Method for conditioning and hydrolysis of extruded film
The hydrolysis of perfluorosulfonyl fluoride membranes using triethylsilanol and DBU addresses high production costs in PEM electrolyzers by enhancing ionic conductivity, leading to cost-effective and efficient tubular electrochemical cells.
Patent Information
- Application Number
- JP2024058724
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-04-01
- Publication Date
- 2024-11-13
AI Technical Summary
Existing electrochemical cells, particularly proton exchange membrane (PEM) electrolyzers, face high production costs due to the use of expensive materials like platinum group metals and membranes, and there is a need for a cost-effective method to pretreat extruded membranes for improved ionic conductivity.
A method involving hydrolysis of perfluorosulfonyl fluoride membranes using triethylsilanol and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) to convert fluoride groups into sulfonic acid groups, optimizing reactant concentrations and reaction conditions for enhanced ionic conductivity, and using coextrusion techniques to form tubular cells with a higher electrode volume-to-membrane area ratio.
Reduces production costs and enhances the ionic conductivity of extruded membranes, enabling efficient water electrolysis with improved performance and stability of tubular cells.
Smart Images

Figure 2024160203000001_ABST
Abstract
Description
[Technical field]
[0001] The disclosed invention relates generally to the field of electrochemical cells. More specifically, embodiments of the disclosed invention provide methods for conditioning and / or hydrolysis of extruded membranes. [Background technology]
[0002] Electrochemical cells can be planar, tubular, or monolithic in design and are the basic building blocks of electrochemical devices. The various designs have some deficiencies, such as the very long start-up time of planar solid oxide fuel cells (SOFCs) and the lower volumetric power density of tubular SOFCs. Direct current (DC) electricity is generated by electrochemical fuel cells, which convert the chemical bond energy potential of the fuel into electrical energy. Currently, fuel cells are being considered as an alternative to traditional power plants and battery storage systems.
[0003] Electrical energy storage is of great importance in the context of the energy transition, since the Renewable Energy Act threatens to jeopardize the technical and economic stability of the power grid as a result of the increased production of renewable and inherently unstable energy sources. Several storage technologies must be integrated for the absorption and release of different amounts of energy over different time scales. High energy efficiency, low cost and resource conservation must all be met by the storage solution. In addition to mechanical (compressed air, water columns) and thermal storage options, electrochemical devices (batteries, electrolysis / fuel cells) form a very important component of such options.
[0004] Industrial water electrolysis is mostly carried out in two different types of cells. In alkaline electrolytes, high currents can be generated using relatively cheap electrode materials, but usually at high overpotentials, which results in low energy efficiency and is unfavourable for energy storage. Low overpotentials are possible with PEM electrolysis, which runs the electrolysis under acidic conditions, but this relies on the use of the valuable metals platinum and iridium as catalysts. It is the use in large quantities that is problematic from an economic and raw material point of view.
[0005] Alkaline water electrolyzers are becoming more widespread in commercial use, and proton exchange membrane water electrolyzers (PEMWEs) are attracting more attention due to less gas crossover through the membrane, higher conversion efficiency, less corrosion issues, and compact design. On the other hand, there are still few challenges to be addressed. One of them is the high cost of traditional planar electrolyzers, due to the high cost of bipolar plates, porous transfer layers, platinum group metal (PGM) catalysts, and membranes. Transferring the cell geometry from planar to tubular can be a strategy to reduce the production and assembly costs.
[0006] An anode and a cathode, two porous electrodes, and a dense solid electrolyte and / or membrane separating the electrodes are commonly used in cells that constitute solid-state electrochemical devices.
[0007] The electrolysis device described in WO2008 / 048103A1 comprises an externally walled vessel vertically divided into four successive chambers, with electrodes located in the first and last chambers. The chambers are separated from each other by semipermeable membranes, which are substantially permeable to cations and preferably substantially impermeable to multivalent cations. However, diffusion of gases is not addressed in WO2008 / 048103A1.
[0008] Document DE102016005144A1 describes a longitudinal device with a tubular cross section suitable as a building part for an electrochemical cell, a composite formed from structural elements that include an inner electrode or are included by an outer electrode, the electrodes being either porous electrodes or gas diffusion layers, the structural elements in the contact area between the inner electrode and the included structural elements exhibiting a shape forming a flow channel or the structural elements in the contact area between the outer electrode and the included structural elements exhibiting a shape forming a flow channel. Due to the shaped structural elements the electrical resistance along the composite is significantly reduced and pressure losses along the electrochemical cell, which are generally disadvantageous during use of the electrochemical cell, are mitigated.
