Lithium ion secondary battery

A lithium-ion secondary battery with a high Ni content lithium-transition metal composite oxide coated with tungsten or phosphorus and a Si-containing negative electrode material addresses cobalt depletion concerns, achieving low initial resistance and stable storage performance.

JP2024160552AActive Publication Date: 2024-11-14PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023075674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14
Estimated Expiration
2043-05-01

AI Technical Summary

Technical Problem

The increasing demand for lithium-ion secondary batteries has raised concerns about the depletion of cobalt (Co) used in their positive electrode active materials, leading to higher initial resistance and resistance during storage when the Co content is reduced.

Method used

A lithium-ion secondary battery design featuring a positive electrode with a high Ni content lithium-transition metal composite oxide coated with a tungsten or phosphorus compound, and a negative electrode containing a carbon material and a Si-containing material, which suppresses initial resistance and resistance increase during storage while reducing cobalt content.

Benefits of technology

The battery design effectively reduces cobalt usage while maintaining low initial resistance and preventing resistance increases during storage, enhancing the battery's performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160552000001_ABST
    Figure 2024160552000001_ABST
Patent Text Reader

Abstract

To provide a lithium ion secondary battery in which initial resistance and an increase in resistance during storage are suppressed while the cobalt content in a positive electrode active material is reduced.SOLUTION: In a lithium ion secondary battery 100 disclosed herein, a positive electrode active material 56 includes: a layer-structured lithium transition metal composite oxide 56a containing Li, Ni, and Mn; and a coating part 56c. The lithium transition metal composite oxide 56a has the content of Ni to the total of metal elements other than Li of 75 mol% or more, and is secondary particles which each are formed by aggregation of primary particles 56p. The coating part 56c includes a tungsten compound and / or a phosphorus compound. On the other hand, a negative electrode active material 66 contains a carbon material 66c and a Si-containing material 66s, and when the total amount of the negative electrode active material 66 is 100 mass%, the content ratio of a Si element in the negative electrode active material 66 is 5 mass% or more and 10 mass% or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to lithium-ion secondary batteries. [Background technology]

[0002] Lithium ion secondary batteries are suitable for use as driving power sources mounted on vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs), and the demand for lithium ion secondary batteries is rapidly expanding. As a positive electrode active material used in lithium ion secondary batteries, lithium transition metal composite oxides are used, and among them, lithium nickel cobalt manganese composite oxides containing Ni, Co, and Mn as shown in Patent Document 1 are exemplified. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-191662 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, in recent years, as the demand for lithium ion secondary batteries increases, there is concern about the depletion of cobalt (Co) used in lithium ion secondary batteries. As a countermeasure, it is considered to reduce the content of Co in the positive electrode active material. However, as a result of intensive research by the present inventors, it has been found that when the content of Co in the positive electrode active material is reduced, the initial resistance and the resistance during storage of the lithium ion secondary battery increase significantly.

[0005] The technology disclosed herein has been made in consideration of the above circumstances, and aims to provide a lithium-ion secondary battery in which the cobalt content in the positive electrode active material is reduced while suppressing the initial resistance and the increase in resistance during storage. [Means for solving the problem]

[0006] The technology disclosed herein relates to a lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, the positive electrode comprising a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprising a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, and a coating portion disposed on at least a part of a surface of the lithium transition metal composite oxide, the lithium transition metal composite oxide having a Ni content of 75 mol % or more with respect to a total of metal elements other than Li and being secondary particles formed by aggregation of primary particles, the coating portion comprising a tungsten compound and / or a phosphorus compound, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprising a carbon material and a Si-containing material, and a content ratio of Si element in the negative electrode active material being 5 mass % or more and 10 mass % or less when the total amount of the negative electrode active material is taken as 100 mass %.

[0007] According to this configuration, the composition of the positive electrode active material, specifically the content of Ni in the lithium transition metal composite oxide, is set to a predetermined range. Also, a coating portion containing a tungsten compound and / or a phosphorus compound is disposed on at least a part of the lithium transition metal composite oxide. Furthermore, the negative electrode active material contains a predetermined amount of a Si-containing material in addition to a carbon material. This makes it possible to provide a lithium ion secondary battery that reduces the cobalt content in the positive electrode active material while suppressing the initial resistance and the increase in resistance during storage. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic internal structure of a lithium-ion secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the configuration of a positive electrode active material according to one embodiment. [Figure 4] FIG. 4 is a schematic diagram showing the configuration of a negative electrode sheet (negative electrode) according to one embodiment. [Diagram 5] FIG. 5 is a view corresponding to FIG. 4 and showing the configuration of a negative electrode sheet (negative electrode) according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, some preferred embodiments of the lithium ion secondary battery disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure (for example, the general configuration and manufacturing process of a lithium ion secondary battery that does not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The lithium ion secondary battery disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field.

[0010] In the following drawings, the same reference numerals are used for components and parts that perform the same function, and duplicated explanations may be omitted or simplified. In this specification, the notation "A to B" indicating a range includes not only the meaning of A or more and B or less, but also the meanings of "preferably larger than A" and "preferably smaller than B." In this specification, a "lithium ion secondary battery" (hereinafter sometimes simply referred to as a "battery") refers to a general electricity storage device that uses lithium ions as a charge carrier and can be repeatedly charged and discharged by the transfer of charge associated with the lithium ions between the positive and negative electrodes.

[0011] Hereinafter, the present disclosure will be described in detail using as an example a flat prismatic lithium ion secondary battery having a flat electrode body and a flat battery case, but it is not intended that the present disclosure be limited to the embodiment described therein.

[0012] FIG. 1 is a cross-sectional view showing a schematic internal structure of a lithium ion secondary battery according to an embodiment. The lithium ion secondary battery 100 shown in FIG. 1 is a sealed battery constructed by housing a flat electrode body 20 and a non-aqueous electrolyte 80 in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the non-aqueous electrolyte 80. The positive electrode terminal 42 is electrically connected to the positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to the negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.

[0013] Fig. 2 is a schematic exploded view showing the configuration of an electrode body of a lithium ion secondary battery according to one embodiment. As shown in Figs. 1 and 2, the electrode body 20 has a configuration in which a strip-shaped positive electrode sheet 50 and a strip-shaped negative electrode sheet 60 are overlapped with two strip-shaped separators 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized positive electrode collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long-sized negative electrode collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are respectively joined to the positive electrode current collector 42a and the negative electrode current collector 44a. The positive electrode sheet 50 is an example of the "positive electrode" disclosed herein, and the negative electrode sheet 60 is an example of the "negative electrode" disclosed herein.

[0014] <Positive electrode> The positive electrode (positive electrode sheet 50) disclosed herein includes a positive electrode active material layer 54. As shown in Fig. 2, the positive electrode (positive electrode sheet 50) here includes a positive electrode current collector 52 and a positive electrode active material layer 54 supported by the positive electrode current collector 52. Note that, although the positive electrode active material layer 54 is illustrated only on one surface of the positive electrode current collector 52 in this embodiment, the positive electrode active material layer 54 may be provided on both surfaces of the positive electrode current collector 52.

[0015] 3 is a schematic diagram showing a configuration of a positive electrode active material 56 according to one embodiment. The positive electrode active material layer 54 contains a positive electrode active material 56 capable of reversibly absorbing and releasing charge carriers. The positive electrode active material 56 according to this embodiment includes a lithium transition metal composite oxide 56a serving as a base material, and a coating portion 56c disposed on at least a portion of the surface of the lithium transition metal composite oxide 56a. The coating portion 56c is typically disposed on the lithium transition metal composite oxide 56a by physical and / or chemical bonding.

[0016] The lithium transition metal composite oxide 56a according to this embodiment has a layered structure and contains lithium (Li), nickel (Ni), and manganese (Mn) as essential elements. The lithium transition metal composite oxide 56a according to this embodiment is a so-called high Ni content lithium transition metal composite oxide in which the content of Ni relative to the total of metal elements other than Li is 75 mol % or more. The high Ni content lithium transition metal composite oxide is an example of the "lithium transition metal composite oxide in which the content of Ni relative to the total of metal elements other than Li is 75 mol % or more" disclosed herein.

