Method for manufacturing molded object
The method for manufacturing shaped articles with reinforcing bars using a mortar material with controlled water content and additives addresses the issue of material deterioration, ensuring long-term stability and integrity of the concrete structure.
Patent Information
- Application Number
- JP2024074258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for additive manufacturing with hydraulic materials fail to stabilize shaped objects containing reinforcing bars over time due to material selection issues that lead to deterioration of internal reinforcing elements.
A manufacturing method for shaped articles using a mortar material with a specific water content range (27 to 34 parts by mass when the binder content is 100 parts by mass) and a composition including binders, fine aggregates, and additives to form a dense structure that protects reinforcing bars from external factors.
The method effectively suppresses the deterioration of reinforcing bars within the shaped objects by limiting water content and using specific additives, ensuring long-term stability and integrity of the concrete structure.
Smart Images

Figure 2024160700000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a shaped object. [Background technology]
[0002] In recent years, a method of modeling using hydraulic materials such as cement and gypsum and an additive manufacturing device has been proposed. For example, Patent Document 1 discloses an additive manufacturing method capable of stably manufacturing objects having delicate and diverse designs even when the hydration of a cementitious kneaded material progresses and the fluidity of the kneaded material decreases. Patent Document 2 discloses a hydraulic composition for additive manufacturing that has excellent extrudability and lamination properties and high interlayer adhesion strength after curing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-122539 A [Patent Document 2] JP 2020-105023 A Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, when actually creating a model, there are cases where reinforcing bars, etc. are included inside the model. In such cases, if the material used for additive manufacturing is not appropriately selected, the reinforcing bars, etc. inside may deteriorate. In addition, there are a wide range of other needs for stabilizing the model for a long period of time.
[0005] In view of the above circumstances, the present invention provides an effective manufacturing method for obtaining a shaped object containing reinforcing bars. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided a method for manufacturing a shaped object containing reinforcing bars therein. The method includes the steps of preparing a mortar material for additive manufacturing containing a binder (A), a fine aggregate (B), and water, molding the mortar material for additive manufacturing by additive manufacturing, and hardening the molded mortar material for additive manufacturing. The content of water in the mortar material for additive manufacturing is in the range of 27 to 34 parts by mass when the content of the binder (A) is 100 parts by mass.
[0007] According to the above aspect, a manufacturing method and the like that is effective for obtaining a shaped object including a reinforcing bar is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described. Note that the various features shown in the following embodiments can be combined with each other. Also, as long as there is no technical contradiction, for example, the features shown as the first embodiment may be combined with the second or third embodiment. Also, in this specification, "~" means "above" through "below" unless otherwise specified.
[0009] <<First embodiment>> That is, the method for producing a shaped object according to the first embodiment is as follows. A method for manufacturing a structure containing a reinforcing bar therein, comprising the steps of: Preparing a mortar material for additive manufacturing, comprising a binder (A), a fine aggregate (B), and water; shaping the additive manufacturing mortar material by additive manufacturing; hardening the shaped additive manufacturing mortar material; Equipped with A method for manufacturing a shaped object, wherein the content of the water in the mortar material for additive manufacturing is in the range of 27 to 34 parts by mass when the content of the binder (A) is 100 parts by mass.
[0010] [Manufacturing method for objects] The manufacturing method of the shaped object of this embodiment uses a mortar material for additive manufacturing. In this specification, additive manufacturing (or additive manufacturing method) refers to a processing method for shaping while layering materials. That is, the manufacturing method of this embodiment has a feature that a desired shaped object is obtained by shaping using a predetermined mortar material for additive manufacturing (sometimes simply referred to as "mortar material") and hardening the shaped object.
[0011] Such modeling can be performed using an additive manufacturing device (3D printer). The additive manufacturing device is a type of industrial robot that uses 3D data created by a computer as a design drawing and stacks cross-sectional shapes to create a three-dimensional object. The additive manufacturing device may be a commercially available product or a known device. More specifically, the above-mentioned modeling can be performed by filling a tank provided in the additive manufacturing device with mortar material and extruding the mortar material from a nozzle provided in the additive manufacturing device. The use of the model obtained here may be set appropriately, but one example is a construction.
[0012] The manufacturing method of the present embodiment also includes a step of hardening the shaped mortar material. In other words, the shaped object obtained by the manufacturing method of the present embodiment has a hardened product of the mortar material for additive manufacturing. The curing conditions used in this production method are arbitrary, that is, the temperature conditions, humidity conditions, etc. can be set arbitrarily.
[0013] The object obtained by the manufacturing method of this embodiment contains reinforcing bars inside. From another perspective, the mortar material for additive manufacturing of this embodiment is used in a process for forming at least a part of an object containing reinforcing bars by additive manufacturing. Conventional materials tend to cause the reinforcing bars in the object to deteriorate over time, but the manufacturing method of this embodiment reduces such a risk.
[0014] Specifically, the amount of water contained in the mortar material for additive manufacturing of this embodiment is limited to a predetermined range, and as a result, the mortar material for additive manufacturing forms a dense structure when hardened, and this prevents water and chlorine components present outside the resulting model from acting on the reinforcing steel bars inside the model (providing a deterioration suppression effect).
[0015] In one embodiment, the shaped object obtained by the manufacturing method of the present embodiment has a portion where the reinforcing bar and the hardened product of the additive manufacturing mortar material are in contact with each other. In such an embodiment, the deterioration suppression effect described above is significantly exhibited.
[0016] On the other hand, the shaped object may have no portions where the reinforcing bar and the hardened product of the additive manufacturing mortar material are in contact with each other. Typically, the shaped object may be produced by the manufacturing method of this embodiment in which a formwork (residual formwork) is formed by the additive manufacturing mortar material and a reinforced concrete structure is formed inside the formwork.
[0017] That is, in the manufacturing method of this embodiment, in the process of forming the mortar material for additive manufacturing described above, a formwork into which concrete is poured may be formed using the mortar material for additive manufacturing. Then, a reinforced concrete structure may be formed in the formwork by pouring concrete onto the reinforcing bars present in the hardened formwork. Even in such a case, deterioration of the reinforced concrete structure inside the formwork can be suppressed.
[0018] Let us return to the characteristics of the mortar material used in this embodiment. The additive manufacturing mortar material of this embodiment contains at least a binder (A), a fine aggregate (B), and water, and the content of water is set to a predetermined range with respect to the content of the binder (A). Specifically, the content of water in the additive manufacturing mortar material is in the range of 27 to 34 parts by mass, more preferably in the range of 28 to 33.5 parts by mass, and even more preferably in the range of 29 to 33 parts by mass, when the content of the binder (A) is 100 parts by mass. By setting the content of water in such a range, the above-mentioned deterioration suppression effect can be significantly exhibited while maintaining the fluidity as a mortar material.
[0019] Although not necessarily limited thereto, the mortar material of this embodiment is typically obtained by mixing a powder composition (premix) containing a binder (A) and a fine aggregate (B) with water. That is, the above-mentioned process of preparing the mortar material for additive manufacturing may be a process of obtaining a mortar material for additive manufacturing by mixing a powder composition containing a binder (A) and a fine aggregate (B) with water. The mortar material may be obtained by adding various components such as the binder (A) and the fine aggregate (B) to a predetermined amount of water. The mixing method may be appropriately selected depending on the scale, etc.
[0020] Next, various components that may constitute the mortar material and powder composition of this embodiment, and characteristics of the materials will be described.
[0021] [Binding material (A)] The mortar material and the powder composition of the present embodiment contain a binder (A). Here, the binder (A) is a general term for inorganic materials that contribute to the development of strength in mortar or concrete.
[0022] Here, the binder (A) may contain a cement component (A1). The cement component (A1) may contain a component selected from the group consisting of ordinary Portland cement, moderate-heat Portland cement, low-heat Portland cement, high-early-strength Portland cement, sulfate-resistant Portland cement, blast-furnace cement, and fly ash cement.
[0023] In addition, the binder (A) may contain an admixture (A2). The admixture (A2) may contain a component selected from the group consisting of fly ash, blast furnace slag (fine) powder, limestone (fine) powder, stone powder, silica fume, expansive material (lime composite expansive material), and sewage sludge incineration ash. These admixtures (A2) are typically mixed in combination with the above-mentioned cement component (A1), but the binder (A) may be composed of only these admixtures (A2).
[0024] The binder (A) may be used alone or in combination of two or more. When using two or more types in combination, binders having different particle sizes may be mixed.
