation criteria are shown below. 〔Judgment criteria〕 ◎: Peel strength of negative electrode composite layer (N / cm) is 0.5 or more (excellent) ○: The peel strength (N / cm) of the negative electrode mixture layer is 0.4 or more and less than 0.5 (good) △: Peel strength of negative electrode mixture layer (N / cm) is 0.3 or more and less than 0.4 (acceptable) ×: Peel strength (N / cm) of the negative electrode mixture layer is less than 0.3 (defective)
[0158] (Cycle characteristics) First, a standard positive electrode (SC) was prepared as follows. Capacity 150cm 393 parts by mass of a positive electrode active material (manufactured by BASF Toda Battery Materials LLC, HED (registered trademark) NCM-111 1100), 4 parts by mass of acetylene black (manufactured by Denka Co., Ltd., Denka Black (registered trademark) HS100), and 3 parts by mass of PVDF (manufactured by Kureha Battery Materials Japan Co., Ltd., Kureha KF Polymer W#1300) were added to the plastic container, and then mixed with a spatula until the powder was uniform. Then, 20.5 parts by mass of NMP were added, and the mixture was stirred for 30 seconds at 2000 rpm using a rotation-revolution mixer. Then, the mixture in the plastic container was mixed with a spatula until it was uniform, and the mixture was stirred for 30 seconds at 2000 rpm using the rotation-revolution mixer. Then, 14.6 parts by mass of NMP were added, and the mixture was stirred for 30 seconds at 2000 rpm using the rotation-revolution mixer. Finally, the mixture was stirred at 3000 rpm for 10 minutes using a high-speed stirrer to obtain a standard positive electrode composite slurry. The standard positive electrode composite slurry was then applied to an aluminum foil with a thickness of 20 μm as a current collector using an applicator, and then dried in an electric oven at 120° C. for 30 minutes to obtain a coating weight per unit area of the electrode of 20 mg / cm. 2 Further, a rolling process was performed using a roll press, and the density of the composite layer was adjusted to 3.1 g / cm 3 A standard positive electrode (SC) was fabricated.
[0159] Separately, the obtained negative electrode composite slurry was applied to a copper foil having a thickness of 20 μm as a current collector using an applicator, and then dried in an oven at 80° C. for 30 minutes to obtain an electrode with a coating weight of 10 mg / cm. 2 Then, the negative electrode mixture layer was rolled to a density of 1.6 g / cm. 3 Thus, a negative electrode having the above structure was fabricated. The obtained negative electrode and the standard positive electrode obtained above were punched out to 50 mm x 45 mm and 45 mm x 40 mm, respectively, and a separator (porous polypropylene film) was inserted between them into an aluminum laminate bag and dried in an electric oven at 70° C. for 1 hour. Then, 2 mL of electrolyte was injected into a glove box filled with argon gas, and the aluminum laminate bag was sealed to prepare a nonaqueous electrolyte secondary battery. The above electrolyte is a non-aqueous electrolyte prepared by dissolving LiPF6 at a concentration of 1M in a mixed solvent of ethylene carbonate, dimethyl carbonate, and diethyl carbonate in a 1:1:1 (volume ratio) ratio, to which 1 part of VC (vinylene carbonate) is added per 100 parts of electrolyte as an additive.
