Polarizing film with pressure-sensitive adhesive layer, and image display device
The polarizing film with an adhesive layer on both sides addresses uneven thickness and curling issues, enhancing UV protection and durability in image display devices by using specific materials and configurations.
Patent Information
- Application Number
- JP2024102594
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2015-12-25
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polarizing films in image display devices face issues with uneven thickness, poor yield, and workability, as well as the need for higher UV absorption and prevention of curling due to thinner films, which accelerate the deterioration of optical components and are prone to curling.
A polarizing film with an adhesive layer on both sides, featuring a polarizer and transparent protective films, where the adhesive layer on the viewing side has a UV absorption function, using specific materials and thicknesses to ensure high UV protection and prevent curling.
The solution addresses the issues of uneven thickness, poor yield, and curling while providing enhanced UV protection, ensuring the durability and performance of image display devices by suppressing the deterioration of optical components.
Smart Images

Figure 2024160182000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film with a pressure-sensitive adhesive layer for use in an image display device. The present invention also relates to an image display device using the above-mentioned pressure-sensitive adhesive layer-attached polarizing film. , liquid crystal display devices, organic EL (electroluminescence) display devices, PDP (plasma display display panels, electronic paper, etc. [Background technology]
[0002] Liquid crystal display devices and organic EL display devices are classified into two types based on their image formation method: In such a device, it is essential to place polarizing elements on both sides of the liquid crystal cell. In addition, polarizing films are used for display panels such as liquid crystal panels and organic EL panels. In addition to films, various optical elements are used to improve the display quality. It is becoming more and more common.
[0003] The polarizing films used in these image display devices generally have a polarizer and two protective films. The protective film is triacetyl cellulose (TAC) ) is widely used.
[0004] In recent years, with the trend towards lighter and thinner image display devices, the components used in image display devices have There is a demand for thinner protective films for polarizing films. When the thickness of the protective film is thin, it is difficult to sufficiently block ultraviolet rays incident on the image display device. This has led to the use of polarizers as well as liquid crystal panels and other devices used in image display devices. There is a problem that ultraviolet rays accelerate the deterioration of various optical components, including electroluminescent devices. I did.
[0005] In order to solve such a problem, for example, a surface protection panel and a liquid crystal display device A double-sided adhesive sheet is placed between the viewing side of the crystal module to integrate the two components. The present invention has at least one ultraviolet absorbing layer and a light transmittance of 30% at a wavelength of 380 nm. % or less, and the visible light transmittance at wavelengths longer than 430 nm is 80% or more. A transparent double-sided adhesive sheet for an image display device (see, for example, Patent Document 1) and an acrylic poly A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing a triazine-based ultraviolet absorber is known. (For example, see Patent Document 2). In addition, a pressure-sensitive adhesive layer is provided on one or both sides of the optical film. In the pressure-sensitive adhesive optical film, the pressure-sensitive adhesive layer can be provided with ultraviolet absorbing ability. It is known (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-211305 A [Patent Document 2] JP 2013-75978 A [Patent Document 3] Patent No. 4208187 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, as described in Patent Documents 1 to 3, transparent adhesives having an ultraviolet absorbing function have been developed. It is known that various members used in an image display device are bonded together using the same. There were issues with regard to uneven thickness, reduced yield, and workability.
[0008] In addition, depending on the application of the polarizing film, a higher ultraviolet absorbing function is required. Specifically, if the product is exposed to ultraviolet light for a long period of time (specifically, about 300 hours), Even when exposed to ultraviolet light with a wide wavelength range, the optical properties do not change. It is required that the polarizing film has a higher ultraviolet absorbing function. was desired.
[0009] In addition, by making the polarizer and protective film thinner, the resulting polarizing film There was also the problem of curling.
[0010] Therefore, the present invention can solve the problem of the decrease in yield and the polarizing film Even in the case of a thin film, it can provide a higher level of UV protection and prevent curling. Another object of the present invention is to provide a polarizing film with a pressure-sensitive adhesive layer that can suppress the above-mentioned phenomenon. Another object of the present invention is to provide an image display device using the above polarizing film with a pressure-sensitive adhesive layer. . [Means for solving the problem]
[0011] As a result of intensive research conducted by the present inventors to solve the above problems, the following polarizing filter with an adhesive layer was discovered. This led to the completion of the present invention.
[0012] That is, the present invention relates to an adhesive used on the viewing side of an image display unit in an image display device. A layered polarizing film, The polarizing film with the pressure-sensitive adhesive layer comprises a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film. having The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, The transparent protective film on the viewing side of the polarizer has a transmittance of less than 6% at a wavelength of 380 nm. Yes, and The adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function. The present invention relates to a polarizing film having an adhesive layer.
[0013] The transparent protective film on the viewing side of the polarizer is a triacetyl cellulose film, an acrylic film, Polyethylene terephthalate film, and cyclo- or norbornene At least one film selected from the group consisting of polyolefin films having a structure It is preferable that the thickness of the film is 40 μm or less.
[0014] The thickness of the pressure-sensitive adhesive layer on the viewing side of the polarizing film is It is preferable that the thickness is at least twice the thickness of the adhesive layer.
[0015] The pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm, In addition, it is preferable that the transmittance at a wavelength of 400 nm is 60% or more.
[0016] The pressure-sensitive adhesive layer on the viewing side of the polarizing film preferably has a b* value of 3.0 or less.
[0017] The pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm, In addition, it is preferable that the transmittance at a wavelength of 420 nm is 75% or less.
[0018] The pressure-sensitive adhesive layer on the viewing side of the polarizing film is made of an acrylic polymer as a base polymer. It is preferable that it contains.
[0019] The pressure-sensitive adhesive layer-attached polarizing film of the present invention can be used in a liquid crystal display device or an organic EL display device. is preferred.
[0020] In addition, the present invention relates to a polarizing film having a pressure-sensitive adhesive layer of the present invention, which is used on the viewing side of an image display section. The present invention relates to an image display device. Effect of the Invention
[0021] The polarizing film with a pressure-sensitive adhesive layer of the present invention is a polarizing film in which the pressure-sensitive adhesive layer having an ultraviolet absorbing function is Since the film is pre-laminated on the visible side of the film, it solves the problem of process elimination and reduced yield. Even if the polarizing film is thin, it can still provide high UV protection. The image display of the present invention can be provided with a function to suppress curling. Since the device uses the above-mentioned polarizing film with an adhesive layer, it is possible to use a liquid crystal display device. It is possible to suppress the deterioration of various optical components, including liquid crystal panels and organic EL elements, caused by ultraviolet rays. This can be done. [Brief description of the drawings]
[0022] [Figure 1] 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a pressure-sensitive adhesive layer-attached polarizing film of the present invention. [Diagram 2] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. [Diagram 3] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. [Figure 4] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] 1. Polarizing film with adhesive layer The pressure-sensitive adhesive layer-attached polarizing film of the present invention is disposed on the viewing side of the image display unit in an image display device. Used, The polarizing film with the pressure-sensitive adhesive layer comprises a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film. having The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, The transparent protective film on the viewing side of the polarizer has a transmittance of less than 6% at a wavelength of 380 nm. Yes, and The pressure-sensitive adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function.
[0024] As shown in FIG. 1, the pressure-sensitive adhesive layer-attached polarizing film 1 of the present invention comprises a viewer-side pressure-sensitive adhesive layer 2a / a viewer-side pressure-sensitive adhesive layer 2b. Transparent protective film 3a on the viewing side / polarizer 4 / transparent protective film 3b on the image display side / image display section It is sufficient that the side adhesive layer 2b is included, and it may further include a retardation film or the like. Specifically, the visible-side pressure-sensitive adhesive layer 2a / the visible-side transparent protective film 3a / the polarizer 4 / the image Transparent protective film 3b on the display side / adhesive layer 2b on the image display side / retardation film (not shown) The polarizing film 5 may be configured as a viewing side / image display side adhesive layer (not shown). It is composed of a transparent protective film 3a / polarizer 4 / image display portion side transparent protective film 3b. Each layer is described in detail below.
[0025] (1) Visible side adhesive layer In the present invention, the pressure-sensitive adhesive layer on the viewing side of the polarizing film (the viewing-side pressure-sensitive adhesive layer) is an ultraviolet absorbing layer. The visible side pressure-sensitive adhesive layer may have an ultraviolet absorbing function. The composition is not particularly limited.
[0026] The visible-side adhesive layer can be formed using an appropriate adhesive. There are no particular limitations. The adhesive may be a rubber adhesive, an acrylic adhesive, or a silicone adhesive. adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol adhesives Adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, cellulose-based adhesives Among these pressure sensitive adhesives, those having excellent optical transparency, appropriate adhesion and cohesiveness, etc. Acrylic adhesives are preferred because they exhibit adhesive properties and are excellent in weather resistance and heat resistance. The acrylic adhesive (composition) is a polymer based on an acrylic polymer. Contains as mer.
[0027] The acrylic pressure-sensitive adhesive composition is, for example, a monomer containing an alkyl (meth)acrylate. Partial polymer of the monomer component and / or (meth)acrylic polymer obtained from the monomer component. It is preferable that the composition contains a polymer and an ultraviolet absorbing agent.
[0028] (1-1) Partially polymerized product of monomer component, and (meth)acrylic polymer The acrylic pressure-sensitive adhesive composition is a monomer composition containing an alkyl (meth)acrylate. A (meth)acrylic polymer obtained from the partial polymer of the monomer component and / or the monomer component. include.
[0029] The alkyl (meth)acrylate may be a linear or branched alkyl (meth)acrylate having 1 to 24 carbon atoms. Examples of alkyl (meth)acrylates include those having an alkyl group at the ester end. One type may be used alone or two or more types may be used in combination. The acrylate refers to an alkyl acrylate and / or an alkyl methacrylate. No (meta) has a similar meaning.
[0030] The alkyl (meth)acrylate may be, for example, the branched alkyl (meth)acrylate having 1 to 9 carbon atoms. A preferred example of the alkyl (meth)acrylate is an alkyl (meth)acrylate having the above structure. ) Acrylates are preferred because they have a well-balanced adhesive property. butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, iso Pentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate acrylate, isononyl (meth)acrylate, etc., which may be used alone or in combination. Two or more species can be used in combination.
[0031] In the present invention, the alkyl group having 1 to 24 carbon atoms at the ester terminal is Meth)acrylate is a monofunctional monomer component that forms a (meth)acrylic polymer. It is preferable that the content of the component (A) is 40% by weight or more, and more preferably 50% by weight or more, based on the total amount. It is more preferably 0% by weight or more.
[0032] The monomer component includes, as a monofunctional monomer component, the alkyl(meth)acrylate. The copolymerization monomer may contain a copolymerization monomer other than the copolymerization monomer. The alkyl (meth)acrylate may be used as the remainder of the alkyl (meth)acrylate.
