Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery

The positive electrode active material with a controlled composition and oxygen release profile addresses thermal runaway issues in lithium-ion batteries by distributing oxygen release across multiple temperature zones, improving safety and stability.

JP2024160882AActive Publication Date: 2024-11-15BASF SE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023076374
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15
Estimated Expiration
2043-05-02

AI Technical Summary

Technical Problem

Existing positive electrode active materials in lithium-ion secondary batteries, particularly those with high Ni content, face challenges in suppressing thermal runaway due to rapid oxygen release, which can lead to uncontrollable temperature rises and thermal instability.

Method used

A positive electrode active material with a specific composition, Li1+xNi1-y-z-wCoyMzO2, where M is one or more elements other than Li, Ni, Co, and Mn, is designed to release oxygen in multiple temperature zones by controlling the differential thermogravimetric curve to have distinct peaks, thereby reducing the rate of oxygen release and suppressing thermal runaway.

Benefits of technology

The proposed active material effectively suppresses thermal runaway by distributing oxygen release over multiple temperature zones, reducing the risk of uncontrollable temperature rises and enhancing the safety of non-aqueous electrolyte secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160882000001_ABST
    Figure 2024160882000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material capable of suppressing a thermal runway, and provide a non-aqueous electrolyte secondary battery using the same.SOLUTION: A positive electrode active material for a non-aqueous electrolyte secondary battery is expressed by Li[Lix(Ni1-y-z-wCoyMnzMw)1-x]O2 (where M is one or more kinds of elements other than Li, Ni, Co, Mn and O, and satisfies -0.1≤x≤0.15, 0<y≤0.4, 0≤z≤0.4, and 0≤w≤0.1), and includes: a first peak in which a value of a DTG in a peak top indicates the maximum value under 150°C or more and 350°C or less when a DTG curve for a sample of which a counter electrode is charged as a lithium is separated into a plurality of peaks; and a second peak in which the value of the DTG of the peak indicating the peak top at a temperature that has a difference of 20°C or more against a temperature indicating their peak top indicates the maximum value. The value of the DTG in the peak top of the first peak against the value of the DTG in the peak top of the second peak is 1 or more and 9 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Lithium ion secondary batteries have attracted attention as a power source for driving electronic devices such as AV equipment and personal computers because of their advantages of being small, lightweight, high energy density, high charge / discharge voltage, and large charge / discharge capacity.

[0003] Lithium ion secondary batteries usually use flammable organic solvents as electrolytes, and therefore require high thermal stability. For example, in lithium ion secondary batteries, when heat is applied during charging, oxygen is released from the positive electrode active material crystals, and it is known that this oxygen reacts with the electrolyte to cause thermal runaway.

[0004] In particular, active materials containing Ni, Co, and Mn have been widely used as positive electrode active materials in recent years. In such positive electrode active materials, the higher the Ni content, the lower the temperature at which the phase transition reaction of the positive electrode active material occurs, and oxygen is released rapidly, making the positive electrode active material more likely to experience thermal runaway. On the other hand, there is a demand for materials with a high Ni content that have a large battery capacity, and as a result, there is a tendency for the thermal stability specific to materials with a high Ni content to decrease.

[0005] In order to suppress the thermal runaway of such a positive electrode active material, for example, Patent Document 1 proposes a positive electrode active material containing a lithium transition metal composite oxide containing 80 mol % or more of Ni and 0.1 mol % to 1.5 mol % or less of B relative to the total number of moles of metal elements other than Li, in which B and at least one element (M1) selected from Groups 4 to 6 are present at least on the particle surface of the lithium transition metal composite oxide, and the molar fraction of M1 relative to the total number of moles of metal elements other than Li on the surface of particles smaller than 30% particle size is greater than the molar fraction of M1 relative to the total number of moles of metal elements other than Li on the surface of particles with a volume-based particle size larger than 70% particle size. Patent Document 1 also describes that by using such a composite oxide in a lithium ion secondary battery, the self-heating rate is suppressed even at high temperatures. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-51979 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the positive electrode active material of Patent Document 1, by coating the particle surfaces of the positive electrode active material with a boron compound, it is expected that there will be a certain degree of suppression effect against thermal runaway caused by the reaction between the oxygen released from the positive electrode active material and the electrolyte. However, this alone is not sufficient to suppress thermal runaway, and there is still room for improvement.

[0008] Therefore, there is a need for a method for suppressing thermal runaway other than the above-mentioned method of coating the surface of the positive electrode active material with a compound.

[0009] The present disclosure has been made in view of the above circumstances, and has an object to provide a positive electrode active material capable of suppressing thermal runaway in a nonaqueous electrolyte secondary battery, and a nonaqueous electrolyte secondary battery using the same. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above-mentioned problems. 1+x Ni 1-y-z-w Co y Mn z M w A composite oxide represented by the formula: O2 (wherein M is one or more elements other than Li, Ni, Co, Mn, and O, and -0.1≦x≦0.15, 0≦y≦0.4, 0≦z≦0.4, 0≦w≦0.1), wherein the composite oxide is charged to 4.30 V using lithium as a counter electrode, and the differential thermogravimetric curve obtained by heating the sample from 50°C to 600°C at a rate of 5°C / min is separated into a plurality of peaks, the first peak being the peak having the maximum differential thermogravimetric value at the peak top within a temperature range of 150°C to 350°C. It has been found that when a positive electrode active material having a first peak and a second peak, the value of the differential thermogravimetry at the peak top being the maximum value among the peaks that have a peak top at a temperature 20°C or more away from the temperature showing the peak top of the first peak, and the value of the differential thermogravimetry of the first peak relative to the value of the differential thermogravimetry of the second peak is 1 or more and 9 or less, is used in a non-aqueous electrolyte secondary battery, the maximum rate of oxygen release from the positive electrode active material (hereinafter referred to as "maximum oxygen release rate") can be suppressed, and further thermal runaway can be suppressed. Specifically, the present disclosure provides the following.

[0011] (1) General formula Li 1+x Ni 1-y-z-w Co y Mn z M wO2 (where M is one or more elements other than Li, Ni, Co, Mn, and O, -0.1 ≦ x ≦ 0.15, 0 ≦ y ≦ 0.4, 0 ≦ z ≦ 0.4, 0 ≦ w ≦ 0.1), and when the differential thermogravimetric curve obtained by heating the composite oxide from 50°C to 600°C at 5°C / min per minute for a sample with the counter electrode charged to 4.30V with lithium is separated into a plurality of peaks, in the temperature range of 150°C or higher and 350°C or lower, there is a first peak where the value of the differential thermogravimetry at the peak top shows the maximum value, and among the peaks showing the peak top at a temperature 20°C or more away from the temperature showing the peak top of the first peak, there is a second peak where the value of the differential thermogravimetry at the peak top shows the maximum value, and the value of the differential thermogravimetry at the peak top of the first peak with respect to the value of the differential thermogravimetry at the peak top of the second peak is 1 or more and 9 or less. A positive electrode active material for a non-aqueous electrolyte secondary battery.

[0012] (2) The positive electrode active material for a non-aqueous electrolyte secondary battery according to (1), wherein in the composite oxide, 0 < x ≦ 0.15.

[0013] (3) The positive electrode active material for a non-aqueous electrolyte secondary battery according to (1) or (2), wherein the value of the differential thermogravimetry at the peak top of the first peak is 3% / min or less.

[0014] (4) A non-aqueous electrolyte secondary battery comprising a positive electrode containing the positive electrode active material according to (1) or (2).

Advantages of the Invention

[0015] According to the present disclosure, a positive electrode active material capable of suppressing thermal runaway when used in a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery using the same can be provided.

Brief Description of the Drawings

[0016] [Figure 1] It is a DTG curve of the composite oxide sample of Example 1. [Diagram 2] It is a DTG curve of the composite oxide sample of Example 2. [Diagram 3]1 is a DTG curve of a composite oxide sample of Example 3. [Figure 4] 1 is a DTG curve of a composite oxide sample of Example 4. [Diagram 5] 1 is a DTG curve of a composite oxide sample of Example 5. [Figure 6] 1 is a DTG curve of a composite oxide sample of Example 6. [Figure 7] 1 is a DTG curve of a composite oxide sample of Example 7. [Figure 8] 1 is a DTG curve of a composite oxide sample of Example 8. [Figure 9] 1 is a DTG curve of a composite oxide sample of Example 9. [Figure 10] 1 is a DTG curve of a composite oxide sample of Example 10. [Figure 11] 1 is a DTG curve of a composite oxide sample of Example 11. [Figure 12] 1 is a DTG curve of a composite oxide sample of Example 12. [Figure 13] 1 is a DTG curve of a composite oxide sample of Example 13. [Figure 14] 1 is a DTG curve of a composite oxide sample of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present disclosure will be described, however, the present disclosure is not limited in any way to the description of the embodiments and can be implemented with appropriate modifications.

[0018] <Cathode active material for nonaqueous electrolyte secondary batteries> The positive electrode active material for a non-aqueous electrolyte secondary battery according to an embodiment of the present disclosure is represented by the general formula Li 1+x Ni 1-y-z-w Co y Mn z M wThe present invention relates to a composite oxide having a composite oxide represented by the formula: O2 (wherein M is one or more elements other than Li, Ni, Co, Mn, and O, and -0.1≦x≦0.15, 0≦y≦0.4, 0≦z≦0.4, 0≦w≦0.1), and when the composite oxide is charged to 4.30 V using lithium as a counter electrode and the temperature is increased from 50°C to 600°C at a rate of 5°C / min to obtain a differential thermogravimetric curve that is separated into a plurality of peaks, the composite oxide has a first peak having a maximum value of the differential thermogravimetric value at its peak top in a temperature range of 150°C to 350°C, and a second peak having a maximum value of the differential thermogravimetric value at its peak top among the peaks that have a peak top at a temperature that is 20°C or more away from the temperature at which the first peak has a peak top, and the differential thermogravimetric value at the peak top of the second peak is 1 or more and 9 or less.

[0019] When oxygen release from the positive electrode active material occurs in multiple temperature zones that are mutually separated, oxygen release is suppressed in each temperature zone, and as a result, the reaction with the electrolyte is also suppressed, and the amount of heat generated is reduced, compared to when oxygen release from the positive electrode active material occurs only in one narrow temperature zone. Therefore, by making oxygen release from the positive electrode active material occur in multiple temperature zones that are mutually separated, thermal runaway of the positive electrode active material can be suppressed.

[0020] The inventors have confirmed by TG-MS that the weight loss at temperatures up to about 350°C is almost entirely due to oxygen release when the composite oxide is subjected to TG measurement. As a result, oxygen release from the positive electrode active material occurs in a temperature range of 150°C to 350°C, while the positive electrode active material does not undergo any other reactions in this temperature range. Therefore, when the differential thermogravimetric curve (hereinafter sometimes referred to as "DTG curve") of the positive electrode active material is separated into multiple peaks, the positive electrode active material has a first peak that is the largest in the temperature range of 150°C to 350°C and a second peak that is separated from each other by a temperature of 20°C or more, and the magnitude of the first peak is 9 times or less than the magnitude of the second peak, which means that oxygen release from the positive electrode active material occurs in multiple temperature zones that are separated from each other.

[0021] On the other hand, when the DTG curve cannot be separated into multiple peaks (consists of a single peak), or when the DTG curve can be separated into multiple peaks but the magnitude of the first peak is much larger than the magnitude of the second peak, oxygen is released from the positive electrode active material in a narrow temperature range, making thermal runaway more likely to occur.

[0022] The requirements for a positive electrode active material to show such a DTG curve are related to many factors such as the elemental composition, crystal structure, crystallinity, and synthesis conditions of the positive electrode active material, and can also change depending on the balance between them. Materials that tend to show such a DTG curve include those with the general formula Li 1+x Ni 1-y-z-w Co y Mn z M w An example of such a composite oxide is represented by the formula: O2 (wherein M is one or more elements other than Li, Ni, Co, Mn, and O, and -0.1≦x≦0.15, 0≦y≦0.4, 0≦z≦0.4, 0≦w≦0.1). However, even if such a composition is present, the two specified peaks in the DTG curve do not necessarily satisfy the above-mentioned requirements. In other words, the two specified peaks in the DTG curve do not depend only on the composition of the compound.