[0025] When using a powder composition, the content of the binder (A) in the entire powder composition can be appropriately set, but when the mass of the entire powder composition is 100 parts by mass, the content of the binder (A) is preferably 20 to 80 parts by mass, more preferably 25 to 75 parts by mass, and most preferably 30 to 70 parts by mass. By setting it in such a range, it becomes easier to balance the hardening property of the obtained mortar material and the strength of the obtained hardened product. In addition, for the mortar material for additive manufacturing, it is preferable that the content of the binder (A) satisfies the above range when the total mass excluding water is 100 parts by mass.
[0026] The mortar material and powder composition of the present embodiment preferably contain slag powder and / or limestone powder as the binder (A). By including such components in the binder (A), chloride ions are easily fixed in the slag powder or limestone powder, and as a result, the deterioration suppression effect described above is easily exhibited. In addition, when slag powder and / or limestone powder are contained as the binder (A), the blending amount (total) of the slag powder and / or limestone powder is preferably 40 mass% or more, more preferably 50 mass% or more, and most preferably 60 mass% or more, based on the entire binder (A). By setting such a blending amount, the fixation of the above-mentioned chloride ions is more likely to proceed. On the other hand, the upper limit of the content of the slag powder in the mortar material or powder composition can be appropriately set according to other blending agents, etc. That is, the entire binder (A) may be slag powder, or the content of the slag powder may be set to 95 mass parts or less, 90 mass parts or less, 80 mass parts or less, 75 mass parts or less, 70 mass parts or less, or 65 mass parts or less, based on 100 mass parts of the entire binder (A). The slag powder that can be used in the mortar material and powder composition of this embodiment can be appropriately selected from various materials, but typically, blast furnace slag powder or the like can be used. On the other hand, when limestone powder is contained as the binder (A), the blending amount of this limestone powder is preferably in the range of 3 to 30 mass% of the whole binder (A), more preferably in the range of 5 to 20 mass%, and particularly preferably in the range of 7 to 10 mass%. By setting it in such a range, it is possible to easily achieve both the ease of handling when the mortar material is produced and the assurance of the physical properties of the hardened product obtained by hardening, while keeping the material cost low. When the binder (A) contains slag powder or limestone powder as described above, the remainder of the binder (A) can be composed of the cement component (A1).
[0027] From another point of view, the mortar material and powder composition of the present embodiment preferably contain moderate heat Portland cement and / or low heat Portland cement. By including such a component in the binder (A), it becomes easier to control the heat generated when the mortar material is cured, and it becomes easier to produce a dense cured product. As a result, it becomes easier to exhibit the deterioration suppression effect described above. The amount of the moderate heat Portland cement and / or low heat Portland cement is preferably 40 mass% or more, more preferably 50 mass% or more, and most preferably 60 mass% or more, based on the total amount of the binder (A). On the other hand, the upper limit of the amount of the moderate heat Portland cement and / or low heat Portland cement in the mortar material and powder composition is not particularly limited. That is, all of the binder (A) may be moderate-heat Portland cement and / or low-heat Portland cement, or the content of moderate-heat Portland cement and / or low-heat Portland cement may be set to 95 parts by mass or less, 90 parts by mass or less, or 80 parts by mass or less per 100 parts by mass of the total binder (A).
[0028] From another point of view, the mortar material or powder composition of the present embodiment preferably contains fly ash. By including such a component in the binder (A), it becomes easier to control the heat generated when the mortar material is cured, and it becomes easier to produce a dense cured product. As a result, it becomes easier to exhibit the above-mentioned deterioration suppression effect. The amount of the fly ash is preferably in the range of 3 to 30 mass% of the entire binder (A), more preferably in the range of 5 to 20 mass%, and particularly preferably in the range of 7 to 10 mass%. By setting it in such a range, it is possible to make it easier to achieve both the ease of handling when the mortar material is produced and the physical properties of the cured product obtained by curing while keeping the material cost low.
[0029] From another point of view, it is preferable that the mortar material or powder composition of this embodiment contains silica fume. By including such a component in the binder (A), it becomes easier to control the heat generated when the mortar material is cured, and it becomes easier to produce a dense cured product. As a result, it becomes easier to exhibit the above-mentioned deterioration suppression effect. The amount of silica fume to be mixed is preferably in the range of 5 to 20 mass% of the entire binder (A), more preferably in the range of 7 to 18 mass%, and particularly preferably in the range of 9 to 15 mass%. By setting it in such a range, it becomes easier to produce a mortar material with a viscosity that is easily applicable to additive manufacturing processes.
[0030] In addition, the mortar material or powder composition of this embodiment may contain ordinary Portland cement as the binder (A). By appropriately adding this ordinary Portland cement, it is possible to ensure an appropriate setting speed while contributing to improving the strength of the resulting shaped object, and to improve the balance between stackability and pumpability. The amount of this ordinary Portland cement is preferably 40 to 90 parts by mass, more preferably 50 to 85 parts by mass, and most preferably 60 to 75 parts by mass, when the total mass of the binder (A) is 100 parts by mass.
[0031] [Fine aggregate (B)] The mortar material and the powder composition of the present embodiment contain fine aggregate (B). In the present embodiment, the fine aggregate (B) refers to aggregate that passes entirely through a 10 mm mesh sieve and 85% or more by mass through a 5 mm mesh sieve (JIS A 0203:2014).
[0032] The type of fine aggregate (B) may be appropriately set depending on the application and the like. As an example, the fine aggregate (B) may contain one or more components selected from the group consisting of sand, mountain sand, land sand, sea sand, silica sand, crushed sand, and slag fine aggregate. The mortar material and powder composition of the present embodiment may contain a carbon fixing material and / or a waste concrete material as the fine aggregate (B). The mortar material and powder composition of the present embodiment may contain waste tile fine aggregate as the fine aggregate (B). These fine aggregates (B) may be used alone or in combination of two or more types. When using two or more types in combination, fine aggregates with different particle sizes may be mixed.
[0033] When using a powder composition, the content of the fine aggregate (B) in the entire powder composition can be appropriately set, but when the mass of the entire powder composition is 100 parts by mass, the content of the fine aggregate (B) is preferably 20 to 80 parts by mass, more preferably 25 to 75 parts by mass, and most preferably 30 to 70 parts by mass. By setting it in such a range, it becomes easier to achieve both hardening property and strength of the obtained hardened product. In addition, for the mortar material for additive manufacturing, when the total mass excluding water is 100 parts by mass, the content of the fine aggregate (B) preferably satisfies the above range.
[0034] [Admixture that imparts thixotropy (C)] The mortar material or powder composition of this embodiment may contain an admixture (C) that imparts thixotropy. This admixture (C) can contribute to improving the thixotropy of the resulting mortar material. That is, as described above, the mortar material is used in additive manufacturing, and is typically subjected to an extrusion process during the manufacturing process. Here, if the mortar material has thixotropy, the extrudability is improved and the shape after extrusion is easily stabilized. The admixture (C) here refers to any agent that does not fall under the above-mentioned binder (A) and fine aggregate (B) and contributes to improving the thixotropy of the resulting mortar material.
[0035] The admixture (C) may be appropriately selected from known materials capable of imparting the above-mentioned properties. As an example, the admixture (C) that imparts thixotropy may contain one or more components selected from the group consisting of cellulose, modified cellulose, minerals, nanofibers, urethane, xanthan gum, diutan gum, starch ether, guar gum, polyacrylamide, carrageenan gum, agar, protein, and latex.
[0036] Examples of modified cellulose that can be used as the admixture (C) of this embodiment include carboxymethyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose. Although cellulose and the modified cellulose described above are usually in a fibrous form, they are treated as the admixture (C) in this specification because they have a high effect of imparting thixotropy.
[0037] Examples of minerals that can be used as the admixture (C) in this embodiment include clay minerals such as attapulgite, bentonite, montmorillonite, kaolin, and sepiolite.
[0038] Examples of nanofibers that can be used as the admixture (C) of this embodiment include carbon nanofibers, cellulose nanofibers, etc. Although these nanofibers are usually in a fibrous form, they are treated as the admixture (C) in this specification because they have a high effect of imparting thixotropy.
[0039] Examples of synthetic fibers that can be used as the admixture (C) in this embodiment include polyolefin compounds such as polypropylene and polyethylene, polyvinyl alcohol, and polyvinyl acetate.