[0017] The positive electrode active material may contain a positive electrode active material other than the lithium transition metal composite oxide 56a within a range that does not impair the effects of the present disclosure (for example, less than 10 mass % relative to the total mass of the positive electrode active material, preferably 5 mass % or less). Also, the positive electrode active material may be composed only of the lithium transition metal composite oxide 56a.

[0018] From the viewpoint of high volumetric energy density of the lithium ion secondary battery, the content of Ni in the total of metal elements other than Li in the lithium transition metal composite oxide 56a is preferably 80 mol % or more, more preferably 90 mol % or more. On the other hand, from the viewpoint of high stability, the content of Ni in the total of metal elements other than Li is preferably 95 mol % or less, more preferably 93 mol % or less.

[0019] Examples of the lithium transition metal composite oxide 56a having a layered structure include lithium nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide. These may be used alone or in combination of two or more. It can be confirmed by a known method (e.g., X-ray diffraction method) that the particles of the high Ni-containing lithium transition metal composite oxide have a layered structure (i.e., a layered crystal structure).

[0020] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.

[0021] In some preferred embodiments, the lithium transition metal composite oxide 56a preferably has a composition represented by the following general formula (i): Li α Ni xMn y M z O2...Equation (i) In the above formula (i), x, y, z, and α respectively satisfy the following: 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1. M in the formula (i) is at least one element selected from the group consisting of Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.

[0022] In the above formula (i), α preferably satisfies 0.9≦α≦1.2, and more preferably satisfies 1.0≦α≦1.1. From the viewpoint of battery characteristics (e.g., energy density, cycle characteristics, and thermal stability), x preferably satisfies 0.8≦x≦0.95, and more preferably satisfies 0.8≦x≦0.9. From the viewpoint of, for example, energy density, thermal stability, and cost, y preferably satisfies 0.1≦y≦0.25, and more preferably satisfies 0.17≦y≦0.25. Z preferably satisfies 0≦z≦0.1, and more preferably satisfies 0≦z≦0.03, and further preferably is 0. In addition, in the above formula (i), "x+y+z=1" includes the case where x+y+z is 1, and is substantially regarded as 1 as long as the effect of the technology disclosed herein can be realized, and typically, x+y+z=0.95 to 1.1, and preferably x+y+z=0.99 to 1.05.

[0023] In some preferred embodiments, the lithium transition metal composite oxide 56a is preferably doped with W as an additive element. This stabilizes the layered structure of the lithium transition metal composite oxide 56a, and thus improves the initial resistance more preferably, and suppresses the elution of Mn into the non-aqueous electrolyte 80, thereby more preferably suppressing the increase in resistance during storage. When W is doped (solid-dissolved) as an additive element into the lithium transition metal composite oxide 56a, it is preferably doped at 0.1 to 0.5 mol %, and more preferably doped at 0.1 to 0.3 mol %, based on the total transition metal elements of the lithium transition metal composite oxide 56a other than W.

[0024] The lithium transition metal composite oxide 56a has the following relationship between the Co element content (mol) and the Mn element content (mol): 0≦Co / Mn≦0.42 It is preferable that the ratio be 0≦Co / Mn≦0.32. This controls the content ratio of Co and Mn in the lithium transition metal composite oxide 56a. In the above-mentioned relationship, the smaller the value of Co / Mn, the more effectively the cobalt content in the lithium transition metal composite oxide 56a can be reduced while suppressing the initial resistance and the increase in resistance during storage. Therefore, it is preferable that the ratio be 0≦Co / Mn≦0.32, more preferably 0≦Co / Mn≦0.25, and even more preferably 0≦Co / Mn≦0.21.

[0025] In lithium transition metal composite oxides used in conventional lithium ion secondary batteries, the content ratio of Co element to metal elements other than Li is typically about 10 mol % to 40 mol %. However, since cobalt resources are limited, in this embodiment, it is preferable to reduce the Co content of the lithium transition metal composite oxide 56a compared to the conventional case. Therefore, in some preferred embodiments, the content ratio of Co to the total of metal elements other than Li is, for example, preferably 5 mol % or less, more preferably 3 mol % or less, and even more preferably 0 mol % (i.e., Co-free).

[0026] As shown in FIG. 3, the lithium transition metal composite oxide 56a is in the form of secondary particles in which a plurality of primary particles 56p are typically aggregated by physical or chemical bonding forces. The number of primary particles 56p of the lithium transition metal composite oxide 56a constituting the secondary particles of the lithium transition metal composite oxide 56a is not particularly limited, but is, for example, approximately 10 or more, preferably approximately 30 or more, and more preferably approximately 50 or more. The number of primary particles 56p is not particularly limited, but may be, for example, approximately 120 or less. In this specification, the term "primary particle" refers to the smallest unit of particles constituting the positive electrode active material, and more specifically, refers to the smallest unit determined from the geometric shape of the appearance observed under an electron microscope. In this specification, an aggregate formed by aggregation of 10 or more such primary particles 56p is called a "secondary particle".

[0027] A coating portion 56c is disposed on at least a part of the surface of the lithium transition metal composite oxide 56a. The coating portion 56c contains a tungsten compound and / or a phosphorus compound. By providing the coating portion 56c having such a configuration, the Li ion conductivity of the lithium transition metal composite oxide 56a is improved. In other words, the inflow and outflow of Li ions on the surface of the lithium transition metal composite oxide 56a is more favorably performed. Therefore, the initial resistance can be reduced. The coating portion 56c may contain either a tungsten compound or a phosphorus compound, or may contain both a tungsten compound and a phosphorus compound. The fact that the coating portion 56c contains a tungsten compound and / or a phosphorus compound can be confirmed, for example, by analysis using energy dispersive X-ray spectroscopy (TEM-EDX) using a transmission electron microscope (TEM).

[0028] The tungsten compound contained in the coating portion 56c is not particularly limited, but examples thereof include lithium tungstate, tungsten oxide, nickel tungstate, and cobalt tungstate. Among them, it is preferable to use lithium tungstate as the tungsten compound. The atomic ratio of Li and W constituting the lithium tungstate is not particularly limited. For example, lithium tungstate may be Li2WO4, Li4WO5, Li6WO6, Li2W4O 13 , Li2W2O7, Li6W2O9, Li2W2O7, Li2W5O 16 , Li9W 19 O 55 , Li3W 10 O 30 , Li 18 W5O 15 Among these, Li p WO q It is preferable that the composition be expressed by (0.3≦p≦6.0, 3.0≦q≦6.0), and it is particularly preferable that the composition be expressed by Li2WO4. The proportion of the tungsten compound as coating portion 56c may be, for example, 0.1 to 1.0 mol %, and is preferably 0.1 to 0.5 mol %, calculated as tungsten (W) when the total amount of Ni and Mn in lithium transition metal composite oxide 56a is taken as 100 mol %.

[0029] The phosphorus compound contained in the coating portion 56c is not particularly limited, but may be, for example, lithium phosphate (Li3PO4), dilithium hydrogen phosphate (Li2HPO4), lithium dihydrogen phosphate (LiH2PO4), diphosphorus pentoxide (P2O5), orthophosphoric acid (H3PO4), pyrophosphoric acid (H4P2O7), triphosphoric acid (H5P3O 10 ), polyphosphoric acid (HO(HPO3) n H). Among them, it is preferable that the covering portion 56c contains lithium phosphate (Li3PO4) as the phosphorus compound. The ratio of the phosphorus compound as the covering portion 56c can be, for example, 0.1 to 1.0 mol %, and preferably 0.1 to 0.5 mol %, calculated as phosphorus (P) when the total amount of Ni and Mn in the lithium transition metal composite oxide 56a is taken as 100 mol %.

[0030] In some preferred embodiments, the coating portion 56c may further include aluminum oxide (Al2O3). More specifically, aluminum oxide has a function of trapping hydrogen fluoride gas (hydrofluoric acid) generated by decomposition of the nonaqueous electrolyte 80. This makes it possible to suppress dissolution of Mn into the nonaqueous electrolyte 80 caused by a reaction between the positive electrode active material 56 (lithium transition metal composite oxide 56a) and hydrogen fluoride gas. Therefore, by disposing aluminum oxide on the surface, it is possible to more suitably suppress an increase in resistance during storage. The proportion of aluminum oxide as the coating portion 56c may be, for example, 0.1 to 0.5 mol %, and is preferably 0.3 to 0.5 mol %, calculated as aluminum (Al) when the total amount of Ni and Mn in the lithium transition metal composite oxide 56a is taken as 100 mol %.