[0023] In the following, the mechanism by which a composite oxide releases oxygen in a charged state, when a large amount of lithium is released from the crystal structure and the crystal structure is generally unstable, is called Li 1-x-δ We will use NiO2 as an example. When such a composite oxide is used as the positive electrode active material and heated in a charged state, the crystal state undergoes a phase transition from a layered rock salt structure (R-3m) to a spinel structure (Fd-3m) or rock salt structure (Fm3m) in a specific temperature range, as shown in the following formulas (1) and (2). The temperature of these phase transitions depends on the depth of charge, but they occur in a temperature range of about 190 to 310°C. In addition, as is clear from formulas (1) and (2), it is believed that the transitions proceed while generating oxygen gas.

[0024] Formula (1): Li 1-x-δ NiO2 (layered rock salt structure R-3m) →{(1-x-δ) / (1-δ)}Li 1-δ NiO2 (Layered rock salt structure 1 R-3m) +{x / 3(1-δ)}Ni3O4 (spinel structure Fd-3m) +{x / 3(1-δ)}O2↑

[0025] Formula (2): ·{(1-x-δ) / (1-δ)}Li 1-δ NiO2 (Layered rock salt structure 1 R-3m) →(1-x-δ)LiNiO2 (layered rock salt structure 2 R-3m) +{δ(1-x-δ) / (1-δ)}NiO(Halite structure 1 Fm3m) +{δ(1-x-δ) / 2(1-δ)}O2↑ ·{x / 3(1-δ)}Ni3O4 (spinel structure Fd-3m) →{x / 3(1-δ)}NiO (rock salt structure 2 Fm3m) +{x / 6(1-δ)}O2↑

[0026] In addition, the "-" in R-3m is normally placed above the 3, but for convenience it is written as above. Similarly, the "-" in Fd-3m is normally placed above the 3, but for convenience it is written as above.

[0027] The present inventors believe that this sudden generation of oxygen gas has a significant effect on the thermal stability of a charged non-aqueous electrolyte secondary battery.

[0028] When a non-aqueous electrolyte secondary battery in a charged state overheats and the temperature rises, the oxygen gas generated by the reactions of formula (1) and formula (2) mainly oxidizes (including combustion) the organic electrolyte in the non-aqueous electrolyte secondary battery. Because this reaction is exothermic, the temperature of the non-aqueous electrolyte secondary battery rises. This temperature rise further oxidizes the electrolyte, generating heat, causing the temperature rise to become uncontrollable, leading to thermal runaway.

[0029] The increase in temperature is proportional to the difference between the amount of heat generated per unit time in the non-aqueous electrolyte secondary battery and the amount of heat dissipated per unit time from the non-aqueous electrolyte secondary battery. Therefore, by preventing the heat generation and heat flow from being concentrated in a short period of time according to Formula (1) and Formula (2), the temperature increase can be suppressed, and the safety can be enhanced by preventing the uncontrollable thermal runaway.

[0030] From the above, the inventors considered that it is most important to suppress the oxygen release rate from the positive electrode active material in order to suppress the uncontrollable thermal runaway. And for that purpose, as in the present disclosure, it can be said that it is effective to adjust so that the oxygen release of the composite oxide occurs in a plurality of temperature ranges and to control so that rapid oxygen release does not occur in a narrow temperature range.

[0031] 〔Chemical Structure〕 As the composite oxide, as long as it is represented by the general formula Li[Li x (Ni 1-y-z-w Co y Mn z M w ) 1-x O2 (wherein M is one or more elements other than Li, Ni, Co, Mn, and O, and -0.1 ≦ x ≦ 0.15, 0 < y ≦ 0.4, 0 ≦ z ≦ 0.4, 0 ≦ w ≦ 0.1), it is not particularly limited.

[0032] In the present disclosure, the reason why the composite oxide as the positive electrode active material exhibits a plurality of peaks is not necessarily clear and is not limited to a specific theory, but the inventors consider as follows. In such a composite oxide, at a high SOC charge state, most of the Ni in the positive electrode active material is oxidized to a high-valent Ni 4+ and is reduced in the temperature range of 150°C to 350°C to become Ni 2+ state. At this time, since the ionic radius of Ni 2+ is almost the same as that of Li + , Ni 2+ will move to the Li layer. The inventors believe that this reduction of Ni 4+ and Ni 2+The movement of Ni to the Li layer occurred almost simultaneously, and it was thought that if this movement could be suppressed, the reduction could also be suppressed. 2+ In order for Ni to move to the Li layer, 2+ The oxygen must move from the oxygen octahedral position in the metal layer, through the vacant oxygen tetrahedral position adjacent to it, and then to the vacant oxygen octahedral position in the Li layer adjacent to it. Therefore, Ni 2+ If the energy barrier for Ni to move to vacant tetrahedral or octahedral sites can be increased, the extra energy required for the transfer will be required, and Ni will be reduced at a higher temperature. 2+ By distributing the height of the barrier required for the movement of Ni, it is possible to distribute the temperature range in which high-valent Ni is reduced. This allows the amount of Ni reduced in one narrow temperature range to be suppressed, thereby suppressing the amount of oxygen generated, and therefore the DTG peak in one narrow temperature range can be lowered. Therefore, if a complex oxide in which such a phenomenon occurs depending on the ratio of Li, Ni, Co, Mn, and element M, the type of element M, the crystallinity of the complex oxide, and the synthesis conditions of the complex oxide, etc., is used as a positive electrode active material, it is possible to distribute the temperature range in which oxygen is released to multiple ranges while maintaining the basic functions (charge capacity and cycle characteristics) of a non-aqueous electrolyte secondary battery, and it was found that the DTG peak value can be lowered as described above.

[0033] Specifically, depending on the combination of other elements contained in the complex oxide, the crystallinity of the complex oxide, synthesis conditions, etc., if the complex oxide contains Co, it is heated at about 230 to 270°C. 3+ and Co 4+ Co 2+ It is believed that the Co3O4 spinel structure is reduced to Co3O4 and resides in the oxygen tetrahedral sites of the Li layer. 2+ This is the oxygen octahedral migration path of Co. 2+ By occupying Ni 2+It is considered that the migration of oxygen to the octahedral position is easily suppressed. Therefore, in such a case, when the composite oxide is used as a positive electrode active material, the temperature range in which oxygen is released can be dispersed into multiple regions while maintaining the basic functions (charging capacity and cycle characteristics) of the nonaqueous electrolyte secondary battery, and the DTG peak value can be reduced as described above.

[0034] In the general formula, the value of x is not particularly limited as long as it is within the range of -0.10≦x≦0.15, and may be, for example, -0.095 or more, -0.09 or more, -0.085 or more, -0.08 or more, -0.075 or more, -0.07 or more, -0.065 or more, -0.06 or more, -0.055 or more, -0.05 or more, -0.045 or more, -0.04 or more, -0.035 or more, -0.03 or more, -0.025 or more, -0.02 or more, -0.015 or more, -0.01 or more, -0.0095 or more. ,-0.009 or more,-0.0085 or more,-0.008 or more,-0.0075 or more,-0.007 or more,-0.0065 or more,-0.006 or more,-0.0055 or more,-0.005 or more,-0.0045 or more,-0.004 or more,-0.0035 or more,-0.003 or more,-0.0025 or more,-0.0015 or more,-0.001 or more,0 or more,0.001 or more,0.0015 or more,0.002 or more,0.0025 or more,0.003 or more, 0.0035 or more, 0.004 or more, 0.0045 or more, 0.005 or more, 0.0055 or more, 0.006 or more, 0.0065 or more, 0.007 or more, 0.0075 or more, 0.008 or more, 0.0085 or more, 0.009 or more, 0.0095 or more, 0.01 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0.045 or more, 0.05 or more, 0.055 or more, 0.06 or more, 0.065 or more, 0.07 or more, It is preferable that the molecular weight is 0.075 or more, 0.08 or more, 0.085 or more, 0.09 or more, 0.095 or more, 0.1 or more, 0.102 or more, 0.105 or more, 0.107 or more, 0.11 or more, 0.112 or more, 0.115 or more, 0.117 or more, 0.12 or more, 0.122 or more, 0.125 or more, 0.127 or more, 0.13 or more, 0.132 or more, 0.135 or more, 0.137 or more, 0.14 or more, 0.142 or more, 0.145 or more, 0.147 or more, or 0.15 or more.On the other hand, the values ​​of x are 0.147 or less, 0.145 or less, 0.142 or less, 0.14 or less, 0.137 or less, 0.135 or less, 0.132 or less, 0.13 or less, 0.127 or less, 0.125 or less, 0.122 or less, 0.12 or less, 0.117 or less, 0.115 or less, 0.112 or less, 0.11 or less, 0.107 or less, 0.105 or less, 0.102 or less, 0.1 or less, 0.095 or less, 0.09 or less, 0.085 or less, 0.08 or less, 0. 075 or less, 0.07 or less, 0.065 or less, 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.015 or less, 0.0 1 or less, 0.0095 or less, 0.009 or less, 0.0085 or less, 0.008 or less, 0.0075 or less, 0.007 or less, 0.0065 or less, 0.006 or less, 0.0055 or less, 0.005 or less, 0.0045 or less, 0 .004 or less, 0.0035 or less, 0.003 or less, 0.0025 or less, 0.002 or less, 0.0015 or less, 0.001 or less, 0 or less, -0.001 or less, -0.0015 or less, -0.002 or less, -0.0025 or less , -0.003 or less, -0.0035 or less, -0.004 or less, -0.0045 or less, -0.005 or less, -0.0055 or less, -0.006 or less, -0.0065 or less, -0.007 or less, -0.0075 or less, -0. It is preferable that x is 0.008 or less, -0.0085 or less, -0.009 or less, -0.0095 or less, -0.01 or less, -0.015 or less, -0.02 or less, -0.025 or less, -0.03 or less, -0.035 or less, -0.04 or less, -0.045 or less, -0.05 or less, -0.055 or less, -0.06 or less, -0.065 or less, -0.07 or less, -0.075 or less, -0.08 or less, -0.085 or less, -0.09 or less, or -0.095 or less. The value of x being within the required range means that the Li content is within the required range. By setting the value of x to a required value or more, the Li content can be increased, Li vacancies can be reduced, and the first reduction of Ni occurring between about 200 and 250° C. can be suppressed, while the proportion of the second reduction occurring between about 260 and 320° C. can be increased. This tends to decrease the peak top on the low temperature side of the differential thermogravimetry curve, and increase the peak top on the high temperature side.By setting the value of x to a required value or less, a certain amount of Li vacancies can be ensured, and a decrease in charge capacity can be suppressed.

[0035] In the general formula, the value of 1-yzw is not particularly limited as long as it is a combination of y, z, and w within the range that can be taken, and may be, for example, 0.6 or more, 0.605 or more, 0.61 or more, 0.615 or more, 0.62 or more, 0.625 or more, 0.63 or more, 0.635 or more, 0.64 or more, 0.645 or more, 0.65 or more, 0.655 or more, 0.66 or more, 0.665 or more, 0.67 or more, 0.675 or more, 0.68 or more, 0. It is preferable that the molecular weight is 685 or more, 0.69 or more, 0.695 or more, 0.70 or more, 0.705 or more, 0.71 or more, 0.715 or more, 0.72 or more, 0.725 or more, 0.73 or more, 0.735 or more, 0.74 or more, 0.745 or more, 0.75 or more, 0.755 or more, 0.76 or more, 0.765 or more, 0.77 or more, 0.775 or more, 0.78 or more, 0.785 or more, 0.79 or more, or 0.795 or more. On the other hand, the value of 1-yzw may be 1 or less, 0.995 or less, 0.99 or less, 0.985 or less, 0.98 or less, 0.975 or less, 0.97 or less, 0.965 or less, 0.96 or less, 0.955 or less, 0.95 or less, 0.945 or less, 0.94 or less, 0.935 or less, 0.93 or less, 0.925 or less, 0.92 or less, 0.915 or less, 0.91 or less, 0.905 or less, 0.90 or less, 0.895 or less, 0.89 or less, 0.885 or less, 0.88 or less, 0.875 or less, 0.87 or less, 0.865 or less, 0.86 or less, 0.855 or less, 0.85 or less, 0.845 or less, or 0.84 or less. The value of 1-yzw being within the required range means that the Ni content is within the required range. By setting the value of 1-yzw to a required value or more, it is possible to increase the amount of Ni that moves within the composite oxide. On the other hand, by setting the value of 1-yzw to a certain value or less, it is possible to provide room for the inclusion of an element having functionality that can inhibit the movement of some of the Ni, depending on the balance with other elements, etc.