[0009] Due to the fact that hydrogen gas serves both as an energy carrier and as a raw material for the chemical industry, the combination of water electrolysis for the production of hydrogen and oxygen with a fuel cell for the re-release of the energy contained in the fuel H2 is particularly economically attractive in the present invention. Its distinct added value comes from its dual functionality.
[0010] In this context, lowering the cost of producing PEM electrolysis cells is a goal that several organizations have tried to achieve by using various strategies, but always with ever-increasing costs and performance parameters using technological parameters available in conventional planar stack systems. By utilizing a production method that is entirely new to the field of electrolysis technology, the present invention aims to provide an alternative method possibility for the pretreatment of membranes that can be used in the presence of electrodes sensitive to corrosion, such as catalyst-coated electrodes in electrolyzers or fuel cells.
[0011] Therefore, in light of the above discussion, there is an urgent need for technical solutions that overcome the above-mentioned limitations.The present disclosure focuses on methods for conditioning and / or hydrolyzing extruded membranes. Summary of the Invention
[0012] Disclosure Summary The following is a general description of illustrative embodiments of the present invention. Provided as a prelude to aid those skilled in the art in more quickly assimilating the detailed design discussion, the following discussion is not intended to limit in any manner the scope of the claims appended hereto to particularly point out the present invention.
[0013] According to an illustrative embodiment, the present disclosure focuses on a method for conditioning or pre-treatment, e.g., hydrolysis, of extruded membranes. The extrusion of the membrane allows for the tubular structure of the electrolysis cell. After the extrusion process, the membrane needs to be pre-treated to ensure the ionic conductivity of the membrane. The proton conductivity of the membrane is essential for the efficiency of water electrolysis or the operation of the electrolyzer.
[0014] According to an aspect of the present disclosure, a method for conditioning / pretreatment / hydrolysis of extruded membranes is disclosed. The method for pretreatment of cation exchange membranes includes converting water to hydrogen using multiple water electrolyzers (WEs) and fuel cells, and flow batteries. The method also includes sealing half cells of a tubular cell manufactured by a co-extrusion technique to obtain a higher ratio of electrode volume per membrane area. The method also includes extruding a perfluorosulfonyl fluoride membrane from perfluorosulfonyl fluoride granules, which are polymers containing perfluorinated polymer chains substituted with sulfonyl fluoride groups. The method also includes increasing the ionic conductivity of the extruded perfluorosulfonyl fluoride membrane using a pretreatment technique before using the membrane in an electrolysis cell. The method also includes applying a milder pretreatment technique by activating the SF bond to perform nucleophilic exchange of the fluoride group in a reaction. The method also includes hydrolyzing the sulfonyl fluoride group to sulfonic acid using triethylsilanol.
[0015] In one embodiment of the present invention, a perfluorosulfonyl fluoride membrane is commercially pretreated and the fluoride groups are exchanged for hydroxyl groups using sodium hydroxide.
[0016] In one embodiment of the present invention, when the perfluorosulfonyl fluoride membrane is commercially pretreated, the sodium sulfonate groups are protonated by storing the perfluorosulfonyl fluoride membrane in 1 M sulfuric acid.
[0017] In one embodiment of the present invention, a commercially pretreated perfluorosulfonyl fluoride membrane is characterized by a number of parameters, including but not limited to, proton diffusion, in-plane conductivity, ion exchange capacity, and water uptake.
[0018] In one embodiment of the invention, the method involves using measurement techniques to calculate parameters such as water absorption, swelling ratio, and ion exchange capacity.
[0019] In one embodiment of the present invention, the measurement techniques include Raman spectroscopy and nuclear magnetic resonance (NMR) techniques.
[0020] In one embodiment of the invention, the method further comprises transferring a fluoride ion from the strong covalent bond to a leaving group, which, if a catalyst is used, can be H + and / or R3Si + This is aided by interaction with
[0021] In one embodiment of the present invention, the catalyst comprises triethylsilanol in the presence of 1,8 diazabicyclo(5.4.0)undec-7-ene (DBU).
[0022] In an embodiment of the invention, the reaction exchanges fluoride groups to form silanolates, F - and sulfur(VI)-fluoride exchange (SuFEx), which involves releasing the ester to give a sulfonic acid group.
[0023] In an embodiment of the invention, the method comprises optimizing multiple reactants.
[0024] In one embodiment of the present invention, the perfluorosulfonyl fluoride membrane is conditioned / treated at room temperature with optimized reactant concentrations for a pre-defined conditioning time.
[0025] In one embodiment of the present invention, the predetermined conditioning time is increased in 24 h intervals, and after each interval, the perfluorosulfonic acid (PFSA) membrane is stored in water for 24 h and in 1 M H2SO4 for an additional 24 h.