[0031] In addition to the above-mentioned configuration, the covering portion 56c may further contain other elements as long as the effects of the technology disclosed herein are not significantly impaired. Examples of such elements include transition metal elements, other metal elements, and semimetal elements. Specific examples include B, Na, Mg, Ca, Si, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Mo, In, Sn, La, Ce, and Y. In addition, the other elements that may be contained in the covering portion 56c may be contained in the form of a compound (e.g., an oxide or a Li compound).

[0032] The method for forming the coating portion 56c is not particularly limited, and the coating portion 56c can be formed by a conventionally known method. For example, the coating portion 56c can be formed by mixing the lithium transition metal composite oxide 56a and the raw material for forming the coating portion 56c and drying the mixture. The mixing may be a dry mixing or a wet mixing.

[0033] The coating portion 56c is preferably disposed at least on the surface of the secondary particle of the lithium transition metal composite oxide 56a. In this case, the coverage of the positive electrode active material 56 by the coating portion 56c may be 60% or more. The fact that the coating portion 56c is disposed on the surface of the secondary particle and the ratio (coverage) of the portion covered by the coating portion 56c can be confirmed by, for example, XPS (X-ray Photoelectron Spectroscopy) analysis of the positive electrode active material 56.

[0034] When the lithium transition metal composite oxide 56a has voids, the coating portion 56c is preferably present inside the secondary particles in addition to or instead of the surface of the secondary particles. Specifically, the coating portion 56c is preferably present on the surface of the primary particles 56p inside the secondary particles. The amount of the coating portion 56c present inside the secondary particles may be greater or less than the amount of the coating portion 56c present on the surface of the secondary particles. This allows the effect of the technology disclosed herein to be exerted at a higher level. The presence of the coating portion 56c inside the secondary particles can be confirmed by LA-ICP-MS (Laser Ablation Inductively Coupled Plasma Mass Spectrometry) analysis.

[0035] The average particle diameter (D50) of the lithium transition metal composite oxide 56a (secondary particles) is not particularly limited. From the viewpoint of particularly high filling property of the positive electrode active material layer 54 and high volumetric energy density of the lithium ion secondary battery 100, the average particle diameter (D50) of the lithium transition metal composite oxide 56a (secondary particles) is preferably 5 μm to 30 μm, and more preferably 10 μm to 20 μm.

[0036] In this specification, the term "average particle size (D50)" refers to the median size (D50) and also refers to the particle size corresponding to a cumulative frequency of 50 volume % from the fine particle side with a small particle size in the volume-based particle size distribution based on the laser diffraction / scattering method. Therefore, the average particle size (D50) can be determined using a laser diffraction / scattering type particle size distribution measuring device or the like.

[0037] The average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a is not particularly limited. For example, from the viewpoint of the energy density and output characteristics of the positive electrode active material 56, the average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a is 0.05 μm to 2.5 μm, preferably 1.2 μm or more, more preferably 1.5 μm or more, and further preferably 1.7 μm or more. On the other hand, from the viewpoint of higher cycle characteristics of the positive electrode active material 56, the average particle diameter of the primary particles 56p of the lithium transition metal composite oxide 56a is preferably 2.2 μm or less, more preferably 2.1 μm or less.

[0038] The "average particle size of the primary particles of the lithium transition metal composite oxide" refers to the average particle size of the major axis of the primary particles 56p of the lithium transition metal composite oxide 56a, which is grasped from a cross-sectional electron microscope image of the lithium transition metal composite oxide 56a and refers to the average value of the major axes of a plurality of primary particles 56p selected arbitrarily. The plurality of primary particles 56p may be, for example, 20 or more. Specifically, the average particle size of the primary particles 56p is determined, for example, by a cross-section polisher process to prepare a cross-sectional observation sample of the lithium transition metal composite oxide 56a. Next, a SEM image of the cross-sectional observation sample of the lithium transition metal composite oxide 56a is obtained using a scanning electron microscope (SEM). Then, the major axes of a plurality of primary particles 56p arbitrarily selected from the SEM image are determined using image analysis type particle size distribution measurement software (for example, "Mac-View"), and the average value is calculated.

[0039] The primary particles 56p of the lithium transition metal composite oxide 56a are typically substantially spherical. However, they may be of an indefinite shape. In this specification, the term "substantially spherical" refers to a shape that can be regarded as roughly a sphere as a whole, and an average aspect ratio (major axis / minor axis ratio) based on a cross-sectional observation image taken with an electron microscope is, for example, 1 to 1.5.

[0040] The average particle diameter (D50) of the secondary particles of the lithium transition metal composite oxide 56a is not particularly limited. From the viewpoint of improving the energy density and output characteristics of the positive electrode active material layer, the average particle diameter (D50) of the secondary particles of the lithium transition metal composite oxide 56a is preferably 5 μm to 30 μm, more preferably 10 μm to 20 μm. In this specification, the term "average particle diameter (D50)" refers to the median diameter (D50) and also means a particle diameter corresponding to a cumulative frequency of 50 volume % from the smaller particle diameter side (fine particle side) in a volume-based particle size distribution based on a laser diffraction / scattering method. Therefore, the average particle diameter (D50) can be obtained using a laser diffraction / scattering type particle size distribution measuring device or the like.

[0041] In this embodiment, the lithium transition metal composite oxide 56a has a so-called solid structure formed by simple aggregation of primary particles 56p. However, the lithium transition metal composite oxide 56a is not limited to this, and may have voids inside the secondary particles originating from gaps between the aggregated primary particles 56p. The voids may or may not be open. When the voids are open, one void may have two or more openings.

[0042] When the lithium transition metal composite oxide 56a (secondary particles) has voids, the porosity is preferably 2% or more and 10% or less. The porosity of the secondary particles is, for example, 2% or more, and may be 3% or more, or 5% or more. By making the porosity of the secondary particles greater than a predetermined value, the initial resistance of the lithium ion secondary battery 100 can be reduced. In addition, appropriate voids can be secured inside the secondary particles of the lithium transition metal composite oxide 56a. In addition, when the lithium transition metal composite oxide 56a has the coating portion 56c, the coating portion 56c can be evenly arranged up to the inside of the secondary particles. On the other hand, if the porosity of the secondary particles is excessive (typically, the porosity exceeds 10%), the resistance increase during storage increases. Therefore, the porosity of the secondary particles is, for example, 10% or less, and may be 9% or less, or 8% or less. In this specification, the "average porosity of the lithium transition metal composite oxide" is understood from a cross-sectional electron microscope image of the lithium transition metal composite oxide, and the average value can be calculated by measuring the porosity of a plurality of arbitrarily selected secondary particles. The number of secondary particles may be, for example, 20 or more. First, a cross-sectional observation sample of the lithium transition metal composite oxide 56a is prepared by cross-section polisher processing or the like. Next, a SEM image of the cross-sectional observation sample is obtained using a scanning electron microscope (SEM). From the obtained SEM image, the area of ​​the entire secondary particles and the total area of ​​all voids inside the secondary particles are calculated using image analysis software (e.g., "ImageJ"). Then, the following formula (ii): Porosity (%) = (total area of ​​all voids / total area of ​​secondary particles) x 100...(ii) The porosity is calculated using the formula below, and the average value is calculated.

[0043] The porosity of the lithium transition metal composite oxide 56a can be adjusted, for example, by changing the synthesis conditions when a hydroxide, which is a precursor of the lithium transition metal composite oxide 56a, is synthesized by a crystallization method. Specifically, in the crystallization method, a raw material aqueous solution containing metal elements other than lithium and a pH adjusting solution are added to a reaction solution to synthesize the hydroxide. The porosity of the hydroxide can be adjusted by changing the pH value of the reaction solution and the stirring speed at this time. The hydroxide is mixed with a lithium source compound (e.g., lithium hydroxide, etc.) and baked to obtain the lithium transition metal composite oxide 56a in the form of secondary particles and with an adjusted porosity.

[0044] The BET specific surface area of ​​the lithium transition metal composite oxide 56a is not particularly limited. Since this can impart excellent output characteristics to the lithium ion secondary battery 100, the BET specific surface area of ​​the lithium transition metal composite oxide 56a is preferably 0.50 m 2 / g~0.85m 2 / g, more preferably 0.55m 2 / g~0.80m 2 The BET specific surface area of ​​the lithium transition metal composite oxide 56a can be measured by a nitrogen adsorption method using a commercially available specific surface area measuring device.

