Membrane electrode assembly and polymer electrolyte fuel cell

The integration of conductive fibers in electrode catalyst layers and optimized gas diffusion layers in the membrane electrode assembly enhances conductivity, leading to improved power generation performance and output voltage in polymer electrolyte fuel cells.

JP2024160576APending Publication Date: 2024-11-14TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075723
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing configurations of polymer electrolyte fuel cells do not adequately consider the combination of electrode catalyst layers and gas diffusion layers, limiting their power generation performance.

Method used

A membrane electrode assembly is designed with electrode catalyst layers containing catalyst-supported particles and conductive fibers, and gas diffusion layers with a surface resistance value of 1.3Ω/□ or less, enhancing conductivity in both surface and thickness directions.

Benefits of technology

This configuration improves the power generation performance of polymer electrolyte fuel cells by increasing conductivity and maintaining high output voltage, even with gas diffusion layers having higher resistance values.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160576000001_ABST
    Figure 2024160576000001_ABST
Patent Text Reader

Abstract

To provide a membrane electrode assembly and a polymer electrolyte fuel cell capable of improving power generation performance.SOLUTION: A membrane electrode assembly 10 includes a polymer electrolyte membrane 11, a pair of electrode catalyst layers 12A, 12C in contact with the surfaces of the polymer electrolyte membrane 11 with the polymer electrolyte membrane 11 sandwiched therebetween, and gas diffusion layers 13A, 13C laminated on each of the pair of electrode catalyst layers 12A, 12C. At least one of the pair of electrode catalyst layers 12A, 12C is a target catalyst layer containing catalyst-supporting particles, a polymer electrolyte, and conductive fibers, and the surface resistance of the gas diffusion layer 13A, 13C laminated on the target catalyst layer is 1.3 Ω / square or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a membrane electrode assembly and a polymer electrolyte fuel cell. [Background technology]

[0002] Fuel cells have been attracting attention as a type of battery that can contribute to solving environmental and energy problems. Fuel cells generate electricity by utilizing a chemical reaction between fuel such as hydrogen and an oxidant such as oxygen. Among fuel cells, polymer electrolyte fuel cells can be operated at low temperatures and made compact, so they are expected to be used as portable power sources, domestic power sources, and vehicle-mounted power sources.

[0003] A polymer electrolyte fuel cell includes a membrane electrode assembly having a fuel electrode (anode), an air electrode (cathode), and a polymer electrolyte membrane sandwiched between the fuel electrode and the air electrode. Each of the fuel electrode and the air electrode includes a laminate of an electrode catalyst layer and a gas diffusion layer.

[0004] A fuel gas containing hydrogen is supplied to the fuel electrode, and an oxidant gas containing oxygen is supplied to the air electrode. Protons and electrons are generated from the fuel gas supplied to the fuel electrode due to the action of the catalyst contained in the electrode catalyst layer. The protons are conducted by the polymer electrolyte contained in the electrode catalyst layer and the polymer electrolyte membrane, and move to the air electrode through the polymer electrolyte membrane. The electrons are extracted from the fuel electrode to an external circuit, and move to the air electrode through the external circuit. At the air electrode, the oxidant gas reacts with the protons and electrons that have moved from the fuel electrode to produce water. In this way, an electric current is generated by the electrons passing through the external circuit (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-115299 A Summary of the Invention [Problem to be solved by the invention]

[0006] In general, the electrode catalyst layer contains a carbon material carrying a catalytic substance such as platinum, and a polymer electrolyte. The carbon material contributes to the conduction of electrons, and the polymer electrolyte contributes to the conduction of protons. Therefore, the type and ratio of the carbon material and the polymer electrolyte are important factors for improving the power generation performance of a polymer electrolyte fuel cell. Furthermore, improvement in the diffusibility of gas in the electrode catalyst layer and the drainage of water generated during power generation also contribute to the improvement of the power generation performance.

[0007] On the other hand, the gas diffusion layer is involved in supplying gas to the electrode catalyst layer, collecting electrons generated in the electrode reaction, and managing the amount of water in the cell by discharging water generated during power generation. Therefore, the characteristics of the gas diffusion layer are also an important factor in improving the power generation performance of solid polymer electrolyte fuel cells.

[0008] To date, many proposals have been made to improve the electrode catalyst layer and the gas diffusion layer individually, but little attention has been paid to the combination of the electrode catalyst layer and the gas diffusion layer, and there is still room for improvement in the configuration that can improve power generation performance. [Means for solving the problem]

[0009] Various aspects of a membrane electrode assembly and a polymer electrolyte fuel cell for solving the above problems will be described below. [Aspect 1] A membrane electrode assembly comprising: a polymer electrolyte membrane; a pair of electrode catalyst layers sandwiching the polymer electrolyte membrane and in contact with the surfaces of the polymer electrolyte membrane; and a gas diffusion layer laminated on each of the pair of electrode catalyst layers, wherein at least one of the pair of electrode catalyst layers is a target catalyst layer containing catalyst-supporting particles, a polymer electrolyte, and conductive fibers, and the gas diffusion layer laminated on the target catalyst layer has a surface resistance of 1.3 Ω / □ or less.

[0010] According to the above configuration, the electrical conductivity in the direction along the surface of the target catalyst layer is increased, thereby improving the power generation performance of the fuel cell and allowing the use of a gas diffusion layer with a higher surface resistance than when the electrode catalyst layer does not contain conductive fibers.

[0011] [Aspect 2] The membrane electrode assembly according to [Aspect 1], wherein the conductive fibers are carbon fibers. According to the above configuration, the electrical conductivity of the target catalyst layer is suitably increased.

[0012] [Aspect 3] The mass per unit area of ​​the gas diffusion layer laminated on the target catalyst layer (g / m 2 ) is 0.02 or less. According to the above configuration, the power generation performance of the fuel cell is suitably improved.