[0026] According to an embodiment of the invention, a method includes hydrolyzing a perfluorosulfonyl fluoride film using a concentration of a reactant for conditioning the perfluorosulfonyl fluoride film.
[0027] In an embodiment of the invention, the method involves hydrolyzing a perfluorosulfonyl fluoride film in EtSiOH and storing it in 1 M HSO solution until the measured conductivity is greater than 90 mS / cm.
[0028] In an embodiment of the invention, the method includes measuring the conductivity of a perfluorosulfonic acid membrane.
[0029] In one embodiment of the present invention, co-extrusion techniques include simple extrusion, multi-layer extrusion, woven extrusion, and the like.
[0030] In one embodiment of the present invention, the method includes optimizing the hydrolysis reaction parameters and evaluating the stability of the half-cells.
[0031] These and other advantages will become apparent from the present application of the embodiments described herein.
[0032] The above is a simplified summary to provide an understanding of some embodiments of the present invention. This summary is not an extensive or exhaustive overview of the present invention and its various embodiments. This summary presents selected concepts of embodiments of the present invention in a simplified form as a prelude to the more detailed description presented below. As will be appreciated, other embodiments of the present invention can utilize, alone or in combination, one or more of the features described above or in detail below.
[0033] In order to more clearly describe the technical solutions in the embodiments of the present disclosure or in the prior art, the accompanying drawings required for describing the embodiments or the prior art are briefly described below. Obviously, the accompanying drawings in the following description only show some embodiments of the present disclosure, and those skilled in the art can derive other implementations from these accompanying drawings without inventive efforts. All of the embodiments or implementations belong to the protection scope of the present disclosure. [Brief description of the drawings]
[0034] [Figure 1A] FIG. 1 illustrates a perspective view of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the present invention. [Figure 1B] FIG. 2 illustrates another perspective view of a tubular water electrolysis cell according to an embodiment of the invention disclosed herein. [Diagram 2] FIG. 1 illustrates a top view SEM image of a porous anodized electrode of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the invention disclosed herein. [Figure 3A] FIG. 1 illustrates a cross-sectional SEM image of a porous anodized electrode surface of a tubular water electrolysis cell for generating hydrogen and oxygen according to an embodiment of the invention disclosed herein. [Figure 3B] FIG. 2 illustrates an image of a film before (left) Raman measurement according to one or more embodiments of the invention disclosed herein. [Figure 3C]FIG. 1 illustrates an image of a film after Raman measurement (right) according to one or more embodiments of the invention disclosed herein. [Figure 3D] FIG. 1 illustrates an H-cell for measuring proton diffusion of extruded membranes according to embodiments of the invention disclosed herein. [Figure 4] FIG. 2 illustrates a perspective view of individual components of a PEME water electrolysis device according to an embodiment of the invention disclosed herein. [Diagram 5] FIG. 1 illustrates a flow chart of a method for conditioning and / or hydrolyzing an extruded membrane according to an embodiment of the invention disclosed herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] The electrochemical cell system and method for conditioning and / or hydrolysis of extruded membranes are illustrated in the accompanying drawings, in which like reference characters indicate corresponding parts in the various views. It should be noted that the accompanying figures are intended to provide illustrations of exemplary embodiments of the present disclosure. These figures are not intended to limit the scope of the present disclosure. It should also be noted that the accompanying figures are not necessarily drawn to scale.
[0036] Those skilled in the art will recognize that the present disclosure may be modified and altered in addition to those specifically described. The present disclosure should be understood to include all such modifications and alterations. The disclosure also includes all such steps, features, compositions, and compounds referred to or shown in this specification, individually or collectively, and any and all combinations of any or more of such steps or features.
[0037] For convenience, before further description of the present disclosure, certain terms and examples used herein are summarized here.These definitions should be read in light of other parts of the disclosure and understood as understood by those skilled in the art.Terms used herein have meanings that are recognized and known by those skilled in the art, but for convenience and completeness, certain terms and their meanings are described below.
[0038] The articles "a", "an" and "the" are used to refer to one or to more than one (i.e. to at least one) of the grammatical object of the article.
[0039] The terms "comprise" and "comprising" are used in an inclusive and open sense, meaning that additional elements may be included. It is not intended to be interpreted as "consisting only of." Throughout this specification, unless the context requires otherwise, the term "comprise" and variations thereof, such as "comprises" and "comprising," will be understood to imply the inclusion of a described element or step, or group of elements or steps, but not the exclusion of any other element or step, or group of elements or steps.