[0045] The content of the positive electrode active material 56 in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material 56 relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is, for example, 80 mass% or more, preferably 87 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 97 mass% or more.

[0046] The positive electrode current collector 52 may be a known material used in the lithium ion secondary battery 100, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). Aluminum foil is preferable as the positive electrode current collector 52 according to this embodiment.

[0047] The dimensions of the positive electrode current collector 52 are not particularly limited and can be appropriately determined according to the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness of the positive electrode current collector 52 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.

[0048] <Negative electrode> The negative electrode (negative electrode sheet 60) disclosed herein includes a negative electrode active material layer 64. As shown in Fig. 2, the negative electrode (negative electrode sheet 60) includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported on the negative electrode current collector 62. Note that, although the negative electrode active material layer 64 is illustrated only on one surface of the negative electrode current collector 62 in this embodiment, the negative electrode active material layer 64 may be provided on both surfaces of the negative electrode current collector 62.

[0049] The negative electrode active material layer 64 contains a negative electrode active material 66 capable of reversibly absorbing and releasing charge carriers. FIG. 4 is a schematic diagram showing the configuration of a negative electrode sheet 60 (negative electrode) according to one embodiment. The negative electrode active material 66 according to this embodiment essentially contains a carbon material 66c and a Si-containing material 66s. However, the negative electrode active material 66 may further contain other negative electrode active materials in addition to the carbon material 66c and the Si-containing material 66s. Although not shown here for convenience of explanation, the negative electrode active material layer 64 may contain a conductive material, a binder, a thickener, and the like in addition to the negative electrode active material 66.

[0050] As the carbon material 66c, for example, graphite, hard carbon, soft carbon, etc. are used, and among them, graphite is preferably used. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.

[0051] The average particle size of the carbon material 66c is not particularly limited, but is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle size (D50) of the carbon material can be determined, for example, by a laser diffraction scattering method.

[0052] The Si-containing material 66s includes, for example, silicon (Si), SiO x (0.05 < x < 1.95) silicon oxide represented by, Si-C composite containing Si particles in carbon particles, lithium silicate (Li x Si y O z ) and the like. As the Si-containing material 66s, silicon, silicon oxide, and Si-C composite can be preferably used. Further, as the Si-containing material 66s, an alloy composed of Si and an element other than Si can be used. Examples of the element other than Si include Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, Ti, and the like. By including the Si-containing material 66s in the negative electrode active material 66, formation of a coating layer starting from Mn eluted from the positive electrode active material on the surface of the negative electrode active material layer 64 can be suppressed. Therefore, an increase in resistance during storage can be preferably suppressed.

[0053] The average particle diameter of the Si-containing material 66s is not particularly limited, but is, for example, 0.1 μm or more and 50 μm or less, preferably 1 μm or more and 25 μm or less, and more preferably 5 μm or more and 20 μm or less. The average particle diameter (D50) of the carbon material can be determined by, for example, the laser diffraction scattering method.

[0054] In the present embodiment, when the total amount of the negative electrode active material 66 is 100% by mass, the content ratio of the Si element in the negative electrode active material 66 is 5% by mass or more and 10% by mass or less from the viewpoint of achieving both the effect of suppressing an increase in resistance during storage and the capacity retention rate. When the content ratio of the Si element is small (typically less than 5% by mass), the effect of suppressing the formation of the coating layer starting from Mn eluted from the positive electrode active material on the surface of the negative electrode active material layer 64 cannot be preferably obtained, and the effect of suppressing the storage resistance cannot be obtained well. On the other hand, when the content ratio of the Si element is too high (typically exceeding 10% by mass), the capacity retention rate during storage decreases.

[0055] The distribution of the Si-containing material 66s in the negative electrode active material layer 64 is not particularly limited, and the Si-containing material may be dispersed throughout the entire negative electrode active material layer 64, may be concentrated and dispersed in the upper layer (the surface layer side of the negative electrode active material layer 64) of the negative electrode active material layer 64, or may be concentrated and dispersed in the lower layer (the negative electrode current collector 62 side) of the negative electrode active material layer 64. In some preferred embodiments, the Si-containing material 66s is preferably concentrated and dispersed in the upper layer (corresponding to the negative electrode upper layer 164u in FIG. 5) of the negative electrode active material layer 64, as shown in the second embodiment (FIG. 5) described later. As shown in FIG. 4, in this embodiment, the Si-containing material 66s is dispersed almost uniformly throughout the entire negative electrode active material layer 64. Note that "concentrated and dispersed in the upper layer of the negative electrode active material layer 64" is an example of "the content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%" disclosed herein.

[0056] The negative electrode active material layer 64 may contain components other than the negative electrode active material 66, such as a conductive material, a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc., which have been used conventionally in lithium secondary batteries, may be used without any particular limitation. As the thickener, for example, carboxymethyl cellulose (CMC) may be used.

[0057] The negative electrode active material layer 64 preferably further contains a conductive material. As the conductive material, for example, carbon black (CB) such as acetylene black (AB) or Ketjen black, carbon nanotubes (CNT), carbon fibers such as vapor grown carbon fiber (VGCF), activated carbon, graphite, and other carbon materials can be suitably used, and among them, it is preferable to contain CNT. By containing CNT as the conductive material, the capacity retention rate can be suitably maintained. As the CNT, any one of single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT) may be used, and these may be used alone or in combination of two or more. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to use SWCNT. When CNT is used as the conductive material of the negative electrode active material layer 64, it is preferable to contain 0.5 mass % or less of CNT with respect to the entire negative electrode active material layer.

[0058] The content of the negative electrode active material 66 in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.

[0059] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm, when the negative electrode active material layer 64 is provided only on one surface of the negative electrode current collector 62. When the negative electrode active material layer 64 is provided on both surfaces of the negative electrode current collector 62, the thickness of each surface (each of the thicknesses of one surface and the other surface) is, for example, 10 μm to 200 μm, and preferably 20 μm to 100 μm.

[0060] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.

[0061] The dimensions of the negative electrode current collector 62 are not particularly limited and can be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness of the negative electrode current collector 62 is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.

[0062] As the separator 70, various porous sheets similar to those conventionally used in lithium ion secondary batteries can be used, and examples thereof include porous resin sheets made of resins such as polyethylene (PE) and polypropylene (PP). Such porous resin sheets may have a single-layer structure or a multi-layer structure of two or more layers (for example, a three-layer structure in which PP layers are laminated on both sides of a PE layer). The separator 70 may be provided with a heat-resistant layer (HRL).

[0063] The non-aqueous electrolyte 80 can be the same as that used in conventional lithium ion secondary batteries, and typically can be an organic solvent (nonaqueous solvent) containing a supporting salt. As the non-aqueous solvent, aprotic solvents such as carbonates, esters, and ethers can be used. Among them, carbonates are preferred because they have a particularly high effect of reducing low-temperature resistance due to the positive electrode material. Examples of carbonates include ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As the supporting salt, for example, lithium salts such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.

[0064] In addition, the nonaqueous electrolyte 80 may contain various additives such as gas generating agents, film forming agents, dispersants, and thickeners, other than the above-mentioned nonaqueous solvent and supporting salt, as long as the effect of the present disclosure is not significantly impaired. Examples of additives used in the nonaqueous electrolyte 80 include positive and negative electrode film forming agents such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and 1,3-propane sultone (PS); overcharge inhibitors such as biphenyl (BP), cyclohexylbenzene (CHB), t-butylbenzene, and t-amylbenzene. Among them, the nonaqueous electrolyte 80 preferably contains FEC. When the nonaqueous electrolyte 80 contains FEC as an additive, it is preferable that the nonaqueous electrolyte 80 contains FEC at a ratio of 20 vol% or less.

[0065] The positive electrode active material of the lithium ion secondary battery 100 configured as above includes a lithium transition metal composite oxide that is a high Ni lithium transition metal composite oxide, and includes a coating portion including a tungsten compound and / or a phosphorus compound on the surface of the lithium transition metal composite oxide. The negative electrode active material of the lithium ion secondary battery 100 includes a carbon material and a Si-containing material, and includes a negative electrode active material in which the content ratio of Si element in the negative electrode active material is 5 mass% or more and 10 mass% or less when the total amount of the negative electrode active material is taken as 100 mass%. This makes it possible to suppress an increase in initial resistance and suppress an increase in resistance during storage while reducing the cobalt content in the positive electrode active material.