[0013] [Aspect 4] A polymer electrolyte fuel cell comprising the membrane electrode assembly according to any one of [Aspect 1] to [Aspect 3] and a pair of separators sandwiching the membrane electrode assembly therebetween. According to the above configuration, the power generation performance is improved and a high output voltage can be obtained. Effect of the Invention

[0014] According to the present invention, the power generation performance of a polymer electrolyte fuel cell can be improved. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram showing a cross-sectional structure of a membrane electrode assembly according to an embodiment. [Diagram 2] FIG. 4 is a diagram showing a schematic distribution of conductive fibers in an electrode catalyst layer according to one embodiment. [Diagram 3] FIG. 1 is an exploded perspective view showing a polymer electrolyte fuel cell according to an embodiment of the present invention; [Figure 4] FIG. 4 is a diagram showing measurement points of surface resistance value in a gas diffusion layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of a membrane electrode assembly and a polymer electrolyte fuel cell will be described with reference to FIGS. 1 to 3. FIG.

[0017] [Configuration of membrane electrode assembly] The structure of the membrane electrode assembly will be described with reference to FIG. 1, the membrane electrode assembly 10 includes a polymer electrolyte membrane 11, a pair of electrode catalyst layers, and a pair of gas diffusion layers. The pair of electrode catalyst layers are electrode catalyst layer 12A and electrode catalyst layer 12C. The pair of gas diffusion layers are gas diffusion layer 13A and gas diffusion layer 13C.

[0018] The polymer electrolyte membrane 11 is sandwiched between the electrode catalyst layer 12A and the electrode catalyst layer 12C in the thickness direction. The electrode catalyst layer 12A is in contact with one of the two surfaces of the polymer electrolyte membrane 11, and the electrode catalyst layer 12C is in contact with the other of the two surfaces of the polymer electrolyte membrane 11.

[0019] Gas diffusion layer 13A is laminated on electrode catalyst layer 12A, and gas diffusion layer 13C is laminated on electrode catalyst layer 12C. In other words, a laminate of polymer electrolyte membrane 11, electrode catalyst layer 12A, and electrode catalyst layer 12C is sandwiched between gas diffusion layer 13A and gas diffusion layer 13C.

[0020] The electrode catalyst layer 12A and the gas diffusion layer 13A constitute a fuel electrode, which is an anode of the polymer electrolyte fuel cell, while the electrode catalyst layer 12C and the gas diffusion layer 13C constitute an air electrode, which is a cathode of the polymer electrolyte fuel cell.

[0021] When viewed from a position facing one surface of the polymer electrolyte membrane 11, the electrode catalyst layers 12A, 12C and the gas diffusion layers 13A, 13C have substantially the same outer shape. The outer shape of the polymer electrolyte membrane 11 is larger than the outer shapes of the electrode catalyst layers 12A, 12C and the gas diffusion layers 13A, 13C. There are no particular limitations on the outer shapes of the polymer electrolyte membrane 11, the electrode catalyst layers 12A, 12C and the gas diffusion layers 13A, 13C, and they may be, for example, rectangular.

[0022] [Membrane electrode assembly materials] The materials and detailed configurations of the members of the membrane electrode assembly 10 will be described below. The polymer electrolyte membrane 11 includes a polymer electrolyte. The polymer electrolyte used in the polymer electrolyte membrane 11 may be any polymer electrolyte having proton conductivity, such as a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte. Examples of fluorine-based polymer electrolytes include Nafion (registered trademark: manufactured by DuPont), Flemion (registered trademark: manufactured by Asahi Glass Co., Ltd.), Aciplex (registered trademark: manufactured by Asahi Kasei Corporation), and Gore-Select (registered trademark: manufactured by Gore Japan LLC). Examples of hydrocarbon-based polymer electrolytes include sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene. Among them, fluorine-based polymer electrolytes, specifically, Nafion (registered trademark: manufactured by DuPont) and its related materials can be suitably used.

[0023] The electrode catalyst layers 12A and 12C each contain a catalyst-supporting particle and a polymer electrolyte. The catalyst-supporting particle is a carrier that supports a catalyst substance. Furthermore, at least one of the electrode catalyst layers 12A and 12C contains conductive fibers.

[0024] The catalytic substance has a particulate shape. The material of the catalytic substance is, for example, a metal, an alloy, a metal oxide, a metal complex oxide, etc. The metal complex oxide is an oxide containing two kinds of metals. Examples of metals contained in the catalytic material include platinum group elements such as platinum, palladium, ruthenium, iridium, rhodium, and osmium, gold, iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum.

[0025] When the catalytic substance is one or more metals selected from platinum, gold, palladium, rhodium, ruthenium, and iridium, the membrane electrode assembly 10 has excellent reactivity in the electrode reaction and can efficiently and stably proceed with the electrode reaction. In this case, the power generation performance of a polymer electrolyte fuel cell including the membrane electrode assembly 10 is also improved.

[0026] From the viewpoint of increasing the activity of the catalytic substance, the average particle diameter of the catalytic substance is preferably 20 nm or less, more preferably 5 nm or less. From the viewpoint of stabilizing the activity of the catalytic substance, the average particle diameter of the catalytic substance is preferably 0.5 nm or more, more preferably 1 nm or more. The average particle diameter of the catalytic substance is the average particle diameter obtained by X-ray diffraction if the measurement is performed in a state in which the catalytic substance is supported on a carrier, and is the arithmetic average particle diameter obtained by particle size measurement if the measurement is performed in a state in which the catalytic substance is not supported on a carrier.

[0027] The support is a particle that is not eroded by the catalyst material and has electrical conductivity. An example of the support is carbon particles. Specific examples of the support are carbon black, graphite, activated carbon, carbon fiber, carbon nanotubes, and fullerene.

