Resin having acid group and polymerizable unsaturated group, curable resin composition, resin material for solder resist, cured product, insulation material and resist member

A resin composition with acid groups and polymerizable unsaturated groups, formed from a phenolic hydroxyl group-containing resin and other components, addresses the need for high alkali developability and low dielectric properties in solder resist materials, enhancing the performance of printed wiring boards.

JP2024160638APending Publication Date: 2024-11-14DIC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075857
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing solder resist materials struggle to form cured products with high alkali developability, high heat resistance, low elastic modulus, and low dielectric properties, which are essential for fine-pattern formation and durability in advanced printed wiring boards.

Method used

A resin with acid groups and polymerizable unsaturated groups, comprising a phenolic hydroxyl group-containing resin, a (meth)acrylate compound with an epoxy group, and a polybasic acid anhydride, which are reacted to form a curable resin composition that can be cured to achieve the desired properties.

Benefits of technology

The resin composition forms a cured product with high alkali developability, high heat resistance, low elastic modulus, and low dielectric properties, suitable for advanced printed wiring boards and semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160638000001
    Figure 2024160638000001
  • Figure 2024160638000002
    Figure 2024160638000002
  • Figure 2024160638000003
    Figure 2024160638000003
Patent Text Reader

Abstract

To provide a resin which enables formation of a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric loss tangent.SOLUTION: There is provided a resin having an acid group and a polymerizable unsaturated group which is a reaction product of a phenolic hydroxyl group-containing resin, a (meth)acrylate compound having an epoxy group, and a polybasic acid anhydride, wherein the phenolic hydroxyl group-containing resin is a reaction product of a fluorene compound (having no substituent at 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by formula (1), in the formula (1), Ar is an aromatic cyclic group that may have a substituent, R1 is each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, and X is a desorption group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin having an acid group and a polymerizable unsaturated group, a curable resin composition, a resin material for a solder resist, a cured product, an insulating material, and a resist member. [Background technology]

[0002] Solder resists are widely used as materials to prevent solder from adhering to areas other than the mounted area when electronic components are mounted and soldered on a printed wiring board, or as materials to form a coating that semi-permanently prevents oxidation and corrosion of wiring (e.g., Patent Document 1). As a technique for forming such solder resist patterns, there is a photoresist method that can accurately form fine patterns, and in particular, due to environmental considerations, an alkali-developing liquid photoresist method has become mainstream.

[0003] In addition, printed wiring boards are becoming increasingly finer, more multi-layered, and one-board in order to achieve higher density. The mounting method for printed wiring boards is also shifting to surface mount technology (SMT). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2023-028337 A Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, a material for forming a solder resist film is required to be capable of forming a cured product having high alkaline developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric tangent.

[0006] Therefore, an object of the present invention is to provide a resin capable of forming a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric tangent. [Means for solving the problem]

[0007] The resin having an acid group and a polymerizable unsaturated group according to the present invention is The resin having an acid group and a polymerizable unsaturated group is A phenolic hydroxyl group-containing resin; A (meth)acrylate compound having an epoxy group; A polybasic acid anhydride, is the reaction product of The phenolic hydroxyl group-containing resin is A fluorene compound (provided that the fluorene compound does not have a substituent at the 9-position); A phenolic hydroxyl group-containing compound, A compound represented by general formula (1), [ka] is the reaction product of In general formula (1), Ar represents an aromatic ring group which may have a substituent. R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a resin having an acid group and a polymerizable unsaturated group, which are leaving groups, and can form a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant, and low dielectric tangent.

[0008] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, the ratio (Mf / M1) of the moles (Mf) of the fluorene compound to the moles (M1) of the compound represented by general formula (1) is 0.01 to 0.99.

[0009] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, the phenolic hydroxyl group-containing resin is represented by general formula (5), [ka] In general formula (5), Each Ar is independently as defined in general formula (1), p is the average value, which is a number greater than 0 and less than or equal to 10; R 1 is as defined in general formula (1), Z is, independently of each other, a structural unit represented by general formula (2A) or general formula (3A), [ka] In general formula (2A), R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, * is a bond to general formula (5), In general formula (3A), R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is an integer from 0 to 3, * is a bond to general formula (5), Each Z' is independently a structural unit represented by general formula (2A') or general formula (3A'), [ka] In general formula (2A'), R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, Each m' is independently an integer of 0 to 4, * is a bond to general formula (5), In general formula (3A'), R 3’are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, n' is an integer from 0 to 4, * is a bond to general formula (5), The phenolic hydroxyl group-containing resin contains at least one structural unit selected from the group consisting of general formula (2A) and general formula (2A') and at least one structural unit selected from the group consisting of general formula (3A) and general formula (3A').

[0010] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, the phenolic hydroxyl group-containing resin contains at least one compound represented by general formula (5-1): [ka] In general formula (5-1), Ar and R 1 is as defined in general formula (1), Z is as defined in general formula (5), R 3’ and n' are as defined in general formula (3A'), p is 1 or 2.

[0011] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, the phenolic hydroxyl group-containing resin has a hydroxyl group equivalent of 100 to 2000 g / equivalent.

[0012] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, the phenolic hydroxyl group-containing resin has a number average molecular weight of 100 to 10,000.

[0013] In one embodiment of the resin having an acid group and a polymerizable unsaturated group according to the present invention, Ar is 1 -Y-Ar 1 and Ar1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group, R a is an aromatic ring group.

[0014] The curable resin composition according to the present invention comprises: Any of the above-mentioned resins having an acid group and a polymerizable unsaturated group; A photopolymerization initiator; This makes it possible to form a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric tangent.

[0015] In one embodiment of the curable resin composition according to the present invention, the composition further contains a resin having an acid group and a polymerizable unsaturated group other than the resin having an acid group and a polymerizable unsaturated group.

[0016] A resin material for a solder resist according to the present invention comprises any one of the curable resin compositions described above.

[0017] The cured product according to the present invention is a cured product of any of the curable resin compositions described above.

[0018] The insulating material according to the present invention comprises the above-mentioned cured product.

[0019] The resist member according to the present invention comprises the above-mentioned cured product. Effect of the Invention

[0020] According to the present invention, it is possible to provide a resin capable of forming a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric tangent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, embodiments of the present invention will be described. These descriptions are intended to be illustrative of the present invention and are not intended to limit the present invention in any way.

[0022] In the present invention, two or more embodiments can be combined in any manner.

[0023] term In this specification, (meth)acrylate refers to one or more selected from the group consisting of acrylate and methacrylate.

[0024] In this specification, the term "reaction raw material" refers to a compound that is used to obtain a target compound by a chemical reaction such as synthesis or decomposition, and that partially constitutes the chemical structure of the target compound. The term "reaction raw material" does not include substances that act as auxiliary agents in chemical reactions, such as solvents and catalysts, but do not partially constitute the chemical structure of the target compound.

[0025] In this specification, the term "structural unit" refers to a unit (repeating unit) of a chemical structure formed during a reaction or polymerization. In other words, in a product compound formed by a reaction or polymerization, it refers to a partial structure other than the structure of the chemical bonds involved in the reaction or polymerization, and is a so-called residue.

[0026] The aliphatic hydrocarbon group in this specification may be any one of a straight-chain type, a branched type and a cyclic type, and may have an unsaturated bond in the structure. The number of carbon atoms in the aliphatic hydrocarbon group is, for example, 1 to 20.

[0027] In this specification, the monovalent aliphatic hydrocarbon group includes an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkenyl group, and a cycloalkynyl group.

[0028] The alkyl group in this specification may be either linear or branched, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a 3-pentyl group, a sec-pentyl group, a tert-pentyl group, a neopentyl group, an amyl group, a hexyl group, a heptyl group, an octyl group, a cumyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group.

[0029] The alkenyl group in this specification may be either a straight-chain type or a branched type, and examples thereof include a vinyl group, an allyl group, a butenyl group, a butadienyl group, a pentenyl group, a hexyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, and a dodecenyl group.

[0030] The alkynyl group in this specification may be either straight-chain or branched, and examples thereof include an ethynyl group, a propargyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, an octynyl group, a nonynyl group, a decynyl group, an undecynyl group, and a dodecynyl group.

[0031] The cycloalkyl group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkyl group is, for example, 3 to 30. Examples of the cycloalkyl group include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, an adamantyl group, a methylcyclohexyl group, and an ethylcyclohexyl group.

[0032] The cycloalkenyl group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkenyl group is, for example, 3 to 30. Examples of the cycloalkenyl group include a cyclohexenyl group, a methylcyclohexenyl group, and an ethylcyclohexenyl group.

[0033] The cycloalkynyl group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkynyl group is, for example, 4 to 30. Examples of the cycloalkynyl group include a cyclohexynyl group, a methylcyclohexynyl group, and an ethylcyclohexynyl group.