[0066] In detail, when a lithium transition metal composite oxide having a layered structure containing Mn is used as a positive electrode active material, the stability of the lithium transition metal composite oxide decreases when the Co content in the lithium transition metal composite oxide is reduced. Typically, the interlayer space of the lithium transition metal composite oxide becomes narrow, and the Li ion conductivity decreases, thereby increasing the initial resistance. In addition, the stability of the lithium transition metal composite oxide decreases, and thus Mn elution from the positive electrode active material layer (specifically, the lithium transition metal composite oxide) becomes significant during storage. For example, Mn eluted from the positive electrode active material layer precipitates on the surface (typically the graphite surface) of the negative electrode active material layer, and further, a film growth occurs starting from the precipitated Mn. This film causes the durability deterioration of the lithium ion secondary battery. Therefore, in the past, a lithium ion secondary battery using a lithium transition metal composite oxide having a layered structure containing Mn and having a reduced Co content as a positive electrode active material had the problem of a deterioration in initial resistance and a large increase in resistance during storage.

[0067] In contrast, in the lithium ion secondary battery 100 according to this embodiment, the content of Ni in the lithium transition metal composite oxide 56a relative to the total of the metal elements other than Li is 75 mol % or more, so that the Mn ratio in the lithium transition metal composite oxide 56a can be suppressed. The coating portion 56c containing a tungsten compound and / or a phosphorus compound is disposed on at least a part of the surface of the lithium transition metal composite oxide 56a, so that the diffusion path of Li ions between the lithium transition metal composite oxide 56a and the non-aqueous electrolyte 80 is increased. This improves the conductivity of Li ions, and can suppress an increase in initial resistance. Furthermore, the Si-containing material 66s contained in the negative electrode active material 66 suppresses the precipitation of Mn on the surface of the negative electrode active material layer 64. This can suppress the formation of a Mn coating on the surface of the negative electrode active material layer 64. Therefore, even if the Co content in the lithium transition metal composite oxide is reduced, a lithium ion secondary battery 100 can be provided in which an increase in initial resistance is suppressed and an increase in resistance during storage is suppressed.

[0068] The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as an electric vehicle (BEV; Battery Electric Vehicle), a hybrid electric vehicle (HEV; Hybrid Electric Vehicle), and a plug-in hybrid electric vehicle (PHEV; Plug-in Hybrid Electric Vehicle). The lithium ion secondary battery 100 can also be used as a storage battery for a small power storage device or the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or parallel.

[0069] As an example, a rectangular lithium ion secondary battery 100 including an electrode body 20 having a flat wound structure has been described. However, the lithium ion secondary battery disclosed herein can also be configured as a lithium ion secondary battery including a laminated electrode body (i.e., an electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated). The laminated electrode body may include a plurality of separators such that one separator is interposed between each of the positive electrodes and the negative electrodes, and may be one in which the positive electrodes and the negative electrodes are alternately laminated while one separator is folded. The lithium ion secondary battery according to this embodiment can also be constructed in the form of a cylindrical lithium ion secondary battery, a coin-type lithium ion secondary battery, a laminated lithium ion secondary battery, or the like. Furthermore, an all-solid-state secondary battery using a solid electrolyte as the electrolyte can also be constructed.

[0070] <Second embodiment> Fig. 5 is a view of a negative electrode sheet 160 (negative electrode) according to the second embodiment, corresponding to Fig. 4. In Fig. 5, the negative electrode sheet 160 may be similar to the above-mentioned lithium ion secondary battery 100, except that a negative electrode active material layer 164 is provided instead of the negative electrode active material layer 64. As shown in Fig. 5, the negative electrode active material layer 164 has a so-called multi-layer structure including a negative electrode upper layer 164u and a negative electrode lower layer 164d.

[0071] In some preferred embodiments, the negative electrode active material layer 164 may include a negative electrode lower layer 164d in contact with the negative electrode current collector 62, and a negative electrode upper layer 164u that is farther from the negative electrode current collector 62 than the negative electrode lower layer 164d is, as viewed in the thickness direction. However, the negative electrode active material layer 164 may have a multi-layer structure of three or more layers. For example, a layer having a composition different from those of the negative electrode upper layer 164u and the negative electrode lower layer 164d may be formed between the negative electrode upper layer 164u and the negative electrode lower layer 164d.

[0072] The negative electrode upper layer 164u is a layer located closer to the surface than the negative electrode lower layer 164d when viewed in the thickness direction of the negative electrode active material layer 164. The negative electrode upper layer 164u is located farther from the negative electrode current collector 62 than the negative electrode lower layer 164d. Here, the negative electrode upper layer 164u constitutes the outermost layer of the negative electrode active material layer 164. In other words, the negative electrode upper layer 164u is located closer to the positive electrode (positive electrode sheet 50) than the negative electrode lower layer 164d.

[0073] The negative electrode active material 66 of the negative electrode upper layer 164u essentially contains a Si-containing material 66s. When the amount of Si element in the entire negative electrode active material layer 164 is taken as 100 mass%, the content ratio of the Si element contained in the negative electrode upper layer 164u is preferably 90 mass% or more, more preferably 95 mass% or more, and further preferably 98 mass% or more. Typically, the content of the Si element contained in the negative electrode upper layer 164u is greater than the content of the Si element contained in the negative electrode lower layer 164d. In other words, in the negative electrode active material layer 164, the Si element is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side.

[0074] As described above, Mn dissolved from the positive electrode active material layer 54 (typically, the lithium transition metal composite oxide 56a) precipitates on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 64, in other words, on the surface layer of the negative electrode active material layer 164, to form a coating. Here, by adopting a configuration in which the Si-containing material is concentrated and dispersed on the positive electrode (positive electrode sheet 50) side of the negative electrode active material layer 164, i.e., on the negative electrode upper layer 164u side, the effect of suppressing the formation of a coating by Mn on the surface of the negative electrode active material layer 164 is more efficiently exhibited. Therefore, an increase in resistance during storage can be suitably suppressed.

[0075] In this specification, the "content ratio (mass%) of the Si element contained in the negative electrode upper layer when the amount of Si element in the entire negative electrode active material layer is taken as 100%" can be calculated as follows. First, the thickness of the negative electrode upper layer is obtained by observing a cross-sectional SEM image of the negative electrode active material layer 164. Next, for a predetermined area of ​​the negative electrode active material layer, a sample is collected by scraping off the negative electrode active material layer by the thickness of the obtained negative electrode upper layer, and an ICP (Inductively Coupled Plasma) analysis is performed to calculate the amount of Si element in the negative electrode upper layer. Similarly, for the negative electrode lower layer, a sample is collected by scraping off a predetermined area of ​​the negative electrode active material layer, and the amount of Si element in the negative electrode lower layer is calculated by ICP analysis. Then, the content ratio of the Si element in the negative electrode upper layer to the amount of Si element in the entire negative electrode active material layer can be obtained from the values ​​of the Si element amounts of the negative electrode upper layer and the negative electrode lower layer obtained respectively.

[0076] The content of Si element contained in the negative electrode upper layer 164u is preferably 2 mass % or more, and more preferably 5 mass % or more, when the total amount of the negative electrode active material 66 in the negative electrode upper layer 164u is taken as 100 mass %.

[0077] The negative electrode lower layer 164d is a layer located closer to the negative electrode current collector 62 than the negative electrode upper layer 164u when viewed in the thickness direction of the negative electrode active material layer 64. Here, the negative electrode lower layer 164d is in contact with the negative electrode current collector 62.

[0078] The negative electrode active material 66 of the negative electrode lower layer 164d essentially contains a carbon material 66c. The negative electrode lower layer 164d may contain a Si-containing material 66s, or may not contain a Si-containing material 66s. The content of the Si element contained in the negative electrode lower layer 164d is not particularly limited, but may be, for example, 2% by mass or less, and preferably 1% by mass or less, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass. The content of the C element contained in the negative electrode lower layer 164d is not particularly limited, but is preferably 98% by mass or more, and more preferably 99% by mass or more, when the negative electrode active material of the negative electrode lower layer 164d is taken as 100% by mass.