[0028] The catalyst-supporting particles may be covered with a hydrophobic coating. The hydrophobic coating imparts hydrophobicity to the catalyst-supporting particles and has gas permeability for allowing fuel gas and oxidant gas to pass through. From the viewpoint of increasing the water dischargeability in the electrode catalyst layers 12A, 12C, the thickness of the hydrophobic coating is preferably 2 nm or more. From the viewpoint of increasing gas permeability, the thickness of the hydrophobic coating is preferably 40 nm or less.

[0029] An example of the material of the hydrophobic coating is a fluorine-based compound having at least one polar group. The polar group is, for example, a hydroxyl group, an alkoxy group, a carboxyl group, an ester group, an ether group, a carbonate group, or an amide group. A hydrophobic coating having a polar group is easily fixed to the outermost surface of a support. The portion other than the polar group in the fluorine-based compound is preferably a structure consisting of fluorine and carbon because of its high hydrophobicity and chemical stability. However, as long as the structure provides sufficient hydrophobicity and chemical stability, the structure of the portion other than the polar group in the fluorine-based compound is not limited.

[0030] The polymer electrolyte may be any polymer electrolyte having proton conductivity, such as a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte. An example of a fluorine-based polymer electrolyte is Nafion (registered trademark: manufactured by DuPont). An example of a hydrocarbon-based polymer electrolyte is sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, sulfonated polyphenylene, etc. Among them, a fluorine-based polymer electrolyte, specifically Nafion (registered trademark: manufactured by DuPont) and its related materials can be preferably used. The polymer electrolyte contained in the electrode catalyst layers 12A and 12C is preferably the same material as that of the polymer electrolyte membrane 11.

[0031] The conductive fiber is a fiber made of a material having electronic conductivity, such as a carbon fiber. Specific examples of the conductive fiber include carbon fiber, carbon nanofiber, carbon nanotube, and conductive polymer nanofiber. Among them, carbon nanofiber and carbon nanotube are preferably used.

[0032] When the electrode catalyst layers 12A, 12C contain conductive fibers, a structure in which the conductive fibers are entangled is formed, and pores are suitably formed in the electrode catalyst layers 12A, 12C. This improves the gas diffusion and drainage properties in the electrode catalyst layers 12A, 12C. In addition, the occurrence of cracks in the electrode catalyst layers 12A, 12C is suppressed, and the mechanical strength is improved, so the durability of the electrode catalyst layers 12A, 12C is also improved.

[0033] Furthermore, as shown in the example of electrode catalyst layer 12C in Fig. 2, due to the entanglement of the conductive fibers, a structure in which the conductive fibers 20 are connected in a mesh-like manner is formed in each of an in-plane region R1 extending along the thickness direction of the electrode catalyst layer and an in-plane region R2 extending in a direction along the surface of the electrode catalyst layer. Therefore, the inclusion of the conductive fibers increases the conductivity in both the direction along the surface and the thickness direction of the electrode catalyst layer.

[0034] The average fiber diameter of the conductive fibers is preferably 0.5 nm or more and 500 nm or less, and more preferably 10 nm or more and 300 nm or less. If the average fiber diameter is 0.5 nm or more, the flexibility of the conductive fibers is not excessively strong, so that a structure in which the conductive fibers are entangled is suitably formed. If the average fiber diameter is 500 nm or less, it is possible to prevent the flexibility of the conductive fibers from being excessively weak, which makes it difficult to form a structure in which the conductive fibers are entangled. In addition, it is possible to prevent the pores from becoming coarse, which causes an increase in the resistance value. The average fiber diameter is obtained by averaging the diameters of five conductive fibers selected arbitrarily in the cross section of the electrode catalyst layers 12A and 12C imaged by a scanning electron microscope (SEM).

[0035] The fiber length of the conductive fibers is preferably 1 μm or more and 200 μm or less, and more preferably 1 μm or more and 50 μm or less. When the fiber length of the conductive fibers is within the above range, the mesh-like structure is suitably formed by the entanglement of the conductive fibers.

[0036] The content of the conductive fibers in the electrode catalyst layers 12A, 12C is preferably 0.1 to 2.0 times the weight of the carrier alone in the catalyst-supported particles. If the content of the conductive fibers is 0.1 times or more the weight of the carrier, a structure in which the conductive fibers are entangled is suitably formed. If the content of the conductive fibers is 2.0 times or less the weight of the carrier, an increase in the volume of the electrode catalyst layers 12A, 12C is suppressed, and therefore an increase in the resistance value is suppressed.

[0037] The gas diffusion layers 13A and 13C have gas diffusivity and electrical conductivity. The gas diffusion layers 13A and 13C preferably include a porous conductive substrate. The porous conductive substrate is a substrate having gas permeability and electrical conductivity, and is, for example, a porous carbon material such as carbon cloth, carbon paper, carbon felt, or nonwoven fabric. From the viewpoint of exhibiting sufficient water repellency without applying a water repellent treatment, it is preferable to use carbon paper, carbon cloth, or carbon felt that has been baked at a high temperature of 2000° C. or more and graphitized as the porous conductive substrate.

[0038] On the other hand, since firing at high temperatures leads to an increase in manufacturing costs, instead of the porous conductive substrate, a sheet made of a polymer material that has been carbonized to an extent that electrical conductivity can be ensured may be treated with a water repellent agent to form the gas diffusion layers 13A and 13C. As the polymer material, polyacrylonitrile is preferably used.

[0039] In addition, the porous conductive substrate does not have to be made of carbon as long as it has gas permeability, conductivity, and water repellency. For example, the porous conductive substrate may be made of a metal foam mainly made of iron, a metal foam mainly made of nickel, or a metal foam mainly made of iron and nickel.

[0040] In addition, carbon felt and carbon cloth are formed by a structure in which carbon fibers are entangled, but since the carbon fibers themselves do not have binding properties, the carbon fibers may fall off when the entanglement is undone. Therefore, when the porous conductive substrate is made of carbon fibers, it is preferable to fix the shape of the porous conductive substrate by applying or impregnating a binder. Furthermore, in this case, using a water-repellent binder is advantageous in that the manufacturing cost can be reduced. As the water-repellent binder, for example, polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), etc. are preferably used because they are stable materials.