[0036] In the general formula, the value of y is not particularly limited as long as it is within the range of 0≦y≦0.4, and examples thereof include y greater than 0, 0.001 or more, 0.0015 or more, 0.002 or more, 0.0025 or more, 0.003 or more, 0.0035 or more, 0.004 or more, 0.0045 or more, 0.005 or more, 0.0055 or more, 0.006 or more, 0.0065 or more, 0.007 or more, 0.0075 or more, 0.008 or more, 0.0085 or more, 0.009 or more, 0.0095 or more, 0.01 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0.045 or more, 0.05 or more, 0.055 or more, 0.06 or more, 0.065 or more, 0.07 or more, 0.075 or more, 0.08 or more, 0.085 or more, 0.09 or more, 0.095 or more, 0.1 or more, 0.102 or more, 0.105 or more, 0.107 or more, 0.11 or more, 0.112 or more, 0.115 or more, 0.117 or more, 0.12 or more, 0.122 or more, 0.125 or more, 0.127 or more, 0.13 or more, 0.132 or more, 0.135 or more, 0.137 or more, 0.14 or more, 0.142 or more, 0.145 or more, 0.147 or more, 0.15 or more, 0.152 or more, 0.155 or more, 0.157 or more, 0.16 or more, 0.162 or more, 0.165 or more, 0.167 or more, 0.17 or more, 0.172 or more, 0.175 or more, 0.177 or more, 0.18 or more, 0.182 or more, 0.185 or more, 0.187 or more, 0.19 or more, 0.192 or more, 0.195 or more, 0.197 or more, 0.2 or more, 0.202 or more, 0.205 or more, 0.207 or more, 0.21 or more, 0.212 or more, 0.215 or more, 0.217 or more, 0.22 or more, 0.222 or more, 0.225 or more, 0.227 or more, 0.23 or more, 0.232 or more ,0.235 or more,0.237 or more,0.24 or more,0.242 or more,0.245 or more,0.247 or more,0.25 or more,0.252 or more,0.255 or more,0.257 or more,0.26 or more,0.262 or more,0.265 or more,0.267 or more,0.27 or more,0.272 or more,0.275 or more,0.277 or more,0.28 or more,0.282 or more,0.285 or more,0.287 or more,0.29 or more,0.292 or more,0.295 or more,0.297 or more,0.3 or more,0.302 or more,0.305 or more,0.307 or more,0.31 or more,0.312 or more,0.It is preferable that the molecular weight is 315 or more, 0.317 or more, 0.32 or more, 0.322 or more, 0.325 or more, 0.327 or more, 0.33 or more, 0.332 or more, 0.335 or more, 0.337 or more, 0.34 or more, 0.342 or more, 0.345 or more, 0.347 or more, 0.35 or more, 0.352 or more, 0.355 or more, 0.357 or more, 0.36 or more, 0.362 or more, 0.365 or more, 0.367 or more, 0.37 or more, 0.372 or more, 0.375 or more, 0.377 or more, 0.38 or more, 0.382 or more, 0.385 or more, 0.387 or more, 0.39 or more, 0.392 or more, 0.395 or more, or 0.397 or more. On the other hand, the values ​​of y are 0.397 or less, 0.395 or less, 0.392 or less, 0.39 or less, 0.387 or less, 0.385 or less, 0.382 or less, 0.38 or less, 0.377 or less, 0.375 or less, 0 .372 or less, 0.367 or less, 0.365 or less, 0.362 or less, 0.36 or less, 0.357 or less, 0.355 or less, 0.352 or less, 0.35 or less, 0.347 or less, 0.345 or less, 0.342 or less Below, 0.34 or less, 0.337 or less, 0.335 or less, 0.332 or less, 0.33 or less, 0.327 or less, 0.325 or less, 0.322 or less, 0.32 or less, 0.317 or less, 0.315 or less, 0.3 12 or less, 0.31 or less, 0.307 or less, 0.305 or less, 0.302 or less, 0.3 or less, 0.297 or less, 0.295 or less, 0.292 or less, 0.29 or less, 0.287 or less, 0.285 or less, 0. 282 or less, 0.28 or less, 0.277 or less, 0.275 or less, 0.272 or less, 0.27 or less, 0.267 or less, 0.265 or less, 0.26 or less, 0.257 or less, 0.255 or less, 0.252 or less , 0.25 or less, 0.247 or less, 0.245 or less, 0.242 or less, 0.24 or less, 0.237 or less, 0.235 or less, 0.232 or less, 0.23 or less, 0.227 or less, 0.225 or less, 0.222 0.22 or less, 0.217 or less, 0.215 or less, 0.212 or less, 0.21 or less, 0.207 or less, 0.205 or less, 0.202 or less, 0.2 or less, 0.197 or less, 0.195 or less, 0.19 2 or less, 0.19 or less, 0.187 or less, 0.185 or less, 0.182 or less, 0.18 or less, 0.177 or less, 0.175 or less, 0.172 or less, 0.17 or less, 0.167 or less, 0.165 or less, 0.162 or less, 0.16 or less, 0.155 or less, 0.152 or less, 0.15 or less, 0.147 or less, 0.145 or less, 0.142 or less, 0.14 or less, 0.137 or less, 0.135 or less, 0.132 or less, 0.13 or less, 0.127 or less, 0.125 or less, 0.122 or less, 0.12 or less, 0.117 or less, 0.115 or less, 0.112 or less, 0.11 or less, 0.107 or less, 0.105 or less, 0.102 or less, 0.1 or less, 0.095 or less, 0.09 or less, 0.085 or less, 0.08 or less, 0.075 or less, 0.07 or less, 0.065 or less, 0 Preferably, y is 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.015 or less, 0.01 or less, 0.0095 or less, 0.009 or less, 0.0085 or less, 0.008 or less, 0.0075 or less, 0.007 or less, 0.0065 or less, 0.0055 or less, 0.005 or less, 0.0045 or less, 0.004 or less, 0.0035 or less, 0.003 or less, 0.0025 or less, 0.002 or less, 0.0015 or less, or 0.001 or less. The value of y being within the required range means that the Co content is within the required range. By setting the value of y to a value greater than the required value, Co is increased, which results in Ni. 4+ On the other hand, even if the value of y is set to a certain value or more, the increase in the amount of the second reduction may reach a plateau, so the value is set to a required value or less.

[0037] In the general formula, the value of z is not particularly limited as long as it is within the range of 0≦z≦0.4, and may be, for example, 0.001 or more, 0.0015 or more, 0.002 or more, 0.0025 or more, 0.003 or more, 0.0035 or more, 0.004 or more, 0.0045 or more, 0.005 or more, 0.0055 or more, 0.006 or more, 0.0065 or more, 0.007 or more, 0.0075 or more, 0.008 or more, 0.0085 or more, 0.009 or more, 0.0095 or more, 0.01 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0. 045 or more, 0.05 or more, 0.055 or more, 0.06 or more, 0.065 or more, 0.07 or more, 0.075 or more, 0.08 or more, 0.085 or more, 0.09 or more, 0.095 or more, 0.1 or more, 0.102 or more, 0.105 or more, 0.107 or more, 0.11 or more, 0.112 or more, 0.115 or more, 0.117 or more, 0.12 or more, 0.122 or more, 0.125 or more, 0.127 or more, 0.13 or more, 0.132 or more, 0.135 or more, 0.137 or more, 0.14 or more, 0.142 or more, 0.145 or more, 0.147 or more, 0.15 or more, 0.152 or more ,0.155 or more,0.157 or more,0.16 or more,0.162 or more,0.165 or more,0.167 or more,0.17 or more,0.172 or more,0.175 or more,0.177 or more,0.18 or more,0.182 or more,0.185 or more,0.187 or more,0.19 or more,0.192 or more,0.195 or more,0.197 or more,0.2 or more,0.202 or more,0.205 or more,0.207 or more,0.21 or more,0.212 or more,0.215 or more,0.217 or more,0.22 or more,0.222 or more,0.225 or more,0.227 or more,0.23 or more, 0.235 or more, 0.237 or more, 0.24 or more, 0.242 or more, 0.245 or more, 0.247 or more, 0.25 or more, 0.252 or more, 0.255 or more, 0.257 or more, 0.26 or more, 0.262 or more, 0.265 or more, 0.267 or more, 0.27 or more, 0.272 or more, 0.275 or more, 0.277 or more, 0.282 or more, 0.285 or more, 0.287 or more, 0.29 or more, 0.292 or more, 0.295 or more, 0.297 or more, 0.3 or more, 0.302 or more, 0.305 or more, 0.307 or more, 0.31 or more, 0.312 or more, 0.It is preferable that the molecular weight is 315 or more, 0.317 or more, 0.32 or more, 0.322 or more, 0.325 or more, 0.327 or more, 0.33 or more, 0.332 or more, 0.335 or more, 0.337 or more, 0.34 or more, 0.342 or more, 0.345 or more, 0.347 or more, 0.35 or more, 0.352 or more, 0.355 or more, 0.357 or more, 0.36 or more, 0.362 or more, 0.365 or more, 0.367 or more, 0.37 or more, 0.372 or more, 0.375 or more, 0.377 or more, 0.38 or more, 0.382 or more, 0.385 or more, 0.387 or more, 0.39 or more, 0.392 or more, 0.395 or more, or 0.397 or more. On the other hand, the values ​​of z are 0.397 or less, 0.395 or less, 0.392 or less, 0.39 or less, 0.387 or less, 0.385 or less, 0.382 or less, 0.38 or less, 0.377 or less, 0.375 or less, 0 .372 or less, 0.367 or less, 0.365 or less, 0.362 or less, 0.36 or less, 0.357 or less, 0.355 or less, 0.352 or less, 0.35 or less, 0.347 or less, 0.345 or less, 0.342 or less Below, 0.34 or less, 0.337 or less, 0.335 or less, 0.332 or less, 0.33 or less, 0.327 or less, 0.325 or less, 0.322 or less, 0.32 or less, 0.317 or less, 0.315 or less, 0.3 12 or less, 0.31 or less, 0.307 or less, 0.305 or less, 0.302 or less, 0.3 or less, 0.297 or less, 0.295 or less, 0.292 or less, 0.29 or less, 0.287 or less, 0.285 or less, 0. 282 or less, 0.28 or less, 0.277 or less, 0.275 or less, 0.272 or less, 0.27 or less, 0.267 or less, 0.265 or less, 0.26 or less, 0.257 or less, 0.255 or less, 0.252 or less , 0.25 or less, 0.247 or less, 0.245 or less, 0.242 or less, 0.24 or less, 0.237 or less, 0.235 or less, 0.232 or less, 0.23 or less, 0.227 or less, 0.225 or less, 0.222 0.22 or less, 0.217 or less, 0.215 or less, 0.212 or less, 0.21 or less, 0.207 or less, 0.205 or less, 0.202 or less, 0.2 or less, 0.197 or less, 0.195 or less, 0.19 2 or less, 0.19 or less, 0.187 or less, 0.185 or less, 0.182 or less, 0.18 or less, 0.177 or less, 0.175 or less, 0.172 or less, 0.17 or less, 0.167 or less, 0.165 or less, 0.162 or less, 0.16 or less, 0.155 or less, 0.152 or less, 0.15 or less, 0.147 or less, 0.145 or less, 0.142 or less, 0.14 or less, 0.137 or less, 0.135 or less, 0.132 or less, 0.13 or less, 0.127 or less, 0.125 or less, 0.122 or less, 0.12 or less, 0.117 or less, 0.115 or less, 0.112 or less, 0.11 or less, 0.107 or less, 0.105 or less, 0.102 or less, 0.1 or less, 0.095 or less, 0.09 or less, 0.085 or less, 0.08 or less, 0.075 or less, 0.07 or less, 0.065 or less, 0 Preferably, z is 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.015 or less, 0.01 or less, 0.0095 or less, 0.009 or less, 0.0085 or less, 0.008 or less, 0.0075 or less, 0.007 or less, 0.0065 or less, 0.0055 or less, 0.005 or less, 0.0045 or less, 0.004 or less, 0.0035 or less, 0.003 or less, 0.0025 or less, 0.002 or less, 0.0015 or less, or 0.001 or less. The value of z being within the required range means that the Mn content is within the required range. By setting the value of z to a required value or more, it becomes easier to form Li2MnO3, increasing the number of Li vacancies and promoting the migration of Ni and Co to the Li layer. By setting the value of z to a required value or less, the increase in the formation of Li2MnO3 can be suppressed, which can prevent a decrease in charge capacity due to an excessive increase in Li vacancies.