[0040] Examples of urethane usable as the admixture (C) of this embodiment include various urethane-based thickeners used as urethane-based associative thickeners. Examples of the urethane-based associative thickeners include "Thixostar" manufactured by Japan Materials Technology Co., Ltd., "Adekanol" series manufactured by ADEKA Corporation, and "SN Thickener" series manufactured by San Nopco Ltd.
[0041] Proteins that can be used as the admixture (C) of this embodiment include amino acid condensates having a predetermined molecular weight.
[0042] Examples of the latex that can be used as the admixture (C) in this embodiment include chloroprene rubber latex and acrylic latex.
[0043] When using a powder composition, the content of the admixture (C) in the entire powder composition can be appropriately set, but the content of the admixture (C) is preferably in the range of 0.02 to 0.14 parts by mass, more preferably in the range of 0.04 to 0.12 parts by mass, and most preferably in the range of 0.06 to 0.10 parts by mass, relative to 100 parts by mass of the entire powder composition. By setting it in such a range, it becomes easier to improve the strength of the obtained hardened product while maintaining the handleability of the obtained mortar material. In addition, for the mortar material for additive manufacturing, it is preferable that the content of the admixture (C) satisfies the above range when the total mass excluding water is 100 parts by mass.
[0044] From another point of view, the mortar material and powder composition of the present embodiment preferably contain cellulose and / or modified cellulose among the above-mentioned admixtures (C). By including such a component, not only does it contribute to improving the thixotropy of the mortar material, but it also provides an effect of making it easier to control the amount of water in the system when the mortar material is hardened. As a result, the deterioration suppression effect described above is more easily exhibited. In addition, when a powder composition is used, the blending amount of this cellulose and / or modified cellulose is preferably in the range of 0.02 to 0.20 parts by mass, more preferably in the range of 0.04 to 0.18 parts by mass, and most preferably in the range of 0.06 to 0.16 parts by mass, relative to 100 parts by mass of the entire powder composition. By setting it in such a range, the above-mentioned effect can be more easily exhibited. In addition, with respect to the mortar material for additive manufacturing, it is preferable that the content of cellulose and / or modified cellulose satisfies the above range when the total mass excluding water is 100 parts by mass.
[0045] Fiber In addition, the mortar material or powder composition of the present embodiment may contain a fiber material (D). By appropriately adding this fiber material (D), it is possible to contribute to improving the strength of the obtained shaped object, and to achieve a balance between lamination property and pumpability. Note that the fiber material (D) in this specification does not correspond to the components listed as the thickener (C).
[0046] The type of the fiber material (D) can be appropriately set. As an example, the fiber material (D) may include at least one fiber material selected from the group consisting of metal fiber, carbon fiber, aramid fiber, PP (polypropylene) fiber, PVA (polyvinyl acetate) fiber, PE (polyethylene) fiber, glass fiber, nylon fiber, and PBO (polybenzoxazole) fiber.
[0047] In addition, the fiber material (D) may include a fiber material of natural origin. Examples of such a fiber material of natural origin include fiber materials derived from plants and fiber materials derived from animals. Here, the "plant" in the fiber material derived from plants includes bamboo grass, bamboo, hemp, rice, wheat, etc., which can provide fiber materials industrially. Also, the "animal" in the fiber material derived from animals typically includes sheep, etc.
[0048] The fiber length (average fiber length) of the fibrous material (D) is preferably 1 to 30 mm, more preferably 3 to 25 mm, and most preferably 5 to 20 mm. The amount of the fibrous material (D) is preferably 0.05 to 5 parts by volume, more preferably 0.08 to 3 parts by volume, and most preferably 0.1 to 1.5 parts by volume, when the total volume of the binder (A) and the fine aggregate (B) is taken as 100 parts by volume.
[0049] [Other ingredients] In addition, the powder composition of this embodiment may contain other components other than the above-mentioned components (A) to (D) in order to impart desired properties. Examples of other components include rheology modifiers (including water reducing agents, dispersants, fluidizing agents, etc.), antifoaming agents, setting retarders, gas foaming substances, setting regulators, air-enhancing agents, rust inhibitors, water repellents, antibacterial agents, colorants, antifreeze agents, anion exchangers such as hydrotalcite, and moisturizing agents such as urea. The amounts of these components to be blended are arbitrary.
[0050] In addition, the mortar material and the powder composition of this embodiment preferably contain a rheology modifier. By appropriately containing this rheology modifier, it is possible to achieve a balance between lamination property and pumpability. In one embodiment, the rheology modifier may be a polycarboxylic acid-based rheology modifier or a melamine-based rheology modifier. The amount of these rheology modifiers is preferably 0.01 to 3 parts by mass, more preferably 0.03 to 1 part by mass, and most preferably 0.05 to 0.5 parts by mass, when the total mass of the binder (A) and the fine aggregate (B) is 100 parts by mass. In addition, this rheology modifier may also be called a "water reducing agent", a "dispersant", or a "fluidizing agent".
[0051] From another point of view, it is preferable that the mortar material and powder composition of the present embodiment contain a water reducing agent and / or a fluidizing agent. By including such a water reducing agent or fluidizing agent, the amount of water used when generating the mortar material can be reduced while maintaining fluidity. This makes it easier to obtain a dense hardened material, and as a result, the deterioration suppression effect described above is more likely to be exhibited. As the water reducing agent or fluidizing agent, a component called a high-performance water reducing agent or a high-performance AE agent can be used. As commercially available water reducing agents, the powder-type high-performance water reducing agent "Coreflow" series manufactured by Pacific Materials Co., Ltd. and the high-performance water reducing agent "Master Grenium" series manufactured by Pozzolith Solutions Co., Ltd. can be used. The water-reducing agent and / or the fluidizing agent are usually used together with the cement component (A1). The amount (total) of the water-reducing agent and / or the fluidizing agent can be appropriately set depending on the application, etc., but is preferably 0.4 to 2.0 parts by mass, more preferably 0.7 to 1.8 parts by mass, and most preferably 1.0 to 1.5 parts by mass, relative to 100 parts by mass of the total cement component (A1).
[0052] In one embodiment, the mortar material or powder composition preferably contains a water-absorbing material in addition to the binder (A). By including the water-absorbing material in this way, the mortar material is more likely to retain water in the system. This allows the hardening speed to be appropriately controlled, making it easier to obtain a dense hardened material. The amount of water that the water-absorbing material can absorb is appropriately set depending on the other components, but typically, the following materials are used as the water-absorbing material.
[0053] That is, in the mortar material or powder composition of this embodiment, it is preferable that at least a part of the fine aggregate (B) contains waste tile fine aggregate as a water absorbing material. Such waste tile fine aggregate has a suitable amount of voids and therefore is easy to hold (absorb) water. Therefore, by including such waste tile fine aggregate in the mortar material, the mortar material is easy to hold water in the system. This makes it easier to obtain a dense hardened material, and as a result, it is easier to exert the deterioration suppression effect described above. The content of this waste tile fine aggregate can be appropriately selected, and may be 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 30 parts by mass or more, or 50 parts by mass or more, when the entire fine aggregate (B) is taken as 100 parts by mass. On the other hand, the entire fine aggregate (B) may be waste tile fine aggregate. Furthermore, the content of the waste tile fine aggregate may be 90 parts by mass or less, or 80 parts by mass or less, when the entire fine aggregate (B) is taken as 100 parts by mass.
[0054] In addition, the mortar material and powder composition of this embodiment preferably contain a water-absorbing polymer. By including such a water-absorbing polymer, the mortar material is more likely to retain water in the system. This makes it easier to obtain a dense hardened material, and as a result, the deterioration suppression effect described above is more likely to be exhibited. As the water-absorbing polymer, components such as polymethacrylate and polyacrylate can be used. As a commercially available water-absorbing polymer, the salt-resistant water-absorbing resin "Aqualic CS" series manufactured by Nippon Shokubai Co., Ltd. can be used. This water-absorbing polymer is usually used together with the cement component (A1). The amount of the water-absorbing polymer can be appropriately set depending on the application, etc., but is preferably 0.05 to 0.6 parts by mass, more preferably 0.1 to 0.5 parts by mass, and most preferably 0.2 to 0.4 parts by mass, relative to 100 parts by mass of the total cement component (A1).
[0055] In addition, the mortar material and powder composition of this embodiment preferably contain a water-absorbent fiber material. By including such a fiber material, the mortar material is more likely to retain water in the system. This makes it easier to obtain a dense hardened material, and as a result, the aforementioned deterioration suppression effect is more likely to be exhibited. The fiber material is appropriately selected from the aforementioned fiber materials (D), and is preferably a fiber material derived from a plant selected from the group consisting of bamboo grass, bamboo, hemp, rice, and wheat. This water-absorbent fibrous material is usually used together with the cement component (A1). The amount of the water-absorbent fibrous material can be appropriately set depending on the application, etc., but is preferably 0.05 to 0.6 parts by mass, more preferably 0.1 to 0.5 parts by mass, and most preferably 0.2 to 0.4 parts by mass, relative to 100 parts by mass of the total cement component (A1).
[0056] From another viewpoint, it is preferable to devise a shape of the fine aggregate (B) in order to improve the fluidity even under the condition of a limited water content of the mortar material.
[0057] Typically, the fine aggregate (B) contained in the mortar material or powder composition preferably has an average particle size of 1 mm or less, more preferably 0.8 mm or less, and even more preferably 0.6 mm or less. By setting the average particle size in such a range, it is possible to contribute to improving the fluidity of the mortar material. The lower limit of the average particle size is not particularly limited, but an example is 0.1 mm or more. The average particle size of the fine aggregate (B) can be defined as a value calculated from the opening of each sieve and the mass fraction of the aggregate remaining therein by measuring the mass fraction of the aggregate remaining in each sieve by a sieving test described in JIS A 1102:2014 "Sieving test method for aggregate".
[0058] The gradation index of the fine aggregate (B) contained in the mortar material or powder composition is preferably 20 or more, more preferably 30 or more, and even more preferably 45 or more. Setting the gradation index in this range contributes to improving the fluidity of the mortar material. The upper limit of the gradation index is not particularly limited, but an example is 200 or less. The gradation index of the fine aggregate (B) means the index specified in JIS Z 2601:1993 "Testing method for casting sand".
[0059] [Method of producing powder composition] The powder composition of the present embodiment can be produced by mixing the various raw materials described above. The mixing method may be appropriately selected from among known methods, and is not particularly limited. The powder composition obtained here preferably satisfies the following physical properties (physical properties (1) and (2)).
[0060] [Physical properties of powder compositions (1)] The powder composition of the present embodiment preferably satisfies the predetermined characteristics when a sample is prepared by adding water. Specifically, the powder composition of the present embodiment is preferably cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition, and a predetermined measurement value is given when a predetermined test specimen is obtained. In addition, the conditions for preparing and storing the test specimens and carrying out the tests in the following various tests are set in accordance with each standard, but unless there is a particular restriction in the standard, the tests are carried out in an environment of 20°C. The above-mentioned preparation conditions, storage conditions, and test conditions of the specimen are set in order to discuss the physical properties in this section. On the other hand, when applying the powder composition of this embodiment to an additive manufacturing process, various conditions not limited to the above conditions can be adopted.
[0061] Here, the amount of water added when discussing the physical properties of the powder composition in this specification is set based on 14.5 parts by mass relative to 100 parts by mass of the powder composition. In this specification, the tolerance for the amount of water added as this standard is set to ±1.5 parts by mass, but this tolerance may be discussed with a different value depending on the scale of the prepared sample, etc. That is, in this specification, the above-mentioned tolerance may be discussed as ±1.0 parts by mass, ±0.8 parts by mass, ±0.5 parts by mass, ±0.3 parts by mass, or ±0.1 parts by mass.
[0062] The measured values in each test shown below can be achieved by appropriately selecting a combination of types of binder (A), fine aggregate (B), etc.
[0063] That is, the powder composition of this embodiment is obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and hardening it to obtain a test specimen conforming to the standard JSCE-G 571. When the apparent diffusion coefficient of chloride ions was measured in accordance with the same standard, the apparent diffusion coefficient of chloride ions was 0.5 cm 2It is preferable that the apparent diffusion coefficient of chloride ions in this test is set to such a value, and when a molded object is made from the mortar material, the life of the molded object is easily improved. Note that the apparent diffusion coefficient of chloride ions in this test is 0.3 cm 2 / year or less is preferable, and 0.25 cm 2 / year or less is more preferable, and 0.2cm 2 It is particularly preferable that the apparent diffusion coefficient of chloride ions is not particularly limited, but an example of the lower limit is 0.05 cm 2 / year or more.
[0064] In addition, the powder composition of this embodiment is hardened by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JIS A 1153. When the carbonation rate coefficient was measured in accordance with the same standard, the carbonation rate coefficient was 0.35 cm / year. (1 / 2) It is preferable that the carbonation rate coefficient in this test is set to such a value, which makes it easier to improve the lifespan of a model made from the mortar material. The carbonation rate coefficient here is 0.30 cm / year. (1 / 2) More preferably, 0.25 cm / year or less. (1 / 2) It is particularly preferable that the carbonation rate coefficient is equal to or less than 0.10 cm / year. The lower limit of the carbonation rate coefficient is not particularly limited, but an example is 0.10 cm / year. (1 / 2) That's all.
[0065] In addition, the powder composition of this embodiment is preferably prepared by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the composition to obtain a test specimen conforming to the standard JIS A 1148 (A method), and when the relative dynamic modulus of elasticity is measured in accordance with the standard, the relative dynamic modulus of elasticity is preferably 90% or more. By setting the relative dynamic modulus of elasticity in this test to such a value, when a molded object is produced from the mortar material, the life of the molded object is easily improved. Here, the relative dynamic modulus of elasticity is more preferably 92% or more, and particularly preferably 95% or more. In addition, the upper limit of the relative dynamic modulus of elasticity is not particularly limited, but as an example, it is 105% or less.
[0066] In addition, the powder composition of this embodiment is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JSCE-G 582. When the moisture penetration rate coefficient was measured in accordance with the same standard, the moisture penetration rate coefficient was 0.8 mm / hour. (1 / 2) It is preferable that the moisture penetration rate coefficient in this test is set to such a value, and when a model is made from the mortar material, the life of the model is easily improved. The moisture penetration rate coefficient here is 0.7 mm / hour. (1 / 2) More preferably, it is 0.6 mm / hour or less. (1 / 2) The lower limit of the moisture permeation rate coefficient is not particularly limited, but an example is 0.35 mm / hour. (1 / 2) That's all.
[0067] In addition, the powder composition of this embodiment is preferably prepared by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the powder composition to obtain a test specimen conforming to the standard JSCE-K 571, and measuring the water permeability for 60 minutes according to the water permeability test (3) of the same standard, so that the water permeability is preferably 2.5 mL or less. By setting the water permeability in this test to such a value, when a molded object is produced from the mortar material, the life of the molded object is easily improved. The water permeability here is more preferably 2.0 mL or less, and particularly preferably 1.5 mL or less. In addition, the lower limit of the water permeability in this test is not particularly limited, but as an example, it is 0.5 mL or more.
[0068] In addition, the powder composition of the present embodiment is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard NDIS 3436. When the surface layer air permeability coefficient was measured in accordance with the same standard, the surface layer air permeability coefficient was 0.1×10 -16 m 2 By setting the surface layer air permeability coefficient in this test to such a value, it is easy to improve the life of a model made from the mortar material. -16 m 2 More preferably, it is 0.05×10 or less. -16 m 2 The lower limit of the surface layer air permeability coefficient is not particularly limited, but an example is 0.001×10 -16 m 2 That's all.
[0069] [Physical properties of powder composition (2)] The powder composition of this embodiment preferably satisfies a predetermined characteristic when a sample is prepared by adding water. Specifically, the powder composition of this embodiment preferably gives a predetermined measured value when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B), and the sample is subjected to various tests 1 to 3 described below. In the following various tests, the sample is prepared, stored, and the test is performed in an environment of 20°C. In addition, in this specification, powders that cannot be tested are treated as not having measured values in the first place. The above sample preparation conditions, storage conditions, and test conditions are set in order to discuss the physical properties in this section. However, when applying the powder composition of this embodiment to an additive manufacturing process, various conditions not limited to the above conditions can be used.
[0070] (Test 1; Slump test) That is, in the powder composition of this embodiment, when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the binder (A) and the fine aggregate (B) in total, and a slump test is performed on the sample at 20°C in accordance with JIS A 1171, T1(5) is 2 cm or less. Here, T1(5) is the slump value of the slump test performed on the sample 5 minutes after preparation.