[0041] The gas diffusion layers 13A and 13C may include a microporous layer formed on the surface of a porous conductive substrate. The microporous layer is provided on the surface of the gas diffusion layers 13A and 13C that contacts the electrode catalyst layers 12A and 12C. By providing the microporous layer, the moisture content in the electrode catalyst layers 12A and 12C is easily maintained.

[0042] The microporous layer is composed of a mixture of a conductive material and a water-repellent resin. Carbon powder is preferably used as the conductive material, and carbon powder with a small particle size is preferably used because it can smooth the surface of the microporous layer, i.e., the surfaces of the gas diffusion layers 13A and 13C. The water-repellent resin is, for example, a fluororesin such as polytetrafluoroethylene (PTFE), perfluoroethylene-propene copolymer (FEP), or tetrafluoroethylene-ethylene copolymer (ETFE).

[0043] The mass per unit area of ​​the gas diffusion layers 13A and 13C is 50 g / m 2 It is preferable that the thickness is 60 g / m or more. 2 More preferably, it is 80 g / m or more. 2 If the basis weight is within the above range, the gas diffusion layers 13A, 13C can have sufficient rigidity and tensile strength, and therefore the gas diffusion layers 13A, 13C can be easily handled. In addition, the basis weight of the gas diffusion layers 13A, 13C is preferably 150 g / m or more. 2 It is preferable that the thickness is less than 120 g / m 2 If the basis weight is within the above range, sufficient voids are ensured in the gas diffusion layers 13A and 13C, resulting in good gas diffusibility.

[0044] The thickness of the gas diffusion layers 13A, 13C is preferably 0.05 mm or more, more preferably 0.1 mm or more. The thickness of the gas diffusion layers 13A, 13C is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.35 mm or less. If the thickness is 0.05 mm or more, the tensile strength of the gas diffusion layers 13A, 13C is easily sufficient, making them easy to handle. If the thickness is 2 mm or less, the gas permeability of the gas diffusion layers 13A, 13C is easily sufficient.

[0045] The surface resistance of the gas diffusion layers 13A, 13C is preferably 1.3 Ω / □ or less, and more preferably 1.0 Ω / □ or less. The lower the surface resistance of the gas diffusion layers 13A, 13C, the higher the output voltage of the fuel cell. For example, even if there are localized areas of extremely low conductivity due to variations in water content in a laminate of an electrode catalyst layer and a gas diffusion layer, the electronic conduction in the laminate is compensated for by electronic conduction in the direction along the surface, thereby improving power generation performance.

[0046] The above surface resistance is the surface resistance of the surface of the gas diffusion layer 13A, 13C in contact with the electrode catalyst layer 12A, 12C, and is measured in accordance with JIS K 7194-1994 (a resistivity test method for conductive plastics using a four-probe method). The surface resistance of the gas diffusion layer 13A, 13C can be changed depending on the material of the gas diffusion layer 13A, 13C, the type of porous conductive substrate, the presence or absence of a microporous layer, etc.

[0047] In general, an electrode catalyst layer has pores to enhance the reactivity of the catalyst with the fuel gas or oxidant gas, and in a configuration including catalyst-supported particles and a polymer electrolyte, an aggregate of conductive carrier particles is responsible for electronic conduction. Therefore, the electrical conductivity is likely to be low due to the low interfacial resistance between particles and the low number of contacts between aggregates. In contrast, in this embodiment, the electrode catalyst layers 12A and 12C include conductive fibers, and as described above, a path for electronic conduction is formed by the connection of fibers not only in the thickness direction of the electrode catalyst layer but also in the direction along the surface, thereby enhancing the electrical conductivity. Therefore, the surface resistance of the electrode catalyst layers 12A and 12C is low, and a high output voltage can be obtained even when gas diffusion layers 13A and 13C having a high surface resistance are used, compared to when the electrode catalyst layers do not include conductive fibers.

[0048] For example, if the electrode catalyst layer does not contain conductive fibers, the surface resistance of the gas diffusion layer needs to be reduced to about 0.5 Ω / □ or less to obtain a sufficient output voltage. On the other hand, if the electrode catalyst layer 12A, 12C contains conductive fibers, a sufficient output voltage can be obtained even when the gas diffusion layer 13A, 13C having a surface resistance of 1.3 Ω / □ is used. This increases the freedom of selection of the gas diffusion layer 13A, 13C. In particular, the surface resistance of the gas diffusion layer 13A, 13C having a microporous layer is likely to be high, but good power generation performance can be obtained even when such a gas diffusion layer 13A, 13C is used.

[0049] Furthermore, the power generation performance of the fuel cell is also affected by the gas permeability and drainage of the gas diffusion layers 13A, 13C. The basis weight of the gas diffusion layers 13A, 13C is a factor that greatly affects the gas permeability and drainage. The ratio of the surface resistance to the basis weight of the gas diffusion layers 13A, 13C is a parameter that standardizes the effects of the gas permeability and drainage, and is a parameter that more accurately indicates the effect of the surface resistance on the power generation performance. In the gas diffusion layers 13A, 13C, the surface resistance to the basis weight is preferably 0.02 or less.

[0050] In addition, when only one of the electrode catalyst layer 12A and the electrode catalyst layer 12C contains conductive fibers, the gas diffusion layer laminated on the electrode catalyst layer containing conductive fibers may have a surface resistance of 1.3 Ω / □ or less and a surface resistance per unit area of ​​0.02 or less. For example, only the electrode catalyst layer 12C of the air electrode where water is produced during operation of the fuel cell may contain conductive fibers, thereby improving drainage.

[0051] [Structure of solid polymer fuel cell] The configuration of a polymer electrolyte fuel cell including the above-mentioned membrane electrode assembly 10 will be described with reference to FIG.