[0034] In this specification, the divalent aliphatic hydrocarbon group includes an alkylene group, an alkenylene group, an alkynylene group, a cycloalkylene group, a cycloalkenylene group, and a cycloalkynylene group.

[0035] The alkylene group in this specification may be either a straight-chain type or a branched type, and examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, and a dodecylene group.

[0036] The alkenylene group in this specification may be either a straight-chain type or a branched type, and examples thereof include a vinylene group, a propenylene group, a butenylene group, a butadienylene group, an octenylene group, a decenylene group, and a dodecenylene group.

[0037] The alkynylene group in this specification may be either a straight-chain type or a branched type, and examples thereof include an ethynylene group, a propynylene group, a butynylene group, a butadinylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, and a dodecynylene group.

[0038] In the present specification, an alkoxy group has an alkyl-O- structure, and the definition of an alkyl group is applied to the alkyl portion in the structure. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a n-butoxy group, a sec-butoxy group, a tert-butoxy group, and an allyloxy group.

[0039] The cycloalkylene group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkylene group is, for example, 3 to 30. The cycloalkylene group is, for example, a divalent group corresponding to the groups exemplified as the cycloalkyl group.

[0040] The cycloalkenylene group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkenylene group is, for example, 3 to 30. The cycloalkenylene group is, for example, a divalent group corresponding to the groups exemplified as the cycloalkenyl group.

[0041] The cycloalkynylene group in this specification may be a monocyclic group or a polycyclic group. The number of carbon atoms in the cycloalkynylene group is, for example, 4 to 30. The cycloalkynylene group is, for example, a divalent group corresponding to the groups exemplified as the cycloalkynyl group.

[0042] In this specification, the aromatic ring is a hydrocarbon ring having aromaticity and consisting of a single ring, multiple rings, or condensed rings. The number of carbon atoms in the aromatic ring is, for example, 6 to 20. Examples of the aromatic ring include a benzene ring, a biphenyl ring, a naphthalene ring, an indene ring, an anthracene ring, and an adamantane ring. The aromatic ring group is a residue of an aromatic ring.

[0043] The aryl group in this specification is a monovalent aromatic hydrocarbon group. The number of carbon atoms in the aryl group is, for example, 6 to 20. Examples of the aryl group include a phenyl group, a naphthyl group, a biphenyl group, and a phenanthryl group.

[0044] In the present specification, the arylalkyl group is an alkyl group in which one or more, preferably one or two, particularly one hydrogen atom of the alkyl group is substituted with an aryl group, and the above description of the aryl group and the alkyl group is applied to the aryl group and the alkyl group. The arylalkyl group can be, for example, a benzyl group and a phenethyl group.

[0045] As used herein, halogen atoms include fluorine, chlorine, bromine and iodine.

[0046] In this specification, the number average molecular weight (Mn) and weight average molecular weight (Mw) are values ​​measured using gel permeation chromatography (hereinafter referred to as "GPC") under the measurement conditions described in the examples described later.

[0047] In this specification, the hydroxyl equivalent is a value measured by neutralization titration method in accordance with JIS K0070.

[0048] In this specification, the alicyclic polybasic acid anhydride refers to a compound in which an acid anhydride group is bonded to an alicyclic structure, and the presence or absence of an aromatic ring in other structural portions is not important.

[0049] The materials, components, compounds, resins, catalysts and solvents described herein may be used alone or in combination of two or more, unless otherwise specified.

[0050] In this specification, unless otherwise specified, numerical ranges are intended to include the upper and lower limits of the range. For example, 100 to 2000 g / equivalent means a range of 100 g / equivalent to 2000 g / equivalent.

[0051] In this specification, the symbols 1, 2, step (1), step (2), step (3), etc. are used to distinguish certain elements, materials, steps, etc. from other elements, materials, steps, etc., and are not intended to limit the amount of the elements or materials or the order of the steps.

[0052] In this specification, the compound represented by general formula (1), the compound represented by general formula (2), the compound represented by general formula (3), the phenolic hydroxyl group-containing resin represented by general formula (5), the phenolic hydroxyl group-containing resin represented by general formula (5-0), the phenolic hydroxyl group-containing resin represented by general formula (5-0'), and the compound represented by general formula (5-1) may be simply referred to as "compound (1)," "compound (2)," "compound (3)," "resin (5)," "resin (5-0)," "resin (5-0')," and "compound (5-1)," respectively.

[0053] In this specification, the structural unit represented by general formula (1A), the structural unit represented by general formula (2A), the structural unit represented by general formula (2A'), the structural unit represented by general formula (3A), and the structural unit represented by general formula (3A') may be simply referred to as "structural unit (1A)", "structural unit (2A)", "structural unit (2A')", "structural unit (3A)" and "structural unit (3A')", respectively.

[0054] In this specification, the resin of the present invention having an acid group and a polymerizable unsaturated group may be referred to as a "first resin," and a resin other than the resin of the present invention having an acid group and a polymerizable unsaturated group may be referred to as a "second resin."

[0055] (Resin having an acid group and a polymerizable unsaturated group) The resin having an acid group and a polymerizable unsaturated group according to the present invention is A phenolic hydroxyl group-containing resin; A (meth)acrylate compound having an epoxy group; A polybasic acid anhydride, is the reaction product of The phenolic hydroxyl group-containing resin is A fluorene compound (provided that the fluorene compound does not have a substituent at the 9-position); A phenolic hydroxyl group-containing compound, A compound represented by general formula (1), [ka] is the reaction product of In general formula (1), Ar represents an aromatic ring group which may have a substituent. R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group, a resin having an acid group and a polymerizable unsaturated group.

[0056] Phenolic hydroxyl group-containing resin The phenolic hydroxyl group-containing resin is a reaction product of a fluorene compound (wherein the fluorene compound does not have a substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1). In other words, the fluorene compound, the phenolic hydroxyl group-containing compound, and the compound represented by general formula (1) are used as reaction raw materials.

[0057] Fluorene Compounds The fluorene compound is not particularly limited, except that it has a substituent at the 9th position of the fluorene. The fluorene compound may be unsubstituted or substituted at a position other than the 9th position.

[0058] In a preferred embodiment, the fluorene compound is unsubstituted fluorene.

[0059] An example of the fluorene compound is a compound represented by the following general formula (2). [ka] In general formula (2), R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, Each m is independently an integer of 0 to 4.

[0060] R 2 Examples of the aliphatic hydrocarbon group include an alkyl group having a carbon number of 1 to 4. The alkyl group is preferably a methyl group, an ethyl group, a propyl group, or a butyl group.

[0061] R 2 Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, an indenyl group, and an indanyl group.

[0062] R 2 Examples of the arylalkyl group include a benzyl group, a phenethyl group, and a cumyl group.

[0063] R 2 Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group.

[0064] R 2 Examples of the halogen atom include fluorine, chlorine, and bromine.

[0065] m is an integer of 0, 1, 2, 3 or 4, preferably an integer of 0, 1 or 2.

[0066] In a preferred embodiment, the two m's are the same.

[0067] When both m are 1 or more, R of the two benzene rings 2 may be the same as each other or may be different.

[0068] When m is 2 or more, R 2 may be the same as each other or may be different.

[0069] In another preferred embodiment, compound (2) has two m's of 0, that is, compound (2) is an unsubstituted fluorene.

[0070] Phenolic hydroxyl group-containing compounds The phenolic hydroxyl group-containing compound is a compound having one phenolic hydroxyl group in the molecule.

[0071] An example of the phenolic hydroxyl group-containing compound is a compound represented by the general formula (3). [ka] In general formula (3), R 3” are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3” may form a ring together with the carbon atom to which they are attached, n″ is an integer from 0 to 4.

[0072] R 3” Examples of the aliphatic hydrocarbon group include an alkyl group having 1 to 4 carbon atoms. In a preferred embodiment, the alkyl group is one or more selected from the group consisting of a methyl group, an ethyl group, a propyl group, and a butyl group.

[0073] R 3” Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.

[0074] R 3” Examples of the arylalkyl group include a benzyl group, a phenethyl group, and a cumyl group.

[0075] R 3” Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group.

[0076] R 3” Examples of the halogen atom include fluorine, chlorine, and bromine.

[0077] In one preferred embodiment, R 3” is one or more selected from the group consisting of alkyl groups and aryl groups.

[0078] The Two R's 3”may form a ring together with the carbon atom to which they are bonded. Examples of the ring include a hydrocarbon ring having 6 to 20 carbon atoms constituting the ring. Examples of the ring include a benzene ring, a naphthalene ring, an anthracene ring, an adamantane ring, an indane ring, and an indene ring. Two R 3” The ring formed by may have a substituent. Examples of the substituent include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, and a halogen atom. 3” The ring formed by may be a heterocycle containing a heteroatom.