[0038] In the general formula, the value of w is not particularly limited as long as it is within the range of 0≦w≦0.1, and may be, for example, 0.001 or more, 0.0012 or more, 0.0015 or more, 0.0017 or more, 0.002 or more, 0.0022 or more, 0.0025 or more, 0.0027 or more, 0.003 or more, 0.0032 or more, 0.0035 or more, 0.0037 or more, 0.004 or more, 0.0042 or more. above,0.0045 or more,0.0047 or more,0.005 or more,0.0052 or more,0.0055 or more,0.0057 or more,0.006 or more,0.0062 or more,0.0065 or more,0.0067 or more,0.007 or more,0.0072 or more,0.0075 or more,0.0077 or more,0.008 or more,0.0082 or more,0.0085 or more,0.0087 or more,0 .009 or more, 0.0092 or more, 0.0095 or more, 0.0097 or more, 0.01 or more, 0.012 or more, 0.015 or more, 0.017 or more, 0.02 or more, 0.022 or more, 0.025 or more, 0.027 or more, 0.03 or more, 0.032 or more, 0.035 or more, 0.037 or more, 0.04 or more, 0.042 or more, 0.045 or more, 0.047 or more, 0.0 It is preferable that the ratio is 5 or more, 0.052 or more, 0.055 or more, 0.057 or more, 0.06 or more, 0.062 or more, 0.065 or more, 0.067 or more, 0.07 or more, 0.072 or more, 0.075 or more, 0.077 or more, 0.082 or more, 0.085 or more, 0.087 or more, 0.09 or more, 0.092 or more, 0.095 or more, or 0.097 or more.On the other hand, the values ​​of w are 0.097 or less, 0.095 or less, 0.092 or less, 0.09 or less, 0.087 or less, 0.085 or less, 0.082 or less, 0.08 or less, 0.077 or less, 0.075 or less, 0.072 or less, 0.07 or less, 0.067 or less, 0.065 or less, 0.062 or less, 0.06 or less, 0.057 or less, 0.055 or less, 0. 052 or less, 0.05 or less, 0.047 or less, 0.045 or less, 0.042 or less, 0.04 or less, 0.037 or less, 0.035 or less, 0.032 or less, 0.03 or less, 0. 027 or less, 0.025 or less, 0.022 or less, 0.02 or less, 0.017 or less, 0.015 or less, 0.012 or less, 0.01 or less, 0.0097 or less, 0.0095 or less , 0.0092 or less, 0.009 or less, 0.0087 or less, 0.0085 or less, 0.0082 or less, 0.008 or less, 0.0077 or less, 0.0075 or less, 0.0072 less than or equal to 0.007, less than or equal to 0.0067, less than or equal to 0.0065, less than or equal to 0.0062, less than or equal to 0.006, less than or equal to 0.0057, less than or equal to 0.0055, less than or equal to 0.0052, 0.00 It is preferable that w is 5 or less, 0.0047 or less, 0.0045 or less, 0.0042 or less, 0.004 or less, 0.0037 or less, 0.0035 or less, 0.0032 or less, 0.003 or less, 0.0027 or less, 0.0025 or less, 0.0022 or less, 0.002 or less, 0.0017 or less, 0.0015 or less, 0.0012 or less, or 0.001 or less. The value of w being within the required range means that the content of element M is within the required range. By setting the value of w to a required value or more, the effect of adding element M can be expressed. By setting the value of w to a required value or less, the content of Ni, Co, and Mn can be guaranteed, and the battery performance including the high charging capacity due to these can be maintained.

[0039] In the formula, the element M is not particularly limited as long as it is one or more elements other than Li, Ni, Co, Mn, and O, and examples thereof include Al, Ti, Mg, Zn, Nb, W, Mo, Sb, V, Cr, Ca, Fe, Ga, Sr, Y, Ru, In, Sn, Ta, Bi, Zr, and B. The type of element M may be selected according to the purpose of addition. When the element M contains multiple elements, the value of w represents the total amount of the multiple elements.

[0040] Among these, it is preferable to use Al as the element M. When Al is used as the element M, Al is fixed at a specific site to form a stable structure. This allows Li + It becomes difficult to move, and Li + and Ni 2+ Cation mixing with Li2MnO3 is suppressed, and a higher temperature is required to release oxygen from some parts of the composite oxide. Therefore, when the composite oxide contains Al, the peak due to oxygen release occurring between about 200 and 250°C in the DTG curve becomes broader than when it does not contain Li2MnO3, making it easier to suppress thermal runaway.

[0041] The content of Al only in w AlThe value of is not particularly limited, but may be, for example, 0 or more, 0.001 or more, 0.0012 or more, 0.0015 or more, 0.0017 or more, 0.002 or more, 0.0022 or more, 0.0025 or more, 0.0027 or more, 0.003 or more, 0.0032 or more, 0.0035 or more, 0.0037 or more, 0.004 or more, 0.0042 or more, 0.0045 or more, or 0. 0047 or more, 0.005 or more, 0.0052 or more, 0.0055 or more, 0.0057 or more, 0.006 or more, 0.0062 or more, 0.0065 or more, 0.0067 or more, 0.007 or more, 0.0072 or more, 0.0075 or more, 0.0077 or more, 0.008 or more, 0.0082 or more, 0.0085 or more, 0.0087 or more, 0.009 or more, 0. 0092 or more, 0.0095 or more, 0.0097 or more, 0.01 or more, 0.012 or more, 0.015 or more, 0.017 or more, 0.02 or more, 0.022 or more, 0.025 or more, 0.027 or more, 0.03 or more, 0.032 or more, 0.035 or more, 0.037 or more, 0.04 or more, 0.042 or more, 0.045 or more, 0.047 or more, 0.05 or more, 0 It is preferable that the ratio is 0.052 or more, 0.055 or more, 0.057 or more, 0.06 or more, 0.062 or more, 0.065 or more, 0.067 or more, 0.07 or more, 0.072 or more, 0.075 or more, 0.077 or more, 0.082 or more, 0.085 or more, 0.087 or more, 0.09 or more, 0.092 or more, 0.095 or more, or 0.097 or more.On the other hand, the value of w is 0.1 or less, 0.097 or less, 0.095 or less, 0.092 or less, 0.09 or less, 0.087 or less, 0.085 or less, 0.082 or less, 0.08 or less, 0.077 or less, 0.075 or less, 0.072 or less, 0.07 or less, 0.067 or less, 0.065 or less, 0.062 or less, 0.06 or less, 0.057 or less, 0.055 or less Below, 0.052 or less, 0.05 or less, 0.047 or less, 0.045 or less, 0.042 or less, 0.04 or less, 0.037 or less, 0.035 or less, 0.032 or less, 0.03 or less Lower, 0.027 or less, 0.025 or less, 0.022 or less, 0.02 or less, 0.017 or less, 0.015 or less, 0.012 or less, 0.01 or less, 0.0097 or less, 0.009 5 or less, 0.0092 or less, 0.009 or less, 0.0087 or less, 0.0085 or less, 0.0082 or less, 0.008 or less, 0.0077 or less, 0.0075 or less, 0.0 072 or less, 0.007 or less, 0.0067 or less, 0.0065 or less, 0.0062 or less, 0.006 or less, 0.0057 or less, 0.0055 or less, 0.0052 or less, 0. It is preferable that the molecular weight is 0.005 or less, 0.0047 or less, 0.0045 or less, 0.0042 or less, 0.004 or less, 0.0037 or less, 0.0035 or less, 0.0032 or less, 0.003 or less, 0.0027 or less, 0.0025 or less, 0.0022 or less, 0.002 or less, 0.0017 or less, 0.0015 or less, 0.0012 or less, or 0.001 or less. Al The value of w being within the required range means that the Al content is within the required range. Al By setting the value of w to a required value or more, the peak due to oxygen release occurring between about 200 and 250°C in the DTG curve obtained by adding Al can be broadened, and the effect of suppressing thermal runaway can be exerted. Al By keeping the value of at most a required value, the contents of Ni, Co, and Mn can be ensured, and the battery performance including a high charge capacity provided by these elements can be maintained.