[0052] 3, the polymer electrolyte fuel cell 30 includes a membrane electrode assembly 10 and a pair of separators 31A, 31C. The membrane electrode assembly 10 is sandwiched between the separators 31A and 31C.

[0053] The separators 31A and 31C are made of a conductive and gas-impermeable material. The separator 31A faces the gas diffusion layer 13A, and the separator 31C faces the gas diffusion layer 13C. The separator 31A has a gas flow path 32A formed on the surface facing the gas diffusion layer 13A, and a cooling water flow path 33A formed on the surface opposite the gas diffusion layer 13A. Similarly, the separator 31C has a gas flow path 32C formed on the surface facing the gas diffusion layer 13C, and a cooling water flow path 33C formed on the surface opposite the gas diffusion layer 13C.

[0054] When the polymer electrolyte fuel cell 30 is in use, a fuel gas such as hydrogen is passed through the gas flow passage 32A of the separator 31A, and an oxidant gas such as oxygen is passed through the gas flow passage 32C of the separator 31C. Cooling water is passed through the cooling water flow passages 33A and 33C of the separators 31A and 31C. Then, the fuel gas is supplied from the gas flow passage 32A to the fuel electrode, and the oxidant gas is supplied from the gas flow passage 32C to the air electrode, whereby an electrode reaction proceeds and an electromotive force is generated between the fuel electrode and the air electrode. An organic fuel such as methanol may be supplied to the fuel electrode.

[0055] The polymer electrolyte fuel cell 30 may be used in the form of a single cell as shown in Fig. 3, or a plurality of polymer electrolyte fuel cells 30 may be stacked and connected in series to be used as one fuel cell. In addition to the above-mentioned components, the polymer electrolyte fuel cell 30 may also include a gasket or the like for preventing gas leakage.

[0056] [Method of manufacturing membrane electrode assembly] A method for producing the membrane electrode assembly 10 will now be described. First, a catalyst ink, which is a coating liquid for forming the electrode catalyst layers 12A and 12C, is prepared. The catalyst ink contains catalyst-supporting particles, a polymer electrolyte, and a solvent. When forming the electrode catalyst layers 12A and 12C containing conductive fibers, the catalyst ink further contains conductive fibers.

[0057] The solvent functions as a dispersion medium for the catalyst ink. There are no particular limitations on the solvent as long as it does not corrode the catalyst-supporting particles, the polymer electrolyte, and the conductive fibers, and can dissolve the polymer electrolyte in a highly fluid state or disperse it as a fine gel. The solvent preferably contains a volatile organic solvent.

[0058] The solvent may be, for example, alcohols, ketones, ethers, or other polar solvents. Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, and pentanol. Examples of ketones include acetone, methyl ethyl ketone, pentanone, methyl isobutyl ketone, heptanone, cyclohexanone, methylcyclohexanone, acetonylacetone, and diisobutyl ketone. Examples of ethers include tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, anisole, methoxytoluene, and dibutyl ether. Examples of other polar solvents include dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, diacetone alcohol, and 1-methoxy-2-propanol.

[0059] The solvent may be a mixed solvent containing two or more of the above-mentioned materials. The solvent may also contain water, which has a high affinity with the polymer electrolyte. There is no particular limit to the amount of water added, as long as it does not cause cloudiness due to separation of the polymer electrolyte or gelation of the polymer electrolyte. When the solvent contains a lower alcohol, it is preferable to use a mixed solvent containing water to reduce the risk of fire.

[0060] In order to improve the dispersibility of the catalyst-supported particles, the catalyst ink may contain a dispersant. Examples of dispersants include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Furthermore, the catalyst ink may be subjected to a dispersion treatment, if necessary. Examples of the dispersion treatment include stirring with a ball mill or roll mill, stirring with a shear mill, stirring with a wet mill, stirring by applying ultrasonic waves, and stirring with a homogenizer. Depending on the conditions of the dispersion treatment, the viscosity of the catalyst ink and the size of the particles contained in the catalyst ink can be controlled.

[0061] The solid content of the catalyst ink is preferably 1% by mass or more and 50% by mass or less. If the solid content is 1% by mass or more, the decrease in the film formation rate is suppressed, and therefore the decrease in productivity is suppressed. If the solid content is 50% by mass or less, the viscosity of the catalyst ink is prevented from becoming excessively high, and therefore the occurrence of cracks in the electrode catalyst layers 12A and 12C can be suppressed.

[0062] The solid content of the catalyst ink includes polymer electrolyte, catalyst-supported particles, and conductive fibers. Even with the same solid content, the viscosity of the catalyst ink will be higher if the content of catalyst-supported particles is higher. The viscosity of the catalyst ink can also be adjusted by adding a dispersant. The proportion of catalyst-supported particles in the solid content is preferably 10% by mass or more and 80% by mass or less. The viscosity of the catalyst ink is preferably 0.1 mPa·s or more and 500 mPa·s or less, and more preferably 5 mPa·s or more and 100 mPa·s or less.

[0063] In general, the greater the content of polymer electrolyte in the catalyst ink, the smaller the volume of the pores formed in the electrode catalyst layers 12A, 12C, and the greater the content of catalyst-supported particles in the catalyst ink, the larger the volume of the pores formed in the electrode catalyst layers 12A, 12C. Furthermore, the volume of the pores is reduced by the inclusion of a dispersant in the catalyst ink. When the catalyst ink is subjected to a dispersion treatment, the longer the treatment time, the more the agglomerates of the catalyst-supported particles are broken down, and the smaller the volume of the pores.

[0064] The catalyst ink may contain a pore-forming agent. By removing the pore-forming agent after the formation of the electrode catalyst layers 12A, 12C, pores can be formed. As the pore-forming agent, for example, a substance that dissolves in acid, alkali, or water, a sublimating substance such as camphor, or a thermally decomposing substance can be used. When the pore-forming agent is a substance that dissolves in hot water, the pore-forming agent may be removed by the water generated during power generation.