[0160] The obtained non-aqueous electrolyte secondary battery was placed in a constant temperature room at 40°C, and charge / discharge measurements were performed using a charge / discharge device (SM-8, manufactured by Hokuto Denko Corporation). After constant current / constant voltage charging (cutoff current 2.5mA (0.05C)) was performed with a charge current of 25mA (0.5C) and a charge end voltage of 4.3V, constant current discharging was performed with a discharge current of 25mA (0.5C) and a discharge end voltage of 3V. This operation was repeated 200 times. The cycle characteristics can be expressed by the following formula 2 as the ratio of the 3rd 0.5C discharge capacity at 25°C to the 200th 0.5C discharge capacity. The criteria for judgment are as follows: (Formula 2) Cycle characteristics = 200th 0.5C discharge capacity / 3rd 0.5C discharge capacity × 100(%) 〔Judgment criteria〕 ◎◎: Cycle characteristics are 85% or more (best) ◎: Cycle characteristics are 80% or more and less than 85% (excellent) ○: Cycle characteristics are 70% or more but less than 80% (excellent) 〇△: Cycle characteristics are 60% or more and less than 70% (good) △: Cycle characteristics are 50% or more and less than 60% (acceptable) ×: Cycle characteristics are less than 50% (defective)
[0161] (Change in film thickness before and after cycling) The cells before and after the evaluation of cycle characteristics were disassembled, and the rate of change in thickness of the composite layer was calculated from cross-sectional observation with an SEM and evaluated according to the following criteria. S: The change rate (%) of the thickness of the negative electrode mixture layer is less than 8% A: The change rate (%) of the thickness of the negative electrode mixture layer is 8% or more and less than 10% B: The change rate (%) of the thickness of the negative electrode mixture layer is 10% or more and less than 12% C: The change rate (%) of the thickness of the negative electrode composite layer is 12% or more
[0162] [Table 2]
[0163] The abbreviations in Table 2 are as follows: Dispersant (1): Polyvinylpyrrolidone (K-30, manufactured by Nippon Shokubai Co., Ltd.) Dispersant (2): Carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., APP-084) Dispersant (3): Carboxymethylcellulose ammonium salt (manufactured by Shin-Etsu Kogyo Co., Ltd., Metolose (registered trademark) SM-4) Dispersant (4): Polyacrylic acid (Toagosei Co., Ltd., Jurimer AC-10LP) Dispersant (5): Carboxymethylcellulose sodium salt (Sunrose (registered trademark) F01MC, manufactured by Nippon Paper Industries Co., Ltd.) Defoamer (A): SN DEFORMER 1312 manufactured by San Nopco Ltd.
[0164] According to Table 2, the electrode using the carbon nanotube dispersion of the present disclosure, which is made of carbon nanotubes having an average diameter of 3 nm to 30 nm and contains bundled carbon nanotubes having a predetermined outer diameter and fiber length, had excellent cycle characteristics. It is presumed that the carbon nanotube dispersion of the present disclosure contains a predetermined amount of predetermined bundled carbon nanotubes, thereby maintaining the coating film shape and suppressing deterioration, thereby exhibiting good cycle characteristics. On the other hand, in Comparative Examples 1 and 2, the dispersibility and conductivity of the carbon nanotubes in the dispersion are good, but the bundling is not maintained in the carbon nanotube dispersion, and it is difficult to maintain the shape of the coating film, which is thought to result in poor cycle characteristics. Also, the carbon nanotube dispersion using carbon nanotubes that were wet-treated using a boron source had better cycle characteristics. This is presumably due to the fact that the use of a boron source increases the strength of the bundle of bundled carbon nanotubes and improves dispersibility, making it easier to maintain the bundle shape.
[0165] The present disclosure includes the following embodiments. (Item 1) A carbon nanotube dispersion liquid containing bundled carbon nanotubes using carbon nanotubes having an average diameter of 3 nm to 30 nm and a solvent, A carbon nanotube dispersion in which the proportion of bundle-shaped carbon nanotubes (X) having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% or more, based on the number of carbon nanotubes having an outer diameter of 10 nm or more contained in the carbon nanotube dispersion. (Item 2) The carbon nanotube dispersion according to item 1, wherein the bundle-shaped carbon nanotubes (X) have an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm and have an average aspect ratio of 5 to 100. (Item 3) The carbon nanotube dispersion according to item 1 or 2, wherein the proportion of the bundle-shaped carbon nanotubes (X) having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% to 20% by number. (Item 4) The carbon nanotube dispersion according to any one of Items 1 to 3, wherein the proportion of the number of bundle-shaped carbon nanotubes (Y) having an outer diameter of 10 nm or more and less than 50 nm, and a fiber length of 1 μm to 5 μm is 10% to 60% based on the number of carbon nanotubes having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion. (Item 5) The carbon nanotube dispersion according to Item 4, wherein the proportion of the number of the bundle-shaped carbon nanotubes (Y) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 1 μm to 5 μm is 20% to 35%. (Item 6) The carbon nanotube dispersion according to any one of Items 1 to 5, wherein the proportion of the number of bundle-shaped carbon nanotubes (Z) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion is 50% to 80% based on the number of carbon nanotubes having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more. (Item 7) The carbon nanotube dispersion according to Item 6, wherein the ratio of the number of the bundled carbon nanotubes (Y) to the number of the bundled carbon nanotubes (Z) (the number of (Y) / the number of (Z)) is 0.3 to 0.6. (Item 8) The carbon nanotube dispersion liquid according to any one of Items 1 to 7, further comprising a dispersant. (Item 9) A conductive film which is a coating film of the carbon nanotube dispersion liquid according to any one of items 1 to 8. (Item 10) A carbon nanotube resin composition comprising the carbon nanotube dispersion liquid according to any one of items 1 to 8 and a binder. (Item 11) A composite slurry containing the carbon nanotube resin composition according to item 10 and an active material. (Item 12) An electrode film which is a coating film of the composite slurry according to item 11. (Item 13) A nonaqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein at least one of the positive electrode and the negative electrode comprises the electrode film according to item 12.
[0166] The disclosure of this application is related to the subject matter described in Patent Application No. 2022-153032, filed in Japan on September 26, 2022, the entire disclosure of which is incorporated herein by reference.
Claims
1. A carbon nanotube dispersion liquid containing bundled carbon nanotubes using carbon nanotubes having an average diameter of 3 nm to 30 nm and a solvent, A carbon nanotube dispersion in which the proportion of the number of bundle-shaped carbon nanotubes (X) having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% or more, based on the number of carbon nanotubes having an outer diameter of 10 nm or more contained in the carbon nanotube dispersion.
2. 2. The carbon nanotube dispersion according to claim 1, wherein the bundle-shaped carbon nanotubes (X) have an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm and have an average aspect ratio of 5 to 100.
3. 2. The carbon nanotube dispersion according to claim 1, wherein the proportion of the number of bundle-shaped carbon nanotubes (X) having an outer diameter of 50 nm to 5 μm and a fiber length of 1 μm to 100 μm is 0.2% to 20%.
4. 2. The carbon nanotube dispersion according to claim 1, wherein the proportion of bundle-shaped carbon nanotubes (Y) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 1 μm to 5 μm is 10% to 60% based on the number of carbon nanotubes having an outer diameter of 10 nm or more and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion.
5. 5. The carbon nanotube dispersion according to claim 4, wherein the proportion of the number of bundle-shaped carbon nanotubes (Y) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 1 μm to 5 μm is 20% to 35%.
6. 6. The carbon nanotube dispersion according to claim 1, wherein the proportion of the number of bundle-shaped carbon nanotubes (Z) having an outer diameter of 10 nm or more and less than 50 nm and a fiber length of 0.2 μm or more contained in the carbon nanotube dispersion is 50% to 80%.
7. The carbon nanotube dispersion liquid according to claim 6, wherein the ratio of the number of the bundled carbon nanotubes (Y) to the number of the bundled carbon nanotubes (Z) (the ratio of the number of (Y) / the ratio of the number of (Z)) is 0.3 to 0.
6.
8. The carbon nanotube dispersion liquid according to any one of claims 1 to 5, further comprising a dispersant.
9. A conductive film which is a coating film of the carbon nanotube dispersion liquid according to any one of claims 1 to 5.
10. A carbon nanotube resin composition comprising the carbon nanotube dispersion liquid according to any one of claims 1 to 5 and a binder.
11. A composite slurry comprising the carbon nanotube resin composition according to claim 10 and an active material.
12. An electrode film which is a coating film of the composite slurry according to claim 11.
13. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein at least one of the positive electrode and the negative electrode comprises the electrode film according to claim 12.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP1992155776A
Nonaqueous electrolyte secondary battery
JP1992237971A
Negative electrode material and secondary battery using the same
JP2004178922A
Conductive material dispersion and lithium secondary battery manufactured using the same
JP2018534731A
Conductive material dispersion and lithium secondary battery manufactured using the same
JP2018534747A
Cited By
Carbon nanotube dispersion composition, composition for secondary battery electrodes, electrode film, secondary battery, and vehicle
JP7917018B1
Current collector and manufacturing method therof
KR102923248B1
Carbon nanotube assembly, conductive material, electrode, secondary battery, planar assembly, filter, electromagnetic wave shield, and pellicle for extreme ultraviolet rays
WO2026203950A1