[0033] The copolymerizable monomer may include, for example, a cyclic nitrogen-containing monomer. As the nitrogen-containing monomer, an unsaturated double bond such as a (meth)acryloyl group or a vinyl group can be used. and having a cyclic nitrogen structure can be used without any particular limitation. The cyclic nitrogen structure preferably has a nitrogen atom in the cyclic structure. Examples of the monomers that can be contained include N-vinylpyrrolidone and N-vinyl-ε-caprolactone. vinyl lactam monomers such as vinylpyridine, methylvinylpyrrolidone; Peridone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, Nitrogen-containing heterocycles such as nylimidazole, vinyloxazole, and vinylmorpholine Vinyl monomers and the like. Also, morpholine rings, piperidine rings, pyrrolidine rings, Examples of the (meth)acrylic monomer include a heterocyclic ring such as a piperazine ring. , N-Acryloylmorpholine, N-Acryloylpiperidine, N-Methacryloylpiperidine Among the cyclic nitrogen-containing monomers, lysine, N-acryloylpyrrolidine, etc. Of these, lactam vinyl monomers are preferred.
[0034] In the present invention, the cyclic nitrogen-containing monomer is a monomer that forms a (meth)acrylic polymer. The content of the functional monomer component is preferably 0.5 to 50% by weight, more preferably 0.5 to 50% by weight. The content is more preferably 40% by weight, and further preferably from 0.5 to 30% by weight.
[0035] The monomer components used in the present invention include, as monofunctional monomer components, hydroxyl group-containing The hydroxyl group-containing monomer may include (meth)acryloyl groups. and having a polymerizable functional group having an unsaturated double bond such as a hydroxyl group or a vinyl group. There are no particular limitations on the hydroxyl group-containing monomers that may be used. Examples of the acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropionate (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxy Cyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10 -Hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate Hydroxyalkyl (meth)acrylates such as 4-hydroxymethylcyclohexane Hydroxyalkylcycloalkane (meth)acrylate, such as hydroxyalkyl (meth)methyl (meth)acrylate Other examples include hydroxyethyl (meth)acrylamide, allyl alkenyl amide, Cole, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, Diethylene glycol monovinyl ether, etc. These may be used alone or in combination. Among these, hydroxyalkyl (meth)acrylates are preferred. .
[0036] In the present invention, the hydroxyl group-containing monomer is a (meth)acrylic polymer. 1% by weight based on the total amount of monofunctional monomer components to be formed in order to increase adhesive strength and cohesive strength It is preferably at least 2% by weight, more preferably at least 3% by weight. On the other hand, if the amount of the hydroxyl group-containing monomer is too large, the adhesive layer The adhesive may become too hard and lose its adhesive strength. Therefore, the hydroxyl group-containing monomer is preferably a (meth) hydroxyl group-containing monomer. The amount of the monofunctional monomer components forming the alkyl polymer is 30% by weight or less. It is preferably 27% by weight or less, more preferably 27% by weight or less, and even more preferably 25% by weight or less.
[0037] In addition, the monomer components forming the (meth)acrylic polymer include monofunctional monomers and In addition, other functional group-containing monomers may be included, for example, carboxyl group-containing monomers. Monomers having a cyclic ether group are also included.
[0038] The carboxyl group-containing monomer may be an unsaturated monomer such as a (meth)acryloyl group or a vinyl group. The polymerizable functional group having a monovalent double bond and a carboxyl group are particularly limited. The carboxyl group-containing monomer can be used without any need for (meth)acrylic acid. Acrylic acid, Carboxyethyl (meth)acrylate, Carboxypentyl (meth)acrylate Examples of the acid include glycerol, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. These may be used alone or in combination. Itaconic acid and maleic acid are anhydrides thereof. Among these, acrylic acid and methacrylic acid are preferred, and particularly Acrylic acid is preferred. The mer component may optionally contain a carboxyl group-containing monomer. The xyl group-containing monomer does not have to be used.
[0039] Examples of monomers having a cyclic ether group include monomers having a (meth)acryloyl group or a vinyl group. A compound having a polymerizable functional group having an unsaturated double bond and a ring such as an epoxy group or an oxetane group. There are no particular limitations on the epoxy group-containing monomer. Examples of the acrylates include glycidyl (meth)acrylate and 3,4-epoxycyclohexyl. Methyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ester Examples of the oxetane group-containing monomer include 3-oxetanyl Methyl (meth)acrylate, 3-methyl-oxetanyl methyl (meth)acrylate, 3-Ethyl-oxetanylmethyl (meth)acrylate, 3-Butyl-oxetanylmethyl 3-hexyl-oxetanylmethyl (meth)acrylate, 3-hexyl-oxetanylmethyl (meth)acrylate, etc. These can be used alone or in combination.
[0040] In the present invention, the carboxyl group-containing monomer and the monomer having a cyclic ether group is 30 to the total amount of the monofunctional monomer components forming the (meth)acrylic polymer. % by weight or less, more preferably 27% by weight or less, and even more preferably 25% by weight or less. Preferred.
[0041] The monomer components forming the (meth)acrylic polymer of the present invention include copolymerizable monomers and For example, CH2=C(R 1 )COOR 2 (The above R 1 is hydrogen or a methyl group, R 2 is carbon represents a substituted alkyl group or a cyclic cycloalkyl group having 1 to 3 carbon atoms; (meth)acrylate.
[0042] Here, R 2 As the substituent of the substituted alkyl group having 1 to 3 carbon atoms, An aryl group having 3 to 8 carbon atoms or an aryloxy group having 3 to 8 carbon atoms is preferred. The aryl group is not limited, but a phenyl group is preferred.
[0043] Such CH2=C(R 1 )COOR 2 Examples of monomers represented by the formula: Ethyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate Acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, Isoborone These may be used alone or in combination. .
[0044] In the present invention, the CH2=C(R 1 )COOR 2 The (meth)acrylate represented by 50 times the amount of the monofunctional monomer components forming the (meth)acrylic polymer. % by weight or less, preferably 45% by weight or less, and more preferably 40% by weight or less. It is preferably 35% by weight or less.
[0045] Other copolymerizable monomers include vinyl acetate, vinyl propionate, styrene, and α-methyl (meth)acrylate, Polyethylene glycol, (meth)acrylate Pyrene glycol, (meth)acrylate methoxyethylene glycol, (meth)acrylic acid Glycol-based acrylic ester monomers such as methoxy polypropylene glycol; Tetrahydrofurfuryl acrylate, fluorine (meth)acrylate, silicone (meth)acrylate p) Acrylic acid ester monomers such as acrylate and 2-methoxyethyl acrylate Amido group-containing monomers, amino group-containing monomers, imido group-containing monomers, N-acrylo Also usable are copolymerized monomers such as arylmorpholine and vinyl ether monomers. Mers include terpene (meth)acrylate and dicyclopentanyl (meth)acrylate. Monomers having a cyclic structure such as cyclic amines can be used.
[0046] Further, silane-based monomers containing silicon atoms can be used. Examples of the silane include 3-acryloxypropyltriethoxysilane and vinyltrimethoxysilane. silane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyl Triethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyl Triethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-a Cryloyloxydecyltrimethoxysilane, 10-Methacryloyloxydecyltriethylene Examples of the silane include 10-acryloyloxydecyltriethoxysilane and 10-acryloyloxydecyltriethoxysilane.
[0047] The monomer components forming the (meth)acrylic polymer of the present invention include the above-exemplified monofunctional monomers. In addition to the functional monomer, a polyfunctional monomer may be used as necessary to adjust the cohesive strength of the adhesive. It can contain.
[0048] The polyfunctional monomer has an unsaturated double bond such as a (meth)acryloyl group or a vinyl group. A monomer having at least two polymerizable functional groups, for example, (poly)ethylene glycol. Lithium di(meth)acrylate, (poly)propylene glycol di(meth)acrylate Neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate Acrylate, Pentaerythritol tri(meth)acrylate, Dipentaerythritol 1,2-ethylene glycol di(meth)acrylate, 1,6-Hexanediol di(meth)acrylate, 1,12-Dodecanediol di(meth)acrylate methacrylate, trimethylolpropane tri(meth)acrylate, tetramethylol Esters of polyhydric alcohols such as methyltri(meth)acrylate and (meth)acrylic acid Allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene Epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, hexyl di(meth)acrylate, etc. However, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate acrylate, dipentaerythritol hexa(meth)acrylate is preferably used. The polyfunctional monomers can be used alone or in combination of two or more. This can be done.
[0049] The amount of polyfunctional monomer used varies depending on the molecular weight and number of functional groups. It is preferable to use 3 parts by weight or less, and 2 parts by weight or less, based on 100 parts by weight of the total of the mers. More preferably, the amount is 1 part by weight or less, and even more preferably 1 part by weight or less. However, it is preferably 0 part by weight or more, and more preferably 0.001 part by weight or more. By using the polyfunctional monomer in an amount within the above range, the adhesive strength can be improved. can be done.
[0050] The (meth)acrylic polymer can be produced by a method using a radiation such as solution polymerization or ultraviolet (UV) polymerization. Any known production method such as radical polymerization, bulk polymerization, emulsion polymerization, etc. can be appropriately selected. The (meth)acrylic polymer obtained may be a random copolymer, a block copolymer, or A graft copolymer or the like may be used.
[0051] In the present invention, a partial polymer of the monomer component can also be suitably used. .
[0052] When the (meth)acrylic polymer is produced by radical polymerization, - Add polymerization initiators, chain transfer agents, emulsifiers, etc. used in radical polymerization to the components as appropriate. The polymerization initiator, the chain transfer agent, the emulsion, and the like used in the radical polymerization can be used. The curing agent and the like are not particularly limited and can be appropriately selected and used. The weight average molecular weight of the polymer can be controlled by the amount of polymerization initiator and chain transfer agent used and the reaction conditions. The amount of each of these substances used is adjusted according to their type.
[0053] For example, in solution polymerization, the polymerization solvent may be, for example, ethyl acetate or toluene. As a specific example of solution polymerization, the reaction is started under a stream of inert gas such as nitrogen. An initiator is added, and the reaction is usually carried out at about 50 to 70°C for about 5 to 30 hours.
[0054] Examples of thermal polymerization initiators used in solution polymerization include 2,2'-azobisisobutyrate. Tyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis( 2-Methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, 2,2'-Azobis(2-amidinopropane)dihydrochloride Lid, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane dihydrochloride, 2,2'-azobis(2-methylpropionamidine) disulfate Salt, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), 2,2'-azo Bis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate( Azo initiators such as VA-057 (manufactured by Wako Pure Chemical Industries, Ltd.); potassium persulfate, ammonium persulfate persulfates such as monium, di(2-ethylhexyl) peroxydicarbonate, di(4- t-Butylcyclohexyl) peroxydicarbonate, di-sec-butylperoxy Dicarbonate, t-butyl peroxy neodecanoate, t-hexyl peroxy piva t-Butyl peroxypivalate, dilauroyl peroxide, di-n-octyl Noyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexyl Sanoate, di(4-methylbenzoyl) peroxide, dibenzoyl peroxide, t -Butylperoxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane Peroxide initiators such as tert-butyl hydroperoxide and hydrogen peroxide, persulfates, Sodium bisulfite combination, sodium peroxide and sodium ascorbate combination Examples of the redox initiator include a combination of a peroxide and a reducing agent, such as However, the present invention is not limited to these.
[0055] The polymerization initiators may be used alone or in combination of two or more. It is preferably about 1 part by weight or less based on 100 parts by weight of the total amount of the monomer components, It is more preferable that the amount is about 0.005 to 1 part by weight, and more preferably about 0.02 to 0.5 parts by weight. It is even more preferable that
[0056] In addition, when 2,2'-azobisisobutyronitrile is used as the polymerization initiator, The amount of initiator used is about 0.2 parts by weight or less per 100 parts by weight of the total amount of monomer components. It is preferable that the amount is about 0.06 to 0.2 parts by weight.
[0057] Examples of the chain transfer agent include lauryl mercaptan, glycidyl mercaptan, mercaptan, Mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethyl thioglycolate The chain transfer agent may be, for example, 2,3-dimercapto-1-propanol, 2,3-dimercapto-1-propanol, etc. They may be used alone or in combination of two or more kinds, but the total content is about 0.3 parts by weight or less relative to 100 parts by weight of the total amount of the monomer components.
[0058] Examples of emulsifiers used in emulsion polymerization include sodium lauryl sulfate, Ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, polyoxyethylene Ammonium polyoxyethylene alkyl ether sulfate, polyoxyethylene alkyl phenyl ether sulfate Anionic emulsifiers such as sodium acetate, polyoxyethylene alkyl ethers, polyoxyethylene Ethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, polyoxyethylene Examples of the emulsifier include nonionic emulsifiers such as ethylene-polyoxypropylene block polymers. These emulsifiers may be used alone or in combination of two or more kinds.
[0059] Furthermore, as the reactive emulsifier, radical polymerizable functional groups such as propenyl groups and allyl ether groups may be used. Specific examples of emulsifiers having functional groups introduced therein include Aqualon HS-10 and HS-2. 0, KH-10, BC-05, BC-10, BC-20 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (manufactured by ADEKA Co., Ltd.), and Adeka Reasoap SE10N (manufactured by ADEKA Co., Ltd.). The amount of emulsifier used is The amount is preferably 5 parts by weight or less relative to 100 parts by weight of the total amount of the monomer components.
[0060] In addition, when the (meth)acrylic polymer is produced by radiation polymerization, It is produced by polymerizing the monomer component by irradiating it with electron beams, ultraviolet (UV) rays, etc. Among these, ultraviolet polymerization is preferred. Next, ultraviolet polymerization, which is a new embodiment, will be described.
[0061] When performing UV polymerization, the monomer components are It is preferable to incorporate a photopolymerization initiator in the composition. Therefore, when carrying out ultraviolet polymerization, for example, The monomer component containing the alkyl (meth)acrylate and / or the monomer component A UV-curable acrylic adhesive composition containing a partial polymer of the above, an UV absorber, and a photopolymerization initiator. It is preferable that the ultraviolet-curable acrylic resin composition is polymerized by ultraviolet light. The adhesive layer formed by ultraviolet polymerization of the adhesive composition has a thickness of 150 μm or more. This is preferable because it is possible to form adhesive layers of various thicknesses. stomach.
[0062] The photopolymerization initiator may be a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more. When the pressure-sensitive adhesive composition contains an ultraviolet absorbing agent, the ultraviolet polymerization If this is done, the ultraviolet light will be absorbed by the ultraviolet absorber and the polymerization will not be sufficient. However, if the photoinitiator (A) has an absorption band at wavelengths of 400 nm or more, It is preferable to use such a composition since it can be sufficiently polymerized despite containing an ultraviolet absorber.
[0063] The photopolymerization initiator (A) having an absorption band of 400 nm or more is, for example, bis(2,4,6 -Trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819 , manufactured by BASF), 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxa Examples of such copolymers include LUCIRIN TPO (manufactured by BASF).
[0064] The photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more may be used alone. It is also possible to use two or more of them in combination.
[0065] The amount of the photopolymerization initiator (A) having an absorption band at wavelengths of 400 nm or more is particularly Although not limited thereto, it is preferable that the amount is less than the amount of the ultraviolet absorbing agent to be added, which will be described later. , relative to 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer, The amount is preferably about 0.005 to 1 part by weight, and more preferably about 0.02 to 0.5 parts by weight. It is more preferable that the amount of the photopolymerization initiator (A) added is within the above range. This is preferable since it allows sufficient progress.
[0066] The photopolymerization initiator may include a photopolymerization initiator having an absorption band at a wavelength of less than 400 nm (B The photopolymerization initiator (B) may contain an absorption band at a wavelength of 400 nm or more. It is preferable that the photopolymerization initiator (B) does not have a radical-generating property when exposed to ultraviolet light. It is generated and initiates photopolymerization, and has an absorption band at wavelengths of less than 400 nm. There is no particular limitation as long as the photopolymerization initiator is used, and any photopolymerization initiator that is commonly used can be suitably used. For example, benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-keto Toluene-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, Benzylic photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thio By using a xanthone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, etc. This can be done.
[0067] Specifically, the benzoin ether-based photopolymerization initiator is, for example, benzoin methyl Ether, Benzoin Ethyl Ether, Benzoin Propyl Ether, Benzoin Isopropyl Ether Benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenyl ether methyl ethene, anisole methyl ether, etc.
[0068] Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone. , 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl Phenyl ketone, 4-phenoxydichloroacetophenone, 4-t-butyldichloroacetophenone Fenone et al. can be done.
[0069] Examples of α-ketol photopolymerization initiators include 2-methyl-2-hydroxypropionate. phenone, 1-[4-(2-hydroxyethyl)phenyl]-2-hydroxy-2-methyl propan-1-one, etc.
[0070] Examples of photoactive oxime-based photopolymerization initiators include 1-phenyl-1,2-propanediol. 2-(O-ethoxycarbonyl)-oxime and the like.
[0071] An example of the benzoin-based photopolymerization initiator is benzoin.
[0072] The benzyl-based photopolymerization initiator includes, for example, benzyl.
[0073] Benzophenone-based photopolymerization initiators include, for example, benzophenone, benzoylbenzoic acid, 3,3'-Dimethyl-4-methoxybenzophenone, Polyvinylbenzophenone, α-Hydroxybenzophenone hydroxycyclohexyl phenyl ketone, etc.
[0074] Ketal-based photopolymerization initiators include benzyl dimethyl ketal and the like.
[0075] Thioxanthone-based photopolymerization initiators include, for example, thioxanthone and 2-chlorothioxane. thioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone Xanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2, These include 4-diisopropylthioxanthone, dodecylthioxanthone, and the like.
[0076] Acylphosphine oxide photopolymerization initiators include, for example, 2,4,6-trimethyl Benzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl) phenylphosphine oxide, etc.
[0077] The photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm may be used alone or in combination of two or more. The photopolymerization method having an absorption band at a wavelength of less than 400 nm can be used in combination. The initiator (B) can be added in an amount not impairing the effects of the present invention. For 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer, The amount is preferably about 0.005 to 0.5 parts by weight, and more preferably about 0.02 to 0.1 parts by weight. It is more preferable that:
[0078] In the present invention, when the monomer component is polymerized by ultraviolet light, the monomer component is subjected to ultraviolet light. A photopolymerization initiator (B) having an absorption band of less than 400 nm is added first, and then ultraviolet light is irradiated. The partially polymerized monomer component (prepolymer composition) was subjected to irradiation with the above-mentioned 400 nm wavelength light. Add a photopolymerization initiator (A) having an absorption band above m and a UV absorber to polymerize with UV light. It is preferable to use a partially polymerized monomer component (prepolymer) that is partially polymerized by irradiating ultraviolet rays. (a) a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more is added to the composition. In this case, it is preferable to add the photopolymerization initiator after dissolving it in the monomer.
[0079] (1-2) Ultraviolet absorbers The ultraviolet absorbing agent contained in the acrylic pressure-sensitive adhesive composition is not particularly limited, but may be For example, triazine-based UV absorbers, benzotriazole-based UV absorbers, benzophenone-based UV absorbers, UV absorbers based on benzophenone, UV absorbers based on salicylic acid Examples of the ultraviolet absorbing agent include a cyanoacrylate-based ultraviolet absorbing agent. Or two or more of them can be used in combination. Among these, triazine-based ultraviolet The absorbent is preferably a benzotriazole-based ultraviolet absorbent, and has two hydroxyl groups in one molecule. Triazine-based ultraviolet absorbers having one or less benzotriazole skeletons in one molecule At least one selected from the group consisting of benzotriazole-based ultraviolet absorbers The fact that it is an ultraviolet absorber makes it easy to dissolve in the monomers used to form the acrylic adhesive composition. This is preferred because it has good dissolving ability and high ultraviolet absorbing ability at a wavelength of about 380 nm.
[0080] Triazine-based ultraviolet absorbers having two or less hydroxyl groups in one molecule include, specifically, Specifically, 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy]-furan phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (Tinosorb S, manufactured by BASF), 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-( 2,4-dibutoxyphenyl)-1,3,5-triazine (TINUVIN 460, B ASF), 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (C10-C16 (mainly C12-C1 3) Reaction products with alkyloxy)methyl]oxirane (TINUVIN400, BA SF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine -2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol ), 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl) Reaction products of (2-ethylhexyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester Composition (TINUVIN 405, manufactured by BASF), 2-(4,6-diphenyl-1,3,5- Triazin-2-yl)-5-[(hexyl)oxy]-phenol (TINUVIN1 577, manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl )-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADK S TAB LA46, manufactured by ADEKA), 2-(2-hydroxy-4-[1-octyloxy Carbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5 -triazine (TINUVIN 479, manufactured by BASF) and the like.
[0081] In addition, benzotriazole-based ultraviolet absorbing compounds having one benzotriazole skeleton per molecule are The collector is 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1- Phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (TINU VIN 928, manufactured by BASF), 2-(2-hydroxy-5-tert-butylphenyl )-2H-benzotriazole (TINUVIN PS, manufactured by BASF), benzenepropanol Acid and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl ETHER COMPOUNDS (TINU)-4-HYDROXY(C7-9 SIDE CHAIN AND STRAIGHT CHAIN ALKYL) VIN384-2, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4, 6-Bis(1-methyl-1-phenylethyl)phenol (TINUVIN900, BA SF), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenyl (1,1,3,3-tetramethylbutyl)phenol (TINUVI N928, manufactured by BASF), methyl-3-(3-(2H-benzotriazol-2-yl) -5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol Reaction product of 300 (TINUVIN 1130, manufactured by BASF), 2-(2H-benzotriazole) Azol-2-yl)-p-cresol (TINUVIN P, manufactured by BASF), 2(2H -benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl) Phenol (TINUVIN234, manufactured by BASF), 2-[5-chloro(2H)-benzo[ Triazol-2-yl]-4-methyl-6-(tert-butyl)phenol (TIN UVIN326, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6 -Di-tert-pentylphenol (TINUVIN328, manufactured by BASF), 2-(2 H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl) phenol (TINUVIN329, manufactured by BASF), methyl 3-(3-(2H-benzotriazole) Azol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate Reaction product of ethylene glycol 300 with TINUVIN 213 (BASF) ), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (TINUVIN 571, manufactured by BASF), 2-[2-hydroxy-3-(3,4,5, 6-Tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole ( Sumisorb 250 (manufactured by Sumitomo Chemical Co., Ltd.) and the like.
[0082] In addition, the benzophenone-based ultraviolet absorbers (benzophenone-based compounds) and oxybenzo Examples of phenone-based ultraviolet absorbers (oxybenzophenone-based compounds) include 2,4- Dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy 4-Methoxy-4-benzophenone-5-sulfonic acid (anhydrous and trihydrate), 2-Hydroxy 4-Octyloxybenzophenone, 4-Dodecyloxy-2-hydroxybenzophenone Phenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2´,4,4´- Tetrahydroxybenzophenone, 2,2´-dihydroxy-4,4-dimethoxybenzo Phenone and the like.
[0083] The salicylic acid ester-based ultraviolet absorber (salicylic acid ester-based compound) may also be For example, phenyl-2-acryloyloxybenzoate, phenyl-2-acryloyl phenyl-2-acryloyloxy-4-methylbenzoate benzoate, phenyl-2-acryloyloxy-5-methylbenzoate, phenyl- 2-Acryloyloxy-3-methoxybenzoate, Phenyl-2-hydroxybenzoate , phenyl-2-hydroxy-3-methylbenzoate, phenyl-2-hydroxy Phenyl-4-hydroxy-5-methylbenzoate, phenyl-2-hydroxy-5-methylbenzoate, Nyl 2-hydroxy-3-methoxybenzoate, 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate (TINUVIN12 0, manufactured by BASF).
[0084] Examples of the cyanoacrylate-based ultraviolet absorber (cyanoacrylate-based compound) include For example, alkyl-2-cyanoacrylate, cycloalkyl-2-cyanoacrylate, Alkoxyalkyl-2-cyanoacrylate, alkenyl-2-cyanoacrylate, Alkynyl-2-cyanoacrylate and the like can be mentioned.
[0085] Furthermore, as an ultraviolet absorbing agent, for example, a product name "FDB-001" (Yamada Chemical Co., Ltd.) (manufactured by Hayashibara Co., Ltd.), product name "SMP-122" (manufactured by Hayashibara Co., Ltd.), azomethine compound (product name: BON ASORB UA-3911, manufactured by Orient Chemical Industry Co., Ltd.), indole chemicals (product Name: BONASORB UA-3701, manufactured by Orient Chemical Industry Co., Ltd., Disper se Yellow54 (Product name: KAYASET YELLOW AG, Nippon Kayaku Co., Ltd. )), quinophthalone compound (product name: MS YELLOW HD-137, Yamada Chemical Industries, Ltd. (Manufactured by Nippon Paint Holdings Co., Ltd.), Solvent Yellow 93 (PLASTYELLOW 8000 , Arimoto Chemical Industry Co., Ltd.), Solvent Yellow 163 (KP Plast Yellow MK (manufactured by Kiwa Chemical Industry Co., Ltd.) or other dyes can also be used.
[0086] The ultraviolet absorbents may be used alone or in combination of two or more. However, the total content is the monofunctional monomer components that form the (meth)acrylic polymer. The amount is preferably about 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, based on 100 parts by weight of the component. By setting the amount of the ultraviolet absorbing agent to the above range, the adhesiveness can be improved. In the case of ultraviolet polymerization, the ultraviolet absorbing function of the agent layer can be fully exhibited. This is preferable since it does not interfere with the polymerization.
[0087] (1-3) Silane coupling agents Furthermore, the acrylic pressure-sensitive adhesive composition used in the present invention contains a silane coupling agent. The amount of the silane coupling agent to be blended is determined based on the amount of the (meth)acrylic polymer to be formed. It is preferably 1 part by weight or less per 100 parts by weight of the monofunctional monomer component, and more preferably 0.0 The amount is more preferably 1 to 1 part by weight, and further preferably 0.02 to 0.6 part by weight.
[0088] Examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane. Silane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyl Diethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane Epoxy group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N -2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxy Diphenyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-γ- Amino group-containing silane coupling agents such as aminopropyltrimethoxysilane, 3-acryloyl 3-Methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. (Meth)acrylic group-containing silane coupling agent, 3-isocyanate propyl triethoxy Examples of the silane coupling agent include isocyanate group-containing silane coupling agents such as silane.
[0089] (1-4) Crosslinking agent The acrylic pressure-sensitive adhesive composition used in the present invention may contain a crosslinking agent. Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, silicone-based crosslinking agents, and oxazolidinyl crosslinking agents. Aziridine-based crosslinking agents, silane-based crosslinking agents, alkyl etherified melamine-based crosslinking agents Crosslinking agents include crosslinking agents such as crosslinkers, metal chelate crosslinkers, and peroxides. Two or more of these may be combined. Among these, isocyanate-based crosslinking agents are preferred. It is often used.
[0090] The above crosslinking agents may be used alone or in combination of two or more. The total content is the monofunctional monomer component that forms the (meth)acrylic polymer. It is preferably 5 parts by weight or less, and more preferably 0.01 to 5 parts by weight, per 100 parts by weight. More preferably, the amount is 0.01 to 4 parts by weight, and even more preferably, the amount is 0.02 to 3 parts by weight. I wish.
[0091] Isocyanate-based crosslinking agents are used to block isocyanate groups (isocyanate groups) Contains two isocyanate regenerating functional groups temporarily protected by polymerization, etc., in one molecule. The isocyanate crosslinking agent is tolylene diisocyanate. , aromatic isocyanates such as xylylene diisocyanate, isophorone diisocyanate, etc. Alicyclic isocyanates, aliphatic isocyanates such as hexamethylene diisocyanate, etc. Examples include:
[0092] More specifically, for example, butylene diisocyanate, hexamethylene diisocyanate lower aliphatic polyisocyanates such as cyclopentene diisocyanate, cyclohexene diisocyanate, Alicyclic isocyanates such as xylylene diisocyanate and isophorone diisocyanate; 2,4-Tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, Aromatic diisocyanates such as silylene diisocyanate and polymethylene polyphenyl isocyanate Cyanates, trimethylolpropane / tolylene diisocyanate trimer adduct (product Name: Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd., trimethylolpropane / hexa Methylene diisocyanate trimer adduct (product name: Coronate HL, Nippon Polyurethane Industry Co., Ltd.) (Product name: Coronet) Isocyanate adducts such as xylylenediamine (HX, Nippon Polyurethane Industry Co., Ltd.) Socyanate trimethylolpropane adduct (product name: D110N, manufactured by Mitsui Chemicals, Inc.) ), Hexamethylene diisocyanate trimethylolpropane adduct (product name: D16 0N, Mitsui Chemicals, Inc.); Polyether polyisocyanate, polyester polyisocyanate Anates and their adducts with various polyols, isocyanurate bonds, butylene glycol Examples of the polyisocyanates include polyfunctionalized polyisocyanates with isopropyl bonds, allophanate bonds, etc. can be done.
[0093] (1-5) Other additives In addition to the above-mentioned components, the acrylic adhesive composition used in the present invention may contain appropriate Additives may be included. For example, tackifiers (e.g., rosin derivative resins, polytetrafluoroethylene). Solid, semi-solid, or non-solid at room temperature, consisting of ruthenium resin, petroleum resin, oil-soluble phenolic resin, etc. liquids); hollow glass balloons and other fillers; plasticizers; antioxidants; antioxidants, etc. Can be obtained.
[0094] (1-6) Method for forming visible side adhesive layer In the present invention, the acrylic pressure-sensitive adhesive composition has a viscosity suitable for application to a substrate. The viscosity of the acrylic pressure-sensitive adhesive composition is preferably adjusted to a desired degree by, for example, adding a thickening additive. Addition of various polymers such as additives and polyfunctional monomers, and addition of monofunctional monomers in acrylic adhesive compositions The partial polymerization is carried out by partially polymerizing the mer component. This may be carried out before or after the addition of the seed polymer, the polyfunctional monomer, etc. The viscosity of the acrylic adhesive composition varies depending on the amount of additives, etc. The polymerization rate when the monomer components in the agent composition are partially polymerized cannot be uniquely determined. However, as a guideline, it is preferable that the ratio is about 20% or less, and more preferably about 3 to 20%. More preferably, the content is about 5 to 15%. If the content exceeds 20%, the viscosity becomes too high. It becomes difficult to apply to materials.
[0095] The visible-side pressure-sensitive adhesive layer is formed by applying the acrylic pressure-sensitive adhesive composition to at least one surface of a substrate. The coating film formed from the acrylic pressure-sensitive adhesive composition is dried, or is irradiated with ultraviolet light or the like. The film can be formed by irradiating the film with active energy rays.
[0096] The substrate is not particularly limited, and examples thereof include a release film, a transparent resin film, and the like. Various substrates such as a film substrate and a polarizing film described later can also be suitably used as the substrate. When the visible-side pressure-sensitive adhesive layer is formed on a substrate other than a polarizing film, the visible-side pressure-sensitive adhesive layer can be transferred by laminating it onto a polarizing film.
[0097] The material of the release film may be, for example, polyethylene, polypropylene, or polypropylene. Resin films such as ethylene terephthalate and polyester films, paper, cloth, nonwoven fabric, etc. Appropriate thin materials such as porous materials, nets, foam sheets, metal foils, and laminates thereof However, a resin film is preferably used because of its excellent surface smoothness. .
[0098] The resin film may be, for example, a polyethylene film or a polypropylene film. , polybutene film, polybutadiene film, polymethylpentene film, polysalt Vinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film , polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate Copolymer films and the like.
[0099] The thickness of the release film is usually 5 to 200 μm, and preferably about 5 to 100 μm. The release film may contain, as required, a silicone-based, fluorine-based, long-chain alkyl, Release agents such as oleyl or fatty acid amide release agents, release and antifouling treatments using silica powder, etc., coating types, It is also possible to carry out antistatic treatment such as kneading or deposition. By appropriately performing release treatment such as silicone treatment, long chain alkyl treatment, fluorine treatment, etc. on the surface, This can further improve the releasability from the pressure-sensitive adhesive layer.
[0100] The transparent resin film substrate is not particularly limited, but may be any of various resins having transparency. A film is used. The resin film is formed of a single layer of film. For example, For example, the material may be polyethylene terephthalate, polyethylene naphthalate, or the like. Ester resin, acetate resin, polyethersulfone resin, polycarbonate resin Resin, polyamide resin, polyimide resin, polyolefin resin, (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, poly Vinyl alcohol resin, polyarylate resin, polyphenylene sulfide resin, etc. Among these, polyester resins and polyimide resins are particularly preferred. and polyethersulfone resin.
[0101] The thickness of the film substrate is preferably 15 to 200 μm, and more preferably 25 to 188 μm. It is more preferable that m.
[0102] The method for applying the acrylic pressure-sensitive adhesive composition onto the substrate is a roll coating method, a kissro method, or the like. Le coat, gravure coat, reverse coat, roll brush, spray coat, direct roll coat, bar coat, knife coat, air knife coat, curtain coat, Any known suitable method such as lip coating or die coating can be used without any particular limitation.
[0103] The visible side pressure-sensitive adhesive layer is formed by drying a coating film formed from the acrylic pressure-sensitive adhesive composition. In this case, the drying conditions (temperature, time) are not particularly limited, and the pressure-sensitive adhesive composition The temperature can be appropriately set depending on the composition, concentration, etc. of the catalyst. For example, the temperature is preferably about 60 to 170° C. The heating is carried out at a temperature of 60 to 150° C. for 1 to 60 minutes, preferably 2 to 30 minutes.
[0104] The acrylic pressure-sensitive adhesive composition is an ultraviolet-curable acrylic pressure-sensitive adhesive composition, When a coating film formed from an ultraviolet-curable acrylic adhesive composition is irradiated with ultraviolet light, In this case, the illuminance of the ultraviolet light is 5mW / cm 2 The illuminance of the ultraviolet light is preferably 5m or more. W / cm 2 If the polymerization time is less than 10 minutes, the polymerization reaction time becomes long, and the productivity may be poor. The UV light intensity is 200mW / cm 2 The illuminance of the ultraviolet light is preferably 200mW / cm 2 If the polymerization temperature exceeds this limit, the photoinitiator is rapidly consumed, causing the polymer to degrade in molecular weight. In particular, the retention strength may decrease at high temperatures. Also, the cumulative amount of ultraviolet light is 100 mJ / cm 2 ~5000mJ / cm 2 It is preferable that:
[0105] The ultraviolet lamp used in the present invention is not particularly limited, but an LED lamp is preferred. LED lamps emit less heat than other UV lamps, so they are more viscous. The temperature during polymerization of the adhesive layer can be suppressed, so that the molecular weight of the polymer can be prevented from decreasing. This prevents the cohesive strength of the adhesive layer from decreasing, and when used as an adhesive sheet, it can be maintained at high temperatures. It is also possible to combine multiple UV lamps. In addition, ultraviolet light is irradiated intermittently, and a light period in which ultraviolet light is irradiated and a dark period in which ultraviolet light is not irradiated are separated. It can also be set up.
[0106] In the present invention, the final polymerization of the monomer components in the ultraviolet-curable acrylic pressure-sensitive adhesive composition The ratio is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more.
[0107] In the present invention, the peak of the ultraviolet light irradiated to the ultraviolet-curable acrylic pressure-sensitive adhesive composition is The wavelength is preferably in the range of 200 to 500 nm, and more preferably in the range of 300 to 450 nm. It is more preferable that the peak wavelength of the ultraviolet light is within 500 nm. The agent may not decompose and the polymerization reaction may not start. If it is less than m, the polymer chain may be broken, resulting in a decrease in adhesive properties.
[0108] The reaction is inhibited by oxygen in the air, so to block oxygen, UV-curable acrylic is used. A release film is formed on the coating film formed from the pressure-sensitive adhesive composition, and a photopolymerization reaction is suppressed. It is preferable to carry out the process under a vacuum atmosphere. In addition, when a release film is used, the release film can be directly attached to the pressure-sensitive adhesive layer. It can be used as a separator for a polarizing film with a polarizing film.
[0109] In addition, the ultraviolet-curable acrylic pressure-sensitive adhesive composition used in the present invention contains a photopolymerization initiator (B). In the case where it is contained, the monomer component containing alkyl (meth)acrylate and the photopolymerization initiator are A composition containing initiator (B) (sometimes called a "pre-added polymerization initiator") is irradiated with ultraviolet light. a partial polymer of the monomer component is formed, and the partial polymer of the monomer component is subjected to ultraviolet ray absorption and a photoinitiator (A) having an absorption band of 400 nm or more ("Post-addition polymerization initiator" An ultraviolet-curable acrylic adhesive composition is prepared by adding a UV-curable acrylic adhesive agent. The polymerization rate of the partial polymer is preferably about 20% or less, and more preferably 3 to 2 The ultraviolet irradiation conditions are as described above. That is correct.
[0110] As described above, the ultraviolet-curable acrylic pressure-sensitive adhesive composition containing the photopolymerization initiator (B) is When forming a pressure-sensitive adhesive layer, the monomer components are polymerized in two steps as described above. The adhesive layer can be formed by the above-mentioned method, and the ultraviolet absorbing function of the adhesive layer can be improved. It is possible.
[0111] The thickness of the pressure-sensitive adhesive layer on the viewing side is determined based on the polarizing filter described below in order to ensure the ultraviolet absorbing function. The thickness of the adhesive layer on the image display side of the film (adhesive layer on the image display side) must be at least twice as thick. It is preferable that the ratio is 5 times or more, and it is even more preferable that the ratio is 10 times or more. Specifically, the thickness of the visible side pressure-sensitive adhesive layer is preferably 50 μm or more, and more preferably 10 It is more preferable that the thickness is 0 μm or more, and further more preferable that the thickness is 150 μm or more. The upper limit of the thickness of the adhesive layer on the receiving side is not particularly limited, but it is preferably 10 mm or less. If the thickness of the adhesive layer exceeds 10 mm, it becomes difficult for ultraviolet rays to penetrate, and the polymerization of the monomer components This is not preferable because it takes a long time to complete the process and may result in poor productivity.
[0112] The gel fraction of the visible side pressure-sensitive adhesive layer of the present invention is not particularly limited, but is preferably 35% or more. It is preferable that the ratio is 50% or more, more preferable that the ratio is 75% or more. It is more preferable that the gel fraction of the visible-side pressure-sensitive adhesive layer is 85% or more, and particularly preferable that the gel fraction of the visible-side pressure-sensitive adhesive layer is 85% or more. If it is too small, the cohesive strength may be poor, and if it is too large, the adhesive strength may be poor.
[0113] The transmission b* value of the visible side pressure-sensitive adhesive layer is not particularly limited, but is preferably 3.0 or less. It is preferable that the ratio is 1.5 or less, and more preferable that the ratio is 0.5 or less. The above b* value is the b* value in the L*a*b* color system conforming to JIS Z8729 ( For example, a spectrophotometer (product name: U4100, Hitachi High-Technologies Corporation) Measurements can be performed using a fluoroscopy (manufactured by FUJIFILM Corporation).
[0114] The transmittance of the pressure-sensitive adhesive layer on the viewing side at a wavelength of 380 nm is preferably 9% or less. It is more preferable that the ratio is 7% or less, and further preferably 5% or less, and more preferably 3% or less. It is particularly preferable that the transmittance at a wavelength of 380 nm is within the above range. This allows for a high degree of blocking of incoming ultraviolet light, making it ideal for use in LCD panels and organic EL devices. This can significantly suppress the deterioration of optical members such as polarizers.
[0115] The transmittance of the pressure-sensitive adhesive layer on the viewing side at a wavelength of 400 nm is preferably 60% or more. It is preferable that the wavelength is 70% or more, and more preferable that the wavelength is 75% or more. By having the transmittance at 00 nm in the above range, the incident visible light is sufficiently transmitted. This is preferable because sufficient visibility can be ensured in the image display device.
[0116] In addition, when the pressure-sensitive adhesive layer-attached polarizing film of the present invention is used in an organic electroluminescence display device (OLED), The transmittance of the pressure-sensitive adhesive layer on the viewing side at a wavelength of 420 nm is preferably 75% or less. It is preferably 50% or less, and more preferably 40% or less. By setting the transmittance at a wavelength of 420 nm within the above range, it is possible to protect the light emitting element of the OLED. It is preferable from the viewpoint.
[0117] When the visible side pressure-sensitive adhesive layer is exposed, the pressure-sensitive adhesive layer is covered with a release film until it is put into practical use. The release film may be used as it is for protecting the separator of the pressure-sensitive adhesive layer-attached polarizing film. This can be used as a regulator, simplifying the process.
[0118] (2) Adhesive layer on the image display side The adhesive layer on the image display portion side surface of the polarizing film (adhesive layer on the image display portion side) is particularly The adhesive layer may be formed of the same acrylic adhesive composition as described above in detail for the visible side adhesive layer. Various commonly used pressure-sensitive adhesive layers may be used.
[0119] A suitable adhesive can be used to form the adhesive layer on the image display unit side surface. There are no particular limitations on the adhesive. Examples of adhesives include rubber adhesives, acrylic adhesives, silicone adhesives, etc. Adhesives based on acrylic acid, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol Polyvinylpyrrolidone adhesives, polyacrylamide adhesives, cellulose Among these adhesives, those with excellent optical transparency, suitable adhesion, and Acrylic adhesives are popular because they exhibit cohesive and adhesive properties and are excellent in weather resistance and heat resistance. The agent is preferably used.
[0120] Acrylic adhesives are based on the monomer unit of (meth)acrylic acid alkyl ester. The base polymer is an acrylic polymer that is a major component of the polymer chain. As the (meth)acrylic acid alkyl ester, an acrylic acid alkyl ester that forms the visible side adhesive layer is used. The same ones as those used in the copolymer-based pressure-sensitive adhesive composition can be mentioned. The monomers and their ratios may be the same as those used in the acrylic pressure-sensitive adhesive composition. It is possible.
[0121] The acrylic polymer can be produced by various known methods, for example, bulk polymerization. Radical polymerization methods such as polymerization, solution polymerization, suspension polymerization, etc. can be appropriately selected. As the reaction agent, various known azo and peroxide-based agents can be used. The reaction temperature is usually 50 The reaction temperature is about 1 to 80°C and the reaction time is 1 to 8 hours. As a solvent for an acrylic polymer, ethyl acetate, toluene, etc. are generally used. The solution concentration is usually about 20 to 80% by weight.
[0122] The pressure-sensitive adhesive may be a pressure-sensitive adhesive composition containing a crosslinking agent. As the crosslinking agent, those mentioned above can be mentioned, but isocyanate-based crosslinking agents are particularly preferred. The blending ratio of the acrylic polymer and the crosslinking agent is not particularly limited, but is usually an acrylic polymer ( The crosslinking agent (solid content) is about 0.001 to 20 parts by weight per 100 parts by weight of the solid content. and more preferably about 0.01 to 15 parts by weight.
[0123] Furthermore, the adhesive may contain, as necessary, a tackifier, a plasticizer, glass fiber, glass Fillers made of beads, metal powders, other inorganic powders, etc., pigments, colorants, fillers, antioxidants agents, ultraviolet absorbers, silane coupling agents, etc., within the scope of the present invention. Various additives can be appropriately used. The silane coupling agent may be any of those mentioned above.
[0124] The pressure-sensitive adhesive layer on the image display section side is formed by applying the pressure-sensitive adhesive composition to a polarizing film, a release film, or the like. The adhesive layer is applied to various substrates such as release films and dried. When the pressure-sensitive adhesive layer is formed on the polarizing film, the pressure-sensitive adhesive layer can be transferred by being attached to the polarizing film. The pressure-sensitive adhesive coating method and the various substrates are the same as those of the acrylic pressure-sensitive adhesive composition coating method and the various substrates. The same materials as those for the substrate can be used.
[0125] In the coating step, the adhesive layer is formed to a predetermined thickness (thickness after drying). The thickness of the pressure-sensitive adhesive layer on the image display section side is not particularly limited. However, it is preferable that the thickness is 1 / 2 or less of the thickness of the visible side adhesive layer, and is 1 / 5 or less. The thickness of the pressure-sensitive adhesive layer on the image display section side is preferably 1 / 10 or less. Generally, the thickness is preferably about 1 to 100 μm, and more preferably about 3 to 50 μm. A thickness of about 5 to 30 μm is more preferable.
[0126] In forming the image display section side adhesive layer, the applied adhesive is dried. The drying temperature and drying time are not particularly limited and are set appropriately. For example, The temperature is preferably about 200° C. for 0.5 to 10 minutes.
[0127] When the pressure-sensitive adhesive layer on the image display section side is exposed, the pressure-sensitive adhesive layer is adhered with a release film until it is used in practice. The release film may be used as it is for the pressure-sensitive adhesive layer-attached polarizing film. This can be used as a separator, which can simplify the process.
[0128] (3) Polarizing film The polarizing film used in the present invention has a polarizer and transparent protective films on both sides of the polarizer. The transparent protective film on the viewing side of the polarizer (visual side transparent protective film) is The transmittance in the optical fiber is characterized by being less than 6%.
[0129] (3-1) Transparent protective film on the viewing side The transmittance of the visible-side transparent protective film used in the present invention at a wavelength of 380 nm is less than 6%. and is preferably 3% or less, more preferably 2% or less, and is preferably 1% or less. In the present invention, the transmittance at a wavelength of 380 nm is more preferably 6%. The visible-side transparent protective film is less than 100% by weight, and the visible-side pressure-sensitive adhesive layer (containing an ultraviolet absorbing agent) is combined. By combining these two materials, it is possible to achieve a higher level of ultraviolet absorption capability. In addition, the lower limit of the transmittance of the visible-side transparent protective film at a wavelength of 380 nm is not particularly limited. It is not essential that the size of the pores is large, and the smaller the size, the more preferable it is from the viewpoint of the ultraviolet absorbing function.
[0130] The material for forming the visible side transparent protective film is required to have transparency, mechanical strength, thermal stability, and water resistance. It is preferable to use a material that has excellent polarization blocking properties and isotropy. For example, polyethylene terephthalate or Polyester polymers such as polyethylene naphthalate, diacetyl cellulose, triacetate, etc. cellulose-based polymers such as ethyl cellulose, acrylic polymers such as polymethyl methacrylate, Styrene such as polystyrene and acrylonitrile-styrene copolymer (AS resin) Polyethylene, polypropylene, polycarbonate, etc. Polyolefins having cyclo- or norbornene structures, ethylene / propylene Pyrene copolymers and other polyolefin polymers, vinyl chloride polymers, nylon and aromatics Amide-based polymers such as aromatic polyamides, imide-based polymers, sulfone-based polymers, polyethersulfones, etc. Tersulfone polymers, polyetheretherketone polymers, polyphenylene sulfonates vinyl chloride polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl bromide polymers, Chiral polymers, arylate polymers, polyoxymethylene polymers, epoxy The polymer forming the transparent protective film may be a polymer based on the above-mentioned polymer or a blend of the above-mentioned polymers. Examples of transparent protective films include acrylic, urethane, and acrylic urethane. As a hardening layer for thermosetting and UV-curing resins such as urethane, epoxy, and silicone. Among these, the visible side transparent protective film is preferably triacetyl. cellulose film, acrylic film (film using acrylic polymer), Polyethylene terephthalate film and poly(ethylene terephthalate) film having a cyclo- or norbornene structure At least one film selected from the group consisting of polyolefin films. A triacetyl cellulose film is preferred, and a triacetyl cellulose film is more preferred.
[0131] The thickness of the visible-side transparent protective film is not particularly limited, but is preferably 40 μm or less. It is preferable that the thickness is 35 μm or less, more preferable that the thickness is 30 μm or less. The lower limit of the thickness of the visible side transparent protective film is not particularly limited, but is preferably 1 μm or more. When the thickness of the viewer-side transparent protective film is in the above range, the polarizing film This is preferable because it allows the film to be sufficiently thin and does not impair the protective function of the polarizer. stomach.
[0132] The polarizer and the viewing side protective film described later are preferably bonded to each other via a water-based adhesive or the like. Water-based adhesives include isocyanate adhesives, polyvinyl alcohol adhesives, Examples include gelatin adhesives, vinyl latex adhesives, water-based polyurethane, and water-based polyester. In addition to the above, the adhesive between the polarizer and the visible-side transparent protective film can be an ultraviolet-curing adhesive. Electron beam curing adhesives for polarizing films are available. It shows suitable adhesion to the various transparent protective films on the viewing side. The adhesive may contain a metal compound filler.
[0133] The surface of the visible-side transparent protective film to which the polarizer is not attached is provided with a hard coat layer or an anti-reflection layer. Anti-sticking, anti-glare, diffusion or anti-glare treatments It may be.
[0134] (3-2) Polarizer The polarizer is not particularly limited, and various polarizers can be used. Vinyl alcohol film, partially formalized polyvinyl alcohol film, ethyl Hydrophilic polymer films such as partially saponified polyethylene-vinyl acetate copolymer films are treated with iodine or Dichroic dyes are adsorbed on the material and uniaxially stretched. Polyvinyl alcohol is dehydrated. Examples of such films include polyene-based oriented films such as polyvinyl chloride dehydrochlorination products and polyene-based oriented films. Among them, a polarizer made of a polyvinyl alcohol film and a dichroic substance such as iodine is preferred. The thickness of these polarizers is not particularly limited, but is generally about 5 to 80 μm. do.
[0135] A polarizer obtained by dyeing a polyvinyl alcohol film with iodine and stretching it uniaxially is, for example, Polyvinyl alcohol is dyed by immersing it in an aqueous solution of iodine, and the film is stretched to 3 to 7 times its original length. It can be made by stretching. If necessary, it may contain boric acid, zinc sulfate, zinc chloride, etc. Alternatively, the plate may be immersed in an aqueous solution of potassium iodide or the like, which may contain potassium iodide. Before dyeing, the polyvinyl alcohol film may be immersed in water and washed. By washing the polyvinyl alcohol film with water, dirt and blockages on the surface of the polyvinyl alcohol film can be removed. In addition to being able to wash away the anti-sticking agent, it also swells the polyvinyl alcohol-based film. This also has the effect of preventing unevenness in the dyeing. Alternatively, the film may be stretched while being dyed, or may be dyed with iodine after being stretched. Good. It can be stretched in an aqueous solution of boric acid, potassium iodide, etc., or in a water bath.
[0136] In the present invention, a thin polarizer having a thickness of 10 μm or less can also be used. From the viewpoint of miniaturization, the thickness is preferably 1 to 7 μm. The product has little unevenness in thickness, excellent visibility, and little dimensional change, making it highly durable. Moreover, it is preferable that the thickness of the polarizing film can be reduced.
[0137] Representative examples of thin polarizers include those described in JP-A-51-069644 and JP-A-2000 -338329, International Publication No. 2010 / 100917, International Publication No. 2010 / 100917, or the specification of Patent No. 4751481 or JP-A-20 Examples of the thin polarizing film include those described in Japanese Patent Publication No. 12-073563. The polarizing film is made of a polyvinyl alcohol resin (hereinafter referred to as PVA resin) layer and a stretching resin layer. It can be obtained by a manufacturing method including a step of stretching the oil base material in a laminate state and a step of dyeing it. With this manufacturing method, even if the PVA resin layer is thin, it is supported by the stretchable resin substrate. This makes it possible to perform stretching without problems such as breakage due to stretching.
[0138] The thin polarizing film is produced by a process including a step of stretching the laminate and a step of dyeing the laminate. However, it is a film that can be stretched at a high ratio and has improved polarization performance. / 100917 pamphlet, International Publication No. 2010 / 100917 pamphlet, or As described in Japanese Patent No. 4751481 and Japanese Patent Publication No. 2012-073563, It is preferable to use a method including a step of stretching in an aqueous solution of boric acid. Stretching in an aqueous boric acid solution as described in JP-A-2012-073563 and JP-A-2012-073563 Preferably, the film is produced by a process which includes a supplementary in-air stretching step prior to the film being stretched.
[0139] (3-3) Transparent protective film on the image display side Regarding the transparent protective film on the image display side, a conventional one can be used as appropriate. Specifically, it is possible to provide a film that is excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. A transparent protective film made of a material such as polyethylene terephthalate is preferred. polyester polymers such as polyethylene naphthalate and diacetyl cellulose; cellulose-based polymers such as triacetyl cellulose, acrylates such as polymethyl methacrylate, Polymers such as styrene, polystyrene, and acrylonitrile-styrene copolymers (AS resins) Examples of the polymer include polyethylene, polycarbonate, etc. Polypropylene, polyolefins having cyclo- or norbornene structures, ethylene Polyolefin polymers such as propylene copolymers, vinyl chloride polymers, nylon Amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyamides, etc. Polyethersulfone polymers, polyetheretherketone polymers, polyphenylene Sulfide-based polymers, vinyl alcohol-based polymers, vinylidene chloride-based polymers, vinyl Nylbutyral polymers, arylate polymers, polyoxymethylene polymers, ethylene The transparent protective film may be formed of an epoxy-based polymer or a blend of the above polymers. Examples of polymers that can be used include transparent protective films, acrylic, urethane, and Cured layer of thermosetting or UV-curable resin such as urethane, epoxy, or silicone. It can also be formed as
[0140] The thickness of the image display unit side protective film can be determined appropriately, but is generally determined based on strength, ease of handling, etc. From the viewpoints of workability, thin film property, etc., the thickness is about 1 to 500 μm.
[0141] The polarizer and the transparent protective film on the image display side are usually adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include those mentioned above.
[0142] The surface of the transparent protective film on the image display section side to which the polarizer is not attached is provided with a hard coat layer or Anti-reflective, anti-sticking, diffusion or anti-glare treatment It may be something like that.
[0143] 2. Image display device The image display device of the present invention is characterized by using the polarizing film with the pressure-sensitive adhesive layer of the present invention. do.
[0144] As an example of a specific configuration of the image display device, for example, as shown in FIG. Glass or cover plastic 6 / visible side adhesive layer 2a / visible side transparent protective film 3a / Polarizer 4 / Transparent protective film 3b on image display section side / Adhesive layer 2b on image display section side / Liquid crystal display Device (LCD) or organic light-emitting display (OLED) 7 (Figure 2); cover glass or cover Plastic 6 / adhesive layer 8a / sensor layer 9 / visual side adhesive layer 2a / visual side transparent protective film Film 3a / Polarizer 4 / Transparent protective film 3b on the image display section side / Adhesive layer 2b on the image display section side / Liquid crystal display (LCD) or organic light emitting diode (OLED) 7 (Figure 3); cover glass or cover plastic 6 / adhesive layer 8a / sensor layer 9 / adhesive Adhesive layer 8b / sensor layer 9 / visible-side adhesive layer 2a / visible-side transparent protective film 3a / polarizer 4 / Image display section side transparent protective film 3b / Image display section side adhesive layer 2b / Liquid crystal display device (LC D) or an organic light-emitting diode (OLED) 7 (Figure 4); each layer is stacked in this order. The pressure-sensitive adhesive layer-attached polarizing film 1 of the present invention can be an image display device such as the above-mentioned. In the configuration, "visible-side adhesive layer 2a / visible-side transparent protective film 3a / polarizer 4 / image display section side The transparent protective film 3b / image display section side adhesive layer 2b portion is also referred to as the phase In the case where a retardation film is included, specifically, Image display portion side adhesive layer 2b and liquid crystal display device (LCD) or organic electroluminescence display device (OLED) 7 can be laminated via an adhesive layer. Adhesive and / or adhesive layers may be used.
[0145] Image display devices include liquid crystal display devices and organic EL (electroluminescence) display devices. These include display devices, PDPs (plasma display panels), and electronic paper. Among them, liquid crystal display devices and organic EL (electroluminescence) display devices having the above-mentioned configurations Apparatus etc. are preferred. EXAMPLES
[0146] The present invention will be described in detail below with reference to examples. In the examples, all parts and percentages are by weight.
[0147] Production Example 1 (Production of Acrylic Pressure Sensitive Adhesive Composition (a-1)) 2-Ethylhexyl acrylate (2EHA) 78 parts by weight, N-vinyl-2-pyrrolidone (NVP) 18 parts by weight and 2-hydroxyethyl acrylate (HEA) 4 parts by weight The monomer mixture was mixed with 1-hydroxycyclohexylphenyl as a photopolymerization initiator. Luketone (product name: Irgacure 184, has an absorption band in the wavelength range of 200 to 370 nm, B ASF Co., Ltd.) 0.035 parts by weight, 2,2-dimethoxy-1,2-diphenylethane-1- On (product name: Irgacure 651, has an absorption band at wavelengths of 200 to 380 nm, BAS After mixing 0.035 parts by weight of F company), the viscosity (measurement conditions: BH viscometer No. 5 rotor The temperature was 30°C and the UV radiation was irradiated until the temperature reached approximately 20 Pa·s. A prepolymer composition (polymerization rate: 8%) in which a portion of the monomer component was polymerized was obtained. The polymer composition contained 0.15 parts by weight of hexanediol diacrylate (HDDA), silane Add 0.3 parts by weight of a coupling agent (product name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) The ingredients were added and mixed to obtain an acrylic pressure-sensitive adhesive composition (a-1).
[0148] Production Example 2 (Production of acrylic pressure-sensitive adhesive composition (a-2)) 2-Ethylhexyl acrylate (2EHA) 72 parts by weight, methacrylic acid acrylate (MMA) 1 part by weight, N-vinylpyrrolidone (NVP) 12 parts by weight, hydroxyethyl A monomer mixture consisting of 15 parts by weight of acrylate (HEA) was added as a polymerization initiator. Add 0.2 parts by weight of azobisbutylnitrile (AIBN) and 233 parts by weight of ethyl acetate. After that, the mixture was reacted at 60°C for 7 hours in a nitrogen atmosphere, whereby a portion of the monomer components was polymerized. Next, a silane coupling agent (product name: KBM -403, Shin-Etsu Chemical Co., Ltd.) 0.3 parts by weight, isocyanate-based crosslinking agent as crosslinking agent (Product name: Takenate D110N, manufactured by Mitsui Chemicals, Inc.) 0.21 parts by weight was added to the acrylic acid solution. A dispersant-based pressure-sensitive adhesive composition (a-2) was obtained.
[0149] Production Example 3 (Production of Pressure-Sensitive Adhesive Layer (B-1) on Image Display Side) A separable flask equipped with a thermometer, stirrer, reflux condenser, and nitrogen gas inlet tube was 95 parts by weight of ethyl acrylate, 5 parts by weight of acrylic acid, and azobisisobutyronitrile as a polymerization initiator. After adding 0.2 parts by weight of nitrile and 233 parts by weight of ethyl acetate, nitrogen gas was introduced and the mixture was stirred. The mixture was purged with nitrogen for about 1 hour while stirring. The flask was then heated to 60°C and reacted for 7 hours. As a result, an acrylic polymer having a weight average molecular weight (Mw) of 1.1 million was obtained. The acrylic polymer solution (solid content: 100 parts by weight) was mixed with an isocyanate crosslinker. As a crosslinking agent, trimethylolpropane tolylene diisocyanate (product name: Coronate L , Nippon Polyurethane Industry Co., Ltd.) 0.8 parts by weight, silane coupling agent (product name: KB M-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) (0.1 parts by weight) was added to prepare an adhesive composition (solution). did. A 38 μm thick separator (polyethylene terephthalate film with a release-treated surface) The obtained adhesive composition solution was applied onto a film (film) so that the thickness after drying would be 12 μm. The solvent was removed by drying at 100°C for 3 minutes to obtain a pressure-sensitive adhesive layer. This adhesive layer was hereinafter referred to as the "adhesive layer on the image display portion side (B-1 )"
[0150] Production Example 4 (Production of Pressure-Sensitive Adhesive Layer (B-2) on Image Display Side) A 38 μm thick separator (polyethylene terephthalate film with a release-treated surface) The adhesive composition solution obtained in Production Example 3 was applied onto a film (3) so that the thickness after drying became 15 μm. The adhesive layer was then dried at 100°C for 3 minutes to remove the solvent, and an adhesive layer was obtained. The adhesive layer was heated at 0° C. for 48 hours to carry out a crosslinking treatment. Hereinafter, this adhesive layer is referred to as the “image display portion side adhesive layer.” This layer is called "Layer (B-2)".
[0151] Example 1 (Production of adhesive composition with ultraviolet absorbing function) The obtained acrylic pressure-sensitive adhesive composition (a-1) was mixed with butyl acrylate at a solid content of 15% and 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxyphenyl]- {4-methoxyphenyl}-6-(4-methoxyphenyl)-1,3,5-triazine (Product Name: Tinosorb S, "UV absorber 1" in Tables 1 and 2, manufactured by BASF Japan) 1.4 parts by weight of bis(2,4,6-trimethylbenzoyl)-phenylphosphine Oxide (product name: Irgacure 819, has absorption resistance in the wavelength range of 200 to 450 nm, B Add 0.2 parts by weight of ASF Japan Co., Ltd. and stir to give it an adhesive with UV absorbing properties. A pharmaceutical composition was obtained.
[0152] The pressure-sensitive adhesive composition having an ultraviolet absorbing function is applied onto a release-treated film of a release film. The adhesive composition was applied so that the thickness of the adhesive layer formed would be 150 μm. A release film was attached to the surface. Then, the illuminance was 6.5 mW / cm 2 , Light output: 15 00mJ / cm 2 The pressure-sensitive adhesive composition layer was irradiated with ultraviolet light at a peak wavelength of 350 nm. The resultant was photocured to form a visible-side pressure-sensitive adhesive layer (A-1).
[0153] (Production of polarizing film (P-1)) A polarizer made of a 5 μm-thick stretched polyvinyl alcohol film impregnated with iodine. On the viewing side, a cycloolefin polyimide film with a thickness of 25 μm was applied using a polyvinyl alcohol adhesive. A COP film was attached to the image display surface of the polarizer. A 20 μm thick acrylic film was laminated using a acrylic adhesive to create a polarizing film (P-1). The polarization degree of the polarizing film was 99.995.
[0154] (Manufacture of polarizing film with adhesive layer) The viewing side of the polarizing film (P-1) (i.e., a cycloolefin polymer having a thickness of 25 μm) The visible side pressure-sensitive adhesive layer (A-1) was laminated on the surface of the polarizing plate (COP film). The image display surface of the film (P-1) (i.e., the acrylic film having a thickness of 20 μm) The pressure-sensitive adhesive layer (B-1) on the image display portion side is laminated on the surface of the laminate, and further, a retardation film (thickness: 56 μm, material: polycarbonate) and the image display side adhesive layer (B-2) are laminated and adhered. The obtained polarizing film with the pressure-sensitive adhesive layer was layer (A-1) / polarizing film (P-1) / adhesive layer on image display side (B-1) / retardation film The adhesive layer had a structure of (B-1) / (image display portion side pressure-sensitive adhesive layer).
[0155] Examples 2 to 3 Type of acrylic adhesive composition, amount of ultraviolet absorber 1 added, and after formation of visible side adhesive layer The polarizing film with the adhesive layer was prepared in the same manner as in Example 1, except that the thickness of the polarizing film was set as shown in Table 1. A new system was formed.
[0156] Example 4 The pressure-sensitive adhesive layer on the viewing side was removed from the pressure-sensitive adhesive layer on the viewing side (A-1) by the pressure-sensitive adhesive layer on the viewing side ( A polarizing film with adhesive was formed in the same manner as in Example 1, except that A-2) was used.
[0157] (Production of Visible Side Adhesive Layer (A-2)) The acrylic pressure-sensitive adhesive composition (a-2) obtained in Production Example 2 was dissolved in ethyl acetate at a solid content of 15%. 2,4-bis-[{4-(4-ethylhexyloxy)-4-phenylene] hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (commercial Add 1.4 parts by weight of Tinosorb S (BASF Japan) and stir. Thus, a pressure-sensitive adhesive composition with an ultraviolet absorbing function was obtained.
[0158] The pressure-sensitive adhesive composition having an ultraviolet absorbing function is applied onto a release-treated film of a release film. The adhesive layer was applied so that the thickness after formation was 150 μm, and then heated at 60°C for 2 minutes and at 120°C for 2 minutes. After drying for 10 minutes, the visible side adhesive layer (A-2 ) was formed.
[0159] Examples 5 to 6 The thickness of the visible side adhesive layer after formation, and the adhesive layer on the image display section side were as shown in Table 1. A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 4.
[0160] Example 7 (Production of Visible Side Adhesive Layer (A-3)) The acrylic adhesive composition (a-1) obtained in Production Example 1 was mixed with butyl acrylate in a solid state. 2,4-bis-[{4-(4-ethylhexyloxy) -4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-trimethyl gin (Product name: Tinosorb S, manufactured by BASF Japan) 0.7 parts by weight, Solven t Yellow 163 (KP Plast Yellow MK, "UV Absorption" in Table 2 Collector 2 (Kiwa Chemical Industry Co., Ltd.) 0.2 parts by weight, bis(2,4,6-trimethylbenzoyl) Il)-phenylphosphine oxide (product name: Irgacure 819, wavelength 200~ Add 0.2 parts by weight of BASF Japan Co., Ltd. (having absorption resistance at 450 nm) and stir. Thus, a pressure-sensitive adhesive composition with an ultraviolet absorbing function was obtained.
[0161] The pressure-sensitive adhesive composition having an ultraviolet absorbing function is applied onto a release-treated film of a release film. The adhesive composition was applied so that the thickness of the adhesive layer formed would be 150 μm. A release film was attached to the surface. Then, the illuminance was 6.5 mW / cm 2 , Light output: 30 00mJ / cm 2 The pressure-sensitive adhesive composition layer was irradiated with ultraviolet light at a peak wavelength of 350 nm. The resultant was photocured to form a visible-side pressure-sensitive adhesive layer (A-3).
[0162] The pressure-sensitive adhesive layer on the viewing side was removed from the pressure-sensitive adhesive layer on the viewing side (A-1) by the above-obtained pressure-sensitive adhesive layer on the viewing side ( A polarizing film with adhesive was formed in the same manner as in Example 1, except that A-3) was used.
[0163] Comparative Example 1 The visible side pressure-sensitive adhesive layer (A-1), the retardation film, and the image display side pressure-sensitive adhesive layer (B-2) A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 1, except that no adhesive layer was formed.
[0164] Comparative Example 2 The adhesive layer was formed in the same manner as in Example 1, except that the visible-side adhesive layer (A-1) was not formed. A polarizing film was formed.
[0165] Comparative Examples 3 and 4 Except that no ultraviolet absorbing agent was added to the visible side pressure-sensitive adhesive layers (A-1) and (A-2), A polarizing film with adhesive was formed in the same manner as in Examples 1 and 4.
[0166] Comparative Example 5 (Production of polarizing film (P-2)) A polarizer made of a 12 μm-thick stretched polyvinyl alcohol film impregnated with iodine. On the viewing side, a 25 μm thick triacetyl cellulose film was attached using a polyvinyl alcohol adhesive. A polyvinyl alcohol adhesive is applied to the image display surface of the polarizer. A 20 μm thick acrylic film was laminated using the polarizing film (P-2). The polarization degree of the optical film was 99.995.
[0167] In Example 2, the polarizing film (P-1) was changed to the polarizing film (P-2). Other than that, a polarizing film with adhesive was formed in the same manner as in Example 2.
[0168] The obtained pressure-sensitive adhesive layer and the polarizing film with the pressure-sensitive adhesive layer were evaluated as follows.
[0169] <Polymerization rate> The release film of the visible side pressure-sensitive adhesive layer obtained in the Examples and Comparative Examples was peeled off and the weight was measured. Only the adhesive layer on the viewing side was placed on the aluminum petri dish. (Aluminum petri dish + adhesive layer on the viewing side) The weight was measured to determine the weight of the adhesive layer before drying. After drying at 130°C for 2 hours, the weight of the adhesive layer was approximately 2 After cooling for 10 minutes, the weight of the aluminum dish and adhesive was measured again. The weight of the adhesive layer was measured. The polymerization rate was calculated using the following formula:
number
[0170] <Gel fraction> Approximately 0.1 g of the visible side pressure-sensitive adhesive layer obtained in each of the Examples and Comparative Examples was sampled, and the average pore size was 0.2 μm. 100 mm porous tetrafluoroethylene sheet (product name: NTF1122, manufactured by Nitto Denko Corporation) ), then tied with a kite string, and the weight at that time was measured (Zg), and this weight was used as the weight before immersion. The weight before immersion was the weight of the visible side adhesive layer (the adhesive layer collected above) and the tetrafluoroethylene The weight of the tetrafluoroethylene sheet and the kite string is the total weight of the tetrafluoroethylene sheet and the kite string. The total weight of the yarn was also measured (Yg). Next, the adhesive layer on the viewing side was The sample was wrapped in a plastic bag and tied with kite string. The sample was then placed in a 50-mL container filled with ethyl acetate. The samples were then placed in a 1000 ml container and left at 23°C for 7 days. After that, the samples (treated with ethyl acetate) were taken out of the container. After that, the mixture was taken out, transferred to an aluminum cup, and dried in a dryer at 130°C for 2 hours. After removing the ethyl acetate by immersion, the weight was measured (X g), and this weight was recorded as the weight after immersion. The gel fraction was calculated from the formula. Gel fraction (wt%)=(XY) / (ZY)×100
[0171] <Measurement of transmittance and b* value of visible side adhesive layer> The release film of the visible side adhesive layer obtained in the Examples and Comparative Examples was peeled off, and the visible side adhesive The layer was attached to a measuring jig and measured with a spectrophotometer (product name: U4100, Hitachi High-Technologies Corporation). The transmittance was measured using a 380 nm, 400 nm, and 420 nm wavelength FT-IR. The transmittance was measured (however, the measurement was performed at a wavelength of 420 nm only in Examples 2 and 7).
[0172] <Residual stress> A piece of 30 mm wide and 50 mm long was cut out from the visible side pressure-sensitive adhesive layer obtained in the Examples and Comparative Examples. The specimen was then placed with a chuck distance of 20 mm and subjected to tension. The specimen was pulled 60 mm (300%) at a speed of 200 mm / min (the distance between the chucks after pulling was 80 m). m). The specimen is pulled 60 mm and held at this position for 300 seconds. The stress value after 300 seconds (N The residual stress was calculated using the following formula: Residual stress after 300 seconds = stress value after 300 seconds (N) / (4 x thickness of test piece / 10)
[0173] <Optical reliability> The COP film of the polarizing film (P-1) used in Example 1 was The pressure-sensitive adhesive layers on the viewing side obtained in Comparative Examples 3 to 5 were laminated together. On the other side of the polarizing film (acrylic film side), apply 15μm adhesive and 56μm A retardation film (manufactured by Nitto Denko Corporation) was attached to the sample. Both sides of the sample were covered with glass (commercially available). Product name: S200200, thickness: 1.3mm, size: 45mm x 50mm, Matsunami Glass Industry (Made by Co., Ltd.) and autoclaved (pressure: 0.5 MPa, temperature: 50°C) ) was carried out for 15 minutes. After that, it was placed under the following various reliability conditions and measured with a spectral transmittance measuring instrument ( The transmittance was measured using a product called DOT-3 (manufactured by Murakami Color Research Laboratory Co., Ltd.). The change in the transmittance was determined and evaluated according to the following criteria. (Various reliability conditions) (Condition 1) 85℃×500h (Condition 2) 60℃, 95% x 500h (Condition 3) Heat shock (HS) (-40℃ to 85℃) x 300 cycles (Condition 4) Under UV irradiation × 100h, illuminance: 500W / cm 2 (300~700nm), ring Environmental temperature: 60~65℃, environmental humidity: 50% (Condition 5) Under Xenon irradiation × 300h, illuminance: 2.40W / cm 2 (420nm), ring Environmental temperature: 50℃, environmental humidity: 30% (Evaluation Criteria) ◯: The change in transmittance is 2.0% or less. △: The amount of change in transmittance exceeds 2.0% and is 3.0% or less. ×: The change in transmittance exceeds 3.0%.
[0174] <Glue stains, dimensional accuracy, edge appearance> The polarizing films with the pressure-sensitive adhesive layer obtained in the Examples and Comparative Examples were cut into 25 pieces by a super cutter. The pieces were then cut into pieces measuring 30 mm x 30 mm. Then, they were processed using a cutting machine (Megalo Technica Co., Ltd.). Therefore, 0.05 mm was cut off from the four sides of the cut piece to prepare a sample. The side of the sample was visually inspected to see if there was any glue staining. The result was observed under an optical microscope and evaluated according to the following criteria. (Dimensional accuracy) ○:Within ±0.3mm ×: Exceeds ±0.3 mm (Exterior view of end) ○: When the edge is not sticky when touched with the hand ×: If the edge is sticky when touched with your hand
[0175] <Curl measurement> A sample cut to 50 mm x 40 mm was placed on a flat table and the gap was The curl was measured by a tape measure. (curl) ○: Within ±1.0mm △: More than ±1.0mm, within ±2.0mm ×: Greater than ±2.0mm
[0176] [Table 1]
[0177] [Table 2]
[0178] In Table 1, P-1 indicates the polarizing film (P-1), and P-2 indicates the polarizing film (P-2). a-1 is the acrylic pressure-sensitive adhesive composition (a-1) obtained in Production Example 1, and a-2 is the acrylic pressure-sensitive adhesive composition (a-2) obtained in Production Example 2. The acrylic pressure-sensitive adhesive composition (a-2) obtained in Example 2 was mixed with the ultraviolet absorber 1, -[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4- Methoxyphenyl)-1,3,5-triazine (trade name: Tinosorb S, BAS F Japan Co., Ltd.), and UV absorber 2 is Solvent Yellow 163 (KP Plast Yellow MK, manufactured by Kiwa Chemical Industry Co., Ltd.) and B-1 is the one obtained in Production Example 3. The pressure-sensitive adhesive layer (B-1) on the image display portion side obtained in Production Example 4 was used as B-2. The pressure-sensitive adhesive layer (B-2) is shown. [Explanation of symbols]
[0179] 1. Polarizing film with adhesive layer 2a Visible side adhesive layer 2b Adhesive layer on image display side 3a Transparent protective film on the viewing side 3b Transparent protective film on image display side 4 Polarizer 5. Polarizing Film 6 Cover glass or cover plastic 7 Liquid crystal display (LCD) or organic light emitting diode (OLED) 8a, 8b Adhesive layer 9 Sensor Layer
Claims
1. A polarizing film with a pressure-sensitive adhesive layer for an organic electroluminescence display device, which is used on a viewing side of an image display unit in an image display device, The polarizing film with a pressure-sensitive adhesive layer for an organic EL display device includes a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film, The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, The transparent protective film on the viewing side of the polarizer has a transmittance at a wavelength of 380 nm of less than 6%, the transparent protective film on the viewing side of the polarizer is at least one film selected from the group consisting of a triacetyl cellulose film, a polyethylene terephthalate film, and a polyolefin film having a cyclo- or norbornene structure, the material of the transparent protective film on the image display portion side of the polarizer is a polyester-based polymer, an acrylic-based polymer, a styrene-based polymer, a polycarbonate-based polymer, a polyolefin-based polymer, a vinyl chloride-based polymer, an amide-based polymer, an imide-based polymer, a sulfone-based polymer, a polyethersulfone-based polymer, a polyetheretherketone-based polymer, a polyphenylene sulfide-based polymer, a vinyl alcohol-based polymer, a vinylidene chloride-based polymer, a vinyl butyral-based polymer, an arylate-based polymer, a polyoxymethylene-based polymer, an epoxy-based polymer, or a blend of the above polymers; the pressure-sensitive adhesive layer on the viewing side of the polarizing film is formed from an ultraviolet-curable acrylic pressure-sensitive adhesive composition, the ultraviolet-curable acrylic pressure-sensitive adhesive composition being prepared by irradiating with ultraviolet light a composition containing a monomer component containing an alkyl(meth)acrylate and a photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm to form a partial polymer of the monomer component, and adding an ultraviolet absorber and a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more to the partial polymer of the monomer component; the pressure-sensitive adhesive layer on the viewing side of the polarizing film contains, as the ultraviolet absorbing agent, one or more of a triazine-based ultraviolet absorbing agent, a benzotriazole-based ultraviolet absorbing agent, a benzophenone-based ultraviolet absorbing agent, an oxybenzophenone-based ultraviolet absorbing agent, a salicylic acid ester-based ultraviolet absorbing agent, and a cyanoacrylate-based ultraviolet absorbing agent, and a dye; A polarizing film with an adhesive layer for an organic electroluminescence display device, wherein the adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function.
2. 2. The polarizing film with a pressure-sensitive adhesive layer for an organic EL display device according to claim 1, wherein the transparent protective film on the viewing side of the polarizer has a thickness of 40 μm or less.
3. 3. The polarizing film with an adhesive layer for an organic electroluminescent display device according to claim 1, wherein the thickness of the adhesive layer on the viewing side of the polarizing film is at least twice the thickness of the adhesive layer on the image display side of the polarizing film.
4. The polarizing film with an adhesive layer for an organic EL display device according to any one of claims 1 to 3, characterized in that the adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 60% or more at a wavelength of 400 nm.
5. The polarizing film with an adhesive layer for an organic EL display device according to any one of claims 1 to 3, characterized in that the adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 75% or less at a wavelength of 420 nm.
6. 5. The polarizing film with an adhesive layer for an organic EL display device according to claim 1, wherein the b* value of the adhesive layer on the viewing side of the polarizing film is 3.0 or less.
7. 7. The polarizing film with an adhesive layer for an organic EL display device according to claim 1, wherein the adhesive layer on the viewing side of the polarizing film contains an acrylic polymer as a base polymer.
8. 8. An image display device, comprising the pressure-sensitive adhesive layer-attached polarizing film for an organic EL display device according to claim 1, on a viewing side of an image display section.
Citation Information
Patent Citations
Polarizing plate protection film, and polarizing plate and liquid crystal display using same
JP2006184883A
Polarizing plate
JP2008040277A
Polarizing plate and liquid crystal display device using the same
JP2011232493A
Polarizer protective film, polarizing plate, and image display device
JP2012003269A
Optical film having adhesive agent on both sides, and manufacturing method of image display unit using the same
JP2014115468A