[0040] The term "including" is used to mean "including but not limited to." "Including" and "including but not limited to" are used interchangeably.
[0041] Anodization is a method frequently used in industry to achieve nanostructuring.
[0042] SEM and scanning electron microscope may be used interchangeably for convenience throughout this invention.
[0043] PEM and polymer electrolyte membrane may be used interchangeably for convenience throughout this invention.
[0044] Inductively Coupled Plasma Optical Emission Spectroscopy and ICP-OES may be used interchangeably for convenience throughout this invention.
[0045] IEC and ion exchange chromatography may be used interchangeably for convenience throughout this invention.
[0046] Polytetrafluoroethylene and PTFE may be used interchangeably for convenience throughout this invention.
[0047] DMF and dimethylformamide may be used interchangeably for convenience throughout this invention.
[0048] The following abbreviations may be used interchangeably throughout the present invention for convenience:
[0049] XRD for X-ray powder diffraction
[0050] TEM for Transmission Electron Microscopy
[0051] EDX for Energy Dispersive X-ray Analysis
[0052] AFM for atomic force microscopy
[0053] BET on Brunauer-Emmett-Teller
[0054] GC-MS vs. Gas Chromatography-Mass Spectrometry
[0055] ICP-MS for Inductively Coupled Plasma Mass Spectrometry
[0056] AAS for atomic absorption spectroscopy
[0057] TOC to Total Organic Carbon
[0058] IC vs. Ion Chromatography
[0059] ADL for electrocatalytically active materials
[0060] PFSA for Perfluorosulfonic Acids
[0061] 1A illustrates a perspective view of a tubular water electrolysis cell 100 for generating hydrogen and oxygen according to an embodiment of the present invention. The tubular water electrolysis cell 100 includes an outer current collector 1, an outer electrode 2, an ion exchange membrane 3, an inner electrode 4, and an inner current collector 5, etc.
[0062] According to an embodiment of the present invention, the tubular cell 100 may also include an outer current collector 1 that defines an exterior surface area of the tubular electrochemical cell 100. The outer current collector 1 may include an elongated hollow portion for containing an outer electrode 2 having a plurality of physical, chemical, and mechanical parameters using additive manufacturing 102, the outer electrode 2 being shaped as depicted in FIG.
[0063] Additive manufacturing 102 may enable the production of porous metal outer and inner electrodes 2, 4 with configurable microstructures, macrostructures, and regularly stacked three-dimensional pore structures tailored to expected voltage profiles.
[0064] According to embodiments of the present invention, several physical, chemical, and mechanical parameters include high porosity, large active reaction area, water and gas permeability for transport of reactants and reaction products, high electrical and thermal conductivity, good corrosion resistance, and sufficient strength and dimensional stability under certain flow pressures.
[0065] Additionally, the outer current collector 1 includes an ion exchange membrane 3 for exchanging ions within the interior region from the outer electrode to the inner electrode 4. The ion exchange membrane 3 may be disposed in the inner cavity of the outer electrode 2 directly onto the inner electrode 4 by multiple extrusion techniques.
[0066] 2 and 3A-3D simultaneously, various embodiments of the present invention will now be described.
[0067] 2 illustrates a top view 200 SEM image of a porous anodized electrode of a tubular water electrolysis cell 100 for generating hydrogen and oxygen according to an embodiment of the present invention. In particular, planar high purity metal samples can be anodized under strict temperature and potential control, and accordingly have nearly defect-free cylindrical pore shapes and arrangements. In addition, anodization may be used on structural titanium workpieces for the first time.
[0068] The diameter and length of the pores forming on the outer electrode 2 and the inner electrode 4 may be adjusted in one or more embodiments of the present invention. In addition, using atomic layer deposition (ALD) 104, the inner pore walls of the outer electrode 2 and the inner electrode 4 may be uniformly coated with a thin (20 nm) to ultra-thin (2 nm) layer of electrocatalytically active material, also depicted in FIG. 3A. With the help of oxides, sulfides, and / or any other noble metal, electrocatalytically active material, atomic layer deposition (ALD) has a remarkable ability to uniformly coat even deep pores.
[0069] In an exemplary scenario, a tubular geometry is used in a PEM fuel cell. In particular, in a tubular cell, only half cells are sealed at the ends, resulting in a higher electrode volume per membrane area ratio. Furthermore, the half cells can be manufactured in a single step by a co-extrusion process, which allows for continuous industrial cell production and reduces the number of parts in the stack assembly process.
[0070] According to an embodiment of the present invention, the co-extrusion process, perfluorosulfonyl fluoride membranes are extruded from perfluorosulfonyl fluoride granules. Furthermore, the perfluorosulfonyl fluoride membranes are pretreated before they are used as ion exchanger membranes.
[0071] According to an embodiment of the present invention, for commercial pretreatment, the fluoride groups are exchanged for hydroxyl groups using sodium hydroxide. The sodium sulfonate groups are then protonated by storage in 1M sulfuric acid. The following reaction TIFF2024160203000002.tif22170 occurs.
[0072] For the production of tubular cells, the membranes are extruded onto tubular electrodes made in the embodiment of TiAlV coated with catalyst. These materials may corrode during pretreatment with sodium hydroxide. A milder pretreatment process may be required to hydrolyze the stable SF bonds in the membrane to withstand the harsh reaction conditions. The stable SF bonds may be activated in the presence of a suitable catalyst, and the fluoride groups can undergo nucleophilic exchange in a reaction known as sulfur (VI)-fluoride exchange (SuFEx). This type of reaction, click chemistry, has been used in polymer chemistry to build the core backbone of polymers, functionalize monomers as side chains, and provide post-polymerization modification of polymers.
[0073] In the presence of sufficient catalyst, fluoride ions are converted to H + and / or R3Si + Transfer from a strong covalent bond to the leaving group is aided by interactions with
[0074] Therefore, in the present invention, triethylsilanol is used as a catalyst in the presence of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) to achieve hydrolysis using less corrosive chemicals. The reaction is a two-step reaction in which the first step is the formation of an intermediate and the second step is the protonation of this intermediate to obtain the desired sulfonic acid group. The feasibility of hydrolysis of sulfonyl fluoride groups to sulfonic acids by a less aggressive process using triethylsilanol is demonstrated by the following reaction: Shown in TIFF2024160203000003.tif33170.
[0075] In particular, the pretreated membranes are characterized to ensure good proton diffusion, in-plane conductivity, ion exchange capacity, water absorption, and stability of the coextruded half-cells during the pretreatment process.
[0076] According to an embodiment of the present invention, the tubular cation exchange membrane is manufactured by extrusion of perfluorosulfonyl fluoride / PTFE copolymer granule material VM-Fumasep® FFT (FumaTech BWT) with a particle size of 2 mm. For hydrolysis of sulfonyl fluoride groups, N,N-dimethylformamide (DMF, ≧99.9%, UV / IR grade, Carl Roth GmbH), DBU (>99%, Sigma Aldrich), triethylsilanol (97%, Thermo Scientific), and sodium hydroxide (10%, Carl Roth GmbH) are used. For protonation, 1 M sulfuric acid (diluted from 75% sulfuric acid, pure, Carl Roth GmbH) was used. Alternatively, ultrapure water (PURELAB® Ultra, Elga LabWater) may be used.
[0077] In an embodiment of the present invention, the hydrolysis of sulfonyl fluoride groups was carried out by the SuFEx reaction (reaction 2). In particular, the membrane is stored in a solution of Et3SiOH, DBU, and DMF at 70°C with shaking at 200 rpm for 24 h. Then, the membrane is washed with water and stored in water at room temperature for 24 h. Furthermore, the water is changed at least three times during storage. Furthermore, the membrane is protonated in 1 M sulfuric acid at room temperature at 60 rpm for 24 h and stored in 1 M sulfuric acid at room temperature overnight. Then, the membrane is dried at 80°C for 5 h and weighed to obtain the dry mass. The water absorption is calculated according to the following equation:
[0078] W 吸収 (%)=[(W 湿潤 -W 乾燥 ) / W 乾燥 ](%)×100 Calculated using the formula:
[0079] W 湿潤 -Wet mass of membrane
[0080] W 乾燥 - Dry weight
[0081] The membranes were then stored in 0.5 M NaCl solution at room temperature for 24 h, so that all protonated sulfonic acid groups were exchanged with sodium cations. The membranes were then stored in 1 M sulfuric acid for 24 h, and the final Na concentration was determined by inductively coupled plasma optical emission spectroscopy (ICP-OES). + The concentration was measured. The IEC is calculated using the following equation: IEC(mmol / g)=[Na]·V H2SO4 / W 乾燥 Mw Na It is calculated using During the ceremony, [Na] is the concentration of sodium in mg / L measured by ICP-OES; V H2SO4 is the volume of 1 M sulfuric acid in L used to reprotonate the membrane, W 乾燥 is the dry mass of the membrane in g, Mw Na is the molar mass of sodium in mg / mmol.
[0082] In an embodiment of the present invention, the ion exchange membrane 3 may comprise a polymer electrolyte membrane (PEM).
[0083] In an embodiment of the present invention, Raman spectroscopy of the films is carried out after storing them in 1 M sulfuric acid at room temperature overnight. Measurements are carried out using a sample holder with which water can be inserted so that the films remain hydrated. A confocal microscopic Raman spectrometer (InVia Reglex, Renishaw, Kingswood, UK) is used, with a spot size of 1 mm and a high-resolution diffraction gratin density of 1800 grooves mm-1, a laser beam (He-Ne, 633 nm, 0.85 mW) focused through a 50x objective lens (DM2500, Leica, Mannheim, Germany). A single spectrum is acquired by accumulating 50 spectra with an integration time of 10 s. To determine the thermal degradation of the films, before and after images are collected, as shown in Figure 3B and Figure 3C.
[0084] 3D and 3D, proton diffusion was measured using an H-cell, in which the membrane was cut and rolled into a flat membrane and separated into two compartments by a membrane clamped between two PTFE gaskets. The surface of the membrane used was 0.196 cm. 2 and is designated by the sealing area of the gasket. One of the compartments is filled with 0.1 M HCl and the other with 0.5 M NaCl. + Due to the different concentrations of NaCl, there is diffusion from the compartment with the higher concentration to the compartment with the lower concentration. Following the increasing proton concentration in the NaCl compartment, pH measurements were taken over 30 min, and the proton diffusion in the membrane is given by the equation J H d =n B / A·t It is calculated using During the ceremony, J H d is μmol / cm 2 is the proton diffusion in min, n B is the increase in proton concentration in the NaCl compartment in μmol A is cm2 is the area of the membrane at t is the time at s.
[0085] Before measuring the in-plane conductivity, the membrane was protonated in sulfuric acid at room temperature overnight and washed several times with water to remove sulfuric acid residues. A four-electrode setup MK3 cell (FUMATECH BWT) was used, placing the membrane on the four platinum electrodes of the probe head and placing the cap of the probe head on the membrane so that the insulating Teflon side of the cap faces the sample. The cap was fixed by hand with two screws. To avoid dehydration of the membrane, the cell was immersed in demineralized water at room temperature. Single frequency impedance measurements were performed with a Gamry potentiostat (Gamry ref. 3000 potentiostat / galvanostat / ZRA) at 1000 Hz, with an open circuit voltage and an amplitude of 10 mV. Proton conductivity was calculated using the equation, σ=L / W·T·R, where σ is the in-plane conductivity in S / cm, L is the distance between the electrodes in cm, B is the width of the membrane in cm, D is the thickness of the membrane in cm, and R is the resistance measured in Ohms.
[0086] In a preferred embodiment of the present invention, the stability test of the coextruded half-cells was carried out using optimized hydrolysis reaction parameters. The reactant concentrations and reaction duration were varied until the optimum condition for proton conductivity was achieved. First, the reactants were optimized and the concentrations used are listed in Table 1. TIFF2024160203000004.tif94170
[0087] 5 mL of DMF is used as the solvent, and the reaction is carried out at 70° C., 200 rpm for 24 h. The measured conductivity is compared to Fumasep® F10100 membrane (FumaTech BWT), a commercially available PFSA planar membrane. The conductivity achieved with membrane 1d was comparable to that of the commercial one. Therefore, these reactant concentrations (1 equivalent of membrane, 1 equivalent of Et3SiOH, and 1 equivalent of DBU) are used.
[0088] The reproducibility of the results is studied, as illustrated in Table 2. Two extruded membranes are conditioned with optimal reactant concentrations (1 equivalent of membrane, 1 equivalent of Et3SiOH, and 1 equivalent of DBU) and the proton conductivity is measured and compared with sample 1d. The conductivity of three membranes hydrolyzed with the same concentrations of reactants. Since the standard deviation was 3%, it can be concluded that the hydrolysis reaction is sufficiently reproducible. TIFF2024160203000005.tif38170
[0089] The hydrolysis reaction was carried out by pretreating the membrane with optimized reactant concentrations at room temperature. The conditioning time was increased at 24 h intervals. After each interval, the membrane was stored in water for 24 h and in 1 M H2SO4 for another 24 h. The conductivity was then measured and the membrane was again stored in the same solution for another 24 h. The reaction time was increased until a conductivity >90 mS / cm was achieved. Table 3 shows the reaction time and membrane conductivity, respectively. TIFF2024160203000006.tif70170
[0090] In one embodiment of the present invention, the stability testing of the coextruded half-cells includes physicochemical characterization. After the hydrolysis reaction is completed, all the membranes are characterized to ensure that the physicochemical properties of the membranes are conditioned. Water imbibition swelling ratio and ion exchange capacity are calculated, and Raman and NMR measurements are performed.
[0091] The ion exchange membrane 3 may comprise a tubular membrane welded or extruded to the inner electrode 4 as seen in FIGS.
[0092] According to an embodiment of the present invention, multiple extrusion techniques include simple extrusion, multi-layer extrusion, woven extrusion, and the like.
[0093] The inner electrode 4 may include a first end and a second end shaped by additive manufacturing 102. In an embodiment of the invention, the inner electrode 4 comprises a Ti-Fleece GDE.
[0094] For extrusion type production of the tubular water electrolysis cell 100, the outer current collector 1 and the inner current collector 5 may further utilize multiple extrusion techniques.
[0095] The outer and inner electrodes 2, 4 may comprise porous outer and inner electrodes 2, 4 having an effective active surface area for enhancing the electrochemical reaction depending on the open porosity and pore size.
[0096] In preferred embodiments of the present invention, the outer electrode 2 and the inner electrode 4 may include various configuration parameters of pores and coatings.
[0097] In one embodiment of the present invention, the diameter and length of the pores formed in the outer electrode 2 and the inner electrode 4 may be adjustable. Furthermore, the inner pore walls of the outer electrode 2 and the inner electrode 4 may be uniformly coated with a thin (<20 nm) to ultra-thin (<2 nm) layer of electrocatalytically active material by atomic layer deposition (ALD) 104.
[0098] The tubular electrochemical cell 100 further includes an inner current collector 5 embedded in the surrounding wall of the longitudinally extending inner electrode 4. In addition, the inner current collector 5 may extend across a first end and a second end of the inner current electrode 4.
[0099] In addition, as additional components of such a cell, the inner current collector 5 and the outer current conductor 1 may also be produced by extrusion 106, which has the potential to significantly simplify the production of the tubular water electrolysis cell 100.
[0100] FIG. 4 illustrates a perspective view of the individual components of a PEM water electrolysis device according to an embodiment of the invention. One half-cell serves as a flow-by electrode and is formed by a tubular membrane electrode assembly made of titanium hollow fiber and titanium nonwoven fabric, respectively. The other half-cell is made of graphite felt. In addition to the straightforward configuration with flow channels, titanium flow fields with multiple starting helices are also available. Both half-cells are separated by a tubular ion exchanger membrane.
[0101] FIG. 5 illustrates a flow chart of a method 500 for a method for conditioning and / or hydrolyzing an extruded membrane according to an embodiment of the present invention.
[0102] At 502, converting water into hydrogen using a plurality of water electrolyzers (WEs).
[0103] At 504, sealing the half-cells of the tubular cell 100 manufactured by co-extrusion technique to obtain a higher electrode volume per membrane area ratio.
[0104] At 506, extruding a perfluorosulfonyl fluoride membrane from the perfluorosulfonyl fluoride granules. In an embodiment of the present invention, the perfluorosulfonyl fluoride membrane is commercially pretreated and the fluoride groups are exchanged for hydroxyl groups using sodium hydroxide. When the perfluorosulfonyl fluoride membrane is commercially pretreated, the sodium sulfonate groups are protonated by 1M sulfuric acid.
[0105] At 508, a pretreatment technique is used to increase the ionic conductivity of an extruded perfluorosulfonyl fluoride membrane prior to using the perfluorosulfonic acid membrane as a cation exchange membrane.
[0106] At 510, applying a milder pretreatment technique by activating the S-F bond and performing a nucleophilic exchange of the fluoride group. According to an embodiment of the invention, the reaction may be sulfur(VI)-fluoride exchange (SuFEx) involving the exchange of the fluoride group. Furthermore, storage in sulfuric acid may involve protection of the ester to obtain a sulfonic acid group.
[0107] In 512, the sulfonyl fluoride groups are hydrolyzed to sulfonic acid groups using triethylsilanol.
[0108] In one embodiment of the present invention, commercially pretreated perfluorosulfonic acid (PFSA) perfluorosulfonyl fluoride membranes are characterized by a number of parameters, including but not limited to, proton diffusion, in-plane conductivity, ion exchange capacity, and water uptake.
[0109] In one embodiment of the invention, the method 500 further includes calculating parameters such as water absorption, swelling ratio, and ion exchange capacity using measurement techniques. According to an embodiment of the invention, the measurement techniques may include Raman spectroscopy and nuclear magnetic resonance (NMR) techniques, among others.
[0110] In one embodiment of the invention, the method further comprises transferring a fluoride ion from the strong covalent bond to a leaving group, which, if a catalyst is used, can be H + and / or R3Si + The catalyst comprises triethylsilanol in the presence of 1,8 diazabicyclo[5.4.0]undec-7-ene (DBU).
[0111] According to one implementation of the present invention, the method 500 may include optimizing a plurality of reactants. The perfluorosulfonyl fluoride membrane is conditioned at room temperature with the optimized reactant concentrations for a predetermined conditioning time. In an embodiment of the present invention, the predetermined conditioning time is increased at 24 h intervals, and after each interval, the pretreated perfluorosulfonyl fluoride membrane is stored in water for 24 h and in 1 M H2SO4 for another 24 h.
[0112] While the invention has been described in connection with what is believed to be its most practical and various embodiments, it will be understood that the invention is not to be limited to the disclosed embodiments, but on the contrary, is intended to cover various modifications and equivalent arrangements included within the scope of the appended claims.
[0113] Those skilled in the art will recognize that the units and algorithm steps, in combination with the examples illustrated in the embodiments disclosed herein, may be implemented by electronic hardware, computer software, or a combination thereof.
Claims
1. A method (500) for conditioning and / or hydrolysis of an extruded membrane, comprising: an ion exchange process in a partitioned electrochemical cell using a cation exchanger membrane; pretreatment of a perfluorosulfonyl fluoride membrane extruded from granules of a polymer comprising perfluorinated polymer chains substituted with sulfonyl fluoride groups; Increasing the ionic conductivity of an extruded perfluorosulfonyl fluoride membrane using a pretreatment technique; applying a pretreatment technique by activating the S-F bonds and carrying out a nucleophilic exchange of the fluoride groups of the extruded membrane in a reaction using triethylsilanol to hydrolyze the sulfonyl fluoride groups to sulfonic acids; optimizing the concentration of reactants and the duration of the reaction to a polymer comprising perfluorinated polymer chains substituted with sulfonic acid groups; As a cation exchange membrane, a perfluorosulfonic acid membrane of a polymer containing perfluorinated polymer chains substituted with sulfonic acid groups is used. The method includes:
2. 10. The method (500) of claim 1, wherein the pre-processing technique additionally calculates the parameters proton diffusion, in-plane conductivity, ion exchange capacity, water absorption, or any combination of the foregoing.
3. 3. The method (500) of claim 2, comprising using measurement techniques to calculate parameters such as water absorption, swelling ratio, and ion exchange capacity.
4. The method (500) of claim 3, wherein the measurement techniques include Raman spectroscopy and nuclear magnetic resonance (NMR) techniques, or any of the aforementioned combinations thereof, or the like.
5. H + and / or R 3 S + 10. The method of claim 1, further comprising assisting the hydrolysis of the fluoride ions by interaction with a hydrolysis catalyst.
6. 6. The method (500) of claim 5, wherein the catalyst comprises triethylsilanol in the presence of 1,8 diazabicyclo[5.4.0]undec-7-ene (DBU).
7. The reaction was, Exchange of the fluoride group to form an intermediate and protonation of this intermediate to obtain a sulfonic acid group. The method (500) of claim 1, wherein the sulfur(VI)-fluoride exchanged (SuFEx) comprises:
8. 8. The method (500) of claim 7, wherein the perfluorosulfonyl fluoride membrane is pretreated at room temperature for a predetermined conditioning time.
9. The pre-determined pretreatment time was increased in 24 h intervals, and after each interval, the pre-treated perfluorosulfonyl fluoride membrane was incubated in water for 24 h and in 1 M H 2 9. The method of claim 8 (500), wherein the data is stored in SO4.
10. 10. The method of claim 1, comprising hydrolyzing a perfluorosulfonyl fluoride membrane using a concentration of reactants for pretreatment of the perfluorosulfonyl fluoride membrane to achieve an increase in conductivity.
11. 10. The method of claim 1, comprising measuring the conductivity of a hydrolyzed perfluorosulfonic acid (PFSA) membrane.
12. Hydrolyzed perfluorosulfonic acid (PFSA) membranes were placed in water and in 1M H 2 SO 4 10. The method of claim 1 (500), comprising storing in solution and measuring the conductivity of the hydrolyzed perfluorosulfonic acid membrane until a conductivity of >90 mS / cm is achieved.
13. The method (500) of claim 1, wherein the co-extrusion technique comprises simple extrusion, multi-layer extrusion, woven extrusion, or any of the aforementioned combinations thereof.
14. The method (500) of claim 1, comprising stability testing of the coextruded half-cells by calculating water absorption, swelling ratio, and ion exchange capacity, as well as physicochemical characterization of the hydrolyzed perfluorosulfonic acid (PFSA) membranes by measuring Raman and NMR of the hydrolyzed perfluorosulfonic acid (PFSA) membranes.