[0065] Examples of pore-forming agents that dissolve in acid, alkali, or water include acid-soluble inorganic salts, inorganic salts that are soluble in an aqueous alkaline solution, metals that are soluble in acid or alkali, water-soluble inorganic salts, and water-soluble organic compounds. Examples of acid-soluble inorganic salts include calcium carbonate, barium carbonate, magnesium carbonate, magnesium sulfate, and magnesium oxide. Examples of inorganic salts that are soluble in an aqueous alkaline solution include alumina, silica gel, and silica sol. Examples of metals that are soluble in acid or alkali include aluminum, zinc, tin, nickel, and iron. Examples of water-soluble inorganic salts include sodium chloride, potassium chloride, ammonium chloride, sodium carbonate, sodium sulfate, and monosodium phosphate. Examples of water-soluble organic compounds include polyvinyl alcohol and polyethylene glycol. One type of pore-forming agent may be used alone, but it is preferable to use two or more types in combination.

[0066] The catalyst ink is applied to a substrate to form a coating film, and the coating film is dried to form the electrode catalyst layers 12A and 12C. Examples of methods that can be used to apply the catalyst ink include a doctor blade method, a dipping method, a screen printing method, and a roll coating method.

[0067] As the substrate, for example, a transfer substrate is used which is peeled off after the electrode catalyst layers 12A, 12C are transferred to the polymer electrolyte membrane 11. The material of the transfer substrate is, for example, a fluororesin or an organic polymer compound other than a fluororesin. Examples of the fluororesin include ethylene tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkylvinylether copolymer (PFA), and polytetrafluoroethylene (PTFE). Examples of the organic polymer compound include polyimide, polyethylene terephthalate, polyamide, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyetherimide, polyarylate, and polyethylene naphthalate.

[0068] Furthermore, the substrate for forming the electrode catalyst layers 12A, 12C may be the polymer electrolyte membrane 11 or the gas diffusion layers 13A, 13C. When the substrate for forming the electrode catalyst layers 12A, 12C is a transfer substrate, the electrode catalyst layers 12A, 12C are bonded to the polymer electrolyte membrane 11 by thermocompression bonding, and then the transfer substrate is peeled off from the electrode catalyst layers 12A, 12C. Then, the gas diffusion layers 13A, 13C are laminated on the electrode catalyst layers 12A, 12C on the polymer electrolyte membrane 11. In this way, the membrane electrode assembly 10 is formed.

[0069] When the substrate for forming the electrode catalyst layers 12A, 12C is the gas diffusion layers 13A, 13C, the electrode catalyst layers 12A, 12C supported by the gas diffusion layers 13A, 13C are joined to the polymer electrolyte membrane 11 by thermocompression bonding to form the membrane electrode assembly 10.

[0070] When the substrate for forming the electrode catalyst layers 12A, 12C is the polymer electrolyte membrane 11, the electrode catalyst layers 12A, 12C are formed directly on the surfaces of the polymer electrolyte membrane 11, and then the gas diffusion layers 13A, 13C are laminated on the electrode catalyst layers 12A, 12C, thereby forming the membrane electrode assembly 10.

[0071] When the gas diffusion layers 13A, 13C each include a microporous layer, the microporous layer is formed by applying a coating liquid prepared by dispersing a material for the microporous layer in a dispersion medium to the surface of the porous conductive substrate, and then removing the dispersion medium by drying the coating film.

[0072] The conductive material can be divided into smaller particles by dispersing the coating liquid. For the dispersion, a pot mill, a ball mill, a bead mill, a disperser, a planetary mixer, a kneader, or an ultrasonic disperser can be used.

[0073] The coating liquid can be applied by known techniques such as an applicator method, a bar coater method, a doctor blade method, a screen printing method, a gravure printing method, a coater coating method, a spray coating method, a transfer method, an inkjet method, etc. Among these, the applicator method, the doctor blade method, and the coater coating method are preferably used because they require a small load for setting conditions for forming a smooth surface of the microporous layer.

[0074] The coating is preferably dried slowly to prevent cracks from occurring in the microporous layer. For example, it is preferable to use a dispersion medium with a high boiling point to slow down the drying rate, or to dry at a lower temperature for a longer period of time.

[0075] [Example] The above-mentioned membrane electrode assembly and solid polymer fuel cell will be described with reference to specific examples and comparative examples.

[0076] Example 1 <Adjustment of catalyst ink> A platinum-supported carbon catalyst with a catalytic substance loading density of 50 mass% was used as the catalyst-supported particles, carbon fibers with an average fiber diameter of 150 nm and a fiber length of 20 μm were used as the conductive fibers, and a fluorine-based polymer electrolyte was used as the polymer electrolyte, and the platinum-supported carbon catalyst, the carbon fibers, and the polymer electrolyte solution (Nafion (registered trademark) dispersion liquid, manufactured by Wako Pure Chemical Industries, Ltd.) with a concentration of 25 mass% were mixed in a solvent to prepare a catalyst ink. The catalyst ink was subjected to a dispersion process for 30 minutes using a planetary ball mill.

[0077] A mixed solvent of ultrapure water and 1-propanol was used as the solvent. The volume ratio of ultrapure water to 1-propanol in the mixed solvent was 1:1. The blending ratio of each material in the catalyst ink was such that the mass of the carrier in the catalyst-supported particles was 1, the mass of the conductive fiber was 0.5, and the mass of the polymer electrolyte was 0.6. The solid content in the catalyst ink was adjusted to be 15% by mass.

[0078] <Formation of electrode catalyst layer> A polytetrafluoroethylene sheet was used as a transfer substrate for forming the electrode catalyst layer, and the catalyst ink was applied to the substrate by the doctor blade method to form a coating film. The coating film was then dried at 80°C in the air to form the electrode catalyst layer. The amount of catalyst ink applied was 0.05 mg / cm2 for the platinum loading when forming the electrode catalyst layer of the fuel electrode. 2 When forming the electrode catalyst layer of the air electrode, the platinum loading was 0.2 mg / cm 2 Each was adjusted so that In Example 1, both the electrode catalyst layer of the fuel electrode and the electrode catalyst layer of the air electrode contain conductive fibers.

[0079] <Fabrication of membrane electrode assembly and polymer electrolyte fuel cell> The transfer substrate on which the electrode catalyst layer of the fuel electrode was formed and the transfer substrate on which the electrode catalyst layer of the air electrode was formed were each punched out into a square shape with a side of 5 cm. The electrode catalyst layer of the fuel electrode was then transferred from the transfer substrate to one side of the polymer electrolyte membrane, and the electrode catalyst layer of the air electrode was transferred from the transfer substrate to the other side of the polymer electrolyte membrane. The electrode catalyst layers were transferred at a temperature of 120° C. and 5.0×10 6 The hot pressing was performed at a pressure of 100 Pa. As the polymer electrolyte membrane, a fluorine-based polymer electrolyte (Nafion (registered trademark) 211, manufactured by DuPont) was used.

[0080] A laminate of a polymer electrolyte membrane and two electrode catalyst layers was sandwiched between a pair of gas diffusion layers to form a membrane electrode assembly of Example 1, and the membrane electrode assembly was sandwiched between separators to form a solid polymer electrolyte fuel cell of Example 1.

[0081] The gas diffusion layer was a carbon fiber sheet (manufactured by SGL, weight: 70 g / m) punched into a square shape with a side length of 5 cm. 2 ) was used. The carbon fiber sheet of Example 1 was a carbon paper having a microporous layer formed thereon. When the surface resistance of the carbon fiber sheet was measured by the method described below, the surface resistance was 1.22 Ω / □.

[0082] Example 2 The gas diffusion layer was a carbon fiber sheet (manufactured by Freudenberg, basis weight: 130 g / m) which is a nonwoven fabric with a microporous layer formed thereon. 2 ), a membrane electrode assembly and a fuel cell of Example 2 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Example 2 was 0.56 Ω / □.

[0083] Example 3 The gas diffusion layer was a carbon fiber sheet (manufactured by Mitsubishi Chemical Corporation, basis weight: 73 g / m) which is carbon paper with a microporous layer formed thereon. 2 ), a membrane electrode assembly and a fuel cell of Example 3 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Example 3 was 0.74 Ω / □.

[0084] Example 4 The gas diffusion layer was a carbon fiber sheet (manufactured by SGL, basis weight: 105 g / m) which is a carbon paper with a microporous layer formed thereon. 2 ), a membrane electrode assembly and a fuel cell of Example 4 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Example 4 was 0.73 Ω / □.

[0085] Comparative Example 1 The gas diffusion layer was a carbon fiber sheet (AvCarb, basis weight: 55 g / m) made of carbon paper with a microporous layer. 2 ), a membrane electrode assembly and a fuel cell of Comparative Example 1 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Comparative Example 1 was 1.89 Ω / □.

[0086] Comparative Example 2 The gas diffusion layer was a carbon fiber sheet (AvCarb, basis weight: 77 g / m) made of carbon paper with a microporous layer. 2 ), a membrane electrode assembly and a fuel cell of Comparative Example 2 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Comparative Example 2 was 1.77 Ω / □.

[0087] Comparative Example 3 In the catalyst ink, carbon particles with an average particle size of 2 nm were added as a conductive material instead of conductive fibers, and the gas diffusion layer was made of a carbon fiber sheet (manufactured by SGL, basis weight: 70 g / m), which is carbon paper with a microporous layer formed thereon. 2 ), a membrane electrode assembly and a fuel cell of Comparative Example 3 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Comparative Example 3 was 1.77 Ω / □.

[0088] Comparative Example 4 In the catalyst ink, carbon particles with an average particle size of 2 nm were added as a conductive material instead of conductive fibers, and the gas diffusion layer was made of a carbon fiber sheet (manufactured by Freudenberg, basis weight: 130 g / m) which is a nonwoven fabric with a microporous layer. 2 ), a membrane electrode assembly and a fuel cell of Comparative Example 4 were obtained using the same materials and processes as in Example 1. The surface resistance value of the gas diffusion layer of Comparative Example 4 was 0.57 Ω / □.

[0089] <Measurement of surface resistance> The surface resistance of the gas diffusion layer of each example and each comparative example was measured in accordance with JIS K 7194-1994. Specifically, first, a rectangular test piece with a length of 50 mm and a width of 80 mm was prepared for the gas diffusion layer, and the test piece was placed in an environment with a temperature of 23±2°C and a relative humidity of 50±5%, and left for 24 hours or more. Thereafter, in a test room with the same relative humidity as the environment, the resistance values ​​were measured at five points on the surface of the test piece using a digital four-probe low resistance meter, and the average value was taken as the surface resistance value of the test piece. Then, the surface resistance values ​​of three test pieces were obtained for each example and comparative example, and the average value was taken as the surface resistance value of the gas diffusion layer.

[0090] The measurement points of the resistance value of the test piece are shown in Fig. 4. In Fig. 4, in the horizontal direction of the test piece 40, a position 12.5 mm from the left end is indicated by a reference line X1, a central position between the right end and the left end is indicated by a reference line X2, and a position 12.5 mm from the right end is indicated by a reference line X3. In the vertical direction of the test piece 40, a position 10 mm from the upper end is indicated by a reference line Y1, a central position between the upper end and the lower end is indicated by a reference line Y2, and a position 10 mm from the lower end is indicated by a reference line Y3. The length between the reference line X2 and each of the reference lines X1 and X3 is 27.5 mm, and the length between the reference line Y2 and each of the reference lines Y1 and Y3 is 15 mm.