[0042] In the general formula, the value of z+w is not particularly limited as long as it is within the range of 0≦z≦0.4, 0≦w≦0.1. For example, the value may be 0 or more, more than 0, 0.001 or more, 0.0015 or more, 0.002 or more, 0.0025 or more, 0.003 or more, 0.0035 or more, 0.004 or more, 0.0045 or more, 0.005 or more, 0.0055 or more, 0.006 or more, 0.0065 or more, 0.007 or more, 0.0075 or more, 0.008 or more, 0.0085 or more, 0.009 or more, 0.0095 or more, 0.01 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0 .035 or more, 0.04 or more, 0.045 or more, 0.05 or more, 0.055 or more, 0.06 or more, 0.065 or more, 0.07 or more, 0.075 or more, 0.08 or more, 0.085 or more, 0.09 or more, 0.095 or more, 0.1 or more, 0.102 or more, 0.105 or more, 0.107 0.11 or more, 0.112 or more, 0.115 or more, 0.117 or more, 0.12 or more, 0.122 or more, 0.125 or more, 0.127 or more, 0.13 or more, 0.132 or more, 0.135 or more, 0.137 or more, 0.14 or more, 0.142 or more, 0.145 or more, 0.147 or more Up, 0.15 or more, 0.152 or more, 0.155 or more, 0.157 or more, 0.16 or more, 0.162 or more, 0.165 or more, 0.167 or more, 0.17 or more, 0.172 or more, 0.175 or more, 0.177 or more, 0.18 or more, 0.182 or more, 0.185 or more, 0.187 or more, 0.19 or more, 0.192 or more, 0.195 or more, 0.197 or more, 0.2 or more, 0.202 or more, 0.205 or more, 0.207 or more, 0.21 or more, 0.212 or more, 0.215 or more, 0.217 or more, 0.22 or more, 0.222 or more, 0.225 or more, 0.227 or more, 0.23 or more, 0.232 or more, 0.235 or more, 0.237 or more, 0.24 or more, 0.242 or more, 0.245 or more, 0.247 or more, 0.25 or more, 0.252 or more, 0.255 or more, 0.257 or more, 0.26 or more, 0.262 or more, 0.265 or more, 0.267 or more, 0.27 or more, 0.272 or more, 0.275 or more, 0.277 or more, 0.28 or more, 0.282 or more, 0.285 or more, 0.287 or more, 0.29 or more, 0.292 or more, 0.295 or more, 0.297 or more, 0.3 or more, 0.302 or more, 0.305 or more, 0.307 or more, 0.31 or more, 0.312 or more, 0.315 or more, 0.317 or more, 0.32 or more, 0.322 or more, 0.325 or more, 0.327 or more, 0.33 or more, 0.332 or more, 0.335 or more, 0.337 or more, 0.34 or more, 0.342 or more, 0.345 or more, 0.347 or more, 0.35 or more, 0.352 or more, 0.355 or more, 0.35 7 or more, 0.36 or more, 0.362 or more, 0.365 or more, 0.367 or more, 0.37 or more, 0.372 or more, 0.375 or more, 0.377 or more, 0.38 or more, 0.382 or more, 0.385 or more, 0.387 or more, 0.39 or more, 0.392 or more, 0.395 or more, 0.397 or more, 0.4 or more, 0.402 or more, 0.405 or more ,0.407 or more,0.41 or more,0.412 or more,0.415 or more,0.417 or more,0.42 or more,0.422 or more,0.425 or more,0.427 or more,0.43 or more,0.432 or more,0.435 or more,0.437 or more,0.44 or more,0.442 or more,0.445 or more,0.447 or more,0.45 or more,0.452 or more,0 It is preferable that the refractive index is 0.455 or more, 0.457 or more, 0.46 or more, 0.462 or more, 0.465 or more, 0.467 or more, 0.47 or more, 0.472 or more, 0.475 or more, 0.477 or more, 0.482 or more, 0.485 or more, 0.487 or more, 0.49 or more, 0.492 or more, 0.495 or more, or 0.497 or more. On the other hand, the values ​​of z+w are 0.5 or less, 0.497 or less, 0.495 or less, 0.492 or less, 0.49 or less, 0.487 or less, 0.485 or less, 0.482 or less, 0.48 or less, 0.477 or less, 0.475 or less, 0.472 or less, 0.467 or less, 0.465 or less, 0.462 or less, 0.46 or less, 0.457 or less, 0.455 or less, 0.452 or less, 0.45 or less, 0.447 or less, 0.445 or less, 0.442 or less, 0.44 or less, 0. 437 or less, 0.435 or less, 0.432 or less, 0.43 or less, 0.427 or less, 0.425 or less, 0.422 or less, 0.42 or less, 0.417 or less, 0.415 or less, 0.412 or less, 0.41 or less, 0.407 or less, 0 .405 or less, 0.402 or less, 0.4 or less, 0.397 or less, 0.395 or less, 0.392 or less, 0.39 or less, 0.387 or less, 0.385 or less, 0.382 or less, 0.38 or less, 0.377 or less, 0.375 or less, 0.372 or less, 0.367 or less, 0.365 or less, 0.362 or less, 0.36 or less, 0.357 or less, 0.355 or less, 0.352 or less, 0.35 or less, 0.347 or less, 0.345 or less, 0.342 or less, 0.34 or less, 0.337 or less, 0.335 or less, 0.332 or less, 0.33 or less, 0.327 or less, 0.325 or less, 0.322 or less, 0.32 or less, 0.317 or less, 0.315 or less, 0.312 or less, 0.31 or less, 0.307 or less, 0.305 or less, 0.302 or less, 0.3 or less, 0.297 or less, 0.295 or less, 0.292 or less, 0. 29 or less, 0.287 or less, 0.285 or less, 0.282 or less, 0.28 or less, 0.277 or less, 0.275 or less, 0.272 or less, 0.27 or less, 0.267 or less, 0.265 or less, 0.26 or less, 0.257 or less, 0.255 or less, 0.252 or less, 0.25 or less, 0.247 or less, 0.245 or less, 0.242 or less, 0.24 or less, 0.237 or less, 0.235 or less, 0.232 or less, 0.23 or less, 0.227 or less, 0.225 or less, 0.222 or less, 0.22 or less, 0.217 or less, 0.215 or less, 0.212 or less, 0.21 or less, 0.20 7 or less, 0.205 or less, 0.202 or less, 0.2 or less, 0.197 or less, 0.195 or less, 0.192 or less, 0.19 or less, 0.187 or less, 0.185 or less, 0.182 or less, 0.18 or less, 0.177 or less, 0.175 or less, 0.172 or less, 0.17 or less, 0.167 or less, 0.165 or less, 0.162 or less, 0.16 or less, 0.155 or less, 0.152 or less, 0.15 or less, 0.147 or less, 0.145 or less, 0.142 or less, 0.14 or less, 0.137 or less, 0.135 or less, 0.132 or less, 0.13 or less, 0.127 or less, 0.125 or less 0.122 or less, 0.12 or less, 0.117 or less, 0.115 or less, 0.112 or less, 0.11 or less, 0.107 or less, 0.105 or less, 0.102 or less, 0.1 or less, 0.095 or less, 0.09 or less, 0.085 or less, 0.08 or less, 0.075 or less, 0.07 or less, 0.065 or less, 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.015 or less, 0.01 or less, 0.0095 or less, 0.009 or less, 0.0085 or less, 0.008 or less, 0.It is preferable that the value is 0075 or less, 0.007 or less, 0.0065 or less, 0.006 or less, 0.0055 or less, 0.005 or less, 0.0045 or less, 0.004 or less, 0.0035 or less, 0.003 or less, 0.0025 or less, 0.002 or less, 0.0015 or less, or 0.001 or less.

[0043] The form of the composite oxide is not particularly limited, and may be, for example, particulate. When particulate is used, the particles may be aggregated as primary particles to form secondary particles, may exist as primary particles, or may be a mixture of secondary particles and primary particles. As long as the primary particles have the same particle size distribution, the temperature at which oxygen is released from the composite oxide does not change significantly regardless of the state in which they exist.

[0044] The average particle size of the primary particles of the composite oxide is not particularly limited, but is preferably, for example, 80 nm or more, 100 nm or more, 120 nm or more, 150 nm or more, 170 nm or more, 200 nm or more, 250 nm or more, 300 nm or more, 350 nm or more, 400 nm or more, or 450 nm or more. By making the average particle size of the composite oxide a required value or more, the oxygen release temperature can be increased. On the other hand, the average particle size of the primary particles is preferably 15 μm or less, 14.5 μm or less, 14 μm or less, 13.5 μm or less, 13 μm or less, 12.5 μm or less, 12 μm or less, 11.5 μm or less, 11 μm or less, 10.5 μm or less, 10 μm or less, 9.5 μm or less, 9 μm or less, 8.5 μm or less, 8 μm or less, 7.5 μm or less, 7 μm or less, 6.5 μm or less, 6 μm or less, 5.5 μm or less, 5 μm or less, or 4.5 μm or less. By having the average particle size of the primary particles be equal to or less than the required value, the energy density can be increased, and particle destruction and deterioration of rate characteristics due to cycles can be suppressed. The average particle size of the primary particles of the composite oxide is calculated by observing electron micrographs at 3000 to 20000 times magnification using a field emission scanning electron microscope (JSM-7100F: manufactured by JEOL Ltd.) with an acceleration voltage of 10 kV. Specifically, a field of view in which 100 or more primary particles whose outlines can be confirmed are randomly selected, and an electron micrograph is obtained for all particles whose outlines can be confirmed among the particles contained in that field of view by changing the magnification within the above-mentioned range as necessary. Next, the sphere equivalent diameter is calculated for the electron micrograph using image processing software (e.g., ImageJ, etc.) to be the particle size of the primary particles.

[0045] The average particle size (D50) of the composite oxide is not particularly limited, but is preferably, for example, 80 nm or more, 100 nm or more, 120 nm or more, 150 nm or more, 170 nm or more, 200 nm or more, 250 nm or more, 300 nm or more, 350 nm or more, 400 nm or more, or 450 nm or more. By having D50 equal to or greater than a required value, the oxygen release temperature can be increased, and the electrode density can be improved. On the other hand, for D50, 25μm or less, 24.5μm or less, 24μm or less, 23.5μm or less, 23μm or less, 22.5μm or less, 22μm or less, 21.5μm or less, 21μm or less, 20.5μm or less, 20μm or less, 19.5μm or less, 19μm or less, 18.5μm or less, 18μm or less, 17.5μm or less, 17μm or less, 16.5μm or less, 16μm or less, 15.5μm or less, 15 It is preferable that the D50 of the complex oxide is less than or equal to a required value, and the energy density of the non-aqueous electrolyte secondary battery using the complex oxide can be increased, and particle destruction and deterioration of rate characteristics due to cycles can be suppressed. Note that D50 is measured by a wet laser method using a laser particle size distribution measuring device (Microtrac HRA, manufactured by Nikkiso Co., Ltd.) on a volume basis.

[0046] [DTG curve] The DTG curve of the composite oxide of the present disclosure was obtained when the composite oxide was charged by the charging method described below and the temperature was increased from 50° C. to 600° C. at a rate of 5° C. / min.

[0047] The differential thermogravimetric curve thus obtained is fitted using a log-normal distribution function to separate the peaks, and the temperature and weight loss rate (oxygen release rate) at the peak top of each peak are calculated.

[0048] Specifically, a thermal analysis weight curve is obtained using a thermogravimetric differential thermal analyzer (TG-DTA) (DTG-60H, manufactured by Shimadzu Corporation) according to the method described below, and then the first and second peaks are analyzed.

[0049] (Sample preparation) According to the method described below, a 2032 type coin cell with a lithium counter electrode was prepared, and in an environment of 25°C, it was charged at a constant current of 0.3C to 4.30V, and then charged at a constant voltage until the current value reached 0.05C. After that, it was left to rest for 20 minutes after charging was completed, and discharged at a constant current of 0.3C to 2.50V, and then discharged at a constant current of 0.1C, and then left to rest for 20 minutes. This charging and discharging was repeated twice. Next, it was charged at a constant current of 0.3C to 4.30V, and then charged at a constant voltage until the current value reached 0.05C, and then left to rest for 20 minutes after charging was completed.

[0050] The charged coin cell is disassembled in a glove box (dew point: -70°C or less) while being careful not to short circuit, and the positive electrode is separated. The separated positive electrode is washed with dimethyl carbonate (DMC) for 10 minutes and dried under vacuum in a side box. Then, in the same glove box, the positive electrode mixture is scraped off from the Al foil using a spatula. 15 mg of the obtained powder of the positive electrode mixture is filled into an Al TG measurement container, the lid is put on, and it is sealed using a crimping machine.

[0051] The Al measurement container thus obtained is taken out of the glove box and placed on the measurement side balance of the TG-DTA apparatus.

[0052] (TG-DTA measurement) Reference: Pt container filled with 15-20 mg of Al2O3 Maximum temperature: 600℃ Heating rate: (1) 25℃ (room temperature) to 50℃: 1℃ / min (2) 50℃~600℃: 5℃ / min Measurement environment: N2 gas atmosphere (200ml / min)

[0053] Just before the measurement, a small hole is opened in the lid of the sealed aluminum measurement container in the TG-DTA device, which is in a N2 gas atmosphere, and then the temperature is increased. By using this method, the measurement target, the positive electrode composite powder, can be measured without being exposed to the air atmosphere.

[0054] Based on the obtained results, a DTG curve is created with the horizontal axis representing temperature and the vertical axis representing the value obtained by differentiating the weight change (TG) with respect to time (differential thermogravimetric DTG, which means the weight loss rate, and corresponds to the oxygen release rate of the complex oxide in the range of 150 to 350°C).

[0055] Among the peaks having a peak top at 150 to 350°C in this DTG curve, the peak whose differential thermogravimetry peak top shows the maximum value is defined as the first peak. The value of the differential thermogravimetry at the peak top is defined as the oxygen release rate (% / min). Furthermore, among the peaks whose peak tops are at a temperature 20°C or more away from the temperature showing the peak top of the first peak, the peak whose differential thermogravimetry peak top value shows the maximum value is defined as the second peak.

[0056] The value of the differential thermogravimetry at the peak top of the first peak relative to the value of the differential thermogravimetry at the peak top of the second peak is then calculated.

[0057] [First peak] The first peak is a peak that, when the DTG curve obtained as described above is separated into multiple peaks, exhibits a maximum value of the differential thermogravimetry at the peak top in the temperature range of 150°C or higher and 350°C or lower.

[0058] The value of the differential thermogravimetry at the peak top of the first peak is not particularly limited, but is preferably, for example, 3% or less, 2.9% or less, 2.8% or less, 2.7% or less, 2.6% or less, 2.5% or less, 2.4% or less, 2.3% or less, 2.2% or less, 2.1% or less, or 2% or less.

[0059] [Second peak] The second peak is a peak that has a maximum value of the differential thermogravimetry at its peak top among the peaks that have a peak top at a temperature that is 20° C. or more away from the temperature at which the first peak has its peak top.

[0060] The temperature at which the second peak shows its top may be at least 20° C. higher than the temperature at which the first peak shows its top, and there is no limitation on this. That is, the temperature at which the second peak shows its top may be at least 20° C. higher or lower than the temperature at which the first peak shows its top.