[0079] n″ is an integer of 0, 1, 2, 3 or 4, and is preferably 0, 1 or 2.

[0080] In a preferred embodiment, when n″ is 2, two R 3” together with the carbon atoms to which they are attached form a benzene or naphthalene ring.

[0081] In a preferred embodiment, compound (3) is one or more selected from the group consisting of phenol, o-cresol, 2,6-dimethylphenol, 2,3,6-trimethylphenol, 1-naphthol, and 2-naphthol.

[0082] A compound represented by formula (1) Compound (1) can modify the hydrogen atom at the 9-position of the fluorene structural unit to an aralkyl. Compound (1) can also react with a compound containing a phenolic hydroxyl group, and therefore can function as a binder. [ka] In general formula (1), Ar is an aromatic ring group which may have a substituent. R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group.

[0083] The aromatic ring group as Ar is not particularly limited, and examples thereof include a phenylene group, a biphenylene group, a naphthylene group, and an anthracenylene group. In the case of a phenylene group, it is preferable that the bonds are located at the 1- and 4-positions, in the case of a naphthylene group, it is preferable that the bonds are located at the 2- and 6-positions, and in the case of an anthracenylene group, it is preferable that the bonds are located at the 9- and 10-positions.

[0084] Examples of the substituent in the aromatic ring group include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, and a halogen atom.

[0085] Examples of the aliphatic hydrocarbon group as a substituent of the aromatic ring group include an alkyl group having 1 to 4 carbon atoms. In a preferred embodiment, the alkyl group is one or more selected from the group consisting of a methyl group, an ethyl group, a propylene group, and a butylene group.

[0086] Examples of the aryl group as a substituent of the aromatic ring group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.

[0087] Examples of the arylalkyl group as a substituent of the aromatic ring group include a benzyl group, a phenethyl group, and a cumyl group.

[0088] Examples of the alkoxy group as a substituent of the aromatic ring group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group.

[0089] Examples of the halogen atom as a substituent of the aromatic ring group include fluorine, chlorine and bromine.

[0090] In a preferred embodiment, the substituents on the aromatic ring group are one or more selected from the group consisting of alkyl groups and aryl groups.

[0091] R 1Examples of the aliphatic hydrocarbon group include a methyl group, an ethyl group, a propyl group, and a butyl group.

[0092] In one preferred embodiment, R 1 is one or more selected from the group consisting of a hydrogen atom and methyl.

[0093] R 1 may be the same or different. The four R 1 are preferably the same.

[0094] Examples of X include a hydroxyl group, a halogen atom, and an alkoxy group.

[0095] Examples of the halogen atom of X include chlorine, bromine, and iodine.

[0096] Examples of the alkoxy group for X include an alkoxy group having 1 to 4 carbon atoms. In a preferred embodiment, the alkoxy group is one or more selected from the group consisting of a methoxy group, an ethoxy group, a propyloxy group, and a butoxy group.

[0097] In a preferred embodiment, X is one or more selected from the group consisting of chlorine, bromine, iodine, a hydroxyl group, and a methoxy group.

[0098] The two X's may be the same or different.

[0099] In one embodiment, in general formula (1), Ar, Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group, R a is an aromatic ring group.

[0100] In a preferred embodiment, compound (1) is one or more selected from the group consisting of 1,4-bis(chloromethyl)benzene, 2,6-bis(chloromethyl)naphthalene, and 4,4'-bis(chloromethyl)biphenyl.

[0101] Method for producing phenolic hydroxyl group-containing resin An example of a method for producing the phenolic hydroxyl group-containing resin will be described.

[0102] The amounts of the fluorene compound, the phenolic hydroxyl group-containing compound and the compound (1) are, for example, as follows.

[0103] From the viewpoint of introducing the compound (3), the amount of the fluorene compound is preferably less than 1 mole per mole of the total of the compound (1). The amount of the fluorene compound is, for example, 0.01 moles or more or 0.05 moles or more, and 0.99 moles or less or 0.90 moles or less per mole of the total of the compound (1). In one embodiment, the amount of the fluorene compound is 0.01 to 0.99 moles per mole of the total of the compound (1).

[0104] In one embodiment, the ratio (Mf / M1) of the moles (Mf) of the fluorene compound to the total moles (M1) of the compound represented by the general formula (1) is 0.01 to 0.99. In another embodiment, Mf / M1 is 0.01 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, 0.60 or more, 0.70 or more, 0.80 or more, 0.90 or more, or 0.95 or more. In yet another embodiment, Mf / M1 is 0.99 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, 0.20 or less, or 0.10 or less. In yet another embodiment, Mf / M1 is 0.35 to 0.50.

[0105] Since substantially the entire amounts of the fluorene compound and compound (1) react with each other, the molar ratio of the fluorene compound to compound (1) used in the reaction is substantially the same as the molar ratio of the structural units derived from the fluorene compound to the structural units derived from compound (1) in the obtained phenolic hydroxyl group-containing resin.

[0106] The amount of the phenolic hydroxyl group-containing compound is, for example, an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 0.01 moles or more or 0.02 moles or more, and 10 moles or less or 9.5 moles or less, per mole of the total of the compound (1). In one embodiment, the amount of the phenolic hydroxyl group-containing compound is an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 0.01 to 10 moles, per mole of the total of the compound (1). As for the phenolic hydroxyl group-containing compound, some unreacted phenolic hydroxyl group-containing compound is also generated, but the amount of the reacted phenolic hydroxyl group-containing compound can be calculated from the hydroxyl group equivalent of the phenolic hydroxyl group-containing resin.

[0107] The phenolic hydroxyl group-containing resin can be produced, for example, by the following steps 1 and 2.

[0108] Process 1 The entire amount of the fluorene compound, the entire amount of the compound (1), and a portion of the phenolic hydroxyl group-containing compound are reacted in an organic solvent at 10 to 100° C. in the presence of an alkali catalyst.

[0109] Examples of organic solvents include toluene, xylene, mesitylene, Solvesso (trade name), dimethyl sulfoxide, dimethylformamide, and dimethylacetamide. In addition, for example, organic solvents described in JP-A-2023-028337 may be used. In a preferred embodiment, the organic solvent is one or more selected from the group consisting of toluene, xylene, mesitylene, Solvesso, dimethyl sulfoxide, dimethylformamide, and dimethylacetamide.

[0110] The amount of the organic solvent is not particularly limited, and is, for example, 50 to 500% by mass based on the total mass of compound (1) and the fluorene compound.

[0111] Examples of the alkali catalyst include lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium methoxy, sodium ethoxy, sodium tert-butoxy, potassium methoxy, potassium ethoxy, potassium tert-butoxy, triethylamine, pyridine, and dimethylaminopyridine. In a preferred embodiment, the alkali catalyst is one or more selected from the group consisting of sodium hydroxide and potassium hydroxide. The alkali catalyst may be used, for example, as a 1 to 50 mass % aqueous solution.

[0112] The amount of the alkali catalyst is, for example, 10 to 1000 mol % based on the number of moles of compound (1).

[0113] In step 1, a phase transfer catalyst may be used. Examples of the phase transfer catalyst include ammonium-based catalysts such as tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium, tetrabutylammonium iodide, tetrabutylammonium hydroxide, benzyltriethylammonium chloride, benzyltriethylammonium bromide, benzyltriethylammonium iodide, and benzyltriethylammonium hydroxide; phosphonium-based catalysts such as tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, and tetrabutylphosphonium hydroxide; and crown ether-based catalysts such as 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, and tribenzo-18-crown-6-ether. In a preferred embodiment, the phase transfer catalyst is one or more selected from the group consisting of tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltriethylammonium bromide, and benzyltriethylammonium iodide.

[0114] Additives may be used. Examples of additives include halides such as lithium bromide, sodium bromide, potassium bromide, cesium bromide, lithium iodide, sodium iodide, potassium iodide, and cesium iodide. In a preferred embodiment, the additive is one or more selected from the group consisting of sodium iodide and potassium iodide.

[0115] The reaction temperature in step 1 is, for example, 10 to 100° C. In terms of reactivity, the reaction temperature is preferably 20 to 80° C.

[0116] The reaction time in step 1 is, for example, 1 to 72 hours.

[0117] After the reaction is completed, the reaction mixture is separated into upper and lower layers as appropriate, and the lower layer, which is the aqueous layer, is removed to obtain the product. At this time, water may be added as necessary to dissolve the salt and remove the lower layer. The aqueous layer may be basic, neutral, or acidic. Examples of neutralizing agents used for neutralization include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, sodium monophosphate, and ammonium chloride; and organic acids such as methanesulfonic acid, paratoluenesulfonic acid, and oxalic acid.

[0118] Process 2 The remainder of the phenolic hydroxyl group-containing compound is added to the product obtained in step 1, and the mixture is reacted at 60 to 250° C. in the presence of an acid catalyst.

[0119] The phenolic hydroxyl group-containing compound used in step 2 may be the same as or different from the phenolic hydroxyl group-containing compound used in step 1.

[0120] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, organic acids such as methanesulfonic acid, paratoluenesulfonic acid, and oxalic acid, and Lewis acids such as boron trifluoride, aluminum chloride, and zinc chloride. In a preferred embodiment, the acid catalyst is one or more selected from the group consisting of paratoluenesulfonic acid and methanesulfonic acid.

[0121] The amount of the acid catalyst is, for example, 0.01 to 10% by mass based on the total mass of the reaction raw materials.

[0122] The reaction temperature in step 2 is, for example, 60 to 250°C. In a preferred embodiment, the reaction temperature is 80 to 240°C.

[0123] The reaction time in step 2 is, for example, 1 to 72 hours.

[0124] After the reaction in step 2 is completed, neutralization and water washing are carried out, and unreacted reactant materials, organic solvents, etc. are distilled off under reduced pressure and heating conditions to obtain a phenolic hydroxyl group-containing resin.

[0125] In the method for producing the phenolic hydroxyl group-containing resin of the present invention, for example, instead of step 1, a fluorene compound and compound (1) may be reacted in an organic solvent in the presence of a catalyst at 10 to 100°C, and then a part of the phenolic hydroxyl group-containing compound may be added and reacted at 10 to 100°C, after which the water layer is removed and a water washing treatment is performed. In this case, the product of step 1 may have a reactive group at the end. The reactive group may be an ether, a halogen group, or a hydroxyl group depending on the type of compound used.

[0126] In one embodiment, compound (2) can generate a structural unit represented by general formula (2A) or general formula (2A'), compound (3) can generate a structural unit represented by general formula (3A) or general formula (3A'), and compound (1) can generate a structural unit represented by general formula (1A). [ka] In general formulas (2A) and (2A'), m and m' are the same as m in general formula (2), R 2 and R 2’ is R in general formula (2). 2 is the same as * represents a bond. In the general formula (3A) or (3A'), n is an integer of 0 to 3, preferably 0, 1 or 2. n' is an integer of 0 to 4, preferably 0, 1 or 2; R 3 and R 3’ is R in general formula (3). 3” is the same as * represents a bond. In general formula (1A), Ar and R 1 are Ar and R in general formula (1). 1 is the same as * represents a bond.

[0127] The phenolic hydroxyl group-containing resin can contain a structure in which the structural unit (1A) is bonded to one or more units selected from the group consisting of the structural unit (2A) and the structural unit (2A').

[0128] In a preferred embodiment, at least one molecular chain terminal of the phenolic hydroxyl group-containing resin is the structural unit (3A'). In another preferred embodiment, both molecular chain terminals of the phenolic hydroxyl group-containing resin are the structural unit (3A').

[0129] In a preferred embodiment, the phenolic hydroxyl group-containing resin is composed of one or more structural units selected from the group consisting of structural units (2A) and (2A'), one or more structural units selected from the group consisting of structural units (3A) and (3A'), and structural unit (1A). A bond of the structural unit (1A) may be bonded to a bond of the structural unit (2A). When the structural unit (2A') is present, the structural unit constitutes a molecular chain terminal.

[0130] In a preferred embodiment, at least one molecular chain terminal of the phenolic hydroxyl group-containing resin is the structural unit (3A'). In another preferred embodiment, both molecular chain terminals of the phenolic hydroxyl group-containing resin are the structural unit (3A').

[0131] Preferred examples of the structural unit represented by general formula (1A) are as follows: [ka]

[0132] In one embodiment, the phenolic hydroxyl group-containing resin is represented by the following general formula (5): [ka] In general formula (5), Each Ar is independently as defined in general formula (1), p is the average value, which is a number greater than 0 and less than or equal to 10; R 1 is as defined in general formula (1), Z is, independently of each other, a structural unit represented by general formula (2A) or general formula (3A), Each Z' is independently a structural unit represented by general formula (2A') or general formula (3A'), The phenolic hydroxyl group-containing resin contains one or more structural units selected from the group consisting of general formula (2A) and general formula (2A'), and one or more structural units selected from the group consisting of general formula (3A) and general formula (3A').

[0133] In a preferred embodiment, the resin (5) is a mixture of compounds in which p in the general formula (5) is a natural number of 1 or more, and includes a compound containing, in the molecule, both one or more structural units selected from the group consisting of the structural unit (2A) and / or the structural unit (2A') and one or more structural units selected from the group consisting of the structural unit (3A) and / or the structural unit (3A').

[0134] In the phenolic hydroxyl group-containing resin, the total amount of one or more structural units selected from the group consisting of the structural unit (2A) and the structural unit (2A') is preferably 0.1 to 10 mol, and more preferably 0.5 to 9.5 mol, per 1 mol of the total amount of one or more structural units selected from the group consisting of the structural unit (3A) and the structural unit (3A').

[0135] In a preferred embodiment, the phenolic hydroxyl group-containing resin is represented by the following general formula (5-0): [ka] In general formula (5-0), Ar, R 1 , Z, R 3’ , n' and p are as defined in general formula (5).

[0136] In another preferred embodiment, the phenolic hydroxyl group-containing resin is represented by the following general formula (5-0'): [ka] In the general formula (5-0'), R 2 and m are as defined in general formula (2A), R 3 and n is as defined in general formula (3A), R 3’ and n' are as defined in general formula (3A'), Ar' is [ka] and s is the mean value and is a number greater than 0, t is the average value, and is a number equal to or greater than 0; The order of the structural units marked with s and the structural units marked with t is not limited.

[0137] s is, for example, a number from 1 to 10, or 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10. t is, for example, a number from 0 to 10, or 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10. The sum of s and t is, for example, 10 or less.

[0138] Each of the resin (5) and the resin (5-0) may be a mixture of compounds having a structural unit with p added thereto, the structural unit being a natural number of 1 or more.

[0139] In a preferred embodiment, the resin (5) contains at least one compound represented by general formula (5-1). [ka] In general formula (5-1), Ar and R 1 is as defined in general formula (1), p is 1 or 2; R 3’ and n' are as defined in general formula (3A'), Z is as defined in general formula (5).

[0140] In one embodiment, in compound (5-1), at least one Z is structural unit (2A).

[0141] The phenolic hydroxyl resin of the present invention may be a mixture of phenolic hydroxyl resins of the present invention, and the mixture may contain a compound represented by general formula (6). [ka] In general formula (6), Ar and R 1 is as defined in general formula (1), R 3’ and n' are as defined in general formula (3A').

[0142] The number average molecular weight (Mn) of the phenolic hydroxyl group-containing resin may be, for example, in the range of 100 to 10,000, and preferably in the range of 200 to 8,000. In one embodiment, the Mn of the phenolic hydroxyl group-containing resin is in the range of 300 to 1,200.

[0143] The weight average molecular weight (Mw) of the phenolic hydroxyl group-containing resin may be, for example, in the range of 100 to 50,000, and is preferably in the range of 300 to 4,000.

[0144] The molecular weight distribution (Mw / Mn) of the phenolic hydroxyl group-containing resin is in the range of, for example, 1-5, and preferably 1-4.

[0145] The hydroxyl equivalent of the phenolic hydroxyl group-containing resin is, for example, in the range of 100 to 2000 g / equivalent, preferably in the range of 200 to 1800 g / equivalent. In one embodiment, the hydroxyl equivalent of the phenolic hydroxyl group-containing resin is in the range of 200 to 400 g / equivalent.

[0146] (Meth)acrylate compound having an epoxy group The (meth)acrylate compound having epoxy group is not particularly limited, except that it has (meth)acryloyl group and epoxy group in the molecular structure.The (meth)acrylate compound having epoxy group can be, for example, (meth)acrylate monomer having glycidyl group such as glycidyl acrylate, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether, 4-hydroxybutyl methacrylate glycidyl ether, epoxycyclohexylmethyl acrylate and epoxycyclohexylmethyl methacrylate; and mono(meth)acrylate of diglycidyl ether compound such as dihydroxybenzene diglycidyl ether, dihydroxynaphthalene diglycidyl ether, biphenol diglycidyl ether and bisphenol diglycidyl ether. In a preferred embodiment, the (meth)acrylate compound having an epoxy group is one or more selected from the group consisting of glycidyl acrylate, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether, 4-hydroxybutyl methacrylate glycidyl ether, epoxycyclohexylmethyl acrylate, and epoxycyclohexylmethyl methacrylate.

[0147] In a preferred embodiment, from the viewpoint of obtaining a curable resin composition that has excellent alkali developability and is capable of forming a cured product excellent in elongation, adhesion and dielectric properties, the amount of the (meth)acrylate compound having an epoxy group is in a range such that the number of moles of the epoxy group in the (meth)acrylate compound having an epoxy group is 0.9 to 1.1 moles, or the number of moles of the epoxy group is 0.95 to 1.1 moles, per mole of the phenolic hydroxyl group in the phenolic hydroxyl group-containing resin.

[0148] Polybasic Acid Anhydrides Examples of the polybasic acid anhydride include aliphatic polybasic acid anhydrides; alicyclic polybasic acid anhydrides; aromatic polybasic acid anhydrides; acid halides of aliphatic polybasic acid anhydrides; acid halides of alicyclic polybasic acid anhydrides; and acid halides of aromatic polybasic acid anhydrides.

[0149] Examples of the aliphatic polybasic acid anhydride include oxalic acid anhydride and succinic acid anhydride. In addition, for example, the aliphatic polybasic acid anhydride described in JP-A-2023-028337 may be used. The aliphatic hydrocarbon group of the aliphatic polybasic acid anhydride may be either a straight chain type or a branched type, and may have an unsaturated bond in the structure.

[0150] Examples of the alicyclic polybasic acid anhydride include 1,2,3,6-tetrahydrophthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, and cyclohexanedicarboxylic anhydride. In addition, for example, the alicyclic polybasic acid anhydride described in JP-A-2023-028337 may be used.

[0151] Examples of aromatic polybasic acid anhydrides include phthalic anhydride. In addition, aromatic polybasic acid anhydrides described in JP-A-2023-028337 may be used.

[0152] From the viewpoint of obtaining a curable resin composition that has excellent alkaline developability and is capable of forming a cured product excellent in elongation, adhesion and dielectric properties, the polybasic acid anhydride is preferably one or more selected from the group consisting of 1,2,3,6-tetrahydrophthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, succinic anhydride and cyclohexanedicarboxylic anhydride.

[0153] The amount of the polybasic acid anhydride may be appropriately adjusted. For example, from the viewpoint of obtaining a curable resin composition having excellent alkali developability and capable of forming a cured product having excellent elongation, adhesion and dielectric properties, the amount of the polybasic acid anhydride is preferably in the range of 0.2 to 1.05 mol, more preferably in the range of 0.3 to 0.95 mol, and even more preferably in the range of 0.3 to 0.9 mol, per mol of the phenolic hydroxyl group of the phenolic hydroxyl group-containing resin.

[0154] From the viewpoint of obtaining a curable resin composition that has excellent alkaline developability and is capable of forming a cured product excellent in elongation, adhesion and dielectric properties, the total mass of the phenolic hydroxyl group-containing resin, the (meth)acrylate compound having an epoxy group and the polybasic acid anhydride is preferably 70 mass% or more based on the total mass of the solid contents of the raw materials of the resin having an acid group and a polymerizable unsaturated group.

[0155] Method for producing resin having acid group and polymerizable unsaturated group The method for producing the resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. For example, the resin may be produced by a method in which all of the reaction raw materials containing a phenolic hydroxyl group-containing resin, a (meth)acrylate compound having an epoxy group, and a polybasic acid anhydride are reacted at once, or the reaction raw materials are reacted sequentially. Since the reaction can be easily controlled, a method in which a phenolic hydroxyl group-containing resin and a (meth)acrylate compound having an epoxy group are reacted in the presence of a basic catalyst at a temperature range of 80 to 140°C, and then a polybasic acid anhydride is added and reacted at a temperature range of 80 to 140°C is preferred.

[0156] The reaction of the phenolic hydroxyl group-containing resin, the (meth)acrylate compound having an epoxy group, and the polybasic acid anhydride can be carried out in an organic solvent if necessary. A polymerization inhibitor or an antioxidant can also be used if necessary.

[0157] Examples of the basic catalyst include amine compounds such as triethylamine. In addition, the basic catalyst described in JP-A-2023-028337 may be used. The basic catalyst may be used in the form of an aqueous solution of about 10 to 55% by mass, or in the form of a solid.

[0158] The amount of the basic catalyst may be appropriately adjusted. For example, since a curable resin composition having excellent alkali developability and capable of forming a cured product having excellent elongation, adhesion and dielectric properties can be obtained, the amount of the basic catalyst is preferably in the range of 0.01 to 1 part by mass, more preferably in the range of 0.05 to 0.8 parts by mass, based on 100 parts by mass in total of the phenolic hydroxyl group-containing resin, the (meth)acrylate compound having an epoxy group and the polybasic acid anhydride.

[0159] Examples of the organic solvent include diethylene glycol monoethyl ether acetate and propylene glycol monomethyl ether acetate. In addition, the organic solvents described in JP-A-2023-028337 may be used.

[0160] The amount of the organic solvent is not particularly limited and may be appropriately adjusted. The amount of the organic solvent is preferably in the range of about 0.1 to 5 times the total mass of the reaction raw materials, since this improves the reaction efficiency.

[0161] A mixed solvent of an organic solvent and water may be used. The amount of water in the mixed solvent is preferably in the range of 5 to 60 parts by mass, more preferably 10 to 50 parts by mass, per 100 parts by mass of the mixed solvent.

[0162] Examples of the polymerization inhibitor include methoquinone. In addition, the polymerization inhibitors described in JP-A-2023-028337 may be used.

[0163] As the antioxidant, the compounds exemplified as the polymerization inhibitor can be used.

[0164] (Curable resin composition) The curable composition according to the present invention comprises A resin having an acid group and a polymerizable unsaturated group of the present invention, A photopolymerization initiator; The curable resin composition comprises:

[0165] The amount of the resin having an acid group and a polymerizable unsaturated group in the curable resin composition is not particularly limited and may be appropriately adjusted. For example, the amount of the resin having an acid group and a polymerizable unsaturated group in the curable resin composition is 30 to 98 parts by mass in terms of the solid content of the resin having an acid group and a polymerizable unsaturated group relative to 100 parts by mass of the solid content of the curable resin composition.

[0166] As the photopolymerization initiator, a known photopolymerization initiator can be used. As the photopolymerization initiator, for example, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one and the like can be mentioned. In addition, for example, the polymerization inhibitor described in JP-A-2023-028337 can also be used.

[0167] The amount of the photopolymerization initiator may be appropriately adjusted, for example, in the range of 0.5 to 20 parts by mass with respect to 100 parts by mass of the curable resin composition.

[0168] The curable resin composition of the present invention may contain a resin component other than the resin having an acid group and a polymerizable unsaturated group of the present invention (hereinafter, sometimes referred to as "other resin components"). Examples of the other resin components include a second resin and a (meth)acrylate monomer.

[0169] In addition, the curable resin composition of the present invention may contain additives such as a curing accelerator, an ultraviolet absorber, a polymerization inhibitor, an antioxidant, an organic solvent, an inorganic filler, a polymer fine particle, a pigment, an antifoaming agent, a viscosity modifier, a leveling agent, a flame retardant, and a storage stabilizer, as necessary. Examples of these additives include the additives described in JP-A-2023-028337.

[0170] Examples of the second resin include epoxy resins having an acid group and a polymerizable unsaturated group, urethane resins having an acid group and a polymerizable unsaturated group, acrylic resins having an acid group and a polymerizable unsaturated group, amide-imide resins having an acid group and a polymerizable unsaturated group, acrylamide resins having an acid group and a polymerizable unsaturated group, and ester resins having an acid group and a polymerizable unsaturated group, as described in JP 2023-028337 A.

[0171] The amount of the second resin may be appropriately adjusted, for example, within the range of 10 to 900 parts by mass with respect to 100 parts by mass of the first resin.

[0172] One embodiment of the curable resin composition according to the present invention further contains a second resin.

[0173] Examples of the (meth)acrylate monomer include EO-modified diacrylate of bisphenol A, dipentaerythritol hexaacrylate, and dipentaerythritol hexamethacrylate. Other examples include the (meth)acrylate monomers described in JP-A-2023-028337.

[0174] The amount of the (meth)acrylate monomer may be appropriately adjusted, for example, from 1 to 90 parts by mass relative to 100 parts by mass of the curable resin composition.

[0175] The curing accelerator has a function of accelerating the curing reaction, and examples of the curing accelerator include phosphorus compounds, amine compounds, imidazole, organic acid metal salts, Lewis acids, and amine complex salts.

[0176] The amount of the curing accelerator may be appropriately adjusted, for example, in the range of 0.01 to 10 parts by mass with respect to 100 parts by mass of the solid content of the curable resin composition.

[0177] The curable resin composition can be obtained by mixing the resin having an acid group and a polymerizable unsaturated group of the present invention, a photopolymerization initiator, and any optional components.

[0178] In addition, the cured product of the curable resin composition of the present invention has excellent alkali developability and is excellent in elongation, adhesion and dielectric properties, and therefore can be suitably used, for example, in semiconductor device applications, such as solder resists, insulating materials, packaging materials, underfill materials, and package adhesive layers for circuit elements and the like; adhesive layers between integrated circuit elements and circuit boards; and in thin display applications, such as thin film transistor protective films, liquid crystal color filter protective films, resist members and spacers.

[0179] A cured product can be obtained by irradiating the curable resin composition of the present invention with active energy rays. Examples of active energy rays include ultraviolet rays.

[0180] Examples of ultraviolet light sources include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, gallium lamps, metal halide lamps, sunlight, and LEDs.

[0181] The curing method of the curable resin composition is not particularly limited, and a known curing method for a photocurable resin composition can be used. For example, the curing method described in JP-A-2023-028337 can be used.

[0182] A resin material for a solder resist according to the present invention comprises any one of the curable resin compositions described above.

[0183] The cured product according to the present invention is a cured product of any of the curable resin compositions described above.

[0184] The resist member according to the present invention comprises the above-mentioned cured product.

[0185] The resist member of the present invention can be obtained, for example, by applying a solder resist resin material onto a substrate, drying the applied material at about 60 to 100°C, exposing the applied material to active energy rays through a photomask having a desired pattern formed thereon, developing the unexposed areas with an alkaline aqueous solution, and further heating and curing the applied material at about 140 to 200°C.

[0186] Substrates include, for example, metals such as copper and aluminum.

[0187] The insulating material according to the present invention comprises the above-mentioned cured product. EXAMPLES

[0188] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0189] GPC measurements The Mn, Mw and Mw / Mn of the phenolic hydroxyl group-containing resins obtained in the Examples and Comparative Examples were calculated using the following measuring equipment and conditions. Sample: Filtrate (50 μL) obtained by filtering a tetrahydrofuran solution of 1.0% by mass (based on resin solid content) of the phenolic hydroxyl group-containing resin obtained in the synthesis example through a microfilter The measuring device, column, detector, data processing, measuring conditions and polystyrene used are the same as those described in paragraph

[0191] of JP 2023-028337 A.

[0190] softening point Measurement method: The softening points (° C.) of the phenolic hydroxyl group-containing resins obtained in the synthesis examples shown below were measured according to JIS K7234 (ring and ball method).

[0191] FD-MS measurements The FD-MS spectrum of the phenolic hydroxyl group-containing resin was measured using the measurement device and measurement conditions described in paragraph

[0157] of JP 2021-102714 A.

[0192] 13 C-NMR measurement Phenolic hydroxyl group-containing resin 13 C-NMR spectra were measured using the following equipment and conditions. 13 C-NMR: Manufactured by JEOL, product name "JNM-ECZ400S" Resonance frequency: 100MHz Number of times: 4000 Solvent: Chloroform-d Sample concentration: 12% by mass Relaxation agent: Chromium(III) acetylacetonate

[0193] Details of the components in Tables 2 and 3 are as follows. Hardener: Orthocresol novolac epoxy resin, manufactured by DIC Corporation, product name "EPICLON N-680", epoxy equivalent: 214g / equivalent Organic solvent: Diethylene glycol monoethyl ether acetate Photopolymerization initiator: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, manufactured by IGM Resins, trade name "Omnirad 907" Acrylate monomer: dipentaerythritol hexaacrylate Heat cure accelerator: 2-ethyl-4-methylimidazole

[0194] Comparative Example Phenolic Resin Biphenyl aralkyl phenol resin: Meiwa Kasei Co., Ltd., product name "MEHC-7851SS", hydroxyl equivalent: 212g / equivalent

[0195] Copper foil: Manufactured by Furukawa Sangyo Co., Ltd., electrolytic copper foil, product name "F2-WS", 18μm Viscoelasticity measuring device: DMA: Rheometrics, solid viscoelasticity measuring device, product name "RSAII" Tensile testing machine: Shimadzu Corporation, precision universal testing machine Autograph, product name "AG-IS"

[0196] The compound names and their abbreviations are as follows: Dimethyl sulfoxide: DMSO Methyl isobutyl ketone: MIBK

[0197] Synthesis Example 1: Preparation of Phenolic Hydroxyl Group-Containing Resin A1 In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer, 100.0 parts by mass of fluorene, 273.4 parts by mass of 1,4-bis(chloromethyl)benzene, 147.0 parts by mass of phenol, 520.4 parts by mass of toluene and 520.4 parts by mass of DMSO were added, and the mixture was heated to 40°C and homogenized. Then, 269.4 parts by mass of 49% by mass of sodium hydroxide aqueous solution were dropped so that the temperature was 60°C or less. After the dropping, the temperature was raised to 60°C and reacted for 8 hours, after which 383.9 parts by mass of water was added, the salt was dissolved, and the lower layer was removed by separation. Then, the organic layer was neutralized with 6.88 parts by mass of 89% by mass of phosphoric acid aqueous solution, and then washed three times with 383.9 parts by mass of water. Next, 283.1 parts by mass of phenol and 10.4 parts by mass of p-toluenesulfonic acid monohydrate were added, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 4.52 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while adding 812.8 parts by mass of MIBK, and washed three times with 575.8 parts by mass of water at 80°C. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, and a phenolic hydroxyl group-containing resin A1 was obtained. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=558.3, 754.4, and 826.4, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0198] Synthesis Example 2: Preparation of Phenolic Hydroxyl Group-Containing Resin A2 In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer, 100.0 parts by mass of fluorene, 210.6 parts by mass of 1,4-bis(chloromethyl)benzene, 130.1 parts by mass of o-cresol, 440.7 parts by mass of toluene and 440.7 parts by mass of DMSO were added, and the mixture was heated to 40°C and homogenized. Then, 297.7 parts by mass of 49% by mass of sodium hydroxide aqueous solution were dropped so that the temperature was 60°C or less. After the dropping, the temperature was raised to 60°C and reacted for 8 hours, after which 424.2 parts by mass of water was added, the salt was dissolved, and the lower layer was removed by separation. Then, the organic layer was neutralized with 3.97 parts by mass of 89% by mass of phosphoric acid aqueous solution, and then washed three times with 424.2 parts by mass of water. Next, 325.3 parts by mass of o-cresol and 8.81 parts by mass of p-toluenesulfonic acid monohydrate were added, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 3.83 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while adding 661.1 parts by mass of toluene, and washed three times with 424.2 parts by mass of water at 80°C. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, and a phenolic hydroxyl group-containing resin A2 was obtained. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=586.4, 796.5, and 1064.7, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0199] Synthesis Example 3: Preparation of Phenolic Hydroxyl Group-Containing Resin A3 A flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer was charged with 75.0 parts by mass of fluorene, 158.0 parts by mass of 1,4-bis(chloromethyl)benzene, 110.3 parts by mass of 2,6-dimethylphenol, 343.2 parts by mass of toluene and 343.2 parts by mass of DMSO, and the temperature was raised to 40°C to homogenize. Then, 223.3 parts by mass of 49% by mass of sodium hydroxide aqueous solution was dropped so that the temperature was 60°C or less. After dropping, the temperature was raised to 60°C and reacted for 8 hours, after which 318.2 parts by mass of water was added, the salt was dissolved, and the lower layer was removed by separation. Then, the organic layer was neutralized with 2.98 parts by mass of 89% by mass of phosphoric acid aqueous solution, and then washed three times with 318.2 parts by mass of water. Next, 165.4 parts by mass of 2,6-dimethylphenol and 6.86 parts by mass of p-toluenesulfonic acid monohydrate were added, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 2.98 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while adding 343.2 parts by mass of toluene, and washed three times with 318.2 parts by mass of water at 80°C. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, and a phenolic hydroxyl group-containing resin A3 was obtained. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=614.4 and 838.5, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0200] Synthesis Example 4: Production of Phenolic Hydroxyl Group-Containing Resin A4 In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer, 75.0 parts by mass of fluorene, 158.0 parts by mass of 1,4-bis(chloromethyl)benzene, 130.1 parts by mass of 2-naphthol, 363.1 parts by mass of toluene and 363.1 parts by mass of DMSO were added, and the mixture was heated to 40°C and homogenized. Then, 223.3 parts by mass of 49% by mass of sodium hydroxide aqueous solution were dropped so that the temperature was 60°C or less. After the dropping, the temperature was raised to 60°C and reacted for 8 hours, after which 318.2 parts by mass of water was added, the salt was dissolved, and the lower layer was removed by separation. Then, the organic layer was neutralized with 2.98 parts by mass of 89% by mass of phosphoric acid aqueous solution, and then washed three times with 318.2 parts by mass of water. Next, 195.2 parts by mass of 2-naphthol and 7.26 parts by mass of p-toluenesulfonic acid monohydrate were added, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 3.15 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while adding 544.6 parts by mass of toluene, and washed three times with 435.7 parts by mass of isopropyl alcohol and 318.2 parts by mass of water. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, and a phenolic hydroxyl group-containing resin A4 was obtained. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=658.4, 904.5, and 1172.7, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0201] Synthesis Example 5: Synthesis of phenolic hydroxyl group-containing resin A5 In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer, 75.0 parts by mass of fluorene, 294.2 parts by mass of 4,4'-bis(chloromethyl)biphenyl, 110.3 parts by mass of phenol, 479.5 parts by mass of toluene and 479.5 parts by mass of DMSO were added, and the mixture was heated to 40°C and homogenized. Then, 202.7 parts by mass of 49% by mass of sodium hydroxide aqueous solution were dropped so that the temperature was 60°C or less. After the dropping, the temperature was raised to 60°C and reacted for 8 hours, after which 413.0 parts by mass of water was added, the salt was dissolved and the mixture was cooled to room temperature. Then, 193.5 parts by mass of 89% by mass of phosphoric acid aqueous solution was dropped to neutralize the mixture, and the lower layer was removed by liquid separation. At that time, it was confirmed that the lower layer was acidic. Next, 212.3 parts by mass of phenol and 9.59 parts by mass of p-toluenesulfonic acid monohydrate were added, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted for 3 hours. After the reaction was completed, the mixture was cooled to 80°C while adding 719.2 parts by mass of toluene, and 4.2 parts by mass of a 49% by mass aqueous solution of sodium hydroxide was added, followed by washing with 394.0 parts by mass of water at 80°C four times to neutralize the organic layer. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, thereby obtaining a phenolic hydroxyl group-containing resin A5. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=710.4 and 982.4, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0202] Synthesis Example 6: Synthesis of phenolic hydroxyl group-containing resin A6 In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube and a stirrer, 50.0 parts by mass of fluorene, 79.0 parts by mass of 1,4-bis(chloromethyl)benzene, 37.8 parts by mass of 4,4'-bis(chloromethyl)biphenyl, 7.76 parts by mass of tetrabutylammonium bromide, 4.0 parts by mass of potassium iodide and 333.5 parts by mass of xylene were added, and the mixture was heated to 60°C and homogenized. Then, 154.7 parts by mass of a 48% by mass aqueous sodium hydroxide solution were added dropwise. After the dropwise addition, the mixture was reacted at 60°C for 6 hours. Then, 91.1 parts by mass of 1-naphthol, 64.5 parts by mass of isopropyl alcohol and 142.3 parts by mass of water were added, and the mixture was heated to 75°C and reacted for 5 hours. The lower layer was then removed by separation and washed six times with 209.6 parts by mass of water. Next, 130.1 parts by mass of 1-naphthol and 4.2 parts by mass of p-toluenesulfonic acid were added, and the mixture was heated to 160°C and reacted for 3 hours. After the reaction was completed, the mixture was cooled and neutralized by adding 1.8 parts by mass of a 49% by mass aqueous solution of sodium hydroxide. The mixture was then heated and distilled under reduced pressure to remove the solvent and 1-naphthol, yielding a phenolic hydroxyl group-containing resin A6. 13 The C-NMR chart confirmed that the reaction had started at the 9-position of the fluorene. The FD-MS chart showed m / z=658.4 and 734.4, confirming that the product was the desired phenolic hydroxyl group-containing resin.

[0203] Table 1 shows the Mn, Mw, Mw / Mn, hydroxyl equivalent, softening point and Mf / M1 of the obtained phenolic hydroxyl group-containing resins A1 to A6.

[0204] [Table 1]

[0205] Example 1: Synthesis of resin 1 having an acid group and a polymerizable unsaturated group In a flask equipped with a thermometer, a stirrer and a reflux condenser, 157.3 parts by mass of diethylene glycol monoethyl ether acetate was placed, 225 parts by mass of the phenolic hydroxyl group-containing resin A1 obtained in Synthesis Example 1 was dissolved, 0.9 parts by mass of dibutyl hydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 1.8 parts by mass of triethylamine were added, and the mixture was reacted at 120 ° C for 15 hours while blowing air. Next, 93.5 parts by mass of diethylene glycol monoethyl ether acetate and 98.8 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110 ° C for 3 hours. Next, 1.8 parts by mass of phosphoric acid was added and stirred at 80 ° C for 2 hours to obtain resin 1 having an acid group and a polymerizable unsaturated group. The non-volatile content of resin 1 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 81 mg KOH / g.

[0206] Example 2: Synthesis of resin 2 having an acid group and a polymerizable unsaturated group In a flask equipped with a thermometer, a stirrer and a reflux condenser, 169.7 parts by mass of diethylene glycol monoethyl ether acetate was placed, 254 parts by mass of the phenolic hydroxyl group-containing resin A2 obtained in Synthesis Example 2 was dissolved, 1 part by mass of dibutyl hydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 2 parts by mass of triethylamine were added, and the mixture was reacted at 120°C for 14 hours while blowing air. Next, 100.8 parts by mass of diethylene glycol monoethyl ether acetate and 106.4 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours. Next, 2 parts by mass of phosphoric acid were added and stirred at 80°C for 2 hours to obtain a resin 2 having an acid group and a polymerizable unsaturated group. The non-volatile content of the resin 2 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 81 gKOH / g.

[0207] Example 3: Synthesis of resin 3 having an acid group and a polymerizable unsaturated group In a flask equipped with a thermometer, a stirrer and a reflux condenser, 177 parts by mass of diethylene glycol monoethyl ether acetate was placed, 271 parts by mass of the phenolic hydroxyl group-containing resin A3 obtained in Synthesis Example 3 was dissolved, 1 part by mass of dibutyl hydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 2.1 parts by mass of triethylamine were added, and the mixture was reacted at 120 ° C for 13 hours while blowing air. Next, 104.3 parts by mass of diethylene glycol monoethyl ether acetate and 109.4 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110 ° C for 3 hours. Next, 2.1 parts by mass of phosphoric acid were added, and the mixture was stirred at 80 ° C for 2 hours to obtain a resin 3 having an acid group and a polymerizable unsaturated group. The non-volatile content of the resin 3 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 80 mg KOH / g.

[0208] Example 4: Synthesis of resin 4 having an acid group and a polymerizable unsaturated group In a flask equipped with a thermometer, a stirrer and a reflux condenser, 205.3 parts by mass of diethylene glycol monoethyl ether acetate was placed, 337 parts by mass of the phenolic hydroxyl group-containing resin A4 obtained in Synthesis Example 4 was dissolved, 1.2 parts by mass of dibutyl hydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 2.4 parts by mass of triethylamine were added, and the mixture was reacted at 120 ° C for 13 hours while blowing air. Next, 122.2 parts by mass of diethylene glycol monoethyl ether acetate and 129.2 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110 ° C for 3 hours. Next, 2.4 parts by mass of phosphoric acid were added, and the mixture was stirred at 80 ° C for 2 hours to obtain a resin 4 having an acid group and a polymerizable unsaturated group. The nonvolatile content of the resin 4 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 81 mg KOH / g.

[0209] Example 5: Synthesis of Resin 5 Having Acid Groups and Polymerizable Unsaturated Groups A flask equipped with a thermometer, a stirrer, and a reflux condenser was charged with 183.9 parts by mass of diethylene glycol monoethyl ether acetate, and 287 parts by mass of the phenolic hydroxyl group-containing resin A5 obtained in Synthesis Example 5 was dissolved therein. After adding 1.1 parts by mass of dibutylhydroxytoluene and 0.2 parts by mass of methoquinone, 142 parts by mass of glycidyl methacrylate and 2.1 parts by mass of triethylamine were added, and the mixture was reacted at 120°C for 16 hours while blowing in air. Next, 108.5 parts by mass of diethylene glycol monoethyl ether acetate and 114 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours. Next, 2.1 parts by mass of phosphoric acid were added and stirred at 80°C for 2 hours to obtain a resin 5 having an acid group and a polymerizable unsaturated group. The nonvolatile content of the resin 5 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 80 mgKOH / g.

[0210] Example 6: Synthesis of Resin 6 Having Acid Groups and Polymerizable Unsaturated Groups In a flask equipped with a thermometer, a stirrer and a reflux condenser, 215.1 parts by mass of diethylene glycol monoethyl ether acetate was placed, 360 parts by mass of the phenolic hydroxyl group-containing resin A6 obtained in Synthesis Example 6 was dissolved, 1.3 parts by mass of dibutyl hydroxytoluene and 0.3 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 2.5 parts by mass of triethylamine were added, and the mixture was reacted at 120 ° C for 12 hours while blowing air. Next, 128 parts by mass of diethylene glycol monoethyl ether acetate and 135.3 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and reacted at 110 ° C for 3 hours. Next, 2.5 parts by mass of phosphoric acid were added, and the mixture was stirred at 80 ° C for 2 hours to obtain a resin 6 having an acid group and a polymerizable unsaturated group. The non-volatile content of the resin 6 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 81 mgKOH / g.

[0211] Comparative Example 1: Synthesis of Resin C1 Having Acid Groups and Polymerizable Unsaturated Groups In a flask equipped with a thermometer, a stirrer and a reflux condenser, 151.7 parts by mass of diethylene glycol monoethyl ether acetate was placed, 105 parts by mass of biphenyl aralkyl phenol resin was dissolved, 0.9 parts by mass of dibutyl hydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 142 parts by mass of glycidyl methacrylate and 1.8 parts by mass of triethylamine were added, and the mixture was reacted at 120°C for 17 hours while blowing air. Next, 89.6 parts by mass of diethylene glycol monoethyl ether acetate and 94.2 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride were added and the mixture was reacted at 110°C for 3 hours. Next, 1.8 parts by mass of phosphoric acid was added and stirred at 80°C for 2 hours to obtain a resin C1 having an acid group and a polymerizable unsaturated group. The non-volatile content of the resin C1 having an acid group and a polymerizable unsaturated group was 65% by mass, and the solid acid value was 81 mgKOH / g.

[0212] Examples 7 to 12, Comparative Example 2 Curable resin compositions were prepared by mixing the components according to the formulation shown in Table 2. The amounts of solids other than the organic solvent are shown.

[0213] [Table 2]

[0214] The following evaluation of alkaline developability was carried out using the curable resin compositions 1 to 6 and C1. The results are shown in Table 2.

[0215] Alkaline developability The obtained curable resin composition was applied to a glass substrate with an applicator to a film thickness of 50 μm. Each curable resin composition was dried at 80° C. for 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes, 120 minutes, 130 minutes, 140 minutes, and 150 minutes to prepare 10 samples with different drying times. These were developed with a 1% by mass aqueous sodium carbonate solution at 30° C. for 180 seconds. The drying time (min) at 80° C. of the sample that did not leave any residue on the glass substrate was evaluated as the drying control width. The longer the drying control width, the better the alkaline developability.

[0216] Examples 13 to 18, Comparative Example 3 Curable resin compositions were prepared by mixing the components according to the formulation shown in Table 3. The amounts of solids other than the organic solvent are shown.

[0217] [Table 3]

[0218] The curable resin compositions 7 to 12 and C2 were used to evaluate the heat resistance, elastic modulus, relative dielectric constant and dielectric tangent as follows. The results are shown in Table 3.

[0219] heat resistance The obtained curable resin composition was applied to a copper foil using an applicator to a film thickness of 50 μm, and dried at 80° C. for 30 minutes. 2 The coating film was irradiated with ultraviolet light of 1000 nm. The coating film was heated at 160°C for 1 hour to obtain a cured coating film. The cured coating film was then peeled off from the copper foil to obtain a cured product of the curable resin composition. A test piece 1 of 6 mm x 35 mm was cut out from this cured product, and the temperature (°C) at which the change in elastic modulus was maximum was evaluated as the glass transition temperature (Tg) using a viscoelasticity measuring device by a tensile method (frequency 1 Hz, heating rate 3°C / min). A higher Tg indicates better heat resistance.

[0220] Elasticity In the same manner as in the evaluation of heat resistance, a cured product was obtained from the curable resin composition. A test piece 2 of 10 mm x 80 mm was cut out from the cured product. A tensile test was performed on the test piece 2 using a precision universal testing machine under the following measurement conditions. The elastic modulus (MPa) until the test piece 2 broke was measured. Measurement conditions Temperature: 23℃ Humidity: 50% Distance between gauge lines: 20mm Distance between fulcrums: 20mm Pulling speed: 10mm / min

[0221] Dielectric constant The obtained curable resin composition was applied to a glass substrate using an applicator to a thickness of 50 μm, and dried at 80° C. for 30 minutes. Then, a metal halide lamp was used to apply the applied curable resin composition to a glass substrate at a density of 10 kJ / m 2 The coating film was irradiated with ultraviolet light of 1000 nm. The coating film was heated at 160°C for 1 hour to obtain a cured coating film. The cured coating film was then peeled off from the glass substrate to obtain a cured product of the curable resin composition. The cured product was then stored for 24 hours in a room at a temperature of 23°C and a humidity of 50%, and used as test piece 3. The relative dielectric constant of test piece 3 at 1 GHz was measured by a cavity resonance method using a network analyzer E8362C manufactured by Agilent Technologies.

[0222] Dielectric loss tangent For the test piece 3 obtained in the measurement of the relative dielectric constant, the dielectric loss tangent of the test piece 3 at 1 GHz was measured by the cavity resonance method using the above-mentioned "Network Analyzer E8362C." [Industrial Applicability]

[0223] According to the present invention, it is possible to provide a resin capable of forming a cured product having high alkali developability, high heat resistance, low elastic modulus, low dielectric constant and low dielectric tangent.

Claims

1. A resin having an acid group and a polymerizable unsaturated group, The resin having an acid group and a polymerizable unsaturated group is A phenolic hydroxyl group-containing resin; a (meth)acrylate compound having an epoxy group; A polybasic acid anhydride, is the reaction product of The phenolic hydroxyl group-containing resin is A fluorene compound, wherein the fluorene compound does not have a substituent at the 9-position; A phenolic hydroxyl group-containing compound, A compound represented by general formula (1), 【Chemistry 1】 is the reaction product of In general formula (1), Ar represents an aromatic ring group which may have a substituent. R 1 are each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group, and is a resin having an acid group and a polymerizable unsaturated group.

2. The resin having an acid group and a polymerizable unsaturated group according to claim 1, wherein a ratio (Mf / M1) of the moles (Mf) of the fluorene compound to the moles (M1) of the compound represented by the general formula (1) is 0.01 to 0.

99.

3. The phenolic hydroxyl group-containing resin is represented by general formula (5), 【Chemistry 2】 In general formula (5), Each Ar is independently as defined in general formula (1), p is an average value, which is a number greater than 0 and less than or equal to 10; R 1 is as defined in general formula (1), Each Z is independently a structural unit represented by general formula (2A) or general formula (3A), 【Chemistry 3】 In general formula (2A), R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer from 0 to 4, * is a bond to general formula (5), In general formula (3A), R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is an integer from 0 to 3, * is a bond to general formula (5), Each Z' is independently a structural unit represented by general formula (2A') or general formula (3A'), 【Chemistry 4】 In general formula (2A'), R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer from 0 to 4; * is a bond to general formula (5), In general formula (3A'), R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, n′ is an integer from 0 to 4, * is a bond to general formula (5), The resin having an acid group and a polymerizable unsaturated group according to claim 1, wherein the phenolic hydroxyl group-containing resin comprises at least one structural unit selected from the group consisting of general formula (2A) and general formula (2A'), and at least one structural unit selected from the group consisting of general formula (3A) and general formula (3A').

4. The phenolic hydroxyl group-containing resin contains at least one compound represented by general formula (5-1), 【Chemistry 5】 In general formula (5-1), Ar and R 1 is as defined in general formula (1), Z is as defined in general formula (5), R 3’ and n′ are as defined in general formula (3A′), The resin having an acid group and a polymerizable unsaturated group according to claim 3 , wherein p is 1 or 2.

5. 2. The resin having an acid group and a polymerizable unsaturated group according to claim 1, wherein the phenolic hydroxyl group-containing resin has a hydroxyl group equivalent of 100 to 2000 g / equivalent.

6. 2. The resin having an acid group and a polymerizable unsaturated group according to claim 1, wherein the number average molecular weight of the resin containing several phenolic hydroxyl groups is 100 to 10,000.

7. Ar is Ar 1 -Y-Ar 1 and Ar 1 each independently represents an aromatic ring group which may have a substituent, Y is a single bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, -P(=O)R a - group, an oxygen atom, a sulfur atom or a sulfonyl group, R a The resin having an acid group and a polymerizable unsaturated group according to claim 1 , wherein: is an aromatic ring group.

8. A resin having an acid group and a polymerizable unsaturated group according to claim 1; A photopolymerization initiator; A curable resin composition comprising:

9. The curable resin composition according to claim 8 , further comprising a resin having an acid group and a polymerizable unsaturated group other than the resin having an acid group and a polymerizable unsaturated group.

10. A resin material for a solder resist, comprising the curable resin composition according to claim 8.

11. A cured product of the curable resin composition according to claim 8.

12. An insulating material comprising the cured product according to claim 11.

13. A resist member comprising the cured product according to claim 11.

Citation Information

Patent Citations

  • Resin having acid radical and polymerizable unsaturated group, curable resin composition, cured product, insulating material and resist member

    JP2023028337A