[0091] The measurement points are five points: intersection P1 between reference line X2 and reference line Y2, intersection P2 between reference line X1 and reference line Y1, intersection P3 between reference line X1 and reference line Y3, intersection P4 between reference line X3 and reference line Y1, and intersection P5 between reference line X3 and reference line Y3.

[0092] <Evaluation method> The fuel cells of each Example and Comparative Example were placed in a power generation evaluation cell, and current and voltage measurements were performed using a fuel cell measurement device. The cell temperature during the measurements was 80°C, and the relative humidity was 90% RH for the fuel electrode and 30% RH for the air electrode. Hydrogen was flowed as the fuel gas at a flow rate that gave a hydrogen utilization rate of 90%, and air was flowed as the oxidant gas at a flow rate that gave an oxygen utilization rate of 40%. The back pressure was 50 kPa, and the current density was 1.5 A / cm. 2 The voltage at this time was measured.

[0093] <Evaluation Results> The conductive material contained in the electrode catalyst layer, the surface resistance value of the gas diffusion layer, the basis weight, the surface resistance value relative to the basis weight, and the voltage measurement results in the above evaluation are shown for each Example and Comparative Example in Table 1. The voltage measurement results are expressed as the difference from the reference value A, with the value for Example 1 being taken as the reference value A, for the other Examples and Comparative Examples.

[0094] [Table 1]

[0095] As shown in Table 1, in Examples 1 to 4 in which the electrode catalyst layer contains carbon fiber and the surface resistance of the gas diffusion layer is 1.3 Ω / □ or less, a higher output voltage is obtained compared to Comparative Examples 1 to 4 in which the surface resistance of the gas diffusion layer is high or the electrode catalyst layer contains carbon particles instead of carbon fiber. In Examples 1 to 4, a tendency was confirmed that the lower the surface resistance, the higher the output voltage, and in particular, in Examples 2 to 4 in which the surface resistance is 1.0 Ω / □ or less, a high output voltage was obtained. In Examples 1 to 4, the surface resistance relative to the basis weight is 0.02 or less.

[0096] Here, comparing Example 2 and Comparative Example 4, in which the surface resistance and basis weight of the gas diffusion layer are similar but the conductive material of the electrode catalyst layer is different, Example 2 has a significantly higher output voltage. The output voltage of Comparative Example 4 is only slightly lower than that of Example 1. That is, when the conductive material is carbon particles, even if a gas diffusion layer with a low surface resistance value such as 0.57Ω / □ is used, only the same output voltage as when the conductive material is carbon fiber and a gas diffusion layer with a surface resistance value of 1.22Ω / □ is used is obtained. Therefore, it is suggested that if the conductive material is carbon fiber, a higher output voltage can be obtained than when the conductive material is carbon particles, and even if a gas diffusion layer with a surface resistance value of 0.6Ω / □ to 1.3Ω / □, which is difficult to obtain a sufficient output voltage, can be obtained when the conductive material is carbon particles.

[0097] In addition, comparing Comparative Example 2 and Comparative Example 3, which have similar surface resistance and basis weight of the gas diffusion layer but different conductive materials of the electrode catalyst layer, Comparative Example 2, in which the conductive material is carbon fiber, has a smaller output voltage. Since the surface resistance values ​​of Comparative Examples 2 and 3 are 1.77Ω / □, which is quite high, the influence of inhibition of electronic conduction due to the high surface resistance value is large, and it is considered that the difference in conductivity of the electrode catalyst layer due to the difference in conductive material is not easily reflected in the output voltage. In other words, it can be said that the effect of improving power generation performance by using carbon fiber as the conductive material is highly obtained when the surface resistance value of the gas diffusion layer is in the range of 1.3Ω / □ or less.

[0098] As described above using the examples, the membrane electrode assembly and the polymer electrolyte fuel cell according to the above embodiment provide the following effects. (1) The electrode catalyst layers 12A, 12C contain conductive fibers, and the surface resistance of the gas diffusion layers 13A, 13C is 1.3 Ω / □ or less. With this configuration, the electrical conductivity in the direction along the surface of the electrode catalyst layers 12A, 12C is increased, improving the power generation performance of the fuel cell, and allowing the gas diffusion layers 13A, 13C to be used with a higher surface resistance than when the electrode catalyst layers do not contain conductive fibers.

[0099] (2) The conductive fibers are carbon fibers, which advantageously enhances the electrical conductivity of the electrode catalyst layers 12A and 12C. (3) The surface resistance value of the gas diffusion layers 13A, 13C relative to the basis weight is 0.02 or less. With this configuration, the power generation performance of the fuel cell is suitably improved. [Explanation of symbols]

[0100] 10...Membrane electrode assembly 11...Polymer electrolyte membrane 12A,12C…electrode catalyst layer 13A, 13C...Gas diffusion layer 20...Conductive fiber 30...Polymer fuel cell 31A, 31C…Separator 32A, 32B...Gas flow path 33A, 33C…Cooling water flow path

Claims

1. A polymer electrolyte membrane; a pair of electrode catalyst layers sandwiching the polymer electrolyte membrane and in contact with the surfaces of the polymer electrolyte membrane; a gas diffusion layer laminated on each of the pair of electrode catalyst layers, At least one of the pair of electrode catalyst layers is a target catalyst layer including catalyst-supporting particles, a polymer electrolyte, and conductive fibers; The surface resistance value of the gas diffusion layer laminated on the target catalyst layer is 1.3 Ω / □ or less. Membrane electrode assembly.

2. The conductive fiber is a carbon fiber. The membrane electrode assembly according to claim 1 .

3. The mass per unit area (g / m) of the gas diffusion layer laminated on the target catalyst layer 2 ) the surface resistance is 0.02 or less The membrane electrode assembly according to claim 1 .

4. The membrane electrode assembly according to any one of claims 1 to 3, a pair of separators sandwiching the membrane electrode assembly; A polymer electrolyte fuel cell comprising:

Citation Information

Patent Citations

  • Solid polymer fuel cell

    JP2003115299A