[0061] The temperature showing the peak top of the second peak is preferably away from the temperature showing the peak top of the first peak, for example, by 21°C or more, 22°C or more, 23°C or more, 24°C or more, 25°C or more, 26°C or more, 27°C or more, 28°C or more, 29°C or more, 30°C or more, 31°C or more, 32°C or more, 33°C or more, 34°C or more, 35°C or more, 36°C or more, 37°C or more, 38°C or more, 39°C or more, or 40°C or more. On the other hand, the temperature at which the second peak shows its peak top may be, for example, 160°C or less, 155°C or less, 150°C or less, 145°C or less, 140°C or less, 135°C or less, 130°C or less, 125°C or less, 120°C or less, 115°C or less, 110°C or less, 105°C or less, 100°C or less, 95°C or less, 90°C or less, 85°C or less, 80°C or less, 75°C or less, or 60°C or less away from the temperature at which the first peak shows its peak top.

[0062] [Ratio of differential thermogravimetry values] In the positive electrode active material of the present disclosure, the differential thermogravimetry value of the first peak relative to the differential thermogravimetry value of the second peak (differential thermogravimetry of the first peak / differential thermogravimetry of the second peak) is not particularly limited as long as it is 1 or more and 9 or less, and may be, for example, 8.9 or less, 8.8 or less, 8.7 or less, 8.6 or less, 8.5 or less, 8.4 or less, 8.3 or less, 8.2 or less, 8.1 or less, 8 or less, 7.9 or less, 7.8 or less, 7.7 or less, 7.6 or less, 7.5 or less, 7.4 or less, 7.3 or less, 7.2 or less, 7.1 or less, 7 or less, 6.9 or less, 6.8 or less, 6.7 or less, 6.6 or less, 6.5 or less, 6.4 or less, 6.3 or less, 6.2 or less, 6.1 or less , 6 or less, 5.9 or less, 5.8 or less, 5.7 or less, 5.6 or less, 5.5 or less, 5.4 or less, 5.3 or less, 5.2 or less, 5.1 or less, 5 or less, 4.9 or less, 4.8 or less, 4.7 or less, 4.6 or less, 4.5 or less, 4.4 or less, 4.3 or less, 4.2 or less, 4.1 or less, 4 or less, 3.9 or less, 3.8 or less, 3.7 or less, 3.6 or less, 3.5 or less, 3.4 or less, 3.3 or less, 3.2 or less, 3.1 or less, 3 or less, 2.9 or less, 2.8 or less, 2.7 or less, 2.6 or less, 2.5 or less, 2.4 or less, 2.3 or less, 2.2 or less, 2.1 or less, 2 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less. On the other hand, the differential thermogravimetry value of the first peak relative to the differential thermogravimetry value of the second peak may be 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, 1.8 or more, or 1.9 or more.

[0063] <Method of manufacturing positive electrode active material for non-aqueous electrolyte secondary battery> The positive electrode active material for a non-aqueous electrolyte secondary battery according to the embodiment of the present disclosure can be produced, for example, by carrying out the following steps in this order. Note that in the following, a method for producing a composite oxide containing 30 mol % or more of Ni among elements other than Li is shown as an example, and other composite oxides are produced according to conventional methods.

[0064] Step 1: A precursor complex compound containing at least a transition metal is synthesized, and the precursor complex compound is mixed with a lithium compound to prepare a mixture. Step 2: The mixture prepared in step 1 is fired. Step 3: If necessary, the composite oxide obtained by firing in step 2 is subjected to a water washing treatment. Step 4: If necessary, the composite oxide obtained in step 2 or 3 is subjected to a surface treatment. Step 5: If necessary, the conditions of steps 1 to 3 are changed to mix a plurality of types of composite oxides having different primary particle sizes, average particle sizes, etc.

[0065] [Process 1] First, a precursor composite compound is synthesized as an aggregate of primary particles containing at least a transition metal. The method for synthesizing the precursor composite compound is not particularly limited, and for example, a method can be used in which an aqueous solution containing an aqueous solution of a transition metal and various aqueous solutions of compounds containing other elements according to the composition of the target composite oxide is dropped into a reaction tank in which an alkaline aqueous solution such as an aqueous solution of sodium hydroxide or an ammonia solution is stirred as a mother liquid, and while dropping sodium hydroxide, etc., the pH is monitored and controlled to be in an appropriate range, and co-precipitated by a wet reaction to obtain, for example, a hydroxide, an oxide obtained by calcining the hydroxide, a carbonate, etc.

[0066] In the synthesis reaction, it is preferable to prepare an aqueous alkali solution as a mother liquid, and then to make the reaction tank into a nitrogen atmosphere using an inert gas, or preferably nitrogen gas from an industrial viewpoint, to reduce the oxygen concentration in the reaction tank system and in the solution as much as possible. If the oxygen concentration is too high, there is a risk that the coprecipitated hydroxide may be over-oxidized by a predetermined amount or more of remaining oxygen, or that the formation of aggregates by crystallization may be hindered.

[0067] The aqueous solution of the transition metal is not particularly limited, but for example, an acidic aqueous solution is preferably used, and in the case of a nickel compound, it is more preferable to use an aqueous sulfuric acid solution such as an aqueous nickel sulfate solution. In addition, one or more kinds of aqueous solutions of the transition metal can be used.

[0068] The nickel compound is not particularly limited, but for example, one or more selected from nickel sulfate, nickel oxide, nickel hydroxide, nickel nitrate, nickel carbonate, nickel chloride, nickel iodide, metallic nickel, and the like can be used.

[0069] The cobalt compound is not particularly limited, but may be at least one selected from, for example, cobalt sulfate, cobalt oxide, cobalt hydroxide, cobalt nitrate, cobalt carbonate, cobalt chloride, cobalt iodide, and metallic cobalt.

[0070] The manganese compound is not particularly limited, but for example, one or more compounds selected from manganese sulfate, manganese oxide, manganese hydroxide, manganese nitrate, manganese carbonate, manganese chloride, manganese iodide, and manganese metal can be used.

[0071] The aluminum compound is not particularly limited, but examples thereof include aluminum sulfate, aluminum oxide, aluminum hydroxide, aluminum nitrate, aluminum carbonate, aluminum chloride, aluminum iodide, sodium aluminate, and metallic aluminum.

[0072] The titanium compound is not particularly limited, but for example, one or more compounds selected from titanyl sulfate, titanium oxide, titanium hydroxide, titanium nitrate, titanium carbonate, titanium chloride, titanium iodide, and metallic titanium can be used.

[0073] The iron compound is not particularly limited, but for example, one or more compounds selected from iron sulfate, iron oxide, iron hydroxide, iron nitrate, iron carbonate, iron chloride, iron iodide, metallic iron, and the like can be used.

[0074] The niobium compound is not particularly limited, but for example, one or more compounds selected from niobium oxide, niobium chloride, lithium niobate, niobium iodide, and the like can be used.

[0075] The tungsten compound is not particularly limited, but for example, one or more compounds selected from tungsten oxide, sodium tungstate, ammonium paratungstate, tungsten hexacarbonyl, tungsten sulfide, and the like can be used.

[0076] The magnesium compound is not particularly limited, but for example, one or more compounds selected from magnesium sulfate, magnesium oxide, magnesium hydroxide, magnesium nitrate, magnesium carbonate, magnesium chloride, magnesium iodide, and metallic magnesium can be used.

[0077] The zinc compound is not particularly limited, but for example, one or more compounds selected from zinc sulfate, zinc oxide, zinc hydroxide, zinc nitrate, zinc carbonate, zinc chloride, zinc iodide, and zinc metal can be used.

[0078] As for the other elements, one or more selected from sulfates, oxides, hydroxides, nitrates, carbonates, chlorides, iodides, metals, and the like can be used.

[0079] The mixing ratio of each compound may be adjusted so that the amount of each element is in a desired ratio, taking into consideration the composition of the target composite oxide.

[0080] The appropriate pH range for synthesizing the precursor complex compound is not particularly limited and can be determined so as to obtain the desired secondary particle size and shape, such as the degree of coarseness and density, and is generally in the range of about 10 to 13.

[0081] The precursor complex compound obtained by the wet reaction is preferably subjected to a washing treatment, dehydrated, and then dried.

[0082] By subjecting the precursor composite compound to a washing treatment, impurities such as sulfate radicals, carbonate radicals, and sodium that are incorporated into the aggregated particles during the reaction or that are attached to the surface layer can be washed away. For the washing treatment, a Nutsche washing method using a Buchner funnel can be used if the amount is small, or a method in which the suspension after the reaction is sent to a press filter for washing with water and dehydration can be used. In addition, for example, pure water, an aqueous sodium hydroxide solution, an aqueous sodium carbonate solution, etc. can be used in the washing treatment, but it is preferable to use pure water from an industrial perspective. However, if there is a large amount of residual sulfate radicals, an aqueous sodium hydroxide solution with a pH controlled according to the amount of residual sulfate radicals may be used.

[0083] Next, the precursor composite compound thus synthesized and a lithium compound are mixed in a predetermined ratio to prepare a mixture. The mixing may be a solvent-based mixing in which the precursor composite compound and the lithium compound are each made into a solution such as an aqueous solution and these solutions are mixed in a predetermined ratio, or a non-solvent-based mixing in which a powder of the precursor composite compound and a powder of the lithium compound are weighed out to have a predetermined ratio and mixed in a dry state.

[0084] The lithium compound is not particularly limited, and various lithium salts can be used. Specifically, the lithium compound can be one or more selected from anhydrous lithium hydroxide, lithium hydroxide hydrate, lithium nitrate, lithium carbonate, lithium acetate, lithium bromide, lithium chloride, lithium citrate, lithium fluoride, lithium iodide, lithium lactate, lithium oxalate, lithium phosphate, lithium pyruvate, lithium sulfate, lithium oxide, etc. Among these, it is preferable to use one or more selected from anhydrous lithium hydroxide and lithium hydroxide hydrate.

[0085] The blending ratio of the lithium compound and the precursor composite compound is not particularly limited, but may be appropriately adjusted so that the amount of lithium and the total amount of each element are in a desired ratio, taking into consideration the composition of the target composite oxide.

[0086] [Process 2] As described above, when producing a composite oxide containing at least a transition metal, a lithiation reaction and crystal growth occur during firing, and the lithiation reaction requires a certain oxygen partial pressure. A composite oxide containing lithium is obtained by the lithiation reaction. Then, the temperature is raised to a predetermined temperature to promote crystal growth.

[0087] The maximum temperature of the mixture during firing is preferably 650° C. to 1100° C., 670° C. to 1000° C., or 700° C. to 980° C. Furthermore, the firing time at the maximum temperature is preferably 1 to 24 hours, 1 to 20 hours, 1 to 15 hours, 1 to 10 hours, 2 to 9 hours, or 3 to 8 hours. By setting the firing temperature to be equal to or higher than the melting point of the lithium compound in the mixture and the maximum temperature and time at which the lithium-containing composite oxide undergoes desired crystal growth or particle growth, the desired composite compound can be obtained.

[0088] In general, the calcination is carried out by weighing out the lithium compound, the precursor composite compound, and optionally the compound of element M, mixing them in a mixer, and filling the resulting mixed powder in a container such as a crucible or a sagger. However, particularly in the lithium conversion reaction, it becomes difficult to exhaust the generated gas to the outside and to diffuse the required oxygen concentration, especially toward the bottom of the container where the mixed powder is filled. As a result, it becomes difficult to control the uniformity of the reaction and the primary particle size.

[0089] Therefore, when producing the composite oxide according to the embodiment of the present disclosure, it is preferable to use a method in which pre-calcination is first performed under the following specified conditions in step 2, and then main calcination is performed under the specified conditions. However, pre-calcination is not an essential step.

[0090] In the pre-firing in step 2, it is preferable to adopt a firing method that particularly promotes the lithiation reaction. Specifically, a method can be mentioned in which the mixture is made more susceptible to heat, gas generated from the lithium compound is easily discharged, and gas with a high oxygen partial pressure is diffused within the mixture (inside the particles). For example, it is possible to achieve the desired characteristics by pre-firing a smaller amount of the mixture.

[0091] In step 2, the mixture can be pre-fired by filling it into a sagger or crucible and firing it in a stationary furnace, roller hearth kiln, or pusher furnace, but a rotary kiln in which the mixture is fired while being fluidized can also be used.

[0092] The maximum temperature of the mixture to be pre-baked is not particularly limited, and is preferably adjusted according to the type of lithium compound used in the preparation of the mixture. This allows the precursor composite compound and the lithium compound in the mixture to react reliably, the lithiation reaction to proceed reliably and uniformly, and no heterogeneous phases to be generated, thereby making it possible to obtain the desired composite oxide.