[0079] The ratio (Tu / Ta) of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.8 or less, and preferably 0.7 or less. This allows the Si-containing material 66s (in other words, Si element) in the negative electrode active material layer 164 to be dispersed on the positive electrode (positive electrode sheet 50) side, and thus the effect of suppressing the formation of a coating by Mn is more efficiently exhibited. Therefore, the increase in resistance during storage can be suitably suppressed. In addition, from the viewpoint of packing property, the ratio of the thickness Tu of the negative electrode upper layer 164u to the total thickness Ta of the negative electrode active material layer 164 is, for example, 0.4 or more, and preferably 0.5 or more. Note that the "ratio of the thickness of the negative electrode upper layer to the total thickness of the negative electrode active material layer" in the specification is measured in a cross-sectional SEM image of the negative electrode active material layer 164.

[0080] The above-mentioned negative electrode upper layer 164u and negative electrode lower layer 164d can be produced by a conventionally known method. For example, but not limited to, the negative electrode upper layer 164u and negative electrode lower layer 164d can be formed by preparing a negative electrode active material layer forming slurry using two or more types of negative electrode active materials 66 having different compositions (typically, the content ratio of the Si-containing material) and applying the negative electrode active material layer forming slurry.

[0081] Hereinafter, examples of the technology disclosed herein will be described, but it is not intended that the technology disclosed herein be limited to those shown in these examples.

[0082] <Test Example 1: Examination of the structure of the positive electrode active material and the presence or absence of Si in the negative electrode active material> (Example 1) [Preparation of positive electrode sheet] A positive electrode active material according to Example 1 was prepared. Specifically, first, a lithium transition metal composite oxide (LiNi 0.83 Mn 0.17A base material of lithium transition metal composite oxide (O2) was prepared. Diphosphorus pentoxide (P2O5) was dry mixed with the base material of the lithium transition metal composite oxide prepared above, and heat-treated at 120°C for 3 hours. At this time, the molar ratio of the total amount of Ni and Mn in the lithium transition metal composite oxide to phosphorus (P) was set to 100:0.1. As a result, a positive electrode active material according to Example 1 was obtained in which a phosphorus compound (here, lithium phosphate (Li3PO4)) was arranged as a coating portion on the surface of a lithium transition metal composite oxide having a layered structure with a composition (molar ratio) of Ni, Co, and Mn of Ni:Co:Mn=83:0:17 (corresponding to 83 / 0 / 17 in the "Ni / Co / Mn" column in Table 1) at 0.1 mol% in terms of P with respect to the total amount of Ni and Mn in the lithium transition metal composite oxide (100 mol%).

[0083] The positive electrode active material prepared above, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in a solid mass ratio of positive electrode active material:AB:PVDF=100:1:1. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to the obtained mixture and kneaded to prepare a slurry for forming a positive electrode active material layer. The obtained slurry for forming a positive electrode active material layer was applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 15 μm and dried to form a positive electrode active material layer. The obtained positive electrode active material layer was roll-pressed using a rolling roller, and then cut to a predetermined size to prepare a positive electrode sheet according to Example 1.

[0084] [Preparation of negative electrode sheet] First, graphite as a carbon material and a Si-C composite as a Si-containing material were mixed so that the content ratio of Si element was 10 mass% and the content ratio of C element was 90 mass% when the total amount of the negative electrode active material was 100 mass%, to prepare the negative electrode active material of Example 1.

[0085] The negative electrode active material prepared above, styrene butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and single-walled carbon nanotubes (SWCNT) as a conductive material were mixed in ion-exchanged water at a solid content mass ratio of negative electrode active material:SBR:CMC:SWCNT=100:1:1:0.5 to prepare a slurry for forming a negative electrode active material layer. The obtained slurry for forming a negative electrode active material layer was applied onto a negative electrode current collector made of copper foil with a thickness of 10 μm and dried to form a negative electrode active material layer. The obtained negative electrode active material layer was roll-pressed using a rolling roller and then cut to a predetermined size. As a result, a negative electrode sheet according to Example 1 in which the Si-containing material was almost uniformly dispersed throughout the entire negative electrode active material was produced.

[0086] [Preparing the separator] As a separator, a porous polyolefin sheet having a thickness of 20 μm and a three-layer structure of PP / PE / PE was prepared.

[0087] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving LiPF6 as a supporting electrolyte at a concentration of 1 mol / L in a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) in a volume ratio of EC:EMC:DMC:FEC=25:40:30:5.

[0088] [Preparation of lithium-ion secondary batteries for evaluation] The positive electrode sheet and the negative electrode sheet were stacked with a separator interposed therebetween to obtain a laminate. The laminate was then wound to obtain a wound body, which was then pressed to obtain a flattened electrode body. A current collector terminal was attached to the electrode body, which was then inserted into a battery case and welded, after which a non-aqueous electrolyte was poured in. The battery case was then sealed to produce a lithium ion secondary battery for evaluation.

[0089] [Initial charging process] The obtained lithium ion secondary battery for evaluation according to Example 1 was subjected to a constant current charge at a current value of 0.1 C to a voltage of 4.2 V as an initial charge process in a temperature environment of 25° C., and then constant voltage charge was performed until the current value became 1 / 20 C. Thereafter, the battery was discharged at a constant current value of 0.1 C to 3.0 V.

[0090] (Example 2) A lithium-ion secondary battery for evaluation according to Example 2 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which a tungsten compound (here, lithium tungstate (LiWO)) was arranged at 0.1 mol % in terms of tungsten (W) relative to 100 mol % of the total amount of Ni and Mn in the lithium transition metal composite oxide was used as the coating portion instead of lithium phosphate (LiPO), and an initial charging process was performed.

[0091] (Example 3) A lithium ion secondary battery for evaluation according to Example 3 was produced in the same manner as in Example 1, except that no coating portion was disposed on the surface of the lithium transition metal composite oxide, and an initial charging process was performed.

[0092] (Example 4) A lithium ion secondary battery for evaluation according to Example 4 was produced in the same manner as in Example 1, except that the negative electrode active material was graphite alone (that is, no Si-containing material was included), and an initial charging process was performed.

[0093] (Example 5) A lithium ion secondary battery for evaluation according to Example 5 was produced in the same manner as in Example 1, except that no coating portion was disposed on the surface of the lithium transition metal composite oxide and the negative electrode active material was graphite alone (i.e., no Si-containing material was included), and an initial charging process was performed.

[0094] [Evaluation of initial resistance] First, the lithium ion secondary batteries for evaluation according to Examples 1 to 5 were charged at a constant current and constant voltage (CCCV) at a current value of 0.3 C in a thermostatic chamber at 25° C., and the SOC (State of Charge) was adjusted to 50%. Then, pulse discharge was performed at a current value of 5 C for 10 seconds. The voltage change (ΔV) during the pulse discharge was obtained and calculated using the following formula (I): Resistance value = voltage change (ΔV) / current value (5C)…(I) The resistance value before storage (initial resistance value) was calculated using the above formula. The results are shown in Table 1.

[0095] [Evaluation of storage resistance increase rate] After measuring the initial resistance value, the evaluation lithium ion secondary batteries according to Examples 1 to 5 were adjusted to SOC 100% in a temperature environment of 25°C. Each evaluation lithium ion secondary battery was placed in a thermostatic chamber at 60°C and stored for 14 days. The resistance value after storage was calculated in the same manner as for the initial resistance. Then, the resistance value after storage was calculated using the following formula (II): Resistance increase rate (%) = (resistance value after storage / resistance value before storage) x 100...(II) The resistance increase rate (%) was calculated from the above data, and the results are shown in Table 1.

[0096] [Capacity maintenance rate] In parallel with the evaluation of the storage resistance increase rate described above, the capacity retention rate was evaluated. Specifically, for the evaluation lithium ion secondary batteries according to Examples 1 to 5, the discharge capacity measured during the evaluation of the resistance increase rate was taken as the initial capacity. Thereafter, the discharge capacity of the evaluation lithium ion secondary batteries stored in the above-mentioned storage resistance increase rate evaluation (i.e., after storage at 60°C for 14 days) was determined in the same manner as the initial capacity. Then, the discharge capacity was calculated using the following formula (III): Capacity retention rate (%) = discharge capacity after 14 days storage / initial capacity × 100…(III) The capacity retention rate (%) for each example was calculated using the following formula: The results are shown in Table 1.

[0097] [Table 1]

[0098] From the results of Examples 1 and 5, in Example 1, in which a phosphorus compound (Li3PO4) was arranged as a coating portion on the surface of a lithium transition metal composite oxide and a negative electrode active material containing a carbon material and a Si-containing material was used, both the reduction in initial resistance and the suppression of the resistance increase during storage were favorably observed compared to Example 5. On the other hand, in Example 3, in which a positive electrode active material having no coating portion on the surface of a lithium transition metal composite oxide was used, the reduction in initial resistance was not observed compared to Example 1. From this, it is considered that the effect of reducing the initial resistance can be obtained by using a lithium transition metal composite oxide having a phosphorus compound arranged on the surface as a coating portion. In addition, in Example 4, in which the negative electrode active material was only graphite (i.e., did not contain a Si-containing material), the reduction in the resistance increase rate during storage was not observed compared to Example 1. From the above, it was found that the effect of suppressing the resistance increase during storage can be favorably obtained by satisfying both the use of a lithium transition metal composite oxide having a phosphorus compound arranged on the surface as a coating portion as a positive electrode active material and the use of a negative electrode active material containing a carbon material and a Si-containing material.

[0099] Also, in Example 2, in which a tungsten compound (Li2WO4) was arranged on the surface of the lithium transition metal composite oxide as a coating portion instead of a phosphorus compound, good results were obtained in terms of the initial resistance and the suppression of the resistance increase during storage, similar to Example 1. From this, it was found that the effect of suppressing the initial resistance and the resistance increase during storage can be suitably obtained even when a tungsten compound is used as the coating portion.

[0100] <Test Example 2: Examination of Si ratio> (Examples 6 to 8) Lithium ion secondary batteries for evaluation according to Examples 6 to 8 were produced and subjected to an initial charging process in the same manner as in Example 1, except that the content ratio of Si element when the total amount of the negative electrode active material, that is, graphite as the carbon material and the Si-C composite as the Si-containing material, was taken as 100 mass %, was changed as shown in the "Si content ratio" column in Table 2. The lithium ion secondary batteries for evaluation according to Examples 6 to 8 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 2.

[0101] [Table 2]

[0102] As shown in the results of Table 2, in Example 7 and Example 1, in which the content ratio of the Si element in the negative electrode active material was 5 mass% or 10 mass%, the resistance increase during storage was suitably suppressed, and no decrease in the capacity retention rate was observed. In Example 6, in which the content ratio of the Si element was 2 mass%, the effect of suppressing the resistance increase during storage was not obtained very well. The reason for this is considered to be that in Example 6, the negative electrode did not contain enough Si-containing material to sufficiently suppress the precipitation of Mn on the surface of the negative electrode active material. In addition, the higher the content ratio of the Si element, the better the effect of suppressing the increase in the battery resistance, while in Example 8, in which the content ratio of the Si element was 13 mass%, the capacity retention rate was lower than in other examples. Therefore, from the viewpoint of achieving both the effect of suppressing the resistance increase during storage and the capacity retention rate, the content ratio of the Si element in the negative electrode active material is considered to be in the more suitable range of 5 to 10 mass%.

[0103] <Test Example 3: Examination of Covering Part> (Example 9) A lithium-ion secondary battery for evaluation according to Example 9 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which Li3PO4 and Li2WO4 were arranged at 0.05 mol % each in terms of W and P relative to 100 mol % of the total amount of Ni and Mn in the lithium transition metal composite oxide was used as the coating portion, and an initial charging process was performed.

[0104] (Example 10) A lithium-ion secondary battery for evaluation according to Example 10 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which Li3PO4 and aluminum oxide (Al2O3) were arranged at 0.05 mol % each in terms of P and Al relative to 100 mol % of the total amount of Ni and Mn in the lithium transition metal composite oxide was used as the coating portion, and an initial charging process was performed.

[0105] (Example 11) A lithium-ion secondary battery for evaluation according to Example 11 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which Al2O3 was arranged at 0.1 mol % in terms of Al relative to 100 mol % of the total amount of Ni and Mn in the lithium transition metal composite oxide was used instead of Li3PO4 as the coating portion, and an initial charging process was performed.

[0106] (Example 12) A lithium-ion secondary battery for evaluation according to Example 12 was produced in the same manner as in Example 1, except that a lithium transition metal composite oxide in which LiBO2 was arranged at 0.1 mol % in terms of B relative to 100 mol % of the total amount of Ni and Mn in the lithium transition metal composite oxide was used instead of Li3PO4 as the coating portion, and an initial charging process was performed.

[0107] The evaluation lithium ion secondary batteries according to Examples 9 to 12 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 3.

[0108] [Table 3]

[0109] From the results in Table 3, whether the coating contained either a phosphorus compound (Li3PO4) or a tungsten compound (Li2WO4) (Example 1, Example 2) or both (Example 9), the initial resistance and the suppression of resistance increase during storage were similarly good. On the other hand, in Example 11 in which only Al2O3 was arranged on the surface of the lithium transition metal composite oxide as the coating, and in Example 12 in which only LiBO2 was arranged on the surface of the lithium transition metal composite oxide as the coating, the initial resistance suppression effect was not obtained compared to Examples 1, 2, and 9. From this, it was found that in order to obtain the initial resistance suppression effect, it is necessary to include a tungsten compound and / or a phosphorus compound as the coating.

[0110] Moreover, in Example 10, in which Al2O3 was contained in addition to Li3PO4 as the coating portion, better results were obtained in terms of suppressing the increase in resistance during storage. The reasons for this are considered to be as follows. As described above, Al2O3 as the coating portion does not have the effect of suppressing the initial resistance, but on the other hand, it has the function of trapping hydrogen fluoride gas generated by the decomposition of the non-aqueous electrolyte. It is considered that this function can suppress the elution of Mn caused by hydrogen fluoride gas. Therefore, in Example 10, it is considered that the trapping effect of hydrogen fluoride gas possessed by aluminum oxide is expressed, and better results were obtained in terms of suppressing the increase in resistance during storage.

[0111] <Test Example 4: Examination of Ni compounding ratio in positive electrode active material> (Examples 13-19) Except for changing the composition (molar ratio) of Ni, Co, and Mn in the lithium transition metal composite oxide as shown in the "Ni / Co / Mn" column in Table 4, lithium ion secondary batteries for evaluation according to Examples 13 to 19 were produced and subjected to an initial charging process in the same manner as in Example 1. The lithium ion secondary batteries for evaluation according to Examples 13 to 19 were evaluated in the same manner as in Test Example 1 by the above-mentioned method. The results are shown in Table 4.

[0112] [Table 4]

[0113] As shown in the results of Table 4, in Example 1 and Examples 13 to 15 in which the Ni blending ratio of the lithium transition metal composite oxide is 83 mol%, even when the Co content of the lithium transition metal composite oxide is reduced, the initial resistance was reduced and the resistance increase during storage was suppressed stably. In addition, in Examples 16 to 17 in which the Ni blending ratio of the lithium transition metal composite oxide is 95 mol%, and in Examples 18 to 19 in which the Ni blending ratio of the lithium transition metal composite oxide is 75 mol%, the initial resistance was reduced and the resistance increase during storage was suppressed. In addition, in terms of the Co / Mn ratio of the lithium transition metal composite oxide, Example 15 in which the Co / Mn ratio is 0.42 also preferably achieved both the initial resistance and the resistance increase during storage.

[0114] <Test Example 5: Examination of the distribution of Si-containing material in the negative electrode active material layer> (Examples 20-21) A first negative electrode active material layer-forming slurry was prepared in the same manner as in Example 1, except that the negative electrode active material was graphite alone (i.e., the content ratio of Si element was 0 mass% and the content ratio of C element was 100 mass% when the total amount of the negative electrode active material was 100 mass%). Similarly, a second negative electrode active material layer forming slurry was prepared in the same manner as in Example 1, except that the graphite and the Si-C composite were mixed so that the content ratio of Si element was 20 mass% and the content ratio of C element was 80 mass% when the total amount of the negative electrode active material was 100 mass%.

[0115] The first negative electrode active material layer forming slurry was applied onto the negative electrode current collector made of the same copper foil as that used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the second negative electrode active material layer forming slurry was applied onto the dried coating film of the first negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the second negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 20 was obtained in which the negative electrode lower layer formed by the first negative electrode active material layer forming slurry and the negative electrode upper layer formed by the second negative electrode active material layer forming slurry were supported on the negative electrode current collector. In addition, in the negative electrode sheet of Example 20, the content ratio of the Si element in the negative electrode upper layer was 99 mass% when the Si element in the entire negative electrode active material was 100 mass%. Similarly, the second negative electrode active material layer forming slurry was applied onto the same copper foil negative electrode current collector as used in Example 1, dried, and roll-pressed using a rolling roller to obtain a predetermined density. Next, the first negative electrode active material layer forming slurry was applied onto the dried coating film of the second negative electrode active material layer forming slurry, dried, and roll-pressed using a rolling roller to obtain a predetermined density. At this time, the thickness of the first negative electrode active material layer forming slurry was set to 0.5 with respect to the thickness of the entire negative electrode active material layer. As a result, a negative electrode sheet of Example 21 was obtained in which a negative electrode lower layer formed by the second negative electrode active material layer forming slurry and a negative electrode upper layer formed by the first negative electrode active material layer forming slurry were supported on a negative electrode current collector. In addition, in the negative electrode sheet of Example 21, the content ratio of the Si element in the negative electrode upper layer was 1 mass% when the Si element in the entire negative electrode active material was 100 mass%.

[0116] Except for using the above-mentioned negative electrode sheet, evaluation batteries according to Examples 20 and 21 were produced in the same manner as in Example 1, and an initial charging process was performed. Evaluations were performed in the same manner as in Test Example 1 for the evaluation lithium ion secondary batteries according to Examples 20 and 21, using the above-mentioned method. The results are shown in Table 5.

[0117] [Table 5]

[0118] As shown in the results of Table 5, in all of Examples 1, 20, and 21, the effect of suppressing the resistance increase during storage was observed compared to Example 5, in which only graphite was used as the negative electrode active material. Looking at Examples 1, 20, and 21, in which the Si blending ratio was 10 mass%, almost no difference was observed in the capacity maintenance rate during storage due to the distribution of the Si-containing material. In addition, comparing Examples 1, 20, and 21, in Example 1, in which (Si-containing material, to be revised according to the contents of the teachings) was uniformly distributed throughout the negative electrode active material layer, the effect of suppressing the resistance increase rate during storage was good, and in Example 20, in which the Si-containing material was concentrated and arranged in the upper layer, even better results were obtained in suppressing the resistance increase rate during storage. This is thought to be because the effect of suppressing the precipitation of Mn by the Si-containing material on the surface of the negative electrode active material was more efficiently expressed by concentrating the Si-containing material in the upper layer of the negative electrode active material.

[0119] Although the preferred embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.

[0120] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprising a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, and a coating portion disposed on at least a part of a surface of the lithium transition metal composite oxide, the lithium transition metal composite oxide having a Ni content of 75 mol % or more with respect to a total of metal elements other than Li and being secondary particles formed by aggregation of primary particles, the coating portion comprising a tungsten compound and / or a phosphorus compound, the negative electrode comprises a negative electrode active material layer containing a negative electrode active material, the negative electrode active material comprising a carbon material and a Si-containing material, and a content ratio of Si element in the negative electrode active material is 5 mass % or more and 10 mass % or less when a total amount of the negative electrode active material is taken as 100 mass %. Item 2: The lithium transition metal composite oxide has the following general formula: Li α Ni x Mn y M z Item 2. The lithium ion secondary battery according to item 1, wherein α is 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, and x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W. Item 3: The lithium ion secondary battery according to item 1 or 2, wherein in the lithium transition metal composite oxide, the content (moles) of Co element and the content (moles) of Mn element satisfy the following relationship: 0≦Co / Mn≦0.42. Item 4: The lithium ion secondary battery according to any one of Items 1 to 3, wherein the tungsten compound contains lithium tungstate. Item 5: The lithium ion secondary battery according to any one of Items 1 to 4, wherein the phosphorus compound contains lithium phosphate. Item 6: The lithium ion secondary battery according to any one of Items 1 to 5, wherein the coating portion further contains aluminum oxide. Item 7: The lithium ion secondary battery according to any one of items 1 to 6, wherein the negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector, and a negative electrode upper layer further from the negative electrode current collector than the negative electrode lower layer, when viewed in a thickness direction, and a content ratio of Si element in the negative electrode upper layer is 90 mass % or more when Si element in the entire negative electrode active material is taken as 100 mass %. Item 8: The lithium ion secondary battery according to item 7, wherein a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less. Item 9: The lithium ion secondary battery according to any one of Items 1 to 8, wherein the Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and a Si-C composite. [Explanation of symbols]

[0121] 20 Electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 56 Cathode active material 56a Lithium transition metal complex oxide 56c Covering part 56p primary particle 60, 160 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64, 164 Negative electrode active material layer 164u negative electrode upper layer 164d Negative electrode lower layer 66 Negative electrode active material 66c Carbon Materials 66s Si-containing material 70 Separator 80 Non-aqueous electrolytes 100 Lithium-ion secondary battery

Claims

1. A lithium ion secondary battery comprising a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, The positive electrode includes a positive electrode active material layer containing a positive electrode active material, the positive electrode active material comprises a lithium transition metal composite oxide having a layered structure containing Li, Ni, and Mn, and a coating portion disposed on at least a portion of a surface of the lithium transition metal composite oxide, The lithium transition metal composite oxide is The content of Ni relative to the total of metal elements other than Li is 75 mol% or more, These are secondary particles formed by agglomeration of primary particles, the coating portion contains a tungsten compound and / or a phosphorus compound, the negative electrode includes a negative electrode active material layer containing a negative electrode active material, The negative electrode active material includes a carbon material and a Si-containing material, When the total amount of the negative electrode active material is taken as 100 mass%, the content ratio of Si element in the negative electrode active material is 5 mass% or more and 10 mass% or less. Lithium-ion secondary battery.

2. The lithium transition metal composite oxide has the following general formula: Li α Ni x Mn y M z O 2 (wherein 0.8≦α≦1.2, 0.75≦x≦0.95, 0.05≦y≦0.25, 0≦z≦0.2, x+y+z=1, and M is one or more selected from Mg, Ca, Co, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.) The lithium ion secondary battery according to claim 1 .

3. In the lithium transition metal composite oxide, the content (mol) of Co element and the content (mol) of Mn element have the following relationship: 0≦Co / Mn≦0.42 Fulfilling The lithium ion secondary battery according to claim 1 or 2.

4. The tungsten compound includes lithium tungstate. The lithium ion secondary battery according to claim 1 or 2.

5. The phosphorus compound includes lithium phosphate. The lithium ion secondary battery according to claim 1 or 2.

6. The coating portion further includes aluminum oxide. The lithium ion secondary battery according to claim 1 or 2.

7. The negative electrode further includes a negative electrode current collector, the negative electrode active material layer includes a negative electrode lower layer in contact with the negative electrode current collector and a negative electrode upper layer located farther from the negative electrode current collector than the negative electrode lower layer when viewed in a thickness direction, The content ratio of the Si element in the negative electrode upper layer is 90 mass% or more when the Si element in the entire negative electrode active material is 100 mass%. The lithium ion secondary battery according to claim 1 or 2.

8. a ratio of a thickness of the negative electrode upper layer to a total thickness of the negative electrode active material layer is 0.4 or more and 0.8 or less; The lithium ion secondary battery according to claim 7.

9. The Si-containing material includes at least one selected from the group consisting of Si, silicon oxide, and Si-C composites; The lithium ion secondary battery according to claim 1 or 2.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolytic secondary battery and method of manufacturing the same, and nonaqueous electrolytic secondary battery with the positive electrode active material

    JP2013152866A

  • Lithium-nickel-based positive electrode active material, method for producing the same, and lithium secondary battery including the same

    JP2017504947A

  • Cathode active material for all-solid lithium ion battery, electrode, and all-solid lithium ion battery

    JP2020167145A

  • Positive electrode active material, method for producing positive electrode active material, positive electrode containing positive electrode active material, and lithium secondary battery

    JP2022514966A

  • Lithium secondary battery

    US20220416241A1