[0071] By setting T1(5) to a predetermined value or less in this way, it is possible to improve the lamination property when the mortar material obtained from the powder composition is subjected to an additive manufacturing process. It is more preferable that T1(5) is 1.5 cm or less, and most preferably 1.0 cm or less. The lower limit of T1(5) is not particularly limited, but an example is 0.1 cm or more.
[0072] Furthermore, the powder composition of this embodiment preferably has a difference between the above-mentioned T1(5) and T1(30) in the range of 0.1 to 1.8 cm. Note that T1(30) is the slump value of a slump test performed on a sample 30 minutes after preparation, but since T1(5) is usually larger than the value of T1(30), the above-mentioned difference can be obtained as "T1(5)-T1(30)". In this way, by making T1(5)-T1(30) equal to or less than a predetermined value, when a mortar material obtained from the powder composition is subjected to an additive manufacturing process, the lamination property can be improved for a long time. Note that T1(5)-T1(30) is more preferably 0.3 to 1.5 cm, and most preferably 0.5 to 1.2 cm.
[0073] (Test 2; Flow table test) That is, in the powder composition of this embodiment, when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B), and a flow table test is performed on the sample at 20° C. in accordance with JIS-R5201, it is preferable that T2(5;0) is less than 110 mm. Here, T2(5;0) is the flow value at 0 strokes in the flow table test performed on the sample 5 minutes after preparation.
[0074] By setting T2(5;0) to a predetermined value or less in this way, the lamination property can be improved when the mortar material obtained from the powder composition is subjected to an additive manufacturing process. It is more preferable that T2(5;0) is 108 mm or less, and most preferably 105 mm or less. The lower limit of T2(5;0) is not particularly limited, but an example is 100 mm or more.
[0075] In addition, the powder composition of this embodiment preferably has a T2(5;15) of 110 mm or more when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the binder (A) and fine aggregate (B) in total, and a flow table test is performed on the sample at 20° C. in accordance with JIS-R5201. Here, T2(5;15) is the flow value at 15 strokes in the flow table test performed on the sample 5 minutes after preparation.
[0076] By setting T2(5;15) to a predetermined value or more in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the pumpability and fluidity can be improved. T2(5;15) is more preferably 115 mm or more, and most preferably 120 mm or more. The upper limit of T2(5;15) is not particularly limited, but an example is 140 mm or less.
[0077] Furthermore, the powder composition of this embodiment preferably has a difference between the above-mentioned T2(5;15) and T2(5;0) in the range of 5 to 40 mm. Since T2(5;15) is usually larger than the numerical value of T2(5;0), the above-mentioned difference can be obtained as "T2(5;15)-T2(5;0)". By making T2(5;15)-T2(5;0) equal to or less than a predetermined numerical value, the balance of lamination property, pumpability, and fluidity can be improved when the mortar material obtained from the powder composition is subjected to an additive manufacturing process. Furthermore, T2(5;15)-T2(5;0) is more preferably 7 to 30 mm, and most preferably 10 to 20 mm.
[0078] In addition, the powder composition of this embodiment preferably has a T2(30;0) of less than 108 mm when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B) and a flow table test is performed on the sample at 20°C in accordance with JIS-R5201. Here, T2(30;0) is the flow value at 0 strokes in the flow table test performed on the sample 30 minutes after preparation.
[0079] By setting T2(30;0) to a predetermined value or less in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the lamination property can be improved over a long period of time. It is more preferable that T2(30;0) is 106 mm or less, and most preferably 105 mm or less. The lower limit of T2(30;0) is not particularly limited, but an example is 98 mm or more.
[0080] In addition, the powder composition of this embodiment preferably has a T2(30;15) of 108 mm or more when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the binder (A) and fine aggregate (B) in total, and a flow table test is performed on the sample at 20°C in accordance with JIS-R5201. Here, T2(30;15) is the flow value at 15 strokes in the flow table test performed on the sample 5 minutes after preparation.
[0081] By setting T2(30;15) to a predetermined value or more in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the pumpability and fluidity can be improved over a long period of time. It is more preferable that T2(30;15) is 110 mm or more, and most preferably 115 mm or more. The upper limit of T2(30;15) is not particularly limited, but an example is 130 mm or less.
[0082] Furthermore, the powder composition of this embodiment preferably has a difference between the above-mentioned T2(30;15) and T2(30;0) in the range of 5 to 20 mm. Since T2(30;15) is usually larger than the numerical value of T2(30;0), the above-mentioned difference can be obtained as "T2(30;15)-T2(30;0)". By making T2(30;15)-T2(30;0) equal to or less than a predetermined numerical value in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the balance of lamination property, pumpability, and fluidity can be improved for a long period of time. Furthermore, T2(30;15)-T2(30;0) is more preferably 7 to 15 mm, and most preferably 8 to 12 mm.
[0083] (Test 3; Hand vane shear test) Furthermore, the powder composition of this embodiment preferably has a T3(5) of 1.5 to 5 kPa when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the binder (A) and the fine aggregate (B) in total, and the sample is subjected to a hand vane shear test at 20°C in accordance with JGS 1411. Here, T3(5) is the shear yield value of the hand vane shear test performed on the sample 5 minutes after preparation.
[0084] By setting T3(5) in a predetermined range in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the lamination property can be improved and appropriate workability can be ensured. Note that T3(5) is more preferably 1.7 to 4.5 kPa, and most preferably 2.0 to 4.0 kPa.
[0085] Furthermore, the powder composition of this embodiment preferably has a T3(30) of 3.0 to 8.0 kPa when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the binder (A) and the fine aggregate (B) in total, and the sample is subjected to a hand vane shear test at 20°C in accordance with JGS 1411. Here, T3(30) is the shear yield value of the hand vane shear test performed on the sample 30 minutes after preparation.
[0086] By setting T3(30) in a predetermined range in this way, when a mortar material obtained from the powder composition is subjected to an additive manufacturing process, it is possible to improve lamination property over a long period of time, and in addition, it is possible to ensure appropriate workability over a long period of time. Note that T3(30) is more preferably 3.5 to 7.5 kPa, and most preferably 4.0 to 7.0 kPa.
[0087] Furthermore, in the powder composition of this embodiment, the difference between the above-mentioned T3(30) and T3(5) is preferably in the range of 1.5 to 6.5 kPa. Since T3(30) is usually larger than the numerical value of T3(5), the above-mentioned difference can be obtained as "T3(30)-T3(5)". By setting T3(30)-T3(5) to a predetermined numerical range in this way, when the mortar material obtained from the powder composition is subjected to an additive manufacturing process, the lamination property and processability can be improved over a long period of time. Furthermore, T3(30)-T3(5) is more preferably 2.0 to 6.0 kPa, and most preferably 2.5 to 5.0 kPa.
[0088] The measured values in each of the above-mentioned tests can be realized by appropriately selecting the type of admixture (C), appropriately setting the mixing amount of the admixture (C), appropriately selecting the combination of the type of binder (A) or fine aggregate (B) with the admixture (C), etc.
[0089] As described above, according to the manufacturing method of the first embodiment, since an appropriate mortar material is used, deterioration of the reinforcing bars in the object is suppressed.
[0090] Next, a powder composition according to a second embodiment will be described.
[0091] <<Second embodiment>> That is, the powder composition according to the second embodiment is as follows. 1. A powder composition for producing a mortar material for additive manufacturing, comprising: Contains a binder (A) and a fine aggregate (B), A test specimen conforming to the standard JSCE-G 571 was obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the mixture. When the apparent diffusion coefficient of chloride ions was measured in accordance with the same standard, the apparent diffusion coefficient of chloride ions was found to be 0.5 cm 2 / year or less, powder composition.
[0092] [Powder composition] The powder composition of the present embodiment is used to produce a mortar material for additive manufacturing. Here, additive manufacturing is a processing method in which a shape is formed by layering materials. In this embodiment, a desired object can be obtained by layering a mortar material obtained from a powder composition. The details are as shown in the first embodiment.
[0093] The powder composition of this embodiment is typically a premix material for obtaining such a mortar material. That is, the mortar material for additive manufacturing of this embodiment can be said to be obtained by adding water to the powder composition. Here, the amount of water to be added may be appropriately set depending on the composition of the powder composition, the process conditions to be applied, etc., but is preferably 12.0 to 18.0 parts by mass relative to 100 parts by mass of the powder composition. The water to be added here may be appropriately set depending on the application, but may be tap water or ion-exchanged water. The amount of water to be added is more preferably 13.0 to 16.0 parts by mass, and most preferably 14.0 to 15.0 parts by mass relative to 100 parts by mass of the powder composition.
[0094] The additive manufacturing mortar material produced from the powder composition of this embodiment is used for various applications, but typically, the additive manufacturing mortar material is used in a process for forming at least a part of a concrete structure including reinforcing bars by additive manufacturing. As described above, when a predetermined test specimen is obtained and the apparent diffusion coefficient of chloride ions is measured, the measured value of the powder composition of this embodiment is controlled to a low level. In conventional materials, the high value of the apparent diffusion coefficient tends to cause deterioration of reinforcing bars in concrete structures over time, but when the powder composition of this embodiment is used, such a risk is reduced.
[0095] [Mortar materials for additive manufacturing] As described above, the powder composition of the present embodiment is used as a premix material for obtaining a mortar material for additive manufacturing. That is, the powder composition of the present embodiment is converted into a mortar material for additive manufacturing by adding water.
[0096] [Manufacturing method for objects] Next, a method for manufacturing a model according to this embodiment will be described. That is, the manufacturing method of the object of this embodiment includes a step of preparing a mortar material for additive manufacturing, a step of molding the mortar material for additive manufacturing by an additive manufacturing method, and a step of hardening the molded mortar material for additive manufacturing.
[0097] That is, in the second embodiment, the shaped object has a hardened mortar material for additive manufacturing. Such a shaped object can be obtained by preparing the mortar material for additive manufacturing described above, shaping it by additive manufacturing, and then hardening it. The additive manufacturing method used in this manufacturing method can be a known method, and the curing conditions can be arbitrary. In addition, when curing, temperature conditions, humidity conditions, etc. can be set.
[0098] In the second embodiment, a reinforcing bar may typically be included inside the shaped object. Even if a reinforcing bar is included inside the shaped object thus manufactured, deterioration of the reinforcing bar is unlikely to occur when a mortar material obtained from a predetermined powder composition is used.
[0099] Other than that, various components that can constitute the powder composition of the second embodiment, the production method, and physical properties are the same as those shown in the first embodiment.
[0100] As described above, the powder composition of the second embodiment provides a powder composition that is useful for additive manufacturing processes.
[0101] <<Third embodiment>> The mortar material according to the third embodiment is as follows. 1. A mortar material for additive manufacturing, comprising: Contains a binder (A), fine aggregate (B), and water, The additive manufacturing mortar material was hardened to obtain a test specimen conforming to the standard JSCE-G 571, and the apparent diffusion coefficient of the chloride ion was measured in accordance with the same standard. The apparent diffusion coefficient of the chloride ion was found to be 0.5 cm 2 / year or less, additive manufacturing mortar material.
[0102] [Mortar materials for additive manufacturing] That is, the mortar material of the third embodiment contains water in addition to the above-mentioned components (A) and (B), but it does not necessarily have to be manufactured after obtaining a predetermined powder composition, and the constituent materials may be mixed in any order. In other words, it may be a mortar material obtained by mixing various materials in an additive manufacturing device.
[0103] Furthermore, when the mortar material of the third embodiment is hardened to obtain a test specimen conforming to the standard JSCE-G 571 and the apparent diffusion coefficient of chloride ions is measured in accordance with the same standard, the apparent diffusion coefficient of the chloride ions is 0.5 cm 2 / year or less. The additive manufacturing mortar material of this embodiment may be used in a process for forming at least a part of a concrete structure containing reinforcing bars by additive manufacturing. When the additive manufacturing mortar material of this embodiment is applied to a manufacturing process for a shaped object containing reinforcing bars in this way, it is expected that the reinforcing bars will be less likely to deteriorate as in the second embodiment. The value of the apparent diffusion coefficient of chloride ions in this embodiment may be the same as the various measured values for the test specimen shown in the second embodiment.
[0104] In addition, various raw materials that can be used as the mortar material according to the third embodiment, and properties and uses that the mortar material for additive manufacturing may have may be the same as those shown in the first and second embodiments. That is, the mortar material for additive manufacturing according to the third embodiment may be one that, when hardened, gives the same measured values for the various physical properties as those shown in the item [Physical properties of powder composition (1)] of the first embodiment.
[0105] As described above, the mortar material according to the third embodiment provides a mortar material and the like that is useful for additive manufacturing processes.
[0106] Next, a reference embodiment of the present invention will be described.
[0107] [α1] A method for manufacturing a structure containing a reinforcing bar therein, comprising the steps of: Preparing a mortar material for additive manufacturing, comprising a binder (A), a fine aggregate (B), and water; shaping the additive manufacturing mortar material by additive manufacturing; hardening the shaped additive manufacturing mortar material; Equipped with A method for manufacturing a shaped object, wherein the content of the water in the mortar material for additive manufacturing is in the range of 27 to 34 parts by mass when the content of the binder (A) is 100 parts by mass. [α2] The method for producing a shaped object according to [α1], The method for manufacturing a shaped object, wherein the mortar material for additive manufacturing contains a water-absorbing material in addition to the binder (A). [α3] The method for producing a shaped object according to [α2], The mortar material for additive manufacturing comprises, as the water-absorbing material, at least a portion of the fine aggregate (B) made of waste tile fine aggregate. [α4] The method for producing a shaped object according to [α2] or [α3], The method for manufacturing a shaped object, wherein the mortar material for additive manufacturing contains a water-absorbent polymer and / or a water-absorbent fibrous material as the water-absorbent material. [α5] A method for producing a shaped object according to any one of [α1] to [α4], A method for producing a shaped object, wherein the binder (A) contains 40 mass% or more of slag powder and / or limestone powder based on the total amount of the binder (A). [α6] A method for producing a shaped object according to any one of [α1] to [α5], The mortar material for additive manufacturing comprises an admixture (C) that imparts thixotropy, said method for producing a shaped object. [α7] A method for producing a shaped object according to any one of [α1] to [α6], A method for producing a shaped object, wherein the binder (A) contains fly ash. [α8] A method for producing a shaped object according to any one of [α1] to [α7], A method for producing a shaped object, wherein the fine aggregate (B) has an average particle size of 1 mm or less. [α9] A method for producing a shaped object according to any one of [α1] to [α8], The method for producing a shaped object, wherein the fine aggregate (B) has a grain size index of 20 or more. [α10] A method for producing a shaped object according to any one of [α1] to [α9], The method for producing a shaped object, wherein the additive manufacturing mortar material contains a dispersant and / or a superplasticizer. [α11] A method for producing a shaped object according to any one of [α1] to [α10], The method for manufacturing a molded object, wherein the molded object has a portion where the reinforcing bar and a hardened product of the mortar material for additive manufacturing are in contact with each other. [α12] A method for producing a shaped object according to any one of [α1] to [α10], In the step of modeling the additive manufacturing mortar material, a formwork into which concrete is poured is modeled using the additive manufacturing mortar material; The method for manufacturing a shaped object further comprises a step of forming a reinforced concrete structure within the formwork by pouring the concrete into the hardened reinforcing bars present within the formwork. [α13] A method for producing a shaped object according to any one of [α1] to [α12], The method for manufacturing a molded object, wherein the step of preparing the mortar material for additive manufacturing comprises mixing a powder composition containing a binder (A) and a fine aggregate (B) with water to obtain the mortar material for additive manufacturing. [α14] The method for producing a shaped object according to [α13], The powder composition is hardened by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JSCE-G 571. When the apparent diffusion coefficient of chloride ions is measured in accordance with the same standard, the apparent diffusion coefficient of chloride ions is 0.5 cm 2 A method for manufacturing sculptures in less than one year. [α15] The method for producing a shaped object according to [α13] or [α14], The powder composition is hardened by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JIS A 1153. When the carbonation rate coefficient is measured in accordance with the same standard, the carbonation rate coefficient is 0.35 cm / year. (1 / 2)The manufacturing method of the molded object is as follows. [α16] A method for producing a shaped object according to any one of [α13] to [α15], The powder composition is hardened by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to JIS A 1148 (Method A), and when the relative dynamic modulus of elasticity is measured in accordance with the same standard, the relative dynamic modulus of elasticity is 90% or more. [α17] A method for producing a shaped object according to any one of [α13] to [α16], The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JSCE-G 582. When the moisture penetration rate coefficient is measured according to the same standard, the moisture penetration rate coefficient is 0.8 mm / hour. (1 / 2) The manufacturing method of the molded object is as follows. [α18] A method for producing a shaped object according to any one of [α13] to [α17], The powder composition is added with 14.5±1.5 parts by mass of water per 100 parts by mass of the powder composition, and then cured to obtain a test specimen conforming to the JSCE-K 571 standard, and when the water permeability over 60 minutes is measured in accordance with the (3) Water Permeability Test of the same standard, the water permeability is 2.5 mL or less. [α19] A method for producing a shaped object according to any one of [α13] to [α18], The powder composition is hardened by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard NDIS 3436. When the surface layer air permeability coefficient is measured in accordance with the same standard, the surface layer air permeability coefficient is 0.1×10 -16 m 2 The manufacturing method of the molded object is as follows. [α20] A method for producing a shaped object according to any one of [α13] to [α19], The powder composition has a T2(5;0) of less than 110 mm when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B) and a flow table test is performed on the sample at 20°C in accordance with JIS-R5201, Here, T2(5;0) is the flow value at 0 strokes in the flow table test performed on the sample 5 minutes after its production, in accordance with a method for manufacturing a molded object. [α21] A method for producing a shaped object according to any one of [α13] to [α20], The powder composition has a T2(5;15) of 110 mm or more when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B) and a flow table test is performed on the sample at 20°C in accordance with JIS-R5201; Here, T2(5;15) is the flow value of 15 strokes in the flow table test performed on the sample 5 minutes after its preparation. [α22] A method for producing a shaped object according to any one of [α13] to [α21], When a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B), and a flow table test is performed on the sample at 20°C in accordance with JIS-R5201, the difference between T2(5;15) and T2(5;0) (T2(5;15)-T2(5;0)) is in the range of 5 to 40 mm, Here, T2(5;15) is the flow value at 15 strokes in the flow table test performed on the sample 5 minutes after its preparation, and T2(5;0) is the flow value at 0 strokes in the flow table test performed on the sample 5 minutes after its preparation.
[0108] [β1] 1. A powder composition for producing a mortar material for additive manufacturing, comprising: Contains a binder (A) and a fine aggregate (B), A test specimen conforming to the standard JSCE-G 571 was obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the mixture. When the apparent diffusion coefficient of chloride ions was measured in accordance with the same standard, the apparent diffusion coefficient of chloride ions was found to be 0.5 cm 2 / year or less, powder composition. [β2] In the powder composition according to [β1], The additive manufacturing mortar material is a powder composition used in a process for forming at least a portion of a concrete structure including reinforcing steel by additive manufacturing. [β3] In the powder composition according to [β1] or [β2], A test specimen conforming to the standard JIS A 1153 was obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and hardening it. When the carbonation rate coefficient was measured in accordance with the same standard, the carbonation rate coefficient was 0.35 cm / year. (1 / 2) The powder composition is as follows: [β4] In the powder composition according to any one of [β1] to [β3], A powder composition, in which 14.5±1.5 parts by mass of water is added to 100 parts by mass of the powder composition and cured to obtain a test specimen conforming to JIS A 1148 (Method A), and when the relative dynamic modulus of elasticity is measured in accordance with the same standard, the relative dynamic modulus of elasticity is 90% or more. [β5] In the powder composition according to any one of [β1] to [β4], A test specimen conforming to the standard JSCE-G 582 was obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the mixture. When the moisture penetration rate coefficient was measured in accordance with the same standard, the moisture penetration rate coefficient was 0.8 mm / hour. (1 / 2) The powder composition is as follows: [β6] In the powder composition according to any one of [β1] to [β5], A test specimen conforming to the JSCE-K 571 standard is obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing it, and when the water permeability over 60 minutes is measured in accordance with the (3) Water Permeability Test of the same standard, the water permeability is 2.5 mL or less. [β7] In the powder composition according to any one of [β1] to [β6], A test specimen conforming to the standard NDIS 3436 was obtained by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition and curing the mixture. When the surface layer air permeability coefficient was measured in accordance with the standard, the surface layer air permeability coefficient was 0.1×10 -16 m 2 The powder composition is as follows: [β8] In the powder composition according to any one of [β1] to [β7], The binder (A) is a powder composition containing 40 mass% or more of slag powder and / or limestone powder based on the total amount of the binder (A). [β9] In the powder composition according to any one of [β1] to [β8], A powder composition further comprising an admixture (C) that imparts thixotropy. [β10] 1. A mortar material for additive manufacturing, comprising: A mortar material for additive manufacturing, comprising the powder composition according to any one of [β1] to [β10] and water. [β11] 1. A mortar material for additive manufacturing, comprising: Contains a binder (A), fine aggregate (B), and water, The additive manufacturing mortar material was hardened to obtain a test specimen conforming to the standard JSCE-G 571, and the apparent diffusion coefficient of the chloride ion was measured in accordance with the same standard. The apparent diffusion coefficient of the chloride ion was found to be 0.5 cm 2 / year or less, additive manufacturing mortar material. [β12] In the additive manufacturing mortar material according to [β11], An additive manufacturing mortar material for use in a process for additively forming at least a portion of a concrete structure including reinforcing steel. [β13] A sculpture, A molded object having a hardened mortar material for additive manufacturing according to any one of [β10] to [β12]. [β14] In the object according to [β13], A structure that contains rebar inside. [β15] A method for manufacturing a shaped object, comprising the steps of: A step of preparing a mortar material for additive manufacturing according to any one of [β10] to [β12]; shaping the additive manufacturing mortar material by additive manufacturing; and hardening the shaped mortar material for additive manufacturing. [β16] [β15] The method for producing a shaped object according to the present invention, A method for manufacturing a shaped object, comprising the steps of:
[0109] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0110] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the following examples (test examples).
[0111] [Raw materials used] First, the raw materials used in this example will be described. The raw materials used in this example are as follows: (1) Portland cement: Ordinary Portland cement (Blaine specific surface area 4440 cm 2 / g) (2) Ground granulated blast furnace slag: Ground granulated blast furnace slag (density: 2.91 g / cm 3 , Specific surface area: 8000cm 2 / g) (3) Silica fume: Silica fume (density: 2.25 g / cm 3 , Specific surface area: 2000000cm 2 / g; "MasterLife (registered trademark) SF 610" manufactured by Pozzolith Solutions, Inc. (4) Inorganic expanding material: Lime composite expanding material (Denka Power CSA manufactured by Denka Co., Ltd.) (5) Fine aggregate: No. 4 silica sand (water absorption rate 0.87%) (6) Thickener: Methylcellulose-based thickener, the raw material used is in powder form (7) Rheology modifier: Polycarboxylic acid type, the raw material used is in powder form ("Coaflow NF-100" manufactured by Taiheiyo Cement Corporation) (8) Nylon fiber (fiber length: 10 mm) (9) Moisturizer: Urea
[0112] [Preparation of powder composition] Various raw materials were mixed according to the recipe shown in Table 1 to prepare a powder composition according to Test Example 1. Specifically, each component was mixed for 5 minutes using a Hobart mixer to obtain a powder composition.
[0113] [Preparation of mortar materials] A predetermined amount of tap water was added to 3.0 kg of the obtained powder composition, and the mixture was mixed in a Hobart mixer at low speed (paddle rotation speed: 140 rpm, paddle revolution speed: 62 rpm) for 1 minute, the mortar that had once adhered to the paddle was scraped off, and the mixture was mixed again at high speed (paddle rotation speed: 285 rpm, paddle revolution speed: 125 rpm) for 2 minutes to obtain a mortar material. In addition, in Test Example 1, 15% by mass of tap water was added to the total mass of the binder and fine aggregate (28.1% by mass of tap water was added to the entire binder). In addition, the obtained mortar material was evaluated according to the following test items at 5 minutes and 30 minutes after preparation.
[0114] [Test 1: Slump test (JIS A 1171)] The kneaded mortar paste was filled into the slump cone in two layers. When filling, each layer was poked 15 times with a ram to pack the paste so that there were no gaps. After filling, the top surface was scraped flat and the cone was quickly removed. Immediately after removing the cone, the settled part of the paste was measured with a scale. Table 1 lists the evaluation value of the mortar material for each test example as the "mortar slump value." The lower this test value, the better the layering property when used in an additive manufacturing process.
[0115] [Test 2: Flow table test (JIS R 5201)] The kneaded mortar paste was filled into the flow cone in two layers. When filling, each layer was poked with a poker 15 times to pack the paste so that there were no gaps. After filling, the top surface was scraped to make it flat, and the cone was quickly removed. The diameter of the bottom surface was measured at only two points (orthogonal diameter). The maximum value of the measured value was taken as the flow value at 0 hits. Next, the sample was dropped at 1 cm per second, and this was repeated 15 times, after which the diameter of the bottom surface was measured at two points (orthogonal diameter). The maximum value of the measured value was taken as the flow value at 15 hits. In Table 1, the evaluation value of the mortar material of each test example is listed as the "mortar flow value". The difference between the mortar flow value at 15 hits and the mortar flow value at 0 hits is listed as the "flow spread amount". The smaller the mortar flow value at 0 hits, the better the lamination property can be when used in an additive manufacturing process. In addition, the mortar flow value at 15 strokes and the amount of flow spread can contribute to pumpability and fluidity when used in additive manufacturing processes, the greater the value.
[0116] [Test 3: Hand vane shear test (JGS 1411)] The kneaded mortar paste was divided into two layers and filled into a metal container. When filling, each layer was poked 10 times with a ram or the outer circumference was struck with a wooden hammer to pack the paste so that there were no voids. After filling, a metal cross blade attached to a torque wrench was inserted into the paste and rotated at a speed of 6 rpm. The maximum torque value was recorded, and the disturbed paste was made to flow again and smoothed out. This series of steps was repeated only twice, and the maximum value was taken as the shear yield value. Table 1 lists the evaluation value of the mortar material for each test example as the "shear yield value". The higher this test value, the better the lamination property when used in an additive manufacturing process.
[0117] [Table 1]
[0118] As shown in Table 1, the mortar material prepared from the powder composition of Test Example 1 had an excellent balance between lamination property and pumping / fluidity. The apparent diffusion coefficient of chloride ions shown in the item [Physical properties of powder composition (1)] for the mortar material prepared in Test Example 1 was measured, and the measured value was "0.5 cm 2 In addition, the carbonation rate coefficient of the mortar material prepared in Test Example 1, shown in the section [Physical properties of powder composition (1)], was measured and found to be 0.35 cm / year or less. (1 / 2) It was confirmed that the following conditions were satisfied.
Claims
1. A method for manufacturing a structure containing a reinforcing bar therein, comprising the steps of: Preparing a mortar material for additive manufacturing, comprising a binder (A), a fine aggregate (B), and water; shaping the additive manufacturing mortar material by additive manufacturing; hardening the shaped additive manufacturing mortar material; Equipped with The method for manufacturing a shaped object, wherein the content of the water in the mortar material for additive manufacturing is in the range of 27 to 34 parts by mass when the content of the binder (A) is 100 parts by mass.
2. The method for producing a shaped object according to claim 1 , The method for manufacturing a shaped object, wherein the mortar material for additive manufacturing contains a water-absorbing material in addition to the binder (A).
3. The method for producing a shaped object according to claim 2, The mortar material for additive manufacturing comprises, as the water-absorbing material, at least a portion of the fine aggregate (B) made of waste tile fine aggregate.
4. The method for producing a shaped object according to claim 2, The method for manufacturing a shaped object, wherein the mortar material for additive manufacturing contains a water-absorbent polymer and / or a water-absorbent fibrous material as the water-absorbent material.
5. The method for producing a shaped object according to claim 1 , A method for producing a shaped object, wherein the binder (A) contains 40 mass% or more of slag powder and / or limestone powder based on the total amount of the binder (A).
6. The method for producing a shaped object according to claim 1 , The method for producing a shaped object, wherein the additive manufacturing mortar material contains an admixture (C) that imparts thixotropy.
7. The method for producing a shaped object according to claim 1 , The method for producing a shaped object, wherein the binder (A) contains fly ash.
8. The method for producing a shaped object according to claim 1 , The method for producing a shaped object, wherein the fine aggregate (B) has an average particle size of 1 mm or less.
9. The method for producing a shaped object according to claim 1 , The fine aggregate (B) has a grain size index of 20 or more.
10. The method for producing a shaped object according to claim 1 , The method for producing a shaped object, wherein the additive manufacturing mortar material contains a dispersant and / or a flow agent.
11. The method for producing a shaped object according to claim 1 , The method for manufacturing a molded object, wherein the molded object has a portion where the reinforcing bar and a hardened product of the mortar material for additive manufacturing are in contact with each other.
12. The method for producing a shaped object according to claim 1 , In the step of modeling the additive manufacturing mortar material, a formwork into which concrete is poured is modeled using the additive manufacturing mortar material; The method for manufacturing a shaped object further comprises a step of forming a reinforced concrete structure within the formwork by pouring the concrete into the hardened reinforcing bars present within the formwork.
13. The method for manufacturing a shaped object according to any one of claims 1 to 12, The method for manufacturing a molded object, wherein the step of preparing the mortar material for additive manufacturing comprises mixing a powder composition containing a binder (A) and a fine aggregate (B) with water to obtain the mortar material for additive manufacturing.
14. The method for producing a shaped object according to claim 13, The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JSCE-G 571. When the apparent diffusion coefficient of chloride ions is measured in accordance with the same standard, the apparent diffusion coefficient of chloride ions is 0.5 cm 2 A method for manufacturing a sculpture that takes less than one year.
15. The method for producing a shaped object according to claim 13, The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JIS A 1153. When the carbonation rate coefficient is measured in accordance with the same standard, the carbonation rate coefficient is 0.35 cm / year. (1/2) The manufacturing method of the molded object is as follows.
16. The method for producing a shaped object according to claim 13, The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen in accordance with JIS A 1148 (Method A), and when the relative dynamic modulus of elasticity is measured in accordance with the same standard, the relative dynamic modulus of elasticity is 90% or more.
17. The method for producing a shaped object according to claim 13, The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard JSCE-G 582. When the moisture penetration rate coefficient is measured according to the same standard, the moisture penetration rate coefficient is 0.8 mm / hour. (1/2) The manufacturing method of the molded object is as follows.
18. The method for producing a shaped object according to claim 13, The powder composition is added with 14.5±1.5 parts by mass of water relative to 100 parts by mass of the powder composition, and then cured to obtain a test specimen in accordance with standard JSCE-K 571. When the water permeability for 60 minutes is measured in accordance with (3) Water Permeability Test of the same standard, the water permeability is 2.5 mL or less.
19. The method for producing a shaped object according to claim 13, The powder composition is cured by adding 14.5±1.5 parts by mass of water to 100 parts by mass of the powder composition to obtain a test specimen conforming to the standard NDIS 3436. When the surface layer air permeability coefficient is measured in accordance with the same standard, the surface layer air permeability coefficient is 0.1×10 -16 m 2 The manufacturing method of the molded object is as follows.
20. The method for producing a shaped object according to claim 13, The powder composition has a T2(5;0) of less than 110 mm when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B) and a flow table test is performed on the sample at 20° C. in accordance with JIS-R5201, Here, T2(5;0) is the flow value at 0 strokes in the flow table test performed on the sample 5 minutes after its production, in accordance with a method for manufacturing a molded object.
21. The method for producing a shaped object according to claim 13, The powder composition has a T2(5;15) of 110 mm or more when a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B) and a flow table test is performed on the sample at 20° C. in accordance with JIS-R5201, Here, T2(5;15) is the flow value of 15 strokes in the flow table test performed on the sample 5 minutes after its preparation.
22. The method for producing a shaped object according to claim 13, When a paste-like sample is prepared by adding 15 parts by mass of water to 100 parts by mass of the total of the binder (A) and the fine aggregate (B), and a flow table test is performed on the sample at 20° C. in accordance with JIS-R5201, the difference between T2(5;15) and T2(5;0) (T2(5;15)-T2(5;0)) is in the range of 5 to 40 mm, Here, T2(5;15) is the flow value at 15 strokes in the flow table test performed on the sample 5 minutes after its preparation, and T2(5;0) is the flow value at 0 strokes in the flow table test performed on the sample 5 minutes after its preparation.
Citation Information
Patent Citations
Additional production method
JP2018122539A
Hydraulic composition for forming lamination, hydraulic mortar, and hardened body thereof
JP2020105023A
Cited By
Powder, molded article, and method for producing powder
JP2026141636A
Powder, compact, and method for manufacturing powder
JP7747239B1