[0093] The atmosphere for the preliminary calcination is not particularly limited, and may be an oxidizing atmosphere in which the lithiation reaction proceeds reliably and uniformly. For example, it is preferable to use a decarbonated oxidizing gas atmosphere with a carbon dioxide gas concentration of 30 ppm or less, or an oxygen atmosphere with an oxygen concentration of 80 vol% or more, 90 vol% or more.

[0094] The pre-baking time is not particularly limited as long as the lithium addition reaction proceeds reliably and uniformly, and is preferably 1 to 10 hours, and more preferably 2 to 8 hours.

[0095] The pre-calcined mixture is then subjected to a main calcination at a higher temperature to promote crystal growth and particle growth. At this time, it is necessary to ensure that the crystal growth proceeds uniformly to obtain a composite oxide having a desired crystal structure.

[0096] The atmosphere for the main firing is not particularly limited, and may be any atmosphere that ensures reliable and uniform crystal growth, has an oxygen partial pressure that does not reduce the transition metal contained in the mixture to be fired, and preferably has a low moisture content and carbon dioxide gas concentration. For example, it is preferable to use a decarbonated oxidizing gas atmosphere with a carbon dioxide gas concentration of 30 ppm or less, or an oxygen atmosphere with an oxygen concentration of preferably 80 vol% or more, 90 vol% or more.

[0097] The temperature of the main firing is not particularly limited as long as it is higher than the temperature of the preliminary firing, and can be adjusted according to the composition of the composite oxide to be obtained. For example, it is preferable to adjust the maximum temperature to 700°C to 1100°C, 710°C to 1000°C, or 720°C to 980°C. By setting the maximum temperature within the required range, a composite oxide having a desired crystal structure with reduced unreacted components can be obtained, and the deterioration of the battery characteristics of a non-aqueous electrolyte secondary battery using the obtained composite oxide as a positive electrode can be prevented. In addition, when obtaining a composite oxide with a Ni content of 20 mol% to 80 mol% of elements other than Li, it is preferable to fire the mixture at a maximum temperature not exceeding 1100°C.

[0098] The time for the main firing is not particularly limited as long as it is long enough to form a composite oxide having a desired crystal structure, and is preferably 1 to 15 hours, 2 to 12 hours, or 2 to 10 hours, for example.

[0099] [Step 3] The composite oxide obtained in step 2 may contain impurities such as unreacted lithium compounds and lithium compounds that appear on the particle surface due to the crystal structure during the firing step. Therefore, in order to remove or reduce these impurities, the composite oxide may be washed with water and heat-treated, for example. Note that step 3 is not an essential component.

[0100] [Step 4] By adding and mixing a predetermined element compound to the composite oxide obtained in step 2 or 3 and subjecting it to heat treatment, the surfaces of the primary particles and / or secondary particles of the composite oxide can be surface-treated with a compound of lithium and the added element, and effects such as reducing the amount of lithium compounds remaining on the particle surface, improving lithium ion conductivity, and reducing reaction resistance can be obtained. Note that step 4 is not an essential component.

[0101] The element compound added for the above-mentioned surface treatment can be selected from, for example, aluminum compounds, boron compounds, tungsten compounds, manganese compounds, cobalt compounds, phosphorus compounds, niobium compounds, strontium compounds, antimony compounds, zirconium compounds, titanium compounds, and the like, and one or more of them can be used.

[0102] [Step 5] In cases where the composite oxide obtained in any of steps 2 to 4 does not have multiple specific peaks as described above by itself, or where it satisfies specific requirements for specific peaks but it is desired to further enhance the effect of suppressing thermal runaway, the conditions for producing the composite oxide (conditions in steps 1 to 4) are changed to mix multiple types of composite oxides with different primary particle sizes or average particle sizes. Note that, in cases where the composite oxide obtained in any of steps 2 to 4 satisfies specific requirements for specific peaks by itself, step 5 is not an essential component.

[0103] <Nonaqueous electrolyte secondary battery> The nonaqueous electrolyte secondary battery according to the embodiment of the present disclosure includes a positive electrode containing the above-described composite oxide as a positive electrode active material, and the nonaqueous electrolyte secondary battery is composed of a positive electrode, a negative electrode, and an electrolyte solution containing an electrolyte.

[0104] When manufacturing a positive electrode, a conductive agent and a binder are added to the composite oxide according to the embodiment of the present disclosure and mixed according to a conventional method. As the conductive agent, for example, acetylene black, carbon black, graphite, etc. are preferably used. As the binder, for example, polytetrafluoroethylene, polyvinylidene fluoride, etc. are preferably used.

[0105] The negative electrode is not particularly limited, but may be, for example, not only a negative electrode active material such as lithium metal, graphite, or a low-crystalline carbon material, but also one or more nonmetallic or metallic elements selected from Si, Al, Sn, Pb, Zn, Bi, and Cd, an alloy containing the same, or a chalcogen compound containing the same.

[0106] The solvent for the electrolyte is not particularly limited, but may be, for example, an organic solvent containing one or more selected from carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, and diethyl carbonate, and ethers such as dimethoxyethane.

[0107] As the electrolyte, in addition to lithium hexafluorophosphate (LiPF6), one or more selected from lithium salts such as lithium perchlorate and lithium tetrafluoroborate can be dissolved in a solvent and used. EXAMPLES

[0108] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0109] <Preparation of Complex Oxide Samples> The composite oxide samples of Examples 1 to 13 and Comparative Example 1 were prepared by the methods described below.

[0110] [Preparation of precursor composite hydroxide] (Preparation of precursor composite hydroxide 1) A mixed aqueous solution was obtained by mixing an aqueous nickel sulfate solution, an aqueous cobalt sulfate solution, and an aqueous manganese sulfate solution so that the ratio (molar ratio) of Ni, Co, and Mn was Ni:Co:Mn=83:5:12. 10 L of pure water to which 300 g of an aqueous sodium hydroxide solution and 500 g of an aqueous ammonia solution had been added was prepared in advance in the reaction tank as a mother liquid, and the reaction tank was filled with nitrogen gas at a flow rate of 0.7 L / min to create a nitrogen atmosphere, and the reaction was also carried out in a nitrogen atmosphere.

[0111] Thereafter, while rotating the stirring blade at 1000 rpm, the mixed aqueous solution, the sodium hydroxide aqueous solution, and the ammonia water were simultaneously dropped at a predetermined rate, and the amount of the alkaline solution dropped was adjusted so that the pH became 11.5. Through a crystallization reaction, Ni, Co, and Mn were crystallized and coprecipitated to form agglomerated particles, thereby obtaining a coprecipitate.

[0112] After that, the slurry in the reactor was separated into solid and liquid, and further washed with pure water to reduce residual impurities. The coprecipitate cake was then dried at 100°C for 10 hours in an air environment to obtain the product with the formula Ni 0.83 Co 0.05 Mn 0.12 A nickel-cobalt-manganese composite hydroxide represented by (OH)2 was obtained. The D50 of the obtained composite hydroxide precursor was 14.2 μm.

[0113] (Preparation of precursor composite oxide 2) A mixed aqueous solution was obtained by mixing an aqueous nickel sulfate solution, an aqueous cobalt sulfate solution, and an aqueous manganese sulfate solution so that the ratio (molar ratio) of Ni, Co, and Mn was Ni:Co:Mn=83:12:5. 10 L of pure water to which 330 g of an aqueous sodium hydroxide solution and 500 g of an aqueous ammonia solution had been added was prepared in advance in the reaction tank as a mother liquid, and the reaction tank was filled with nitrogen gas at a flow rate of 0.7 L / min to create a nitrogen atmosphere, and the reaction was also carried out in a nitrogen atmosphere.

[0114] Thereafter, while rotating the stirring blade at 1100 rpm, the mixed aqueous solution, the sodium hydroxide aqueous solution, and the ammonia water were simultaneously dropped at a predetermined rate, and the amount of the alkaline solution dropped was adjusted so that the pH became 12.6. Through a crystallization reaction, Ni, Co, and Mn were crystallized and coprecipitated to form agglomerated particles, thereby obtaining a coprecipitate.

[0115] After that, the slurry in the reactor was separated into solid and liquid, and further washed with pure water to reduce residual impurities. The coprecipitate cake was then dried at 100°C for 10 hours in an air environment to obtain the product with the formula Ni 0.83 Co 0.12 Mn 0.05 The nickel-cobalt-manganese composite hydroxide represented by (OH)2 was obtained by coprecipitation. The D50 of the obtained composite hydroxide precursor was 4.0 μm.

[0116] Example 1 The precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed and mixed so that Li / (Ni+Co+Mn+Al)=1.030 and Al / (Ni+Co+Mn+Al)=2.0 mol%. After that, the mixture was heat-treated at 570°C for 6 hours in an oxygen atmosphere, and then further calcined at 805°C for 6 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The resulting calcined product was pulverized to obtain a lithium nickel composite oxide powder.

[0117] The obtained lithium nickel composite oxide powder was mixed with pure water adjusted to a liquid temperature of 25°C so that the ratio was 1500 g / L to prepare a slurry, which was stirred for 10 minutes and then dehydrated to obtain a cake-like compound. The cake-like compound was dried in a vacuum dryer at 75°C for 2 hours and at 120°C for 10 hours.

[0118] 1000 ppm of boric acid was added as a boron compound to the dried lithium nickel composite oxide, mixed, and heat-treated at 325°C for 2 hours in an oxygen atmosphere (oxygen concentration: 97 vol%) to obtain a composite oxide sample of Example 1. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.009.

[0119] Example 2 A composite oxide sample of Example 2 was obtained in the same manner as in Example 1, except that precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al)=1.050 and Al / (Ni+Co+Mn+Al)=2.0 mol%. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.023.

[0120] Example 3 A composite oxide sample of Example 3 was obtained in the same manner as in Example 1, except that precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al)=1.070 and Al / (Ni+Co+Mn+Al)=2.0 mol%. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.045.

[0121] Example 4 A composite oxide sample of Example 4 was obtained in the same manner as in Example 1, except that precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al)=1.090 and Al / (Ni+Co+Mn+Al)=2.0 mol%. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.06.

[0122] Example 5 The precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed and mixed so that Li / (Ni+Co+Mn+Al)=1.010 and Al / (Ni+Co+Mn+Al)=3.0 mol%. Then, heat treatment was performed at 570°C for 6 hours in an oxygen atmosphere, and then calcined at 810°C for 6 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The calcined product was pulverized to obtain a lithium nickel composite oxide. After that, the composite oxide sample of Example 5 was obtained in the same manner as in Example 1. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.001.

[0123] Example 6 A composite oxide sample of Example 6 was obtained in the same manner as in Example 5, except that the precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al)=1.030 and Al / (Ni+Co+Mn+Al)=3.0 mol%. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.012.

[0124] Example 7 A composite oxide sample of Example 7 was obtained in the same manner as in Example 5, except that precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al) = 1.050 and Al / (Ni+Co+Mn+Al) = 3.0 mol%. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.032.

[0125] Example 8 A composite oxide sample of Example 8 was obtained in the same manner as in Example 5, except that precursor composite hydroxide 1, lithium hydroxide, and aluminum hydroxide were weighed out so that Li / (Ni+Co+Mn+Al) = 1.030 and Al / (Ni+Co+Mn+Al) = 1.0 mol %. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.008.

[0126] Example 9 The precursor composite hydroxide 2 and lithium hydroxide were weighed and mixed so that Li / (Ni+Co+Mn)=1.050. Then, the mixture was further fired at 860° C. for 12 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The fired product was pulverized to obtain a lithium nickel composite oxide powder.

[0127] The obtained lithium nickel composite oxide powder was further calcined in an oxygen atmosphere (oxygen concentration: 97 vol%) at 700° C. for 7 hours.

[0128] 500 ppm of boric acid was added as a boron compound to the calcined lithium nickel composite oxide, mixed, and heat-treated at 330°C for 7 hours in air to obtain a composite oxide sample of Example 9. The Li / (Ni+Co+Mn) of the obtained composite oxide sample was 1.015.

[0129] Example 10 A composite oxide sample of Example 10 was obtained in the same manner as in Example 9, except that precursor composite hydroxide 2 and lithium hydroxide were weighed out so that Li / (Ni+Co+Mn)=1.060. The Li / (Ni+Co+Mn) of the obtained composite oxide sample was 1.029.

[0130] Example 11 A composite oxide sample of Example 11 was obtained in the same manner as in Example 9, except that the precursor composite hydroxide 2 and lithium hydroxide were weighed out so that Li / (Ni+Co+Mn)=1.070. The Li / (Ni+Co+Mn) of the obtained composite oxide sample was 1.048.

[0131] Example 12 The precursor composite hydroxide 2 and lithium hydroxide were weighed and mixed so that Li / (Ni+Co+Mn)=1.070. Then, the mixture was further calcined at 860°C for 12 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The calcined product was pulverized to obtain a lithium nickel composite oxide powder.

[0132] The obtained lithium nickel composite oxide powder was added with 0.5 mol% of aluminum oxide powder Al2O3, and the mixture was heat-treated in air at 700°C for 7 hours. Thereafter, the composite oxide sample of Example 12 was obtained in the same manner as in Example 9. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.012.

[0133] Example 13 The precursor composite hydroxide 2 and lithium hydroxide were weighed and mixed so that Li / (Ni+Co+Mn)=1.050. Then, the mixture was fired at 860° C. for 12 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The fired product was pulverized to obtain a lithium nickel composite oxide powder.

[0134] To the obtained lithium nickel composite oxide powder, 0.8 mol% of aluminum oxide powder, Al2O3, was added, and the mixture was heat-treated at 600℃ in air for 7 hours to obtain a lithium metal composite oxide.

[0135] The lithium nickel composite oxide powder after the heat treatment was mixed with pure water adjusted to a liquid temperature of 25°C so that the ratio was 1500 g / L to prepare a slurry, which was stirred for 10 minutes and then dehydrated to obtain a cake-like compound. It was then dried in a vacuum dryer at 75°C for 2 hours and at 120°C for 10 hours.

[0136] 500 ppm of boric acid was added as a boron compound to the dried lithium nickel composite oxide, mixed, and heat-treated at 300°C for 7 hours in air to obtain a composite oxide sample of Example 13. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 0.989.

[0137] Comparative Example 1 The precursor composite hydroxide 2, lithium hydroxide, and aluminum hydroxide were weighed and mixed so that Li / (Ni+Co+Mn+Al)=1.050. Then, the mixture was fired at 860°C for 12 hours in an oxygen atmosphere (oxygen concentration: 97 vol%). The fired product was pulverized to obtain a lithium nickel composite oxide powder.

[0138] To the obtained lithium nickel composite oxide powder, 0.8 mol% of aluminum oxide powder Al2O3 was added, and the mixture was heat-treated in air at 700°C for 7 hours. Thereafter, the composite oxide sample of Comparative Example 1 was obtained in the same manner as in Example 9. The Li / (Ni+Co+Mn+Al) of the obtained composite oxide sample was 1.

[0139] <Evaluation> The obtained samples were evaluated by the methods described below.

[0140] [Composition analysis of precursor compounds and composite oxides] The composition of the precursor composite compound and composite oxide sample was determined by the following method. 0.2 g of the composite oxide sample was dissolved by heating in 25 ml of 20% hydrochloric acid solution, cooled, transferred to a 100 ml measuring flask, and pure water was added to prepare an adjusted solution. The elements in the resulting adjusted solution were quantified using ICP-AES (Optima 8300, manufactured by PerkinElmer Japan Co., Ltd.).

[0141] [Average particle size of precursor compound (D50)] The particle size distribution was measured by volume using a laser particle size distribution analyzer (Microtrac HRA, manufactured by Nikkiso Co., Ltd.) by the wet laser method.

[0142] [Thermogravimetric differential thermal analysis] To confirm the oxygen release behavior of the composite oxide samples, thermogravimetric differential thermal analysis (TG-DTA) was performed using a thermogravimetric differential thermal analysis (TG-DTA) device (DTG-60H, Shimadzu Corporation).

[0143] (Sample preparation) According to the method described later, a 2032 type coin cell with a lithium counter electrode was prepared, and in an environment of 25°C, it was charged at a constant current of 0.3C to 4.30V, and then charged at a constant voltage until the current value reached 0.05C. After that, it was left to rest for 20 minutes after charging was completed, and discharged at a constant current of 0.3C to 2.50V, and then discharged at a constant current of 0.1C, and then left to rest for 20 minutes. This charge and discharge was repeated twice. Next, it was charged at a constant current of 0.3C to 4.30V, and then charged at a constant voltage until the current value reached 0.05C, and then left to rest for 20 minutes after charging was completed.

[0144] The charged coin cell was disassembled in a glove box (dew point: -70°C or less) while taking care not to short circuit, and the positive electrode was separated. The separated positive electrode was washed with DMC for 10 minutes and dried under vacuum in a side box. After that, in the same glove box, the positive electrode mixture was scraped off from the Al foil using a spatula. 15 mg of the obtained powder of the positive electrode mixture was filled into an Al TG measurement container, and the container was covered and sealed using a crimping machine.

[0145] The Al measurement container thus obtained was taken out of the glove box and placed on the measurement side balance of the TG-DTA apparatus.

[0146] (TG-DTA measurement) Reference: Pt container filled with 15-20 mg of Al2O3 Maximum temperature: 600℃ Heating rate: (1) 25℃ (room temperature) to 50℃: 1℃ / min (2) 50℃~600℃: 5℃ / min Measurement environment: N2 gas atmosphere (200ml / min)

[0147] Just before the measurement, a small hole was opened in the lid of the sealed Al measurement vessel in the TG-DTA apparatus in a N2 gas atmosphere, and then the temperature was increased.

[0148] Based on the obtained results, a DTG curve is created with the horizontal axis representing temperature and the vertical axis representing the value obtained by differentiating the weight change (TG) with respect to time (differential thermogravimetric DTG, which means the weight loss rate, and corresponds to the oxygen release rate of the complex oxide in the range of 150 to 350°C).

[0149] Among the peaks having a peak top at 150 to 350°C in this DTG curve, the peak with the maximum value of the differential thermogravimetry was designated as the first peak (P1). The value of the differential thermogravimetry at the peak top was designated as the oxygen release rate (% / min). Furthermore, among the peaks having a peak top at a temperature 20°C or more away from the temperature showing the peak top of the first peak, the peak with the maximum value of the differential thermogravimetry was designated as the second peak (P2). Figures 1 to 13 are DTG curves of the composite oxide samples of Examples 1 to 13, respectively. Also, Figure 14 is a DTG curve of the composite oxide sample of Comparative Example 1.

[0150] [Crystal structure analysis by Rietveld refinement] Using an X-ray diffractometer [SmartLab, Rigaku Corporation], XRD diffraction data of the composite oxide sample was obtained under the following X-ray diffraction conditions, and then the Rietveld analysis was performed using the XRD diffraction data with reference to "RA Young, ed., "The Rietveld Method", Oxford University Press (1992)". Specifically, the ratio of lithium contained in the 3a site and 3b site, and the unit cell volume were calculated. (X-ray diffraction conditions) Source: Cu-Kα Acceleration voltage and current: 45kV and 200mA Sampling width: 0.02 deg. Scanning width: 15deg.~122deg. Scan speed: 1.0 step / sec Divergence slit: 2 / 3deg. Receiving slit width: 0.15 mm Scattering slit: 2 / 3deg.

[0151] [Evaluation of charging capacity of coin cells using composite oxide samples] In this specification, a 2032 type coin cell using the composite oxide sample as a positive electrode active material was manufactured using a positive electrode, a negative electrode, and an electrolyte prepared by the following methods.

[0152] (positive electrode) Acetylene black and graphite were used as conductive agents in a ratio of 1:1 (weight ratio), and polyvinylidene fluoride was used as a binder. The composite oxide sample, conductive agent, and binder were mixed in a ratio of 90:6:4 (weight ratio) of composite oxide sample:conductive agent:binder, and these were mixed in N-methylpyrrolidone and applied to aluminum foil. This was dried at 110°C to prepare a sheet, which was then punched out to a diameter of 15 mm and then coated with a 3t / cm 2 The resultant was rolled at 100° C. to prepare a positive electrode.

[0153] (Negative electrode) A lithium foil having a thickness of 500 μm and punched to 16 mmφ was used as the negative electrode.

[0154] (electrolyte) A mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) was prepared so that the volume ratio of EC:DMC was 1:2, and a solution in which 1 mol / L of LiPF6 was mixed with the electrolyte was used as the electrolyte solution.

[0155] (Separator) A separator (Celgard#2400, manufactured by Celgard) having a thickness of 0.5 mm and punched out to 20 mm in diameter was used.

[0156] (Total charge capacity measurement) Using the coin cell manufactured by the above-mentioned method, constant current charging was performed at 25°C at 0.3C up to 4.30V, followed by constant voltage charging until the current value reached 0.05C. After that, a 20-minute pause was taken after the completion of charging, and constant current discharging was performed at 0.3C up to 2.50V, followed by constant current discharging at 0.1C, followed by a 20-minute pause. This charging and discharging was repeated twice. Next, constant current charging was performed at 0.3C up to 4.30V, followed by constant voltage charging until the current value reached 0.05C. In the operation, the total charging capacity (mAh / g) was calculated as follows. ·1st charge / discharge 4.3V at 0.3C (constant voltage charging until 0.05C) 20 minute break Discharge at 0.3C to 2.5V, then discharge at 0.1C to 2.5V 20 minute break ·Second charge and discharge 4.3V at 0.3C (constant voltage charging until 0.05C) 20 minute break Discharge at 0.3C to 2.5V, then discharge at 0.1C to 2.5V 3rd charge 4.3V at 0.3C (constant voltage charging until 0.05C) Total charging capacity = 1st charge capacity + (2nd charge capacity - 1st discharge capacity at 0.3C - 1st discharge capacity at 0.1C) + (3rd charge capacity - 2nd discharge capacity at 0.3C - 2nd discharge capacity at 0.1C)

[0157] Table 1 shows the compositions of the composite oxides constituting the samples of Examples 1 to 13 and Comparative Example 1, the ratios of lithium contained in the 3a site and the 3b site, the unit cell volumes, the total charge capacities, the peak-top temperatures of the first peaks of the DTG curves, the differential thermogravimetry (oxygen release rate), and the reduction rates of the differential thermogravimetry compared to Comparative Example 1, the peak-top temperatures and differential thermogravimetry (oxygen release rate) of the second peaks, and the ratios of the thermogravimetry derivative at the peak top of the first peak to the thermogravimetry derivative at the peak top of the second peak (differential thermogravimetry at the peak top of the first peak / differential thermogravimetry at the peak top of the second peak).

[0158]

Table 1

Claims

1. General formula Li 1+x Ni 1-y-z-w Co y Mn z M w O 2 (wherein M is one or more elements other than Li, Ni, Co, Mn, and O, and −0.1≦x≦0.15, 0≦y≦0.4, 0≦z≦0.4, and 0≦w≦0.1), The composite oxide was charged to 4.30 V using lithium as a counter electrode, and the temperature was increased from 50° C. to 600° C. at a rate of 5° C. / min. The differential thermogravimetric curve was separated into multiple peaks. A first peak having a maximum value of the differential thermogravimetry at its peak top in a temperature range of 150° C. or more and 350° C. or less, and a second peak having a maximum value of the differential thermogravimetry at its peak top among the peaks having a peak top at a temperature 20° C. or more away from the temperature showing the peak top of the first peak, the value of the differential thermogravimetry at the peak top of the first peak relative to the value of the differential thermogravimetry at the peak top of the second peak is 1 or more and 9 or less; Positive electrode active material for non-aqueous electrolyte secondary batteries.

2. In the composite oxide, 0<x≦0.

15. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 .

3. The differential thermogravimetry value at the peak top of the first peak is 3% / min or less. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2.

4. A cathode containing the cathode active material according to claim 1 or 2 is provided. Nonaqueous electrolyte secondary battery.

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery and method for producing same

    JP2023511032A

  • Positive electrode active material particles for non-aqueous electrolyte secondary battery and production method therefor, and non-aqueous electrolyte secondary battery

    WO2019177017A1

  • Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery